bolt
A bolt with a specific chemical composition and microstructure, featuring a high number density of MC type carbides, addresses the susceptibility to hydrogen embrittlement in high-strength bolts, ensuring both high tensile strength and improved embrittlement resistance.
Patent Information
- Application Number
- JP2023073936
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Bolts with high tensile strength of 1000 MPa or more are susceptible to hydrogen embrittlement, and existing solutions do not adequately address this issue.
A bolt with a specific chemical composition and microstructure that includes a high number density of MC type carbides, controlled by the ratio of Mo and Ti or Mo and V contents, enhances hydrogen embrittlement resistance.
The bolt achieves high tensile strength of 1000 MPa or more while maintaining excellent hydrogen embrittlement resistance, with a critical hydrogen amount of 1.5 mass ppm or more.
Smart Images

Figure 2024158601000004 
Figure 2024158601000001 
Figure 2024158601000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a bolt. [Background technology]
[0002] Bolts are used in industrial machinery, automobiles, buildings such as bridges, etc. In recent years, with the increasing performance of industrial machinery and automobiles and the increasing size of buildings, etc., there is a demand for bolts with higher strength. Specifically, there is a demand for bolts with a tensile strength of 1000 MPa or more.
[0003] Bolts having such high strength have high susceptibility to hydrogen embrittlement, so high strength bolts are required to have excellent hydrogen embrittlement resistance.
[0004] JP 2019-218584 A (Patent Document 1), WO 2017 / 094487 A (Patent Document 2), and JP 2013-163865 A (Patent Document 3) propose bolts having high strength and excellent resistance to hydrogen embrittlement.
[0005] The bolt disclosed in Patent Document 1 contains, in mass%, C: 0.22 to 0.40%, Si: 0.10 to 1.50%, Mn: 0.20 to less than 0.40%, Cr: 0.70 to less than 1.60%, Al: 0.005 to 0.060%, Ti: 0.010 to 0.050%, B: 0.0003 to 0.0040%, N: 0.0015 to 0.0080%, Cu: 0.50% or less, Ni: 0.30% or less, M The bolt contains O: 0.05% or less, V: 0.050% or less, Nb: 0.050% or less, and one or more selected from the group consisting of Sb: 0.001-0.100%, Sn: 0.001-0.100%, and Bi: 0.001-0.100%, and further contains O: 0.0020% or less, P: 0.020% or less, S: 0.020% or less, with the balance being Fe and impurities. The bolt further satisfies formula (1) (0.50≦C+(1 / 10)×Si+(1 / 5)×Mn+(5 / 22)×Cr≦0.85) and formula (2) (0.003≦Sb+Sn+Bi≦0.100). Patent Document 1 describes that in this bolt, the contents of Sb, Sn, and Bi in the chemical composition satisfy formula (2), so that excellent hydrogen embrittlement resistance can be obtained even with high strength.
[0006] The bolt disclosed in Patent Document 2 contains, by mass%, C: 0.22 to 0.40%, Si: 0.10 to 1.50%, Mn: 0.20 to less than 0.40%, P: 0.020% or less, S: 0.020% or less, Cr: 0.70 to 1.45%, Al: 0.005 to 0.060%, Ti: 0.010 to 0.045%, B: 0.0003 to 0.0040%, N: 0.0015 to 0.0080%, O: 0.0020% or less, Cu: 0 to 0.50%, Ni: 0 to 0.30%, Mo: 0 to 0.04%, V: 0 to 0.05%, and Nb: 0 to 0.050%, with the balance being Fe and impurities. The bolt further satisfies formula (1) (0.50≦C+Si / 10+Mn / 5+5Cr / 22≦0.85) and formula (2) (Si / Mn>1.0). Patent Document 2 describes that this bolt has excellent hydrogen embrittlement resistance because the Si and Mn contents in the chemical composition satisfy formula (2).
[0007] The bolt disclosed in Patent Document 3 contains, by mass%, C: 0.30 to 0.50%, Si: 1.0 to 2.5%, Mn: 0.1 to 1.5%, P: 0.015% or less (excluding 0%), S: 0.015% or less (excluding 0%), Cr: 0.15 to 2.4%, Al: 0.10% or less (excluding 0%), and N: 0.015% or less (excluding 0%), and further contains Cu: 0.10 to 0.50% and Ni: 0.1 to 1.0% so as to satisfy [Ni] / [Cu]≧0.5, further contains Ti: 0.05 to 0.20% and V: 0.20% or less (including 0%) so as to satisfy [Ti]+[V]: 0.085 to 0.30%, with the remainder being Fe and impurities. Furthermore, the austenite grain size number of the bolt shank is 9.0 or more, and the G value (%), which indicates the proportion of carbides precipitated at the austenite grain boundaries in the bolt shank, satisfies formula (1) (G value = (L / L0) × 100 ≦ 60). Note that in formula (1), L is the total length of carbides with a thickness of 50 nm or more precipitated at the austenite grain boundaries, and L0 is the length of the austenite grain boundaries. Patent Document 3 describes that this bolt has excellent hydrogen embrittlement resistance by suppressing carbide precipitation at grain boundaries. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2019-218584 A [Patent Document 2] International Publication No. 2017 / 094487 [Patent Document 3] JP 2013-163865 A Summary of the Invention [Problem to be solved by the invention]
[0009] High strength and excellent hydrogen embrittlement resistance are obtained in the bolts disclosed in Patent Documents 1 to 3. However, high strength and excellent hydrogen embrittlement resistance may be obtained by a means different from those disclosed in Patent Documents 1 to 3.
[0010] An object of the present disclosure is to provide a bolt that has high strength and excellent resistance to hydrogen embrittlement. [Means for solving the problem]
[0011] The bolt according to the present disclosure comprises: Chemical composition, in mass%, C: 0.10-0.50%, Si: 0.01 to 0.30%, Mn: 0.10-2.50%, P:0.030% or less, S: 0.030% or less, Cr: 0.01 to 0.80%, Mo: 0.70-2.00%, Al: 0.005 to 0.100%, N: 0.0010~0.0300%, Ti: 0.001 to 0.300%, and The balance is Fe and impurities. Satisfies formula (1A), The tensile strength TS is 1000 MPa or more, The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all. Mo / 2Ti>4.25 (1A) Here, each element symbol in formula (1A) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass %.
[0012] The bolt according to the present disclosure comprises: Chemical composition, in mass%, C: 0.10-0.50%, Si: 0.01 to 0.30%, Mn: 0.10-2.50%, P:0.030% or less, S: 0.030% or less, Cr: 0.01 to 0.80%, Mo: 0.70-2.00%, Al: 0.005 to 0.100%, N: 0.0010 to 0.0300%, and Ti: 0.001 to 0.300%; Further, it contains one or more selected from the group consisting of Groups 1 to 3, The balance is Fe and impurities. Satisfying formula (1), The tensile strength TS is 1000 MPa or more, The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all. Mo / (2Ti+V)>4.25 (1) Here, each element symbol in formula (1) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass %. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, B: 0.0100% or less, Zr: 0.300% or less, Hf: 0.100% or less, Ta: 0.100% or less, and W: 0.20% or less, one or more selected from the group consisting of [Group 2] V: 0.50% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.0050% or less, Bi: 0.020% or less, and Te: 0.010% or less, one or more selected from the group consisting of Effect of the Invention
[0013] The bolts according to the present disclosure have high strength and excellent resistance to hydrogen embrittlement. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a side view showing an example of a bolt according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventors have investigated bolts that have high strength and excellent hydrogen embrittlement resistance, and as a result, have made the following discoveries.
