Double-sided adhesive sheet, and laminate for image display device

A double-sided adhesive sheet with a specific (meth)acrylic copolymer composition and controlled reflection intensities addresses the issue of wrinkles and bubbles in flexible displays, ensuring high visibility and durability.

JP2024158768AActive Publication Date: 2024-11-08TOYO INK MFG CO LTD +1
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023074280
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Adhesive layers used in electronic devices, particularly in foldable displays, suffer from the formation of wrinkles and bubbles over time, reducing adhesion and visibility, and there is a need for adhesive sheets that can maintain visibility and flexibility without a base material.

Method used

A double-sided adhesive sheet without a base material, composed of a first and second release sheet with an adhesive layer in between, featuring a (meth)acrylic copolymer with specific molecular weight, storage modulus, and glass transition temperature, and adjusted reflection intensities to suppress wrinkles and bubbles.

Benefits of technology

The adhesive sheet maintains excellent visibility and suppresses wrinkles and bubbles even in flexible display applications, with improved adhesion and durability against repeated bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158768000001_ABST
    Figure 2024158768000001_ABST
Patent Text Reader

Abstract

To provide a substrate-less double-sided adhesive sheet that has excellent visibility even when used in optical applications and that can inhibit wrinkles and air bubbles even when used in flexible display applications.SOLUTION: A double-sided adhesive sheet is a substrate-less double-sided adhesive sheet consisting of a first release sheet 1, an adhesive layer 3 and a second release sheet 2 laminated in this order. When a surface of the adhesive layer 3 is measured with a wave scan device, the reflection intensity Wa in the wavelength range from 0.1 to 0.3 mm is from 1 to 26, and the reflection intensity Wd in the wavelength range from 3 to 10 mm is from 0.3 to 8. The adhesive layer 3 is configured to: (i) be either an adhesive layer containing a (meth)acrylic copolymer (a) having a weight average molecular weight of 1,000,000 to 1,800,000 or an adhesive layer obtained by crosslinking an adhesive composition containing the (meth)acrylic copolymer (a); (ii) have a storage modulus at 23°C from 1×103 to 8×104 Pa; and (iii) have a glass transition temperature according to DSC satisfying -70°C≤Tg≤-35°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a double-sided pressure-sensitive adhesive sheet and a laminate for an image display device. [Background technology]

[0002] Since pressure-sensitive adhesive sheets can be bonded to an adherend by the simple means of pasting, they are widely used in electronic devices such as personal computers and smartphones that require bonding of various members, and various proposals have been made for them. For example, Patent Document 1 describes an acrylic polymer that contains an acrylic polymer formed from a monomer that has a Tg of -10°C or higher when it forms a homopolymer, and has a shear storage modulus of 0.8×10 at 23°C. 5 ~5.0×10 5The optical pressure-sensitive adhesive sheet has an acrylic pressure-sensitive adhesive layer with a water content of 0.65% by weight or more after storage for 120 hours under an environment of 60°C and 95% RH. Patent documents 2 and 3 disclose a pressure-sensitive adhesive comprising an acrylic copolymer (A) obtained by radical polymerization of 20 to 90% by weight of an ethylenically unsaturated monomer (A1) having an alkyl group with an SP value of 8 or more and less than 9.00 and 10 to 80% by weight of an ethylenically unsaturated monomer (A2) having a polar group with an SP value of 9.00 or more and 15 or less, a polyisocyanate curing agent (B), and a silane coupling agent (C). Furthermore, Patent Document 4 discloses a pressure-sensitive adhesive composition containing a (meth)acrylic polymer that contains 5% by mass or more of structural units (A) derived from (meth)acrylic acid alkyl esters having an alkyl group with 12 or more carbon atoms, 5% by mass or more of structural units (B) derived from (meth)acrylic acid alkyl esters having an alkyl group with 1 to 8 carbon atoms, and 2% by mass to 30% by mass of structural units (C) derived from monomers having a hydroxyl group, and the total content of structural units (A), structural units (B) and structural units (C) is 80% by mass or more. Patent Document 5 discloses a pressure-sensitive adhesive composition that contains a (meth)acrylic copolymer having an acid value of 2.5 mgKOH / g or less and containing structural units derived from monomers having a hydroxyl group in the range of 0.01 to 1% by mass relative to the total structural units, a tolylene diisocyanate compound in the range of 5 to 30 parts by mass relative to 100 parts by mass of the (meth)acrylic copolymer, and an imidazole compound. Furthermore, Patent Document 6 discloses a pressure-sensitive adhesive composition containing a (meth)acrylic polymer having a carboxy group and 0.005 to 2.5 parts by mass of an alicyclic epoxy-modified silicone relative to 100 parts by mass of the (meth)acrylic polymer. Patent Document 7 discloses a pressure-sensitive adhesive composition having a gel fraction of 40% to 80% immediately after the formation of the pressure-sensitive adhesive layer, and a gel fraction of 60% to 85% after storage for 7 days under conditions of 23°C and 55% RH from the formation of the pressure-sensitive adhesive layer.Patent Document 8 discloses a laminate sheet having a reflection intensity (Wb) of less than 10.0 when the exposed surface of the release film is measured for reflection intensity (Wb) in the wavelength region of 0.3 to 1.0 mm using a wavescan device, and Patent Document 9 discloses a laminate sheet having a film substrate with a thickness of 38 μm or less, a reflection intensity (Wb) of 10 or more when the exposed surface of the release film is measured for reflection intensity (Wb) in the wavelength region of 0.3 to 1.0 mm using a wavescan device, and the pressure-sensitive adhesive layer contains a structure derived from at least a (meth)acrylic copolymer and a chelating crosslinking agent. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2011 / 111575 [Patent Document 2] JP 2013-127012 A [Patent Document 3] China Patent Application Publication No. 104231981 [Patent Document 4] JP 2014-74122 A [Patent Document 5] JP 2016-188309 A [Patent Document 6] JP 2016-79266 A [Patent Document 7] JP 2018-2961 A [Patent Document 8] JP 2020-83908 A [Patent Document 9] JP 2020-83910 A Summary of the Invention [Problem to be solved by the invention]

[0004] As described above, the adhesive layer is widely used in electronic devices because it can bond adherends to each other in a simple manner. However, the adhesive layer does not have high resistance to repeated bending, and when applied to, for example, a folding type foldable display, which has become rapidly popular in recent years, there is a problem that wrinkles and bubbles are likely to occur over time. The occurrence of such wrinkles and bubbles not only reduces adhesion, but also reduces the visibility of surface protection films, etc., which is particularly serious when used for optical components such as displays.

[0005] The market is demanding substrate-less double-sided adhesive sheets due to the need for productivity, versatility, and the need to make various electronic devices lighter, thinner, shorter, and smaller. In addition, even when applied to applications that require flexibility, such as foldable displays, there is a demand for adhesive layers with excellent visibility that can suppress the generation of wrinkles and bubbles over time. In particular, there is a demand for the development of adhesive layers that can suppress the generation of wrinkles and bubbles from low temperatures (0°C) to high temperatures (40°C).

[0006] Although the above describes the problems associated with adhesive layers used for displays, similar problems can arise in all applications where improved visibility is desired.

[0007] The present disclosure has been made in consideration of the above-mentioned problems, and has an objective of providing a substrate-less double-sided pressure-sensitive adhesive sheet that has excellent visibility when applied to optical applications and can suppress wrinkles and air bubbles when applied to flexible displays. [Means for solving the problem]

