Method for manufacturing preform
By swirling and heat-treating resin flakes from recycled polyester resin molded products, the method addresses quality deterioration issues, achieving high-quality preforms with reduced impurities and improved intrinsic viscosity.
Patent Information
- Application Number
- JP2023075249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for recycling polyester resin molded products, such as PET bottles, fail to effectively suppress the deterioration of preform quality during the recycling process, leading to issues like decreased intrinsic viscosity, production of low molecular weight impurities, and contamination of production equipment.
A method involving the preparation of resin flakes from recycled polyester resin molded products, which includes swirling the flakes with a fluid medium to remove insoluble foreign matter, followed by heat-treatment under reduced pressure conditions to promote solid phase polymerization and crystallization, and subsequent plasticization to remove impurities.
This method effectively suppresses preform quality deterioration, reduces low molecular weight impurities, and enhances the intrinsic viscosity of recycled preforms, ensuring high-quality production with minimal contamination.
Smart Images

Figure 2024159323000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a preform. [Background technology]
[0002] Conventionally, synthetic resin containers, which are made by producing a bottomed cylindrical preform using a polyester resin such as polyethylene terephthalate and then molding this preform into a bottle shape by biaxial stretch blow molding or the like, are used in a wide range of fields as containers for various beverages, seasonings, etc. This type of container is generally known as a PET bottle, and in recent years, in response to social demand, a recycling technology called "bottle-to-bottle" has been considered, in which used PET bottles are collected and reused as recycled material to manufacture PET bottles.
[0003] For example, Patent Document 1 discloses a technology in which recovered polyester resin molded products are crushed into flakes to produce resin flakes, which are then decontaminated, melted to produce resin pellets, which are then subjected to solid-state polymerization and transported to an injection molding device to produce preforms. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-98350 Summary of the Invention [Problem to be solved by the invention]
[0005] Means for Solving the Problems The present inventors have considered the above-mentioned background art and have conducted extensive research into how to prevent deterioration in the quality of preforms produced as recycled products by collecting polyester resin molded products, particularly used PET bottles, and reusing them as recycled materials through mechanical recycling. As a result, they have completed the present invention. [Means for solving the problem]
[0006] The method for manufacturing a preform according to the present invention involves the steps of preparing resin flakes by crushing recovered polyester resin molded products into flakes, swirling the resin flakes together with a flowable medium in a cylindrical swirling container, and using the resulting swirling flow to remove insoluble foreign matter that has become mixed into the resin flakes, and then heat-treating the resin flakes under reduced pressure conditions, and then supplying the molten resin obtained by plasticizing the resin flakes to an injection molding apparatus to injection mold a preform. Effect of the Invention
[0007] According to the present invention, when polyester resin molded articles are collected and reused as recycled materials by mechanical recycling to produce preforms as recycled products, deterioration in the quality of the preforms can be suppressed. [Brief description of the drawings]
[0008] [Figure 1] 1 is an explanatory diagram conceptually illustrating an entire apparatus in which an embodiment of the present invention is preferably implemented; [Diagram 2] FIG. 2 is an explanatory diagram showing an example of a swirling container for removing insoluble foreign matter in an embodiment of the present invention. [Diagram 3] FIG. 2 is an explanatory diagram showing an example of an introduction pipe provided in a swirling container for removing insoluble foreign matter in an embodiment of the present invention. [Figure 4] FIG. 2 is an explanatory diagram showing an example of an apparatus for subjecting resin flakes to a heat treatment in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Preferred embodiments of the present invention will now be described.
[0010] In this embodiment, polyester resin molded products, particularly used PET bottles, are collected and reused as recycled materials by mechanical recycling. Needless to say, it is preferable to select and remove plastic containers made of different materials such as olefin resins and polystyrene resins that are mixed into used PET bottles, but in recent years, transparent bottles made of aliphatic polyester resins containing plant-derived polylactic acid as a dicarboxylic acid component have been known. Polylactic acid is highly hydrolyzable, and aliphatic polyester resins containing polylactic acid in their segments have inferior performance compared to aromatic polyester resins, so they are preferably removed from recycled materials. For example, a bale of collected PET bottles (a mass of compressed PET bottles) is heat-treated with water vapor, and transparent bottles made of aliphatic polyester resins containing polylactic acid in their segments are weakened by selective hydrolysis, and can be removed by crushing with mechanical stimulation and physically classifying them.
