Optical communication cable
By aligning the thermal expansion coefficients of POFs and fixing resins in optical communication cables, the cable prevents cracks, maintaining connectivity and durability under harsh conditions.
Patent Information
- Application Number
- JP2023075119
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Optical communication cables experience cracks in plastic optical fibers due to thermal expansion of adhesives under high temperature and humidity conditions, compromising the connectivity of optical-electrical hybrid modules.
The optical communication cable design ensures that the linear expansion coefficient of the plastic optical fiber (POF) and the resin fixing it satisfy a specific relationship, minimizing stress and preventing cracks by matching their thermal expansion rates, and using resins like epoxy for enhanced adhesion and durability.
The cable effectively suppresses cracks in POFs under high temperature and humidity, ensuring reliable connectivity and durability by managing thermal expansion through resin selection and placement.
Smart Images

Figure 2024159254000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an optical communication cable, and more particularly to an optical communication cable that has excellent high-temperature and high-humidity resistance and that suppresses the occurrence of cracks in a plastic optical fiber.
[0002] In recent years, optical communication cables capable of transmitting large amounts of information to electronic devices, etc., have been widely used. Such optical communication cables usually connect an optical cord having a plastic optical fiber (hereinafter sometimes referred to as "POF") or the like to an optical-electrical hybrid board present in a housing (case) of an optical-electrical combined transmission module, and in order to maintain the connection, the end of the optical cord is fixed to the housing (case) or the like with an adhesive (for example, Patent Document 1).
[0003] However, as a result of the progress made in making optical-electrical combined transmission modules lighter and thinner, it was found that when environmental testing (high temperature and high humidity) was conducted on optical communication cables using such optical-electrical combined transmission modules, there was a risk of cracks occurring in the POF placed near the housing (case). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-231896 A Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, an object of the present disclosure is to provide an optical communication cable that is excellent in high-temperature and high-humidity resistance and in which the occurrence of cracks in the POF in the optical cord is suppressed even under high temperature and / or high humidity conditions. [Means for solving the problem]
[0006] In light of these circumstances, the inventors conducted extensive research and discovered that cracks in the POF of the optical cord are caused by thermal expansion of the adhesive that secures the end of the optical cord to the housing (in other words, the case) when exposed to high temperatures and / or high humidity, and that this expanded adhesive places stress on the POF of the optical cord. They then discovered that excessive stress on the optical cord can be suppressed by examining the physical properties of the adhesive and the POF of the optical cord, and thus completed the present disclosure.
[0007] That is, the present disclosure has the following aspects. [1] An optical communication cable, an optical cord having a POF and a coating layer provided around the POF; a connector to be connected to the POF of the optical cord; A first housing arranged on a first surface side of the connector; A second housing arranged on a second surface side of the connector; a resin for fixing the optical cord inside a case formed by combining the first housing and the second housing; an end R of the optical cord that is connected to a connector has a first end region r1 in which no coating layer is formed and the POF is exposed, and a second end region r2 in which a coating layer is formed and the POF is not exposed; a tip end E of the POF in the first end region r1 is connected to the connector, The resin is disposed so as to be in contact with the end R of the optical cord and the second housing, The linear expansion coefficient (t2) of the POF and the linear expansion coefficient (t1) of the resin are set to satisfy the following formula (1): Optical communication cable. t1≦t2+5 (1) [2] [1] An optical communication cable according to the present invention, The linear expansion coefficient (t2) of the POF is 50 ppm / °C or more and 80 ppm / °C or less. Optical communication cable. [3] An optical communication cable according to [1] or [2], The resin is disposed so as to be in contact with the first housing. Optical communication cable. [4] An optical communication cable according to any one of [1] to [3], The resin is a resin having an epoxy group. Optical communication cable. [5] An optical communication cable according to any one of [1] to [4], The length of the end R of the optical cord is 4 mm or more and 8 mm or less. Optical communication cable. [6] An optical communication cable according to any one of [1] to [5], The length of the first end region r1 at the end R of the optical cord is 1 mm or more and 4 mm or less. Optical communication cable. [7] An optical communication cable according to any one of [1] to [6], The resin is disposed so as to be in contact with the first surface of the connector, A base for fixing the position of the connector is provided between the second housing and the connector. Optical communication cable. Effect of the Invention
