Can container, and can container manufacturing method

By limiting lubricant residue to 2 mg/can or less and employing treatments like thermal energy and plasma treatment, the can container design addresses ink repellency and hygiene issues, ensuring effective ink adhesion and successful film insertion, thus improving can container quality.

JP2024158920APending Publication Date: 2024-11-08TOYO SEIKAN KAISHA LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023074551
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing can containers face issues with lubricant residue in the reduced diameter portion leading to ink repellency and hygiene concerns, particularly when forming ink printing layers, and the use of lubricants can cause insertion failures with shrink films.

Method used

The can container design limits lubricant presence to 2 mg/can or less in the reduced diameter section, using methods like thermal energy, plasma treatment, or flame treatment to remove excess lubricant, and employs ink printing layers that may include shrink films or adhesive labels to enhance hygiene and prevent ink repellency.

Benefits of technology

This approach reduces defects and improves hygiene by minimizing lubricant residue, ensuring effective ink adhesion and successful insertion of shrink films, thereby enhancing the quality and functionality of the can containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158920000001_ABST
    Figure 2024158920000001_ABST
Patent Text Reader

Abstract

To enhance a sanitation property by preventing printing failure.SOLUTION: According to the first embodiment of the present invention, there is provided a can container comprising a reduced diameter part 20 and a can-trunk part 40, and a lubricant present in the reduced diameter part has an amount of 2 mg / can or less. According to the second embodiment, there is provided a can container manufacturing method comprising: a molding step of molding a cylindrical can body 110 from a sheet material provided with a metal sheet and a resin film layer for covering at least one face of the metal sheet, or from a sheet material provided with a metal sheet; a lubrication step of coating the lubricant onto the molded can body; a diameter-reducing step of diameter-reducing part of the can body to form the reduced diameter part; and a printing layer formation step of forming an ink printing layer onto an outer peripheral face of the can body.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a can container and a method for manufacturing a can container. [Background technology]

[0002] It is known that in can containers such as beverage cans, a protective layer is formed on the surface of the can body to protect the can body when it is reduced in diameter. For example, Patent Document 1 states that "A base coater (BC) and an overburnisher (OV) are provided before the necker flanger (SDN), and an inside sprayer (INS) is also provided. As a result, in this embodiment, neck processing is performed after protective layers are formed on the outer and inner surfaces of the can body, making it less likely that scratches will occur on the can body (paragraph 0025)." Furthermore, Patent Document 2 describes the lamination technique as follows: "In a manufacturing method for organic resin-coated metal sheets, a heated and molten organic resin is extruded from a T-die in the form of a film directly onto a continuously supplied long strip-shaped metal sheet, and the two are sandwiched and pressed between a pair of laminating rolls, the laminating roll is opened when the seam of the metal sheet (hereinafter referred to as the "stitcher") passes through the laminating roll section, and the laminating roll is replaced by a pair of auxiliary laminating rolls (hereinafter referred to as the "auxiliary rolls") for sandwiching and pressing, and after passing through the stitcher, the auxiliary roll is opened, and the laminating rolls are sandwiched and pressed. (Claim 1)" [Prior art document] [Patent documents] [Patent Document 1] JP 2019-025521 A [Patent Document 2] JP 2004-25640 A Summary of the Invention

[0003] In a first aspect of the present invention, there is provided a can container having a necked portion and a can body portion. The amount of lubricant present in the necked portion may be 2 mg / can or less.

[0004] In the above, the can container may have a layer structure including a cylindrical can body and an ink-printed layer formed on the outer surface of the can body. The amount of lubricant present on the outer surface side of the can body at the reduced diameter portion may be 2 mg / can or less.

[0005] In the above, the ink-printed layer may be a layer formed directly on the can body and the ink cured.

[0006] In the above, the ink-printed layer may be a shrink film that further covers the can body from the outside and has an ink image printed thereon.

[0007] In the above, the can container may have a layer structure including a cylindrical can body and a resin film layer covering at least the outer surface of the can body. The amount of lubricant present on the outer surface of the resin film layer in the narrowed portion may be 2 mg / can or less.

[0008] In the above can container, an ink-printed layer may be formed on the outer surface of the resin film layer. The amount of lubricant present on the outer surface side of the resin film layer in the narrowed portion may be 2 mg / can or less.

[0009] In the above, the ink-printed layer may be a layer formed directly on the resin film layer and in which the ink is cured.

[0010] In the above, the ink-printed layer further covers the resin film layer from the outside, and may be a shrink film on which an ink image is printed.

[0011] In the above, the can container may be a container filled with beverages or food for consumption.

[0012] In a second aspect of the present invention, there is provided a method for manufacturing a can container, comprising a molding step, a lubricating step, a diameter reducing step, and a printed layer forming step. In the molding step, a cylindrical can body may be formed from a sheet material having a metal sheet and a resin film layer covering at least one side of the metal sheet, or a sheet material having a metal sheet. In the lubricating step, a lubricant may be applied to the formed can body. In the diameter reducing step, a diameter reduced portion may be formed by reducing the diameter of a part of the can body. In the printed layer forming step, an ink printed layer may be formed on the outer peripheral surface of the can body.

[0013] In the above, the forming step may be a step of forming a can body from a sheet material having a metal sheet, a resin film, and a lubricating layer formed on one side of the resin film.

[0014] In the above, the forming step may be a step of forming a can body from a sheet material having a metal sheet and a lubricating layer formed on one or both sides of the metal sheet.

[0015] In the above, the method for producing a can container may further include a removing step of removing at least a part of the lubricating layer between the forming step and the lubricating step.

[0016] In a third aspect of the present invention, there is provided a method for manufacturing a can container, comprising a molding step, a diameter reducing step, and a print layer forming step. In the molding step, a cylindrical can body may be molded from a sheet material having a metal sheet, a resin film covering at least one side of the metal sheet, and a lubricating layer formed on one side of the resin film, or a sheet material consisting of a metal sheet and a lubricating layer formed on one or both sides of the metal sheet. In the diameter reducing step, a reduced diameter portion may be formed by reducing the diameter of a part of the can body without applying a lubricant to the molded can body. In the print layer forming step, an ink print layer may be formed on the outer circumferential surface of the can body.