[0016] First, the inventors of the present invention have investigated a bolt having high strength and excellent hydrogen embrittlement resistance from the viewpoint of chemical composition. As a result, the inventors of the present invention have found that the bolt has a composition of, in mass%, C: 0.10-0.50%, Si: 0.01-0.30%, Mn: 0.10-2.50%, P: 0.030% or less, S: 0.030% or less, Cr: 0.01-0.80%, Mo: 0.70-2.00%, Al: 0.005-0.100%, N: 0.0010-0.0300%, Ti: 0.001-0.300%, Cu: 0-0.40%, Ni: 0-0.40%, B: 0-0.0 It was considered that a bolt having a chemical composition of 100%, Zr: 0~0.300%, Hf: 0~0.100%, Ta: 0~0.100%, W: 0~0.20%, V: 0~0.50%, Nb: 0~0.100%, Ca: 0~0.0050%, Bi: 0~0.020%, Te: 0~0.010%, and the remainder being Fe and impurities could potentially achieve a tensile strength TS of 1000 MPa or more and excellent hydrogen embrittlement resistance.
[0017] Therefore, the inventors further investigated means for improving the strength and hydrogen embrittlement resistance from the viewpoint of the microstructure of the bolt having the above-mentioned chemical composition. As a result, the inventors discovered that it is possible to improve the hydrogen embrittlement resistance of a bolt having a tensile strength TS of 1000 MPa or more by dispersing a large number of fine precipitates in the bolt.
[0018] The inventors further considered that the type of alloy carbide affects the hydrogen embrittlement resistance of the bolt. Therefore, further investigation was conducted. Here, the inventors focused on MC type carbides among alloy carbides. MC type carbides are less likely to coarsen and tend to remain fine compared to other alloy carbides (e.g., M2C type carbides, cementite, etc.). Fine precipitates become hydrogen trapping sites and absorb hydrogen. Therefore, the amount of hydrogen that can be stored before hydrogen embrittlement cracking occurs (hereinafter, referred to as the limit hydrogen amount) can be increased. Therefore, if the number density ND of the MC type carbides in the bolt is increased, the hydrogen embrittlement resistance of the bolt may be increased.
[0019] Therefore, the inventors investigated the relationship between the number density ND of MC type carbides and the limiting hydrogen content in a bolt having the above-mentioned chemical composition. As a result, it was found that the number density ND of MC type carbides was 2.0×10 21 pieces / m 3 It was found that if this is the case, even for bolts with a tensile strength TS of 1000 MPa or more, a sufficient limiting hydrogen content can be obtained, and as a result, excellent hydrogen embrittlement resistance can be obtained.
[0020] However, the number density of MC type carbides, N D , is 2.0×10 21 pieces / m 3 Even for bolts with a tensile strength of 1000 MPa or more, sufficient hydrogen embrittlement resistance was still not obtained in some cases.
[0021] Therefore, the inventors conducted further studies. Here, the inventors investigated factors that affect the hydrogen absorption action other than the number density ND of the MC type carbides. Specifically, MC type carbides may have sites (C vacancies) where C is not present in the places where C should be. MC type carbides having C vacancies trap hydrogen in the C vacancies. Therefore, the hydrogen absorption action is enhanced. Therefore, the inventors considered that in order to improve the hydrogen embrittlement resistance of the bolt, it is effective not only to increase the number density ND of the MC type carbides but also to increase the C vacancy rate of the MC type carbides.
[0022] Therefore, the present inventors have investigated means for increasing the C vacancy rate of MC type carbides. As a result, they have found that Mo, Ti and V are elements that increase the C vacancy rate of MC type carbides. The present inventors then considered that the C vacancy rate of MC type carbides could be increased by appropriately controlling the Mo content, Ti content and V content. Therefore, the present inventors have investigated the relationship between the Mo content, Ti content and V content and the limiting hydrogen amount. As a result, they have found that the number density ND of MC type carbides having the above-mentioned chemical composition is 2.0×10 21 pieces / m 3 The inventors have discovered that for a bolt satisfying the above criteria, by further satisfying the following formula (1), a sufficient limiting hydrogen amount can be obtained and excellent hydrogen embrittlement resistance can be obtained, even for a bolt having a tensile strength TS of 1000 MPa or more. Mo / (2Ti+V)>4.25 (1) Here, the content of the corresponding element in the chemical composition of the bolt is substituted for each element symbol in formula (1) in mass percent. If V is not included, formula (1) is expressed as formula (1A) as follows. Mo / 2Ti>4.25 (1A)
[0023] The above-mentioned mechanism is a conjecture, and it is possible that the limit hydrogen amount is increased by a different mechanism. However, when the content of each element in the chemical composition is within the range of this embodiment, the above-mentioned formula (1) is satisfied, the tensile strength TS is 1000 MPa or more, and the number density ND of the MC type carbides is 2.0 × 10 21 pieces / m 3 If the amount is more than this, the limit hydrogen amount increases, as will be demonstrated in the examples described later.
[0024] The bolt of this embodiment has been completed based on the above findings and has the following configuration.
[0025] [1] Chemical composition, in mass%, C: 0.10-0.50%, Si: 0.01 to 0.30%, Mn: 0.10-2.50%, P:0.030% or less, S: 0.030% or less, Cr: 0.01 to 0.80%, Mo: 0.70-2.00%, Al: 0.005 to 0.100%, N: 0.0010~0.0300%, Ti: 0.001 to 0.300%, and The balance is Fe and impurities. Satisfies formula (1A), The tensile strength TS is 1000 MPa or more, The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all. bolt. Mo / 2Ti>4.25 (1A) Here, each element symbol in formula (1A) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass %.
[0026] [2] Chemical composition, in mass%, C: 0.10-0.50%, Si: 0.01 to 0.30%, Mn: 0.10-2.50%, P:0.030% or less, S: 0.030% or less, Cr: 0.01 to 0.80%, Mo: 0.70-2.00%, Al: 0.005 to 0.100%, N: 0.0010 to 0.0300%, and Ti: 0.001 to 0.300%; Further, it contains one or more selected from the group consisting of Groups 1 to 3, The balance is Fe and impurities. Satisfying formula (1), The tensile strength TS is 1000 MPa or more, The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all. bolt. Mo / (2Ti+V)>4.25 (1) Here, each element symbol in formula (1) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass %. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, B: 0.0100% or less, Zr: 0.300% or less, Hf: 0.100% or less, Ta: 0.100% or less, and W: 0.20% or less, one or more selected from the group consisting of [Group 2] V: 0.50% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.0050% or less, Bi: 0.020% or less, and Te: 0.010% or less, one or more selected from the group consisting of
[0027] [3] [2] A bolt according to the present invention, The chemical composition contains the first group, bolt.
[0028] [4] A bolt according to [2] or [3], The chemical composition contains the second group, bolt.
[0029] [5] A bolt according to any one of [2] to [4], The chemical composition contains the third group, bolt.
[0030] The bolt according to this embodiment will be described in detail below. Note that "%" for elements means mass % unless otherwise specified.
[0031] Bolt Configuration The shape of the bolt of this embodiment has a well-known structure. Fig. 1 is a side view showing an example of the bolt of this embodiment. Referring to Fig. 1, the bolt of this embodiment includes a head 10, a neck portion 11, and a shank portion 12. The neck portion 11 is a portion that connects the head 10 and the shank portion 12, and has a curved surface. In other words, the surface of the neck portion 11 has a curvature. The shank portion 12 extends from the neck portion 11 in the direction of the central axis of the bolt. The shank portion 12 has a thread formed on at least a portion of its peripheral surface.