[0008] The present disclosure provides the following double-sided pressure-sensitive adhesive sheet and laminate for an image display device. [1]: A double-sided PSA sheet for use in substrate-less flexible displays, comprising a first release sheet, an adhesive layer, and a second release sheet laminated in that order, The first release sheet is peeled off to expose the surface of the adhesive layer, a glass substrate is attached to the surface, the glass substrate is placed on a white paper, and the second release sheet is peeled off to expose the surface of the adhesive layer. When the surface is measured with a wavescan device, The reflection intensity Wa in the wavelength range of 0.1 to 0.3 mm is 1 to 26, and The reflection intensity Wd in the wavelength range of 3 to 10 mm is 0.3 to 8, The adhesive layer is (i) either an adhesive layer containing a (meth)acrylic copolymer (a) having a weight average molecular weight of 1,000,000 to 1,800,000, or an adhesive layer obtained by crosslinking an adhesive composition containing the (meth)acrylic copolymer (a); (ii) Storage modulus at 23°C is 1×10 3 ~8×10 4 Pa, (iii) The glass transition temperature by DSC is -70°C ≦ Tg ≦ -35°C Double-sided adhesive sheet. [2]: When a glass substrate is attached to the surface of the adhesive layer exposed by peeling off the first release sheet, the glass substrate is placed on a white paper, and the surface of the adhesive layer exposed by peeling off the second release sheet is measured with a wavescan device, The reflection intensity Wc in the wavelength range of 1 to 3 mm is 1 to 12, and The double-sided pressure-sensitive adhesive sheet according to [1], which has a reflection intensity We of 1 to 12 in the wavelength range of 10 to 30 mm. [3]: The double-sided pressure-sensitive adhesive sheet according to [1] or [2], wherein the (meth)acrylic copolymer (a) has a structural unit derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 6 carbon atoms, and a structural unit derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with 7 to 12 carbon atoms. [4]: The double-sided pressure-sensitive adhesive sheet according to any one of [1] to [3], wherein the (meth)acrylic copolymer (a) has a molecular weight dispersity Mw / Mn of less than 5. [5]: A laminate for an image display device, in which adherends are bonded to each other via the adhesive layer of the double-sided adhesive sheet of any one of [1] to [4]. Effect of the Invention

[0009] The present disclosure has the excellent effect of providing a substrate-less double-sided pressure-sensitive adhesive sheet that has excellent visibility when applied to optical applications and can suppress wrinkles and air bubbles when applied to flexible displays. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an example of a double-sided pressure-sensitive adhesive sheet according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a method for measuring the adhesive layer surface using a wavescan device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present disclosure will be described in detail below. Needless to say, other embodiments are also included in the scope of the present disclosure as long as they are consistent with the gist of the present disclosure. In addition, in this specification, a numerical range specified using "~" includes the numerical values ​​written before and after "~" as the range of the lower and upper limits. In addition, "film", "sheet" and "tape" are synonymous and are not distinguished by thickness or shape. (Meth)acrylic means at least one of acrylic and methacrylic, and (meth)acrylic acid alkyl ester means at least one of acrylic acid alkyl ester and methacrylic acid alkyl ester. In addition, various components may be used independently alone or in combination of two or more types, unless otherwise noted. Numerical values ​​in this specification refer to values ​​obtained by the method described in the examples described below.

[0012] 1. Double-sided adhesive sheet The double-sided pressure-sensitive adhesive sheet of the present disclosure (hereinafter also referred to as the present pressure-sensitive adhesive sheet) is a substrate-less sheet in which a first release sheet, a pressure-sensitive adhesive layer, and a second release sheet are laminated in this order. The present pressure-sensitive adhesive sheet can be applied to bonding of various adherends. The present pressure-sensitive adhesive sheet has excellent visibility, and is particularly suitable for optical applications. In addition, the present pressure-sensitive adhesive sheet can suppress wrinkles and bubbles, and is therefore suitable for flexible display applications. In particular, the present pressure-sensitive adhesive sheet has excellent durability against repeated folding, and is therefore suitable for foldable display applications.

[0013] Fig. 1 is a schematic cross-sectional view showing an example of a substrate-less double-sided pressure-sensitive adhesive sheet according to the present embodiment. Double-sided pressure-sensitive adhesive sheet 10 is a substrate-less sheet in which an adhesive layer 3 is sandwiched between a first release sheet 1 and a second release sheet 2. From the viewpoint of release balance, as shown in Fig. 1, a preferred embodiment is one in which the first release sheet 1 and the second release sheet 2 have overhangs w (areas w where the adhesive layer 3 is not formed) relative to the adhesive layer 3 in the longitudinal direction (Z direction in the figure) of both ends of the width direction (X direction in the figure) of the present pressure-sensitive adhesive sheet 10.

[0014] The degree of unevenness of the surface of the adhesive layer 3, for example, undulation, waviness, and orange peel, can be confirmed by a wave scanning device. The reflection intensity Wa in the wavelength range of 0.1 to 0.3 mm obtained by the wave scanning device is an index of a fine structure visible from a close distance of about 40 cm, and usually has a value of 0 to 80. Among these, in order to prevent a decrease in gloss and cloudiness, it is considered that the reflection intensity Wa is preferably in the range of 0 to 1. The reflection intensity Wd in the wavelength range of 3 to 10 mm obtained by the wave scanning device is an index of a fine structure visible from a medium distance of about 3 m, and usually has a value of 0 to 50. Among these, in order to prevent a decrease in adhesive strength due to a decrease in smoothness, it is considered that the reflection intensity Wd is preferably in the range of 8 to 30.

[0015] The reflection intensities Wa, Wd and the reflection intensities Wc, Wd described below are measured by peeling off the first release sheet 1, attaching the surface 31 of the adhesive layer 3 exposed on a glass substrate 4 as shown in Figure 2, placing the glass substrate 4 on a white paper 5, and then peeling off the second release sheet 2 and measuring the surface 32 of the adhesive layer 3 exposed with a wavescan device.

[0016] As a result of extensive research by the present inventors into substrate-less double-sided pressure-sensitive adhesive sheets, it was found that a substrate-less double-sided pressure-sensitive adhesive sheet can be obtained that has excellent visibility even when applied to optical applications, and can suppress the occurrence of air bubbles and wrinkles even when applied to flexible display applications, by combining a reflection intensity Wa of 1 to 26 and a reflection intensity Wd of 0.3 to 8 on the surface 32 of the pressure-sensitive adhesive layer 3. Although the reason for this is only speculation, it is believed that the combination of a small waviness, Wa, within the above range, and a relatively large waviness, Wd, within the above range, improves adhesion to the adherend.

[0017] The value of Wa can be adjusted mainly by the coating process. Specifically, it can be adjusted by the solid content concentration when the adhesive composition is coated in a sheet form. As the solid content concentration decreases, Wa tends to become smaller (as the solid content concentration increases, Wa tends to become larger). The value of Wa can also be adjusted by the coating speed of the adhesive composition. As the coating speed increases, Wa tends to become larger. The value of Wa can also be adjusted by the drying conditions (temperature, time, air volume, etc.) when coating the adhesive composition to form a sheet. As the drying temperature increases, Wa tends to become larger. As the drying time increases, Wa tends to become larger. Wa also varies by adjusting the drying air volume. Furthermore, Wa may be adjusted by the aging conditions (time and temperature) after forming into a sheet form. Wa can also be adjusted by the film thickness, and Wa tends to become larger as the film thickness decreases.

[0018] Methods for adjusting Wd include the same methods as those for Wa. Among them, Wd tends to increase by increasing the drying temperature (Wd tends to decrease by decreasing the drying temperature). Also, Wd tends to increase by increasing the drying time.

[0019] The more preferable range for Wa is 3 to 24, the even more preferable range for Wa is 4 to 23, and the particularly preferable range for Wa is 7 to 19. The more preferable range for Wa is 0.5 to 5, the even more preferable range for Wa is 0.8 to 5, and the particularly preferable range for Wa is 1 to 4.

[0020] From the viewpoint of improving visibility, in addition to satisfying the specific range of Wa and the specific range of Wd, it is preferable that the reflection intensity Wc in the wavelength range of 1 to 3 mm and the reflection intensity We in the wavelength range of 10 to 30 mm measured on the surface 32 of the adhesive layer 3 shown in FIG. 2 by a wave scanning device is 1 to 12. Wc is an index of a fine structure visible from a short to medium distance of about 40 cm to 3 m. By combining the specific ranges of Wa and Wd with the Wc, the effect of reducing haze is improved. By combining the specific ranges of Wa, Wd, and Wc with We in the above range, the effect of reducing the brightness difference is improved. It should be noted that We is an index of a fine structure visible from a long distance of 3 m or more.

[0021] The method for adjusting Wc can be the same as the method for adjusting Wa. Among them, the method of adjusting the solid content concentration and / or the film thickness is preferable. As the solid content concentration increases, Wc tends to increase (as the solid content concentration decreases, Wc tends to decrease). In addition, methods for adjusting We include the same methods as for Wa described above. Among them, a method of adjusting by the aging conditions (time and temperature) after sheet formation is preferable. As the aging temperature increases, We tends to increase (as the aging temperature decreases, We tends to decrease).

[0022] A more preferable range for Wc is 2 to 11, and an even more preferable range is 2 to 7. A more preferable range for We is 1 to 9, and an even more preferable range is 1 to 7.

[0023] From the viewpoint of tackiness, the reflection intensity Wb in the wavelength region of 0.3 to 1.0 mm is preferably in the range of 2 to 30. The term "tackiness" used here refers to an index of stickiness determined by the J.Dow method in accordance with JIS Z-0237:2022. Wb is more preferably 6 to 30, and even more preferably 9 to 25. A suitable method for adjusting Wb is to adjust the coating speed. As the coating speed increases, Wb tends to increase (as the coating speed decreases, Wb tends to decrease).