[0017] In the removing step, the lubricant applied in the lubricating step or at least a portion of the lubricating layer may be removed between the diameter reducing step and the print layer forming step.

[0018] In a fourth aspect of the present invention, there is provided a method for manufacturing a can container, comprising a lubrication step, a diameter reduction step, and a storage step. In the lubrication step, a lubricant may be applied to a can body consisting of a cylindrical can body and a resin film layer covering at least the outer surface of the can body, or to a can body consisting of a cylindrical can body. In the diameter reduction step, a diameter reduction portion may be formed by reducing the diameter of a part of the can body. The can body may be stored in a plain state without being printed.

[0019] In a fifth aspect of the present invention, there is provided a method for manufacturing a can container, comprising a forming step, a diameter reducing step, and a storage step. In the forming step, a cylindrical can body may be formed from a sheet material having a metal sheet, a resin film covering at least one side of the metal sheet, and a lubricating layer formed on one side of the resin film. In the diameter reducing step, a reduced diameter portion may be formed by reducing the diameter of a part of the can body without applying a lubricant to the can body. In the storage step, the can body may be stored in a plain state without being printed.

[0020] In the above, the manufacturing method may further include a removing step of removing a portion of the lubricant from the can body between the diameter reducing step and the storing step.

[0021] In the above, the storage step may be carried out in a light-shielding state so that the can body is not irradiated with ultraviolet light.

[0022] In the above, the storage step may include storing the can body in a light-shielded state for one month or more.

[0023] In the above, the printing layer forming step may include printing on the outer surface of the can body by one or more of inkjet printing and printing with a printing plate.

[0024] In the above, the printing layer forming step may include covering the outer surface of the can body with a shrink film on which an ink image is printed.

[0025] In the above, the removal step may use thermal energy (heat set oven), plasma treatment, or flame treatment.

[0026] In the above, the printed layer forming step may include covering the outer surface of the can body with an adhesive label (tack label) on which an ink image is printed.

[0027] The above summary of the invention does not list all of the features of the present invention. Also, subcombinations of these features may also be inventions. [Brief description of the drawings]

[0028] [Figure 1] 1 shows an example of an overall view of a can container 10 in this embodiment. [Diagram 2] 1 shows an example of a cross section of a can container 10 in this embodiment. [Diagram 3] 2 shows another example of a cross section of the can container 10 in this embodiment. [Figure 4] An example of a flow of a method for manufacturing the can container 10 in this embodiment will be shown. [Diagram 5] An example of a sub-flow (wet molding) of S100 in FIG. 4 is shown. [Figure 6] Another example of the subflow (dry molding) of S100 in FIG. 4 is shown. [Figure 7] Another example of the flow of the method for manufacturing the can container 10 in this embodiment is shown. [Figure 8] Another example of the flow of the method for manufacturing the can container 10 in this embodiment is shown. [Figure 9] Another example of the flow of the method for manufacturing the can container 10 in this embodiment is shown. [Figure 10] Another example of the flow of the method for manufacturing the can container 10 in this embodiment is shown. [Figure 11] Another example of the flow of the method for manufacturing the can container 10 in this embodiment is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present invention will be described below through embodiments of the invention, but the following embodiments do not limit the scope of the invention according to the claims. Furthermore, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.

[0030] 1 shows an example of an overall view of a can container 10 according to the present embodiment. The can container 10 according to the present invention has a lubricant amount present in the reduced diameter portion of 2 mg / can or less, thereby preventing defects in the can body and / or printing formed on the can body surface and improving hygiene.

[0031] The can container 10 may be used for consumption by being filled with beverages or food. The can container 10 may also be filled with contents other than food and beverages, such as medicines, chemicals, gases, liquids and / or solids.

[0032] The can container 10 has a reduced diameter portion 20 provided on one end side, a bottom portion 30 provided on the other end side, and a can body portion 40.

[0033] The reduced diameter portion 20 is a portion where one end of the can container 10 is reduced in diameter. The reduced diameter portion 20 may be provided at the opening of the can container 10. The reduced diameter portion 20 may be formed so that the outer diameter becomes gradually smaller as it approaches one end of the can container 10.

[0034] The reduced diameter portion 20 may be formed by performing neck processing on the end of the can container 10 before the diameter is reduced. The reduced diameter portion 20 may have a flange formed at the same time as the neck processing. A can lid can be attached by the formed flange. By providing the reduced diameter portion 20 on the can container 10, the amount of can lids used to be attached to the opening of the can container 10 can be reduced. The can container 10 may have a can lid attached.

[0035] The bottom 30 is a bottom formed at the other end of the can container 10. The bottom 30 allows the can container 10 to hold a filling such as a beverage. The bottom 30 may be formed so that the outer diameter of the bottom 30 gradually decreases toward the other end of the can container 10. The bottom surface of the bottom 30 may be formed in a dome shape that is convex upward.

[0036] The can body 40 is the region between the reduced diameter portion 20 and the bottom portion 30 of the can container 10. The can body 40 may be a cylindrical shape with a substantially constant outer diameter in the longitudinal direction (the vertical direction in FIG. 1 ) of the can container 10. The can body 40 has a larger outer peripheral surface area than the reduced diameter portion 20 and the bottom portion 30, and has a substantially constant outer diameter, making it a suitable region for printing on the surface.

[0037] The can body 40 may have a generally uniform, flat surface, or alternatively, the can body 40 may have irregularities such as embossing, or may have bent portions.

[0038] 1, the can container 10 may include three regions: a narrowed diameter portion 20, a bottom portion 30, and a can body portion 40. Alternatively, the can container 10 may not have the narrowed diameter portion 20. For example, when the can container 10 is a straight can or a cup, it may not have the narrowed diameter portion 20.

[0039] 2 shows an example of a cross section of a can container 10 in this embodiment. The can container 10 comprises a can body 110 and an ink-printed layer 120. The can body 110 side (left side of the figure) is the inside of the can container 10, and the ink-printed layer 120 side (right side of the figure) is the outside of the can container 10.