[0008] In the present disclosure, the linear expansion coefficient (t2) of the POF of the optical cord and the linear expansion coefficient (t1) of the resin arranged to be in contact with the second housing are set to satisfy the above formula (1), thereby reducing the effects of resin expansion under high temperature and / or high humidity conditions and suppressing the occurrence of cracks in the POF. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing the appearance of a main part of an optical communication cable according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is an exploded perspective view showing a configuration of a main part of an optical communication cable according to an embodiment of the present disclosure. [Diagram 3] FIG. 3 is a partial cross-sectional view illustrating the internal structure of a main part of an optical communication cable according to an embodiment of the present disclosure. [Figure 4] FIG. 4 is a cross-sectional view taken along line II for explaining the internal structure of an optical cord used in the optical communication cable shown in FIG. [Diagram 5] FIG. 5 is a partial cross-sectional view illustrating the internal structure of a main part of an optical communication cable according to an embodiment of the present disclosure. [Figure 6] FIG. 6 is a partial cross-sectional view illustrating the internal structure of a main part of an optical communication cable according to an embodiment of the present disclosure. [Figure 7] FIG. 7 is a partial cross-sectional view illustrating the internal structure of a main part of an optical communication cable according to an embodiment of the present disclosure. [Figure 8] FIG. 8 is a partial cross-sectional view illustrating the internal structure of a main part of an optical communication cable according to an embodiment of the present disclosure. [Figure 9] Fig. 9A is a perspective view illustrating the internal configuration of the analytical model, Fig. 9B is a plan view of the internal configuration of the analytical model as viewed from above, and Fig. 9C is a perspective view illustrating the internal structure of an optical cord used in the analytical model. [Figure 10] FIG. 10A-1 is a perspective view showing the resin arrangement of the analysis model. FIG. 10A-2 is a view showing the analysis model of FIG. 10A-1 as viewed from the connector side. FIG. 10A-3 is a schematic cross-sectional view explaining the structure of the analysis model of FIG. 10A-1. FIG. 10B-1 is a perspective view showing the resin arrangement of the analysis model. FIG. 10B-2 is a view showing the analysis model of FIG. 10B-1 as viewed from the connector side. FIG. 10B-3 is a schematic cross-sectional view explaining the structure of the analysis model of FIG. 10B-1. [Figure 11]FIG. 11A-1 is a perspective view showing the resin arrangement of the analysis model. FIG. 11A-2 is a view showing the analysis model of FIG. 11A-1 as viewed from the connector side. FIG. 11A-3 is a schematic cross-sectional view explaining the structure of the analysis model of FIG. 11A-1. FIG. 11B-1 is a perspective view showing the resin arrangement of the analysis model. FIG. 11B-2 is a view showing the analysis model of FIG. 11B-1 as viewed from the connector side. FIG. 11B-3 is a schematic cross-sectional view explaining the structure of the analysis model of FIG. 11B-1. [Figure 12] Fig. 12A is a diagram showing deformation and stress distribution of the POF in Experimental Example 1. Fig. 12B is a diagram showing deformation and stress distribution of the POF in Experimental Example 5. Fig. 12C is a diagram showing deformation and stress distribution of the POF in Experimental Example 6. [Figure 13] FIG. 13 is a perspective view illustrating the internal configuration of the analysis model of Experimental Example 8 with some parts omitted. [Figure 14] FIG. 13 is a graph showing the results of calculating the longitudinal stress of the POFs of the experimental examples and the reference example. [Figure 15] 11 is a graph showing the results of a simulation of the stress at the bottom of a POF based on the relationship between the distance from a connector and the linear expansion coefficient. FIG. [Figure 16] 11 is a graph showing the results of a simulation of the stress at the bottom of a POF based on the relationship between the distance from a connector and the linear expansion coefficient. FIG. [Figure 17] FIG. 1 is a graph showing the stress at the bottom at a distance of 4.3 mm from the connector for each linear expansion coefficient of the resin. [Figure 18] Fig. 18A is a diagram showing deformation and stress distribution in a POF viewed from the side when a resin with a linear expansion coefficient of 35 is used. Fig. 18B is a diagram showing deformation and stress distribution in a POF viewed from above when a resin with a linear expansion coefficient of 35 is used. [Figure 19] Fig. 19A is a diagram showing deformation and stress distribution in a POF viewed from the side when a resin with a linear expansion coefficient of 85 is used. Fig. 19B is a diagram showing deformation and stress distribution in a POF viewed from above when a resin with a linear expansion coefficient of 85 is used. [Figure 20]Fig. 20A is a diagram showing deformation and stress distribution in a POF viewed from the side when a resin with a linear expansion coefficient of 0 is used, and Fig. 20B is a diagram showing deformation and stress distribution in a POF viewed from the side when a resin with a linear expansion coefficient of 65 is used. [Figure 21] 11 is a graph showing the results of a simulation of the upper stress of a POF based on the relationship between the distance from a connector and the linear expansion coefficient. FIG. [Figure 22] FIG. 1 is a graph showing the upper stress at a distance of 4.3 mm from the connector for each linear expansion coefficient of resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the present disclosure will be described based on examples of embodiments of the present disclosure. However, the present disclosure is not limited to the embodiments described below.
