Repair agent for cast iron tube inner surface and cast iron tube having repaired inner surface
A two-part epoxy resin repair agent with triethylenetetramine and pigments addresses the inefficiencies of existing methods, offering quick and heat-resistant repairs for cast iron pipes, suitable for high-temperature environments.
Patent Information
- Application Number
- JP2023074525
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for repairing casting defects in cast iron pipes, such as heating and melting defects or using resin repair agents with low heat resistance, are time-consuming and costly, and do not effectively address the need for high-temperature applications.
A two-part epoxy resin repair agent containing triethylenetetramine as a hardening agent, along with pigments like iron powder, calcium carbonate powder, and nickel powder, with specific mass ratios, allowing for quick and heat-resistant repairs.
The repair agent enables easy and rapid repair of cast iron pipes with excellent heat resistance, enabling subsequent high-temperature applications without adverse effects, and provides a smooth, durable repair surface.
Smart Images

Figure 2024158902000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a repair agent for the inner surface of a cast iron pipe and a cast iron pipe having an inner recess repaired with said repair agent. [Background technology]
[0002] Straight ductile iron pipes, which are mainly used as water pipes, are usually manufactured by centrifugal casting. When manufacturing cast iron pipes by centrifugal casting, casting defects (dents) may occur on the inner surface of the cast iron pipe. In such cases, the casting defects are generally repaired by welding iron-based materials or applying a resin repair agent.
[0003] Patent Document 1 discloses that a casting defect is heated and melted by arc or plasma to bring the defect to the surface, and then a filler material is added to the molten part to perform overlay welding to repair the defect.
[0004] Furthermore, Patent Document 2 discloses a defect repair agent for aluminum castings that can reduce deformation while maintaining hardness at high temperatures, which is a heat-resistant epoxy resin mixed with 10 to 60% by volume of inorganic material powder that is harder and has a smaller thermal expansion coefficient than aluminum. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 165292 / 1983 [Patent Document 2] JP 2003-183477 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the process of heating and melting the casting defect itself, as in Patent Document 1, is troublesome and time-consuming, resulting in high costs.
[0007] Furthermore, in the case of ductile iron pipes, the pipes are heated to 240°C or higher before the epoxy resin powder coating is applied to the inner surface, but the resin filler described in Patent Document 2 only has a heat resistance of about 200°C, making it difficult to apply to the repair of ductile iron pipes.
[0008] Therefore, an object of the present invention is to provide a repair agent that can be easily and quickly repaired and has excellent heat resistance, and further to provide a cast iron pipe in which the repaired recess on the inner surface of the pipe has excellent heat resistance. [Means for solving the problem]
[0009] In view of the above problems, the applicant of the present invention has discovered that the above problems can be solved by a two-component epoxy resin repair agent that contains at least triethylenetetramine as a curing agent, contains predetermined amounts of pigments including iron powder, calcium carbonate powder and nickel powder, and further contains a predetermined amount of calcium carbonate powder, thereby completing the present invention.
[0010] That is, the present invention provides [1] A repair agent for the inner surface of a cast iron pipe, comprising a first agent containing an epoxy resin and a second agent containing a hardener, The hardener contains at least triethylenetetramine, The repair agent contains 60 to 78 mass % of pigments including iron powder, calcium carbonate powder, and nickel powder, and The content of calcium carbonate powder in the repair agent is 45 to 65% by mass. Repair agent for the inside of cast iron pipes, and [2] A cast iron pipe in which the mixture of the repair agent for the inner surface of the cast iron pipe described in [1] above is filled into the recesses on the inner surface of the pipe and hardened. Regarding. Effect of the Invention
[0011] According to the present invention, in a repair agent for the inner surface of a cast iron pipe, which is composed of a first agent containing an epoxy resin and a second agent containing a hardener, the hardener contains at least triethylenetetramine, and the pigment containing iron powder, calcium carbonate powder, and nickel powder is contained in the repair agent at 60 to 78 mass %, and the content of calcium carbonate powder in the repair agent is 45 to 65 mass %, thereby providing a repair agent for the inner surface of a cast iron pipe that can be easily repaired in a short time and has excellent heat resistance. Also, by filling a mixture of this repair agent for the inner surface of a cast iron pipe into a recess on the pipe inner surface and hardening it, a cast iron pipe that has been repaired with excellent heat resistance can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Repair agent for the inside of cast iron pipes> One aspect of the present invention relates to a repair agent for the inner surface of a cast iron pipe, which comprises a first agent containing an epoxy resin and a second agent containing a curing agent, and is characterized in that the curing agent contains at least triethylenetetramine, the repair agent contains 60 to 78 mass% of pigments including iron powder, calcium carbonate powder, and nickel powder, and the content of calcium carbonate powder in the repair agent is 45 to 65 mass%.