[0040] The can body 110 has a cylindrical shape and forms the structure of the can container 10. The can body 110 may be a seamless can such as a two-piece can or a welded can such as a three-piece can. The can body 110 may be a cup without a metal lid. The can body 110 may be formed of a single metal that can be used for beverage cans and food cans. For example, the can body 110 may be formed of aluminum, steel, or the like.

[0041] The ink-printed layer 120 is a layer of ink images expressing symbols, letters, designs and / or pictures, etc. The ink-printed layer 120 is formed on the outer peripheral surface of the can body 110. The ink-printed layer 120 is formed on at least one of the reduced diameter portion 20 and the can barrel portion 40. Alternatively, the ink-printed layer 120 may not be present.

[0042] The ink-printed layer 120 may be a layer formed directly on the can body 110 and formed by curing the ink. The ink-printed layer 120 may include a coloring material such as a pigment or a dye, a binder resin, and other solids of an ink composition. The ink composition may be, but is not limited to, a water-based ink, a solvent ink, an ultraviolet-curable ink, or an electron beam-curable ink.

[0043] Alternatively, the ink-printed layer 120 may be a shrink film on which an ink image is printed, which further covers the outside of the can body 110. For example, the ink-printed layer 120 may be formed by printing and curing an ink composition on one or both sides of a shrink film and attaching it to the can body 110.

[0044] The ink-printed layer 120 may be a monochrome image or a color image including multiple colors. The ink-printed layer 120 may be a mixture of monochrome and color in different regions.

[0045] A lubricating layer 117, which is a layer of lubricant, may be provided between the can body 110 and the ink-printed layer 120. The lubricating layer 117 may be provided at least in the narrowed portion 20. The lubricating layer 117 may further be provided on the bottom portion 30 and / or the can body portion 40. The presence of the lubricating layer 117 at least in the narrowed portion 20 protects the can body 110 from damage during narrowing.

[0046] The amount of lubricant present in the narrowed portion 20 is 2 mg / can or less. In particular, the amount of lubricant present on the outer surface side of the can body 110 in the narrowed portion 20 may be 2 mg / can or less. "mg / can" indicates the amount of lubricant in the lubricating layer 117 present in one can container 10. By setting the amount of lubricant to 2 mg / can or less, it is possible to prevent ink from being repelled when the ink-printed layer 120 is formed. By setting the amount of lubricant to 2 mg / can or less in places such as the narrowed portion 20 that may come into direct contact with a person's mouth, it is possible to improve the hygiene of the can container 10.

[0047] Furthermore, when the ink-printed layer 120 includes a shrink film, if the amount of lubricant is too large (for example, if the amount of lubricant in the reduced diameter portion 20 exceeds 2 mg / can), insertion failure is likely to occur when inserting the shrink film into the can body 110. From this perspective, it is desirable that the amount of lubricant present in the reduced diameter portion 20 be 2 mg / can or less.

[0048] The amount of lubricant may be 0.01 mg / can or more. In particular, the amount of lubricant present on the outer surface side of the can body 110 at the reduced diameter portion 20 may be 0.01 mg / can or more. By setting the amount of lubricant to 0.01 mg or more, it is possible to maintain lubricity during reduction without causing ink repellency or impairing hygiene. Furthermore, by including a certain amount of lubricant, when the ink-printed layer 20 is formed from a shrink film, it is possible to improve the extrapolation property of the shrink film, and ultimately reduce defects in the can container 10.

[0049] The lubricant may be, for example, one or a combination of one or more selected from waxes of animal or vegetable origin, petroleum waxes, petrolatum, solid paraffin, liquid paraffin, lanolin, polyethylene glycol, edible oils, food-grade lubricants, mineral oils, food-grade greases, and varnishes.

[0050] In particular, when the ink-printed layer 120 includes a shrink film, the lubricant is preferably a solid material, for example, a wax, a petroleum wax, or solid paraffin.

[0051] In this embodiment, the entirety or a part of the can container 10 (e.g., the reduced diameter portion 20) may be immersed in an organic solvent (e.g., a lipophilic solvent such as an alkane or a ketone) to extract the lubricant into the organic solvent, and the lubricant dissolved in the organic solvent may be dried and the measured dry weight may be regarded as the amount of the lubricant. Although this method may cause components other than the lubricant to dissolve from the can container 10, since the main extract is the lubricant, the amount determined by this method may be regarded as the amount of the lubricant. On the other hand, when the extracted components and their content ratio can be determined by chemical analysis such as gas chromatography-mass spectrometry, the total weight of the lubricant components may be regarded as the amount of the lubricant.

[0052] As an example, the amount of lubricant may be measured by the following method. 10 mL of acetone-hexane mixture (1:9) is placed in a 300 mL glass beaker, and the narrowed portion and the flange at the tip of the narrowed portion of the can container held upside down are immersed in the mixture to extract the lubricant and obtain an extract. The extract obtained from 5 can containers is transferred to an eggplant flask and dried under reduced pressure, and then redissolved in 1 mL of acetone-hexane mixture (1:9). This is transferred to an aluminum dish and stored in a thermostatic oven at 75°C for 30 minutes, cooled to room temperature, and then weighed using an electronic balance. The amount of lubricant present in the narrowed portion 20 per can is measured by dividing the weight of the dried product by 5.

[0053] In this embodiment, the ink-printed layer 120 is formed on both the reduced diameter portion 20 and the can body portion 40. Alternatively, the ink-printed layer 120 does not have to be formed on the reduced diameter portion 20.

[0054] The ink printed layer 120 may not be formed on the bottom portion 30. Alternatively, the ink printed layer 120 may be formed on the bottom portion 30.

[0055] The can container 10 may have other layers not shown. For example, an inner surface protective layer may be formed on the inside of the can body 110 (left side of the figure), and / or an outer surface protective layer such as a base coat or varnish may be formed between the can body 110 and the lubricating layer 117. Also, for example, a protective layer may be further formed on the outer surface of the ink-printed layer 120.