[0011] In the present disclosure, when it is expressed as "J or more" (J is any number) or "K or less" (K is any number), it also means that "it is preferably greater than J" or "it is preferably less than K". In addition, in the present disclosure, "J and / or K (J and K are optional configurations)" means at least one of J and K, and means three possibilities: J only, K only, and J and K.
[0012] Fig. 1 is a perspective view showing the appearance of an optical communication cable 13 according to an embodiment of the present disclosure, and Fig. 2 is an exploded perspective view showing the configuration of the optical communication cable 13. The optical communication cable 13 disclosed herein converts the light output from the hybrid cable 2 into electricity and inputs this electricity to an electrical device not shown, and also converts the electricity output from the electrical device not shown into light and inputs this light into the hybrid cable 2. 1 and 2, reference numeral 11 denotes a plug. Examples of the plug include a Type-C plug and an HDMI (registered trademark) plug.
[0013] In other words, in the optical communication cable 13 of the present disclosure, the hybrid cable 2 is fixed within the case 19 by adhering the optical cord 5 and connector 6 of the hybrid cable 2 to the second housing 4 via resin 7 at the connection portion between the optical cord 5 and connector 6.
[0014] For this reason, as shown in FIG. 3, the optical communication cable 13 of the present disclosure comprises an optical cord 5 having a POF 9 and a coating layer 8 provided around the POF 9, a connector 6 connected to the POF 9 of the optical cord 5, a first housing 3 arranged on the first surface 6a side of the connector 6, a second housing 4 arranged on the second surface 6b side of the connector 6, and a resin 7 for fixing the optical cord 5 within a case 19 (see FIG. 1) formed by combining the first housing 3 and the second housing 4.
[0015] The end R of the optical cord 5, which is connected to the connector 6, has a first end region r1 where the coating layer 8 is not formed and the POF 9 is exposed, and a second end region r2 where the coating layer 8 is formed and the POF 9 is not exposed, and the tip E of the POF 9 in the first end region r1 is connected to the connector 6, and the resin 7 is arranged so as to contact the end R of the optical cord 5 and the second housing 4. The details of these configurations are described below.
[0016] <Optical code> As shown in FIG. 4, a cross section perpendicular to the longitudinal direction of the optical fiber cord 5 includes a POF 9, a tensile strength fiber 10 disposed around the POF 9, and a coating layer 8 disposed on the outside of the tensile strength fiber 10. POF9 is typically made of resin with different refractive indexes for the core and cladding. Examples of the core material include highly transparent methacrylic resin and quartz, and examples of the cladding material include fluorine-based resin and epoxy resin. Thus, in POF9, the core and cladding are usually made of different resins, but the core makes up the majority of the fiber. For this reason, in this disclosure, the physical properties of the core are adopted as the physical properties of POF9.
[0017] From the viewpoints of optical connection and strength, the diameter of the POF 9 is preferably 200 μm or more and 400 μm or less, more preferably 210 μm or more and 390 μm or less, and further preferably 220 μm or more and 380 μm or less.
[0018] From the viewpoint of light intensity, the linear expansion coefficient of POF9 is preferably 0 ppm / °C or more and 80 ppm / °C or less, more preferably 0 ppm / °C or more and 70 ppm / °C or less, and even more preferably 0 ppm / °C or more and 60 ppm / °C or less.
[0019] The tensile strength fiber 10 arranged around the POF 9 may be, for example, aramid fiber, tinsel thread, or the like, from the viewpoint of tensile resistance. The covering layer 8 disposed on the outside of the tensile fiber 10 may be made of, for example, ionomer resin, polyvinyl chloride (PVC), etc., in terms of hardness, heat resistance, and flame retardancy.
