Laminate and packaging bag

The laminate with a peeling part and printed layer addresses the inefficiencies of multiple degassing steps and cumbersome openings in existing packaging, providing a clean and efficient packaging solution for articles in clean environments.

JP2024159250APending Publication Date: 2024-11-08DAI NIPPON PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023075113
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing packaging methods for articles in clean environments, such as semiconductor products, involve multiple degassing steps and are cumbersome to open, and there is a need for a packaging material with a printed layer for identification.

Method used

A laminate comprising a peeling part and a main body with a printed layer, where the peeling part is peelable and contains a resin material, and the main body includes a heat-fusible resin layer with polyolefin, allowing the packaging bag to be brought into a clean environment without multiple openings.

Benefits of technology

The laminate enables efficient packaging with a printed layer for identification, reducing the need for multiple degassing steps and minimizing foreign matter entry into clean environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159250000001_ABST
    Figure 2024159250000001_ABST
Patent Text Reader

Abstract

To provide a laminate which is suitable as a packaging material capable of packaging an article used in a clean environment, and has a printed layer.SOLUTION: A laminate includes at least a peeling part and a body part, wherein the peeling part is provided so as to be peelable from the body part, the peeling part includes a resin layer containing a resin material as a main component, and a printed layer provided on the resin layer, and the body part includes at least a heat-fusible resin layer containing polyolefin as a main component as one surface layer of the laminate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate and a packaging bag. [Background technology]

[0002] Semiconductor products are manufactured or used in clean environments such as clean rooms with high levels of cleanliness, because the quality of the products can be reduced if foreign matter such as dust and dirt adheres to the products. When an article is brought into such an environment, a package in which the article is contained in a bag made of plastic film is often brought into the clean environment. Therefore, high cleanliness is also required for packaging bags that contain articles that require a high level of cleanliness, such as semiconductor products.

[0003] Conventionally, a package is manufactured as follows using a double bag having at least an inner bag and an outer bag (see, for example, Patent Document 1). First, an item is placed inside the inner bag, which is vacuum degassed, and the opening of the inner bag is sealed. Next, the inner bag is placed inside the outer bag, which is vacuum degassed, and the opening of the outer bag is sealed. The item is packaged in this double packaging, or triple packaging as necessary. When the item is to be used, the outer bag is opened in the antechamber of the clean room, the clean inner bag is opened inside the clean room, and the item is removed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-126437 A Summary of the Invention [Problem to be solved by the invention]

[0005] When packaging an article using double or triple vacuum packaging, the vacuum packaging is performed multiple times. This may result in low work efficiency in packaging the article. In addition, when opening the packaging bag, it may be troublesome to open the bag multiple times. In addition, such packaging bags are preferably provided with a printing layer, for example, to display the article in the packaging bag.

[0006] An object of the present disclosure is to provide a laminate having a printed layer, which is suitable as a packaging material capable of packaging items used in a clean environment. [Means for solving the problem]

[0007] The present inventors have investigated the production of a packaging bag using a laminate having a peel-off portion and a main body portion, and the provision of a printing layer on the peel-off portion. By peeling off the peel-off portion of the packaging bag in the antechamber of the clean room, the packaging bag in a clean state can be brought into the clean room. Based on this knowledge, the present inventors have found that the above problem can be solved by a laminate having the following configuration.

[0008] A laminate according to one embodiment of the present disclosure comprises at least a peel-off portion and a main body portion, the peel-off portion being configured so as to be peelable from the main body portion, the peel-off portion comprising a resin layer containing a resin material as a main component and a printed layer provided on the resin layer, and the main body portion comprising at least a heat-sealable resin layer containing a polyolefin as a main component as one surface layer of the laminate. Effect of the Invention

[0009] According to the present disclosure, a laminate having a printed layer can be provided, which is suitable as a packaging material capable of packaging items used in a clean environment. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of one embodiment of a laminate of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of one embodiment of a laminate of the present disclosure. [Diagram 3] FIG. 3 is a schematic cross-sectional view of one embodiment of a laminate of the present disclosure. [Figure 4] FIG. 4 is a schematic cross-sectional view of one embodiment of a laminate of the present disclosure. [Diagram 5] FIG. 5 is a schematic cross-sectional view of one embodiment of a laminate of the present disclosure. [Figure 6] FIG. 6 is a schematic cross-sectional view of one embodiment of the packaging bag of the present disclosure. [Figure 7] FIG. 7 is a front view of one embodiment of the packaging bag of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present disclosure will be described in detail. The present disclosure can be implemented in many different forms, and is not to be interpreted as being limited to the description of the embodiments exemplified below. In the drawings, the width, thickness, shape, etc. of each layer may be shown diagrammatically in order to make the explanation clearer, but these are merely examples and do not limit the interpretation of the present disclosure. In this specification and each figure, elements similar to those already explained with respect to the previous figures are given the same reference numerals, and detailed explanations may be omitted as appropriate.

[0012] In the present disclosure, when multiple upper limit candidates and multiple lower limit candidates are listed for a certain parameter, the numerical range of the parameter may be configured by combining any one upper limit candidate and any one lower limit candidate. Examples of the above parameters include physical property values, component content ratios, and layer thicknesses. As an example, the description "Parameter B is preferably A1 or more, more preferably A2 or more, and even more preferably A3 or more. Parameter B is preferably A4 or less, more preferably A5 or less, and even more preferably A6 or less." will be explained. In this example, the numerical range of parameter B may be A1 or more and A4 or less, A1 or more and A5 or less, A1 or more and A6 or less, A2 or more and A4 or less, A2 or more and A5 or less, A2 or more and A6 or less, A3 or more and A4 or less, A3 or more and A5 or less, or A3 or more and A6 or less.

[0013] In the following description of this specification, each of the components (e.g., polyolefins such as polyethylene and polypropylene, α-olefins, resin materials such as heteroatom-containing resins, and additives) that appear may be used alone or in combination of two or more kinds.

[0014] In this specification, polyethylene refers to a polymer in which the content of ethylene-derived structural units in all repeating structural units exceeds 50 mol%. In this polymer, the content of ethylene-derived structural units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more. The content is measured by NMR.

[0015] In this specification, polyethylene may be a homopolymer of ethylene, or a copolymer of ethylene and an ethylenically unsaturated monomer other than ethylene. Examples of the ethylenically unsaturated monomer other than ethylene include α-olefins having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene, vinyl monomers such as vinyl acetate and vinyl propionate, and (meth)acrylic acid esters such as methyl (meth)acrylate and ethyl (meth)acrylate.

[0016] In this specification, polyethylene includes, for example, high density polyethylene, medium density polyethylene, low density polyethylene and linear low density polyethylene, as well as ethylene-vinyl acetate copolymer and ethylene-(meth)acrylic acid ester copolymer.

[0017] In this specification, the density of polyethylene is as follows: The density of the high density polyethylene is preferably 0.945 g / cm 3 The density of the high density polyethylene is preferably greater than 0.965 g / cm 3 The density of the medium density polyethylene is preferably 0.932 g / cm 3 Exceeds 0.945g / cm 3 The density of the low density polyethylene is preferably 0.860 g / cm 3 More than 0.932g / cm 3 Less than or equal to 0.900 g / cm 3 More than 0.932g / cm 3 The density of the linear low density polyethylene is preferably 0.860 g / cm 3 More than 0.932g / cm 3 Less than or equal to 0.900 g / cm 3 More than 0.932g / cm 3The density of polyethylene is measured in accordance with JIS K7112:1999, Method D (density gradient tube method, 23°C).

[0018] Low-density polyethylene is, for example, polyethylene obtained by polymerizing ethylene by high-pressure polymerization (high-pressure low-density polyethylene). Linear low-density polyethylene is, for example, polyethylene obtained by polymerizing ethylene and a small amount of α-olefins by a polymerization method using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst.

[0019] Polyethylenes with different densities or branches can be obtained by appropriately selecting a polymerization method. For example, it is preferable to carry out polymerization in one or more stages by using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst as a polymerization catalyst, by any of gas phase polymerization, slurry polymerization, solution polymerization, and high pressure ion polymerization.

[0020] In this specification, polyethylene may be polyethylene derived from biomass (hereinafter also referred to as "biomass polyethylene"). That is, as a raw material for obtaining polyethylene, ethylene derived from biomass may be used instead of ethylene obtained from fossil fuels. Since biomass polyethylene is a carbon-neutral material, it is possible to reduce the environmental load caused by the laminate or packaging bag. Biomass polyethylene can be produced, for example, by the method described in JP 2013-177531 A. Commercially available biomass polyethylene may be used.

[0021] The polyethylene may be mechanically recycled or chemically recycled. This can reduce the environmental impact of laminates or packaging bags. Mechanical recycling is generally a method in which recovered polyethylene films are crushed, washed with an alkali to remove dirt and foreign matter from the film surface, and then dried at high temperature and reduced pressure for a certain period of time to diffuse contaminants remaining inside the film, decontaminating it, removing the dirt from the film, and returning it to polyethylene. Chemical recycling is generally a method in which recovered polyethylene films are decomposed to the monomer level, and the monomers are polymerized again to obtain polyethylene.

[0022] As used herein, the term "major component" in a layer or film refers to a component whose content in the layer or film is greater than 50% by mass, preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more.

[0023] [Laminate] The laminate of the present disclosure includes at least a release portion and a main body portion. The main body has a first surface and a second surface opposite to the first surface. The peeling portion is provided on the first surface of the main body. The peeling portion is in contact with the main body, specifically, in contact with the first surface of the main body. Therefore, the first surface of the main body is usually a peeling surface when the peeling portion is peeled off.

[0024] <Peeling part> The peelable portion is provided so as to be peelable from the main body portion. In this specification, the film consisting of the release portion obtained by peeling the release portion from the main body of the laminate of the present disclosure is also referred to as a "release film." The film consisting of the main body after peeling is also referred to as a "packaging film."

