Rubber composition for sheet conveyance rollers and sheet conveyance roller

The rubber composition for sheet conveyance rollers, featuring diene rubber and petroleum resin, addresses the challenge of achieving high friction and abrasion resistance, enhancing performance across various sheet types.

JP2024158365APending Publication Date: 2024-11-08SUMITOMO RUBBER INDUSTRIES LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023073514
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing sheet conveyance rollers face challenges in achieving a high coefficient of friction, particularly with the increasing diversity of sheet types in image forming apparatuses, and existing solutions using EPDM or isoprene/natural rubber do not adequately address this need.

Method used

A rubber composition for sheet conveyance rollers is developed, containing diene rubber as the base rubber with a minimum content of 50% by mass, combined with petroleum resin to enhance friction, and optionally including ethylene-α olefin or ethylene-vinyl acetate copolymers for improved ozone resistance, and a crosslinking agent for abrasion resistance.

Benefits of technology

The composition results in sheet conveyance rollers with enhanced friction coefficients and improved abrasion resistance, suitable for diverse sheet types and environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158365000004
    Figure 2024158365000004
  • Figure 2024158365000005
    Figure 2024158365000005
  • Figure 2024158365000001
    Figure 2024158365000001
Patent Text Reader

Abstract

To provide a rubber composition, comprising a base rubber and a crosslinking agent comparable to those used in the conventional art, capable of producing a sheet conveyance roller with enhanced friction coefficients.SOLUTION: A rubber composition for sheet conveyance rollers contains a base rubber and a petroleum resin, where the base rubber contains a diene rubber, and the content of the diene rubber is 50 mass% or more based on the base rubber 100 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition used in forming a sheet-conveying roller. [Background technology]

[0002] Various types of sheet transport rollers are incorporated in the sheet transport mechanisms of image forming devices such as electrostatic copiers, laser printers, plain paper facsimile devices, and multifunction devices thereof, inkjet printers, as well as document processing devices that perform document scanners and sorting. The sheet transport rollers rotate while in contact with a sheet such as paper or plastic film, transporting the sheet by friction.

[0003] As a material for sheet transport rollers, ethylene propylene diene monomer copolymer (EPDM) is often used from the viewpoints of friction coefficient, environmental resistance (e.g., ozone resistance), and cost. Here, in recent years, the types of sheets used in image forming devices and the like have become more diverse, and there are cases in which a high friction coefficient is required for the sheet transport rollers.

[0004] Therefore, a technique for increasing the friction coefficient of a roller using EPDM has been proposed.For example, Patent Document 1 describes a paper feed roller including a roller body made of a rubber composition for forming a roller body of a paper feed roller, the rubber composition containing a non-oil-extended ethylene propylene diene rubber having an ethylene content of 55% or more and 72% or less and an oil-extended ethylene propylene diene rubber as rubber components, the proportion of the non-oil-extended ethylene propylene diene rubber being 20 parts by mass or more and 80 parts by mass or less in 100 parts by mass of the total amount of the rubber (see Patent Document 1 (Claim 5, Table 1)).

[0005] Also, a technique has been proposed for increasing the friction coefficient of the roller by changing the main component of the base rubber to isoprene rubber or natural rubber.For example, Patent Document 2 describes a paper feed roller including a roller body, the roller body being made of a crosslinked product of a rubber composition containing at least one isoprene-based rubber (excluding epoxidized natural rubber) selected from the group consisting of isoprene rubber and natural rubber in a ratio of 55 parts by mass or more per 100 parts by mass of the total amount of rubber (see Patent Document 2 (Claim 1, Table 1)). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-2271 A [Patent Document 2] Patent Publication No. 2021-91549 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a rubber composition containing a similar base rubber and a crosslinking agent, which can be used to produce a sheet conveying roller having an excellent friction coefficient. [Means for solving the problem]

[0008] The rubber composition for a sheet-conveying roller of the present invention, which has been able to solve the above-mentioned problems, is characterized in that it contains a base rubber and a petroleum resin, the base rubber contains a diene-based rubber, and the content of the diene-based rubber is 50 mass% or more in 100 mass% of the base rubber. Effect of the Invention

[0009] According to the present invention, a rubber composition that can be used to prepare a sheet-conveying roller having an excellent friction coefficient can be obtained from a rubber composition that contains the same base rubber and crosslinking agent. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a perspective view showing an example of a sheet conveying roller of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a method for measuring a friction coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The rubber composition for a sheet conveying roller of the present invention (hereinafter, may be simply referred to as the "rubber composition") contains a base rubber and a petroleum resin, the base rubber contains a diene-based rubber, and the content of the diene-based rubber is 50 mass% or more in 100 mass% of the base rubber.

[0012] The rubber composition for a sheet transport roller of the present invention uses a diene rubber as the main component of the base rubber, thereby making it possible to increase the friction coefficient of the resulting sheet transport roller. In addition, by adding a petroleum resin to the rubber composition for a sheet transport roller, the friction coefficient of the resulting sheet transport roller can be further increased.

[0013] (Base rubber) The rubber composition contains a diene rubber as a base rubber. The diene rubber may be used alone or in combination of two or more kinds.

[0014] Examples of the diene rubber include isoprene rubber, natural rubber, styrene-butadiene rubber, butadiene rubber, acrylonitrile butadiene rubber, and chloroprene rubber.

[0015] (Isoprene rubber (IR)) As the isoprene rubber, any of various polymers having a polyisoprene structure, which artificially reproduces the structure of natural rubber, can be used. In particular, in consideration of improving the workability when preparing a rubber composition, molding it into the shape of the roller body, and then crosslinking it to form the roller body, isoprene rubber that is semi-solid or solid at room temperature (5 to 35°C) before crosslinking is preferred.