[0024] From the viewpoint of increasing productivity, the present pressure-sensitive adhesive sheet is preferably produced in the form of a roll sheet in which a long double-sided pressure-sensitive adhesive sheet is wound around a core. For example, a roll sheet can be obtained by winding a long double-sided pressure-sensitive adhesive sheet around a cylindrical core having an outer diameter (diameter) of about 100 to 1000 mm. The width of the double-sided pressure-sensitive adhesive sheet is, for example, 100 to 3000 mm, and the roll length of the pressure-sensitive adhesive sheet is, for example, 10 to 3000 m. In the case of a roll sheet, the present pressure-sensitive adhesive sheet is unwound and cut and / or punched at the time of shipment or use. Then, after peeling and removing the first release sheet 1, the exposed pressure-sensitive adhesive layer 3 is attached to an adherend, and then the second release sheet 2 is peeled and removed, and the thus exposed pressure-sensitive adhesive layer 3 is attached to another adherend. Through such a process, the adherends are joined to each other.

[0025] 2. Adhesive layer The pressure-sensitive adhesive layer is a layer formed from a pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition may be a crosslinked or non-crosslinked pressure-sensitive adhesive, and may be any of an emulsion type, a solvent type, or a solventless type.

[0026] The present adhesive layer has Wa within the above-mentioned specific range and Wd within the above-mentioned specific range, and satisfies the following (i) to (iii). (i) An adhesive layer containing a (meth)acrylic copolymer (a) having a weight average molecular weight of 1,000,000 to 1,800,000 (an adhesive layer made of a non-crosslinked adhesive), or an adhesive layer obtained by crosslinking an adhesive composition containing the (meth)acrylic copolymer (a) (an adhesive layer obtained by crosslinking a crosslinked adhesive). (ii) Storage modulus at 23°C is 1×10 3 ~8×10 4 It is Pa. (iii) The glass transition temperature as determined by DSC is -70°C≦Tg≦-35°C.

[0027] This adhesive layer can effectively suppress deformation of the adhesive layer, for example, at the stage of a roll-shaped double-sided adhesive sheet (first release sheet / adhesive layer / second release sheet). In addition, this adhesive layer can withstand repeated bending and exhibit an excellent recovery rate when returning from a bent state to its original state. The effect of suppressing air bubbles and wrinkles over time is not only excellent at room temperature (23°C), but can also suppress air bubbles and wrinkles in a range from low temperature (0°C) to high temperature (40°C).

[0028] The more preferable range of the storage modulus at 23°C is 3×10 3 ~7×10 4 Pa, and more preferably 1×10 4 ~5×10 4 Pa. In particular, by using an adhesive layer whose storage modulus satisfies the above (ii), it is believed that the uneven parts of the adhesive layer absorb the misalignment that causes air bubbles and wrinkles, and the occurrence of air bubbles and wrinkles can be suppressed. For this reason, it is particularly suitable for flexible display applications such as foldable displays.

[0029] In other words, the adhesive layer that satisfies the above (i) contains (meth)acrylic copolymer (a) as an adhesive resin, or contains crosslinked (meth)acrylic copolymer (a). The crosslinking may be between (meth)acrylic copolymers (a) or between (meth)acrylic copolymer (a) and a curing agent. From the viewpoint of obtaining an adhesive layer that has both adhesive strength and cohesive strength, an adhesive layer having a crosslinked structure between (meth)acrylic copolymer (a) and a curing agent is preferable. In addition to Wa and Wd in the above specific ranges, the adhesive layer is made by combining (ii), (iii) and (i) containing the above (meth)acrylic copolymer component, thereby obtaining excellent transparency in addition to adhesiveness and flexibility.

[0030] Furthermore, when the glass transition temperature by DSC is set to -70°C≦Tg≦-35°C (iii), the adhesive layer having the above specific ranges of Wa and Wd combined with the above (i) and (ii) can bring out excellent flexibility. As a result, an adhesive layer that can suppress wrinkles and bubbles even when applied to flexible display applications can be obtained. A more preferred range is -65°C≦Tg(DSC)≦-50°C, and an even more preferred range is -65°C≦Tg(DSC)≦-55°C.

[0031] From the viewpoint of air bubbles and wrinkles caused by folding under low temperature (0℃) conditions, the storage modulus of the adhesive layer at 0℃ and a frequency of 1Hz is 2×10 3 ~1.5×10 5 Pa is preferred, 1×10 4 ~1.4×10 5 Pa is more preferable, 1.2×10 4 ~9×10 4 Pa is more preferred.

[0032] In addition, from the viewpoint of air bubbles and wrinkles caused by folding under high temperature (40°C) conditions, the storage modulus of the adhesive layer at 40°C and a frequency of 1 Hz is 8×10 2 ~7×10 4 Pa is preferred, 1×10 3 ~5.5×10 4 Pa is more preferable, 8×10 3 ~5×104 Pa is more preferred.

[0033] The thickness Ta of the adhesive layer is arbitrary. From the viewpoint of maintaining good optical transparency, flexibility, and surface structure while exerting adhesive force, the thickness Ta of the adhesive layer is preferably about 5 to 150 μm. The thickness Ta of the adhesive layer is more preferably in the range of 15 to 120 μm, and even more preferably in the range of 25 to 100 μm. The thickness Ta of the adhesive layer is determined by the method of the examples described later.

[0034] The adhesive strength of the adhesive layer can be designed as desired depending on the application. The adhesive strength of the adhesive layer can be controlled by the composition of the adhesive resin constituting the adhesive composition described below, the Tg of the adhesive resin, the amount of the curing agent in the adhesive composition, etc. The adhesive strength can be increased by using a (meth)acrylic copolymer (a) obtained by using a highly polar (meth)acrylic monomer ((meth)acrylic monomer) derived from a carboxyl group-containing monomer as a monomer. The adhesive strength tends to be higher as the Tg of the adhesive resin is lower. Furthermore, the adhesive strength tends to be higher as the amount of the curing agent in the adhesive composition is smaller.

[0035] The adhesive layer may be a layer having an island-type microphase separation structure composed of a continuous phase containing a soft segment and a dispersed phase containing a hard segment, from the viewpoint of effectively preventing cohesive failure and effectively suppressing dents in the double-sided adhesive sheet. The adhesive layer preferably has a structure in which a dispersed phase containing a hard segment is dispersed in a matrix forming a continuous phase containing a soft segment. The microphase separation structure can be confirmed by an atomic force microscope (AFM), TEM, SPM, etc. By forming a microphase separation structure, an adhesive layer that can be provided with excellent elasticity and effectively suppress the occurrence of cracks can be provided.

[0036] The gel fraction of the adhesive layer is preferably 70 to 90% from the viewpoint of air bubbles and wrinkles caused by folding. The gel fraction can be obtained by the method described in the examples below. The gel fraction is more preferably 75 to 90%, and further preferably 75 to 85%.

[0037] 2-1. Adhesive resin As described above, the (meth)acrylic copolymer (a) having a weight average molecular weight (Mw) of 1,000,000 to 1,800,000 is used as the adhesive resin. By using the (meth)acrylic copolymer (a) in the above range, not only excellent strength but also excellent punching processability can be obtained. The lower limit of Mw of the (meth)acrylic copolymer (a) is more preferably 1,100,000. The upper limit of Mw is more preferably 1,700,000, further preferably 1,500,000, and particularly preferably 1,300,000. From the viewpoint of suppressing bubbles and wrinkles over time during folding in the range from low temperature (0°C) to high temperature (40°C), the molecular weight dispersity Mw / Mn of the (meth)acrylic copolymer (a) is preferably less than 5. It is more preferably 2 to 4.5, and even more preferably 2.5 to 4.

[0038] The (meth)acrylic copolymer (a) preferably contains a (meth)acrylic acid ester as a monomer. A suitable example of the (meth)acrylic acid ester is a (meth)acrylic acid alkyl ester monomer. When forming a crosslinked adhesive layer, a (meth)acrylic copolymer obtained by copolymerizing a functional group-containing monomer and a (meth)acrylic acid ester is preferred.

[0039] The alkyl group of the (meth)acrylic acid alkyl ester may be either linear or branched. The alkyl group is preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms. Specific examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate. , nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and lauryl (meth)acrylate.

