Nitride semiconductor element

By employing AlN substrates with AlxGa1-xN films within specific thickness ranges, the nitride semiconductor devices address corrosion, lattice relaxation, and wafer cracking issues, enhancing reliability and efficiency.

JP2024158778AInactive Publication Date: 2024-11-08ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023074298
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing nitride semiconductor devices face issues with corrosion, lattice relaxation, wafer cracking, and reduced optical output due to the use of AlGaN films on AlN substrates, which affect their long-term reliability and manufacturing efficiency.

Method used

The use of AlN substrates with specific film thickness ranges for AlxGa1-xN layers, ranging from 0.5 to 15 μm, to suppress corrosion, lattice relaxation, and prevent wafer cracking, while optimizing optical output and driving voltage.

Benefits of technology

The proposed solution enhances the long-term reliability of nitride semiconductor devices by preventing corrosion, reducing lattice relaxation, and minimizing wafer cracking, thereby improving manufacturing efficiency and optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158778000001_ABST
    Figure 2024158778000001_ABST
Patent Text Reader

Abstract

To provide a nitride semiconductor element capable of suppressing the progress of corrosion.SOLUTION: A nitride semiconductor element includes a first conductivity type semiconductor layer formed of AlxGa1-xN (0.8≤x≤1) disposed on an AlN substrate. The film thickness β [μm] of the first conductivity type semiconductor layer satisfies 0.5<β<15 in at least a portion of the region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitride semiconductor device. [Background technology]

[0002] A method for growing AlGaN, which is a group III nitride, on a sapphire substrate as a nitride semiconductor element is disclosed in Non-Patent Document 1. Furthermore, prior art related to light-emitting elements is disclosed in, for example, Patent Documents 1 to 3. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6621990 [Patent Document 2] JP 2022-117299 A [Patent Document 3] JP 2020-1550252 A [Non-patent literature]

[0004] [Non-Patent Document 1] Applied Physics Express, 12, 012008, 2019 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a nitride semiconductor element capable of suppressing the progress of corrosion from the viewpoint of maintaining the long-term reliability of the nitride semiconductor element. [Means for solving the problem]

[0006] In one embodiment of the present invention, an AlN substrate is x Ga 1-xThe present invention provides a nitride semiconductor device having a first conductive type semiconductor layer formed of N (0.8≦x≦1), the film thickness β [μm] of the first conductive type semiconductor layer satisfying 0.5<β<15 in at least a portion of the region. Effect of the Invention

[0007] According to the present invention, it is possible to provide a nitride semiconductor device capable of suppressing the progress of corrosion. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view showing a nitride semiconductor device according to Example 1 of an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a nitride semiconductor device according to Example 2 of the embodiment of the present invention. [Diagram 3] FIG. 3 is a graph showing the experimental results regarding cracks and warpage. [Figure 4] FIG. 4 is a graph showing the results of a simulation of the relationship between the wafer thickness [μm] and the optical output. [Diagram 5] FIG. 5 is a graph showing the results of a simulation of the relationship between the film thickness [μm] of n-AlxGa1-xN (0.8≦x≦1) and the driving voltage Vf [V]. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described below through embodiments of the invention, but the following embodiments do not limit the scope of the invention according to the claims. Furthermore, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.

[0010] The definitions of directions such as up and down in the following description are merely for the convenience of explanation and do not limit the technical idea of ​​the present invention. For example, if an object is rotated 90 degrees and observed, up and down are converted to left and right and read, and if it is rotated 180 degrees and observed, up and down are reversed and read.

[0011] In the following description, directions may be described using the terms X-axis, Y-axis, and Z-axis. For example, the X-axis and Y-axis directions are parallel to the surface of the AlN substrate 1 (i.e., the surface on which the AlN_HOMO layer 3 is formed), which will be described later. The Z-axis direction is the thickness direction of the AlN substrate 1, and is the normal direction to the surface of the AlN substrate 1. The X-axis, Y-axis, and Z-axis directions are perpendicular to each other.

[0012] First Embodiment The nitride semiconductor device according to the first embodiment is an AlN substrate. x Ga 1-x The first conductive type semiconductor layer is made of AlN (0.8≦x≦1). In the following description, the first conductive type semiconductor layer is made of Al x Ga 1-x N (0.8≦x≦1). The first conductive type semiconductor layer, i.e., Al x Ga 1-x The film thickness β [μm] of N (0.8≦x≦1) is 0.5<β<15 in at least a part of the region.

[0013] The inventors have investigated the AlN substrate under high temperature and high humidity conditions. x Ga 1-x The corrosive properties of Al were investigated. x Ga 1-x It was discovered that the higher the Al content in N, the more likely corrosion occurs. For example, n-type (hereafter, n-) Al 0.7 Ga 0.3 Nitride semiconductor elements using N have high Al composition even under high temperature and high humidity conditions where corrosion does not occur. x Ga 1-x It was discovered that corrosion occurs in nitride semiconductor elements using N (0.8≦x≦1).

[0014] The inventors also investigated the n-AlN substrate x Ga 1-x Corrosiveness of N (0.8≦x≦1) and n-Al placed on AlN substrate x Ga 1-xThe inventors found that there is a correlation between the thickness β [μm] of n-Al (0.8≦x≦1) and the thickness β of n-Al. x Ga 1-x N (0.8≦x≦1) is easily corroded, and when the film thickness β is 0.5 [μm] or more, Al x Ga 1-x It was discovered that N (0.8≦x≦1) is resistant to corrosion.

[0015] In addition, n-Al x Ga 1-x The n-AlN (0.8≦x≦1) film can be formed, for example, by an MOCVD apparatus. The MOCVD apparatus includes a susceptor for holding an AlN substrate and a shower head for supplying source gas to the AlN substrate held by the susceptor. x Ga 1-x We found that by setting the film thickness β [μm] of N (0.8≦x≦1) to an appropriate value, clogging of the shower head and particle deposition on the susceptor can be suppressed. For example, we found that when the film thickness β is less than 15 [μm], clogging of the shower head and particle deposition on the susceptor can be suppressed.

