Optical member, lens unit, and manufacturing method of optical member
The optical member with a titanium dioxide-based hydrophilic layer and antireflection film effectively restores hydrophilicity by UV irradiation, addressing the durability issues of existing hydrophilic lenses.
Patent Information
- Application Number
- JP2023074466
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hydrophilic lenses lose hydrophilicity over time due to dirt adhesion, and UV irradiation does not sufficiently restore the hydrophilic function.
An optical member with a hydrophilic layer containing aggregates of titanium dioxide primary particles, where the primary particles have a diameter of 5-20 nm and secondary particles have a diameter of 15-100 nm, is used, along with an antireflection film and a coating layer to enhance durability and restore hydrophilicity through UV irradiation.
The hydrophilic function can be effectively restored by UV irradiation, maintaining visibility and reducing ghost and flare phenomena, while enhancing wear resistance and transmittance.
Smart Images

Figure 2024158871000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an optical member, a lens unit, and a method for manufacturing an optical member. [Background technology]
[0002] Visibility is impaired by water droplets on window glass of buildings or automobiles exposed to outdoor weather. One solution to the problem of impaired visibility is to make the surface of the window glass hydrophilic. This makes it possible to turn the adhering water into a film, preventing the adhesion of water droplets and ensuring visibility on the window glass.
[0003] However, organic dirt caused by automobile exhaust gases or factory smoke easily adheres to the surface of hydrophilic members, causing water droplets to adhere to the surface, significantly reducing visibility.
[0004] In view of this, a hydrophilic lens including a glass substrate and a hydrophilic layer formed on the glass substrate has been disclosed (for example, Patent Document 1). In the hydrophilic lens of Patent Document 1, the hydrophilic layer contains a silicate material in which fine particles having photocatalytic activity are dispersed, the film thickness of the hydrophilic layer is 30 nm or less, the average particle diameter of the fine particles is 30 nm or less, and the arithmetic mean roughness Ra of the surface of the hydrophilic layer is 0.7 to 1.9 nm. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-77260 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the hydrophilic lens of Patent Document 1 could not maintain hydrophilicity for a long period of time. For example, when the hydrophilic function is reduced due to the adhesion of dirt, the hydrophilic function cannot be fully restored even when exposed to sunlight including ultraviolet rays.
[0007] The present disclosure has been made in consideration of the above-mentioned problems, and its purpose is to provide an optical component, a lens unit, and a method for manufacturing an optical component that can fully restore the hydrophilic function when dirt adheres to the optical component and the hydrophilic function is reduced by irradiating the optical component with ultraviolet light. [Means for solving the problem]
[0008] An exemplary optical member of the present disclosure includes a translucent member and a hydrophilic layer. The translucent member transmits visible light. The hydrophilic layer covers the translucent member. The hydrophilic layer contains secondary particles formed by agglomeration of a plurality of titanium dioxide primary particles. The titanium dioxide primary particles have an average particle size of 5 nm or more and 20 nm or less. The titanium dioxide secondary particles have an average particle size of 15 nm or more and 100 nm or less.
[0009] An exemplary lens unit of the present disclosure includes the optical member described above.
[0010] An exemplary method for manufacturing an optical member according to the present disclosure includes a coating step and a drying step. In the coating step, a hydrophilic material is coated. In the drying step, the hydrophilic material is dried to produce a hydrophilic layer. The hydrophilic material contains a plurality of primary particles of titanium dioxide. The primary particles of titanium dioxide have an average particle size of 5 nm or more and 20 nm or less. The hydrophilic layer contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide. The secondary particles of titanium dioxide have an average particle size of 15 nm or more and 100 nm or less. Effect of the Invention
[0011] According to the exemplary embodiment of the present disclosure, when the hydrophilic function is reduced due to the adhesion of dirt, the hydrophilic function can be sufficiently restored by irradiating with ultraviolet light. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of an optical unit according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of an optical member according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same or corresponding parts are denoted by the same reference symbols, and the description will not be repeated. The dimensions, shapes, and size relationships between components in the drawings are not necessarily the same as the actual dimensions, shapes, and size relationships between components. In particular, the thickness ratio and curvature of the hydrophilic layer and the translucent member in the drawings may differ significantly from the actual ones.