[0020] The length of the end R of the optical cord 5 is preferably 4 mm or more and 8 mm or less, and more preferably 4 mm or more and 6 mm or less, from the viewpoint of the strength of the optical communication cable. In addition, in terms of connectivity with the connector 6, the length of the first end region r1 of the end portion R is preferably 1 mm or more and 4 mm or less, and more preferably 2 mm or more and 4 mm or less.
[0021] The tip E of the POF 9 in the first end region r1 is connected to a connector 6 with the optical axis aligned.
[0022] <Connector> The connector 6 connected to the POF 9 is usually made of polyphenylene sulfide (PPS) and has a function of facilitating optical connection between the optoelectronic hybrid board and the fiber.
[0023] <First housing and second housing> The first housing 3 arranged on the first surface 6a side of the connector 6 can be used in combination with the paired second housing 4 (arranged on the second surface 6b side of the connector 6) to form an approximately box-shaped case 19 that houses the optical cord 5, connector 6, etc. (see Figure 1).
[0024] The first housing 3 and the second housing 4 (hereinafter sometimes referred to as "first housing 3, etc.") are preferably made of a material with as high a thermal conductivity as possible in consideration of the heat dissipation effect, and in particular, a thermal conductivity of 50 W / mK or more is preferable. It is more preferable to use a metal material, since it has high thermal conductivity and strength, and can achieve both heat dissipation effect and internal protection (photoelectric conversion section 5, etc.). Specific metal materials include, for example, aluminum, copper, silver, zinc, nickel, chromium, titanium, tantalum, platinum, gold, and alloys thereof (red brass, stainless steel, etc.). These may be used alone or in combination of two or more kinds. In addition, from the viewpoint of surface protection and aesthetics, the first housing 3, etc. may be subjected to a surface treatment such as plating.
[0025] Considering the balance between heat dissipation effect and weight reduction, the thickness of the first housing 3 etc. is preferably 0.1 mm or more and 0.6 mm or less, and more preferably 0.2 mm or more and 0.5 mm or less.
[0026] <Resin> Resin 7 for fixing optical cord 5 within case 19 formed by combining first housing 3 and second housing 4 is positioned so as to contact end R of the optical cord and second housing 4, as shown in FIG. 3.
[0027] In the present disclosure, the linear expansion coefficient (t1) of the resin 7 and the linear expansion coefficient (t2) of the POF 9 are designed to satisfy the formula (1). t1≦t2+5 (1)
[0028] In other words, by making (t1) and (t2) satisfy the above formula (1), the influence of the expansion of the resin under high temperature and / or high humidity can be reduced, and the occurrence of cracks in the POF 9 housed in the case 19 can be suppressed.
[0029] From the viewpoint of stress, the linear expansion coefficient (t1) of the resin 7 is preferably 35 ppm / ° C. or more and 70 ppm / ° C. or less, more preferably 40 ppm / ° C. or more and 68 ppm / ° C. or less, and even more preferably 45 ppm / ° C. or more and 65 ppm / ° C. or less. The linear expansion coefficient (t1) of the resin 7 may be the same as that of the POF 9.
[0030] The thermal conductivity (W / mK) of the resin 7 is preferably 0.1 W / mK or more and 3 W / mK or less, and more preferably 0.1 W / mK or more and 1 W / mK or less, in terms of a good balance between adhesion and heat resistance.
[0031] Considering these, for example, epoxy resin, acrylic resin, etc. are preferable as the resin 7, and in particular, epoxy resin is preferably used because it is excellent in combination with the POF 9.
[0032] The resin 7 is disposed in order to fix the optical cord 5 inside the case 19. In addition to the arrangement shown in FIG. 3, the resin 7 may be disposed, for example, as shown in FIG. 5 shows an example in which the resin 7 is arranged so as to be in contact with the first housing 3 as well. Arranging it in this manner tends to further suppress the expansion of the POF 9. However, in high heat and humidity conditions, the expansion of the resin 7 may damage the first housing 3 and the second housing 4 (case 19), so it is necessary to carefully consider the resin to be used.
[0033] Moreover, the resin 7 may be arranged as shown in FIG. 6 shows an example in which only the first end region r1 of the end R of the optical cord 5 is arranged to be in contact with the resin 7. With this arrangement, the optical cord 5 can be fixed with a small amount of resin, which tends to be lightweight.