[0013] In this specification, all repair agents according to the present invention are repair agents for the inner surface of cast iron pipes, and "repair agent for the inner surface of cast iron pipes" is also simply referred to as "repair agent".
[0014] (First Agent) The first agent constituting the repair agent for the inner surface of cast iron pipes of the present invention is not particularly limited as long as it contains an epoxy resin, but it is preferable that it also contains a pigment described below. The first agent corresponds to the so-called main agent in a two-liquid type epoxy resin composition, and naturally does not contain a hardener.
[0015] (Epoxy resin) The epoxy resin contained in the first agent is not particularly limited, and examples thereof include bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, novolac type epoxy resins, cyclic aliphatic epoxy resins, glycidylamine type resins, heterocyclic epoxy resins, polyfunctional epoxy resins, epoxy ester resins, etc. Among these, heat-resistant epoxy resins such as bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins are preferred, and bisphenol type epoxy resins are preferably used from the viewpoint of adhesion to the substrate.
[0016] The content of the epoxy resin in the repair agent used in the present invention is preferably 15% by mass or more, more preferably 18% by mass or more. By making the content of the epoxy resin 15% by mass or more, the film-forming property during curing tends to be improved. In addition, the content of the epoxy resin in the repair agent is preferably 25% by mass or less, more preferably 24% by mass or less. By making the content of the epoxy resin 25% by mass or less, the heat resistance tends to be improved.
[0017] (Second agent) The second agent constituting the repair agent for the inner surface of cast iron pipes of the present invention is not particularly limited as long as it contains a hardener, and it is preferable that it also contains a pigment described below. The second agent corresponds to the so-called hardener in a two-liquid type epoxy resin composition, and naturally does not contain an epoxy resin.
[0018] (hardening agent) The repair agent for the inner surface of a cast iron pipe of the present invention contains at least triethylenetetramine as a curing agent. Triethylenetetramine is preferably used in combination with other curing agents, and the other curing agents are not particularly limited as long as they have the property of contributing to the crosslinking reaction between the epoxy groups of the epoxy resin and curing the epoxy resin. Specific compounds of the other curing agents include amine compounds other than triethylenetetramine, amide compounds, imidazole compounds, imidazoline compounds, hydrazide compounds, acid anhydrides, and phenolic compounds, and one or more of these can be used in combination. Among them, it is preferable to use one or more amine compounds other than triethylenetetramine in combination from the viewpoint of adjusting the appropriate curing speed and improving heat resistance.
[0019] Examples of the amine compounds include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines. Specifically, examples of the aliphatic amines include, in addition to triethylenetetramine, ethylenediamine, 1,3-diaminopropane, 1,4-diaminopropane, hexamethylenediamine, 2,5-dimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, iminobispropylamine, bis(hexamethylene)triamine, tetraethylenepentamine, pentaethylenehexamine, N-hydroxyethylethylenediamine, and tetra(hydroxyethyl)ethylenediamine. Examples of the polyether amines include triethyleneglycoldiamine, tetraethyleneglycoldiamine, diethyleneglycolbis(propylamine), polyoxypropylenediamine, and polyoxypropylenetriamine. Examples of alicyclic amines include isophoronediamine, methacenediamine, N-aminoethylpiperazine, bis(4-amino-3-methyldicyclohexyl)methane, bis(aminomethyl)cyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, and norbornenediamine. Examples of aromatic amines include tetrachloro-p-xylylenediamine, m-xylylenediamine, p-xylylenediamine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, 2,4-diaminodiphenylsulfone, 4,4'-diaminodiphenylsulfone, m-aminophenol, m-aminobenzylamine, benzyldimethylamine, 2-dimethylaminomethyl)phenol, triethanolamine, methylbenzylamine, α-(m-aminophenyl)ethylamine, α-(p-aminophenyl)ethylamine, diaminodiethyldimethyldiphenylmethane, and α,α'-bis(4-aminophenyl)-p-diisopropylbenzene. Among them, it is particularly preferable to use triethylenetetramine in combination with other aliphatic amines and alicyclic amines.