[0025] The peeling portion includes a resin layer containing a resin material as a main component and a printed layer provided on the resin layer. In one embodiment, the peeling portion includes a printed film. The printed film includes a resin film containing a resin material as a main component and a printed layer provided on the resin film.

[0026] In one embodiment, the release portion includes a heteroatom-containing resin layer that is in contact with the main body portion and contains a heteroatom-containing resin as a main component. The release portion including the heteroatom-containing resin layer has excellent releasability from the main body portion, for example.

[0027] In one embodiment, the release portion includes a polyolefin layer containing polyolefin as a main component between the printed layer or printed film and the heteroatom-containing resin layer.

[0028] The peeling part may be, for example, a laminated film having a heteroatom-containing resin layer, an optional anchor coat layer, an optional adhesive layer, an optional anchor coat layer, and a printed film in this order, or a laminated film having a heteroatom-containing resin layer, a polyolefin layer, an optional adhesive layer, an optional anchor coat layer, and a printed film in this order. Here, the printed layer is preferably provided on the surface of the resin film facing the heteroatom-containing resin layer for the purpose of protecting the printed layer.

[0029] From the viewpoints of releasability, strength, and heat resistance, the thickness of the peelable portion is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, and particularly preferably 30 μm or more. From the viewpoint of processability, the thickness of the peelable portion is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, and particularly preferably 100 μm or less.

[0030] (Resin layer, printed layer, printed film) The peeling portion includes a resin layer containing a resin material as a main component and a printed layer provided on the resin layer. In one embodiment, the peeling portion includes a printed film. The printed film includes a resin film containing a resin material as a main component and a printed layer provided on the resin film.

[0031] The printing layer has an image. Examples of the image include characters, figures, patterns, symbols, and combinations thereof. The image may include text information such as the product name, the name of the item in the packaging bag, the manufacturer, and the names of ingredients. The image may be a single, solid color (so-called solid image).

[0032] The printed layer, in one embodiment, contains a colorant. Examples of colorants include pigments such as inorganic pigments and organic pigments, as well as dyes such as acid dyes, direct dyes, disperse dyes, oil-soluble dyes, metal-containing oil-soluble dyes, and sublimation dyes. Examples of colorants also include fluorescent materials such as ultraviolet emitting materials that emit fluorescence by absorbing ultraviolet light, and infrared emitting materials that emit fluorescence by absorbing infrared light.

[0033] The content of the colorant in the printed layer is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. The content of the colorant in the printed layer is preferably 90% by mass or less, more preferably 70% by mass or less, and even more preferably 50% by mass or less.

[0034] The print layer may contain a resin material, such as polyolefin, (meth)acrylic resin, vinyl resin, cellulose resin, polyamide, polyester, and ionomer resin. The printing layer may contain additives, such as antiblocking agents, slip agents, UV absorbers, antioxidants, light stabilizers, fillers, reinforcing agents, antistatic agents, compatibilizers, crosslinking agents, pigments, and dyes. The content of the resin material in the printed layer is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more. The content of the resin material in the printed layer is preferably 99% by mass or less, more preferably 97% by mass or less, and even more preferably 95% by mass or less.

[0035] The printing layer can be formed, for example, using an ink composition containing the above-mentioned components and, if necessary, a solvent. Examples of methods for forming the printing layer include gravure printing, offset printing, flexographic printing, screen printing, letterpress printing, and transfer printing. In one embodiment, from the viewpoint of reducing environmental load, flexographic printing may be used.

[0036] The thickness of the printed layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more. The thickness of the printed layer is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less.

[0037] Examples of the resin material in the resin layer or resin film include polyolefin, vinyl resin, polyester, polyamide, and polyurethane. Examples of the polyolefin include polyethylene such as high density polyethylene, medium density polyethylene, low density polyethylene, linear low density polyethylene, ethylene-vinyl acetate copolymer, and ethylene-(meth)acrylic acid ester copolymer, polypropylene, ethylene-propylene copolymer, polybutene, and polymethylpentene. Examples of the vinyl resin include polystyrene, polyacrylonitrile, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, and polytetrafluoroethylene. Examples of the polyester include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyamide include nylon 6, nylon 66, and MXD6 (polymetaxylylene adipamide).

[0038] The resin layer and the resin film may contain the above-mentioned additives.

[0039] In one embodiment, the resin film is a film that has been subjected to a stretching process, that is, a stretched film. Such a film is, for example, excellent in strength, heat resistance, and transparency. The stretching process may be uniaxial stretching or biaxial stretching. The stretching ratio when stretching in the machine direction (flow direction of the substrate, MD direction) is preferably 2 times or more, more preferably 3 times or more, and preferably 10 times or less, more preferably 7 times or less. The stretching ratio when stretching in the width direction (direction perpendicular to the MD direction, TD direction) is preferably 2 times or more, more preferably 3 times or more, and preferably 10 times or less, more preferably 7 times or less. By setting the stretching ratio to 2 times or more, for example, the strength, heat resistance, and transparency of the film can be improved, and the printability of the film can be improved. From the viewpoint of the breaking limit of the film, the stretching ratio is preferably 10 times or less.

[0040] Examples of resin films constituting the printing film include polyolefin films such as polyethylene film and polypropylene film, vinyl resin films, polyester films such as polyethylene terephthalate film, polyamide films such as nylon film, and polyurethane films. These resin films may be uniaxially stretched films or biaxially stretched films.

[0041] In one embodiment, the printed film may further include a transparent vapor deposition film. The printed film may include a resin film, a transparent vapor deposition film, and a printed layer in this order, or a transparent vapor deposition film, a resin film, and a printed layer in this order.

[0042] The transparent vapor deposition film may be, for example, a vapor deposition film containing one or more inorganic oxides. Examples of the inorganic oxide include aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, barium oxide, and silicon carbide oxide (carbon-containing silicon oxide). Among these, aluminum oxide (alumina) vapor deposition film, silicon oxide (silica) vapor deposition film, or silicon carbide oxide vapor deposition film is preferred.

[0043] The thickness of the transparent vapor-deposited film is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more, and is preferably 150 nm or less, more preferably 100 nm or less, and even more preferably 80 nm or less. A laminate having a transparent vapor-deposited film whose thickness is equal to or greater than the lower limit has, for example, excellent gas barrier properties. A laminate having a transparent vapor-deposited film whose thickness is equal to or less than the upper limit can, for example, suppress the occurrence of cracks in the transparent vapor-deposited film.

[0044] The transparent vapor-deposited film may be subjected to a surface treatment such as a corona treatment.

[0045] Examples of methods for forming a transparent vapor deposition film include physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition. The vapor deposition film may be a composite film containing two or more layers of different vapor deposition films formed by combining both physical vapor deposition and chemical vapor deposition. The vapor deposition film may be a single layer formed by one vapor deposition process, or a multilayer formed by multiple vapor deposition processes. When the vapor deposition film is multilayer, each layer may be composed of the same component or different components. Each layer may be formed by the same method or different methods.

[0046] In one embodiment, the resin film constituting the printing film is a polyolefin film containing polyolefin as a main component.The polyolefin may be, for example, polyethylene, polypropylene, or polymethylpentene, and is preferably polyethylene or polypropylene, and more preferably polyethylene.The polyolefin film is preferably a polyethylene film containing polyethylene as a main component, or a polypropylene film containing polypropylene as a main component, and more preferably a polyethylene film.

[0047] Examples of polyethylene include high density polyethylene, medium density polyethylene, low density polyethylene, and linear low density polyethylene. From the viewpoint of strength and heat resistance of the polyethylene film, high density polyethylene and / or medium density polyethylene are preferred.

[0048] The polyolefin content in the polyolefin film is preferably more than 50% by mass, more preferably 80% by mass or more, even more preferably 85% by mass or more, and particularly preferably 90% by mass or more. In one embodiment, the above "polyolefin content in the polyolefin film" can be read as, for example, "polyethylene content in the polyethylene film" or "polypropylene content in the polypropylene film".

[0049] The polyolefin film may contain a resin material other than polyolefin, such as (meth)acrylic resin, vinyl resin, cellulose resin, polyamide, polyester, and ionomer resin. The polyolefin film may contain the above-mentioned additives.

[0050] The resin film can be produced, for example, by forming a resin material or a resin composition thereof into a film by a T-die method, an inflation method, or the like, and then stretching the film as desired. According to the inflation method, film formation and stretching can be carried out simultaneously.

[0051] In one embodiment, the resin film may be subjected to a surface treatment such as a corona treatment. This can improve the adhesion between the resin film and other layers, for example. An easy-adhesion layer may be provided on the surface of the resin film.

[0052] The resin film may have a single-layer structure or a multi-layer structure. The thickness of the resin film is preferably 5 μm or more, more preferably 8 μm or more, and even more preferably 10 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less. A laminate having a resin film whose thickness is equal to or greater than the lower limit has, for example, excellent strength and heat resistance. A laminate having a resin film whose thickness is equal to or less than the upper limit has, for example, excellent processability.

[0053] (Heteroatom-containing resin layer) The heteroatom-containing resin layer contains a heteroatom-containing resin as a main component. The peelable portion including the heteroatom-containing resin layer has, for example, a high Young's modulus and is excellent in peelability from the main body portion. In addition, the laminate including the heteroatom-containing resin layer has, for example, excellent puncture resistance. Therefore, a packaging bag including such a laminate has excellent packaging properties for hard objects. The laminate including the heteroatom-containing resin layer also has, for example, excellent gas barrier properties such as oxygen barrier properties and water vapor barrier properties, heat resistance, and rigidity.