[0032] [Features of the bolt of this embodiment] The bolt of this embodiment satisfies the following features 1 to 4. (Feature 1) The chemical composition, in mass%, is C: 0.10-0.50%, Si: 0.01-0.30%, Mn: 0.10-2.50%, P: 0.030% or less, S: 0.030% or less, Cr: 0.01-0.80%, Mo: 0.70-2.00%, Al: 0.005-0.100%, N: 0.0010-0.0300%, Ti: 0.001-0.300%, Cu: The alloy consists of the following components: 0-0.40%, Ni: 0-0.40%, B: 0-0.0100%, Zr: 0-0.300%, Hf: 0-0.100%, Ta: 0-0.100%, W: 0-0.20%, V: 0-0.50%, Nb: 0-0.100%, Ca: 0-0.0050%, Bi: 0-0.020%, Te: 0-0.010%, and the remainder is Fe and impurities. (Feature 2) The chemical composition of feature 1 further satisfies formula (1). Mo / (2Ti+V)>4.25 (1) Here, each element symbol in formula (1) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass percent. If the corresponding element is not contained, "0" is substituted for that element symbol. (Feature 3) The tensile strength TS is 1000 MPa or more. (Feature 4) The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all.
[0033] The bolt according to this embodiment satisfies the above-mentioned features 1 to 4. Therefore, the bolt according to this embodiment has high strength and excellent hydrogen embrittlement resistance. Features 1 to 4 will be described below.
[0034] [(Feature 1) Chemical composition] The chemical composition of the bolt of this embodiment contains the following elements.
[0035] C: 0.10-0.50% Carbon (C) improves the hardenability of steel material and increases the strength of the bolt. If the C content is less than 0.10%, the above effect cannot be sufficiently obtained. On the other hand, if the C content exceeds 0.50%, the hydrogen embrittlement resistance of the bolt decreases. Therefore, the C content is 0.10 to 0.50%. The lower limit of the C content is preferably 0.12%, more preferably 0.15%, and further preferably 0.18%. The upper limit of the C content is preferably 0.48%, more preferably 0.45%, and further preferably 0.43%.
[0036] Silicon: 0.01 to 0.30% Silicon (Si) improves the hardenability of steel material and increases the strength of the bolt. If the Si content is less than 0.01%, the above effect cannot be sufficiently obtained. On the other hand, if the Si content exceeds 0.30%, the hydrogen embrittlement resistance of the bolt decreases. Therefore, the Si content is 0.01 to 0.30%. The lower limit of the Si content is preferably 0.02%, more preferably 0.03%, and further preferably 0.05%. The upper limit of the Si content is preferably 0.25%, more preferably 0.20%, and further preferably 0.15%.
[0037] Mn: 0.10 to 2.50% Manganese (Mn) improves the hardenability of steel and increases the strength of the bolt. If the Mn content is less than 0.10%, the above effect cannot be sufficiently obtained. On the other hand, if the Mn content exceeds 2.50%, the hydrogen embrittlement resistance of the bolt decreases. Therefore, the Mn content is 0.10 to 2.50%. The lower limit of the Mn content is preferably 0.15%, more preferably 0.20%, and further preferably 0.25%. The upper limit of the Mn content is preferably 2.30%, more preferably 2.20%, and further preferably 2.10%.
[0038] P:0.030% or less Phosphorus (P) is an impurity. If the P content exceeds 0.030%, P segregates at grain boundaries. As a result, the hydrogen embrittlement resistance of the bolt decreases. Therefore, the P content is 0.030% or less. It is preferable that the P content is as low as possible. However, an extreme reduction in the P content significantly increases the production cost. Therefore, in consideration of industrial production, the preferable lower limit of the P content is more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%. The upper limit of the P content is preferably 0.025%, more preferably 0.023%, and further preferably 0.020%.
[0039] S: 0.030% or less Sulfur (S) is an impurity. If the S content exceeds 0.030%, S will segregate at grain boundaries. As a result, the hydrogen embrittlement resistance of the bolt will decrease. Therefore, the S content should be 0.030% or less. The S content is preferably as low as possible. However, an extreme reduction in the S content significantly increases the production cost. Therefore, in consideration of industrial production, the preferred lower limit of the S content is more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%. The upper limit of the S content is preferably 0.025%, more preferably 0.023%, and further preferably 0.020%.
[0040] Cr: 0.01~0.80% Chromium (Cr) improves the hardenability of steel material and increases the strength of the bolt. Cr also improves the temper softening resistance of the steel material and increases the strength of the bolt. If the Cr content is less than 0.01%, the above effects cannot be sufficiently obtained. On the other hand, if the Cr content exceeds 0.80%, the hydrogen embrittlement resistance of the bolt decreases. Therefore, the Cr content is 0.01 to 0.80%. The lower limit of the Cr content is preferably 0.03%, more preferably 0.05%, and further preferably 0.08%. The upper limit of the Cr content is preferably 0.70%, more preferably 0.60%, and further preferably 0.50%.
[0041] Mo: 0.70-2.00% Molybdenum (Mo) increases the temper softening resistance of steel material and increases the strength of bolts. Mo is further concentrated in MC type carbides and enhances the hydrogen trapping function of MC type carbides. As a result, the hydrogen embrittlement resistance of high strength bolts is improved. If the Mo content is less than 0.70%, the above effect cannot be sufficiently obtained. On the other hand, if the Mo content exceeds 2.00%, the hardness of the steel material becomes excessively high. As a result, the cold workability is reduced. Therefore, the Mo content is 0.70 to 2.00%. The lower limit of the Mo content is preferably 0.75%, more preferably 0.80% or 0.85%. The upper limit of the Mo content is preferably 1.90%, more preferably 1.70%, and further preferably 1.50%.
[0042] Al: 0.005 to 0.100% Aluminum (Al) deoxidizes steel. Furthermore, Al bonds with N to form Al nitrides. Al nitrides suppress grain coarsening through a pinning effect. As a result, hydrogen embrittlement resistance of the bolt is improved. If the Al content is less than 0.005%, the above effect cannot be sufficiently obtained. On the other hand, if the Al content exceeds 0.100%, coarse Al nitrides are formed. The coarse Al nitrides become the starting point of fracture. As a result, the workability of the steel material decreases. Therefore, the Al content is 0.005 to 0.100%. The lower limit of the Al content is preferably 0.006%, more preferably 0.007%, and further preferably 0.008%. The upper limit of the Al content is preferably 0.090%, more preferably 0.080%, and further preferably 0.070%. In the chemical composition of the steel material of this embodiment, the Al content means the total Al content.
[0043] N: 0.0010~0.0300% Nitrogen (N) combines with Al to form Al nitrides. Al nitrides suppress the coarsening of crystal grains through a pinning effect. As a result, the hydrogen embrittlement resistance of the bolt is improved. If the N content is less than 0.0010%, the above effect is not sufficiently obtained. On the other hand, if the N content exceeds 0.0300%, coarse nitrides are formed. The coarse nitrides become the starting point of fracture. As a result, the workability of the steel material decreases. Therefore, the N content is 0.0010 to 0.0300%. The lower limit of the N content is preferably 0.0020%, more preferably 0.0025%, and further preferably 0.0030%. The upper limit of the N content is preferably 0.0290%, more preferably 0.0280%, more preferably 0.0270%, more preferably 0.0250%, more preferably 0.0200%, more preferably 0.0150%, and more preferably 0.0100%.
[0044] Ti: 0.001 to 0.300% Titanium (Ti) forms MC type carbides together with Mo to enhance the hydrogen embrittlement resistance of the bolt. If the Ti content is less than 0.001%, the above effect is not sufficiently obtained. On the other hand, if the Ti content exceeds 0.300%, coarse Ti nitrides are generated. The coarse Ti nitrides become the starting points of fracture. As a result, the cold workability of the steel material is reduced. Therefore, the Ti content is 0.001 to 0.300%. The lower limit of the Ti content is preferably 0.002%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the Ti content is preferably 0.250%, more preferably 0.200%, and further preferably 0.150%.
[0045] The balance of the chemical composition of the bolt according to the present embodiment is composed of Fe and impurities. Here, the impurities in the chemical composition refer to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the bolt, and are not intentionally contained, but are allowed within a range that does not adversely affect the bolt according to the present embodiment.