[0020] When triethylenetetramine is used in combination with other curing agents, the content of triethylenetetramine in the repair agent of the present invention is preferably 12% by mass or more, more preferably 13% by mass or more, based on the total mass of the curing agent. By making the content of triethylenetetramine in the repair agent 12% by mass or more, based on the total mass of the curing agent, there is a tendency that an appropriate curing speed can be achieved. In addition, the content of triethylenetetramine in the repair agent is preferably 20% by mass or less, more preferably 18% by mass or less, based on the total mass of the curing agent. By making the content of triethylenetetramine in the repair agent 20% by mass or less, based on the mass of the curing agent, there is a tendency that the decrease in workability due to the increase in the curing speed can be easily suppressed.
[0021] In addition, the total content of the curing agent in the repair agent of the present invention is preferably 40% by mass or more relative to the mass of the epoxy resin. By making the total content of the curing agent in the repair agent 40% by mass or more relative to the mass of the epoxy resin, the curing speed tends to increase. In addition, the total content of the curing agent in the repair agent is preferably 47% by mass or less relative to the mass of the epoxy resin. By making the total content of the curing agent in the repair agent 47% by mass or less relative to the mass of the epoxy resin, the decrease in workability due to the increase in the curing speed tends to be suppressed.
[0022] (Pigments) The repair agent for the inner surface of cast iron pipes of the present invention contains 60 to 75 mass% of pigments including iron powder, calcium carbonate powder, and nickel powder in the repair agent. These pigments may be mixed in the first agent or the second agent, and are usually mixed separately in each agent so that the first agent and the second agent are easily prepared. The pigments may contain pigments other than iron powder, calcium carbonate powder, and nickel powder, but it is necessary to contain 45 to 65 mass% of calcium carbonate powder in the repair agent.
[0023] The content of the pigment in the repair agent of the present invention is 60% by mass or more, preferably 63% by mass or more. If the content of the pigment in the repair agent is less than 60% by mass, the heat resistance tends to decrease. In addition, the content of the pigment in the repair agent is 78% by mass or less, preferably 75% by mass or less. If the content of the pigment in the repair agent exceeds 78% by mass, the viscosity of the repair agent increases, and the workability during kneading and repair tends to decrease.
[0024] The content of iron powder in the repair agent of the present invention is preferably 10% by mass or more. By making the content of iron powder in the repair agent 10% by mass or more, the strength of the repair agent after hardening tends to increase. In addition, the content of iron powder in the repair agent is preferably 20% by mass or less. By making the content of iron powder in the repair agent 20% by mass or less, it becomes easier to add an appropriate amount of calcium carbonate powder to improve heat resistance.
[0025] The content of calcium carbonate powder in the repair agent of the present invention is 45% by mass or more, preferably 48% by mass or more. If the content of calcium carbonate powder in the repair agent is less than 45% by mass, the heat resistance tends to decrease. In addition, the content of calcium carbonate powder in the repair agent is 65% by mass or less, preferably 63% by mass or less. If the content of calcium carbonate powder in the repair agent exceeds 65% by mass, it becomes difficult to appropriately add iron powder to improve the strength of the hardener after hardening.
[0026] The content of nickel powder in the repair agent of the present invention is preferably 3 mass% or more. By making the content of nickel powder in the repair agent 3 mass% or more, the heat resistance and the strength of the curing agent after curing tend to increase.