[0056] 3 shows a modified cross section of the can container 10 in this embodiment. In this example, the can body 110 is not made of a single metal, but has a layered structure including a can body 112 that serves as a core, and a resin film layer 114 and a resin film layer 116 that cover the inner surface and / or the outer surface of the can body 112. In addition, for example, a protective layer may be further formed on the outer surface of the ink-printed layer 120.

[0057] The can body 112 may be a metal layer that can be used for beverage cans and food cans, such as aluminum or steel. The resin film layer 114 and the resin film layer 116 may be a polyethylene terephthalate (PET) film. For example, the can body 110 may be formed by laminating a PET film to the inner and outer surfaces of a metal plate.

[0058] By using the can body 110 covered with a resin film in this manner, it is possible to prevent the can body 110 from being corroded by the contents. In addition, the amount of lubricant and water used during molding of the can body 110 can be reduced.

[0059] In this embodiment, the lubricating layer 117 and the ink printed layer 120 may have the same configuration as described above unless otherwise specified. For example, the ink printed layer 120 may be a layer formed directly on the resin film layer 116 and formed by hardening the ink. Also, for example, the ink printed layer 120 may be a shrink film that further covers the resin film layer 116 from the outside and has an ink image printed on it. For example, the amount of lubricant in the lubricating layer 117 present on the outer surface of the resin film layer 116 in the reduced diameter section 20 may be 2 mg / can or less. Alternatively, the ink printed layer 120 may not be present.

[0060] Fig. 4 shows an example of a flow of a manufacturing method for a can container 10 in this embodiment. The can container 10 in this embodiment can be manufactured by the processes of S100 to S800 in Fig. 4. For convenience of explanation, the processes of S100 to S800 will be explained in order, but each process may be interchanged and / or some of the processes may be omitted without departing from the spirit of the present invention.

[0061] First, in S100, a molding process is performed in which the bottom 30 and the can body 40 of the can container 10 are formed, thereby forming a cylindrical can body 110. There are two types of molding: wet molding, which uses a coolant, which is a lubricant for cooling, and dry molding, which does not use a coolant.

[0062] In the forming step, a cylindrical can body may be formed from a sheet material. For example, in the case of wet forming, the sheet material may have a metal sheet. Here, a lubricating layer may be formed on one or both sides of the metal sheet. In this case, the forming step may be a step of forming the can body 110 from the sheet material having the metal sheet and the lubricating layer formed on one or both sides of the metal sheet.

[0063] For example, in the case of dry molding, the sheet material may have a metal sheet and a resin film layer covering at least one side of the metal sheet. Here, a lubricating layer may be formed on one side of the resin film layer. In this case, the molding process may be a process of molding the can body 110 from the sheet material having the metal sheet, the resin film layer, and the lubricating layer formed on one side of the resin film layer.

[0064] Fig. 5 shows an example of a subflow (wet molding) of S100 in Fig. 4. S100 (wet molding) may be performed by executing S105 to S140 in Fig. 5.

[0065] In S105, a process (uncoiler) is performed to uncoil and stretch the metal sheet, which is a metal plate material wound in a coil shape. The metal sheet may be, but is not limited to, an aluminum plate or a steel plate. The metal sheet becomes a can body 110 after forming.

[0066] In S110, a process (lubricator) is performed to apply a lubricant (lubricant) to the stretched metal sheet. The lubricant may be a known one. The lubricant includes solids such as wax and liquids such as oils and fats. For example, the lubricant may be one or a combination of one or more selected from animal and vegetable waxes, petroleum wax, petrolatum, solid paraffin, liquid paraffin, lanolin, polyethylene glycol, edible oil, food lubricant, mineral oil, food grease, and emulsions thereof.

[0067] In particular, the lubricant in S110 preferably contains wax. In addition to wax, the lubricant may further contain liquid oil or fat that functions as a coolant. This results in a sheet material having a lubricating layer formed of the lubricant on one or both sides of the metal sheet.

[0068] Instead of forming a lubricating layer on the metal sheet after uncoiler, a metal sheet having a lubricating layer formed on one or both sides in advance may be wound into a coil and uncoiled. A lubricant may be further applied to the metal sheet having a lubricating layer formed in advance.

[0069] In S120, a process of punching the sheet material into a cup shape (cupping press) is performed.

[0070] In S130, the cup-shaped member is drawn and ironed to thin and stretch the sides of the cup. A dome-shaped bottom is also formed at the same time to form the can body 40 and bottom 30 (bodymaker). In S130, a lubricant (coolant) similar to that described in S110 may be additionally used for cooling.

[0071] In S140, a process (trimmer) is performed to remove unnecessary portions of the molded member, thereby forming the can body 110.

[0072] Fig. 6 shows an example of a subflow (dry molding) of S100 in Fig. 4. S100 (dry molding) may be performed by executing S105 to S140 in Fig. 6.

[0073] The process of S105 (uncoiler) may be the same as that of S105 in FIG.

[0074] In S115, a resin film is laminated on both sides or one side of the metal sheet. This results in a sheet material having a metal sheet and a resin film layer. The lamination may be performed by a known method, for example, the method described in JP 2004-25640 A may be used. After molding, the metal sheet becomes the can body 112, and the resin film becomes the resin film layer 114 and the resin film layer 116.

[0075] The resin film may be made of a thermoplastic resin such as polyethylene terephthalate (PET). Instead of the thermoplastic resin, a thermosetting resin such as a thermosetting acrylic resin, a thermosetting epoxy resin, a thermosetting polyurethane resin, or a thermosetting polyester resin may be used. By using the resin film, the same effect as the lubricant used in S110 and S130 in FIG. 5 can be achieved without using a lubricant.

[0076] The thickness of the resin film may be 0.5 μm or more and 30 μm or less. If the thickness of the resin film is less than 0.5 μm, the surface of the resin film becomes less slippery, and there is a risk that the can body 110 may be scratched or metal powder may adhere to the tool when forming the reduced diameter portion 20. If the thickness of the resin film exceeds 30 μm, there is a risk that the resin adhesion after the reduction processing and the flange processing may be poor.

[0077] Before laminating the resin film, a primer composition may be applied to the lamination surface of the metal sheet. For example, a primer composition containing a polyester resin, a curing agent and / or a solvent may be roll-coated on a metal sheet, baked to form a primer layer, and then a resin film may be laminated on the primer layer. The curing agent may be, for example, a resol-type phenolic resin derived from m-cresol.