[0016] (Natural Rubber (NR)) Examples of natural rubber include various natural rubbers having any Mooney viscosity, such as SMR (standard Malaysian rubber), SVR (standard Vietnam rubber), SIR (standard Indonesian rubber), STR (standard Thai rubber), SSR (standard Singapore rubber), and SCR (standard Ceylon rubber), which are classified by place of production; and sheet rubbers of various grades, such as ribbed smoked sheet, white crepe, pale crepe, estate brown crepe, compo crepe, thin brown crepe, and thick blanket crepe, which are classified by the Green Book.

[0017] As the natural rubber, for example, modified natural rubber such as deproteinized natural rubber, hydrogenated natural rubber, and grafted natural rubber can be used.

[0018] (Styrene butadiene rubber (SBR)) The styrene-butadiene rubber is a copolymer of styrene and 1,3-butadiene, and any of various crosslinkable styrene-butadiene rubbers can be used. Examples of the styrene-butadiene rubber include those obtained by emulsion polymerization and those obtained by solution polymerization, and those obtained by emulsion polymerization are preferred.

[0019] As the styrene-butadiene rubber, any of high styrene type, medium styrene type, and low styrene type styrene-butadiene rubbers classified according to the styrene content can be used. The styrene content of the styrene-butadiene rubber is preferably 15% by mass or more, more preferably 20% by mass or more, and is preferably 45% by mass or less, more preferably 35% by mass or less.

[0020] The content of the diene rubber in 100% by mass of the base rubber is 50% by mass or more, preferably 55% by mass or more, and more preferably 60% by mass or more, and the base rubber may contain only the diene rubber. If the content of the diene rubber in the base rubber is 50% by mass or more, the friction coefficient of the obtained sheet conveying roller can be increased.

[0021] The rubber composition preferably contains isoprene rubber and / or natural rubber as a diene rubber. In this case, the total content of isoprene rubber and natural rubber in 100% by mass of the base rubber is preferably 30% by mass or more, more preferably 40% by mass or more, and the base rubber may contain only isoprene rubber and / or natural rubber.

[0022] (Other rubber components) The base rubber may contain rubber components other than the diene rubber to the extent that the effects of the present invention are not impaired.

[0023] Examples of the other rubber components include non-diene rubbers such as ethylene-α-olefin copolymers, ethylene-vinyl acetate copolymers, epichlorohydrin rubbers, acrylic rubbers, butyl rubbers, silicone rubbers, etc. These other rubber components may be used alone or in combination of two or more.

[0024] The base rubber may further contain an ethylene-α-olefin copolymer and / or an ethylene-vinyl acetate copolymer, which improves the ozone resistance of the resulting sheet conveying roller.

[0025] When the rubber composition contains an ethylene-α-olefin copolymer and / or an ethylene-vinyl acetate copolymer as the base rubber, the total content of the ethylene-α-olefin copolymer and the ethylene-vinyl acetate copolymer in 100% by mass of the base rubber is preferably 25% by mass or more, more preferably 30% by mass or more, and is preferably less than 50% by mass, more preferably 40% by mass or less.

[0026] (Ethylene-α-olefin copolymer) The ethylene-α-olefin copolymer is a copolymer containing at least ethylene and an α-olefin as constituent components, and also includes an ethylene-α-olefin-diene copolymer in which a double bond is introduced into the main chain by adding a small amount of a diene component to ethylene and an α-olefin.

[0027] Examples of the α-olefin include propylene, 1-butene, 1-hexene, and 1-octene. Examples of the diene component include ethylidene norbornene (ENB), 1,4-hexadiene (1,4-HD), dicyclopentadiene (DCP), and the like, with ethylidene norbornene being preferred.

[0028] Examples of the ethylene-α-olefin copolymer include ethylene-propylene copolymer (EPM), ethylene-butene copolymer (EBR), ethylene-octene copolymer (EOR), etc. Examples of the ethylene-α-olefin-diene copolymer include ethylene-propylene-diene copolymer (EPDM), ethylene-butene-diene copolymer (EBDM), ethylene-propylene-butene-diene copolymer (EPBDM), etc.

[0029] (Ethylene-vinyl acetate copolymer) The ethylene-vinyl acetate copolymer is a copolymer of ethylene and vinyl acetate. The vinyl acetate content of the ethylene-vinyl acetate copolymer is 10% by mass or more, preferably 14% by mass or more, and 50% by mass or less, preferably 46% by mass or less.

[0030] (petroleum resin) The rubber composition contains a petroleum resin. By containing the petroleum resin, the friction coefficient of the sheet conveying roller can be further increased. The petroleum resin may be used alone or in combination of two or more kinds.

[0031] The petroleum resin is a resin obtained by polymerizing or copolymerizing a petroleum fraction obtained as a by-product when petroleum such as naphtha is thermally decomposed to produce olefins such as ethylene. Note that the raw material for the petroleum resin does not need to be entirely petroleum fractions, and may contain chemically synthesized unsaturated compounds.

[0032] Examples of the petroleum fraction include aliphatic olefins having 4 to 10 carbon atoms, aliphatic diolefins having 4 to 10 carbon atoms, and aromatic compounds having 8 or more carbon atoms and an olefinically unsaturated bond.

[0033] Examples of the aliphatic olefins having 4 to 10 carbon atoms include butene, pentene, hexene, heptene, etc. Examples of the aliphatic diolefins having 4 to 10 carbon atoms include butadiene, pentadiene, isoprene, cyclopentadiene, dicyclopentadiene, methylpentadiene, etc. Examples of the aromatic compounds having 8 or more carbon atoms and an olefinically unsaturated bond include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, indene, methylindene, ethylindene, etc.