[0016] Based on the above findings, the nitride semiconductor device according to the first embodiment is x Ga 1-x By setting the thickness β [μm] of N (0.8≦x≦1) to a value in the range of 0.5<β<15 in at least a part of the region, the Al x Ga 1-x The corrosion of N (0.8≦x≦1) can be suppressed. This improves the long-term reliability of the nitride semiconductor device. x Ga 1-x This can prevent clogging of the shower head of the device for depositing a N (0.8≦x≦1) film and particle deposition on the susceptor, thereby reducing the frequency of maintenance of the film deposition device and reducing the manufacturing costs of nitride semiconductor devices.

[0017] <Embodiment 2> The nitride semiconductor device according to the second embodiment is an AlN substrate. x Ga 1-x N (0.8≦x≦1). x Ga 1-x The film thickness β [μm] of N (0.8≦x≦1) is 0.5<β<10 in at least a part of the region.

[0018] The inventors have developed an AlN substrate x Ga 1-x We have investigated the lattice relaxation of the multiple quantum well (MQW) structure, i.e., the light-emitting layer, on AlN. x Ga 1-x We discovered that by setting the N film thickness in an appropriate range, the lattice relaxation of the MQW structure can be suppressed.

[0019] For example, n-Al 0.87 Ga 0.13 In nitride semiconductor devices using N, n-Al 0.87 Ga 0.13 When the N film thickness is 10 μm or more, n-Al 0.87 Ga 0.13 They discovered that N does not undergo lattice relaxation, but in the MQW structure (light-emitting layer) placed on top of it, the lattice constant of AlN is relaxed by 30%. If lattice relaxation occurs in the MQW structure, for example, the threading dislocation density may increase, resulting in a decrease in light emission efficiency.

[0020] In addition, the present inventors have 0.87 Ga 0.13 When the N film thickness is 0.5 [μm] and 3 [μm], n-Al 0.87 Ga 0.13 They discovered that N does not relax, and that the MQW structure placed on it also does not relax. They discovered that the lattice relaxation of the MQW can be suppressed by setting the film thickness of the n-AlGaN in an appropriate range.

[0021] Based on the above findings, the nitride semiconductor device according to the second embodiment is x Ga 1-xBy setting the thickness β [μm] of N (0.8≦x≦1) to a value in the range of 0.5<β<10 in at least a part of the region, the Al x Ga 1-x N (0.8≦x≦1), the lattice relaxation of the MQW structure disposed on the N (0.8≦x≦1) can be suppressed. As a result, for example, the threading dislocation density of the MQW structure (light emitting layer) can be reduced to 1e7 / cm 2 It is possible to set the value to a smaller value, and the decrease in the luminous efficiency can be suppressed.

[0022] In addition, in at least a partial region of the nitride semiconductor device according to the second embodiment, Al x Ga 1-x The range of the film thickness β [μm] of N (0.8≦x≦1) satisfies the range described in the first embodiment. Therefore, the nitride semiconductor device according to the second embodiment also exhibits the effects of the first embodiment (inhibition of the progress of corrosion and inhibition of particle deposition).

[0023] <Embodiment 3> The nitride semiconductor device according to the third embodiment is an AlN substrate. x Ga 1-x N (0.8≦x≦1). The thickness α [μm] of the AlN substrate and the x Ga 1-x The film thickness β [μm] of N (0.8≦x≦1) satisfies all of the following conditions at least in a part of the region: 96<α<600, 0.5<β<10, β<0.026α+0.848.

[0024] The inventors have developed an AlN substrate x Ga 1-x It was discovered that in the manufacturing process of nitride semiconductor devices containing N, when the wafer is fixed with a vacuum chuck or the like, especially in the post-process such as dicing, cracks are likely to occur in the wafer. In lattice strain type nitride semiconductor devices using an AlN substrate, for example, the AlN substrate needs to be thinned to improve the light extraction efficiency. However, when the back surface of the wafer (AlN substrate) is ground and polished to make it thinner in order to improve the light extraction efficiency and increase the output, wafer warping tends to become noticeable. When a warped wafer is fixed with a vacuum chuck or the like, wafer cracks are likely to occur.

[0025] Therefore, the present inventors have conducted extensive research into the conditions under which wafer warpage and wafer cracking occur in nitride semiconductor devices using AlN substrates. x Ga 1-x We found that when the thickness of the AlN (0.8≦x≦1) film is 2 μm or less, the wafer is severely warped. x Ga 1-x We discovered that by setting the film thickness of N (0.8≦x≦1) to an appropriate value, it is possible to prevent wafer cracking during subsequent processes such as dicing.

[0026] From the above findings, the nitride semiconductor device according to the third embodiment has a thickness α [μm] of the AlN substrate and x Ga 1-x By setting the film thickness β [μm] of N (0.8≦x≦1) to a value in the range that satisfies all of the following conditions, at least in a portion of the region: 96<α<600, 0.5<β<10, β<0.026α+0.848, it is possible to prevent cracking of the wafer (AlN substrate) in later processes such as dicing.

[0027] In addition, in at least a partial region of the nitride semiconductor device according to the third embodiment, Al x Ga 1-x The range of the film thickness β [μm] of N (0.8≦x≦1) satisfies the range described in the second embodiment. Therefore, the nitride semiconductor device according to the third embodiment also exhibits the effects of the first and second embodiments (inhibition of the progress of corrosion, inhibition of particle deposition, and inhibition of lattice relaxation of MQW).

[0028] In addition, in the lattice relaxed system using a sapphire substrate, there is no need to thin the wafer by grinding and polishing it, because sapphire transmits light. The process of thinning the wafer by grinding and polishing it is a process specific to the lattice strained system using an AlN substrate.

[0029] <Fourth embodiment> The nitride semiconductor device according to the fourth embodiment is an AlN substrate.x Ga 1-x N (0.8≦x≦1). The thickness α [μm] of the AlN substrate and the x Ga 1-x The film thickness β [μm] of N (0.8≦x≦1) satisfies all of the following conditions at least in a part of the region: 96<α<200, 0.5<β<0.026α+0.848.