[0040] The (meth)acrylic copolymer (a) preferably has a structural unit derived from a linear or branched (meth)acrylic acid alkyl ester monomer (a-1) having an alkyl group with 1 to 6 carbon atoms, and a structural unit derived from a linear or branched (meth)acrylic acid alkyl ester monomer (a-2) having an alkyl group with 7 to 12 carbon atoms. By containing one or more structural units derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 6 carbon atoms, interaction with the adherend interface is easily expressed in a short contact time, and adhesion can be increased. In addition, by containing one or more structural units derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with 7 to 12 carbon atoms, it is easy to wet and spread on the adherend interface in a long contact time, and adhesion can be increased.

[0041] A more preferred embodiment of the (meth)acrylic copolymer (a) is a combination of one or more structural units derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with a carbon number of 1 to 4 and one or more structural units derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with a carbon number of 8 to 12. Suitable combinations include any combination selected from methyl (meth)acrylate and n-butyl (meth)acrylate as (a-1) and 2-ethylhexyl (meth)acrylate and dodecyl (meth)acrylate as (a-2).

[0042] The structural unit derived from a (meth)acrylic acid alkyl ester containing a linear or branched alkyl group is preferably from 10 to 100 mass%, more preferably from 20 to 90 mass%, and even more preferably from 30 to 80 mass%, relative to 100 mass% of the (meth)acrylic copolymer (a).

[0043] As the monomer used in the (meth)acrylic copolymer (a), the (meth)acrylic acid alkyl ester monomer (a-3) in which the alkyl group is cyclic is also preferably used. As such a monomer, for example, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, and isobornyl (meth)acrylate can be mentioned. Among these, cyclohexyl (meth)acrylate and isobornyl (meth)acrylate are particularly preferred from the viewpoint of flexibility and adhesive strength.

[0044] The ratio (a-2) / (a-1) of the monomer (a-2) to the monomer (a-1) is preferably 0.9 to 20, more preferably 1 to 20, even more preferably 3 to 20, and particularly preferably 4 to 20, from the viewpoint of more effectively preventing bubbles and wrinkles during folding under low temperature, normal temperature, and high temperature conditions.

[0045] Among the monomers (a-2), a combination of a linear or branched (meth)acrylic acid alkyl ester having an alkyl group carbon number of 12 and the monomer (a-1) is preferred from the viewpoint of recovery rate. From the viewpoint of recovery rate, a combination of a linear or branched (meth)acrylic acid alkyl ester monomer (a-1) having an alkyl group carbon number of 1 to 6 and a linear or branched (meth)acrylic acid alkyl ester monomer (a-2) having an alkyl group carbon number of 8 to 12, as well as a combination of the monomer (a-3).

[0046] Examples of functional group-containing monomers include carboxyl group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, and amino group-containing monomers. By including a functional group-containing monomer, the cohesive strength of the adhesive is improved, and a tough adhesive layer can be obtained.

[0047] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, p-carboxybenzyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, citraconic acid, and isocrotonic acid. Among these, (meth)acrylic acid is preferred from the viewpoint of cohesive strength and adhesive strength.

[0048] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Among these, from the viewpoint of cohesive strength and adhesive strength, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are more preferred.

[0049] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 6-methyl-3,4-epoxycyclohexylmethyl (meth)acrylate.

[0050] Examples of the amino group-containing monomer include monoalkylamino esters of (meth)acrylic acid such as monoethylaminoethyl (meth)acrylate, monoethylaminopropyl (meth)acrylate, monomethylaminoethyl (meth)acrylate, and monomethylaminopropyl (meth)acrylate.

[0051] From the viewpoint of tack, it is preferable that the Tg (DSC) of the (meth)acrylic copolymer (a) is -70°C < Tg < -35°C. More preferably, it is -65 to -40°C, and still more preferably, it is -65 to -50°C.

[0052] With respect to 100% by mass of the (meth)acrylic copolymer (a), the total of the structural units derived from the functional group-containing monomer is preferably 1 to 20% by mass. By setting it within the above range, the cohesive force can be adjusted by the reaction with the curing agent, and the flexibility and recovery rate can be increased. With respect to 100% by mass of the (meth)acrylic copolymer (a), the structural unit derived from the carboxy group-containing monomer is preferably 1 to 10% by mass. By being within the above range, both the cohesive force and the relaxation property of the adhesive layer can be achieved. Also, with respect to 100% by mass of the (meth)acrylic copolymer (a), the structural unit derived from the hydroxy group-containing monomer is preferably 1 to 10% by mass. By being within the above range, both the adhesive strength and the heat resistance of the adhesive layer can be achieved.

[0053] The (meth)acrylic copolymer (a) may contain a structural unit derived from another monomer copolymerizable with the above-mentioned monomer. Examples of the other monomer include a monomer having an alkyleneoxy group and another vinyl monomer. Other examples include methoxyethyl (meth)acrylic acid ester, methoxydiethylene glycol (meth)acrylic acid ester, vinyl acetate, vinyl crotonate, styrene, acrylonitrile, and acrylamide. The structural unit derived from the other monomer is preferably 0.1 to 20% by mass in 100% by mass of the (meth)acrylic copolymer (a).

[0054] The (meth)acrylic copolymer (a) is obtained by polymerizing a monomer mixture. During polymerization, a polymerization initiator is used as necessary. The content of the polymerization initiator is, for example, 0.01 to 10 parts by mass relative to 100 parts by mass of the monomer mixture. The polymerization method is not limited. For example, the polymerization can be performed by solution polymerization, bulk polymerization, emulsion polymerization, and suspension polymerization. Examples of the solvent used in solution polymerization include acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, and cyclohexanone. The polymerization temperature is, for example, 60 to 120°C, and the polymerization time is about 2 to 12 hours.

[0055] The adhesive resin may contain other resins other than the (meth)acrylic copolymer (a) within the scope of the present disclosure. Examples of other resins include rubber-based resins, silicone-based resins, urethane-based resins, polyamide resins, polyimide resins, polyester resins, and fluororesins. These resins may be used alone or in combination of two or more.

[0056] 2-2. Hardener As described above, the pressure-sensitive adhesive composition may contain a curing agent. Examples of the curing agent include an isocyanate compound, an epoxy compound, an aziridine compound, a carbodiimide compound, and a metal chelate. The curing agent may be a low molecular weight compound or a high molecular weight compound. When the functional group is a hydroxy group or a carboxy group, an isocyanate compound or an epoxy compound is preferred, and among these, an isocyanate compound is preferred from the viewpoint of achieving both high cohesive strength and adhesion.

[0057] Among isocyanate curing agents, aromatic-containing isocyanates are more preferred. By using a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer (a) and an aromatic-containing isocyanate curing agent, a better recovery rate can be obtained. From the viewpoint of compatibility between the (meth)acrylic copolymer (a) and the curing agent, an isocyanate curing agent (b) having an aromatic ring, such as an aromatic polyisocyanate or an aromatic aliphatic polyisocyanate, is preferred.

[0058] The isocyanate compound is an isocyanate having two or more isocyanate groups. The isocyanate compound is preferably, for example, an isocyanate monomer such as an aromatic polyisocyanate, an aliphatic polyisocyanate, an araliphatic polyisocyanate, or an alicyclic polyisocyanate, as well as a biuret, a nurate, or an adduct thereof.

[0059] Examples of aromatic polyisocyanates include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzene, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, and 4,4',4"-triphenylmethane triisocyanate.

[0060] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (also known as HDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0061] Examples of the aromatic aliphatic polyisocyanate include ω,ω'-diisocyanate-1,3-dimethylbenzene, ω,ω'-diisocyanate-1,4-dimethylbenzene, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.

[0062] Examples of alicyclic polyisocyanates include 3-isocyanatemethyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI, isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanatemethyl)cyclohexane.

[0063] The biuret form is a self-condensation product having a biuret bond formed by self-condensation of an isocyanate monomer, for example, a biuret form of hexamethylene diisocyanate.

[0064] The nurate form is a trimer of an isocyanate monomer, such as a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, or a trimer of tolylene diisocyanate.

[0065] The adduct is a bifunctional or higher isocyanate compound obtained by reacting an isocyanate monomer with a bifunctional or higher low-molecular active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, a compound obtained by reacting trimethylolpropane with isophorone diisocyanate, and a compound obtained by reacting 1,6-hexanediol with hexamethylene diisocyanate.