[0014] In this specification, "thickness" refers to the length of an optical member in the optical axis direction. The "outside" of an optical member refers to the direction from the light-transmitting member to the hydrophilic layer. The "inside" of an optical member refers to the direction from the hydrophilic layer to the light-transmitting member.
[0015] The optical member according to this embodiment is suitable as an optical member used in, for example, an optical unit including one or more optical members (particularly, an optical unit used outdoors). The optical member according to this embodiment is particularly suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle. FIG. 1 is a schematic diagram showing an example of an optical unit according to this embodiment. As shown in FIG. 1, an optical unit 1000 includes an optical member 100. The optical unit is an example of a "lens unit".
[0016] The static contact angle of the surface of the optical member 100 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and particularly preferably 10.0° or less. Hereinafter, the static contact angle with pure water may be referred to simply as "contact angle." Note that the contact angle of the surface of the optical member according to this embodiment is a value measured in an environment with a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.
[0017] Moreover, the maximum reflectance of the optical member 100 for light having a wavelength of 480 nm or more and 780 nm or less is preferably 1.5% or less, more preferably 1.0% or less. The lower the maximum reflectance of the optical member 100 according to this embodiment, the more the occurrence of image defects called ghost phenomenon and flare phenomenon can be suppressed. In particular, the lower the maximum reflectance, the more effectively the occurrence of ghost phenomenon can be suppressed. When the maximum reflectance is 1.5% or less, the occurrence of ghost phenomenon can be suppressed. When the maximum reflectance is 1.0% or less, the occurrence of ghost phenomenon can be more effectively suppressed. Note that light having a wavelength of 480 nm or more and 780 nm or less corresponds to light in the visible light region.
[0018] Hereinafter, an example of the optical member 100 according to this embodiment will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the optical member 100 according to this embodiment. The optical member 100 includes a light-transmitting member 10, a hydrophilic layer 20, and an anti-reflection film 30.
[0019] <Translucent member> The light-transmitting member 10 has light-transmitting properties. That is, the light-transmitting member 10 transmits visible light. The light-transmitting member 10 may be transparent or translucent. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.
[0020] The light-transmitting member 10 has a function as, for example, a lens (specifically, for example, a biconvex lens, a biconcave lens, a plano-convex lens, a plano-concave lens, a convex meniscus lens, or a concave meniscus lens). In this specification, when the light-transmitting member 10 is a lens, the lens surface of the light-transmitting member 10 may be spherical or aspherical. The radius of curvature of the lens surface of the light-transmitting member 10 is preferably 9 mm or more and 16 mm or less.
[0021] <Hydrophilic layer> The hydrophilic layer 20 covers the light-transmitting member 10. Specifically, the hydrophilic layer 20 is disposed on the antireflection film 30. The hydrophilic layer 20 has hydrophilic properties.
[0022] The thickness of the hydrophilic layer 20 is preferably 20 nm or more and 200 nm or less, more preferably 30 nm or more and 100 nm or less. If the thickness of the hydrophilic layer 20 is less than 20 nm, the function of restoring hydrophilicity tends to be insufficient. If the thickness of the hydrophilic layer 20 is more than 200 nm, the transmittance of visible light tends to be insufficient.
[0023] In the present specification, the "thickness" may be determined using a stylus-type step gauge. Specifically, a sharp needle is traced over the surface to measure the step between areas with and without a layer (film). The step is measured at three arbitrary locations, and the average value of the step differences at the three locations is taken as the "thickness."
[0024] The hydrophilic layer 20 contains secondary particles formed by agglomeration of multiple titanium dioxide primary particles. Titanium dioxide has a photocatalytic function. For example, when the optical member 100 is used for a long period of time, dirt adheres to the optical member 100, reducing the hydrophilic function. When the optical member 100 is irradiated with ultraviolet light (sunlight), the dirt is decomposed and the hydrophilicity can be restored.