[0030] Unlike a sapphire substrate that transmits light, an AlN substrate absorbs light. Therefore, in order to improve the light output (light intensity), it is necessary to grind and polish the AlN substrate to make it thinner. x Ga 1-x We investigated the relationship between the thickness of the AlN substrate and the optical output in nitride semiconductor devices containing N. As a result, we found that the optical output decreases as the thickness of the AlN substrate increases, and for example, when the thickness of the AlN substrate is 200 μm or more, the optical output is reduced by half compared to when the thickness of the AlN substrate is close to zero (see Figure 4 below).

[0031] From the above, the nitride semiconductor device according to the fourth embodiment has a thickness α [μm] of the AlN substrate and x Ga 1-x By setting the film thickness β [μm] of N (0.8≦x≦1) to a value within the range that satisfies all of 96<α<200 and 0.5<β<0.026α+0.848 in at least a portion of the region, it is possible to suppress a decrease in light output.

[0032] In addition, in at least a part of the region of the nitride semiconductor device according to the fourth embodiment, the thickness α [μm] of the AlN substrate and the Al x Ga 1-x Each range of the film thickness β [μm] of N (0.8≦x≦1) satisfies the range described in the third embodiment. Therefore, the nitride semiconductor device according to the fourth embodiment also exhibits the effects of the first to third embodiments (inhibition of the progress of corrosion, inhibition of particle deposition, inhibition of lattice relaxation of MQW, and prevention of wafer cracking).

[0033] <Fifth embodiment> The nitride semiconductor device according to the fifth embodiment is an AlN substrate. x Ga 1-x N (0.8≦x≦1). The thickness α [μm] of the AlN substrate and the x Ga 1-x The film thickness β [μm] of N (0.8≦x≦1) satisfies all of the following conditions at least in a part of the region: 96<α<200, 4≦β<0.026α+0.848.

[0034] AlN substrate with high Al content x Ga 1-x When depositing N, Al x Ga 1-x The sheet resistance of N is very high. When a nitride semiconductor element is used as a lateral light emitting element, if the sheet resistance is high, the resistance component of the entire nitride semiconductor element increases, and the driving voltage for driving the nitride semiconductor element increases. In addition, if the sheet resistance is high, current tends to concentrate at the mesa end, which creates a new problem of reduced reliability. The thicker the film, the smaller the sheet resistance. In order to reduce the sheet resistance, x Ga 1-x It is necessary to make N (0.8≦x≦1) thicker.

[0035] Therefore, the inventors have developed an AlN substrate x Ga 1-x The relationship between the thickness of the N film and the driving voltage Vf of the nitride semiconductor device was investigated. x Ga 1-x When the thickness of the N (0.8≦x≦1) film is in the range of 0.5 μm to 4 μm, n-Al x Ga 1-x We found that as the thickness of the N (0.8≦x≦1) increases, the driving voltage Vf of the nitride semiconductor device decays exponentially. x Ga 1-x It was discovered that when the film thickness of N (0.8≦x≦1) is 4 μm or more, the attenuation of the driving voltage Vf with respect to the film thickness becomes extremely small (see FIG. 5 described later).

[0036] Considering the reduction of the driving voltage Vf, n-Alx Ga 1-x The film thickness of GaN(0.8≤x≤1) is preferably 4 [μm] or more.

[0037] From the above, in the nitride semiconductor device according to the fifth embodiment, the thickness α [μm] of the AlN substrate and Al x Ga 1-x By setting the film thickness β [μm] of GaN(0.8≤x≤1) to values within the range that satisfies 96 < α < 200 and 4 ≤ β < 0.026α + 0.848 in at least a part of the region, the driving voltage Vf of the nitride semiconductor device can be reduced.

[0038] Also, in at least a part of the region of the nitride semiconductor device according to the fifth embodiment, the range of the thickness α [μm] of the AlN substrate satisfies the range described in the fourth embodiment. Therefore, the nitride semiconductor device according to the fifth embodiment also exhibits the effects of the first to fourth embodiments (suppression of corrosion progression, suppression of particle deposition, suppression of lattice relaxation of MQW, prevention of wafer cracking, suppression of light output reduction).

[0039] Next, matters common to the nitride semiconductor devices of the first to fifth embodiments described above will be described. <Substrate> The substrate of the nitride semiconductor device of this embodiment is an AlN substrate. By using an AlN substrate, it is possible to arrange Al x Ga 1-x GaN(0.8≤x≤1) with high crystallinity. The thickness α [μm] of the AlN substrate is not particularly limited, but may preferably be 96 [μm] or more and 600 [μm] or less from the viewpoint of preventing wafer cracking, etc., and may preferably be 96 [μm] or more and 200 [μm] or less from the viewpoint of improving output, etc.

[0040] In the description of the nitride semiconductor device of this embodiment, "arranging B on A" means both a form of directly arranging B on the surface of A and a form of indirectly arranging B via another substance from the surface of A.

[0041] <HOMO layer> The nitride semiconductor device of this embodiment may include a HOMO layer having the same composition as the substrate between the substrate and the first semiconductor layer. As described above, in the nitride semiconductor device of this embodiment, the substrate is AlN, so the HOMO layer is also made of AlN. The HOMO layer made of AlN (hereinafter, AlN_HOMO layer) is formed as a single crystal by, for example, an epitaxial growth method. The thickness of the AlN_HOMO layer is not particularly limited, but is, for example, 100 nm to 3000 nm, and is preferably 300 nm to 1000 nm from the viewpoint of realizing high crystallinity.

[0042] <First Conductive Type Semiconductor Layer> The first conductive type semiconductor layer of the nitride semiconductor device of this embodiment is Al x Ga 1-x N(0.8≦x≦1). Al x Ga 1-x N (0.8≦x≦1) allows a multiple quantum well (MQW) structure to be placed thereon. The first conductivity type is n-type or p-type. If the first conductivity type is n-type, the second conductivity type is p-type. If the first conductivity type is p-type, the second conductivity type is n-type.