[0078] The primer composition may further contain a coloring material such as a pigment and / or a food coloring, etc. This can enhance the decorativeness even in a portion of the can container 10 where the ink-printed layer 120 is not provided (e.g., the bottom portion 30, etc.).

[0079] After lamination, a lubricant may be applied to one side of the resin sheet to form a lubricating layer, thereby obtaining a sheet material having a metal sheet, a resin film, and a lubricating layer formed on one side of the resin film.

[0080] Instead of the above S105 to S115, a coil-shaped member in which a metal sheet, a resin film, and a sheet material having a lubricating layer formed on one or both sides of the resin film as necessary are wound in advance may be unwound. For example, after lamination in S115, the sheet material may be wound on a coiler to obtain a coiled sheet material, which may then be unwound again as necessary to perform the following processing. Also, for example, a coiled sheet material may be obtained, unwound, and then the following processing may be performed.

[0081] The processes in S120 to S140 may be similar to those described with reference to Fig. 5. In this way, the can body 110 is formed.

[0082] In S200, a removal step is performed to remove at least a portion of the lubricating layer of the can body 110. The removal step may use a water washing process, a heat treatment (i.e., thermal energy), a plasma treatment, or a flame treatment.

[0083] In particular, when the sheet material includes a resin film layer, the heat treatment can also remove distortion of the resin film caused by molding. For example, the heat treatment may involve heating the molded member at 180 to 220°C for 20 to 90 seconds. As a method for the heat treatment, a hot air heating device, an induction heating (IH) device, and / or an infrared (IR) heating device, etc. may be used.

[0084] The water rinsing process may be with cold or hot water, and the water temperature may be lowered if more lubricant is required, or raised if less lubricant is required.

[0085] The plasma treatment may be an atmospheric pressure plasma treatment. The type of gas used in the atmospheric pressure plasma treatment may be at least one of nitrogen, hydrogen, helium, argon, and oxygen. The flow rate of the gas may be 1 to 200 L per minute. The treatment speed of the atmospheric pressure plasma treatment may be 1 to 100 m per minute. The plasma irradiation time may be 0.5 to 10 seconds.

[0086] In the atmospheric pressure plasma treatment, the minimum distance between the can body 110 and the plasma electrode may be 50 mm or less. Preferably, the minimum distance between the can body 110 and the plasma electrode may be 2 mm or less. There may be one electrode or multiple electrodes. By using multiple electrodes, the treatment capacity can be increased and the treatment time can be shortened.

[0087] Flame treatment is a process in which a reducing flame obtained by mixing and burning a combustible gas such as methane or propane with air or oxygen is applied to the object, and can be performed by a known method. For example, it can be performed by using a burner with a heat power of 35 to 40 μA, setting the distance between the burner tip and the container surface at about 25 to 75 mm, uniformly heat-treating the container surface for 0.5 to 2.0 seconds, and then allowing it to cool to room temperature.

[0088] In the removing step, a plurality of treatments may be combined. For example, in the removing step, water washing and one or more of a heat treatment, a plasma treatment, and a flame treatment may be sequentially performed.

[0089] When the sheet material does not include either a resin film or a lubricating layer, the removal step of S200 may be omitted.

[0090] In S300, a lubrication step is performed in which a lubricant is applied to the molded can body 110. The lubricant may be the same as that used in S110. The lubricant may be a solvent with a particularly high volatility. For example, hexane may be used. This forms a lubricant layer 117.

[0091] After S300 and before S400, an inner surface protective layer may be formed on the inner circumferential surface of the can body 110. For example, the inner surface protective layer may be formed by applying paint to the inner circumferential surface and baking the paint. This makes it possible to prevent the inner circumferential surface from being scratched. In the embodiments shown in Fig. 7 and subsequent figures, the inner surface protective layer may also be formed before the diameter reduction step in S400.

[0092] In S400, a diameter reducing step is performed in which the formed can body 110 is subjected to necking to reduce the diameter of a part of the can body 110 and form the reduced diameter portion 20. The necking may be performed using a known die-necking tool. Simultaneously with or after the necking, the can body 110 may be subjected to flange processing to form a flange for attaching a can lid.

[0093] After necking, a process for removing the lubricating layer may be performed. As an example, at least a part of the lubricating layer may be removed by washing with water or heating, as in S200. A hot air heating device, an induction heating (IH) device, and / or an infrared (IR) heating device may be used as a heating method. In particular, when the printing layer forming step S500 is performed after S200, it is preferable to remove the lubricating layer in order to prevent ink repellency, etc.

[0094] In S500, a printing layer formation step is performed to form an ink-printed layer 120 on the outer peripheral surface of the can body 110. The ink-printed layer 120 may be formed by printing the outer surface of the can body 110 using one or more of inkjet printing and / or printing with a printing plate.

[0095] Inkjet printing may be a method in which an ink composition is ejected directly onto the can body 110 from an inkjet head (IJH) of an inkjet printing device, or an offset method in which an ink composition ejected from the IJH onto a blanket (i.e., a transfer plate) is transferred to the can body 110.

[0096] Printing using a printing plate may be printing using a plate-based printing device. For example, printing using a printing plate may be a method of transferring the ink composition to the can body 110 using a plate such as a relief plate. The ink composition may be directly transferred to the can body 110 using a relief plate, or an offset method may be used in which the ink composition transferred to a blanket (i.e., a transfer plate) is further transferred to the can body 110.

[0097] The ink composition may be a water-based ink, a solvent ink, an ultraviolet-curable ink, or an electron beam-curable ink. The ink composition may contain a colorant selected from pigments and dyes, a resin binder, a monomer / oligomer, an initiator, a solvent, and / or additives such as a dispersant, as necessary.

[0098] After printing, the ink composition may be dried and cured by, for example, air drying, heat treatment, ultraviolet irradiation, electron beam irradiation, or a combination of these, depending on the type of ink composition.