[0025] The average particle size of the primary particles of titanium dioxide is 5 nm or more and 20 nm or less, and preferably 5 nm or more and 10 nm or less. If the average particle size of the primary particles of titanium dioxide is less than 5 nm, sufficient hydrophilicity cannot be maintained. If the average particle size of the primary particles of titanium dioxide is more than 20 nm, sufficient transmittance for visible light cannot be obtained, or a uniform film cannot be formed.
[0026] In the present specification, the "average particle size of primary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 primary particles that can be observed in their entirety, the maximum and minimum diameters of each primary particle are measured, the average of the maximum and minimum diameters is defined as the particle size of the single primary particle, and the average of the particle diameters of each of the 50 primary particles is defined as the "average particle size of primary particles."
[0027] Examples of titanium dioxide include anatase type titanium dioxide, rutile type titanium dioxide, and brookite type titanium dioxide. From the viewpoint of photocatalytic activity, anatase type titanium dioxide is preferable.
[0028] The average particle size of the secondary particles of titanium dioxide is 15 nm or more and 100 nm or less, and preferably 20 nm or more and 60 nm or less. If the average particle size of the secondary particles of titanium dioxide is less than 15 nm, the hydrophilicity of the hydrophilic layer 20 cannot be sufficiently restored. If the average particle size of the secondary particles of titanium dioxide is more than 100 nm, sufficient transmittance for visible light cannot be obtained.
[0029] In this specification, the "average particle size of secondary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 secondary particles that can be observed in their entirety, the maximum and minimum diameters of each secondary particle are measured, the average of the maximum and minimum diameters is defined as the particle size of the one secondary particle, and the average of the particle diameters of each of the 50 secondary particles is defined as the "average particle size of secondary particles."
[0030] The content of titanium dioxide in the hydrophilic layer 20 is preferably 50% by mass or more and 70% by mass or less. By having a titanium dioxide content of 50% by mass or more and 70% by mass or less, the hydrophilicity of the hydrophilic layer 20 can be more effectively restored and an increase in reflectance can be more effectively suppressed.
[0031] As described above with reference to FIG. 1, in this embodiment, the hydrophilic layer 20 contains secondary particles of a predetermined size formed by aggregation of primary particles of a predetermined size, so that when dirt adheres to the hydrophilic layer 20 and the hydrophilic function is reduced, the hydrophilic function can be sufficiently restored by irradiating the hydrophilic layer 20 with ultraviolet light.
[0032] The hydrophilic layer 20 preferably further contains tetraethoxysilane, which further improves the abrasion resistance of the optical member 100. The hydrophilic layer 20 may further contain silicon dioxide.
[0033] <Anti-reflective film> The antireflection film 30 covers the light-transmitting member 10. The antireflection film 30 is disposed between the light-transmitting member 10 and the hydrophilic layer 20. The antireflection film 30 suppresses reflection of light. Specifically, by including the antireflection film 30, the optical member 100 suppresses light that attempts to enter the light-transmitting member 10 from the antireflection film 30 from being reflected by the surface on the antireflection film 30 side.
[0034] The anti-reflection film 30 has a multi-layer structure. Specifically, the anti-reflection film 30 has low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction). The refractive indices of the low-refractive index layers and high-refractive index layers are not limited as long as the combination allows the anti-reflection film 30 to exhibit an anti-reflection effect. The refractive index of the low-refractive index layer is, for example, 1.80 or less. The refractive index of the high-refractive index layer is, for example, more than 1.80. The layer located outermost among the low-refractive index layers and high-refractive index layers is the low-refractive index layer. The layer located innermost among the low-refractive index layers and high-refractive index layers is the low-refractive index layer.
[0035] The refractive index of the low refractive index layer may be less than that of the high refractive index layer. For example, the refractive index of the low refractive index layer is preferably 1.30 or more and 1.80 or less, more preferably 1.40 or more and 1.60 or less. By making the refractive index of the low refractive index layer 1.30 or more and 1.80 or less, the reflectance of the optical member 100 is further reduced. The low refractive index layer preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2.