[0043] The method for obtaining a semiconductor layer exhibiting n-type conductivity is not particularly limited, but for example, Si is used as an n-type dopant. Similarly, the method for obtaining a semiconductor layer exhibiting p-type conductivity is not particularly limited, but for example, Mg is used as a p-type dopant. From the viewpoint of crystallinity and surface flatness, Al is used as a p-type dopant. x Ga 1-x It may be preferable that the conductivity type of N (0.8≦x≦1) is n-type.

[0044] Al x Ga 1-x The thickness β [μm] of N (0.8≦x≦1) may preferably be 0.5 μm or more and 15 μm or less from the viewpoint of corrosion prevention, etc., and may preferably be 0.5 μm or more and 10 μm or less from the viewpoint of preventing lattice relaxation of the multiple quantum well (MQW) structure, and may preferably be 4 μm or more from the viewpoint of improving the driving voltage.

[0045] <Multiple quantum well structure> The nitride semiconductor device of this embodiment is made of Al x Ga 1-x The multi-quantum well structure may comprise a multi-quantum well (MQW) structure disposed on AlN (0.8≦x≦1). x Ga 1-x N layer (0.7≦x≦1) and Al y Ga 1-y It has a structure in which N layers (y>x) are repeatedly laminated for 5 to 200 periods.

[0046] As a multi-quantum well structure, Al x Ga 1-x N layer (0.7≦x≦1) and Al y Ga 1-y By adopting a structure in which N layers (y>x) are repeated for 5 to 200 periods, the external quantum efficiency is significantly improved.

[0047] In general, the layer in the repeating structure that has a smaller band gap is called a quantum well layer, and the layer that has a larger band gap is called a barrier layer.

[0048] The film composition is Al x Ga 1-x N layer (0.7≦x≦1) and Al y Ga 1-y By using a repeating structure of N layers (y>x), the external quantum efficiency is improved while suppressing the increase in driving voltage and the deterioration of crystallinity due to lattice relaxation. Note that the external quantum efficiency is defined as the ratio of the number of photons emitted to the outside of the ultraviolet light emitting element per unit time to the current flowing through the ultraviolet light emitting element (i.e., the number of electrons flowing through the ultraviolet light emitting element per unit time), for example. This ratio is expressed as a percentage (%).

[0049] In addition, Al x Ga 1-x N layer (0.7≦x≦1) and Al y Ga 1-yThe repeated structure of N layers (y>x) provides a central emission wavelength of 200 to 240 nm, making it possible to emit short-wavelength ultraviolet light with high external quantum efficiency.

[0050] Al forming a multi-quantum well structure x Ga 1-x N layer (0.7≦x≦1) and Al y Ga 1-y The thickness of each of the N layers (y>x) is not particularly limited. However, from the viewpoint of internal quantum efficiency, x Ga 1-x The thickness of the N layer (0.7≦x≦1) is preferably 0.25 nm or more and 2.0 nm or less, and more preferably 0.25 nm or more and 1.5 nm or less. The internal quantum efficiency is defined, for example, as the ratio of the number of photons generated per unit time inside the crystal of the ultraviolet light emitting element to the current flowing through the ultraviolet light emitting element (i.e., the number of electrons flowing through the ultraviolet light emitting element per unit time). This ratio is expressed, for example, as a percentage (%).

[0051] Al y Ga 1-y The thickness of the N layer (y>x) is not particularly limited, but from the viewpoint of internal quantum efficiency, it may be preferable that the thickness is 2 nm or more and 20 nm or less.

[0052] <Electron Block Layer> In the nitride semiconductor device of this embodiment, from the viewpoint of blocking electrons and injecting more electrons into the multiple quantum well structure, an Al b Ga 1-b N layers (b>x) may be provided. b Ga 1-b The N layer (b>x) may be an AlN layer, i.e., b=1. b Ga 1-b The N layer (b>x) is also called an electron blocking layer.

[0053] <Graded layer> In the nitride semiconductor device of this embodiment, from the viewpoint of improving the efficiency of injection of electrons or holes from the second conductive type semiconductor layer to the multiple quantum well structure, an Al c Ga 1-c The AlN layer (c is 0.15 or more and 0.95 or less, and decreases continuously or stepwise from the multiple quantum well structure side to the second conductive type semiconductor layer side) may be provided. c Ga 1-c The value of c in the N layer may be less than 0.15 or more than 0.95. For example, Al c Ga 1-c The c in the N layer is 0 to 1, and may decrease continuously or stepwise from the multiple quantum well structure side to the second conductive type semiconductor layer side. c Ga 1-c Since the c of the N layer includes a structure in which it decreases continuously or stepwise from 0.15 to 0.95, the Al c Ga 1-c Included in the N layer.

[0054] <Second Conductive Type Semiconductor Layer> The ultraviolet light emitting element of this embodiment may include a second conductive type semiconductor layer disposed on the multiple quantum well structure. The second conductive type semiconductor layer is not particularly limited as long as it is disposed on the multiple quantum well structure. Specific examples of the film composition of the second conductive type semiconductor layer include AlN, GaN, InN, and mixed crystals thereof. From the viewpoint of electrical conduction and contact resistance, it may be preferable that the second conductive type semiconductor layer is p-AlGaN.

[0055] The thickness of the second conductive type semiconductor layer is not particularly limited, but from the viewpoint of realizing high optical output, it is preferably 5 nm or more and 110 nm or less, and more preferably 15 nm or more and 90 nm or less.

[0056] <Electrode> The nitride semiconductor device of this embodiment may have an electrode for efficiently injecting electrons and holes into the multiple quantum well structure. The electrode is not particularly limited, but may be made of Alx Ga 1-x The first electrode may be electrically connected to N (0.8≦x≦1), and the second electrode may be electrically connected to the second conductive type semiconductor layer. The electrodes are preferably in ohmic contact with the layer with which they are in physical contact. The first electrode or the second electrode may be made of a metal such as Al, Au, Ti, Ni, Va, Cr, Rh, Mo, Pt, or Ta, or a mixed crystal of these metals.