[0011] In order to collect used PET bottles and reuse them as recycled materials by mechanical recycling, first, the collected used PET bottles are crushed into flakes to prepare resin flakes. In preparing such resin flakes, any cleaning method such as alkaline cleaning or hot water cleaning can be used to remove dirt such as residues of contents remaining on the surface of the resin flakes and foreign matter that has been mixed in, but it is difficult to remove insoluble foreign matter such as metal pieces and glass pieces by cleaning.
[0012] Therefore, in this embodiment, the resin flakes are swirled together with the flowable medium in a cylindrical swirling container, and the swirling flow generated by this is used to remove insoluble foreign matter that has become mixed in with the resin flakes.
[0013] 2 is a schematic diagram of an example of a swirling container. The swirling container 800 includes a swirling cylinder portion 810, an inlet pipe 820, a discharge pipe 830, and a collection pipe 840. The inlet pipe 820 is connected to a side wall portion on the top surface portion 811 side of the swirling cylinder portion 810 so that the fluid medium is introduced in the tangential direction of the inner peripheral wall surface 813 of the swirling cylinder portion 810. The discharge pipe 830 is connected to the center of the top surface portion 811 of the swirling cylinder portion 810 so as to be coaxial with the swirling cylinder portion 810, and the collection pipe 840 is connected to the center of the bottom portion 812 of the swirling cylinder portion 810 so as to be coaxial with the swirling cylinder portion 810.
[0014] In such a swirling vessel 800, the fluid medium introduced in the tangential direction of the inner peripheral wall surface 813 of the swirling cylinder portion 810 becomes a swirling flow S that descends while swirling along the inner peripheral wall surface 813 of the swirling cylinder portion 810. Then, when it reaches the bottom 812 of the swirling cylinder portion 810, the descending swirling flow S reverses at the swirling center of the descending swirling flow S and flows to become an ascending swirling flow R, and the fluid medium may be a gas such as air or a liquid such as water.
[0015] When air is used as a fluid medium to remove insoluble foreign matter from the resin flakes, the resin flakes are suspended and dispersed in the air in a spare chamber (not shown) installed upstream of the inlet pipe 820, and are then pressurized through the inlet pipe 820 on the air flow sent from the pressure pump, and are introduced from the outlet of the inlet pipe 820 in the tangential direction of the inner wall surface 813 of the swirling cylinder section 810.
[0016] At this time, the flow rate and volume of the airflow are controlled so that the mixed insoluble foreign matter is removed from the resin flakes, but when insoluble foreign matter having a higher density than the resin flakes is swirled with the airflow, it is subjected to centrifugal force and collides with the inner peripheral wall surface 813 of the swirling cylinder portion 810. The insoluble foreign matter that has lost its kinetic energy due to the collision is subjected to gravitational acceleration and falls while traveling along the inner peripheral wall surface 813 of the swirling cylinder portion 810, and can be collected in the collection tube 840 and removed.
[0017] On the other hand, the resin flakes can continue to swirl inside the swirl tube section 810 while suspended and dispersed in the air, and then ride on the ascending swirling flow R to be collected from the discharge pipe 830. At that time, the resin flakes may be collected by applying a reduced pressure and suction from the discharge pipe 830 to the extent that the swirling flows S, R are not broken. By applying a reduced pressure and suction from the discharge pipe 830, the flow rate and amount of the airflow introduced from the introduction pipe 820 into the swirl tube section 810 can also be adjusted.
[0018] In some cases, minute insoluble foreign matter may remain in the resin flakes thus collected. In such a case, similar swirling containers may be connected in series, and the swirling flows S and R may be used again to remove the minute insoluble foreign matter from the resin flakes. For example, by focusing on the particle size of the minute insoluble foreign matter to be removed, the flow rate and flow rate of the swirling flows S and R may be controlled based on the principle of dynamic classification, so that the minute insoluble foreign matter is discharged from the discharge pipe 830 on the ascending swirling flow R, and only the resin flakes may be collected in the collection pipe 840.