[0066] From the viewpoint of forming a sufficient crosslinked structure, the isocyanate compound is preferably a trifunctional isocyanate compound. The isocyanate compound is more preferably an adduct which is a reaction product between an isocyanate monomer and a trifunctional low molecular weight active hydrogen-containing compound, and a nurate. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a nurate of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, a nurate of tolylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, or a nurate of isophorone diisocyanate, and more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, or a trimethylolpropane adduct of isophorone diisocyanate.

[0067] Examples of epoxy compounds include glycerin diglycidyl ether, 1,6-hexanediol diglycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidylaminophenylmethane.

[0068] Examples of the aziridine compound include N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxite), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane.

[0069] The carbodiimide compound is preferably a high molecular weight polycarbodiimide produced by decarboxylation condensation of a diisocyanate compound in the presence of a carbodiimide catalyst. The commercially available high molecular weight polycarbodiimide is preferably the Carbodilite series from Nisshinbo Industries, Ltd. Among them, Carbodilite V-03, 07, and 09 are preferred because of their excellent compatibility with organic solvents.

[0070] The metal chelate is preferably a coordination compound of a polyvalent metal such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, or zirconium with acetylacetone or ethyl acetoacetate. Examples of the metal chelate include aluminum ethyl acetoacetate diisopropylate, aluminum trisacetylacetonate, aluminum bisethyl acetoacetate monoacetylacetonate, and aluminum alkyl acetoacetate diisopropylate.

[0071] The curing agent is preferably contained in an amount of 0.001 to 1 part by mass, more preferably 0.01 to 0.1 part by mass, based on 100 parts by mass of the (meth)acrylic copolymer (a). When the content is 0.001 part by mass or more, the cohesive strength is further improved, and when the content is 1 part by mass or less, it is preferable that both the cohesive strength and flexibility are easily achieved.

[0072] 2-3. Polymerization initiator The polymerization initiator is preferably a radical polymerization initiator. As the radical polymerization initiator, peroxides and azo compounds are suitable. Examples of the azo compound include 2,2'-azobisbutyronitrile such as 2,2'-azobisisobutyronitrile (abbreviation: AIBN) and 2,2'-azobis(2-methylbutyronitrile); 2,2'-azobisvaleronitrile such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); 2,2'-azobispropionitrile such as 2,2'-azobis(2-hydroxymethylpropionitrile); and 1,1'-azobis-1-alkanenitrile such as 1,1'-azobis(cyclohexane-1-carbonitrile). Examples of the peroxide include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(t-butylperoxy)hexyne-3; peroxy esters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; ketone peroxides such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, Examples of the peroxyketals include 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate; hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; and peroxydicarbonates such as bis(t-butylcyclohexyl)peroxydicarbonate.

[0073] 2-4.Hard Segment If necessary, the pressure-sensitive adhesive composition may contain a hard segment to form an island-type microphase separation structure in the pressure-sensitive adhesive layer. The hard segment has a higher Tg than the soft segment and is composed of non-crosslinked bead-like particles. Examples of the bead-like particles include (meth)acrylic resin, polystyrene resin, polyethylene resin, epoxy resin, and silicone resin. A resin that is highly compatible with the pressure-sensitive adhesive resin is preferred. From this viewpoint, it is suitable to use the same type of resin. From the viewpoint of compatibility, a combination of a (meth)acrylic resin as the hard segment and a (meth)acrylic copolymer (a) as the soft segment is preferred.

[0074] 2-5. Other additives The present pressure-sensitive adhesive composition may further contain a solvent, a tackifier, a silane coupling agent, a filler, a colorant, an antioxidant, an antistatic agent, an ultraviolet absorbing agent, and the like, as required.

[0075] Examples of the solvent include esters such as ethyl acetate, propyl acetate, and butyl acetate, and ketones such as acetone, methyl ethyl ketone, and cyclohexanone. In addition, examples of the solvent include aromatic hydrocarbons such as toluene, xylene, benzene, and solvent naphtha, and aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, ethylcyclohexane, diethylcyclohexane, decahydronaphthalene, bicycloheptane, tricyclodecane, hexahydroindenecyclohexane, cyclooctane, α-pinene, terpinolene, and limonene. The solvents may be used alone or in combination.

[0076] Examples of the tackifier include adhesive compounds having a weight-average molecular weight of 10,000 or less. Examples include rosin-based resins, polymerized rosin-based resins, rosin ester-based resins, polymerized rosin ester-based resins, terpene-based resins, terpene phenol-based resins, coumarone-based resins, coumarone-indene-based resins, styrene-based resins, xylene-based resins, phenol-based resins, and petroleum-based resins. Among these, rosin-based resins, polymerized rosin-based resins, rosin ester-based resins, and polymerized rosin ester-based resins are preferred, and rosin ester-based resins and polymerized rosin ester-based resins are more preferred, because they have good compatibility with the (meth)acrylic copolymer (a) and can further improve adhesive performance. The tackifier resin is preferably used in an amount of 0.01 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, per 100 parts by mass of the (meth)acrylic copolymer (a). High adhesive strength can be obtained by using 0.01 to 10 parts by mass of the tackifier resin.

[0077] Examples of the silane coupling agent include alkoxysilane compounds having a (meth)acryloxy group, such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyltripropoxysilane, 3-(meth)acryloxypropyltributoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; Alkoxysilane compounds having a vinyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltributoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane; alkoxysilane compounds having an amino group, such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltripropoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; alkoxysilane compounds having a mercapto group, such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropylmethyldiethoxysilane; alkoxysilane compounds having an epoxy group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltripropoxysilane, 3-glycidoxypropyltributoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; tetraalkoxysilane compounds such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane; Examples of the silane include 3-chloropropyltrimethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-decyltrimethoxysilane, n-decyltriethoxysilane, styryltrimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, hexamethyldisilazane, and silicone resins having alkoxysilyl groups in the molecule.

[0078] The silane coupling agent is preferably used in an amount of 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the (meth)acrylic copolymer (a).

[0079] The optical and mechanical properties can be adjusted by adding a filler, and examples of the filler include inorganic white pigments such as silica, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, and titanium dioxide.

[0080] 3. First release sheet and second release sheet The adhesive layer is sandwiched between the first release sheet and the second release sheet. Wa to We of the adhesive layer are also affected by the type of release layer of the release sheets of the adhesive layer, particularly the second release sheet. The release strength of the first release sheet 1 and the second release sheet 2 can be adjusted by a release treatment of the attachment surface of each release sheet with the adhesive layer. For example, the release strength can be adjusted by the type of release agent. The release strength can also be adjusted by the amount of release agent applied. The release strength can also be adjusted by the surface roughness of the release layer. The release strength can also be adjusted by the adhesive composition forming the adhesive layer. When it is desired to increase the release strength, it is effective to carry out treatments such as smoothing the surface roughness or increasing the amount of release agent applied, and when it is desired to decrease the release strength, the opposite can be done.

[0081] The first release sheet and the second release sheet can be arbitrarily selected, and the same release sheet may be used. From the perspective of handling, it is preferable that the first release sheet is a light release sheet and the second release sheet is a heavy release sheet. The thickness Tl of the light release sheet is in the range of 25 to 100 μm, the thickness of the heavy release sheet is in the range of 50 to 188 μm, and it is preferable to satisfy the relationship of Tl < Th. Also, when using an adhesive sheet roll, it is preferable to provide the light release sheet on the outer side of the roll.

[0082] The peeling force Pl when peeling the first release sheet from the adhesive layer at a peeling angle of 180° and a peeling speed of 300 mm / min in an environment of 23°C and a relative humidity of 50% can be adjusted as appropriate. However, from the perspective of effectively suppressing tunneling phenomena such as the lifting of the adhesive layer and partial peeling, it is preferably 0.02 to 0.30 N / 25 mm. Also, from the perspective of effectively suppressing the phenomenon of peeling between the adhesive layer and the second release sheet, after peeling the first release sheet from the adhesive layer, the peeling force Ph when further peeling the second release sheet from the adhesive layer at a peeling angle of 180° and a peeling speed of 300 mm / min in an environment of 23°C and a relative humidity of 50% is preferably in the range of 0.10 to 0.80 N / 25 mm in the range where Ph / Pl satisfies the range of 2 to 6 in relation to the peeling force Pl.

[0083] Examples of the first release sheet and the second release sheet include a polyethylene sheet, a polypropylene sheet, a polybutene sheet, a polybutadiene sheet, a polymethylpentene sheet, a polyvinyl chloride sheet, a vinyl chloride copolymer sheet, a polyethylene terephthalate sheet, a polyethylene naphthalate sheet, a polybutylene terephthalate sheet, a polyurethane sheet, an ethylene vinyl acetate sheet, an ionomer resin sheet, an ethylene·(meth)acrylic acid copolymer sheet, an ethylene·(meth)acrylate copolymer sheet, a polystyrene sheet, a polycarbonate sheet, a polyimide sheet, and a fluororesin sheet. The first release sheet may be a single layer or a laminate.