[0034] Examples of the chemically synthesized unsaturated compounds include cyclopentadiene and dicyclopentadiene (DCPD).

[0035] The petroleum resins include aliphatic petroleum resins obtained by polymerizing aliphatic olefins and / or aliphatic diolefins; aromatic petroleum resins obtained by polymerizing aromatic compounds having olefinic unsaturated bonds; aliphatic-aromatic copolymer petroleum resins obtained by copolymerizing aliphatic olefins and / or aliphatic diolefins with aromatic compounds having olefinic unsaturated bonds; dicyclopentadiene petroleum resins obtained by polymerizing cyclopentadiene or dicyclopentadiene; and olefins obtained by polymerizing aliphatic olefins and / or aliphatic diolefins with cyclopentadiene or dicyclopentadiene. Examples of such resins include aliphatic-dicyclopentadiene copolymer petroleum resins; aromatic-dicyclopentadiene copolymer petroleum resins obtained by copolymerizing an aromatic compound having an olefinic unsaturated bond with cyclopentadiene or dicyclopentadiene; aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins obtained by polymerizing aliphatic olefins and / or aliphatic diolefins, an aromatic compound having an olefinic unsaturated bond, and cyclopentadiene or dicyclopentadiene; and styrene resins obtained by polymerizing styrene compounds (styrene, α-methylstyrene, β-methylstyrene).

[0036] In addition, the petroleum resin may be a hydrogenated petroleum resin obtained by adding hydrogen atoms to a polymer obtained by polymerizing the petroleum fraction or a chemically synthesized unsaturated compound. By adding hydrogen atoms, the double bonds in the molecule are hydrogenated. The hydrogenated product may be either a fully hydrogenated petroleum resin in which all the double bonds in the molecule are hydrogenated, or a partially hydrogenated petroleum resin in which some of the double bonds in the molecule are hydrogenated.

[0037] Examples of hydrogenated petroleum resins include hydrogenated aliphatic petroleum resins obtained by hydrogenating aliphatic petroleum resins; hydrogenated aromatic petroleum resins obtained by hydrogenating aromatic petroleum resins; hydrogenated aliphatic-aromatic copolymer petroleum resins obtained by hydrogenating aliphatic-aromatic copolymer petroleum resins; hydrogenated dicyclopentadiene petroleum resins obtained by hydrogenating dicyclopentadiene petroleum resins; hydrogenated aliphatic-dicyclopentadiene copolymer petroleum resins obtained by hydrogenating aliphatic-dicyclopentadiene copolymer petroleum resins; hydrogenated aromatic-dicyclopentadiene copolymer petroleum resins obtained by hydrogenating aromatic-dicyclopentadiene copolymer petroleum resins; and hydrogenated aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins obtained by hydrogenating aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins.

[0038] The petroleum resin is preferably one or more petroleum resins selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, aliphatic-aromatic copolymer petroleum resins, dicyclopentadiene petroleum resins, aliphatic-dicyclopentadiene copolymer petroleum resins, aromatic-dicyclopentadiene copolymer petroleum resins, aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aliphatic petroleum resins, hydrogenated aromatic petroleum resins, hydrogenated aliphatic-aromatic copolymer petroleum resins, hydrogenated dicyclopentadiene petroleum resins, hydrogenated aliphatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aromatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins, and styrene-based resins.

[0039] The softening point of the petroleum resin is preferably 50° C. or higher, more preferably 60° C. or higher, and even more preferably 70° C. or higher, and is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 130° C. or lower. If the softening point is 50° C. or higher, the resin is easy to handle during storage and measurement, and if the softening point is 150° C. or lower, the resin is easy to soften during kneading and is easy to knead. The softening point of the petroleum resin is measured in accordance with 7.7 Softening Point of JIS K6220-1 (2015).

[0040] The content of the petroleum resin in the rubber composition is preferably 1.0 part by mass or more, more preferably 1.5 parts by mass or more, and even more preferably 2.0 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 13 parts by mass or less, and even more preferably 12 parts by mass or less, based on 100 parts by mass of the base rubber. If the content of the petroleum resin is 1.0 part by mass or more, the friction coefficient of the sheet conveying roller is further improved, and if it is 15 parts by mass or less, adhesion to the inner wall of the device during kneading is suppressed, and processability is improved.

[0041] (Crosslinking agent) The rubber composition preferably contains a crosslinking agent, which improves the abrasion resistance of the resulting sheet conveying roller. As the crosslinking agent, any of a sulfur-based crosslinking agent, an organic peroxide, and a resin crosslinking agent can be used. In addition, when there is a concern that the friction coefficient of the roller will decrease due to blooming of the sulfur-based crosslinking agent, it is preferable to use an organic peroxide as the crosslinking agent.

[0042] The sulfur-based crosslinking agent may be elemental sulfur or a sulfur donor compound. The elemental sulfur may be powdered sulfur, precipitated sulfur, colloidal sulfur, or insoluble sulfur. The sulfur donor compound may be 4,4'-dithiobismorpholine. The sulfur-based crosslinking agent may be used alone or in combination of two or more kinds.

[0043] When the sulfur-based crosslinking agent is compounded, the content of the sulfur-based crosslinking agent in the rubber composition is preferably 0.1 part by mass or more, more preferably 0.2 part by mass or more, and even more preferably 0.5 part by mass or more, per 100 parts by mass of the base rubber, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less.