[0099] In particular, by using ultraviolet curable ink or electron beam curable ink, the number of heating processes can be reduced, the number of opportunities for applying a thermal load to the can body 110 can be reduced, and the cooling time can be reduced. As an example, inkjet printing can be performed using ultraviolet curable ink or electron beam curable ink.

[0100] In addition to / instead of printing ink on the can body 110, the print layer forming step may be performed by covering the outer surface of the can body 110 with a shrink film on which an ink image is printed. For example, an ink image may be printed on a shrink film in the same manner as above, and the shrink film may be wrapped around the can body 110 and shrunk to form the shrink film on which the image is printed as the ink print layer 120. A tack label may be used instead of the shrink film and attached to the outer surface of the can body 110. The tack label may be made of plastic or paper.

[0101] The use of pre-printed shrink labels or tack labels has the advantage that the problem of the printing being repelled by the lubricant on the surface of the can body 110 does not occur. Furthermore, by containing 0.01 mg / can or more of lubricant in the entire can body 110 or in the reduced diameter portion 20, the extrapolation properties of the shrink film can be improved.

[0102] The shrink film may be made of any known material, for example, polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polyolefin, polyethylene terephthalate, or the like.

[0103] The ink-printed layer 120 may be formed on the entire or partial area of ​​the outer peripheral surface of the can body 110. For example, the ink-printed layer 120 may be formed on the entire or only a portion of the can body 40. For example, the ink-printed layer 120 may be formed on the entire or only a portion of the reduced diameter portion 20 and the entire or only a portion of the can body 40.

[0104] The formation of the ink printing layer 120 may be performed in parallel. For example, the process of S500 may be performed simultaneously by a plurality of inkjet printing devices and / or a plurality of plate-based printing devices. Details will be described later.

[0105] The ink-printed layer 120 may be formed in multiple batches. For example, a common design, common pattern, and / or common characters may be formed in advance by printing with a printing plate or inkjet printing, and then individual designs, individual patterns, and / or individual characters that differ for each product or lot may be formed on demand later by inkjet printing. When the ink-printed layer 120 is not formed, such as when manufacturing plain or white cans to be later printed, the process of S500 may be omitted.

[0106] After S500 and before S600, a protective layer may be further formed on the outer surface of the ink-printed layer 120. For example, the ink-printed layer 120 can be protected by forming a layer containing a UV-curable resin or the like as a protective layer on the outer surface of the ink-printed layer 120.

[0107] In S600, the can container 10 on which each layer has been formed is inspected. The outer or inner surface of the can container 10 may be inspected for dents, holes, and / or scratches. The printed image of the ink-printed layer 120 may be inspected for chips, misalignments, and / or unclear areas.

[0108] In S700, the contents are filled into the can container 10. For example, the can container 10 may be filled with beverages, food, medicines, chemical products, gases, liquids and / or solids, etc.

[0109] In S800, a can lid is attached to the can container 10. For example, the can lid may be attached by placing the lid on the flange portion of the can container 10 and tightening it with a lid tightening machine.

[0110] 4 to 6 show the basic process flow for manufacturing the can container 10, but as described later, the order of the processes may be changed or parallelized. This can improve the efficiency of the can manufacturing process. Also, if the can container 10 is a cup, the processes of S700 to S800 may be omitted.

[0111] S100 to S800 may be performed by a single entity / location, or by multiple different entities / locations. For example, S100 to S600 may be performed at a can factory, and S700 and onward may be performed at a filling factory (also called a packer or bottler).

[0112] Also, for example, S100 to S400 may be performed in a can manufacturing factory, and S500 and subsequent steps may be performed in a filling factory. This allows a printing device to be installed in the filling factory, and can containers 10 with any image can be quickly manufactured and shipped in the number required for filling.

[0113] 7 shows another example of the flow of the manufacturing method of the can container 10 in this embodiment. In this embodiment, the removal step S200 is performed between the diameter reduction step S400 and the print layer formation step S500. In other words, S200 is performed after S400.

[0114] In this embodiment, the removal step S200 removes the lubricant applied in S110, S115, and S300 and / or a portion of the formed lubricant layer. This allows the amount of lubricant remaining on the can container 10 to be significantly reduced. In the removal step, the lubricant layer 117 may be completely removed, or a portion may be left behind. For example, the amount of lubricant present in the reduced diameter portion 20 (particularly the outer surface side of the can body 110 in the reduced diameter portion 20) may be 2 mg / can or less. This makes it possible to prevent printing from being repelled when the printing layer formation step S500 is performed.

[0115] Furthermore, the removal step may be carried out so that the amount of lubricant present in the reduced diameter portion 20 (particularly the outer surface side of the can body 110 in the reduced diameter portion 20) is 0.01 mg / can or more. This can improve the extrapolation property of the shrink film when the ink-printed layer 120 is formed from the shrink film.

[0116] Preferably, the removal step may include washing with water and / or heat treatment. Heat treatment can simultaneously remove the lubricating layer and remove distortion of the resin film. For example, the amount of lubricant can be reduced to 0.01 mg or more and 2 mg or less per can by heating the molded member at 180 to 220°C for 20 to 90 seconds as heat treatment.

[0117] 8 shows another example of the flow of the manufacturing method of the can container 10 in this embodiment. In this embodiment, the removal step S200 is performed between the molding step S100 and the lubrication step S300, and between the diameter reduction step S400 and the print layer formation step S500. That is, the lubrication step is performed twice.

[0118] In this embodiment, the first removal step (S200A) removes the lubricant applied in S110 and S115 and / or a part of the lubricant layer formed. The second removal step (S200B) removes the lubricant applied in S300 and / or a part of the lubricant layer formed. This can further significantly reduce the lubricant remaining on the can container 10. In the removal step, the lubricant layer 117 may be completely removed, or a part may be left. For example, the amount of lubricant present in the reduced diameter portion 20 (particularly the outer surface side of the can body 110 in the reduced diameter portion 20) may be 2 mg / can or less. This can prevent printing from being repellent when the printing layer formation step S500 is performed. If the amount of lubricant applied in S300 and / or the lubricant layer formed is sufficiently small, the second removal step S200 may not be performed.