[0034] The resin 7 may be arranged as shown in FIG. 7 shows an example in which the resin 7 is arranged so as to be in contact with the first surface 6a (the surface facing the first housing 3) of the connector 6. By arranging in this manner, the connector 6 can be reliably fixed in a positioned state, which tends to result in excellent durability. In this case, it is preferable to provide a seat 11 between the connector 6 and the second housing 4. By providing the seat 11, there is a tendency that the connector 6 can be easily fixed at a position where it is easy to connect to the POF 9.
[0035] The base 11 is preferably one that can fix the POF 9 at a distance from the second housing 4, and the material thereof is not particularly limited. However, it is preferable that the base 11 is made of the same material as the second housing 4, since this makes it easier to calculate the stress inside the case 19. In addition, the base 11 may be formed integrally with the second housing 4, or may be formed by adhesively fixing a separately prepared part to the second housing 4. It is preferable to form the base 11 by adhesively fixing a separately prepared part to the second housing 4, since the shape can be easily changed according to the design.
[0036] Furthermore, the resin 7 may be arranged as shown in FIG. 8 shows an example in which two types of resins having different properties are used as the resin 7. That is, resins having different properties are used for the resin 7' that covers the end R of the optical cord 5 and the resin 7 that is placed in other parts. When multiple resins with different properties are used as the resin 7 in this way, the connection strength of the optical cord 5 tends to be excellent. In this case, the linear expansion coefficient (t1) of the resin 7 is the linear expansion coefficient of the resin with the largest amount of resin among multiple resins with different properties, and is used as the linear expansion coefficient (t1) of the resin in the above formula (1). If the resin amounts are the same, the linear expansion coefficient of the resin with the highest linear expansion coefficient is used as the linear expansion coefficient (t1) of the resin in the above formula (1).
[0037] The optical communication cable 13 of the present disclosure can be manufactured, for example, as follows. First, a combined optical and electrical transmission module 1 made of stainless steel, polyimide, or the like is prepared, and if necessary, a base 11 is attached via an adhesive layer 12 to a predetermined position in the second housing 4 to house the combined optical and electrical transmission module 1. Then, a connector 6 provided on the combined optical and electrical transmission module 1 is connected to an optical cord 5 contained in a hybrid cable 2, and a resin 7 is arranged so as to contact an end R of the optical cord 5 and the second housing 4, thereby obtaining the product. In addition to the optical cord 5, the hybrid cable 2 usually has wiring such as copper wires for supplying power.
[0038] According to the optical communication cable 13 of the present disclosure, the occurrence of cracks in the POF 9 in the optical cord 5 is suppressed even under high temperature and / or high humidity conditions, and therefore the cable has excellent high temperature and high humidity resistance. EXAMPLES
[0039] In order to study the stress relationship between the optical cord 5 and the resin 7 that fixes the optical cord 5 in the optical communication cable, an analytical model shown in FIG. 9 was created. The analysis model includes an upper housing 20, a lower housing 21, a connector 6, an optical cord 5, and a base 11. The optical cord 5 includes a POF 9, a tensile strength fiber 10, and a coating layer 8. The optical cord 5 and the connector 6 are connected, and a resin 7 is used to fix the optical cord 5 to the lower housing 21. The base 11 is made of the same material as the lower housing 21, and is attached to the lower housing 21 by using an acrylic adhesive (through an adhesive layer 12). In addition, as shown in Figures 9A to 9C, the analytical model has Z constraint at the location indicated by arrow KZ, ZX constraint by coating layer 8 at the location indicated by arrow KZX, and Y constraint by the end of connector 6 and the end of resin 7 opposite connector 6 at the location indicated by arrow KY. 9C shows a cross section of the end of the optical cord 5 shown in FIG. 9A and FIG. 9B, and this cross section is also subjected to ZX constraints, but the Y direction is free in this cross section. The analytical model was made of the materials shown in Table 1 below. The physical properties of each material are shown in Table 1 below.
[0040] [Table 1] Here, POF is mainly made of Xylex resin. The coefficient of linear expansion (hereinafter sometimes referred to as "CTE") was measured using a PVT test system (manufactured by Toyo Seiki Seisakusho).