[0044] Examples of the organic peroxide include dicumyl peroxide, α,α'-bis(t-butylperoxy-m-diisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, etc. The organic peroxides may be used alone or in combination of two or more kinds.

[0045] When the organic peroxide is compounded, the content of the organic peroxide in the rubber composition is preferably 0.1 part by mass or more, more preferably 0.5 part by mass or more, and even more preferably 1.0 part by mass or more, per 100 parts by mass of the base rubber, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less.

[0046] Examples of the resin crosslinking agent include alkylphenol formaldehyde resins such as alkylphenol formaldehyde resins, heat-reactive phenol resins, phenol dialcohol-based resins, bisphenol resins, and heat-reactive bromomethyl alkylated phenol resins.

[0047] (Crosslinking accelerator) When a sulfur-based crosslinking agent is used as the crosslinking agent, the rubber composition may further contain a crosslinking accelerator. As the crosslinking accelerator, either an inorganic accelerator or an organic accelerator can be used. Examples of the inorganic accelerator include slaked lime, magnesia (MgO), and litharge (PbO). Examples of the organic accelerator include a thiazole-based accelerator, a thiuram-based accelerator, a sulfenamide-based accelerator, and a dithiocarbamate-based accelerator. The crosslinking accelerator may be used alone or in combination of two or more kinds. As the crosslinking accelerator to be combined with the sulfur-based crosslinking agent, it is preferable to use a thiazole-based accelerator and a thiuram-based accelerator in combination.

[0048] Examples of the thiazole-based accelerator include 2-mercaptobenzothiazole, 2,2'-dibenzothiazolyl disulfide, the zinc salt of 2-mercaptobenzothiazole, the cyclohexylamine salt of 2-mercaptobenzothiazole, 2-(N,N-diethylthiocarbamoylthio)benzothiazole, and 2-(4'-morpholinodithio)benzothiazole, and di-2-benzothiazolyl disulfide is preferred.

[0049] Examples of the thiuram accelerator include tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, dipentamethylenethiuram tetrasulfide, and the like, with tetramethylthiuram monosulfide being preferred.

[0050] The amount of the thiazole accelerator used is preferably at least 0.1 part by weight and no more than 10 parts by weight per 100 parts by weight of the base rubber. The amount of the thiuram accelerator used is preferably at least 0.1 part by weight and no more than 10 parts by weight per 100 parts by weight of the base rubber.

[0051] (Crosslinking promoter) The rubber composition may contain a crosslinking promoter. Examples of the crosslinking promoter include zinc oxide and stearic acid. The amount of the crosslinking promoter used is preferably 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the base rubber.

[0052] (Other Ingredients) The rubber composition may contain compounding agents that are generally used as compounding agents for rubber, such as fillers, processing aids, antioxidants, viscosifiers, and pigments, within the scope of the present invention.

[0053] As the filler, those generally used as compounding agents for rubber can be used, such as carbon black, silica, calcium carbonate, talc, clay, magnesium carbonate, aluminum oxide, etc., with carbon black and calcium carbonate being preferred.

[0054] The amount of the filler, per 100 parts by mass of the base rubber, is preferably at least 5 parts by mass, more preferably at least 10 parts by mass, even more preferably at least 15 parts by mass, and particularly preferably at least 20 parts by mass; it is preferably at most 100 parts by mass, more preferably at most 70 parts by mass, and even more preferably at most 50 parts by mass.

[0055] Examples of the processing aid include fatty acids having 12 to 30 carbon atoms (such as stearic acid), fatty acid esters, fatty acid metal salts, fatty acid amides, hydrocarbons (paraffin), and process oils.

[0056] Examples of the antioxidant include nickel diethyldithiocarbamate and nickel dibutyldithiocarbamate.

[0057] The rubber composition preferably does not contain an oil component such as an extender oil, a process oil, etc. The content of the oil component in the rubber composition is preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and further preferably 1 part by mass or less, per 100 parts by mass of the base rubber.

[0058] The hardness (Durometer type A hardness) of the cured product of the rubber composition is preferably 10 or more, more preferably 15 or more, and even more preferably 20 or more, and is preferably 90 or less, more preferably 85 or less, and even more preferably 80 or less. If the hardness of the cured product is 10 or more, the hardness becomes suitable for sheet conveyance, and the conveying force is further improved, and if the hardness is 90 or less, it is easier to press-fit the roller shaft.

[0059] <Production of Rubber Composition for Sheet Conveying Roller> The rubber composition for the sheet conveying roller can be prepared by blending the base rubber and, if necessary, other raw materials, and kneading them with a kneader, a Banbury mixer, an open roll, etc. The kneading method and conditions are appropriately selected depending on the production scale.

[0060] The method for producing the rubber composition for the sheet conveying roller preferably comprises kneading a base rubber containing 50% by mass or more of a diene rubber with the petroleum resin at a temperature equal to or higher than the softening point of the petroleum resin. In other words, the rubber composition for the sheet conveying roller is preferably obtained by kneading a base rubber containing 50% by mass or more of a diene rubber with the petroleum resin at a temperature equal to or higher than the softening point of the petroleum resin.

[0061] The mixing temperature (material temperature) when mixing the base rubber and the petroleum resin is preferably equal to or higher than the softening point of the petroleum resin. By mixing at a temperature equal to or higher than the softening point of the petroleum resin, the petroleum resin can be mixed uniformly into the rubber. When a plurality of petroleum resins are contained, the petroleum resins are mixed at a temperature equal to or higher than the softening point of the petroleum resin having the highest softening point. When the softening point of the petroleum resin is T°C, the mixing temperature is more preferably T+3°C or higher, and even more preferably T+5°C or higher. When a plurality of petroleum resins are contained, the softening point of the petroleum resin having the highest softening point is T°C. The upper limit of the mixing temperature is not particularly limited, but is usually less than 200°C.