[0057] <Emission wavelength> The nitride semiconductor device of this embodiment may be used as a light emitting device. When the nitride semiconductor device of this embodiment is used as a light emitting device, it is preferable that the device emits light having a wavelength of 215 nm or more and 240 nm or less, and more preferable that the device emits light having a central emission wavelength of 220 nm or more and 230 nm or less. There are no particular limitations on the method for emitting light having a wavelength of 215 nm or more and 240 nm or less, but examples of the method include a method of setting the Al composition of the quantum well layer in the multiple quantum well structure to 0.70 or more and 1.0 or less, and a method of setting the film thickness of the quantum well layer in the multiple quantum well structure to 2 nm or less.

[0058] <Insulating layer> From the viewpoint of reliability, the nitride semiconductor device according to this embodiment may have at least a part of its surface covered with an insulating layer. The material of the insulating layer is not particularly limited, but examples thereof include silicon oxide, silicon nitride, and aluminum oxide.

[0059] <Measurement method> (film thickness measurement) The thickness of each layer of the nitride semiconductor device of this embodiment can be measured by cutting out a predetermined cross section perpendicular to the main surface of the substrate, observing this cross section with a transmission electron microscope (TEM), and using a TEM length measurement function. As a measurement method, first, a cross section perpendicular to the main surface of the substrate of the nitride semiconductor device is observed using a TEM. Specifically, for example, the observation width is set to a range of 2 [μm] or more in a direction parallel to the main surface of the substrate in a TEM image showing a cross section perpendicular to the main surface of the substrate of the nitride semiconductor device. Since contrast is observed at the interface between two layers with different compositions within this observation width, the thickness up to this interface is observed in a continuous observation region with a width of 200 nm. The average value of the thickness of each layer included in this 200 nm wide observation region is calculated from five points arbitrarily extracted from the observation width of 2 [μm] or more to obtain the thickness of each layer.

[0060] (composition measurement) The composition of each layer of the nitride semiconductor device of this embodiment can be measured by reciprocal Al space mapping (RSM) using X-ray diffraction (XRD). Specifically, the Al composition can be obtained by analyzing reciprocal Al space mapping data in the vicinity of a diffraction peak obtained using an asymmetric plane as a diffraction plane. Examples of the diffraction plane include the (10-15) plane and the (20-24) plane.

[0061] In addition, layers that do not provide sufficient reflection intensity by XRD, such as quantum well layers and graded layers, can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), and electron energy-loss spectroscopy (EELS).

[0062] In EELS, the composition of a sample is analyzed by measuring the energy lost when an electron beam passes through the sample. Specifically, for example, the energy loss spectrum of the intensity of the transmitted electron beam is measured and analyzed for a thin-sectioned sample used in TEM observation. The position of the peak that appears around 20 eV of energy loss changes depending on the composition of each layer, and the composition can be determined from the peak position.

[0063] In the same manner as in the method for calculating layer thickness by TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation area of ​​2 μm or more.

[0064] In EDX, characteristic X-rays generated by an electron beam in a thin-sectioned sample used in the above-mentioned TEM observation, etc. are measured and analyzed. In the same manner as the layer thickness calculation method using TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation area of ​​2 μm or more.

[0065] In XPS, the evaluation of the depth direction is possible by performing XPS measurement while performing sputter etching using an ion beam. Although Ar+ is generally used as the ion beam, other ion species such as Ar cluster ions can be used as long as they can be irradiated with the etching ion gun mounted on the XPS device. The XPS peak intensities of Al, Ga, and N are measured and analyzed to obtain the depth direction distribution of the Al composition of each layer. Instead of sputter etching, the laser diode may be polished obliquely so that the cross section perpendicular to the main surface of the substrate is enlarged and exposed, and the exposed cross section may be measured by XPS.

[0066] The composition of each layer can be measured not only by XPS but also by Auger electron spectroscopy (AES). In this case, the composition can be measured by performing Auger electron spectroscopy on a cross section exposed by sputter etching or oblique polishing. The composition of each layer can also be measured by SEM-EDX measurement of a cross section exposed by oblique polishing. The number of repeating periods of the multiple quantum well structure of the nitride semiconductor device of this embodiment is defined by the number of quantum well layers, and can be measured by TEM observation in the same manner as above.

[0067] (Emission wavelength measurement) The emission wavelength of the nitride semiconductor device of this embodiment can be measured by photoluminescence (PL) measurement. Details of the PL measurement will be described below.

[0068] In PL measurements, a laser beam with energy greater than the band gap energy of the quantum well layer is irradiated at an angle of about 45 degrees from the sample surface. In this case, a lens can be used to reduce the spot diameter irradiated on the sample, or a filter can be used to change the intensity of the laser beam. The irradiated laser beam excites electrons into conductors in the quantum well layer of the sample, generating electron-hole pairs. The excited electrons then return to the ground state, and in the process of recombining with the holes, they generate light with a wavelength according to the band gap. The generated light is captured from directly above the sample. The captured light is passed through a diffraction grating to separate the light into wavelengths, allowing the emission wavelength of the sample to be measured.

[0069] <Example 1> (structure) 1 is a cross-sectional view showing a nitride semiconductor device 100 according to a first specific example of an embodiment of the present invention. As shown in FIG. 1, the nitride semiconductor device 100 includes, for example, an AlN substrate 1, an AlN_HOMO layer 3 which is a homoepitaxial layer disposed on the AlN substrate 1, and an AlN_HOMO layer 4 which is disposed on the AlN_HOMO layer 3. x Ga 1-x N(0.8≦x≦1)5. Al x Ga 1-xThe film thickness β [μm] of N(0.8≦x≦1)5 is 0.5<β<15 in at least a part of the region.

[0070] Al x Ga 1-x An example of N(0.8≦x≦1)5 is n-type Al 0.87 Ga 0.13 The nitride semiconductor device 100 is used, for example, as an undercoat film for a light emitting device. The application is not limited to the undercoat film of a light emitting device, but may be an undercoat film of a power semiconductor or the like.