[0054] Examples of the heteroatom in the heteroatom-containing resin include oxygen, sulfur, nitrogen, and chlorine. The heteroatom-containing resin has a heteroatom-containing group such as a hydroxyl group, an amide bond, an ester bond, and an ether bond. Examples of the heteroatom-containing resin include polyamide, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, polyvinylidene chloride, polyester, polyether polyol, and polyester polyol. Among these, polyamide, ethylene-vinyl alcohol copolymer, polyester, and polyvinyl alcohol are preferred, and polyamide and ethylene-vinyl alcohol copolymer are more preferred, from the viewpoints of heat resistance, rigidity, and puncture resistance.

[0055] Examples of the polyamide include aliphatic polyamides and semi-aromatic polyamides. As the polyamide, aliphatic polyamides are preferred, and crystalline aliphatic polyamides are more preferred.

[0056] Examples of the aliphatic polyamide include aliphatic homopolyamide and aliphatic copolymer polyamide. In the following examples, polyamide is also referred to as "PA."

[0057] Specific examples of aliphatic homopolyamides include polycaprolactam (PA6), polyenantholactam (PA7), polyundecane lactam (PA11), polylauryl lactam (PA12), polyhexamethylene adipamide (PA66), polytetramethylene dodecamide (PA412), polypentamethylene azelamide (PA59), polypentamethylene sebacamide (PA510), polypentamethylene dodecamide (PA512), polyhexamethylene azelamide (PA69), polyhexamethylene sebacamide (PA610), polyhexamethylene dodecamide (PA612), poly Nonamethylene adipamide (PA96), polynonamethylene azelamide (PA99), polynonamethylene sebacamide (PA910), polynonamethylene dodecamide (PA912), polydecamethylene adipamide (PA106), polydecamethylene azelamide (PA109), polydecamethylene decamamide (PA1010), polydecamethylene dodecamide (PA1012), polydodecamethylene adipamide (PA126), polydodecamethylene azelamide (PA129), polydodecamethylene sebacamide (PA1210) and polydodecamethylene dodecamide (PA1212).

[0058] Specific examples of aliphatic copolymer polyamides include caprolactam / hexamethylenediaminoadipic acid copolymer (PA6 / 66), caprolactam / hexamethylenediaminoazelaic acid copolymer (PA6 / 69), caprolactam / hexamethylenediaminosebacic acid copolymer (PA6 / 610), caprolactam / hexamethylenediaminoundecanoic acid copolymer (PA6 / 611), caprolactam / hexamethylenediaminododecanoic acid copolymer (PA6 / 612), caprolactam / amino undecanoic acid copolymer (PA6 / 11), caprolactam / lauryllactam copolymer (PA6 / 12), caprolactam / hexamethylenediaminoadipic acid / lauryllactam copolymer (PA6 / 66 / 12), caprolactam / hexamethylenediaminoadipic acid / hexamethylenediaminosebacic acid copolymer (PA6 / 66 / 610), caprolactam / hexamethylenediaminoadipic acid / hexamethylenediaminododecanedicarboxylic acid copolymer (PA6 / 66 / 612).

[0059] The relative viscosity of the aliphatic polyamide is preferably 1.5 or more, more preferably 2.0 or more, and even more preferably 2.5 or more. The relative viscosity of the aliphatic polyamide is preferably 5.0 or less, more preferably 4.5 or less. The relative viscosity of the aliphatic polyamide is measured at 25°C by dissolving 1g of polyamide in 100mL of 96% concentrated sulfuric acid in accordance with JIS K6920-2:2009.

[0060] The semi-aromatic polyamide is a polyamide having a constitutional unit derived from an aromatic diamine and a constitutional unit derived from an aliphatic dicarboxylic acid, or a polyamide having a constitutional unit derived from an aliphatic diamine and a constitutional unit derived from an aromatic dicarboxylic acid, for example, a polyamide composed of an aromatic diamine and an aliphatic dicarboxylic acid, or a polyamide composed of an aliphatic diamine and an aromatic dicarboxylic acid.

[0061] Examples of semi-aromatic polyamides include polyhexamethylene terephthalamide (PA6T), polyhexamethylene isophthalamide (PA6I), polynonamethylene terephthalamide (PA9T), polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (PA66 / 6T), polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (PA66 / 6I), polyhexamethylene terephthalamide / polycaproamide copolymer (PA6T / 6), polyhexamethylene isophthalamide / polycaproamide copolymer (PA6I / 6), polyhexamethylene terephthalamide / poly dodecamide copolymer (PA6T / 12), polyhexamethylene isophthalamide / polyhexamethylene terephthalamide copolymer (PA6I / 6T), polyhexamethylene terephthalamide / poly(2-methylpentamethylene terephthalamide) copolymer (PA6T / M5T), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (PA66 / 6T / 6I), polyhexamethylene adipamide / polycaproamide / polyhexamethylene isophthalamide copolymer (PA66 / 6 / 6I) and polymetaxylylene adipamide (PAMXD6).

[0062] The melt volume rate (MVR) of the semi-aromatic polyamide is preferably 5 cm 3 / 10 minutes or more, preferably 10cm 3 The MVR of the semi-aromatic polyamide is preferably 200 cm 3 / 10 minutes or less, preferably 100cm 3 / 10 minutes or less. MVR is measured at a temperature of 275°C and a load of 5.00 kg in accordance with JIS K7210-1:2014.

[0063] The polyamide is preferably a crystalline aliphatic polyamide, such as PA6, PA11, PA12, PA66, PA610, PA612, PA6 / 66, and PA6 / 66 / 12.

[0064] The melting point (Tm) of the crystalline aliphatic polyamide is preferably 180° C. or higher. The Tm of the crystalline aliphatic polyamide is preferably 300° C. or lower, more preferably 250° C. or lower, and even more preferably 230° C. or lower. The Tm of the crystalline aliphatic polyamide is the melting peak temperature obtained by differential scanning calorimetry (DSC) in accordance with JIS K7121:2012.

[0065] From the viewpoint of film-forming property and processability, the polyamide melt flow rate (MFR) is preferably 0.1 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.5 g / 10 min or more. From the viewpoint of film-forming property and processability, the polyamide MFR is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, even more preferably 10 g / 10 min or less, and particularly preferably 5 g / 10 min or less. The polyamide MFR is measured by the A method at a temperature of 235°C and a load of 2.16 kg in accordance with JIS K7210-1:2014. The measurement temperature can be changed depending on the melting point of the polyamide.

[0066] The content of the heteroatom-containing resin in the heteroatom-containing resin layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and particularly preferably 90% by mass or more, which can improve the above-mentioned physical properties such as the heat resistance of the packaging bag.

[0067] The heteroatom-containing resin layer may contain the above-mentioned additives.

[0068] From the viewpoint of heat resistance of the laminate, the thickness of the heteroatom-containing resin layer is preferably 0.5 μm or more, more preferably 1 μm or more, even more preferably 3 μm or more, and particularly preferably 5 μm or more. The thickness of the heteroatom-containing resin layer is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The thickness of the heteroatom-containing resin layer is preferably smaller than the thickness of the polyolefin layer of the peeling portion and the thickness of the heat-fusible resin layer of the main body portion.

[0069] (Polyolefin layer) The polyolefin layer in the peeling portion contains polyolefin as a main component. Examples of polyolefin include polyethylene, polypropylene, and polymethylpentene, and polyethylene and polypropylene are preferred, and polyethylene is more preferred. The polyolefin layer is preferably a polyethylene layer containing polyethylene as a main component, and a polypropylene layer containing polypropylene as a main component, and more preferably a polyethylene layer.

[0070] Examples of polyethylene include high density polyethylene, medium density polyethylene, low density polyethylene, and linear low density polyethylene. From the viewpoint of the heat resistance of the laminate, high density polyethylene is preferred.

[0071] From the viewpoint of heat resistance, the melting point (Tm) of the polyethylene in the polyolefin layer is preferably 100° C. or higher, more preferably 105° C. or higher, even more preferably 110° C. or higher, particularly preferably 120° C. or higher, and preferably 140° C. or lower. Tm is the melting peak temperature obtained by DSC in accordance with JIS K7121:2012.

[0072] The MFR of the polyolefin in the polyolefin layer is preferably 0.1 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.5 g / 10 min or more, from the viewpoint of film-forming property and processability. The MFR of the polyolefin is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, even more preferably 10 g / 10 min or less, and particularly preferably 5 g / 10 min or less, from the viewpoint of film-forming property and processability. The MFR of the polyolefin is measured by the A method under a load of 2.16 kg in accordance with JIS K7210-1:2014. The measurement temperature of the MFR is set according to the melting point of the polyolefin, and is 190 ° C. for polyethylene and 230 ° C. for polypropylene.

[0073] The polyolefin content in the polyolefin layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more. In one embodiment, the above "polyolefin content in the polyolefin layer" can be read as, for example, "polyethylene content in the polyethylene layer" or "polypropylene content in the polypropylene layer".

[0074] The polyolefin layer in the peeling portion may further contain modified polyolefins such as modified polyethylene and modified polypropylene from the viewpoint of adhesion to the heteroatom-containing resin layer. The modified polyolefins include, for example, polyolefins modified with unsaturated carboxylic acids such as maleic acid and fumaric acid, or their acid anhydrides, esters, or metal salts, particularly graft modified polyolefins, and polyethylenes modified with such unsaturated carboxylic acids, particularly graft modified polyethylenes. The modified polyethylene may be modified high density polyethylene or maleic anhydride graft modified high density polyethylene.

[0075] From the viewpoint of film-forming property and processability, the MFR of the modified polyolefin is preferably 0.1 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.5 g / 10 min or more. From the viewpoint of film-forming property and processability, the MFR of the modified polyolefin is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, even more preferably 10 g / 10 min or less, and particularly preferably 5 g / 10 min or less. The MFR of the modified polyolefin is measured by the A method under a load of 2.16 kg in accordance with JIS K7210-1:2014. The measurement temperature of the MFR is set according to the melting point of the modified polyolefin, and is 190 ° C. for modified polyethylene and 230 ° C. for modified polypropylene.