[0062] When the rubber composition contains a crosslinking agent, the method for producing the rubber composition preferably includes a first step of kneading a base rubber containing 50% by mass or more of a diene rubber with a petroleum resin at a temperature equal to or higher than the softening point of the petroleum resin to obtain a kneaded mixture, and a second step of mixing the crosslinking agent into the kneaded mixture. By including the first and second steps, the petroleum resin can be uniformly dispersed in the rubber component, and scorching caused by the crosslinking agent can be suppressed.

[0063] In the first step, the base rubber and the petroleum resin are mixed to prepare a mixture. The mixing temperature (material temperature) when mixing the base rubber and the petroleum resin is preferably equal to or higher than the softening point of the petroleum resin. By mixing at a temperature equal to or higher than the softening point of the petroleum resin, the petroleum resin can be mixed uniformly into the rubber. When a plurality of petroleum resins are contained, the petroleum resins are mixed at a temperature equal to or higher than the softening point of the petroleum resin having the highest softening point. The mixing temperature in the first step is more preferably equal to or higher than T+3°C, and even more preferably equal to or higher than T+5°C, where T°C is the softening point of the petroleum resin. The upper limit of the mixing temperature in the first step is not particularly limited, but is usually less than 200°C. When a plurality of petroleum resins are contained, the softening point of the petroleum resin having the highest softening point is taken as T°C.

[0064] The mixing in the first step can be carried out using a kneader, a Banbury mixer, an open roll, or the like, and is preferably carried out using a kneader.

[0065] In the first step, only the base rubber and the petroleum resin may be mixed, or other components other than the crosslinking agent (crosslinking promoter, filler, processing aid, antioxidant) may also be mixed in. Note that in the first step, the crosslinking agent and the crosslinking promoter are not mixed.

[0066] In the second step, the mixture is mixed with a crosslinking agent to prepare a rubber composition. The mixing temperature (material temperature) when mixing the mixture with the crosslinking agent is preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher, and is preferably 150° C. or lower, more preferably 120° C. or lower, and even more preferably 100° C. or lower. If the mixing temperature is 30° C. or higher, the crosslinking agent can be easily mixed due to the plasticization of the rubber, and if the mixing temperature is 150° C. or lower, scorch can be suppressed.

[0067] The mixing in the second step can be carried out using a kneader, a Banbury mixer, an open roll, or the like, and is preferably carried out using an open roll.

[0068] When the rubber composition contains a crosslinking promoter, the crosslinking promoter is preferably added in the second step. When the rubber composition contains a filler, a processing aid, or an antiaging agent, these components are preferably added in the first step.

[0069] <Sheet transport roller> The sheet conveying roller of the present invention is molded from the rubber composition for a sheet conveying roller. The shape of the sheet transport roller may be cylindrical, columnar, polygonal tubular, or polygonal columnar. When the sheet transport roller is cylindrical or polygonal tubular, it is preferable that the sheet transport roller has a shaft. The material of the shaft is not particularly limited, and may be metal, ceramic, resin, or the like.

[0070] An example of a sheet conveying roller is shown in Fig. 1. The sheet conveying roller 1 shown in Fig. 1 includes a roller body 2 formed into a cylindrical shape from the rubber composition for a sheet conveying roller of the present invention described above. A through hole 3 having a circular cross section is provided in the center of the roller body 2, and a cylindrical shaft 4 connected to a drive system (not shown) is inserted and fixed into the through hole 3. The outer circumferential surface of the roller body 2 is formed into a cylindrical shape concentric with the through hole 3 and the shaft 4.

[0071] The roller body 2 and the shaft 4 are fixed to each other so as not to slip, for example, by press-fitting the shaft 4, whose outer diameter is larger than the inner diameter of the through hole 3, into the through hole 3 of the roller body 2. In other words, a certain amount of slip torque (the limit torque at which slip does not occur) is ensured between the two by the tightening margin based on the diameter difference between the two.

[0072] The shaft 4 is made of, for example, metal, ceramic, hard resin, etc. A plurality of roller bodies 2 may be fixed to a single shaft 4 at a plurality of positions, if necessary. Methods for manufacturing the roller body 2 include a method in which a rubber composition is molded into a cylindrical shape by extrusion molding or the like, and then crosslinked by a press crosslinking method or the like; and a method in which a rubber composition is molded into a cylindrical shape and crosslinked at the same time by transfer molding or the like.

[0073] At any point in the above manufacturing process, the outer circumferential surface of the roller body 2 may be polished to a predetermined surface roughness, knurled, embossed, or the like, as necessary. In addition, both ends of the roller body 2 may be cut so that the outer circumferential surface has a predetermined width. The outer circumferential surface of the roller body 2 may be covered with any coating layer.

[0074] The roller body 2 may be formed in a two-layer structure with an outer layer on the outer peripheral surface side and an inner layer on the through hole 3 side. In that case, it is preferable that at least the outer layer is formed from the rubber composition of the present invention. However, in consideration of simplifying the structure, improving productivity, and reducing manufacturing costs, it is preferable that the roller body 2 has a single-layer structure as shown in FIG.

[0075] The roller body 2 may have a porous structure. However, in order to improve wear resistance and reduce compression set, thereby making it difficult for dents to form due to deformation even if contact at one point continues for a relatively long period of time, it is preferable that the roller body 2 has a substantially non-porous structure.