[0071] Al x Ga 1-x N(0.8≦x≦1)5 is preferably n-type doped with Si. x Ga 1-x The AlN (0.8≦x≦1)5 is deposited using a metalorganic chemical vapor deposition (MOCVD) system. x Ga 1-x It was found that when the thickness of AlN (0.8≦x≦1) is 15 μm or more, a large amount of source gas is used, which causes problems such as clogging of the shower head of the MOCVD apparatus and generation and accumulation of particles on the susceptor. x Ga 1-x For N (0.8≦x≦1), it was concluded that a thickness of 15 μm is the upper limit of the thickness that can be stably produced.

[0072] (Manufacturing method) A (0001) AlN single crystal substrate with a thickness of 550 μm was prepared as the AlN substrate 1. This (0001) AlN single crystal substrate was subjected to an annealing treatment using a metal organic chemical vapor deposition (MOCVD) apparatus. The annealing treatment was performed in two sets of treatments, each set consisting of annealing for 5 minutes in an NH3 atmosphere and annealing for 5 minutes in an H2 atmosphere at 1300°C.

[0073] Next, an AlN layer, which is a homoepitaxial layer, was formed on the AlN single crystal substrate. This AlN layer is the AlN_HOMO layer 3. The AlN layer was formed to a thickness of 500 nm in an environment of 1200°C. Trimethylaluminum (TMAl) was used as the Al raw material. Ammonia (NH3) was used as the N (nitrogen) raw material.

[0074] n-type Al x Ga 1-x N(0.8≦x≦1)5 was formed to a thickness of 350 nm at a temperature of 1080° C. with a degree of vacuum set to 50 mbar. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material. Ammonia (NH3) was used as the N raw material. Monosilane (SiH4) was used as the Si raw material. Through the above steps, the nitride semiconductor device 100 shown in FIG. 1 is completed.

[0075] <Example 2> (structure) 2 is a cross-sectional view showing a nitride semiconductor device 100A according to a specific example 2 of an embodiment of the present invention. As shown in FIG. 2, the nitride semiconductor device 100A includes, as a unit element, an AlN_HOMO layer 3 which is a homoepitaxial layer disposed on an AlN substrate 1, and an n-type Al x Ga 1-x N(0.8≦x≦1) and Al x Ga 1-x An n-electrode 7 (an example of a first electrode) is disposed on the first region of N (0.8≦x≦1), and an Al x Ga 1-x The semiconductor device comprises a multiple quantum well structure 9 disposed on a second region of N (0.8≦x≦1), an electron blocking layer 11 disposed on the multiple quantum well structure 9, a graded layer 13 disposed on the electron blocking layer 11, a p-type GaN layer 15 disposed on the p-type graded layer 13, and a p-electrode 17 (an example of a second electrode) disposed on the p-type GaN layer 15.

[0076] The nitride semiconductor device 100A includes a plurality of the unit elements described above on the AlN substrate 1. For example, the plurality of unit elements UD have the same shape as one another. The plurality of unit elements UD are repeatedly arranged in one direction parallel to the surface 1a of the AlN substrate 1 (in FIG. 2, the left-right direction on the paper).

[0077] The wavelength of light emitted by the nitride semiconductor device 100A is, for example, not less than 200 nm and not more than 240 nm, and the light is extracted from the back surface 1b of the AlN substrate 1. To improve the light extraction efficiency, in the manufacturing process of the nitride semiconductor device 100A, the back surface 1b of the AlN substrate 1 is ground and polished at the wafer level to a thickness of, for example, 100 μm.

[0078] (Manufacturing method) n-type Al x Ga 1-x A multi-quantum well structure 9 having a repeating period of 20 times was formed on a silicon substrate (SiC) having a thickness of 0.8≦x≦1. The multi-quantum well structure 9 is made of a quantum well layer (Al x Ga 1-x The multiple quantum well structure 9 includes a layer (AlyGa1-yN) and a barrier layer (AlyGa1-yN). The multiple quantum well structure 9 has a structure in which quantum well layers and barrier layers are repeatedly stacked for 5 to 200 periods. In this example, the number of periods in which the quantum well layers and barrier layers are repeatedly stacked in the multiple quantum well structure 9 is 20, and the film thickness of the multiple quantum well structure 9 is 134 nm.

[0079] The quantum well layer is Al x Ga 1-x The quantum well layer is 1 nm thick and has an Al composition of 82%. The barrier layer is AlyGa1-yN. The barrier layer is 6 nm thick and has an Al composition of 92%. x Ga 1-x As with N(0.8≦x≦1)5, the conditions for forming the quantum well layers and barrier layers in the multiple quantum well structure 9 were set to a temperature of 1080°C and a degree of vacuum of 50 mbar. Trimethylaluminum (TMAl) was used as the Al raw material, triethylgallium (TEGa) was used as the Ga raw material, and ammonia (NH3) was used as the N raw material. The beginning and end of the repeating period are quantum well layers.

[0080] Next, an electron blocking layer 11 was formed on the multiple quantum well structure 9 having a repeating period. The electron blocking layer 11 was an AlN layer containing no dopant. The electron blocking layer 11 was formed to a thickness of 10 nm at a temperature of 1080° C. and a degree of vacuum of 50 mbar. Trimethylaluminum (TMAl) was used as the Al raw material.

[0081] Next, a p-type graded layer 13 was formed on the electron blocking layer 11. The p-type graded layer 13 was an AlGaN layer having a thickness of 40 nm, in which the Al composition decreases in the direction away from the AlN substrate 1, varying from Al=0.85 to 0.25.

[0082] The p-type graded layer 13 was formed under the conditions of a temperature of 1080° C. and a degree of vacuum of 50 mbar. Trimethylaluminum (TMAl) was used as the Al raw material, and triethylgallium (TEGa) was used as the Ga raw material.

[0083] Next, a p-type GaN layer 15 was formed on the p-type graded layer 13. The p-type GaN layer 15 is a second conductivity type semiconductor layer (contact layer). The conditions for forming the p-type GaN layer 15 were a temperature of 950° C., a degree of vacuum of 50 mbar, and a thickness of 8 nm. Trimethylgallium (TMGa) was used as the Ga raw material.