[0019] Furthermore, since the resin flakes are generally relatively large, with a maximum diameter of about 5 to 20 mm, it is necessary to increase the bore of the inlet pipe 820 for introducing the flakes into the swirling vessel 800 in accordance with their size. Therefore, a large pressure pump may be required to optimize the flow rate and flow rate of the swirling flows S and R. To avoid such problems, it is preferable that the inlet pipe 820 has a multiple pipe structure, for example, as shown in FIG.
[0020] When the air in which the resin flakes are suspended and dispersed is introduced into the swirl tube section 810 by the introduction tube 820 having a multiple tube structure, the air in which the resin flakes are suspended and dispersed is guided to the central tube 821 of the introduction tube 820 having a multiple tube structure, and compressed air is introduced into the outer peripheral tube 822 provided on the outer periphery of the central tube 821, and the compressed air is made to merge into the central tube 821 on the downstream side, thereby amplifying the flow speed and the amount of air flowing in the central tube 821. Although not shown in particular, the outer peripheral tube 822 may be provided in double and compressed air may be introduced into each of them, thereby further amplifying the flow speed and the amount of air flowing in the central tube 821. By making the introduction tube 820 have such a multiple tube structure, it becomes easier to control the flow speed and the amount of air when the air in which the resin flakes are suspended and dispersed is introduced into the swirl tube section 810, improving the work efficiency.
[0021] Next, a case will be described in which insoluble foreign matter is removed from the resin flakes using a liquid such as water as a flow medium. In this case, the resin flakes are dispersed in a liquid such as water in a spare chamber (not shown) installed upstream of the inlet pipe 820, and are pumped through the conduit on the liquid flow sent from the pressure pump. The resin flakes are then introduced from the outlet of the inlet pipe 820 in the tangential direction of the inner peripheral wall surface 813 of the swirling cylinder portion 810.
[0022] The liquid flow introduced into the swirling tube section 810 becomes swirling flows S and R, and insoluble foreign matter having a higher density than the resin flakes settles to the bottom 812 of the swirling tube section 810 while swirling with the liquid flow, and can be collected and removed in the collection tube 840. On the other hand, the resin flakes accumulate from the middle layer area to the upper layer area of the swirling tube section 810 while swirling with the liquid flow, and the accumulated resin flakes can be collected by suction from the discharge tube 830. In this way, when a liquid such as water is used as a flow medium to remove the mixed insoluble foreign matter from the resin flakes, the resin flakes can also be washed.
[0023] When used PET bottles (polyester resin molded products) are collected and reused as recycled materials through mechanical recycling to manufacture recycled products, the decrease in intrinsic viscosity due to deterioration of the resin caused by the heat history during the manufacturing of the collected products can cause defects in the manufacturing process of the recycled products. Furthermore, if a large amount of low molecular weight impurities such as acetaldehyde (AA) generated by thermal decomposition of polyester resin, oligomers such as bishydroxyethyl terephthalate (BHET), monohydroxyethyl terephthalate (MHET), and cyclic trimer (CT) generated by depolymerization of polyester resin, and limonene derived from the contents remain in the recycled materials, they not only affect the quality of the recycled products manufactured, but also cause productivity to decrease by fouling the manufacturing equipment.
[0024] In this embodiment, in order to avoid such problems, the prepared resin flakes are subjected to a heat treatment, preferably in an atmosphere reduced in pressure to 1000 Pa or less and at a temperature of preferably 160 to 240°C, to proceed with the solid-state polymerization reaction of the polyester resin that forms the resin flakes and promote crystallization while keeping the resin flakes in their flake-like form without melting the resin flakes.