[0046] [Optional Elements] The chemical composition of the bolt of this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Groups 1 to 3. All of these elements are optional elements and may not be contained. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, B: 0.0100% or less, Zr: 0.300% or less, Hf: 0.100% or less, Ta: 0.100% or less, and W: 0.20% or less, one or more selected from the group consisting of [Group 2] V: 0.50% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.0050% or less, Bi: 0.020% or less, and Te: 0.010% or less, one or more selected from the group consisting of These optional elements will now be described.
[0047] [Group 1 (Cu, Ni, B, Zr, Hf, Ta and W)] The chemical composition of the bolt according to this embodiment may further contain the above-mentioned elements of Group 1 in place of a portion of Fe. These elements are optional elements, and all of them improve the hardenability of the steel material and increase the strength of the bolt.
[0048] Cu: 0.40% or less Copper (Cu) is an optional element and may not be contained. In other words, the Cu content may be 0%. When Cu is contained, that is, when the Cu content is more than 0%, Cu increases the hardenability of the steel material and increases the strength of the bolt. Even if even a small amount of Cu is contained, the above effect can be obtained to a certain extent. However, when the Cu content exceeds 0.40%, the hardenability becomes too high. As a result, the workability of the steel material decreases. Therefore, the Cu content is 0 to 0.40%, and when contained, the Cu content is 0.40% or less. The lower limit of the Cu content is preferably 0.01%, more preferably 0.03%, and further preferably 0.05%. The upper limit of the Cu content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.
[0049] Ni: 0.40% or less Nickel (Ni) is an optional element and may not be contained. In other words, the Ni content may be 0%. When Ni is contained, that is, when the Ni content is more than 0%, Ni increases the hardenability of the steel material and increases the strength of the bolt. If even a small amount of Ni is contained, the above effect can be obtained to a certain extent. However, when the Ni content exceeds 0.40%, the hardenability becomes too high. As a result, the workability of the steel material decreases. Therefore, the Ni content is 0 to 0.40%, and when contained, the Ni content is 0.40% or less. The lower limit of the Ni content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the Ni content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.
[0050] B: 0.0100% or less Boron (B) is an optional element and may not be contained. In other words, the B content may be 0%. When B is contained, that is, when the B content is more than 0%, B increases the hardenability of the steel material and increases the strength of the bolt. B further suppresses the grain boundary segregation of P and increases the hydrogen embrittlement resistance of the bolt. If even a small amount of B is contained, the above effects can be obtained to a certain extent. However, if the B content exceeds 0.0100%, coarse B nitrides are generated. The coarse B nitrides become the starting points of fracture. As a result, the workability of the steel material decreases. Therefore, the B content is 0 to 0.0100%, and if contained, the B content is 0.0100% or less. The lower limit of the B content is preferably 0.0001%, more preferably 0.0005%, and further preferably 0.0008%. The upper limit of the B content is preferably 0.0090%, more preferably 0.0080%, more preferably 0.0070%, more preferably 0.0060%, and even more preferably 0.0050%.
[0051] Zr: 0.300% or less Zirconium (Zr) is an optional element and may not be contained. In other words, the Zr content may be 0%. When Zr is contained, that is, when the Zr content is more than 0%, Zr increases the hardenability of the steel material and increases the strength of the bolt. If even a small amount of Zr is contained, the above effects can be obtained to a certain extent. However, if the Zr content exceeds 0.300%, coarse Zr nitrides are generated. The coarse Zr nitrides become the starting points of fracture. As a result, the workability of the steel material decreases. Therefore, the Zr content is 0 to 0.300%, and when contained, the Zr content is 0.300% or less. The lower limit of the Zr content is preferably 0.001%, more preferably 0.010%, and further preferably 0.020%. The upper limit of the Zr content is preferably 0.280%, more preferably 0.250%, more preferably 0.200%, more preferably 0.150%, and even more preferably 0.100%.
[0052] Hf:0.100% or less Hafnium (Hf) is an optional element and may not be contained. In other words, the Hf content may be 0%. When Hf is contained, that is, when the Hf content is more than 0%, Hf increases the hardenability of the steel material and increases the strength of the bolt. If even a small amount of Hf is contained, the above effects can be obtained to a certain extent. However, when the Hf content exceeds 0.100%, coarse Hf nitrides are generated. The coarse Hf nitrides become the starting points of fracture. As a result, the workability of the steel material decreases. Therefore, the Hf content is 0 to 0.100%, and when contained, the Hf content is 0.100% or less. The lower limit of the Hf content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the Hf content is preferably 0.080%, more preferably 0.070%, further preferably 0.060%, and further preferably 0.050%.
[0053] Ta:0.100% or less Tantalum (Ta) is an optional element and may not be contained. In other words, the Ta content may be 0%. When Ta is contained, that is, when the Ta content is more than 0%, Ta increases the hardenability of the steel material and increases the strength of the bolt. If even a small amount of Ta is contained, the above effects can be obtained to a certain extent. However, when the Ta content exceeds 0.100%, coarse Ta nitrides are generated. The coarse Ta nitrides become the starting points of fracture. As a result, the workability of the steel material decreases. Therefore, the Ta content is 0 to 0.100%, and when contained, the Ta content is 0.100% or less. The lower limit of the Ta content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the Ta content is preferably 0.080%, more preferably 0.070%, further preferably 0.060%, and further preferably 0.050%.
[0054] W: 0.20% or less Tungsten (W) is an optional element and may not be contained. In other words, the W content may be 0%. When W is contained, that is, when the W content is more than 0%, W increases the hardenability of the steel material and increases the strength of the bolt. If even a small amount of W is contained, the above effect can be obtained to a certain extent. However, when the W content exceeds 0.20%, the hardenability becomes too high. As a result, the workability of the steel material decreases. Therefore, the W content is 0 to 0.20%, and when contained, the W content is 0.20% or less. The lower limit of the W content is preferably 0.01%, more preferably 0.02%, and further preferably 0.05%. The upper limit of the W content is preferably 0.15%, more preferably 0.12%, and further preferably 0.10%.
[0055] [Group 2 (V and Nb)] The chemical composition of the bolt according to this embodiment may further contain the above-mentioned elements of Group 2 in place of a portion of Fe. These elements are optional elements, and all of them improve the hydrogen embrittlement resistance of the bolt.
[0056] V: 0.50% or less Vanadium (V) is an optional element and may not be contained. In other words, the V content may be 0%. When V is contained, that is, when the V content is more than 0%, V forms MC type carbides together with Mo to enhance the hydrogen embrittlement resistance of the bolt. If even a small amount of V is contained, the above effect can be obtained to some extent. However, if the V content exceeds 0.50%, the steel material becomes excessively hard. As a result, the cold workability is reduced. Therefore, the V content is 0 to 0.50%, and when contained, the V content is 0.50% or less. The lower limit of the V content is preferably 0.01%, more preferably 0.03%, and further preferably 0.05%. The upper limit of the V content is preferably 0.45%, more preferably 0.40%, and further preferably 0.35%.
[0057] Nb: 0.100% or less Niobium (Nb) is an optional element and may not be contained. In other words, the Nb content may be 0%. When Nb is contained, that is, when the Nb content is more than 0%, Nb forms fine precipitates such as Nb carbides and refines the crystal grains. As a result, the hydrogen embrittlement resistance of the bolt is improved. If even a small amount of Nb is contained, the above effect can be obtained to a certain extent. However, if the Nb content exceeds 0.100%, coarse Nb carbides and the like are generated. The coarse Nb carbides and the like become the starting point of fracture. As a result, the workability of the steel material is reduced. Therefore, the Nb content is 0 to 0.100%, and when contained, the Nb content is 0.100% or less. The lower limit of the Nb content is preferably 0.001%, more preferably 0.010%, and further preferably 0.020%. The upper limit of the Nb content is preferably 0.090%, more preferably 0.080%, and further preferably 0.070%.