[0084] Next, the p-type GaN layer 15, the p-type graded layer 13, the electron blocking layer 11, and the multiple quantum well structure 9 are patterned into a mesa shape. x Ga 1-x The first region of N(0.8≦x≦1)5 is exposed. x Ga 1-x A mesa-shaped laminate is formed on the second region of N(0.8≦x≦1). The mesa-shaped laminate is made of Al x Ga 1-xOn the second region of N(0.8≦x≦1)5, there are provided a multiple quantum well structure 9, an electron blocking layer 11, a p-type graded layer 13, and a p-type GaN layer 15 in this order.

[0085] Next, Al x Ga 1-x An n-electrode 7 is formed on the first region of N(0.8≦x≦1) 5, and ap electrode 17 is formed on the p-type GaN layer 15. Through the above steps, the nitride semiconductor device 100A shown in FIG.

[0086] (Example) Next, as an embodiment of the present invention, an experiment conducted by the present inventors and the results thereof will be described. (1) Experiment 1: Corrosivity The inventors have developed an n-type (n-)AlN substrate with a high Al composition. x Ga 1-x A long-term reliability test (room temperature, 100 mA applied) was carried out on an element having N (0.8≦x≦1). As a result, it was found that corrosion progressed from the vicinity of the n-electrode, causing open defects. x Ga 1-x When the Al composition of N is low, for example x=0.7, such corrosion does not occur. Therefore, n-Al, which has a high Al composition, x Ga 1-x It was found that N (0.8≦x≦1) is prone to corrosion.

[0087] n-Al x Ga 1-x By increasing the thickness of the N (0.8≦x≦1) film from 0.5 μm to 1 μm, we were able to successfully suppress corrosion. x Ga 1-x It is preferable that the thickness of N (0.8≦x≦1) is greater than 0.5 μm, and it is more preferable that the thickness is greater than 1 μm.

[0088] The presence or absence of corrosion was judged based on the results of analysis using a scanning electron microscope - energy dispersive X-ray microanalyzer (SEM-EDX). When the SEM-EDX analysis detected no N (nitrogen) but only O (oxygen) in the AlGaN, it was judged that corrosion was present. When the SEM-EDX analysis detected N (nitrogen) in the AlGaN but not O (oxygen) (or the O detection intensity was sufficiently low), it was judged that corrosion was not present.

[0089] (2) Experiment 2: Lattice relaxation The inventors have developed n-Al on an AlN substrate. x Ga 1-x It was found through experiments that when N (0.8≦x≦1) is made thicker than 10 μm, stress accumulates and lattice relaxation occurs in the multi-quantum well structure formed on it. x Ga 1-x Table 1 shows the relationship between the thickness of N (0.8≦x≦1) and the lattice relaxation in the multiple quantum well structure. [Table 1]

[0090] From the above results, it can be seen that the n-Al x Ga 1-x The thickness of the multiple quantum well structure formed on N (0.8≦x≦1) is preferably less than 10 μm in terms of suppressing lattice relaxation of the multiple quantum well structure.

[0091] The method for measuring lattice relaxation is as follows. Reciprocal Al Space Mapping (RSM) using X-ray diffraction (XRD) was used to measure the composition of each layer of the nitride semiconductor device. Specifically, the Al composition is obtained by analyzing reciprocal lattice mapping data in the vicinity of a diffraction peak obtained with an asymmetric plane as a diffraction plane. Examples of the diffraction plane include the (10-15) plane and the (20-24) plane.

[0092] (3) Experiment 3: Cracks and warping n-Al x Ga 1-x N (0.8≦x≦1) has a strong stress and causes the AlN substrate 1 to warp. x Ga 1-x If the thickness of the n-AlN (0.8≦x≦1) film is too thick, the warp of the wafer exceeds the boundary point and the wafer breaks. x Ga 1-x We found a relationship between the thickness and thickness of the AlN film and the thickness of the AlN film.

[0093] 3 is a graph showing the results of Experiment 3 (regarding cracks and warpage) according to an embodiment of the present invention. The horizontal axis of FIG. 3 shows the wafer thickness α [μm], and the vertical axis shows n-Al x Ga 1-x This graph shows the thickness of N (0.8≦x≦1) and the thickness β [μm]. As shown in Figure 3, no wafer cracks occurred in the shaded area in the graph. This shaded area is the area that satisfies β<0.026α+0.848.

[0094] The method for measuring wafer cracking is as follows. Wafer cracking was measured by adhering the wafer to a ceramic deck with wax, grinding, heating the wax, and checking whether any cracks were found when peeling it off. A practical problem with wafer warping is that the wafer may crack when it is secured in a vacuum chuck or similar device in later processes such as dicing. Therefore, it was determined that if the wafer does not crack when peeled off after grinding from a wafer secured in wax (similar to a wafer secured in a vacuum chuck or similar device), it will not crack when secured in a vacuum chuck or similar device in later processes.

[0095] (4) Experiment 4: Light output (light intensity) The inventors have developed a n-AlN substrate. x Ga 1-x A simulation was performed on the light output (light intensity) of a light-emitting element having N (0.8≦x≦1).

[0096] Figure 4 is a graph showing the results of a simulation of the relationship between wafer thickness [μm] and light output. The wafer is an AlN substrate before dicing. The horizontal axis of Figure 4 indicates the wafer thickness α [μm], and the vertical axis indicates the light intensity. Note that a light intensity of 1 means the light intensity when the wafer thickness is virtually set to 0 (zero) and there is no attenuation of light due to the wafer.

[0097] As shown in Figure 4, the optical output decreased as the wafer thickness [μm] increased, and the optical intensity was halved when the wafer thickness was 200 μm or more.

[0098] From the above results, it is preferable that the thickness α of the wafer is less than 200 μm, and more preferably less than 110 μm.

[0099] (5) Experiment 5: Driving voltage The inventors have developed a n-AlN substrate. x Ga 1-x A simulation was performed on the driving voltage of a light-emitting device having N (0.8≦x≦1).