[0027] Specific examples of pigments other than iron powder, calcium carbonate powder, and nickel powder include metal or ceramic materials such as stainless steel powder, alumina powder, and silica; color pigments such as titanium oxide, iron oxide, carbon black (for example, trade name MA100, manufactured by Mitsubishi Chemical Corporation), cyanine blue, and cyanine green; extender pigments such as calcium carbonate, talc, barium sulfate, and clay; and rust-preventive pigments such as zinc phosphate, calcium phosphate, and aluminum phosphomolybdate. These may be used alone, or two or more of them may be mixed together as necessary.
[0028] (Repair agent) The repair agent for the inner surface of cast iron pipes of the present invention comprises the above-mentioned first and second agents, and may be in the form of a kit consisting of separate containers containing each agent, or in the form of each agent being contained in each chamber of a multi-chamber container having a partition wall that communicates with each other when in use.
[0029] Since the repair agent of the present invention is a two-part type, the first and second parts are mixed, for example, kneaded, when used, and the resulting mixture, for example, kneaded product, is preferably in a paste or putty form. In addition, since the epoxy resin starts to harden when the first and second parts are mixed, the repair agent of the present invention needs to be used while it maintains a softness suitable for use after mixing or kneading. For this reason, it is preferable to mix or knead the first and second parts of the repair agent of the present invention between immediately before and 10 minutes before use, and it is most preferable to perform a filling operation continuously from mixing or kneading the first and second parts.
[0030] The method of mixing or kneading the first and second parts in the repair agent of the present invention is not particularly limited, but can be performed manually or the like.
[0031] The repair agent for the inner surface of a cast iron pipe of the present invention is filled into the recesses on the inner surface of the cast iron pipe, but the size and depth of the recesses are not particularly limited as long as they can be filled and hardened by the repair agent for the inner surface of a cast iron pipe of the present invention. Usually, it is particularly preferable to apply the repair agent for the inner surface of a cast iron pipe of the present invention to repair recesses caused by casting defects on the inner surface of a centrifugally cast cast iron pipe. With the repair agent for the inner surface of a cast iron pipe of the present invention, repair can be performed by simply filling the mixture of the first agent and the second agent into the recesses with a spatula, trowel, etc., and it does not take much time to harden, and the repaired area can have a smooth surface. In order to further improve the smoothness of the surface, surface treatment can be performed with a grinder or the like after hardening.
[0032] (Cast Iron Pipe) The cast iron pipes to which the cast iron pipe inner surface repair agent of the present invention is applied are not particularly limited, and may be used for water supply and sewerage, water storage, etc., but from the viewpoint of being able to more effectively exert the effects of the present invention, it is preferable to use centrifugally cast cast iron pipes for water supply and sewerage, which have an epoxy resin powder coating on the inner surface, and which may be heated to extremely high temperatures after repair.
[0033] <Repaired cast iron pipe> In another aspect of the present invention, a cast iron pipe is provided in which a recess on the inner surface of the pipe has been repaired with the above-mentioned repair agent for the inner surface of the cast iron pipe. The repair method is as described above, and it is possible to provide a cast iron pipe that has been repaired with excellent heat resistance, and further to provide a cast iron pipe with improved surface smoothness at the repaired portion.
[0034] In this way, the cast iron pipe whose inner surface has had its recesses repaired with the repair agent for the inner surface of cast iron pipes of the present invention has excellent heat resistance, so even if the pipe is heated to a high temperature of 240°C or higher immediately after the repair in order to perform epoxy resin powder coating after the repair, the repair agent is not adversely affected, and the subsequent epoxy resin powder coating can be carried out successfully.