[0058] [Group 3 (Ca, Bi and Te)] The chemical composition of the bolt according to this embodiment may further contain the above-mentioned elements of Group 3 in place of a portion of Fe. These elements are optional elements, and all of them improve the machinability of the steel material.
[0059] Ca:0.0050% or less Calcium (Ca) is an optional element and may not be contained. In other words, the Ca content may be 0%. When Ca is contained, that is, when Ca is more than 0%, Ca enhances the machinability of the steel material. Even if even a small amount of Ca is contained, the above effect can be obtained to some extent. However, when the Ca content exceeds 0.0050%, the workability of the steel material decreases. Therefore, the Ca content is 0 to 0.0050%, and when contained, the Ca content is 0.0050% or less. The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0002%, and further preferably 0.0005%. The upper limit of the Ca content is preferably 0.0040%, more preferably 0.0035%, and further preferably 0.0030%.
[0060] Bi:0.020% or less Bismuth (Bi) is an optional element and may not be contained. In other words, the Bi content may be 0%. When Bi is contained, that is, when Bi is more than 0%, Bi enhances the machinability of the steel material. Even if even a small amount of Bi is contained, the above effect can be obtained to some extent. However, when the Bi content exceeds 0.020%, the workability of the steel material decreases. Therefore, the Bi content is 0 to 0.020%, and when contained, the Bi content is 0.020% or less. The lower limit of the Bi content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the Bi content is preferably 0.018%, more preferably 0.015%, and further preferably 0.013%.
[0061] Te: 0.010% or less Tellurium (Te) is an optional element and may not be contained. In other words, the Te content may be 0%. When Te is contained, that is, when Te is more than 0%, Te enhances the machinability of the steel material. Even if even a small amount of Te is contained, the above effect can be obtained to some extent. However, when the Te content exceeds 0.010%, the workability of the steel material decreases. Therefore, the Te content is 0 to 0.010%, and when contained, the Te content is 0.010% or less. The lower limit of the Te content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%. The upper limit of the Te content is preferably 0.009%, more preferably 0.008%, and further preferably 0.007%.
[0062] [(Feature 2) Regarding formula (1)] The chemical composition of the bolt of this embodiment further satisfies formula (1). Mo / (2Ti+V)>4.25 (1) Here, the content of the corresponding element in the chemical composition of the bolt is substituted for each element symbol in formula (1) in mass percent. If V is not included, formula (1) is expressed as formula (1A) as follows. Mo / 2Ti>4.25 (1A)
[0063] It is defined as F1=Mo / (2Ti+V). When V is not contained, F1=Mo / 2Ti. F1 is an index of the C porosity of MC carbides. As described above, in a chemical composition that satisfies feature 1, the Mo content, Ti content, and V content affect the C porosity of MC carbides. Even if a bolt satisfies features 1, 3, and 4, if F1 is 4.25 or less, the C porosity of the MC carbides is not sufficiently increased. In this case, the hydrogen embrittlement resistance of the bolt decreases. If F1 exceeds 4.25, the C porosity of the MC carbides is sufficiently increased. As a result, the hydrogen embrittlement resistance of the bolt increases.
[0064] The lower limit of F1 is preferably 4.50, more preferably 4.75, and even more preferably 5.00. The upper limit of F1 is not particularly limited. However, when the content of each element in the chemical composition of the bolt is within the range of this embodiment, the upper limit of F1 is, for example, 300.00, for example, 200.00, for example, 100.00, for example, 50.00. The value of F1 shall be rounded off to two decimal places.
[0065] [Feature 3: Tensile strength TS] The bolt according to this embodiment has a tensile strength TS of 1000 MPa or more. The bolt according to this embodiment satisfies Features 1, 2, and 4. As a result, the bolt according to this embodiment has excellent hydrogen embrittlement resistance even when the tensile strength TS is 1000 MPa or more.
[0066] The lower limit of the tensile strength TS is preferably 1050 MPa, and more preferably 1100 MPa. The upper limit of the tensile strength TS is not particularly limited. The upper limit of the tensile strength TS of the bolt according to this embodiment is, for example, 1700 MPa, and for example, 1650 MPa.
[0067] [Method of measuring tensile strength TS] In this embodiment, the tensile strength TS can be determined by the following method. A tensile test is performed in air at room temperature (20±15°C) in accordance with JIS Z 2241:2022 to obtain the tensile strength TS (MPa). The tensile test specimen is taken so as to include the bolt shaft, and the central axis of the tensile test specimen is coaxial with the bolt shaft.
[0068] [(Feature 4) Number density of MC type carbides (ND)] In the bolt of this embodiment, the number density ND of the MC type carbide is further 2.0×10 21 pieces / m 3 That's all.
[0069] MC type carbides are finer than other alloy elements such as cementite and M2C type carbides. Therefore, MC type carbides are more likely to trap hydrogen than other alloy carbides. Therefore, in the bolt of this embodiment, the number density ND of the MC type carbides is increased to increase the limit hydrogen amount of the bolt.
[0070] The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 If the above conditions are met, excellent hydrogen embrittlement resistance can be obtained, provided that Features 1 to 3 are satisfied.
[0071] The preferred lower limit of the number density ND of MC type carbides is 4.0×10 21 pieces / m 3 and more preferably 6.0×10 21 pieces / m 3 and more preferably 8.0×10 21 pieces / m 3 It is. The upper limit of the number density ND of the MC type carbides is not particularly limited. However, when the content of each element in the chemical composition of the bolt is within the range of this embodiment, the upper limit of the number density ND of the MC type carbides is, for example, 200.0×10 21 pieces / m 3 For example, 150.0×10 21 pieces / m 3 For example, 100.0×10 21 pieces / m 3 It is.
[0072] [Method for measuring the number density ND of MC type carbides] The number density ND of MC type carbides in a bolt can be measured using a scanning transmission electron microscope (STEM) as follows. First, a thin film sample for STEM is prepared in the following manner. The lower part of the bolt is cut perpendicular to the axial direction (longitudinal direction) of the bolt, and a disk with a thickness in the axial direction of approximately 2 mm (i.e. a disk with a diameter of 3.0 mm and a thickness of approximately 2 mm) is taken, with the center of the circle located 1.5 mm deep from the surface of the lower part of the bolt's neck. Both sides of the disk (front and back) are polished using emery paper. The disk is polished so that the front surface is parallel to the back surface. One of the front and back surfaces of the disk is defined as the observation surface. The observation surface is then mirror-polished. The mirror-polished observation surface is then further polished using colloidal silica as an abrasive.
[0073] MC type carbides have a specific crystal orientation relationship with the parent phase (Fe). Specifically, MC type carbides are plate-shaped particles extending along the {100} plane of the parent phase. Therefore, electron backscatter diffraction (EBSD) is performed on the observation surface after polishing to identify the crystal orientation of the parent phase. Then, based on the identified crystal orientation of the parent phase, it is determined that the vertical direction (observation direction) of the observation surface of the thin film is the same as that of the parent phase. <001> Focused ion beam processing (FIB processing) is performed on the disk to obtain a crystal orientation, and a thin film sample for STEM is prepared.
[0074] The preparation of a thin film sample for STEM by FIB processing may be performed by a well-known method. For example, a thin film sample for STEM is prepared by a lift-out method using a gallium (Ga) ion beam with an acceleration voltage of 30 kV.
[0075] The surface layer of the STEM thin film sample fabricated with an ion beam with an accelerating voltage of 30 kV contains dislocation loops and amorphous structures, making it unsuitable for observing MC carbides of a few nm in size. Therefore, the surface of the STEM thin film sample is polished using an ion beam with a low accelerating voltage of 1 kV or less. Through the above manufacturing process, a STEM thin film sample with a thickness of 100 nm or less is fabricated.