[0036] The refractive index of the high refractive index layer may be higher than that of the low refractive index layer. For example, the refractive index of the high refractive index layer is preferably 2.40 or more and 3.00 or less, more preferably 2.40 or more and 2.60 or less. By having the refractive index of the high refractive index layer be 2.40 or more and 3.00 or less, the reflectance of the optical member 100 is further reduced. The high refractive index layer preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2 and Nb2O5, and more preferably contains Si3N4.
[0037] The refractive indices of the low refractive index layer and the high refractive index layer described above are merely examples and are not limited thereto. The refractive indices of the low refractive index layer and the high refractive index layer may be set to values optimal for the refractive index of the light-transmitting member 10.
[0038] The total thickness of the antireflection film 30 is preferably 200 nm or more and 700 nm or less, more preferably 200 nm or more and 650 nm or less. If the total thickness of the antireflection film 30 is less than 200 nm, sufficient antireflection effect tends to be insufficient. If the total thickness of the antireflection film 30 exceeds 700 nm, the productivity of the optical member 100 tends to decrease. In addition, if the total thickness exceeds 700 nm, the production cost of the optical member 100 tends to increase.
[0039] The thickness of one low refractive index layer is, for example, from 5.0 nm to 200.0 nm, and the thickness of one high refractive index layer is, for example, from 5.0 nm to 200.0 nm.
[0040] The total number of low refractive index layers and high refractive index layers is usually an odd number, but may be an even number.
[0041] <Coating layer> The optical member 100 preferably further includes a coating layer 60. The coating layer 60 is disposed on the hydrophilic layer 20. The coating layer 60 contains a plurality of primary silica particles. At least a portion of the hydrophilic layer 20 is partially or completely coated with the primary silica particles. As a result, the wear resistance of the optical member 100 is further improved. The coating layer 60 may further contain tetraethoxysilane.
[0042] The average particle size of the primary particles of silica is preferably 5 nm or more and 20 nm or less. If the average particle size of the primary particles of silica is less than 5 nm, the cost tends to increase. If the average particle size of the primary particles of silica is more than 20 nm, the transmittance of visible light tends to be insufficient.
[0043] The content of silica in the hydrophilic layer 20 is preferably 20% by mass or more and 50% by mass or less. When the content of silica is 20% by mass or more and 50% by mass or less, the abrasion resistance of the optical member 100 is further improved and an increase in reflectance can be further suppressed.
[0044] The thickness of the coating layer 60 is preferably 5 nm or more and 20 nm or less. If the thickness of the coating layer 60 is less than 5 nm, sufficient abrasion resistance tends to be insufficient. If the thickness of the coating layer 60 is more than 20 nm, sufficient transmittance for visible light tends to be insufficient.
[0045] <Method of manufacturing optical members> An example of a method for manufacturing the optical member 100 according to this embodiment will be described below. The method for manufacturing the optical member 100 includes a preparation step, a coating step, and a drying step.
[0046] <Preparation steps> A light-transmitting member 10 is prepared. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component. An anti-reflection film 30 may be disposed on the light-transmitting member 10. The anti-reflection film 30 has low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction).
[0047] <Application step> A hydrophilic material is applied. The hydrophilic material contains a plurality of primary particles of titanium dioxide. The primary particles of titanium dioxide have an average particle size of 5 nm or more and 20 nm or less.
[0048] The hydrophilic material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include nitric acid, formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.
[0049] The content of the solvent in the hydrophilic material is preferably 50.0% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50.0% by mass or more and 99.9% by mass or less, coating can be easily performed.
[0050] The method of applying the hydrophilic material is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, or a combination of two or more of these (e.g., dip spin coating). Examples of the wet process include spin coating, dip coating, or dip spin coating.
[0051] <Drying step> The hydrophilic material is dried to produce the hydrophilic layer 20. The hydrophilic layer 20 contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide. The average particle size of the secondary particles of titanium dioxide is 15 nm or more and 100 nm or less.