[0025] By proceeding with the solid-phase polymerization reaction, the end groups of the polyester resin, whose degree of polymerization has decreased due to the cutting of the molecular chains caused by deterioration, are recondensed, and as the degree of polymerization is restored, the intrinsic viscosity corresponding to the molecular weight can be restored. Furthermore, by subjecting the resin flakes to a heat treatment under reduced pressure conditions, particularly by exposing them to a temperature atmosphere of 160 to 240°C under reduced pressure conditions, it is possible to suppress hydrolysis of the polyester resin and to favorably promote crystallization by utilizing the melting point lowering effect. This reduces the free volume between the molecular chains of the polyester resin (reducing the amorphous phase), and selectively bleeds out the low molecular weight impurity components (organic impurity components) as described above that were included in the free volume portion of the resin flakes and the moisture sorbed in the resin flakes to the surface layer of the resin flakes, and these can be volatilized or evaporated, or washed with hot water, steam, an organic solvent, or the like as necessary, to efficiently remove them.
[0026] In this embodiment, the specific method of subjecting the resin flakes to the heat treatment is not particularly limited. For example, it is preferable to subject the resin flakes to the heat treatment using a treatment device 100 as shown in FIG. 4, which includes at least one preheating chamber 102 and a treatment chamber 103 capable of adjusting the internal atmosphere to a temperature and pressure suitable for the heat treatment.
[0027] Here, the outline of the processing apparatus 100 shown in FIG. 4 will be described. The processing apparatus 100 is preferably 7 to 18 m 3 The system includes a sealed container 101 constructed to have an internal volume of 100 mm. A processing chamber 103 is provided inside the sealed container 101, and two preheating chambers 102 are provided above the sealed container 101. The preheating chambers 102 are connected to the sealed container 101 via an opening / closing mechanism such as a sliding shutter (not shown) so as to be able to communicate with the processing chamber 103 while maintaining airtightness from the outside of the system. In FIG. 4, illustration of incidental equipment such as a heating device for adjusting the internal atmosphere of the processing chamber 103, a pressure reducing device, and associated piping is omitted.
[0028] In order to subject resin flakes to a heat treatment using such a treatment apparatus 100, it is preferable to, prior to the heat treatment, put the resin flakes into the preheating chamber 102, seal the preheating chamber 102, heat the resin flakes to a predetermined temperature, and reduce the pressure inside the preheating chamber 102 to a predetermined pressure. At that time, it is preferable to, for example, provide a nozzle opening on the inner wall surface of the preheating chamber 102 to spray heated gas (e.g., an inert gas such as N2 gas) into the preheating chamber 102, and appropriately adjust the direction and amount of the gas to generate an airflow inside the preheating chamber 102, thereby stirring and heating the resin flakes, and to reduce the pressure inside the preheating chamber 102 so that at least a part of the impurity components contained in the resin flakes is dispersed and removed outside the system.
[0029] In this way, when raising the temperature of the resin flakes, it is preferable to appropriately adjust the final temperature and pressure in the preheating chamber 102 taking into consideration the internal atmosphere of the processing chamber 103. Then, it is preferable to open the opening and closing device and, while maintaining airtightness from the outside of the system, allow the resin flakes in the preheating chamber 102 to fall by their own weight, so that the resin flakes are supplied into the processing chamber 103 without damaging the internal atmosphere of the processing chamber 103, which has been adjusted to a temperature and pressure suitable for the heat treatment.
[0030] In the processing apparatus 100 shown in FIG. 4, resin flakes are sequentially fed into two preheating chambers 102, and preheating treatments for raising the temperature of the resin flakes are alternately performed, and the resin flakes are dropped into the processing chamber 103 in the order from the preheating chamber 102 in which the fed resin flakes have been heated to a predetermined temperature, but this is not limited thereto. The number of preheating chambers 102 may be one or three or more depending on the processing capacity of the processing apparatus 100, that is, the total amount of resin flakes that can be subjected to heat treatment per unit time. In any case, it is preferable to repeat the operation of dropping the resin flakes from the preheating chamber 102 into the processing chamber 103, so that the resin flakes are stacked in layers for each group that is dropped. It is preferable to expose the resin flakes to the internal atmosphere of the processing chamber 103 while the resin flakes are piled up in the processing chamber 103, so that the resin flakes can be subjected to heat treatment.