[0041] Using the above analytical model, PVT measurements were carried out based on the following test items and methods. [Pressure-specific volume-temperature (PVT) test] Pre-drying: Dry at 100°C for 10 hours or more, and start measurement within 15 minutes after removing. Test equipment: PVT test system (manufactured by Toyo Seiki Co., Ltd.) Measurement mode: Low pressure temperature change mode Sample size: 1-1.5g Temperature range: Start temperature 250℃~End temperature 50℃ (measurement interval: 5℃) Pressure: 50MPa, 40MPa, 30MPa, 20MPa
[0042] The analysis was performed using an advanced nonlinear simulation solution (Marc by HEXAGON). The stress value was calculated as follows, taking the stress applied to POF9 when the temperature was increased from 25°C to 80°C. In other words, the problem was solved using the finite element method, using three equations: the force balance equation, the equation relating to displacement and strain, and the equation relating to strain and stress (constitutive equation of the material).First, the displacement and strain were obtained from the force balance equation and the equation relating to displacement and strain, and then the stress was calculated from the equation relating to strain and stress (constitutive equation of the material).
[0043] [Experimental Example 1-4] First, in order to study the amount of deformation of the POF 9 due to differences in the arrangement of the resin 7, a silicone resin was used as the resin 7, and analytical models (Experimental Examples 1 to 4) were fabricated in which the arrangement was changed as follows. Experimental Example 1: Silicone resin placed at the position shown in resin 7 in FIG. 10A (lower part only) Experimental Example 2: Silicone resin was placed at the position shown as resin 7 in FIG. 10B (same amount above and below) Experimental Example 3: Silicone resin placed at the position shown in resin 7 in FIG. 11A (more toward the top) Experimental Example 4: Silicone resin placed at the position shown by resin 7 in FIG. 11B (filled)
[0044] As a result, it was found that the deformation amount of the POF 9 was almost the same in Experimental Examples 1 to 3. This is believed to be because a gap exists between the resin 7 and the upper housing 20 in each of the Experimental Examples, and the resin 7 expands toward the gap under high heat. On the other hand, in Experimental Example 4, since there was no gap between the resin 7 and the upper housing 20, the expansion of the resin 7 did not move in a specific direction, and it is understood that the expansion was suppressed.
[0045] From the above results, it was found that arranging resin 7 so that there are no gaps between resin 7 and upper housing 20 is useful in terms of preventing cracks in POF 9. However, if resin 7 is arranged so that there are no gaps between resin 7 and upper housing 20, there is a possibility that upper housing 20 will be damaged by the force of resin 7 expanding under high heat if resin 7 is arranged so that there are no gaps between resin 7 and upper housing 20. For this reason, further studies were conducted to see if there was a method for suppressing the deformation of the POF 9 other than arranging the resin 7 so that no gap exists between the resin 7 and the upper housing 20.
[0046] [Experimental Examples 5 and 6] Next, in order to examine the amount of deformation of the POF 9 due to differences in the type of resin 7, an analytical model (Experimental Example 5) in which the type of resin 7 was changed from that in Experimental Example 1, and an analytical model (Experimental Example 6) in which the arrangement was also changed were fabricated. Experimental Example 5: Epoxy resin placed at the position shown as resin 7 in FIG. 10A (lower part only) Experimental Example 6: Epoxy resin placed at the position shown as resin 7 in FIG. 11B (filled) The deformation and stress distribution of the POF 9 were calculated in the same manner as in Experimental Example 1-4, and the results are shown in FIGS. 12A shows the results of Experimental Example 1, FIG. 12B shows the results of Experimental Example 5, and FIG. 12C shows the results of Experimental Example 6.
[0047] 12A-C, in Experimental Example 1 (FIG. 12A), the POF 9 was significantly deformed at the portion in contact with the resin 7, whereas in Experimental Example 5 (FIG. 12B), the deformation of the POF 9 was suppressed at the portion in contact with the resin 7. As shown in FIGS. 12A-C (particularly FIG. 12A), the vicinity of the connector 6 (i.e., the exposed portion of the POF 9, shown surrounded by the dashed line S1 in FIGS. 12A-C) was in a state of compression, although there was a difference in strength. The region away from the connector 6 (shown surrounded by the dashed line S2 in FIGS. 12A-C) was in a state of tension, although there was a difference in strength. In addition, in Experimental Example 6 (FIG. 12C), although the deformation of POF 9 was suppressed in the portion in contact with resin 7, POF 9 was subjected to compressive stress.
[0048] [Experimental Examples 7 and 8] Furthermore, analytical models in which the type of resin 7 was changed (Experimental Examples 7 and 8) were produced. Experimental Example 7: Acrylic resin placed at the position shown as resin 7 in FIG. 10A (lower part only) Experimental Example 8: After covering POF 9 with acrylic resin, epoxy resin was placed at the position shown as resin 7 in FIG. 10A (acrylic + epoxy) Fig. 13 shows the arrangement of resin 7 in Experimental Example 8. In Experimental Example 8, acrylic resin is arranged in the portion indicated by reference symbol 7a (near POF 9), and epoxy resin is arranged in the portion indicated by reference symbol 7b. Note that in Fig. 13, the illustration of upper housing 20 is omitted in order to make the arrangement of resin 7 easier to see.