[0076] The content of modified polyolefin in the polyolefin layer is preferably less than 50% by mass, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less. The content of modified polyolefin in the polyolefin layer is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. In one embodiment, the above "content of modified polyolefin in the polyolefin layer" can be read as, for example, "content of modified polyethylene in the polyethylene layer" or "content of modified polypropylene in the polypropylene layer".

[0077] The polyolefin layer may contain a resin material other than polyolefin and modified polyolefin, such as (meth)acrylic resin, vinyl resin, cellulose resin, polyamide, polyester, and ionomer resin. The polyolefin layer may contain the additives described above.

[0078] The thickness of the polyolefin layer is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more from the viewpoint of the strength and heat resistance of the laminate. The thickness of the polyolefin layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less from the viewpoint of the processability of the laminate.

[0079] (Adhesive layer) In one embodiment, the adhesive layer in the peeling portion is an extruded resin layer containing polyolefin as a main component. Examples of polyolefin include polyethylene, polypropylene, and polymethylpentene, and polyethylene and polypropylene are preferred, and polyethylene is more preferred. From the viewpoint of adhesiveness, the polyethylene constituting the extruded resin layer is preferably low-density polyethylene and linear low-density polyethylene, and more preferably low-density polyethylene.

[0080] From the viewpoint of film-forming property and processability, the MFR of the polyethylene in the extruded resin layer is preferably 0.1 g / 10 min or more, more preferably 1 g / 10 min or more, even more preferably 3 g / 10 min or more, and preferably 30 g / 10 min or less, more preferably 25 g / 10 min or less, even more preferably 20 g / 10 min or less. The MFR of the polyethylene is measured by the A method in accordance with JIS K7210-1:2014 under the conditions of a temperature of 190° C. and a load of 2.16 kg.

[0081] From the viewpoint of a balance between heat resistance and adhesiveness, the melting point (Tm) of the polyethylene in the extruded resin layer is preferably 100° C. or higher, and preferably 140° C. or lower, more preferably 130° C. or lower, and further preferably 120° C. or lower. Tm is the melting peak temperature obtained by DSC in accordance with JIS K7121:2012.

[0082] The content of polyethylene in the extruded resin layer is preferably 80% by mass or more, more preferably 85% by mass or more, still more preferably 90% by mass or more, and particularly preferably 95% by mass.

[0083] The thickness of the extruded resin layer is preferably 5 μm or more, more preferably 10 μm or more. The thickness of the extruded resin layer is preferably 40 μm or less, more preferably 30 μm or less. A laminate including such an extruded resin layer has excellent interlayer adhesion.

[0084] The extruded resin layer can be formed, for example, by melting polyethylene or a polyethylene resin composition and extruding it onto the film. The melting temperature at this time is preferably 280° C. or higher, more preferably 290° C. or higher, and preferably 340° C. or lower, more preferably 335° C. or lower.

[0085] In one embodiment, the extruded resin layer functions as an adhesive layer between the printed film and a substrate described later. A laminate including such an extruded resin layer has an appropriate peel strength between the peel-off portion and the main body portion, and has excellent peelability at the peel-off portion.

[0086] When an extruded resin layer is formed on a printed layer of a printed film, an anchor coat layer may be formed on the printed layer of the printed film, and then an extruded resin layer may be formed on the anchor coat layer. When an extruded resin layer is formed on a heteroatom-containing resin layer in a substrate described later, an anchor coat layer may be formed on the heteroatom-containing resin layer, and then an extruded resin layer may be formed on the anchor coat layer. This can improve interlayer adhesion. The anchor coat layer is formed by an anchor coat agent. Examples of the anchor coat agent include polyurethane-based, polyester-based, polyether-based, polyolefin-based, and epoxy resin-based anchor coat agents. The anchor coat layer may contain the above-mentioned additives. The thickness of the anchor coat layer is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more, and is preferably 3 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.

[0087] In one embodiment, the adhesive layer in the peeling portion is an adhesive layer made of an adhesive. In one embodiment, the adhesive layer functions as an adhesive layer between the print film and the substrate described below. The adhesive may be any one of a one-component curing adhesive, a two-component curing adhesive, and a non-curing adhesive. The adhesive may be a solventless adhesive or a solvent-based adhesive.

[0088] Examples of solvent-free adhesives, i.e., non-solvent laminate adhesives, include polyether adhesives, polyester adhesives, silicone adhesives, epoxy adhesives, and urethane adhesives. Examples of solvent-based adhesives include rubber adhesives, vinyl adhesives, olefin adhesives, silicone adhesives, epoxy adhesives, phenol adhesives, and urethane adhesives. Among these, urethane adhesives are preferred, and two-liquid curing urethane adhesives are more preferred.

[0089] The thickness of the adhesive layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.5 μm or more. The thickness of the adhesive layer is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less.

[0090] <Main body> The main body portion includes at least a heat-sealable resin layer containing polyolefin as a main component as one surface layer of the laminate. In one embodiment, the heat-sealable resin layer in the main body portion is in contact with the release portion.

[0091] In one embodiment, the body has a density of 0.909 g / cm 3 The polyethylene layer in the main body portion is in contact with the release portion in one embodiment.

[0092] In one embodiment, the body has a density of 0.909 g / cm 3 The laminate includes a polyethylene layer and a heat-sealable resin layer containing polyethylene as a main component as one surface layer of the laminate. In one embodiment, the polyethylene layer in the main body is in contact with the release portion. In one embodiment, the main body has a density of 0.909 g / cm 3 An intermediate layer containing polyethylene as a main component (hereinafter also referred to as "polyethylene intermediate layer") is further provided between the polyethylene layer described below and the heat-sealable resin layer containing polyethylene as a main component.

[0093] In one embodiment, the main body contains polyolefin as a main component. This allows the packaging bag obtained by separating and removing the peelable portion from the laminate to be made into a mono-material. When a packaging bag is produced using the laminate of the present disclosure, the main body is a layer that faces the storage space of the packaging bag.

[0094] Polyolefins include, for example, polyethylene, polypropylene and polymethylpentene, with polyethylene and polypropylene being preferred, and polyethylene being more preferred.

[0095] The MFR of the polyolefin in the main body is preferably 0.1 g / 10 min or more, more preferably 0.3 g / 10 min or more, and even more preferably 0.5 g / 10 min or more, from the viewpoint of film-forming property and processability. The MFR of the polyolefin is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, even more preferably 10 g / 10 min or less, and particularly preferably 5 g / 10 min or less, from the viewpoint of film-forming property and processability. The MFR of the polyolefin is measured by the A method under a load of 2.16 kg in accordance with JIS K7210-1:2014. The measurement temperature of the MFR is set according to the melting point of the polyolefin. The measurement temperature of the MFR is 190°C for polyethylene and 230°C for polypropylene.

[0096] The content of polyolefin in the main body is 80% by mass or more, preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the mass of the main body. A laminate having such a main body is excellent in recyclability. Specifically, the packaging film corresponding to the main body after peeling and removing the peeling portion from the laminate is excellent in recyclability.

[0097] In one embodiment, the above "polyolefin content in the main body portion" can be read as, for example, "polyethylene content in the main body portion" or "polypropylene content in the main body portion."

[0098] In one embodiment, the main body contains polyethylene as a main component. Examples of polyethylene include high density polyethylene, medium density polyethylene, low density polyethylene, and linear low density polyethylene. From the viewpoint of heat sealability, low density polyethylene and linear low density polyethylene are preferred.

[0099] From the viewpoint of a balance between heat resistance and heat sealability, the melting point (Tm) of the polyethylene in the main body is preferably 80° C. or higher, more preferably 85° C. or higher, and preferably 140° C. or lower, more preferably 130° C. or lower. Tm is the melting peak temperature obtained by DSC in accordance with JIS K7121:2012.

[0100] The main body may contain the above-mentioned resin materials other than polyolefin. The main body may contain the additive.

[0101] From the viewpoints of strength and heat sealability, the thickness of the main body is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, and particularly preferably 30 μm or more. From the viewpoint of processability, the thickness of the main body is preferably 250 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, and particularly preferably 100 μm or less.

[0102] (thermal adhesive resin layer) The main body includes a heat-sealable resin layer containing polyolefin as a main component as one surface layer of the laminate. Such a heat-sealable resin layer functions as a seal layer in a packaging bag including the laminate. When a packaging bag is produced using the laminate of the present disclosure, the heat-sealable resin layer is a layer facing the storage space of the packaging bag.

[0103] In one embodiment, the body portion is made of a heat-sealable resin layer. In one embodiment, 0.909 g / cm 3 The polyethylene layer having the following density is one surface layer of the main body, and the heat-fusible resin layer is the other surface layer of the main body.

[0104] Among polyolefins, polyethylene and polypropylene are preferred, and polyethylene is more preferred. Examples of polyethylene include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, and ethylene-(meth)acrylic acid ester copolymer, and linear low-density polyethylene and low-density polyethylene are preferred, and linear low-density polyethylene is more preferred.

[0105] The content of polyolefin in the heat-sealable resin layer is preferably more than 50% by mass, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 85% by mass or more, and particularly preferably 90% by mass or more. A laminate having such a heat-sealable resin layer has, for example, excellent recyclability. In one embodiment, the above-mentioned "content of polyolefin in the heat-sealable resin layer" can be read as, for example, "content of polyethylene in the heat-sealable resin layer" or "content of polypropylene in the heat-sealable resin layer".

[0106] From the viewpoint of heat sealability, the heat-fusible resin layer preferably contains, as a main component, at least one polyethylene selected from linear low-density polyethylene and low-density polyethylene, such as C4-LLDPE, C6-LLDPE, and C8-LLDPE.