[0031] The processing time for heat-treating the resin flakes is usually 30 minutes or more, and is preferably adjusted appropriately within the range of 1 to 8 hours in order to proceed with the solid-phase polymerization reaction while suppressing the deterioration of the resin hue. It is preferable to manage the processing time so that the resin flakes deposited in the processing chamber 103 are sequentially removed from the processing chamber 103 in equal amounts to the amount dropped from the preheating chamber 102, starting from the lower layer side of the resin flakes deposited in layers as described above, after the processing time has elapsed. At that time, the time required for the preheating treatment in the preheating chamber 102 depends on the water content and shape of the resin flakes, and there may be variation in the intervals at which the resin flakes are dropped. Therefore, it is preferable to manage the processing time for each group of dropped resin flakes.
[0032] In this way, in order to suitably manage the processing time when heat-treating the resin flakes, the processing apparatus 100 shown in Fig. 4 is provided with an opening / closing mechanism 104 on the bottom side of the sealed container 101. The opening / closing mechanism 104 forms the bottom surface of the processing chamber 103 and is configured to serve as a partition between the processing chamber 103 and the removal section 105 provided at the bottom of the sealed container 101. This allows the resin flakes to spill into the removal section 105 when the opening / closing mechanism 104 is opened, and by appropriately adjusting the timing of opening and closing the opening / closing mechanism 104, it is possible to remove an amount of resin flakes equal to the amount dropped from the preheating chamber 102, and although there will be some mixing, the resin flakes can be removed for each group dropped from the preheating chamber 102.
[0033] As described above, impurity components can be efficiently removed by performing heat treatment under reduced pressure conditions, but it is not preferable that the volatilized or evaporated impurity components remain in the treatment chamber 103. For this reason, the treatment apparatus 100 shown in FIG. 4 is configured to circulate the gas phase components in the treatment chamber 103, and to include a circulation flow path 106 including a catalyst tank 107 in the path for decomposing low molecular weight impurity components derived from polyester resin, and to connect the circulation flow path 106 to the treatment chamber 103. By configuring the treatment apparatus 100 in this way, it is preferable to reduce the impurity components remaining in the treatment chamber 103 by guiding the gas phase components in the treatment chamber 103 to the circulation flow path 106 and circulating them without damaging the internal atmosphere of the treatment chamber 103, for example, by using an inert gas such as N2 gas as a carrier gas.
[0034] In addition, when cleaning the impurity components selectively bled out on the surface layer of the resin flakes, the resin flakes taken out of the treatment chamber 103 can be liquid cleaned using a rotary or convection type liquid cleaner, or steam cleaned using a pressurized steam convection cleaner, although not shown in the figure. When applying liquid cleaning, the resin flakes after cleaning must be dried. For this drying process, the resin flakes may be subjected to a heat treatment again in an atmosphere equivalent to the internal atmosphere of the treatment chamber 103, or may be dried using a hot air circulation dryer. Furthermore, the resin flakes can be dried by using two jacketed rolls with spiral grooves on the surface, utilizing the shear heat generated by the rotation of the rolls to semi-weld and press the surface layer of the resin flakes, and further removing organic impurities and moisture from the resin flakes using a rotary forward drying device (open roll type twin screw extruder). In this case, the resin flakes dried in the open-roll twin-screw extruder are easily separated and dispersed into flakes by the pressure of the compression rolls in the cooling section downstream of the rolls.
[0035] In this embodiment, the resin flakes are heat-treated under reduced pressure conditions as described above to remove (decontaminate) low molecular weight impurities, and then plasticized. At that time, the heat-treated resin flakes may be fed into the extruder 200 and plasticized while being melt-kneaded by the heat from the heating cylinder and the shear heat from the screw, but it is preferable to use a twin-screw extruder for plasticization. The twin-screw extruder has a high kneading effect, can plasticize the resin flakes more uniformly, and can also shorten the time required for plasticization, so it is also preferable in terms of suppressing deterioration, thermal decomposition, and depolymerization of the resin.