[0084] In addition to using a sheet having releasability for the first release sheet 1 and / or the second release sheet 2 themselves, releasability may be imparted by coating a release agent on the bonding surface with the adhesive layer 3. Examples of the release agent include a method of coating an alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, or wax-based release agent. The release force can be adjusted by changing the type of release agent.

[0085] The method of forming the release layer is preferably a method of forming the release layer by applying a release agent composition onto a release substrate. The release agent may contain a solvent when applied to form the release layer. The solvent is not particularly limited, but examples thereof include organic solvents such as hydrocarbon solvents such as normal hexane, cyclohexane, and normal heptane; aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate and methyl acetate; ketone solvents such as acetone and methyl ethyl ketone; and alcohol solvents such as methanol, ethanol, and butanol.

[0086] The release agent is applied by a microgravure coater, gravure coater, etc. The solid content of the release agent is 0.1 to 2.0 g / m 2 , preferably 0.5 to 1.2 g / m 2 The release layer can be formed by applying the coating material to a thickness of about 100 μm and curing the coating material.

[0087] As a curing method, heat curing is preferred in order to easily promote curing. The curing temperature is not particularly limited, but is preferably 80 to 130°C. If it is 80°C or higher, long-term heating is not required to sufficiently cure, and productivity is improved. If it is less than 130°C, the occurrence of wrinkles due to heat in the substrate or release substrate can be reduced. The thickness of the release layer is not particularly limited. For example, it is about 0.1 to 2 μm.

[0088] 4. Manufacturing of double-sided adhesive sheets The double-sided pressure-sensitive adhesive sheet of the present disclosure can be manufactured by a known method. For example, the double-sided pressure-sensitive adhesive sheet can be manufactured by a process of coating a pressure-sensitive adhesive composition on a second release sheet to form a coating film and curing the coating film to form a pressure-sensitive adhesive layer, and attaching a first release sheet to one exposed surface of the pressure-sensitive adhesive layer. The double-sided pressure-sensitive adhesive sheet thus obtained is then wound into a roll to obtain a roll sheet.

[0089] Coating can be performed, for example, by a microgravure coater, a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a rod blade coater, a knife coater, a spray coater, a die coater, or a curtain coater. If the adhesive composition contains a solvent, the solvent is removed by a drying process after coating. Curing is performed, for example, by aging. In the case of a photocurable adhesive composition, curing is performed by irradiating with UV or the like.

[0090] After or while the double-sided pressure-sensitive adhesive sheet is produced, the double-sided pressure-sensitive adhesive sheet is wound around a core into a roll to obtain a double-sided pressure-sensitive adhesive sheet roll. The winding length can be designed depending on the application. From the viewpoint of increasing productivity, it is preferably 50 m or more, and more preferably 100 m or more. From the viewpoint of production yield, the winding length is preferably 2500 m or less.

[0091] Alternatively, the adhesive layer may be applied to the release surfaces of the first and second release sheets so that the thickness after drying is a specified thickness, thereby forming two adhesive layers, and then the adhesive layers may be attached to each other to produce the adhesive sheet.

[0092] 5.Laminate for image display device In the laminate for image display devices of the present disclosure, adherends are bonded to each other via the adhesive layer of the double-sided adhesive sheet. The laminate for image display devices of the present disclosure is formed using a substrate-free double-sided adhesive sheet that can suppress wrinkles and bubbles even when applied to flexible display applications, and is therefore suitable for optical elements such as liquid crystal elements and organic EL elements that require visibility. Flexible displays are bendable displays, and examples of such displays include organic electroluminescence (organic EL) displays, electrophoretic displays (electronic paper), liquid crystal displays using a plastic substrate (film) as a substrate, and foldable displays that can be folded.

[0093] The adhesive layer formed from this adhesive sheet is suitable for bonding bendable members (adherends) together. For example, it is suitable for bonding any combination of members such as liquid crystal polymer sheets, light-emitting polymer sheets, sheet-like liquid crystal modules, organic EL modules (organic EL sheets), electronic paper modules, transparent conductive sheets, metal mesh sheets, sheet sensors, cover sheets, barrier films, polarizing films, polarizers, retardation films, viewing angle compensation films, brightness improvement films, contrast improvement films, diffusion films, semi-transmissive reflective films, and electrode films. EXAMPLES

[0094] The present disclosure will be described in more detail below based on examples. However, the present disclosure is not limited to these. Unless otherwise specified, "parts" in the examples indicate "parts by mass" and "%" indicates "% by mass". Blanks in the tables indicate that no ingredients are blended.

[0095] (a)Measurement method The values ​​obtained in this example were obtained by the following method. a-1. Tg of (meth)acrylic copolymer (a) The Tg of the adhesive resin was measured by a robot DSC (differential scanning calorimeter, Seiko Instruments' "RDC220"). Approximately 2 mg of the sample was placed in an aluminum pan, weighed, and set in the differential scanning calorimeter. The sample was held at 100°C for 5 minutes, using the same type of aluminum pan without the sample as a reference, and then rapidly cooled to -120°C using liquid nitrogen. The temperature was then increased at a rate of 5°C / min, and the Tg (°C) of the adhesive resin was determined from the obtained DSC chart.

[0096] a-2. Tg of adhesive layer The first and second release sheets were peeled off from the double-sided PSA sheets of each of the Examples and Comparative Examples produced by the method described below, and 2 mg of the adhesive layer was placed in an aluminum pan, weighed, and set in a differential scanning calorimeter. Using an aluminum pan of the same type without a sample as a reference, the sheets were held at 100°C for 5 minutes and then rapidly cooled to -120°C using liquid nitrogen. The temperature was then increased at a rate of 5°C / min, and the Tg (°C) of the adhesive resin was determined from the resulting DSC chart.

[0097] a-3. Weight average molecular weight Mw and molecular weight dispersity Mw / Mn of adhesive resin Mw was measured using a GPC "LC-GPC system" manufactured by Shimadzu Corporation, and Mw and molecular weight dispersity Mw / Mn were calculated by conversion using polystyrene of known molecular weight as a standard substance. Device name: Shimadzu Corporation, LC-GPC system "Prominence" Column: Four GMHXL columns manufactured by Tosoh Corporation and one HXL-H column manufactured by Tosoh Corporation were connected together. Mobile phase solvent: Tetrahydrofuran Flow rate: 1.0mL / min Column temperature: 40℃

[0098] a-4. Thickness of double-sided adhesive sheet Tt, thickness of adhesive layer Ta, thickness of first release sheet Tl, thickness of second release sheet Th Ten equally spaced locations were determined from one end to the other end in the width direction of the double-sided adhesive sheet (first release sheet / adhesive layer / second release sheet), and the thicknesses of the ten locations were measured, and the average value was taken as Tt. The end refers to the end of the region where the first release sheet / adhesive layer / second release sheet are laminated. Next, the first release sheet was peeled off from the double-sided adhesive sheet, and the thicknesses of the peeled first release sheet at the ten locations corresponding to the same positions as described above were measured. The average value was taken as Tl. Then, the second release sheet was peeled off from the adhesive layer, and the thicknesses of the peeled second release sheet at the ten locations corresponding to the same positions as described above were measured. The average value was taken as Th. The thickness Ta of the adhesive layer was calculated by Tt-Tl-Th. In addition, for Reference Example 1 described later, the thickness Tt of the single-sided adhesive sheet was measured in the same manner as the double-sided adhesive sheet, the thickness Tl of the release sheet was measured in the same manner as the first release sheet, and the thickness Th of the base film was measured in the same manner as the second release sheet by removing the adhesive layer from the base film using any solvent.

[0099] a-5. Measurement of the reflection intensity Wa~We of the adhesive layer A glass plate (blue plate glass, manufactured by Kawamura Kyuzo Shoten Co., Ltd.) measuring 200 mm in width, 120 mm in length, and 1.1 mm in thickness was attached to the surface of the adhesive layer exposed by peeling off the first release sheet of the double-sided adhesive sheet cut to a width of 20 mm and a length of 200 mm, and the glass plate was placed on thick white drawing paper (P156J, manufactured by Jointex Co., Ltd.) to prepare a measurement sample. The surface of the adhesive layer exposed by peeling off the second release sheet of the measurement sample was scanned for 150 mm or more in the length direction using a wave-scan device (manufactured by BYK Gardner Co., Ltd., wave-scan 3dual), to measure Wa to We. In addition, for Reference Example 1, the film substrate was placed on the glass plate having a thickness of 1 mm, and the glass plate was placed on the white drawing paper (thick) to prepare the measurement sample, but the measurement was performed in the same manner as in Example 1.

