Ink composition for metal printing

The combination of an alkyd resin with a phthalic acid skeleton and rosin-modified resin in the ink composition addresses repellency and transferability issues, enhancing the quality of metal printing with water-based varnishes and improving whiteness, particularly in high-pigment inks.

JP2024159391APending Publication Date: 2024-11-08SAKATA INX
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023120356
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing metal printing ink compositions face issues with repellency and reduced quality of the coating film when using water-based overprint varnishes, leading to poor transferability and whiteness, especially in high-pigment content inks, and there is a need for improved compatibility with aqueous overprint varnishes to enhance printing speed and productivity.

Method used

An ink composition for metal printing that combines an alkyd resin with a phthalic acid skeleton and a rosin-modified resin, using specific solvents to improve transferability and compatibility with water-based overprint varnishes, while maintaining high whiteness and suppressing repellency.

Benefits of technology

The ink composition achieves favorable transfer properties, suppresses repellency of water-based overprint varnishes, and enhances the whiteness of white ink compositions, ensuring good transferability without excessive oil length, suitable for high-pigment content applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159391000001
    Figure 2024159391000001
  • Figure 2024159391000002
    Figure 2024159391000002
  • Figure 2024159391000003
    Figure 2024159391000003
Patent Text Reader

Abstract

To provide an ink composition for metal printing which can obtain good transferrability in printing and can improve a degree of whiteness in a white ink composition.SOLUTION: An ink composition for metal printing contains a coloring pigment, a rosin-modified resin, an alkyd resin and a solvent, wherein the alkyd resin has a phthalic acid skeleton in the molecule. Specifically, good transferrability in printing can be obtained and a degree of whiteness in a white ink composition is improved by using a substance having a phthalic acid skeleton in the molecule as an alkyd resin added to the ink composition, and combining the substance with a rosin-modified resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink composition for metal printing. [Background technology]

[0002] For printing on the outer metal surfaces of metal materials, such as galvanized or tinned iron sheets, aluminum sheets, or metal cans made from these metal materials, ink compositions for metal printing are used which contain, as the main vehicle components, binder resins such as alkyd resins, polyester resins, and epoxy resins, and organic solvents such as mineral oils or higher alcohols.

[0003] Moreover, these printing surfaces are generally coated with an overprint varnish to improve the adhesion of the ink coating, bending resistance, impact resistance, abrasion resistance, etc. The most widely used overprint varnishes are solvent-based varnishes that contain binder resins such as alkyd resins, polyester resins, acrylic resins, and epoxy resins, hardeners such as melamine resins and benzoguanamine resins, and organic solvents such as mineral oils and cellosolves.

[0004] When printing on the outer metal surface, ink is printed using an offset printing machine, dry offset printing machine, etc., and then an overprint varnish is applied wet-on-wet onto the ink coating using a coater, etc., and then baked at 150 to 280°C.

[0005] However, in recent years, due to the problem of air pollution caused by solvents and the hygienic and safety aspects of the printing work environment, it has become common to adopt water-based overprint varnishes in the field of metal printing instead of the solvent-based overprint varnishes that have been used in the past. However, when a water-based overprint varnish is applied onto an ink coating film of a conventional ink composition for metal printing, there are problems such as the repelling of the water-based overprint varnish and the penetration of the water-based overprint varnish into the ink film, resulting in a significant decrease in the quality of the coating film, such as gloss or adhesion. Therefore, there has been a demand for ink compositions to have excellent suitability for water-based overprint varnishes.

[0006] As a method for improving suitability for such aqueous overprint varnish, for example, Patent Document 1 proposes the use of an alkylene glycol-based solvent having 4 to 8 carbon atoms, Patent Document 2 proposes the use of a polyoxyalkylene glycol-based solvent, Patent Document 3 proposes the use of a polyoxyalkylene alkyl ether-based organic solvent, and Patent Document 4 proposes the use of a polyoxyalkylene alkyl ester-based solvent. These organic solvents used in ink compositions are effective in improving the suitability of the ink composition for aqueous overprint varnish, but there is room for improvement in that the ink composition tends to have insufficient fluidity and tends to cause misting during printing.

[0007] When attempting to improve the fluidity of an ink composition for metal printing or misting during printing, there is a method of using a solvent with low polarity, such as a high-boiling aromatic hydrocarbon, as described in the examples of Patent Document 5. However, in recent years, with the aim of further reducing the environmental load, water-based overprint varnish products in which the solvent content has been reduced to the minimum have been distributed, and when such an overprint varnish is used, there is also a problem of repelling occurring with an ink composition that uses a solvent with low polarity.