[0036] When plasticizing resin flakes using a twin-screw extruder, it is preferable to configure the twin-screw extruder to have a vent port, and for example, to exhaust gas phase components containing low molecular weight impurity components derived from polyester resins retained in the twin-screw extruder by vacuum suction through a vent port provided through a heating cylinder to the outside of the system. This makes it possible to further reduce impurity components remaining in the plasticized polyester resin. In particular, cyclic oligomers are generated during equilibrium reactions during thermal melting, so cyclic oligomers are generated when polyethylene terephthalate is melted. Therefore, it is important to perform the operation of absorbing and removing them under reduced pressure at the vent port of the twin-screw extruder. The optimal conditions (temperature and pressure) for gas-liquid separation of cyclic oligomers are estimated. The melting point of cyclic oligomers is 319°C and they are sublimable. Assuming that the resin melt temperature at the vent port of a twin-screw extruder for polyethylene terephthalate is 300°C, the reduced vacuum pressure at which cyclic oligomers can sublimate (transform into gas) is generally 0.1 KPa (100 Pa) or less, so it is necessary to adjust the pressure to a relatively high vacuum. This increases the possibility of the molten resin venting up at the vent port. To avoid venting up, it is preferable to use a twin-screw extruder with counter-rotating (different) screw rotations rather than the same (same) screw rotation type.
[0037] Furthermore, the resin flakes removed from the treatment chamber 103 as described above may be directly fed into the extruder 200 for plasticization, or may be stored in the buffer tank 300 and then fed into the extruder 200 for plasticization. When managing the treatment time during the heat treatment of the resin flakes as described above, the resin flakes are intermittently removed from the treatment chamber 103 according to the interval at which the operation of dropping the resin flakes from the preheating chamber 102 into the treatment chamber 103 is repeated, and the amount of resin flakes removed each time also depends on the amount of processing in the preheating chamber 102. In such a case, particularly if there is variation in the interval at which the operation of dropping the resin flakes is repeated, the amount of resin flakes removed per unit time will not be constant. Therefore, if the resin flakes are stored in the buffer tank 300 and can be removed from the buffer tank 300 in fixed amounts at any desired intervals, the amount of resin flakes added can be easily adjusted according to the processing capacity of the extruder 200 so that the amount of resin plasticized in the extruder 200 can always be maintained constant.
[0038] When installing the buffer tank 300, it is preferable to appropriately adjust the internal volume of the buffer tank 300 so that a larger amount of resin flakes can be stored. By doing so, even if a problem occurs in the process subsequent to the process of plasticizing the resin flakes, causing the subsequent process to be stopped, the heat treatment of the resin flakes can be continued without being stopped, and the amount that cannot be sent to the subsequent process can be stored in the buffer tank 300.
[0039] Also, in anticipation of such trouble occurring or changes in circumstances such as an increase or decrease in the processing speed of the subsequent process, a relief tank 400 can be installed midway along the transport path that transports the resin flakes removed from the processing chamber 103 to the buffer tank 300. It is preferable to transport the resin flakes to the buffer tank 300 while allowing them to be evacuated to the relief tank 400 during transport.
[0040] In this way, for example, when the subsequent process is stopped, the resin flakes taken out of the processing chamber 103 can be evacuated to the relief tank 400, and the transport to the buffer tank 300 can be limited. When the processing speed of the subsequent process is increased, in addition to the resin flakes taken out of the processing chamber 103, the resin flakes evacuated to the relief tank 400 can also be transported to the buffer tank 300. When the processing speed of the subsequent process is decreased, a part of the resin flakes taken out of the processing chamber 103 can be evacuated to the relief tank 400, and the amount of the resin flakes transported to the buffer tank 300 can be appropriately adjusted. In this way, when the resin flakes are evacuated to the relief tank 400 as necessary, the internal atmosphere of the relief tank 400 is preferably set to 100° C. or higher so that the resin flakes do not become hydrated.
[0041] In this embodiment, after the above-mentioned steps, the molten resin obtained by plasticizing the resin flakes is supplied to the injection molding device 500 to injection mold the preform. At that time, it is preferable to remove residual foreign matter that could not be removed at the stage of the resin flakes from the plasticized molten resin as necessary. In order to remove the residual foreign matter from the plasticized molten resin, for example, a filter 600 for removing residual foreign matter may be provided on the discharge port side of the extruder 200.