[0052] It is preferable to heat-treat the coated hydrophilic material. Heat treatment promotes the removal of the solvent in the hydrophilic material. Heating conditions can be, for example, a treatment temperature of 60°C to 200°C and a treatment time of 10 minutes to 2 hours.
[0053] It is preferable that the method for producing the optical member 100 further includes a coating material application step.
[0054] <Coating material application step> A coating material is applied. The coating material contains a plurality of primary silica particles. The average particle size of the primary silica particles is 5 nm or more and 20 nm or less.
[0055] The coating material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.
[0056] The content of the solvent in the coating material is preferably 50.0% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50.0% by mass or more and 99.9% by mass or less, the coating material can be easily applied.
[0057] The coating material is preferably applied by a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, or a combination of two or more of these (e.g., dip spin coating). Examples of the wet process include spin coating, dip coating, or dip spin coating.
[0058] The above describes the embodiments of the present disclosure with reference to the drawings. However, the above embodiments are merely examples of the present disclosure, and the present disclosure is not limited to the above embodiments, and can be implemented in various aspects without departing from the gist of the present disclosure. The drawings are mainly schematic illustrations of each component for ease of understanding, and the thickness, length, number, etc. of each component shown in the drawings are different from the actual ones due to the convenience of drawing. In addition, the material, shape, dimensions, etc. of each component shown in the above embodiments are only examples and are not particularly limited, and various modifications are possible within a range that does not substantially deviate from the effects of the present disclosure. The configuration of the embodiment may be appropriately modified within a range that does not exceed the technical idea of the present disclosure. In addition, the embodiments may be implemented in combination within a possible range.
[0059] The present technology can also adopt the following configuration.
[0060] (1) a light-transmitting member that transmits visible light; a hydrophilic layer covering the light-transmitting member; Equipped with the hydrophilic layer contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide, The average particle size of the primary particles of the titanium dioxide is 5 nm or more and 20 nm or less, An optical member, wherein the average particle size of the secondary particles of the titanium dioxide is 15 nm or more and 100 nm or less.
[0061] (2) The optical member according to (1), wherein the thickness of the hydrophilic layer is 20 nm or more and 200 nm or less.
[0062] (3) The optical member according to (1) or (2), wherein the titanium dioxide is anatase type titanium dioxide.
[0063] (4) The hydrophilic layer further includes a coating layer disposed on the hydrophilic layer, The coating layer contains a plurality of primary particles of silica, The optical member according to any one of (1) to (3), wherein the average particle size of the primary particles of the silica is 5 nm or more and 20 nm or less.
[0064] (5) The optical member according to (4), wherein the coating layer has a thickness of 5 nm or more and 20 nm or less.
[0065] (6) The optical member according to any one of (1) to (5), further comprising an anti-reflection film disposed between the light-transmitting member and the hydrophilic layer.
[0066] (7) A lens unit comprising the optical member according to any one of (1) to (6). EXAMPLES
[0067] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.
[0068] <Manufacturing of optical components> Optical members according to Examples 1 to 7 and optical members according to Comparative Examples 1 to 4 were manufactured.
[0069] <Example 1> <Preparation steps> A lens ("TAFD-5G" manufactured by HOYA Corporation, composition: glass, diameter 12.9 mm, refractive index: 1.835) was prepared as a light-transmitting member. One surface of the lens was a convex surface (radius of curvature 12 mm) and the other surface was a concave surface (radius of curvature 3.07 mm).
[0070] An anti-reflection film was formed on the convex surface of the lens by vapor deposition. The total number of low and high refractive index layers in the anti-reflection film was nine. Of these, the first, third, fifth, seventh and ninth layers were low refractive index layers. The second, fourth, sixth and eighth layers were high refractive index layers.
[0071] <Application step> A hydrophilic material of Example 1 was prepared, containing 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle size of 7 nm), 0.5 parts by mass of silicon dioxide, 2 parts by mass of water, 76 parts by mass of isopropyl alcohol, 20 parts by mass of methanol, and 1 part by mass of nitric acid.