[0107] The total content of the linear low-density polyethylene and the low-density polyethylene in the heat-sealable resin layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0108] In one embodiment, the heat-sealable resin layer contains linear low-density polyethylene and low-density polyethylene. Such a heat-sealable resin layer has excellent heat sealability. The content ratio of linear low-density polyethylene (LLDPE) to low-density polyethylene (LDPE) in the heat-sealable resin layer (LLDPE:LDPE) is preferably 5:95 to 95:5, more preferably 10:90 to 90:10, and even more preferably 20:80 to 80:20, based on mass.

[0109] From the viewpoint of heat sealability, the melting point (Tm) of the polyethylene in the heat-fusible resin layer is preferably 140° C. or lower, more preferably 130° C. or lower, even more preferably 125° C. or lower, and is preferably 90° C. or higher, more preferably 95° C. or higher, even more preferably 100° C. or higher. Tm is the melting peak temperature obtained by DSC in accordance with JIS K7121:2012.

[0110] The thermally adhesive resin layer may contain the above-mentioned resin material. The heat-fusible resin layer may contain the above-mentioned additives.

[0111] The thickness of the heat-fusible resin layer is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the heat-fusible resin layer is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 60 μm or less, and even more preferably 40 μm or less.

[0112] (Polyethylene layer) In one embodiment, the body has a density of 0.909 g / cm 3 The polyethylene layer has a density of 0.909 g / cm3 in the main body. 3 In one embodiment, the following polyethylene layer is in contact with the heteroatom-containing resin layer in the peeled portion. A laminate including such a polyethylene layer can suppress lifting of the peeled portion from the main body portion during the production of the laminate, and has good peel strength between the peeled portion and the main body portion. Specifically, the density is 0.909 g / cm 3The following polyethylene layer has an excellent balance of adhesion to the heteroatom-containing resin layer and peelability.

[0113] The density of the polyethylene layer is preferably 0.908 g / cm 3 Less than or equal to 0.907 g / cm 3 More preferably, 0.906 g / cm 3 More preferably, 0.905 g / cm 3 Below 0.904 g / cm, particularly preferably 0.904 g / cm 3 The density of the polyethylene layer is preferably 0.860 g / cm 3 More preferably, 0.870 g / cm 3 More preferably, 0.880 g / cm 3 More preferably, 0.890 g / cm 3 More preferably, 0.895 g / cm 3 The density of the polyethylene layer is measured in accordance with JIS K7112:1999, Method D (density gradient tube method, 23° C.).

[0114] In one embodiment, the polyethylene layer has a density of 0.909 g / cm 3 The polyethylene used is preferably polyethylene having a density of 0.909 g / cm 3 It contains the following linear low density polyethylene as a main component. Examples of linear low density polyethylene include C4-LLDPE, C6-LLDPE, and C8-LLDPE.

[0115] The density of the polyethylene, such as linear low density polyethylene, is preferably 0.908 g / cm 3 Less than or equal to 0.907 g / cm 3 More preferably, 0.906 g / cm 3 More preferably, 0.905 g / cm 3 Below 0.904 g / cm, particularly preferably 0.904 g / cm 3 The density of the polyethylene is preferably 0.860 g / cm 3 More preferably, 0.870 g / cm3 More preferably, 0.880 g / cm 3 More preferably, 0.890 g / cm 3 More preferably, 0.895 g / cm 3 That's all.

[0116] Density is 0.909g / cm 3 The polyethylene may be a metallocene-based linear low-density polyethylene. A metallocene-based linear low-density polyethylene is a metallocene-based ethylene-α-olefin copolymer, i.e., an ethylene-α-olefin copolymer produced using a metallocene catalyst, and has a generally linear molecular structure.

[0117] Examples of the α-olefins copolymerized with ethylene include α-olefins having 3 to 12 carbon atoms, specifically propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 4-methyl-1-pentene, 1-decene, and 1-dodecene. Among these, α-olefins having 3 to 8 carbon atoms are preferred. Examples of linear low density polyethylene include C4-LLDPE, C6-LLDPE, and C8-LLDPE.

[0118] The melting point (Tm) of the metallocene-based linear low-density polyethylene is preferably 110° C. or lower, more preferably 105° C. or lower, even more preferably 100° C. or lower, and particularly preferably 95° C. or lower. The melting point (Tm) of the metallocene-based linear low-density polyethylene is preferably 80° C. or higher, more preferably 85° C. or higher, and even more preferably 88° C. or higher. Tm is the melting peak temperature obtained by DSC in accordance with JIS K7121:2012.

[0119] Among the metallocene-based linear low density polyethylenes, resins called metallocene-based ethylene plastomers are preferred. Specifically, metallocene-based ethylene plastomers are a type of copolymer of ethylene and α-olefin (ethylene-α-olefin copolymer) obtained by a metallocene catalyst. Metallocene-based ethylene plastomers have a density in the range called ultra-low density, which is relatively low among low densities, a uniform polymer distribution indexed by a narrow molecular weight distribution (Mw / Mn) derived from a polymerization method using a metallocene catalyst, which is a catalyst having uniform catalytic activity sites, and plastomer properties.

[0120] As the metallocene-based ethylene plastomer, a commercially available product may be used. For example, the commercially available product may be selected from the "Kernel (registered trademark)" series manufactured by Japan Polyethylene. For example, "KF260T", "KF360T" and "KS340T" may be mentioned.

[0121] Density is 0.909g / cm 3 The ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the following polyethylene is preferably 3.5 or less, more preferably 3.3 or less, and even more preferably 3.0 or less. The ratio (Mw / Mn) is 1.0 or more, preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.1 or more.

[0122] Mw / Mn is defined as the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (GPC). Mw and Mn are measured by the following method. Apparatus: Waters GPC 150C type detector: MIRAN 1A infrared spectrophotometer (measurement wavelength, 3.42 μm) Column: Showa Denko AD806M / S x 3 [The column is calibrated by measuring Tosoh monodisperse polystyrene (A500, A2500, F1, F2, F4, F10, F20, F40, F288, each 0.5 mg / ml solution) and approximating the logarithm of the elution volume and molecular weight with a quadratic equation. The molecular weight of the sample is converted to polyethylene using the viscosity equation for polystyrene and polyethylene. The coefficients of the viscosity equation for polystyrene are α=0.723, logK=-3.967, and for polyethylene, α=0.707, logK=-3.407.] Measurement temperature: 140℃ Injection amount: 0.2ml Concentration: 20mg / 10mL Solvent: ortho-dichlorobenzene Flow rate: 1.0ml / min

[0123] The density of the polyethylene layer is 0.909 g / cm 3 The content of the following polyethylene is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0124] The polyethylene layer may contain the above-mentioned resin materials other than polyethylene. The polyethylene layer may contain the additives described above.

[0125] Density is 0.909g / cm 3 From the viewpoint of peel strength, the thickness of the following polyethylene layer is preferably 0.5 μm or more, more preferably 1 μm or more, further preferably 3 μm or more, and particularly preferably 5 μm or more. 3 From the viewpoint of processability in film formation, the thickness of the following polyethylene layer is preferably 50 μm or less, more preferably 40 μm or less, and further preferably 30 μm or less.

[0126] (polyethylene intermediate layer) The density of the main body is 0.909g / cm 3An intermediate layer containing polyethylene as a main component may be further provided between the polyethylene layer and the heat-sealable resin layer described below. From the viewpoint of the puncture resistance of the laminate, the polyethylene intermediate layer more preferably contains linear low-density polyethylene as a main component.

[0127] Examples of polyethylene include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, and high-density polyethylene. From the viewpoint of heat sealability, linear low-density polyethylene and low-density polyethylene are preferred, and linear low-density polyethylene is more preferred. Examples of linear low-density polyethylene include C4-LLDPE, C6-LLDPE, and C8-LLDPE.

[0128] The density of the polyethylene in the polyethylene intermediate layer is preferably 0.925 g / cm 3 More preferably, 0.928 g / cm 3 More preferably, 0.930 g / cm 3 The laminate having such a polyethylene intermediate layer has excellent puncture resistance. The density of the polyethylene in the polyethylene intermediate layer is preferably 0.932 g / cm 3 The following is the result.

[0129] From the viewpoint of heat resistance, the melting point (Tm) of the polyethylene in the polyethylene intermediate layer is preferably 100° C. or higher, more preferably 105° C. or higher, even more preferably 110° C. or higher, particularly preferably 120° C. or higher, and preferably 140° C. or lower. Tm is the melting peak temperature obtained by DSC in accordance with JIS K7121:2012.

[0130] From the viewpoint of the puncture resistance and recyclability of the laminate, the polyethylene content in the polyethylene intermediate layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0131] The polyethylene intermediate layer may contain the above-mentioned resin materials other than polyethylene. The polyethylene intermediate layer may contain the additives described above.

[0132] The thickness of the polyethylene intermediate layer is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, and particularly preferably 10 μm or more. The thickness of the polyethylene intermediate layer is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 25 μm or less.

[0133] <Peel strength> The peel strength between the peeling portion and the main body is preferably 1.0 N / 15 mm width or less, more preferably 0.9 N / 15 mm width or less, even more preferably 0.8 N / 15 mm width or less, even more preferably 0.7 N / 15 mm width or less, and particularly preferably 0.6 N / 15 mm width or less. In the case of a laminate having such a peel strength, the peeling portion can be easily peeled from the main body with a moderate force without damaging the main body. The above peel strength is, for example, 0.01 N / 15 mm width, 0.05 N / 15 mm width, or 0.1 N / 15 mm width or more, preferably 0.15 N / 15 mm width or more, more preferably 0.2 N / 15 mm width or more. In the case of a laminate having such a peel strength, the lifting of the peeling portion from the main body can be suppressed, the appearance of the laminate is excellent, and the peeling portion can be suppressed from being peeled off from the main body at an unintended time. In addition, even if heat-sealed, the increase in the peel strength at the sealed portion can be suppressed to a range that can be peeled off by hand.