[0100] a-6. Measurement of solid content The mass of the aluminum cup (W0) was measured using a precision balance. Next, about 1 g of the sample solution was placed in the aluminum cup, and the mass of the sample in the aluminum cup (W1) was measured using a precision balance. The sample in the aluminum cup was heated in an oven at 150°C for 2 hours, then removed from the oven and allowed to return to room temperature. The residual mass (W2) of the sample in the aluminum cup after heating was measured using a precision balance. The solid content was then calculated using the formula (W2-W0) / (W1-W0)×100(%).

[0101] a-7.Storage modulus Two sets of sheets were prepared by peeling off the first release sheet of the double-sided adhesive sheet, and the adhesive layers were bonded together with a laminator to prepare a laminate of a second release sheet / adhesive layer / second release sheet. The second release sheet on one side of this laminate was peeled off, and the adhesive layers were sequentially bonded together to form a laminate of adhesive layers with a thickness of 1 mm. The storage modulus G' of this laminate was measured using a rheometer (manufactured by TA Instruments, DHR-2) with a φ8 mm measurement probe under conditions of a strain of 0.1%, a frequency of 1 Hz, and a heating rate of 10°C / min from -70°C to 200°C. From the obtained data, the measured values ​​at each temperature of 0°C, 23°C, and 40°C were read.

[0102] a-8. Measurement of gel fraction The double-sided adhesive sheet was cut into a size of 30 mm x 100 mm, the first release sheet was peeled off, and the exposed adhesive layer was attached to a weighed 300 mesh stainless steel wire mesh (mass W0), and the second release sheet was peeled off to obtain a sample. The weight of this sample was W1. The sample was then left to stand in ethyl acetate for 24 hours, and then dried at 100°C for 1 hour. The weight of the sample was then W2. The gel fraction was calculated from the following formula. Gel fraction (%) = {(W2-W0) / (W1-W0)} x 100

[0103] (b) Production Example of (Meth)acrylic Copolymer (a) b-1. (Meth)acrylic copolymer (R1) A reaction vessel (hereinafter simply referred to as "reaction vessel") equipped with a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube was charged with 80 parts of ethyl acetate (EtAc), 30 parts of butyl acrylate (BA), 35 parts of 2-ethylhexyl acrylate (2EHA), 30 parts of isobornyl acrylate (IBXA), 5 parts of 4-hydroxybutyl acrylate (4HBA), and 0.1 parts of 2,2'-azobisisobutyronitrile (hereinafter simply referred to as "AIBN") as an initiator, and the atmosphere in the reaction vessel was replaced with nitrogen gas. Then, the mixture was heated to 65°C while stirring under a nitrogen atmosphere to start the reaction. The reaction solution was then reacted at 65°C for 4 hours. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate (EtAc) to obtain a (meth)acrylic copolymer (R1) solution with a solid content of 50%. The Mw of the obtained copolymer (R1) was 1 million and the Tg was -39°C.

[0104] Except for changing the compositions and blending amounts (parts by mass) to those shown in Table 1, the (meth)acrylic copolymers (R2 to R7) were produced in the same manner as in the production of the (meth)acrylic copolymer (R1). [Table 1]

[0105] The abbreviations in the table are as follows. (Linear or branched (meth)acrylic acid alkyl ester monomer) MA: Methyl acrylate (alkyl group carbon number 1) BA: n-butyl acrylate (alkyl group carbon number: 4) 2EHA: 2-ethylhexyl acrylate (alkyl group carbon number: 8) 2EHMA: 2-ethylhexyl methacrylate (alkyl group carbon number: 8) DOA: Dodecyl acrylate (alkyl group carbon number: 12) (Other monomers) IBXA: Isobornyl acrylate CHA: Cyclohexyl acrylate AA: Acrylic acid 4HBA: 4-hydroxybutyl acrylate

[0106] (c) Preparation of Pressure Sensitive Adhesive Composition c-1. Preparation of adhesive composition C1 A (meth)acrylic copolymer (R1 (based on 100 parts of solid content) was mixed with 0.1 part of xylylene diisocyanate (XDI) (Takenate D-110N, manufactured by Mitsui Chemicals) as a curing agent, 0.1 part of a silane coupling agent (KBM-303, manufactured by Shin-Etsu Silicones) as an additive, and ethyl acetate (EtAc) to give a solid content of 25%, followed by stirring to obtain a pressure-sensitive adhesive composition C1.

[0107] c-2. Production of Pressure Sensitive Adhesive Compositions C2 to C11 Pressure-sensitive adhesive compositions C2 to C11 were obtained in the same manner as for pressure-sensitive adhesive composition C1, except that the types of (meth)acrylic copolymer, curing agent, and additives were changed as shown in Table 2. The solid content of C3 was appropriately adjusted in accordance with the examples described later. [Table 2]

[0108] The abbreviations in the table are as follows. (hardening agent) XDI: Xylylene diisocyanate (Takenate D-110N, manufactured by Mitsui Chemicals) TDI: Toluene diisocyanate (Cosmonate T100, manufactured by Mitsui Fine Chemicals) HDI: Hexamethylene diisocyanate (adduct of trimethylolpropane) (Takenate D-160N, manufactured by Mitsui Chemicals) EP: Epoxy hardener (E-5XM, manufactured by Soken Chemical Industries, Ltd.) SC: Silane coupling agent (KBM-303, Shin-Etsu Silicone Co., Ltd.) TF: Tackifier (D-125, manufactured by Arakawa Chemical Industries Co., Ltd.)

[0109] (d) Manufacturing example of double-sided adhesive sheet d-1. Example 1 The adhesive composition C1 was applied to the release layer of a second release sheet (heavy release polyethylene terephthalate separator) having a thickness of 75 μm and a width of 30 cm at a speed of 10 m / min using a die coater so that the adhesive layer after drying had a thickness of 50 μm and a width of 20 cm, and then dried in a hot air oven at 120 ° C. for 2 minutes to form an adhesive layer. Next, the release layer of a first release sheet (light release polyethylene terephthalate separator) having a thickness of 50 μm and a width of 30 cm was attached to this adhesive layer to prepare a double-sided adhesive sheet. The obtained double-sided adhesive sheet was wound up to a length of 50 m at a tension of 50 N while being careful not to wrinkle the ABS core having a diameter of 3 inches, to prepare a roll-shaped double-sided adhesive sheet. The roll-shaped double-sided adhesive sheet prepared was aged for one week under conditions of a temperature of 40 ° C. and a relative humidity of 50%. The roll was then unwound from the outer side, and starting from a position 5 m unwound, a further 50 cm was unwound in the longitudinal direction and cut out to obtain an outer-wound double-sided PSA sheet measuring 30 cm wide and 50 cm long. Separately, starting from a position 5 m from the end of the double-sided adhesive sheet on the inner side (core side) of the roll, a section was cut out extending 50 cm in the longitudinal direction toward the outer side, obtaining an inwardly wound double-sided adhesive sheet measuring 30 cm wide and 50 cm in the longitudinal direction.

[0110] d-2. Examples 2 to 35 and Comparative Examples 1 to 6 Double-sided pressure-sensitive adhesive sheets according to Examples 2 to 35 and Comparative Examples 1 to 6 were obtained in the same manner as in Example 1, except that the pressure-sensitive adhesive compositions and coating conditions were changed as shown in Tables 3 to 5.

[0111] d-3. Reference example 1 The adhesive composition C9 was applied to the release layer of a release film (BX8A, manufactured by Toray Film Processing Co., Ltd.) having a thickness of 75 μm and a width of 30 cm at a speed of 10 m / min using a die coater so that the thickness after drying was 50 μm and the width was 20 cm, and the adhesive layer was formed by drying for 2 minutes in a hot air oven at 120 ° C. Next, a film substrate (U403, manufactured by Toray Industries, Inc.) having a thickness of 23 μm and a width of 30 cm was laminated to this adhesive layer to prepare a single-sided adhesive sheet. The obtained single-sided adhesive sheet with the substrate was wound up to a length of 50 m at a tension of 50 N while being careful not to wrinkle the ABS core having a diameter of 3 inches, to prepare a roll-shaped single-sided adhesive sheet. The prepared roll-shaped single-sided adhesive sheet was aged for one week under conditions of a temperature of 40 ° C. and a relative humidity of 50%. Thereafter, an outer-wound single-sided adhesive sheet and an inner-wound single-sided adhesive sheet were obtained in the same manner as in Example 1.