[0076] Depending on the application of the sheet conveying roller 1, the through hole 3 may be provided at a position eccentric to the center of the roller body 2. In addition, the outer circumferential surface of the roller body 2 may be irregularly shaped rather than cylindrical, for example, with a part of the cylindrical outer circumferential surface cut out in a flat shape. To manufacture the sheet conveying roller 1 having the roller body 2 of such an irregular shape, the roller body 2 of the irregular shape may be directly molded by the manufacturing method described above and then crosslinked, or the roller body 2 molded into a cylindrical shape may be post-processed to have the irregular shape.

[0077] Alternatively, the roller body 2 may be deformed into the irregular shape by press-fitting the shaft 4 having a deformed shape corresponding to the irregular shape of the roller body 2 formed into a cylindrical shape into the through hole 3 of the roller body 2 . In this case, the polishing, knurling, embossing, etc. of the outer peripheral surface 5 is performed on the cylindrical outer peripheral surface before deformation. 5, improving workability.

[0078] <Image forming device> The sheet transport roller of the present invention can be incorporated in, for example, various image forming devices utilizing electrophotography, such as laser printers, electrostatic copying machines, plain paper facsimile machines, or multifunction machines thereof, document processing devices that perform document scanners and sorting, etc. The sheet transport roller of the present invention can also be incorporated in, for example, inkjet printers, ATMs, etc. In particular, the sheet transport roller of the present invention contains a petroleum resin and thus has an excellent friction coefficient, and is therefore suitable as a roller for a document processing device that requires high transport capacity.

[0079] The sheet conveying roller of the present invention rotates while in contact with the sheet, and conveys the sheet by friction. The sheet may be a single sheet such as a sheet of paper, or a continuous sheet such as continuous paper. The sheet conveying roller can be used as, for example, a paper feed roller, a conveying roller, a platen roller, a paper discharge roller, etc. EXAMPLES

[0080] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.

[0081] [Evaluation method] (1)Hardness The hardness of the cured rubber composition was measured using a hardness tester (manufactured by Kobunshi Keiki Co., Ltd.) in accordance with JIS K6253-3 (2012). Specifically, the rubber composition was pressed at 170°C for 20 minutes to produce a sheet with a thickness of 2 mm. Three of these sheets were stacked together so as to avoid the influence of the measurement substrate, and the pressure plate of a type A durometer was brought into contact with the sheets, and the value was read 3 seconds after the contact.

[0082] (2) Tensile strength, elongation at break The tensile strength and breaking elongation (elongation at break) of the cured rubber composition were measured in accordance with JIS K6251 (2017). Specifically, the rubber composition was pressed at 170°C for 20 minutes to produce a sheet with a thickness of 2 mm, which was then punched into a dumbbell shape (dumbbell shape No. 3, thickness of parallel part 2 mm, initial gauge distance 20 mm) to produce a test specimen. The physical properties were measured using a tensile test measuring device (measurement temperature 23°C, tensile speed 500 mm / min). The tensile strength was calculated by dividing the maximum tensile force recorded when the test specimen was pulled until it broke by the cross-sectional area of ​​the test specimen before the test.

[0083] (3) Friction coefficient measurement As shown in Fig. 2, plain paper 11 (P paper (width 60 mm, length 210 mm) manufactured by Fujifilm Business Innovation) was placed on a horizontally placed polytetrafluoroethylene (PTFE) plate 10. The roller body 2 of the sheet transport roller 1 was placed on this paper 11, and a vertical load W1 (=300 gf) was applied to the shaft 4 to press it against the plate 10. Next, in an environment of a temperature of 23°C and a relative humidity of 55%, the roller body 2 was rotated at 200 rpm in the direction indicated by the dashed arrow R1, and the conveying force F (gf) applied to the load cell 12 connected to one end of the paper 11 was measured. The initial friction coefficient μ was calculated from the measured conveying force F and the vertical load W1 (=300 gf) using formula (1). μ = F(gf) / W1(gf) (1)

[0084] (4) Forced wear test As shown in Fig. 2, plain paper 11 (P paper, manufactured by Fujifilm Business Innovation) was placed on a horizontally placed polytetrafluoroethylene (PTFE) plate 10. The roller body 2 of the sheet transport roller 1 was placed on this paper 11, and a vertical load W1 (=500 gf) was applied to the shaft 4 to press it against the plate 10. Next, the roller body 2 was rotated continuously for 10 minutes at 200 rpm in the direction indicated by the dashed arrow R1 at a temperature of 23°C and a relative humidity of 55%. After that, the abrasion weight loss rate (%) was calculated from the mass W0 (g) of the roller body 2 before rotation and the mass W1 (g) of the roller body 2 after rotation according to the following formula (2). Abrasion weight loss rate (%) = 100 × (W0-W1) / W0(2)

[0085] [Preparation of Rubber Composition] The raw materials were mixed to prepare the rubber compositions according to the formulations shown in Tables 1 to 3. Specifically, the base rubber, petroleum resin, and filler were first mixed using a kneader to prepare a mixture. At this time, mixing was continued for 1 minute after the temperature (material temperature) in the kneader tank reached a predetermined temperature. The resulting mixture was then cooled, and the mixture was mixed with a crosslinking agent, and if necessary, a crosslinking accelerator and a crosslinking accelerator assistant, using an open roll with a surface temperature controlled to 30°C to 50°C to prepare a rubber composition. The measurement results of the cured product of the obtained rubber composition are shown in Tables 1 to 3.