[0119] This allows the amount of lubricant remaining on the can container 10 to be further significantly reduced. In the removal step, the lubricant layer 117 may be completely removed, or a portion may be left behind. For example, the amount of lubricant present in the reduced diameter portion 20 (particularly on the outer surface side of the can body 110 in the reduced diameter portion 20) may be 2 mg / can or less. This makes it possible to prevent printing from being repellent when the printing layer forming step S500 is performed. If the amount of lubricant applied and / or the lubricant layer formed in S300 is sufficiently small, the second removal step S200 does not need to be performed.

[0120] In S100, when the process of Figure 5 (wet molding) is performed, it is preferable to perform water washing in the first removal step (S200A) to thoroughly remove the lubricant, and it is desirable to perform frame treatment and / or plasma treatment in the second removal step (S200B), which is expected to have a surface modification effect on the can body 110.

[0121] In S100, when the process of Figure 6 (dry molding) is performed, it is preferable to carry out a heat treatment in the first removal step (S200A) that can also remove distortion from the resin film, and it is desirable to carry out a frame treatment and / or plasma treatment in the second removal step (S200B), which can also be expected to have a surface modification effect on the can body 110.

[0122] Other points may be the same as those of the embodiment described in Fig. 7. After the removal step of S200B, the printing layer forming step (S500) to the can lid attachment (S800) may be performed as in Fig. 7. Alternatively, the inspection step (S600) and / or the storage step (S900) may be performed as in Figs. 10 and 11 described below.

[0123] 9 shows another example of the flow of the method for manufacturing the can container 10 in this embodiment. In this embodiment, the lubrication step S300 is not performed, and the removal step S200 is performed after the diameter reduction step S400.

[0124] As a result, a diameter reduction step is performed in which a portion of the can body 110 is reduced in diameter to form reduced diameter portion 20, without applying a lubricant to the formed can body 110 in the lubrication step S300. In this embodiment, a lubricant layer is formed in advance in S110 or S115 on the sheet material before it is formed, or the forming step S100 is performed using a sheet material on which a lubricant layer has been formed in advance on a metal sheet or a resin film.

[0125] The removal step of S200 may be performed in the same manner as in the embodiment of Fig. 7. In the embodiment of Fig. 9, since the lubrication step of S300 does not exist, the removal step may be performed in a simplified manner compared to Fig. 7. For example, in this embodiment, the application time of the heat treatment may be 20 to 40 seconds, the irradiation time of the plasma treatment may be 0.5 to 5 seconds, and the heating time of the frame treatment may be 0.5 to 1 second.

[0126] According to this embodiment, the forming step and the diameter reduction step are performed using the lubricating layer of the sheet material applied for the forming step S100, so there is no need to perform the lubrication step. This makes it possible to reduce resources such as lubricant and time required for the lubrication step. This makes it possible to reduce the amount of lubricant present in the reduced diameter portion 20 (particularly the outer surface side of the can body 110 in the reduced diameter portion 20) to 2 mg / can or less. If the lubricating layer of the sheet material is sufficiently small, the removal step S200 does not need to be performed.

[0127] Fig. 10 shows another example of the flow of the method for manufacturing the can container 10 in this embodiment. In this embodiment, the molding step S100, the lubrication step S300, the diameter reduction step S400, and the removal step S200 may be performed similarly to the embodiment in Fig. 7. After S200, the inspection step S600 may be performed without performing the printing layer formation step.

[0128] In this embodiment, the removal step S200 is performed between the diameter reduction step S400 and the storage step S900. The processes of S100 to S600 may be performed in the same manner as described above.

[0129] The inspection step S600 may be followed by a storage step S900. In the storage step, the can body 110 is stored in a plain state with no printing applied. The storage step may be performed in a light-shielded state so that the can body is not exposed to ultraviolet rays. In particular, the storage step is preferably performed by storing the can body in a light-shielded state for one month or more. This protects the ink-printed layer 120 from ultraviolet rays and prevents deterioration such as fading. Storing the can body for one month or more can further reduce the amount of lubricant (especially volatile lubricant) present on the surface of the can body 110.

[0130] After the storage step of S900, the can body 110 may be shipped as necessary. For example, the can body 110 may be shipped to a filling factory, where one or more of the printing layer formation step of S500, the can container inspection step of S600, the filling step of S700, and the can lid attachment step of S800 may be performed.

[0131] In this embodiment, the amount of lubricant present on the surface of the can body 110 can be reduced by the removal process. For example, the amount of lubricant present in the reduced diameter portion 20 may be reduced to 2 mg / can or less. This makes it possible to prevent the printing from being repelled when the printing layer formation process of S500 is performed later at a filling factory.

[0132] Furthermore, in this embodiment, the removal step is expected to have the effect of cleaning the can body 110. Therefore, the lubricant can be prevented from deteriorating or absorbing moisture during the storage step of S900. In particular, when plasma treatment or flame treatment is used in the removal step, a high effect can be expected.

[0133] In addition, the amount of lubricant present in the reduced diameter portion 20 (particularly the outer surface side of the can body 110 in the reduced diameter portion 20) may be 0.01 mg / can or more. This can improve the extrapolation property of the shrink film when the ink-printed layer 120 is formed later using the shrink film at a filling factory.

[0134] On the other hand, the removal step of S200 may be omitted. For example, in cases where there is little concern about the printing being repellent, such as when the ink-printed layer 120 is formed later using a shrink film at a filling factory, it is desirable to omit the removal step.

[0135] Fig. 11 shows another example of the flow of the method for manufacturing the can container 10 in this embodiment. The embodiment in Fig. 11 differs from the embodiment in Fig. 10 in that it does not include the lubrication step S300 and the removal step S200. In this embodiment, a diameter reduction step is performed on a part of the can body 110 without applying a lubricant to the can body 110. In S100 of this embodiment, as described in the embodiment in Figs. 4 to 5, a lubricating layer is formed on the surface of the sheet material before the coupling press in S120 is performed.