[0042] The specific configuration of the injection molding apparatus 500 is not particularly limited, and for example, a preform can be injection molded using an injection molding apparatus 500 equipped with at least one injection pot configured to measure the supplied molten resin and then inject a fixed amount of the molten resin, and a preform mold.
[0043] When supplying the molten resin obtained by plasticizing the resin flakes to the injection molding apparatus 500, it is undesirable for the resin to deteriorate (especially its hue) during transportation. To this end, in order to shorten the time that the molten resin remains in the transportation path, it is preferable to set the transportation distance until it is supplied to the injection molding apparatus 500 after removing residual foreign matter, more specifically, the distance from the outlet of the gear pump 700 installed downstream of the filter 600 to the inlet of the injection pot provided in the injection molding apparatus 500, to 1 to 7 m. In this case, the transportation amount of the molten resin is preferably 900 to 1500 kg / h.
[0044] According to the present embodiment as described above, when polyester resin molded products, particularly used PET bottles, are collected and reused as recycled materials by mechanical recycling to manufacture preforms as recycled products, deterioration of the quality of the preforms can be suppressed. In particular, according to the present embodiment, although the preforms are manufactured by recycling the collected polyester resin molded products, the residual amount of acetaldehyde is 1 to 15 ppm, preferably 1 to 10 ppm, more preferably 1 to 5 ppm, the residual amount of bishydroxyethyl terephthalate is 1 to 35 ppm, preferably 1 to 30 ppm, more preferably 1 to 20 ppm, the residual amount of monohydroxyethyl terephthalate is 1 to 35 ppm, preferably 1 to 30 ppm, more preferably 1 to 20 ppm, the residual amount of cyclic trimer is 6000 ppm or less, preferably 4000 ppm or less, more preferably 3000 ppm or less, and preferably, when the mass of the preform is 14 to 50 g, the residual amount of cyclic trimer is 6000 ppm or less, preferably 4000 ppm or less, more preferably 3000 ppm or less. * a * b * L in color space * Value 70-90, b * Preforms having a value of 2 to 18 can be successfully manufactured.
[0045] Here, the remaining amounts of acetaldehyde, bishydroxyethyl terephthalate (BHET), monohydroxyethyl terephthalate (MHET), and cyclic trimer (CT) can be determined, for example, as follows.
[0046] <Residual amount of acetaldehyde> Using the section cut out from the preform as a sample, weigh 1.0 g of such a sample into a glass bottle, add 5.0 mL of pure water, and seal it. After heating this suspension in an oven adjusted to 120°C for 60 minutes, cool it in ice water. Collect 1.0 mL of the supernatant of the suspension, add 0.2 mL of a 2,4-dinitrophenylhydrazine·phosphoric acid solution with a concentration of 0.1% thereto, and measure the one left standing for 30 minutes by high performance liquid chromatography. At the same time, measure the standard solution, and calculate the acetaldehyde content based on the obtained calibration curve.
[0047] <Residual amounts of BHET, MHET, and CT> Using the section cut out from the preform as a sample, weigh 0.2 g of such a sample, add 1 mL of a mixed solvent of hexafluoroisopropanol and chloroform (weight ratio 1 / 1) thereto, and completely dissolve it. After adding 4 mL of chloroform to the solution, gradually add 5 mL of acetonitrile, and leave it standing for 3 hours to precipitate the PET polymer. Collect 1 mL from this suspension, filter it through a membrane filter with a pore size of 0.45 μm, and measure the filtrate by high performance liquid chromatography. At the same time, measure the standard solution, and calculate the contents of MHET, BHET, and CT in the pellet based on the obtained calibration curve.
[0048] Also, L * a * b * L in the color system * value, b * The value shall be measured with a spectrocolorimeter under the measurement conditions of a D65 light source and a 2° field of view, with the body part of the preform as the measurement site.
[0049] As described above, the present invention has been described by showing preferred embodiments. However, it goes without saying that the present invention is not limited only to the above-described embodiments, and various modifications can be made within the scope of the present invention.