[0072] The hydrophilic material according to Example 1 was applied onto the anti-reflection film. Specifically, 100 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member. Next, the light-transmitting member was rotated at a rotation speed of 5000 rpm using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.). At this time, the rotation axis was aligned with the optical axis of the light-transmitting member.
[0073] <Drying step> A heat treatment was carried out at 90° C. for 30 minutes to form a hydrophilic layer having a thickness of 200 nm. The average particle size of the secondary particles of titanium dioxide was 60 nm.
[0074] <Coating material application step> A coating material according to Example 1 was prepared, containing 1 part by mass of silica particles (average particle size of primary particles: 5 nm), 99 parts by mass of water, and 0.2 parts by mass of ammonia. The coating material according to Example 1 was applied onto the hydrophilic layer. Specifically, 60 μL of the coating material according to Example 1 was dropped onto the optical axis of the light-transmitting member. Next, the light-transmitting member was rotated at a rotation speed of 5000 rpm using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.). At this time, the rotation axis was aligned with the optical axis of the light-transmitting member. A heat treatment was performed at 120° C. for 30 minutes to form a coating layer having a thickness of 5 nm, and an optical member according to Example 1 was obtained.
[0075] <Example 2> An optical member according to Example 2 was manufactured in the same manner as the optical member according to Example 1, except that in the <coating step>, 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle diameter 20 nm) were used instead of 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle diameter 7 nm), and 80 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the translucent member instead of 100 μL of the hydrophilic material according to Example 1. The thickness of the hydrophilic layer was 100 nm.
[0076] <Example 3> An optical member according to Example 3 was produced in the same manner as in the production of the optical member according to Example 1, except that in the <drying step>, heat treatment at 80° C. for 30 minutes was performed instead of at 90° C. for 30 minutes. The average particle size of the secondary particles of titanium dioxide was 100 nm.
[0077] <Example 4> An optical member according to Example 4 was manufactured in the same manner as the optical member according to Example 1, except that in the <coating step>, 50 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member instead of 100 μL of the hydrophilic material according to Example 1. The thickness of the hydrophilic layer was 19 nm.
[0078] <Example 5> An optical member according to Example 5 was manufactured in the same manner as the optical member according to Example 1, except that in the <coating step>, 110 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member instead of 100 μL of the hydrophilic material according to Example 1. The thickness of the hydrophilic layer was 201 nm.
[0079] <Example 6> The optical member of Example 6 was manufactured in the same manner as the optical member of Example 1, except that the <coating material application step> was not performed.
[0080] <Example 7> The optical member of Example 7 was manufactured in the same manner as the optical member of Example 6, except that in the <preparatory step>, instead of forming an antireflection film on the convex surface of the lens, an antireflection film was not formed on the convex surface of the lens.
[0081] <Comparative Example 1> The optical member of Comparative Example 1 was manufactured in the same manner as the optical member of Example 1, except that in the <Coating Step>, 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle diameter of 7 nm) were used instead of 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle diameter of 4 nm).
[0082] <Comparative Example 2> An optical member according to Comparative Example 2 was manufactured in the same manner as in the manufacture of the optical member according to Example 1, except that in the <Coating Step>, 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle diameter of 7 nm) were used instead of 0.5 parts by mass of titanium dioxide particles (anatase type titanium dioxide, average primary particle diameter of 25 nm).
[0083] <Comparative Example 3> An optical member according to Comparative Example 3 was produced in the same manner as in the production of the optical member according to Example 1, except that in the <drying step>, heat treatment at 120° C. for 30 minutes was carried out instead of at 90° C. for 30 minutes. The average particle size of the secondary particles of titanium dioxide was 14 nm.
[0084] <Comparative Example 4> An optical member according to Comparative Example 4 was produced in the same manner as in the production of the optical member according to Example 1, except that in the <drying step>, heat treatment at 70° C. for 30 minutes was performed instead of at 90° C. for 30 minutes. The average particle size of the secondary particles of titanium dioxide was 250 nm, and the thickness of the hydrophilic layer was 250 nm.