[0076] The prepared thin film specimen is observed with the STEM optical system. Specifically, the crystal orientation of the martensite parent phase in the STEM thin film specimen is <001> The thin film sample for STEM is tilted so that the incidence is on the zone axis of the sample. The observation magnification is set to 320,000 times, and the acceleration voltage is set to 300 kV. The detector is set under known high-angle annular dark-field (HAADF) conditions, known low-angle annular dark-field (LAADF) conditions, and known bright-field (BF) conditions, and 10 arbitrary observation fields are observed. Images are created under these observation conditions for each observation field. Of the images generated for each observation field, the image in which the MC carbides can be most clearly recognized is selected.
[0077] The area of each observation field is 280 nm × 280 nm. In all observation fields, the thickness of the thin film sample for STEM is measured by the log-ratio method of electron energy loss spectroscopy (EELS).
[0078] In the images taken in each observation field, the precipitates can be identified by contrast. Then, from among the identified precipitates, precipitates with a maximum length of 2 nm or more are identified. Here, the "maximum length" in STEM observation means the maximum line length when any two points are selected on the interface between the precipitate and the parent phase, and the entire line segment connecting the two points is included within the precipitate. It is extremely difficult to identify precipitates with a maximum length of less than 2 nm. Then, in this embodiment, precipitates with a maximum length of 2 nm or more are identified.
[0079] Among the precipitates with a maximum length of 2 nm or more, MC type carbides are identified by the following method. An electron beam is irradiated onto the precipitates with a maximum length of 2 nm or more to obtain an electron diffraction pattern. The electron diffraction patterns of MC type carbides are different from those of other precipitates. Therefore, based on the obtained electron diffraction pattern, MC type carbides are identified from among the identified precipitates.
[0080] Based on the total number of MC carbides identified in all observation fields by the above-mentioned method and the total volume calculated from the area of all observation fields and the thickness of the STEM thin film sample, the number density ND (number / m 3 ) is required.
[0081] In addition, when the content of each element in the chemical composition is within the range of this embodiment, the electron diffraction pattern of the precipitates obtained by STEM observation showed that the precipitates with a maximum length of 10 nm or less were almost MC type carbides, and precipitates other than MC type carbides were hardly present. Moreover, the maximum lengths of precipitates other than MC type carbides such as M2C type carbides and cementite all far exceeded 10 nm. Therefore, as a method for identifying the above-mentioned MC type carbides, instead of the electron diffraction pattern, precipitates with a maximum length of 10 nm or less (i.e., a maximum length of 2 to 10 nm) may be identified as MC type carbides.
[0082] [Bolt effect] The bolt of this embodiment satisfies the above-mentioned features 1 to 4. As a result, the bolt of this embodiment has excellent hydrogen embrittlement resistance even when the tensile strength TS is as high as 1000 MPa or more.
[0083] As described above, the limiting hydrogen content can be used as an index of hydrogen embrittlement resistance. The higher the limiting hydrogen content, the better the resistance to hydrogen embrittlement. The limiting hydrogen content refers to the upper limit of the amount of hydrogen that will not cause delayed fracture of the bolt.
[0084] In the bolt of this embodiment, the limit of the hydrogen amount is 1.5 ppm by mass or more. The lower limit of the limit of the hydrogen amount is preferably 2.0 ppm by mass, and more preferably 2.5 ppm by mass.
[0085] [Method for measuring limit hydrogen amount] The limiting hydrogen content can be found by the following method. A round bar test piece with an annular notch (hereinafter simply referred to as a round bar test piece) is taken from the inside of the bolt, at a depth of 1 mm or more from the surface. The size of the round bar test piece is not particularly limited, but for example, the parallel part has a diameter of 7 mm and a length of 70 mm. A circular notch extending in the circumferential direction is formed in the longitudinal center of the round bar test piece. The R (radius of curvature) of the bottom of the notch is 0.175 mm.
[0086] A number of round bar test pieces are prepared. Hydrogen is charged to the round bar test pieces under various conditions using the cathodic hydrogen charging method. The cathodic hydrogen charging method is as follows: An aqueous solution (cathode charging solution) is prepared at room temperature by adding 0 to 20 g of ammonium thiocyanate to 1 L of a 3 mass % sodium chloride aqueous solution. The round bar test pieces are immersed in the cathodic charging solution for 72 hours, with the cathodic current density kept at 0.03 to 1.00 mA / cm. 2 Hydrogen is added to the round bar test specimen by generating a constant current controlled within the range of 1000 V. The amount of hydrogen in the round bar test specimen is adjusted by adjusting the concentration of ammonium thiocyanate in the cathode charging solution and the cathode current density.
[0087] After carrying out the cathodic hydrogen charging method, the round bar test specimen is left at room temperature for 96 hours. A zinc plating film is then formed on the surface of the hydrogen-charged round bar test specimen to prevent hydrogen from leaking out of the round bar test specimen. A constant load test is carried out at room temperature and atmospheric pressure, in which a constant load is applied to the round bar test specimen so that a load of 90% of the tensile strength TS is applied to the round bar test specimen. The test time is a maximum of 100 hours, and the test is stopped if the round bar test specimen can withstand more than 100 hours without breaking. A constant load test is carried out using multiple round bar test specimens that have been hydrogen-charged under various conditions.
[0088] After 100 hours have passed, the amount of hydrogen in the round bar test specimens that have not broken is determined. Specifically, first, the zinc plating coating is removed from the surface of the round bar test specimen. After the zinc plating coating is removed, the round bar test specimen is subjected to thermal desorption hydrogen analysis using a gas chromatograph. In the thermal desorption hydrogen analysis, the temperature is raised from room temperature to 600°C at a rate of 100°C / hour. The amount of hydrogen released from the round bar test specimen during the temperature rise is measured. The measured amount of hydrogen (ppm by mass) is regarded as the amount of hydrogen (ppm by mass) that had been charged to the round bar test specimen.
[0089] The maximum hydrogen content in the round bar test piece that did not break during the 100-hour constant load test was defined as the "limit hydrogen content" (ppm by mass).
[0090] [Bolt microstructure] The microstructure of the bolt of this embodiment includes a hard structure with an area ratio of 90% or more. The microstructure of the bolt here means a microstructure of a bolt manufactured by quenching and tempering in a manufacturing process described later. The hard structure is made of martensite and / or bainite. When the microstructure of the bolt includes a phase other than the hard structure, the remainder of the microstructure of the bolt other than the hard structure is made of one or more selected from the group consisting of retained austenite, ferrite, and pearlite. Preferably, the microstructure includes a hard structure with an area ratio of 90% or more, and the remainder is made of retained austenite. The tensile strength TS of the bolt correlates with the microstructure.
[0091] [Manufacturing method] An example of a method for manufacturing a bolt according to this embodiment will be described. The method for manufacturing a bolt described below is one example for manufacturing a bolt according to this embodiment. Therefore, a bolt having the above-mentioned configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing a bolt according to this embodiment.
[0092] An example of a method for manufacturing a bolt according to this embodiment includes the following steps. (Process 1) Steel material preparation process (Process 2) Bolt manufacturing process Each step will be described below.
[0093] [(Process 1) Steel material preparation process] In the steel preparation step, a steel material (steel material for bolts) that will be the material for bolts is prepared. The steel material for bolts may be manufactured. Alternatively, a third party may prepare the steel material for bolts. In the steel preparation step, a steel material whose chemical composition satisfies Features 1 and 2 is prepared.
[0094] When manufacturing steel material for bolts, for example, the steel material is manufactured by the following method. First, molten steel is manufactured, in which the content of each element in the chemical composition falls within the range of this embodiment. A raw material is manufactured using the molten steel. For example, the molten steel may be used to manufacture a bloom (cast piece) as the raw material by a continuous casting method, or the molten steel may be used to manufacture an ingot as the raw material by an ingot casting method. The manufactured raw material (bloom or ingot) is subjected to rough rolling (splashing rolling, or splashing rolling and hot rolling in a continuous rolling mill) to manufacture a billet.