[0050] For example, in the above-described embodiment, prior to heat-treating the resin flakes under reduced pressure conditions, the resin flakes are swirled together with the fluid medium in the cylindrical swirling vessel 800, and the resulting swirling flows S and R are used to remove insoluble foreign matter mixed into the resin flakes, but this is not limiting. The resin flakes may be heat-treated under reduced pressure conditions, and then the insoluble foreign matter mixed into the resin flakes may be removed. [Explanation of symbols]
[0051] 100 Processing equipment 102 Preheating Room 103 Processing Room 107 Catalyst tank 200 Extruder (twin screw extruder) 300 Buffer Tank 400 Relief Tank 500 injection molding equipment 600 Filters 700 Gear Pump 800 Swirling vessel S. Descending swirling flow R Upward swirling flow
Claims
1. The collected polyester resin molded products are pulverized into flakes to prepare resin flakes; A step of rotating the resin flakes together with a fluidized medium in a cylindrical rotating vessel, and removing insoluble foreign matter mixed in the resin flakes by utilizing the resulting swirling flow; heat-treating the resin flakes under reduced pressure; After that, A method for producing a preform, comprising the steps of: supplying a molten resin obtained by plasticizing the resin flakes to an injection molding device and injection molding the preform.
2. The method for producing a preform according to claim 1, wherein the heat-treated resin flakes are fed into a twin-screw extruder to be plasticized.
3. The method for producing a preform according to claim 2, wherein the twin-screw extruder is provided with a vent port, and gas phase components containing low molecular weight impurity components derived from the polyester resin remaining in the twin-screw extruder are sucked under reduced pressure through the vent port and discharged outside the system.
4. 2. The method for producing a preform according to claim 1, wherein residual foreign matter is removed from the plasticized molten resin, and the transport distance until the molten resin is supplied to the injection molding device after the residual foreign matter removal is 1 to 7 m.
5. The method for producing a preform according to claim 1, wherein the resin flakes are heat-treated in an atmosphere reduced to 1000 Pa or less and at a temperature of 160 to 240°C.
6. A method for manufacturing a preform as described in claim 5, comprising the steps of: putting the resin flakes into a preheating chamber, heating the resin flakes to a predetermined temperature, reducing the pressure inside the preheating chamber to a predetermined pressure, and then dropping the resin flakes from the preheating chamber into a processing chamber whose internal atmosphere is adjusted to a predetermined temperature and pressure while maintaining airtightness from the outside of the system, and repeating this operation to deposit the resin flakes in the processing chamber and subject them to a heat treatment.
7. A method for manufacturing a preform as described in claim 6, wherein the heat-treated resin flakes are sequentially removed from the treatment chamber in amounts equal to the amount dropped from the preheating chamber, starting from the lower layer deposited in the treatment chamber, and plasticized.
8. A method for manufacturing a preform as described in claim 6, wherein the heat-treated resin flakes are sequentially removed from the treatment chamber in amounts equal to the amount dropped from the preheating chamber, starting from the lower layer side of the layer piled up in the treatment chamber, stored in a buffer tank, and then plasticized.
9. A method for manufacturing a preform as described in claim 8, wherein a relief tank is installed midway along a transport path for transporting the resin flakes removed from the processing chamber to the buffer tank, so that the resin flakes can be evacuated to the relief tank during transport while being transported to the buffer tank.
10. The method for manufacturing a preform according to any one of claims 6 to 9, wherein the resin flakes are sequentially fed into a plurality of preheating chambers, and the resin flakes are dropped into the processing chamber in the order of the preheating chamber in which the fed resin flakes have been heated to a predetermined temperature.
11. The method for manufacturing a preform according to any one of claims 6 to 9, further comprising: blowing a heated gas into the preheating chamber to heat the resin flakes while stirring them, and suctioning the inside of the preheating chamber under reduced pressure.
12. A method for manufacturing a preform according to any one of claims 6 to 9, wherein the treatment chamber is connected to a circulation flow path that allows the gas phase components in the treatment chamber to circulate and includes a catalyst tank in the path that decomposes low molecular weight impurity components derived from polyester-based resins, and the gas phase components in the treatment chamber are guided to the circulation flow path and circulated, thereby reducing the impurity components remaining in the treatment chamber.
Citation Information
Patent Citations
Resin product manufacturing method, resin product manufacturing system, and transfer device
JP2021098350A