[0086] [Table 1]

[0087] [Table 2]

[0088] [Table 3]

[0089] The raw materials used in Tables 1 to 3 are as follows. IR: "Nipol(R) IR2200" (isoprene rubber) manufactured by Zeon Corporation NR: Made in Vietnam, natural rubber (CV-60) SBR: Nipol (registered trademark) 1502 (non-oil extended styrene butadiene rubber, bound styrene content: 23.5% by mass, Mooney viscosity ML) manufactured by Zeon Corporation 1+4(100℃) 52.0) EPDM: Sumitomo Chemical's "Esprene (registered trademark) 505A" (non-oil extended EPDM) (ethylene-propylene-ethylidene norbornene copolymer, ethylene content 50% by mass, diene component content 9.5% by mass). Petroleum resin 1: ENEOS, "T-REZ (registered trademark) HA085" (hydrogenated dicyclopentadiene-based petroleum resin, softening point 88.0°C) Petroleum resin 2: ENEOS, "T-REZ PR801" (hydrogenated aromatic-dicyclopentadiene copolymer petroleum resin, softening point 90.0°C) Petroleum resin 3: Manufactured by ENEOS, "T-REZ RB093" (aliphatic petroleum resin, softening point 93.0℃) Petroleum resin 4: Manufactured by ENEOS, "T-REZ RD104" (aliphatic-aromatic copolymer petroleum resin, softening point 103.0℃) Petroleum resin 5: Tosoh Corporation, "Petrotack (registered trademark) 100V" (aliphatic-aromatic copolymer petroleum resin, softening point 96°C) Petroleum resin 6: Tosoh Corporation, "Petcol (registered trademark) LX" (aromatic petroleum resin, softening point 98°C) Petroleum resin 7: Arakawa Chemical Industries, "ARKON (registered trademark) M-100" (partially hydrogenated aromatic petroleum resin, softening point 100°C) Petroleum resin 8: Arakawa Chemical Industries, "ARKON P-100" (fully hydrogenated aromatic petroleum resin, softening point 100°C) Petroleum resin 9: Yasuhara Chemical's "YS Resin SX100" (styrene resin, softening point 100°C) Carbon black: Tokai Carbon Co., Ltd., Seast (registered trademark) 3 Calcium carbonate: BF-300, manufactured by Bihoku Powder Industry Co., Ltd. Zinc oxide: Mitsui Mining & Smelting Co., Ltd., zinc oxide type 2 Stearic acid: NOF Corp., Tsubaki stearate Sulfur: Tsurumi Chemical, 5% oil-containing sulfur Crosslinking accelerator 1: "Noccela (registered trademark) TOT-N" (tetrakis(2-ethylhexyl)thiuram disulfide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Crosslinking accelerator 2: Ouchi Shinko Chemical Industry's "Noccela DM" (2,2'-dibenzothiazolyl disulfide) Organic peroxide: NOF Corp.'s "Percumyl (registered trademark) D" (dicumyl peroxide)

[0090] [Manufacturing of sheet transport rollers] The rubber composition obtained above was transferred into a cylindrical shape at 170°C for 30 minutes. A shaft (outer diameter 12 mm) was pressed into the cylindrical molded body, and the rubber roller was ground using a cylindrical grinder so that the outer diameter of the rubber roller was 22 mm. The width of the rubber roller portion was cut to 25 mm to produce a sheet conveying roller. The evaluation results of the obtained sheet conveying roller are shown in Tables 1 to 3.

[0091] Rubber compositions No. 1 to 9 contain isoprene rubber (diene rubber) as the base rubber, petroleum resin, and sulfur as a crosslinking agent. Rubber composition No. 10 contains isoprene rubber (diene rubber) and sulfur, but does not contain petroleum resin. The sheet conveying rollers formed from rubber compositions No. 1 to 9 had improved friction coefficients compared to the sheet conveying roller formed from rubber composition No. 10, which does not contain petroleum resin.

[0092] Rubber compositions No. 11 to 19 contain isoprene rubber (diene rubber) as the base rubber, petroleum resin, and organic peroxide as a crosslinking agent. Rubber composition No. 20 contains isoprene rubber (diene rubber) and organic peroxide, but does not contain petroleum resin. The sheet conveying rollers formed from rubber compositions No. 11 to 19 had improved friction coefficients compared to the sheet conveying roller formed from rubber composition No. 20, which does not contain petroleum resin.

[0093] Rubber compositions No. 21 to No. 23 contain natural rubber (diene rubber) as the base rubber, petroleum resin, and sulfur as a crosslinking agent. Rubber composition No. 24 contains natural rubber (diene rubber), sulfur as a crosslinking agent, and does not contain petroleum resin. The sheet conveying rollers formed from rubber compositions No. 21 to No. 23 had improved friction coefficients compared to the sheet conveying roller formed from rubber composition No. 24, which does not contain petroleum resin.

[0094] Rubber compositions No. 25 to 28 contain isoprene rubber (diene rubber) and EPDM as base rubber, petroleum resin, and organic peroxide as crosslinking agent, and the content of diene rubber in the base rubber is 50 mass% or more. Rubber composition No. 29 contains isoprene rubber (diene rubber) and EPDM as base rubber, and organic peroxide as crosslinking agent, but does not contain petroleum resin. The sheet conveying rollers formed from rubber compositions No. 25 to 28 had improved friction coefficients compared to the sheet conveying roller formed from rubber composition No. 29, which does not contain petroleum resin.

[0095] Rubber compositions No. 30 and 31 contain isoprene rubber (diene rubber), styrene butadiene rubber (diene rubber), and EPDM as base rubber, petroleum resin, and organic peroxide as a crosslinking agent, and the content of diene rubber in the base rubber is 50 mass% or more. Rubber composition No. 32 contains isoprene rubber (diene rubber), styrene butadiene rubber (diene rubber), EPDM, and organic peroxide, but does not contain petroleum resin. The sheet conveying rollers formed from rubber compositions No. 30 and 31 had improved friction coefficients compared to the sheet conveying roller formed from rubber composition No. 32, which does not contain petroleum resin.