[0134] The peel strength is measured under the conditions of a peel angle of 180 degrees and a test speed of 50 mm / min. Specifically, the laminate is cut to cut out a test piece having a width of 15 mm and a length of 100 mm. The peeled portion at one end of the length direction of the test piece is peeled and folded back, and the end of the partially peeled peeled portion (peeling film) is attached to one grip of a tensile tester, and the end of the main body (packaging film) after the partial peeling is attached to the other grip of the tensile tester. The initial chuck distance is 100 mm. Next, the grip to which the end of the peeled portion is attached is pulled at a speed of 50 mm / min in a direction of 180 degrees with respect to the surface of the test piece while maintaining the position of the test piece so that the angle is maintained, and the maximum strength (N) is measured. The maximum strength (N) measured for the 15 mm wide test piece is taken as the peel strength (N / 15 mm width).

[0135] <Configuration and manufacturing method of laminate> 1 to 5 show schematic cross-sectional views of a laminate according to one embodiment of the present disclosure. The laminate 1 in FIG. 1 includes a peel-off portion 2 and a main body portion 4 in this order in the thickness direction. The laminate 1 in Fig. 2 comprises a printed film 10, an adhesive layer 20, and a substrate 30, in this order. In the laminate 1 in Fig. 2, the substrate 30 comprises a thermally adhesive resin layer 32 and a heteroatom-containing resin layer 36. In the laminate 1 in Fig. 3, the substrate 30 comprises a thermally adhesive resin layer 32, a heteroatom-containing resin layer 36, and a polyolefin layer 38, in this order. In the laminate 1 in Fig. 4, the substrate 30 comprises a thermally adhesive resin layer 32 and a polyolefin layer 38 having a density of 0.909 g / cm. 3 The laminate 1 in FIG. 5 includes, in this order, a polyethylene layer 34, a heteroatom-containing resin layer 36, and a polyolefin layer 38. In the laminate 1 in FIG. 5, the substrate 30 includes a heat-sealable resin layer 32, a polyethylene intermediate layer 33, and a polyolefin layer 38 having a density of 0.909 g / cm. 3 The film comprises a polyethylene layer 34, a heteroatom-containing resin layer 36, and a polyolefin layer 38 in this order.

[0136] The total thickness of the laminate of the present disclosure is preferably 20 μm or more, more preferably 40 μm or more, even more preferably 60 μm or more, even more preferably 80 μm or more, and particularly preferably 100 μm or more, from the viewpoint of the strength and heat resistance of the laminate. The total thickness of the laminate of the present disclosure is preferably 350 μm or less, more preferably 300 μm or less, even more preferably 250 μm or less, even more preferably 200 μm or less, and particularly preferably 150 μm or less, from the viewpoint of the processability of the laminate.

[0137] The laminate of the present disclosure can be produced, for example, by bonding a printed film and a substrate via an adhesive layer. The details of the printed film and the adhesive layer are as described above. Specifically, the laminate can be produced by laminating the printed film and the substrate using a melt extrusion lamination method, particularly a sand lamination method, a dry lamination method using a solvent-based adhesive, or a non-solvent lamination method using a solvent-free adhesive.

[0138] In one embodiment, the substrate comprises a heat-sealable resin layer, a heteroatom-containing resin layer, and optionally a polyolefin layer in this order. 3 The following polyethylene layer, heteroatom-containing resin layer, and optionally a polyolefin layer may be provided in this order, and the heat-sealable resin layer, the polyethylene intermediate layer, and a polyolefin layer having a density of 0.909 g / cm 3 The following polyethylene layer, heteroatom-containing resin layer, and optionally a polyolefin layer may be provided in this order. The heat-sealable resin layer corresponds to a seal layer, and the heteroatom-containing resin layer or the polyolefin layer corresponds to a laminate layer. The heat-sealable resin layer, optionally a polyethylene intermediate layer, and optionally a polyolefin layer having a density of 0.909 g / cm 3 The following polyethylene layer constitutes the above-mentioned main body, and the heteroatom-containing resin layer and, if desired, the polyolefin layer constitute a part of the above-mentioned release portion. In one embodiment, the substrate may be subjected to a surface treatment such as a corona treatment.

[0139] From the viewpoint of heat sealability, the substrate is preferably an unstretched film. An unstretched film is a film that has not been stretched, for example, an extrusion-molded film that has not been stretched. The concept of the "unstretched film" includes not only a film that has not been stretched at all, but also a film that has been slightly stretched due to tension applied during film formation by an inflation method or the like.

[0140] It is difficult to print on unstretched films, and the heat of drying during printing can cause the film to shrink. In addition, the heat during printing can cause the layer corresponding to the peeling portion of the substrate to peel off from the layer corresponding to the main body of the substrate. In this regard, by bonding the printed film and the substrate via the adhesive layer as described above, a printed layer can be introduced into the laminate, and the peeling caused by the heat during printing can be suppressed.

[0141] The substrate can be produced by a conventional method. The substrate is preferably a coextruded multilayer film, and can be produced, for example, by a coextrusion film forming method, more preferably by a T-die method or an inflation method. The substrate can be formed, for example, by extruding the resin or resin composition forming each layer from an extruder in a molten state.

[0142] According to the above method, the first surface of the main body that contacts the peel-off portion is not directly exposed to the outside air during and after the production of the laminate. Therefore, it is possible to prevent foreign matter such as dust and dirt from adhering to the first surface of the main body from the time of production of the laminate until the peel-off portion is peeled off and removed. When the packaging bag is used, the first surface of the main body is exposed by peeling off the peel-off portion from the main body of the laminate. This first surface is a clean surface in which the adhesion of foreign matter is prevented.

[0143] In one embodiment, the polyolefin content in the laminate of the present disclosure is preferably 75% by mass or more or 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, based on the mass of the laminate. Such a laminate has excellent recyclability. The above "polyolefin content in the laminate" can be read as, for example, "polyethylene content in the laminate" or "polypropylene content in the laminate."

[0144] [Application] The laminate of the present disclosure can be suitably used as a packaging material for forming a packaging bag. The second surface of the main body of the laminate forms an inner surface (a surface that comes into contact with an article in the packaging bag) facing the storage space in the packaging bag.

[0145] A high level of cleanliness is required for an article used in a clean environment such as a clean room. A packaging bag containing the article is brought into the clean environment and opened. Therefore, a high level of cleanliness is also required for the packaging bag. That is, when the packaging bag containing the article is brought into the clean environment, it is necessary to prevent foreign matter such as dust and dirt from adhering to the surface of the packaging bag and the foreign matter from entering the clean environment together with the packaging bag. By using a packaging bag including the laminate of the present disclosure, the intrusion of such foreign matter can be prevented, for example, as follows.

[0146] First, an article is placed in the packaging bag of the present disclosure, and degassed by vacuum degassing or the like as necessary, and the opening of the packaging bag is sealed to obtain a package in which the article is placed in the packaging bag. Degassing is not limited to vacuum degassing as long as the gas in the packaging bag can be removed. For example, degassing may be performed by pressing the packaging bag from the outside using a pressing member. The packaging body is brought into an anterior chamber of a clean environment. Here, the peelable portion (peeling film) of the laminate constituting the packaging bag is peeled and removed. This exposes the first surface of the main body portion (packaging film) of the laminate constituting the packaging bag. As described above, the first surface of the main body portion is a clean surface in which adhesion of foreign matter is suppressed. The packaging bag obtained by peeling and removing the peelable portion has a small amount of foreign matter attached to its surface. Such a packaging bag is brought into a clean environment. In the clean environment, the packaging bag is opened to take out the article and use it. In this way, intrusion of foreign matter into the clean environment together with the packaging bag is suppressed.

[0147] According to the above configuration, the packaging bag of the present disclosure does not need to be configured as a double-ply bag having at least an inner bag and an outer bag, or a triple-ply or more bag. However, there is no restriction on using the packaging bag of the present disclosure as an outer bag in a double-ply bag or a triple-ply or more bag.

[0148] Examples of the goods to be stored in the packaging bag include semiconductor products such as ICs and LSIs, semiconductor-related parts such as valves for semiconductor devices and filters for semiconductor manufacturing, precision machinery, magnetic disks, silicon wafers, O-rings, bellows, pharmaceutical products, products for regenerative medicine, and medicinal liquid products such as diluents for blood cell testing devices and artificial dialysis fluids. Examples of the goods to be stored in the packaging bag include dustproof clothing, dustproof gloves, and tools used in clean environments.

[0149] The packaging bag of the present disclosure comprises the laminate of the present disclosure. In one embodiment, the packaging bag of the present disclosure includes a top sheet constituting the front surface and a back sheet constituting the back surface. The top sheet may be composed of one laminate of the present disclosure, and the back sheet may be composed of another laminate of the present disclosure. The top sheet and the back sheet may be integrated, or may be composed of one laminate of the present disclosure.

[0150] A packaging bag usually has a heat-sealed portion (heat-sealed portion, hereinafter also referred to as "sealed portion"). Examples of heat-sealing methods include bar sealing, rotary roll sealing, belt sealing, impulse sealing, high-frequency sealing, and ultrasonic sealing.

[0151] Examples of packaging bags include packaging bags of various shapes such as a standing pouch type, a side seal type, a two-sided seal type, a three-sided seal type, a four-sided seal type, an envelope seal type, a grooving seal type (pillow seal type), a pleated seal type, a flat bottom seal type, a square bottom seal type, and a gusset type. The planar shape of the packaging bag may be, for example, rectangular or a shape other than rectangular, such as a circle.

[0152] An example of how to make a packaging bag using the laminate of the present disclosure will be described. Two laminates are prepared. The two laminates are stacked with their main bodies facing each other. Next, heat seal parts are formed on the three sides of the outer peripheral edge of the laminate, that is, the left and right sides and the bottom. In this way, a packaging bag having an opening on one side is obtained.