[0100] Figure 5 shows the n-Al x Ga 1-x 5 is a graph showing the results of a simulation of the relationship between the film thickness [μm] of N (0.8≦x≦1) and the driving voltage Vf [V]. x Ga 1-x The vertical axis shows the thickness β [μm] of N (0.8≦x≦1), and the vertical axis shows the driving voltage Vf [V]. x Ga 1-x Three patterns were prepared for the shape of N (0.8≦x≦1). The above relationship was simulated when a current of 100 mA was applied to each pattern.

[0101] As shown in Fig. 5, in all patterns, n-Al x Ga 1-xIt was found that the driving voltage Vf decreases as the thickness of the N (0.8≦x≦1) film increases. x Ga 1-x When the thickness of the N (0.8≦x≦1) film is in the range of 0.5 μm to 4 μm, n-Al x Ga 1-x It was found that as the thickness of the N (0.8≦x≦1) increases, the driving voltage Vf of the nitride semiconductor device decays exponentially. x Ga 1-x It was found that when the film thickness of N (0.8≦x≦1) was 4 μm or more, the attenuation of the driving voltage Vf with respect to the film thickness became extremely small.

[0102] As explained in the fifth embodiment, in consideration of reducing the driving voltage Vf, n-Al x Ga 1-x The thickness of N (0.8≦x≦1) is preferably 4 μm or more.

[0103] <Other embodiments> As described above, the present disclosure has been described by the embodiments, specific examples, and examples, but the descriptions and drawings forming a part of this disclosure should not be understood as limiting the present disclosure. From this disclosure, various alternative embodiments, examples, and operation techniques will become apparent to those skilled in the art. Of course, the present technology includes various embodiments not described here. At least one of various omissions, substitutions, and modifications of components can be made within the scope of the gist of the above-mentioned embodiments and modified examples. In addition, the effects described in this specification are merely examples and are not limited, and other effects may be present.

[0104] The present disclosure can also be configured as follows. (1) Al on an AlN substrate x Ga 1-x A first conductive type semiconductor layer formed of N (0.8≦x≦1), The thickness β [μm] of the first conductive type semiconductor layer is, in at least a part of the region, A nitride semiconductor element with β of 0.5<β<15. (2) The film thickness β [μm] is, in at least a part of the region, The nitride semiconductor device according to (1) above, wherein 0.5<β<10. (3) The thickness α [μm] of the AlN substrate and the film thickness β [μm] are, at least in a part of the region, 96<α<600, 0.5<β<10, β<0.026α+0.848, The nitride semiconductor device according to (1) or (2), which satisfies all of the above. (4) The thickness α [μm] of the AlN substrate and the film thickness β [μm] are, in at least a part of the region, 96<α<200, 0.5<β<0.026α+0.848, The nitride semiconductor device according to any one of (1) to (3), which satisfies all of the above. (5) The thickness α [μm] of the AlN substrate and the film thickness β [μm] are, in at least a part of the region, 96<α<200, 4≦β<0.026α+0.848, The nitride semiconductor device according to any one of (1) to (4) above, which satisfies all of the above. (6) The nitride semiconductor device according to any one of (1) to (5) above, which is a light emitting device. (7) The nitride semiconductor device according to (6) above, further comprising a light emitting layer on the first conductive type semiconductor layer. (8) The nitride semiconductor device according to (7) above, wherein the emission wavelength of the light emitting layer is not less than 215 nm and not more than 240 nm. (9) A film composition of Al is formed in a part of the light-emitting layer. x Ga 1-x The nitride semiconductor device according to (7) or (8) above, having a quantum well layer where N is a (0.7≦x≦1) n=1. (10) The nitride semiconductor device according to any one of (1) to (9) above, wherein the conductivity type of the first conductivity type semiconductor layer is n-type. [Explanation of symbols]

[0105] 1. AlN substrate 1a surface 1b back side 3 HOMO layer 5. Al x Ga 1-x N(0.8≦x≦1) 7n electrode 9. Multiple quantum well structure 11 Electron Block Layer 13 Graded Layer 15 GaN layer 17p electrode 71, 171 Extension part 72, 172 Joint 100, 100A, 100B Nitride semiconductor element

Claims

1. Al placed on an AlN substrate x G 1-x N (0.8≦x≦1), The thickness β [μm] of the first conductive type semiconductor layer is, in at least a part of the region, A nitride semiconductor device in which 0.5<β<15.

2. The film thickness β [μm] is, in at least a part of the region, 2. The nitride semiconductor device according to claim 1, wherein 0.5<β<10.

3. The thickness α [μm] of the AlN substrate and the film thickness β [μm] are, in at least a part of the region, 96<α<600、 0.5<β<10、 β<0.026α+0.848、 The nitride semiconductor device according to claim 1 , wherein all of the above conditions are satisfied.

4. The thickness α [μm] of the AlN substrate and the film thickness β [μm] are, in at least a part of the region, 96<α<200、 0.5<β<0.026α+0.848、 The nitride semiconductor device according to claim 1 , wherein all of the above conditions are satisfied.

5. The thickness α [μm] of the AlN substrate and the film thickness β [μm] are, in at least a part of the region, 96<α<200、 4≦β<0.026α+0.848、 The nitride semiconductor device according to claim 1 , wherein all of the above conditions are satisfied.

6. 6. The nitride semiconductor device according to claim 1, which is a light emitting device.

7. The nitride semiconductor device according to claim 6 , further comprising a light emitting layer on the first conductive type semiconductor layer.

8. The nitride semiconductor device according to claim 7, wherein the emission wavelength of the light emitting layer is not less than 215 nm and not more than 240 nm.

9. A film composition of Al is formed in a part of the light emitting layer. x G 1-x 8. The nitride semiconductor device according to claim 7, further comprising a quantum well layer having N (0.7≦x≦1).

10. The nitride semiconductor device according to claim 1 , wherein the conductivity type of the first conductivity type semiconductor layer is n-type.

Citation Information

Patent Citations

  • JP2020-1550252A

  • Ultraviolet light emitting element

    JP2022117299A

  • ultraviolet light-emitting diode

    JP6621990B2