[0085] <Evaluation> By the following methods, the reflectance, contact angle, and abrasion test were measured for the optical members according to Examples 1 to 7 and Comparative Examples 1 to 4. The measurement results are shown in Table 1 below. All measurements were performed in an environment with a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.
[0086] <Reflectance> Using a reflectance measuring device (Olympus Corporation, "USPM-RU"), the maximum reflectance of the optical members was measured for light having a wavelength of 480 nm or more and 780 nm or less. The incident angle of the incident light was set to 0 degrees. The maximum reflectance of the optical members was evaluated according to the following criteria. The evaluation results are shown in Table 1.
[0087] ○: 1.0% or less △: More than 1.0% but less than 1.5% ×: More than 1.5%
[0088] <Contact angle recovery> Before using the optical member, the static contact angle with respect to pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). After using the optical member, the static contact angle with respect to pure water was measured using an ultraviolet light source (peak wavelength 365 nm, FL15BL-B, manufactured by Toshiba Corporation) with an illuminance of 1 mW / cm. 2 The optical component was irradiated with ultraviolet light of 1000 nm. Thereafter, the static contact angle with respect to pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). The static contact angle before use was calculated relative to the static contact angle after irradiation. The degree of recovery of the contact angle of the optical component was evaluated according to the following criteria. The evaluation results are shown in Table 1.
[0089] 〇: 80% or more △: 70% or more but less than 80% ×: Less than 70%
[0090] <Wear test> The optical components were placed in an abrasion tester and abraded 1,000 times with a car wash brush with a load of 1 kg applied to the surface. They were then observed at 466x magnification with a laser microscope. The durability of the optical components was evaluated according to the following criteria. The evaluation results are shown in Table 1.
[0091] 〇: No optical influence △: Some optical effect ×: Optical influence present
[0092] [Table 1]
[0093] The optical members according to Comparative Example 1 to Comparative Example 4 were not good in terms of the degree of recovery of the contact angle. In contrast, the optical members according to Examples 1 to 7 were good in terms of the degree of recovery of the contact angle. In particular, the optical members according to Examples 1 to 3, 6, and 7 were good in terms of the degree of recovery of the contact angle. [Explanation of symbols]
[0094] 10...Translucent member 20...Hydrophilic layer 100 Optical components
Claims
1. a light-transmitting member that transmits visible light; a hydrophilic layer covering the light-transmitting member; Equipped with the hydrophilic layer contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide, The average particle size of the primary particles of the titanium dioxide is 5 nm or more and 20 nm or less, An optical member, wherein the average particle size of the secondary particles of the titanium dioxide is 15 nm or more and 100 nm or less.
2. The optical member according to claim 1 , wherein the hydrophilic layer has a thickness of 20 nm or more and 200 nm or less.
3. 2. The optical member according to claim 1, wherein the titanium dioxide is anatase type titanium dioxide.
4. Further comprising a coating layer disposed on the hydrophilic layer, The coating layer contains a plurality of primary particles of silica, 2. The optical member according to claim 1, wherein the average particle size of the primary particles of the silica is 5 nm or more and 20 nm or less.
5. The optical member according to claim 4 , wherein the coating layer has a thickness of 5 nm or more and 20 nm or less.
6. The optical member according to claim 1 , further comprising an anti-reflection film disposed between the light-transmitting member and the hydrophilic layer.
7. A lens unit comprising the optical member according to claim 1 .
8. A coating step of coating a hydrophilic material; a drying step of drying the hydrophilic material to form a hydrophilic layer; Including, the hydrophilic material comprises a plurality of primary particles of titanium dioxide; The average particle size of the primary particles of the titanium dioxide is 5 nm or more and 20 nm or less, the hydrophilic layer contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide, The method for producing an optical member, wherein the average particle size of the secondary particles of the titanium dioxide is 15 nm or more and 100 nm or less.
Citation Information
Patent Citations
Hydrophilic lens
JP2018077260A