[0112] (e) Evaluation of double-sided adhesive sheets, etc. The double-sided PSA sheets of each of the Examples and Comparative Examples and the single-sided PSA sheet of the Reference Example were evaluated as follows. The results are shown in Tables 3 to 5. In these Examples and Comparative Examples, the first release sheet was a so-called light release sheet, and the second release sheet was a so-called heavy release sheet. e-1. Visibility evaluation The outer-wrapped double-sided adhesive sheet of each Example and Comparative Example was cut to 80 mm x 40 mm, the first release sheet was peeled off, and the sheet was attached to a glass plate. The second release sheet was then peeled off, and the sheet was attached to an organic EL module (manufactured by TAYDEC, REC001602A-W) to form a display. The display displayed white characters (32 characters in total, including capital letters A to P and small letters a to p) on a black background, and was placed on a horizontal table. The observer observed the display light from three angles: an angle 30° above the horizontal, an angle 45° above the horizontal, and an angle 90° above the vertical. The observer visually compared and evaluated the distortion and blurring of the image displayed on the display before and after the application of the double-sided adhesive sheet. For Reference Example 1, the release sheet was peeled off, and the film was attached to an organic EL module (REC001602A-W manufactured by TEIDEC Co., Ltd.), and a glass plate was placed on the substrate film to form a display. Except for this, the film was evaluated in the same manner as in Example 1. The evaluation criteria were as follows: 3 or above is good, and 2 is practical. 5: No distortion or blurring of edges is observed under any angle conditions. 4: Slight distortion and / or blurring of edges is observed under any one of the angle conditions. 3: Some distortion and / or blurring of edges is observed under any two angle conditions. 2: There is some distortion and / or blurring of the edges under all angle conditions, but this does not cause any problems in practical use. 1: Under one or more angle conditions, distortion and / or blurring of edges is observed beyond the range of "slight," making many characters difficult to distinguish. In the above, "slight" means that two or fewer characters out of 32 are difficult to read due to distortion or blurred outlines.

[0113] e-2. Evaluation of air bubbles and wrinkles (roll) An arbitrary portion of the inwardly wrapped double-sided PSA sheet of each of the Examples, Comparative Examples, and Reference Examples was cut into four 10 cm square pieces, and the presence or absence of air bubbles and wrinkles resulting from storage in a roll was visually observed. The evaluation criteria are as follows: 3 or above is good, and 2 is practical. 5: No air bubbles or wrinkles larger than 1 mm are found on any of the four double-sided adhesive sheets. 4: No air bubbles or wrinkles larger than 1 mm are found on the three double-sided adhesive sheets. 3: No air bubbles or wrinkles larger than 1 mm are found on the two double-sided adhesive sheets. 2: No air bubbles or wrinkles larger than 1 mm are found on one double-sided adhesive sheet. 1: All double-sided adhesive sheets have air bubbles and wrinkles larger than 1 mm.

[0114] e-3. Evaluation of air bubbles and wrinkles (folding) The first release sheet was peeled off from the outer double-sided pressure-sensitive adhesive sheet of each of the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was laminated onto a polyimide film. The second release sheet was then peeled off from the adhesive layer, and the exposed adhesive layer was laminated onto an easy-adhesion PET film. The laminate was placed in an autoclave and held at 50°C for 20 minutes. The laminate was then removed and left at 25°C and 50% RH for 30 minutes, after which it was cut into a size of 70 mm wide and 100 mm long to obtain a test laminate consisting of an easy-adhesion PET film / adhesive layer / polyimide. Next, the test laminate was subjected to 200,000 cycles of bending and twisting in a planar body no-load tester (manufactured by Yuasa System Co., Ltd.) at 23°C and 50% RH. One cycle was defined as the time from bending to returning to the original state before bending. The test was performed with N=5, and the appearance after the test was evaluated visually. Reference Example 1 was evaluated in the same manner as Example 1, except that the release sheet was peeled off to obtain an adhesive layer with a film substrate, and the exposed adhesive layer was laminated to a polyimide film. The evaluation criteria were as follows. 5: No bubbles or wrinkles are observed in any of the 5 samples. Air bubbles and / or wrinkles were observed in the 4:1 sample. 3: Air bubbles and / or wrinkles were observed in the 2 sample. In the 2:3 sample, bubbles and / or wrinkles were observed. Air bubbles and / or wrinkles were observed in the 1:4 sample or in all samples. The evaluation of bubbles and wrinkles (folding) was carried out in the same manner, except that the temperature was changed from 23° C. to 0° C. and 40° C. The evaluation criteria were the same as for 23° C.

[0115] [Table 3]

[0116] [Table 4]

[0117] [Table 5]

[0118] Double-sided pressure-sensitive adhesive sheets that do not satisfy both the reflection intensity Wa of 1 to 26 and the reflection intensity Wd of 0.3 to 8 were found to have problems with reduced visibility and air bubbles and wrinkles, as shown in Comparative Examples 1 to 4. Double-sided pressure-sensitive adhesive sheets that satisfy both the reflection intensity Wa of 1 to 26 and the reflection intensity Wd of 0.3 to 8 but whose adhesive layer does not satisfy the above (i) to (iii) were found to have problems with air bubbles and wrinkles (folding), as shown in Comparative Examples 5 to 6. In contrast, double-sided pressure-sensitive adhesive sheets that satisfy both the reflection intensity Wa of 1 to 26 and the reflection intensity Wd of 0.3 to 8 and whose adhesive layer satisfies the above (i) to (iii) were found to have excellent visibility and suppressed wrinkles and air bubbles, as shown in Examples 1 to 35. [Explanation of symbols]

[0119] 1: First release sheet 2: Second release sheet 3: Adhesive layer 4: Glass substrate 5: Blank paper 10: Double-sided adhesive sheet 31, 32: Surface

Claims

1. A double-sided PSA sheet for use in substrate-less flexible displays, comprising a first release sheet, a pressure-sensitive adhesive layer, and a second release sheet laminated in this order, The first release sheet is peeled off to expose the surface of the adhesive layer, a glass substrate is attached to the surface, the glass substrate is placed on a white paper, and the second release sheet is peeled off to expose the surface of the adhesive layer. When the surface is measured with a wavescan device, The reflection intensity Wa in the wavelength range of 0.1 to 0.3 mm is 1 to 26, and The reflection intensity Wd in the wavelength range of 3 to 10 mm is 0.3 to 8, The adhesive layer is (i) either an adhesive layer containing a (meth)acrylic copolymer (a) having a weight average molecular weight of 1,000,000 to 1,800,000, or an adhesive layer obtained by crosslinking an adhesive composition containing the (meth)acrylic copolymer (a); (ii) A storage modulus at 23° C. of 1×10 3 ~8×10 4 Pa, (iii) The glass transition temperature as determined by DSC is −70° C.≦Tg≦−35° C. Double-sided adhesive sheet.

2. The first release sheet is peeled off to expose the surface of the adhesive layer, a glass substrate is attached to the surface, the glass substrate is placed on a white paper, and the second release sheet is peeled off to expose the surface of the adhesive layer. When the surface is measured with a wavescan device, The reflection intensity Wc in the wavelength range of 1 to 3 mm is 1 to 12, and 2. The double-sided pressure-sensitive adhesive sheet according to claim 1, which has a reflection intensity We of 1 to 12 in a wavelength range of 10 to 30 mm.

3. The double-sided pressure-sensitive adhesive sheet according to claim 1, wherein the (meth)acrylic copolymer (a) has a structural unit derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 6 carbon atoms, and a structural unit derived from a linear or branched (meth)acrylic acid alkyl ester monomer having an alkyl group with 7 to 12 carbon atoms.

4. 2. The double-sided pressure-sensitive adhesive sheet according to claim 1, wherein the (meth)acrylic copolymer (a) has a molecular weight dispersity Mw / Mn of less than 5.

5. A laminate for an image display device, comprising adherends bonded together via the adhesive layer of the double-sided adhesive sheet of any one of claims 1 to 4.

Citation Information

Patent Citations

  • Coating method and coated body obtained by the method

    JP2017023941A

  • Adhesive for flexible displays, adhesive sheet, flexible laminated member, and flexible display

    JP2018045213A

  • Protective sheet

    JP2018172611A

  • Laminate sheet

    JP2020083908A

  • Optical adhesive sheet for foldable device

    JP2022116860A