[0049] In addition to Experimental Examples 7 and 8, the longitudinal stress of the POF 9 (hereinafter sometimes referred to as "the longitudinal stress of the POF") was calculated for Experimental Examples 1 to 6, and the results are also shown in FIG. 14 also shows an analysis model (Reference Example 1) that does not use the resin 7. It has been confirmed that the POF 9 cracks when subjected to a stress of about 14.22 MPa.
[0050] From the results shown in FIG. 14, it can be seen that even if the arrangement of the resin 7 is the same, if the type of the resin 7 is different, the stress in the longitudinal direction of the POF is different (see Experimental Examples 1, 5, 7, and 8). In particular, when comparing experimental examples 5 and 8, which are subjected to stress equal to or less than that of reference example 1, which is not affected by the expansion of resin 7, with experimental examples 1 and 7, which are subjected to stress close to the stress at the time when cracks occur, it can be seen that resin 7 with a different linear expansion coefficient is used.
[0051] With this knowledge, we investigated the relationship between the linear expansion coefficient of resin 7 and the stress on POF 9. That is, using the above-mentioned advanced nonlinear simulation solution (Marc by HEXAGON), we calculated the relationship between the longitudinal stress on the bottom surface of POF 9 and the distance from connector 6 when resin 7 with a different linear expansion coefficient was used. Fig. 15 shows the results when the linear expansion coefficient of the resin 7 is 35 to 85, and Fig. 16 shows the results when the linear expansion coefficient of the resin 7 is 0 to 40. Note that Figs. 15 and 16 also show the results when silicone resin (linear expansion coefficient 153) is used.
[0052] Based on these results, the POF longitudinal stress on the bottom surface of the POF 9 at a distance of 4.3 mm from the connector 6 where the stress is the largest is also shown by linear expansion coefficient in Fig. 17. In Fig. 17, the POF longitudinal stress of 12.6 MPa when using a silicon resin (linear expansion coefficient 153) is shown as dashed line Q. A POF having a POF longitudinal stress lower than this dashed line Q is suitable as the resin 7 of the present disclosure.
[0053] On the other hand, in the exposed portion of the POF 9 (the first end region of the optical cord end), a force is generated that causes the POF 9 to expand in the longitudinal direction (Y direction) as the temperature rises. However, in the vicinity of the portion fixed by the connection with the connector 6, the expansion of the POF 9 is suppressed, and a compressive stress is generated. This is more noticeable as the linear expansion coefficient of the resin 7 decreases. 18A and 18B show the stress in the longitudinal direction of the POF applied to the POF 9 and the connector 6 when the linear expansion coefficient of the resin 7 is 35. As shown in the area surrounded by the dashed line F1 in Fig. 18A as viewed from the side, compressive stress occurs in the POF 9 near the connector 6. At this time, as shown in the area surrounded by the dashed line F2 in Fig. 18B as viewed from above, no deformation of the connector 6 is observed.
[0054] 19 also shows the stress in the POF longitudinal direction acting on the POF 9 and the connector 6 when the linear expansion coefficient of the resin 7 is 85. When the linear expansion coefficient of the resin 7 becomes high, the POF 9 is pushed upward by the expansion of the resin 7, as shown in the area surrounded by the dashed line G1 in Fig. 19A as viewed from the side. Moreover, the connector 6 is pressed by the thermal expansion of the resin 7, causing deformation, as shown in the area surrounded by the dashed line G2 in Fig. 19B as viewed from above.
[0055] Furthermore, we will also consider the case where the linear expansion coefficient of resin 7 is reduced. Figure 20A shows the longitudinal stress applied to POF 9 and connector 6 as viewed from the side when the linear expansion coefficient of resin 7 is 0. In the area surrounded by dashed line H1 in Figure 20A, there is a tendency for the stress on the top surface of POF 9 to increase. This tendency is also clear when compared with FIG. 20B, which shows the state in which the POF longitudinal direction stress on the POF 9 and the connector 6 when the linear expansion coefficient of the resin 7 is 65, viewed from the side. That is, in the area surrounded by the dashed line H2 in FIG. 20B, there is no tendency for the stress in the longitudinal direction of the POF to increase on the top surface of the POF 9 as in the area surrounded by the dashed line H1 in FIG. 20A.