[0136] According to this embodiment, the forming step S100 and the diameter reduction step S400 are performed using the lubricating layer of the sheet material applied for the forming step S100, so there is no need to perform the lubrication step. This makes it possible to reduce resources such as lubricant and time required for the lubrication step. This makes it possible to reduce the amount of lubricant present in the reduced diameter portion 20 (particularly the outer surface side of the can body 110 in the reduced diameter portion 20) to 2 mg or less. A removal step S200 may be added after the diameter reduction step S400.

[0137] According to this embodiment, the storage step S900 protects the ink-printed layer 120 from ultraviolet rays and prevents deterioration such as fading. By storing the can body for one month or more, the amount of lubricant (especially volatile lubricant) present on the surface of the can body 110 can be reduced without going through a removal step.

[0138] Although the present invention has been described above using the embodiments, the technical scope of the present invention is not limited to the scope described in the above embodiments. It is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. It is clear from the description of the claims that such modifications and improvements can also be included in the technical scope of the present invention.

[0139] It should be noted that the order of execution of each process, such as operations, procedures, steps, and stages, in the can body, can container, and method shown in the claims, specification, and drawings is not specifically indicated as "before," "prior to," etc., and can be realized in any order, as long as the can body or can container from the previous process is not used in the subsequent process. Even if the operational flow in the claims, specification, and drawings is described using "first," "next," etc. for convenience, it does not mean that it is essential to perform the process in this order. [Explanation of symbols]

[0140] 10 Can containers 20 Reduced diameter part 30 bottom 40 Can body 110 Can body 112 Can body 114 Resin film layer 116 Resin film layer 117 Lubricating layer 120 Ink printing layer

Claims

1. A reduced diameter portion; A can body portion, The amount of lubricant present in the reduced diameter portion is 2 mg / can or less. Tin container.

2. A cylindrical can body; An ink printed layer formed on the outer surface of the can body; The layer structure includes the amount of lubricant present on the outer surface side of the can body in the reduced diameter portion is 2 mg / can or less; The can container according to claim 1.

3. The ink printing layer is a layer formed directly on the can body and formed by curing the ink. The can container according to claim 2.

4. The ink printing layer further covers the can body from the outside and is a shrink film on which an ink image is printed. The can container according to claim 2.

5. A cylindrical can body, a resin film layer covering at least the outer surface of the can body; The layer structure includes the amount of lubricant present on the outer surface of the resin film layer in the reduced diameter portion is 2 mg / can or less; The can container according to claim 1.

6. An ink printed layer is formed on the outer surface of the resin film layer, 6. The can container according to claim 5, wherein the amount of lubricant present on the outer surface side of the resin film layer in the reduced diameter portion is 2 mg / can or less.

7. The ink printed layer is formed directly on the resin film layer and is a layer in which the ink is cured. The can container according to claim 6.

8. The ink printing layer further covers the resin film layer from the outside and is a shrink film on which an ink image is printed. The can container according to claim 6.

9. A can container according to any one of claims 1 to 8, which is filled with a beverage or food for consumption.

10. A forming step of forming a cylindrical can body from a sheet material having a metal sheet and a resin film layer covering at least one side of the metal sheet, or from a sheet material having a metal sheet; a lubricating step of applying a lubricant to the formed can body; a diameter reducing step of reducing a diameter of a part of the can body to form a reduced diameter portion; a printing layer forming step of forming an ink printing layer on the outer peripheral surface of the can body; A method for manufacturing a can container comprising the steps of:

11. The forming step is a step of forming a can body from a sheet material having the metal sheet, the resin film layer, and a lubricating layer formed on one side of the resin film layer. The method for manufacturing the can container according to claim 10.

12. The forming step is a step of forming a can body from the metal sheet and a sheet material having a lubricating layer formed on one or both sides of the metal sheet. The method for manufacturing the can container according to claim 10.

13. The method further includes a removing step of removing at least a portion of the lubricating layer between the molding step and the lubricating step. The method for producing the can container according to claim 11.

14. A forming process of forming a cylindrical can body from a sheet material having a metal sheet, a resin film covering at least one side of the metal sheet, and a lubricating layer formed on one side of the resin film, or a sheet material consisting of a metal sheet and a lubricating layer formed on one or both sides of the metal sheet; a diameter reducing step of reducing a diameter of a part of the formed can body to form a reduced diameter portion without applying a lubricant to the formed can body; a printing layer forming step of forming an ink printing layer on the outer peripheral surface of the can body; A method for manufacturing a can container comprising the steps of:

15. The method further includes a removing step of removing at least a part of the lubricant or the lubricant layer applied in the lubricating step between the diameter reducing step and the printing layer forming step. A method for producing a can container according to any one of claims 10 to 14.

16. A lubricating step of applying a lubricant to a can body including a cylindrical can body and a resin film layer covering at least an outer surface of the can body, or to a can body including a cylindrical can body; a diameter reducing step of reducing a diameter of a part of the can body to form a reduced diameter portion; a storage step of storing the can body in a plain state without any printing; A method for manufacturing a can container comprising the steps of:

17. A forming process of forming a cylindrical can body from a sheet material having a metal sheet, a resin film covering at least one side of the metal sheet, and a lubricating layer formed on one side of the resin film; a diameter reducing step of reducing a diameter of a part of the can body to form a reduced diameter portion without applying a lubricant to the can body; a storage step of storing the can body in a plain state without any printing; A method for manufacturing a can container comprising the steps of:

18. Between the diameter reducing step and the storage step, a removing step of removing a portion of the lubricant from the can body; The method of claim 16 further comprising:

19. The storage step is carried out in a light-shielding state so that the can body is not irradiated with ultraviolet light. A method for producing a can container according to claim 16 or 17.

20. The storage step includes storing the can body in a light-shielded state for one month or more. A method for producing the can container according to claim 19.

21. The printing layer forming step includes performing printing on the outer surface of the can body by one or more of inkjet printing or printing with a printing plate. A method for producing a can container according to claim 10 or 14.

22. The printing layer forming step includes covering the outer surface of the can body with a shrink film on which an ink image is printed. A method for producing a can container according to claim 10 or 14.

23. The removing step uses thermal energy, plasma treatment, or flame treatment. The method for producing the can container according to claim 13.

24. The removing step uses thermal energy, plasma treatment, or flame treatment. A method for producing a can container according to claim 15.