[0153] Instead of using two sheets of the laminate of the present disclosure, one sheet of the laminate of the present disclosure may be prepared, folded and stacked so that the second surfaces of the main body of the laminate face each other, and then heat-sealed portions are formed on both the left and right outer peripheral edges to produce a packaging bag. In this way, a packaging bag having an opening on one side is obtained. In this case, a heat-sealed portion may also be formed on the folded lower portion, and further, a lower portion of the lower heat-sealed portion may be cut and removed. This allows the peeling portions to be peeled off on both the front sheet and back sheet of the packaging bag.

[0154] An article is inserted through the opening of the unheat-sealed portion of the packaging bag produced above. The opening of the packaging bag is then heat-sealed to form a heat-sealed portion, thereby obtaining a package in which the article is housed in the packaging bag.

[0155] Fig. 6a is a cross-sectional view showing one embodiment of the packaging bag of the present disclosure. The sealed portion of the packaging bag 50 is formed by overlapping and heat-sealing a laminate 1 having a peel-off portion 2 and a main body portion 4. Fig. 6b is a cross-sectional view showing one embodiment of a usage form of the packaging bag of the present disclosure. For example, the peel-off portions 2, 2 are peeled off from the main body portions 4, 4 of the packaging bag 50, respectively, immediately before being brought into a clean room.

[0156] The packaging bag may have an easy-open portion. Examples of the easy-open portion include a notch portion that serves as a starting point for tearing the packaging bag, and an easy-open line formed by laser processing or a cutter as a path for tearing the packaging bag.

[0157] FIG. 7 is a front view showing one embodiment of the packaging bag of the present disclosure. Hereinafter, an example of the packaging bag will be described with reference to FIG. 7. The packaging bag 50 of FIG. 7 has a storage section 50a for storing an item. The packaging bag 50 includes an upper section 51, a lower section 52, and side sections 53, 53, and has a substantially rectangular outline in a front view. Note that names such as "upper section," "lower section," and "side section," as well as terms such as "upper" and "lower" merely relatively indicate the positions and directions of the packaging bag 50 and its components. The posture, etc. of the packaging bag 50 during transportation or use are not limited by the names and terms in this specification.

[0158] As shown in Fig. 7, the packaging bag 50 includes a top sheet 54 constituting the top surface and a back sheet 55 constituting the back surface. In the packaging bag 50 shown in Fig. 7, the top sheet 54 and the back sheet 55 are each formed of a single laminate. Although not shown, in the packaging bag 50, the top sheet 54 and the back sheet 55 may be integrated or may be formed of a single laminate. In this case, the laminate is folded back at the lower part 52 so that the main body portion constitutes the inner surface of the packaging bag 50. In this case, the packaging bag 50 has seal portions extending along three sides of the packaging bag 50.

[0159] The inner surfaces of the top sheet 54 and the back sheet 55 are joined together by a sealed portion. In the front view of the packaging bag 50 shown in Fig. 7, the sealed portion is hatched. The sealed portion is a portion where the heat-fusible resin layers of the laminate are joined together.

[0160] 7, the packaging bag 50 has heat-sealed portions extending along the four sides of the packaging bag 50. The sealed portions include an upper sealed portion 51a extending along the upper portion 51, a pair of side sealed portions 53a, 53a extending along a pair of side portions 53, 53, and a lower sealed portion 52a extending along the lower portion 52. In the packaging bag 50 before an article is contained therein (a state in which no article is contained therein), an opening (not shown) is formed in the upper portion 51 of the packaging bag 50. After an article is contained in the packaging bag 50, the inner surface of the top sheet 54 and the inner surface of the back sheet 55 are joined at the upper portion 51 to form the upper sealed portion 51a and seal the packaging bag 50.

[0161] The upper seal portion 51a, the side seal portions 53a, 53a and the lower seal portion 52a are seal portions formed by joining the inner surface of the top sheet 54 and the inner surface of the back sheet 55 together.

[0162] There is no particular limitation on the method for forming the sealed portion as long as it is possible to join opposing sheets 54, 55 together to seal packaging bag 50. For example, the sealed portion is formed by melting the inner surfaces of the sheets by heating or the like and fusing the inner surfaces together, that is, by heat sealing.

[0163] In one embodiment, the laminate constituting the packaging bag has a half-cut line. The half-cut line is a cut line that extends from the surface of the peel-off portion constituting the laminate to the interface between the peel-off portion and the main body portion, but does not penetrate the laminate. Starting from the half-cut line, the peel-off portion of the laminate can be easily peeled off and removed by hand.

[0164] The position where the half-cut line is formed is not particularly limited. For example, in the case of a packaging bag having a rectangular planar shape, it is preferable to provide the half-cut line at at least one corner of the packaging bag. It is preferable that the half-cut line is formed on both the top sheet and the back sheet of the packaging bag. In one embodiment, the half-cut line extends from the side outer edge to the lower outer edge of the top sheet and the back sheet at the corners of the sheets.

[0165] The half-cut line can be formed, for example, by mechanically cutting the laminate in the thickness direction using a cutter or by irradiating the laminate with a laser. As shown in Fig. 7, a half-cut line 60 is formed at one corner of the sealed portion of the packaging bag 50.

[0166] The present disclosure relates to, for example, the following [1] to

[14] . [1] A laminate comprising at least a peel-off portion and a main body portion, the peel-off portion being provided so as to be peelable from the main body portion, the peel-off portion comprising a resin layer containing a resin material as a main component and a printed layer provided on the resin layer, and the main body portion comprising at least a heat-fusible resin layer containing a polyolefin as a main component as one surface layer of the laminate. [2] The laminate described in [1] above, wherein the peel-off portion comprises a printed film having a resin film as the resin layer and the printed layer provided on the resin film, and the resin film is at least one selected from a polyolefin film, a vinyl resin film, a polyester film, a polyamide film and a polyurethane film. [3] The laminate described in [2], wherein the printed film further comprises a transparent vapor deposition film. [4] The laminate according to any one of [1] to [3] above, wherein the peeling portion comprises a heteroatom-containing resin layer that contacts the main body portion and contains a heteroatom-containing resin as a main component. [5] The laminate according to [4] above, wherein the heteroatom-containing resin comprises at least one selected from the group consisting of polyamide, ethylene-vinyl alcohol copolymer, polyester, and polyvinyl alcohol. [6] The laminate according to [4] or [5], wherein the peel-off portion further comprises a polyolefin layer containing polyolefin as a main component between the printing layer and the heteroatom-containing resin layer. [7] The laminate according to [6], wherein the polyolefin layer further contains a modified polyolefin in addition to the polyolefin. [8] The laminate described in any one of [1] to [7], wherein the peel-off portion comprises a printed film, an extruded resin layer containing polyolefin as a main component, and a heteroatom-containing resin layer containing a heteroatom-containing resin as a main component, the printed film comprises a resin film as the resin layer, and the printed layer provided on the resin film, and the heteroatom-containing resin layer is in contact with the main body portion. [9] The body has a density of 0.909 g / cm 3 The laminate according to any one of the above [1] to [8], comprising: a polyethylene layer; and a heat-sealable resin layer containing polyethylene as a main component as one surface layer of the laminate, wherein the polyethylene layer in the main body portion is in contact with the heteroatom-containing resin layer in the peel-off portion.

[10] The laminate comprises at least a printed film, an adhesive layer, and a substrate, the printed film comprises a resin film as the resin layer, and the printed layer provided on the resin film, the substrate comprises a heteroatom-containing resin layer containing a heteroatom-containing resin as a main component, and a 0.909 g / cm 3 The laminate according to any one of the above [1] to [9], comprising at least a polyethylene layer and a heat-sealable resin layer containing polyethylene as a main component, in this order:

[11] The laminate according to

[10] , wherein the substrate is a coextruded multilayer film.

[12] The laminate according to any one of [1] to

[11] , wherein the peel strength between the peel portion and the main body portion, measured under conditions of a peel angle of 180 degrees and a test speed of 50 mm / min, is 1.0 N / 15 mm width or less.

[13] A packaging bag comprising the laminate according to any one of [1] to

[12] above.

[14] The packaging bag according to

[13] , having a seal portion formed by fusing the heat-sealable resin layers in the laminate together. EXAMPLES

[0167] The laminate of the present disclosure will be described more specifically based on examples, but the laminate of the present disclosure is not limited to the examples in any way.

[0168] [material] The materials used in the following examples and comparative examples are shown below. Polyamide (PA) UBE, 5033B, polyamide 6 / 66 copolymer, Melting point: 197°C, density: 1.14g / cm 3 , MFR: 4.0g / 10min (Temperature 235℃, Load 2.16kg) · Linear low density polyethylene (LLDPE) Made by Nippon Polyethylene, KF260T, C6-LLDPE, Melting point: 93℃, density: 0.901g / cm 3 , MFR: 2.0g / 10min · Linear low density polyethylene (LLDPE) Prime Polymer, UZ2021L, C6-LLDPE, Melting point: 120℃, density: 0.919g / cm 3 , MFR: 2.0g / 10min · Linear low density polyethylene (LLDPE) Prime Polymer, UZ3520L, C6-LLDPE, Melting point: 124℃, density: 0.931g / cm 3 , MFR:2.1g / 10min ·Low Density Polyethylene (LDPE) Ube Maruzen polyethylene, B128, Melting point: 114℃, density: 0.928g / cm 3 , MFR: 1.0g / 10min ·Medium Density Polyethylene (MDPE) Dow Chemical, Elite5538G, Melting point: 129℃, density: 0.941g / cm 3 , MFR:1.3g / 10min High density polyethylene (HDPE) Prime Polymer, HZ3300F, Melting point: 130℃, density: 0.949g / cm 3 , MFR:1.1g / 10min Maleic anhydride grafted high density polyethylene Dow Chemical, BYNEL 40E 1053, adhesive resin, Melting point: 130℃, density: 0.960g / cm 3 , MFR: 2.0g / 10min

[0169] [Uniaxially oriented polyethylene film (1)] MDPE (Elite5538G) was formed by inflation molding to obtain a polyethylene film with a thickness of 125 μm. This polyethylene film was stretched in the machine direction (MD) at a stretch ratio of 5 times, and one side was subjected to corona treatment to adjust the wettability index to 52 dyn, to obtain a uniaxially stretched polyethylene film (1) (MDOPE film (1)) with a thickness of 25 μm.