[0056] Based on this finding, the relationship between the linear expansion coefficient of the resin 7 and the stress in the longitudinal direction of the POF on the upper surface of the POF 9 was also examined. That is, using the above-mentioned advanced nonlinear simulation solution (Marc by HEXAGON), the relationship between the stress in the longitudinal direction of the POF on the upper surface of the POF 9 and the distance from the connector 6 when resins with different linear expansion coefficients were used as the resin 7 was examined.
[0057] The results are shown in Fig. 21. Based on these results, the stress in the longitudinal direction of the POF on the upper surface of the POF 9 at a distance of 4.3 mm from the connector 6, where the stress is the largest, is also shown in Fig. 22 for each linear expansion coefficient. 22, the POF longitudinal stress of 12.6 MPa when using silicone resin (linear expansion coefficient 153) is shown as dashed line Q. Resins having a POF longitudinal stress lower than dashed line Q are suitable for resin 7 of the present disclosure, but all of the POF longitudinal stresses are lower than dashed line Q, and it can be understood that even if resin 7 has a low linear expansion coefficient, there is no problem with the stress on the upper surface.
[0058] From the results of these experimental examples, it was found that, regardless of the arrangement of the resin 7, when the linear expansion coefficient of the resin 7 and the linear expansion coefficient of the POF 9 satisfy certain conditions, the occurrence of cracks in the POF 9 under high temperature and high humidity conditions is suppressed.
[0059] In the above embodiment, specific embodiments of the present invention are shown, but the above embodiment is merely illustrative and should not be interpreted as being limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention. [Industrial Applicability]
[0060] INDUSTRIAL APPLICABILITY The optical communication cable of the present disclosure can be used as an optical communication cable that suppresses the occurrence of cracks in POF and has excellent durability under high temperature and high humidity conditions. [Explanation of symbols]
[0061] 1. Optical and electrical combined transmission module 2 Hybrid Cable 3. First Case 4 Second Case 5 Optical cord 6 Connectors 7. Resin 8 Covering layer 9 Plastic Optical Fiber (POF) 10 Tensile Fibers 11 Pedestal 12 Adhesive layer 13 Optical communication cable 19 cases 20 Upper case 21 Lower case E Tip of plastic optical fiber R The end of the optical cord that connects to the connector r1: a first end region where the plastic optical fiber is exposed r2: the second end region where the plastic optical fiber is not exposed
Claims
1. An optical communication cable, an optical cord having a plastic optical fiber and a coating layer provided around the plastic optical fiber; a connector to be connected to a plastic optical fiber of the optical cord; A first housing arranged on a first surface side of the connector; A second housing arranged on a second surface side of the connector; a resin for fixing the optical cord inside a case formed by combining the first housing and the second housing; The end R of the optical cord on the side to be connected to a connector has a first end region r1 in which no coating layer is formed and the plastic optical fiber is exposed, and a second end region r2 in which a coating layer is formed and the plastic optical fiber is not exposed, The tip E of the plastic optical fiber in the first end region r1 is connected to the connector, The resin is disposed so as to be in contact with the end R of the optical cord and the second housing, The linear expansion coefficient (t2) of the plastic optical fiber and the linear expansion coefficient (t1) of the resin are set to satisfy the following formula (1): Optical communication cable. t1≦t2+5 ... (1)
2. 2. The optical communication cable according to claim 1, The linear expansion coefficient (t2) of the plastic optical fiber is 50 ppm / ° C. or more and 80 ppm / ° C. or less. Optical communication cable.
3. 3. The optical communication cable according to claim 1, The resin is disposed so as to be in contact with the first housing. Optical communication cable.
4. 3. The optical communication cable according to claim 1, The resin is a resin having an epoxy group. Optical communication cable.
5. 3. The optical communication cable according to claim 1, The length of the end R of the optical cord is 4 mm or more and 8 mm or less. Optical communication cable.
6. 3. The optical communication cable according to claim 1, The length of the first end region r1 at the end R of the optical cord is 1 mm or more and 4 mm or less. Optical communication cable.
7. 3. The optical communication cable according to claim 1, The resin is disposed so as to be in contact with the first surface of the connector, A base for fixing the position of the connector is provided between the second housing and the connector. Optical communication cable.