[0035] In addition, unless otherwise stated, all of the contents described above in the repair agent of the present invention are applicable to the cast iron pipe of the present invention, and all of the contents described above in the cast iron pipe of the present invention are applicable to the repair agent of the present invention. EXAMPLES
[0036] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0037] First, the components used in the examples are shown below. (Epoxy resin) Epoxy resin: BPA-type epoxy resin (EPICLON 850, manufactured by DIC Corporation) (hardening agent) Tetraethylenepentamine: T0098 (Tokyo Chemical Industry Co., Ltd.) Triethylenetetramine: T0429 (Tokyo Chemical Industry Co., Ltd.) N-(2-aminoethyl)piperazine: A2517 (Tokyo Chemical Industry Co., Ltd.) (Pigments) Iron powder: MT032500 (Mitsuwa Chemical Co., Ltd.) Calcium carbonate powder: 03000625 (Kyowa Pure Chemical Industries, Ltd.) Nickel powder: Ni-HWQ 5μm-W (manufactured by Fukuda Metal Foil and Powder Co., Ltd.)
[0038] Examples 1 and 2 and Comparative Examples 1 and 2 The components were mixed according to the composition in Table 1 to prepare the first and second agents. The first and second agents were then kneaded with a spatula in a mass ratio of 1:1 to obtain a kneaded product. The obtained kneaded products were evaluated in the following Test Examples 1 to 3. Note that the preparation of the kneaded products in each Test Example was carried out within 10 minutes before application to the cast iron pieces.
[0039] [Table 1]
[0040] Test Example 1: Curability A ductile iron pipe (φ300×150 mm) was cut and processed, and the inner surface was polished to clean the resulting cast iron piece (150×90 mm). A roughly circular depression was then formed on the inner surface of the resulting piece, 10 mm in diameter and 1 mm deep, in plan view, using a hand drill. The kneaded material (repair agent) obtained in Examples 1 and 2 and Comparative Examples 1 and 2 was filled into the depression using a spatula, and the surface was then smoothed using the spatula. The sample was then left for 4 hours in an environment of room temperature 25° C. and humidity 50%, and the hardening state was evaluated by touching it with a finger according to the following criteria. The results are shown in Table 1. Note that the surface of Comparative Example 2 was rough, and it was not possible to judge whether it was sticky or not. ○: No stickiness (sufficiently cured) ×: Sticky (poor curing)
[0041] Test Example 2: Heat resistance The cast iron pieces filled with the repair agent and hardened in the same manner as in Test Example 1 were left in a heating furnace at 270°C for 7 hours, after which the appearance of the repaired portion was visually inspected and the heat resistance of the repair agent was evaluated according to the following criteria. As for Comparative Example 2, as described above, the hardenability could not be judged in Test Example 1, so Test Example 2 was not carried out. ○: No abnormalities in appearance ×: Repair agent has abnormalities such as blisters or cracks on the surface.
[0042] Test Example 3: Film Formation Except for changing the standing time to 24 hours, ductile cast iron pieces were obtained in the same manner as in Test Example 1. The obtained cast iron pieces were visually inspected and touched with the fingers to evaluate the film formation state according to the following criteria. ○: The surface is smooth ×: The surface is rough (aggregates are floating)
[0043] From Table 1, it can be seen that the repair agents of Examples 1 and 2, in which the hardener contains at least triethylenetetramine, and further contains 60 to 75 mass% of pigments including iron powder, calcium carbonate powder, and nickel powder, and the content of calcium carbonate powder in the repair agent is 45 to 65 mass%, enable simpler and more heat-resistant repair than Comparative Examples 1 and 2.
Claims
1. A repair agent for the inner surface of a cast iron pipe, comprising a first agent containing an epoxy resin and a second agent containing a hardener, The hardener contains at least triethylenetetramine, The repair agent contains 60 to 78 mass % of pigments including iron powder, calcium carbonate powder, and nickel powder, and The content of calcium carbonate powder in the repair agent is 45 to 65 mass %. Repair agent for the inside of cast iron pipes.
2. 2. A cast iron pipe having a recess on its inner surface filled with a mixture of the repair agent for the inner surface of a cast iron pipe according to claim 1 and hardened.
Citation Information
Patent Citations
Numerical controller
JP1982017019A
Repairing method of pipe
JP1982107495A
Lining resin composition
JP1984059719A
Ductile cast iron pipe
JP1986006481A
Epoxy resin composition
JP2012012518A