[0096] The present invention (1) is a rubber composition for a sheet-conveying roller, comprising a base rubber and a petroleum resin, the base rubber containing a diene-based rubber, and a content of the diene-based rubber in 100% by mass of the base rubber being 50% by mass or more.

[0097] The present invention (2) relates to the rubber composition for sheet conveying rollers according to the present invention (1), wherein the petroleum resin is one or more petroleum resins selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, aliphatic-aromatic copolymer petroleum resins, dicyclopentadiene petroleum resins, aliphatic-dicyclopentadiene copolymer petroleum resins, aromatic-dicyclopentadiene copolymer petroleum resins, aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aliphatic petroleum resins, hydrogenated aromatic petroleum resins, hydrogenated aliphatic-aromatic copolymer petroleum resins, hydrogenated dicyclopentadiene petroleum resins, hydrogenated aliphatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aromatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins, and styrene-based resins.

[0098] The present invention (3) relates to the rubber composition for a sheet-conveying roller according to the present invention (1) or (2), wherein the diene rubber contains isoprene rubber and / or natural rubber.

[0099] The present invention (4) is the rubber composition for a sheet-conveying roller according to any one of the present inventions (1) to (3), wherein the content of the petroleum resin is 1 part by mass to 15 parts by mass per 100 parts by mass of the base rubber.

[0100] The present invention (5) is a rubber composition for a sheet-conveying roller according to any one of the present inventions (1) to (4), wherein the base rubber further contains an ethylene-α-olefin copolymer and / or an ethylene-vinyl acetate copolymer.

[0101] The present invention (6) is the rubber composition for a sheet-conveying roller according to any one of the present inventions (1) to (5), in which the sheet is a paper sheet.

[0102] The present invention (7) is a sheet-conveying roller characterized by being molded from the rubber composition for a sheet-conveying roller according to any one of the present inventions (1) to (6).

[0103] The present invention (8) is a method for producing a rubber composition for a sheet-conveying roller, which contains a base rubber and a petroleum resin, and is characterized in that the base rubber containing 50 mass % or more of a diene rubber and the petroleum resin are kneaded at a temperature equal to or higher than the softening point of the petroleum resin.

[0104] The present invention (9) is a method for producing a rubber composition for a sheet conveying roller, which contains a base rubber, a petroleum resin, and a crosslinking agent, and is characterized in that the method includes a first step of kneading a base rubber containing 50 mass % or more of a diene rubber and the petroleum resin at a temperature equal to or higher than the softening point of the petroleum resin to obtain a kneaded mixture, and a second step of mixing a crosslinking agent with the kneaded mixture. [Explanation of symbols]

[0105] 1: sheet transport roller, 2: roller body, 3: through hole, 4: shaft, 10: plate, 11: paper, 12: load cell

Claims

1. Contains base rubber and petroleum resin, the base rubber contains a diene rubber, A rubber composition for a sheet-conveying roller, comprising: a base rubber having a diene rubber content of 50% by mass or more based on 100% by mass of the base rubber.

2. The rubber composition for sheet conveying rollers according to claim 1, wherein the petroleum resin is one or more petroleum resins selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, aliphatic-aromatic copolymer petroleum resins, dicyclopentadiene petroleum resins, aliphatic-dicyclopentadiene copolymer petroleum resins, aromatic-dicyclopentadiene copolymer petroleum resins, aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aliphatic petroleum resins, hydrogenated aromatic petroleum resins, hydrogenated aliphatic-aromatic copolymer petroleum resins, hydrogenated dicyclopentadiene petroleum resins, hydrogenated aliphatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aromatic-dicyclopentadiene copolymer petroleum resins, hydrogenated aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins, and styrene-based resins.

3. 3. The rubber composition for a sheet-conveying roller according to claim 1, wherein the diene rubber contains isoprene rubber and / or natural rubber.

4. 3. The rubber composition for a sheet-conveying roller according to claim 1, wherein the content of the petroleum resin is 1 to 15 parts by mass per 100 parts by mass of the base rubber.

5. 3. The rubber composition for a sheet-conveying roller according to claim 1, wherein the base rubber further contains an ethylene-α-olefin copolymer and / or an ethylene-vinyl acetate copolymer.

6. The rubber composition for a sheet-conveying roller according to claim 1 or 2, wherein the sheet is a paper sheet.

7. A sheet conveying roller, which is molded from the rubber composition for a sheet conveying roller according to claim 1 or 2.

8. A method for producing a rubber composition for a sheet-conveying roller, comprising: A method for producing a rubber composition for a sheet-conveying roller, comprising kneading a base rubber containing 50% by mass or more of a diene rubber and the petroleum resin at a temperature equal to or higher than the softening point of the petroleum resin.

9. A method for producing a rubber composition for a sheet-conveying roller, comprising: A first step of kneading a base rubber containing 50% by mass or more of a diene rubber with the petroleum resin at a temperature equal to or higher than the softening point of the petroleum resin to obtain a kneaded mixture; and a second step of mixing the kneaded mixture with a crosslinking agent.

Citation Information

Patent Citations

  • Composition for elastomer crosslinked foam

    JP1993214142A

  • Rubber composition

    JP1995330989A

  • Low hardness rubber composition, paper-feeding member and paper-feeding device

    JP1998195246A

  • Rubber composition for conveyer belt and conveyer belt

    JP2009215339A

  • Tire for winter

    JP2017203111A