[0095] The billet is subjected to finish rolling using a continuous rolling mill to produce a steel material (steel material for bolts). The steel material is, for example, a steel bar or a wire rod.
[0096] [(Process 2) Bolt manufacturing process] In the bolt manufacturing process, the above-mentioned steel material (steel material for bolts) is used to manufacture bolts. The bolt manufacturing process includes the following steps. (21) Wire drawing process (22) Bolt forming process (23) Heat treatment process Each step will be described below.
[0097] [(21) Wire drawing process] In the wire drawing process, the above-mentioned steel material is subjected to a well-known wire drawing process to manufacture a steel wire. The wire drawing process may be a primary wire drawing process only, or may be a multiple-step wire drawing process such as a secondary wire drawing process.
[0098] [(22) Bolt forming process] In the bolt forming process, the steel wire after the wire drawing process is cut to a predetermined length, and the cut steel wire is cold forged, rolled or cut to produce a bolt intermediate having a head, a neck portion and a shaft portion.
[0099] The bolt forming process includes the following steps. (221) Head forming process (222) Thread forming process Each step will be described below.
[0100] [(221) Head forming process] In the head forming process, the steel wire is cold forged to form a bolt-shaped intermediate product (bolt intermediate product). Specifically, the steel wire is first cut to a predetermined length. Then, the steel wire is forged using a punch and a die to form a bolt intermediate product having a head 10, a neck portion 11, and a shaft portion 12.
[0101] In the head forming process, strain is imparted to the neck portion 11 of the intermediate bolt product. The strain imparted to the neck portion 11 of the intermediate bolt product becomes the driving force for generating MC type carbides in the next heat treatment process. The strain imparted to the neck portion 11 of the intermediate bolt product in the head forming process will be described later.
[0102] [(222) Thread forming process] In the thread forming process, a threaded portion is formed on at least a part of the shank 12 of the bolt intermediate product. In the thread forming process, the threaded portion may be formed on at least a part of the shank 12 by well-known rolling. Alternatively, instead of rolling, the threaded portion may be formed on at least a part of the shank 12 by cutting. As described below, the thread forming process may be performed after the head forming process but not before the heat treatment process, but after the heat treatment process.
[0103] [(23) Heat treatment process] In the heat treatment process, the following steps are carried out on the intermediate bolt product after the bolt forming process. (231) Quenching process (232) Tempering process Each step will be described below.
[0104] [(231) Quenching process] In the quenching process, a known quenching process is performed. The quenching temperature and the holding time at the quenching temperature are not particularly limited. The quenching temperature is, for example, 870 to 1050°C. The holding time at the quenching temperature is, for example, 15 minutes to 240 minutes (4 hours). After the holding time has elapsed, the intermediate bolt is quenched. Specifically, the intermediate bolt is water-cooled or oil-cooled.
[0105] [(232) Tempering process] In the tempering process, the intermediate bolts after the quenching process are tempered under the following conditions: (Condition 1) Tempering temperature T: 570 to 650°C (Condition 2) Holding time at tempering temperature t: 0.5 to 5.0 hours (Condition 3) Tempering parameter Fn: 11500 or less Here, the tempering parameter Fn is defined by formula (A). Fn=(ε -0.5 )×((T+273)×(20+ln(t))×((Mo / 96) / (Mo / 96+Ti / 48))×(1+(Mo / 96) / (Ti / 48+Mo / 96))-25000) (A) In formula (A), ε is substituted for the strain applied to the neck portion of the intermediate bolt during the bolt forming process. T is substituted for the tempering temperature (°C). t is substituted for the holding time (hours) at the tempering temperature. Mo is substituted for the Mo content (mass%) in the bolt. V is substituted for the V content (mass%) in the bolt.
[0106] The strain ε applied to the neck portion 11 of the intermediate bolt in the bolt forming process is found by the following finite element method (FEM analysis). Specifically, for the bolt to be analyzed, an axisymmetric model of 1 / 6 size is created based on the symmetry of the shape. The 1 / 6 axisymmetric model to be analyzed is divided into multiple elements using tetrahedral primary elements with one side of the tetrahedron being 0.05 to 1.00 mm.
[0107] A three-dimensional elastic-plastic analysis using FEM is performed on the model divided into the above number of elements. A commercially available forging analysis code can be used for the analysis. An example of a commercially available forging analysis code is DEFORM-3D.
[0108] The workpiece (steel for bolts) is assumed to be an elastoplastic body, and the die is assumed to be a rigid body. The flow stress of the workpiece is the actual measured value of spheroidized annealed SCM435 material specified in JIS G 4053:2018. The physical properties of the workpiece are Young's modulus: 210 GPa, Poisson's ratio: 0.30. The die is set to dimensions that are sufficiently large compared to the workpiece. The Coulomb friction coefficient between the workpiece and the die is set to μ = 0.05. An FEM analysis is performed under the above conditions to determine the strain ε imparted to the neck portion 11 of the intermediate bolt product.
[0109] Conditions 1 to 3 of the tempering step will be explained below.
[0110] [Tempering temperature T and holding time t] The tempering temperature T is 570℃ to 650℃. If the tempering temperature T is less than 570°C, the number density ND of the MC type carbides is 2.0 × 10 21 pieces / m 3 If the tempering temperature T exceeds 650°C, the tensile strength TS will be less than 1000 MPa. The holding time t at the tempering temperature T is 0.5 to 5.0 hours. If the holding time t is less than 0.5 hours, the number density ND of the MC type carbides is 2.0 × 10 21 pieces / m 3 If the holding time t exceeds 5.0 hours, the tensile strength TS will be less than 1000 MPa.
[0111] [About the tempering parameter Fn] In the tempering process, the tempering parameter Fn defined by the formula (A) is 11500 or less. If Fn exceeds 11500, the number density ND of the generated MC type carbides is 2.0×10 21 pieces / m 3 If Fn is 11,500 or less, in a bolt having a chemical composition that satisfies Features 1 and 2, the number density ND of MC type carbides is 2.0×10 21 pieces / m 3 (Feature 4). Furthermore, the tensile strength TS can be adjusted to 1000 MPa or more (Feature 3).
[0112] The bolt according to this embodiment can be manufactured by the above manufacturing method. The above manufacturing method is a preferred example of the manufacturing method of the bolt according to this embodiment. Therefore, a bolt having the above configuration may be manufactured by a manufacturing method other than the above manufacturing method. In short, as long as the bolt according to this embodiment having the above configuration can be manufactured, the manufacturing method is not particularly limited.
[0113] [Other processes] The bolt manufacturing process according to this embodiment may include other steps in addition to the steps described above. For example, a spheroidizing heat treatment step may be performed after the wire drawing step and before the bolt forming step. Also, the thread forming step may be performed after the heat treatment step, rather than after the head forming step and before the heat treatment step. Furthermore, a compressive residual stress imparting step may be performed after the heat treatment step. EXAMPLES
[0114] The effect of the bolt of this embodiment will be described more specifically with reference to an example. The conditions in the following example are one example of conditions adopted to confirm the feasibility and effect of the bolt of this embodiment. Therefore, the bolt of this embodiment is not limited to this one example of conditions.
[0115] Steel materials (steel bars) having the chemical compositions shown in Tables 1A and 1B and serving as bolt materials were prepared.
[0116] [Table 1A]
[0117] [Table 1B]
[0118] [Steel preparation process] Steel materials of each steel grade number were manufactured by the following method. Blooms having the chemical compositions shown in Tables 1A and 1B were subjected to rough rolling (splashing and hot rolling in a continuous rolling mill) to manufacture billets. The heating temperature of the blooms was 1200°C. The manufactured billets were subjected to finish rolling to manufacture steel bars having a diameter of 20 mm. The heating temperature of the billets during finish rolling was 1200°C.