[0170] [Base material (A)] A mixture of 80% by mass of HDPE (HZ3300F) and 20% by mass of adhesive resin (BYNEL 40E 1053), polyamide (5033B), LLDPE (KF260T), LLDPE (UZ3520L), and a mixture of 80% by mass of LLDPE (UZ2021L) and 20% by mass of LDPE (B128) were co-extruded by the inflation method. In this way, a film having a total thickness of 75 μm was obtained, which includes a 15 μm thick HDPE layer (laminate layer), a 5 μm thick polyamide layer, a 20 μm thick LLDPE layer, a 15 μm thick LLDPE layer, and a 20 μm thick polyethylene blend layer (seal layer). The laminate layer was subjected to a corona treatment to adjust the wetting index to 42 dyn. This film was used as the substrate (A). The mass % of a mixture indicates the content of each component in the mixture.

[0171] [Example 1] A 12 μm thick polyethylene terephthalate film (Toyobo, E5102, PET film) and a substrate (A) were prepared. A 1 μm thick printed layer was formed by gravure printing on the corona-treated surface of the PET film using gravure ink (DIC Graphics, Finart). The printed layer was coated with a 0.3 μm thick two-component curing polyurethane adhesive (Mitsui Chemicals, A-3210 / A-3075) as an anchor coating agent to form an anchor coat layer (AC layer), and then a low-density polyethylene (Japan Polyethylene, LC600A, melting point: 106° C., density: 0.918 g / cm 3 ) was applied to the surface of the AC layer. 3 (MFR: 7.0 g / 10 min) was melt extruded to a thickness of 20 μm and sandwich-laminated with the laminate layer of the substrate (A) to obtain a laminate. The seal layers of this laminate were placed together and sandwiched in a high-speed three-sided seal automatic bag making machine (BH-60D, manufactured by Totani Giken Kogyo) at a temperature of 130° C., a compression time of 1 second, and a pressure of 1 kgf / cm. 2 The mixture was heat sealed under the above conditions to create a three-sided pouch.

[0172] [Examples 2 to 5] A laminate and a three-sided pouch were prepared in the same manner as in Example 1, except that a 15 μm-thick biaxially oriented nylon film (Unitika, PTM-RT, ON film), a 20 μm-thick biaxially oriented polypropylene film (Toyobo, P2171, OPP film), a 12 μm-thick transparent vapor-deposited polyethylene terephthalate (Dai Nippon Printing, IB-PET PUB, transparent vapor-deposited PET film), or a uniaxially oriented polyethylene film (1) was used instead of the PET film.

[0173] [Comparative Example 1] Only the substrate (A) was prepared. No other film was attached to the laminate layer of the substrate (A), and the seal layers of the substrate (A) were joined together and heat sealed to prepare a three-sided pouch.

[0174] [Physical property evaluation] The methods for evaluating the physical properties of the laminate are described below. Unless otherwise specified, the environment during measurement of each physical property was a temperature of 23° C. and a humidity of 50% RH. Measurements were performed on three test pieces for each physical property, and the arithmetic mean value of the three values ​​obtained was recorded as the value of each physical property.

[0175] <Peel strength> The laminate was cut to obtain a test piece having a width of 15 mm and a length of 100 mm. Using the above test piece and a tabletop tensile compression tester MCT-1150 (manufactured by AND Co., Ltd.) as a measuring instrument, the peel strength (N / 15 mm width) between the peeled portion and the main body of the laminate was measured in accordance with JIS Z1707:2019 under the conditions of an initial chuck distance of 100 mm, a peel angle of 180 degrees, and a test speed of 50 mm / min. A test piece having a width of 15 mm and a length of 100 mm was cut out from the heat-sealed portion of the three-sided pouch. Using this test piece, the peel strength (N / 15 mm width) between the peeled portion and the main body of the laminate was measured in the same manner as above.

[0176] <Puncture strength> The puncture strength of the laminate was measured in accordance with JIS Z1707:2019. The laminate was cut to obtain a test piece having a width of 5 cm and a length of 5 cm. A tabletop tensile compression tester MCT-1150 (manufactured by AND Co., Ltd.) was used as a measuring instrument. A semicircular needle having a diameter of 1.0 mm and a tip shape radius of 0.5 mm was pierced into the test piece at a test speed of 50 mm / min, and the maximum strength (N) until the needle penetrated the test piece was measured. The above needle was pierced into the seal layer surface (from the inner layer) and the print film surface (from the outer layer) of the laminate, and the puncture strength (N) of each was measured.

[0177] <Seal strength> The laminate was cut to obtain a test piece having a width of 15 mm and a length of 100 mm. Two test pieces were overlapped so that the seal layers were in contact with each other, and the temperature was 130°C (one-sided heating), the compression time was 1 second, and the pressure was 1 kgf / cm. 2 A 15 mm x 15 mm portion of one end of the test piece was heat-sealed under the conditions above to form a sealed portion, and a test specimen was obtained. Except for the test conditions being changed as follows, the seal strength (N / 15 mm width) was measured in accordance with JIS Z1707:2019 using a tabletop tensile compression tester MCT-1150 (manufactured by AND Co., Ltd.) as a measuring instrument under the conditions of chuck distance: 100 mm, test speed: 300 mm / min. Specifically, the test specimen was opened 180 degrees so that the sealed portion of the test specimen was in the center of the two grips of the test machine, and both ends of the test specimen were attached to the two grips of the test machine, respectively, and pulled at a speed of 300 mm / min until the sealed portion broke, to obtain the maximum strength (N). The maximum strength (N) measured for the 15 mm wide test specimen was taken as the heat seal strength (N / 15 mm width).

[0178] [Table 1] [Explanation of symbols]

[0179] 1 ...Laminate 2 … Peeling part 4. Main body 10...Printed film 20...Adhesive layer (extruded resin layer or adhesive layer) 30...Base material 32…Thermofusible resin layer 33…Polyethylene intermediate layer 34…Density is 0.909g / cm 3 Polyethylene layer below 36...Heteroatom-containing resin layer 38...Polyolefin layer 40...Goods 50...Packaging bag 50a…Storage section 51…Upper 51a…Upper seal part 52…Lower 52a…Lower seal part 53…Side 53a...Side seal part 54…Surface sheet 55…Back sheet 60...Half cut wire

Claims

1. A laminate including at least a peeling portion and a main body portion, The peeling portion is provided so as to be peelable from the main body portion, the peeling portion includes a resin layer containing a resin material as a main component, and a printing layer provided on the resin layer, The main body portion includes at least a heat-sealable resin layer containing polyolefin as a main component as one surface layer of the laminate. Laminate.

2. 2. The laminate according to claim 1, wherein the peel-off portion comprises a printed film having a resin film as the resin layer and the printed layer provided on the resin film, and the resin film is at least one selected from a polyolefin film, a vinyl resin film, a polyester film, a polyamide film, and a polyurethane film.

3. The laminate of claim 2 , wherein the printed film further comprises a transparent vapor deposition film.

4. The laminate according to claim 1 , wherein the release portion comprises a heteroatom-containing resin layer that contacts the main body portion and contains a heteroatom-containing resin as a main component.

5. The laminate according to claim 4, wherein the heteroatom-containing resin comprises at least one selected from polyamide, ethylene-vinyl alcohol copolymer, polyester, and polyvinyl alcohol.

6. The laminate according to claim 4 , wherein the release portion further comprises a polyolefin layer containing polyolefin as a main component between the printed layer and the heteroatom-containing resin layer.

7. The laminate of claim 6, wherein the polyolefin layer further comprises a modified polyolefin in addition to the polyolefin.

8. The peeling portion is Printing film, An extruded resin layer containing polyolefin as a main component; a heteroatom-containing resin layer containing a heteroatom-containing resin as a main component; Equipped with The printed film includes a resin film as the resin layer and the printed layer provided on the resin film, The heteroatom-containing resin layer is in contact with the main body portion. The laminate according to claim 1 .

9. The body has a density of 0.909 g / cm 3 2. The laminate according to claim 1, comprising: a polyethylene layer; and a heat-sealable resin layer containing polyethylene as a main component as one surface layer of the laminate; and the polyethylene layer in the main body portion is in contact with the heteroatom-containing resin layer in the peel-off portion.

10. The laminate comprises: Printing film, An adhesive layer; A substrate; At least The printed film includes a resin film as the resin layer and the printed layer provided on the resin film, The substrate is a heteroatom-containing resin layer containing a heteroatom-containing resin as a main component; Density is 0.909 g / cm 3 A polyethylene layer comprising: A heat-sealable resin layer containing polyethylene as a main component; In this order, The laminate according to claim 1 .

11. The laminate of claim 10, wherein the substrate is a coextruded multilayer film.

12. 2. The laminate according to claim 1, wherein a peel strength between the peel portion and the main body portion measured under conditions of a peel angle of 180 degrees and a test speed of 50 mm / min is 1.0 N / 15 mm width or less.

13. A packaging bag comprising the laminate according to any one of claims 1 to 12.

14. The packaging bag according to claim 13 , further comprising a seal portion formed by fusing the heat-fusible resin layers in the laminate together.

Citation Information

Patent Citations

  • Double bag

    JP2012126437A