[0119] [Bolt manufacturing process] Bolts were manufactured using the manufactured steel material (steel bars). First, the 20 mm diameter steel material of each test number was subjected to wire drawing under the same conditions for each test number to manufacture a steel wire of 16 mm diameter. A head forming process was carried out for the steel wire of each test number to manufacture a hexagonal bolt intermediate product with a diagonal distance of 30 mm, a head height of 10 mm, and a nominal length of 100 mm. After the head forming process, a thread forming process was carried out under the same conditions for each test number to form a threaded portion on the shaft of the bolt intermediate product.
[0120] [Table 2]
[0121] The strain ε applied to the neck portion of the intermediate bolt produced by the bolt forming process was calculated by carrying out the above-mentioned FEM analysis. The calculated strain ε is shown in the "Strain ε" column of the "Bolt forming process" section in Table 2.
[0122] Furthermore, whether or not cracks occurred in the intermediate bolt products after the bolt forming process was judged by visual inspection. If cracks of 1 mm or more in length were confirmed on the surface of the intermediate bolt products, the cold forgeability was judged to be low (indicated as "F (Fail)" in the "Cold forgeability" column of the "Bolt forming process" column in Table 2). On the other hand, if no cracks of 1 mm or more in length were confirmed on the surface of the intermediate bolt products, the cold forgeability was judged to be good (indicated as "P (Pass)" in the "Cold forgeability" column of the "Bolt forming process" column in Table 2). For steel products with low cold forgeability, production was discontinued, and the next heat treatment process and the evaluation test described below were not carried out.
[0123] A heat treatment process was carried out on the intermediate bolts of the test numbers that had good cold forgeability. First, a quenching process was carried out on the intermediate bolts of each test number under the same conditions. In the quenching process, the quenching temperature was 880-1050°C for each test number, and the holding time at the quenching temperature was 60 minutes (1 hour). After the holding time had elapsed, the intermediate bolts were water-cooled.
[0124] The intermediate bolts after quenching were tempered. The tempering temperature T (℃) and the holding time t (hours) at the tempering temperature T for each test number are shown in Table 2. Furthermore, Fn defined by formula (A) is shown in Table 2. Bolts with each test number were manufactured according to the above manufacturing process.
[0125] [Evaluation test] The following evaluation tests were carried out on the bolts with each test number. (Test 1) Tensile test (Test 2) MC type carbide number density ND measurement test (Test 3) Limit hydrogen amount measurement test
[0126] [(Test 1) Tensile test] The tensile strength TS (MPa) of the bolts with each test number was determined based on the method described in the above [Method of measuring tensile strength TS]. The determined tensile strength TS is shown in the "TS (MPa)" column in Table 2.
[0127] For test numbers in which the obtained tensile strength TS was less than 1000 MPa, the subsequent evaluation tests (Test 2 and Test 3) were not carried out.
[0128] [(Test 2) Measurement of the number density ND of MC type carbides] Based on the method described in [Method for measuring the number density ND of MC type carbides] above, the number density ND (pieces / m 3 The number density ND thus obtained was calculated using the "Number density ND (× 10 21 pieces / m 3 ) column.
[0129] [(Test 3) Limit hydrogen amount measurement test] The limit hydrogen amount (ppm by mass) of the bolt with each test number was measured based on the method described in [Method for measuring limit hydrogen amount] above. The limit hydrogen amount (ppm by mass) obtained is shown in the "Limit hydrogen amount (ppm by mass)" column in Table 2.
[0130] [Test Results] The evaluation results are shown in Table 2. Referring to Tables 1A, 1B and 2, in the bolts with test numbers 1 to 27, the content of each element in the chemical composition was within the range of this embodiment, and the tensile strength TS was 1000 MPa or more. Furthermore, the number density ND of the MC type carbides was 2.0×10 21 pieces / m 3 As a result, the limit hydrogen content of the bolts with these test numbers was 1.5 mass ppm or more, and they had excellent hydrogen embrittlement resistance.
[0131] On the other hand, in test number 28, the Mo content in the bolt was too low, and as a result, the tensile strength TS was low at less than 1000 MPa.
[0132] In test number 29, the Mo content in the bolt was too high. As a result, cracks were confirmed in the intermediate bolt after the bolt forming process, and the cold forgeability was poor.
[0133] In test number 30, the Ti content in the bolt was too high. As a result, cracks were confirmed in the intermediate bolt after the bolt forming process, and the cold forgeability was poor.
[0134] In test numbers 31 and 32, F1 was below the lower limit and did not satisfy formula (1). Therefore, although the number density ND of the MC carbides in the bolt was appropriate, the limit hydrogen content was less than 1.5 ppm by mass, and the hydrogen embrittlement resistance was low.
[0135] In test numbers 33 and 34, the chemical composition of the bolts was appropriate, but the tempering temperature T was too low. Therefore, the number density ND of the MC carbides in the bolts was too low. As a result, the limit hydrogen content was less than 1.5 mass ppm, and the hydrogen embrittlement resistance was low.
[0136] In test numbers 35 and 36, the chemical composition of the bolts was appropriate, but the tempering temperature T was too high. As a result, the tensile strength TS was low at less than 1000 MPa.
[0137] In test numbers 37 and 38, the chemical composition of the bolts was appropriate, but the holding time t at the tempering temperature T was too short. Therefore, the number density ND of the MC carbides in the bolts was too low. As a result, the limit hydrogen content was less than 1.5 mass ppm, and the hydrogen embrittlement resistance was low.
[0138] In test numbers 39 and 40, the chemical composition of the bolts was appropriate, but the holding time t at the tempering temperature T was too long. As a result, the tensile strength TS was low at less than 1000 MPa.
[0139] In the bolts of test numbers 41 and 42, although the chemical composition of the bolts was appropriate, the tempering parameter Fn was too high. Therefore, the number density ND of the MC type carbides in the bolts was too low. As a result, the limit hydrogen content was less than 1.5 mass ppm, and the hydrogen embrittlement resistance was low.
[0140] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.
Claims
1. The chemical composition, in mass%, is C: 0.10-0.50%, Si: 0.01-0.30%, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Cr: 0.01-0.80%, Mo: 0.70-2.00%, Al: 0.005-0.100%, N: 0.0010-0.0300%, Ti: 0.001 to 0.300%, and The balance is Fe and impurities. Satisfies formula (1A), The tensile strength TS is 1000 MPa or more, The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all. bolt. Mo / 2Ti>4.25 (1A) Here, each element symbol in formula (1A) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass %.
2. The chemical composition, in mass%, is C: 0.10-0.50%, Si: 0.01-0.30%, Mn: 0.10 to 2.50%, P: 0.030% or less, S: 0.030% or less, Cr: 0.01-0.80%, Mo: 0.70-2.00%, Al: 0.005-0.100%, N: 0.0010 to 0.0300%, and Ti: 0.001 to 0.300%; Further, the composition contains one or more selected from the group consisting of Groups 1 to 3, The balance is Fe and impurities. Satisfies formula (1), The tensile strength TS is 1000 MPa or more, The number density ND of MC type carbides is 2.0×10 21 pieces / m 3 That's all. bolt. Mo / (2Ti+V)>4.25 (1) Here, each element symbol in formula (1) is substituted with the content of the corresponding element in the chemical composition of the bolt in mass %. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, B: 0.0100% or less, Zr: 0.300% or less, Hf: 0.100% or less, Ta: 0.100% or less, and W: 0.20% or less, one or more selected from the group consisting of [Group 2] V: 0.50% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.0050% or less, Bi: 0.020% or less; and Te: 0.010% or less, one or more selected from the group consisting of
3. 3. The bolt according to claim 2, The chemical composition contains the first group, bolt.
4. 3. The bolt according to claim 2, The chemical composition contains the second group, bolt.
5. 3. The bolt according to claim 2, The chemical composition contains the third group, bolt.
Citation Information
Patent Citations
Bolt and method for producing bolt
JP2013163865A
bolt
JP2019218584A
High-strength bolt
WO2017094487A1