[0008] In recent years, the printing speed of metal printing has been increased in order to improve productivity. From the viewpoint of responding to such high-speed printing, the transferability of the ink composition is important. From the viewpoint of ensuring the transferability of the ink composition, it is effective to increase the oil length of the alkyd resin contained in the ink composition. However, an ink composition containing an alkyd resin with a long oil length is incompatible with the above-mentioned aqueous overprint varnish, and is likely to cause the problem of repelling of the aqueous overprint varnish on the surface of the printed ink composition. In other words, there is a trade-off between the increase in oil length based on the viewpoint of transferability and the suitability for application to the aqueous overprint varnish, which has been one of the technical challenges.

[0009] Furthermore, there is a demand for a white ink composition that provides high whiteness for metal cans such as beverage cans, and this has also been an issue in designing ink compositions. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Special Publication No. 5-75031 [Patent Document 2] Special Publication No. 5-40791 [Patent Document 3] Special Publication No. 5-40792 [Patent Document 4] Japanese Patent Application Publication No. 64-60670 [Patent Document 5] JP 2009-249435 A Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in consideration of these circumstances, and has an object to provide an ink composition for metal printing that can obtain good transferability during printing and can improve the whiteness of a white ink composition. [Means for solving the problem]

[0012] As a result of intensive research into solving the above problems, the present inventors discovered that the above problems can be solved by using an alkyd resin having a phthalic acid skeleton in the molecule as an alkyd resin to be added to an ink composition and combining this with a rosin-modified resin, and thus completed the present invention. Specifically, the present invention provides the following.

[0013] (1) The present invention is an ink composition for metal printing comprising a color pigment, a rosin-modified resin, an alkyd resin, and a solvent, wherein the alkyd resin has a phthalic acid skeleton in its molecule.

[0014] (2) The present invention also provides the ink composition for metal printing according to item (1), wherein the alkyd resin has an oil length of 20 to 50 mass %.

[0015] (3) The present invention also relates to the ink composition for metal printing according to item (1) or (2), in which the alkyd resin has a weight average molecular weight of 10,000 or less.

[0016] (4) The present invention also provides the ink composition for metal printing according to any one of (1) to (3), wherein the rosin-modified resin has a hydroxyl value of 10 mgKOH / g or more.

[0017] (5) The present invention also relates to an ink composition for metal printing according to any one of items (1) to (4), characterized in that the solvent contains at least one compound selected from the group consisting of compounds represented by the following general formula (1): [ka] (In the above general formula (1), each A is independently an alkylene group having 2 to 4 carbon atoms which may have a branch, R is an alkyl group having 1 to 13 carbon atoms which may have a branched and / or cyclic structure, and n is an integer of 2 to 8.)

[0018] (6) The present invention also relates to the ink composition for metal printing according to any one of (1) to (5), wherein the rosin-modified resin is a rosin ester resin. Effect of the Invention

[0019] According to the present invention, there is provided an ink composition for printing on metal, which can provide good transferability during printing and can improve the whiteness of a white ink composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, one embodiment of the ink composition for metal printing of the present invention will be described. Note that the present invention is not limited to the following embodiment, and can be practiced by making appropriate modifications within the scope of the present invention.

[0021] The ink composition of the present invention is for metal printing, and is preferably applied to printing by the so-called dry offset printing method using a relief plate as a printing plate, or the offset printing method using a lithographic plate as a printing plate, but can be applied to all printing methods commonly used in metal printing. In addition, the ink composition of the present invention can suppress repelling of the applied OP varnish even if an aqueous overprint varnish (OP varnish) is applied wet-on-wet immediately after printing with the ink composition, so it can be preferably applied to two-piece can printing in which such printing and coating methods are adopted, and can also be preferably used in three-piece can printing. According to the ink composition of the present invention, good transferability can be maintained even in cases where the pigment content must be set high, such as in a white ink composition. Furthermore, according to the ink composition of the present invention, good transferability during printing can be obtained without extremely increasing the oil length of the alkyd resin, so that printing can be performed that achieves both suppression of repelling and good transferability during printing, even if an aqueous OP varnish with a reduced solvent component is applied wet-on-wet.

[0022] The ink composition of the present invention is an ink composition for printing on metal, comprising a color pigment, a rosin-modified resin, an alkyd resin and a solvent, and is characterized in that the alkyd resin has a phthalic acid skeleton in the molecule. Each component will be described below.

[0023] [Rosin modified resin] The ink composition of the present invention contains a rosin-modified resin. The rosin-modified resin is a resin prepared using rosin as one of the raw materials. Rosin contains a mixture of resin acids such as abietic acid, palustric acid, isopimaric acid, and levopimaric acid, and these resin acids contain hydrophilic and chemically active carboxyl groups, and some of them have conjugated double bonds. Therefore, various rosin-modified resins are prepared by combining polyhydric alcohols and polybasic acids and polycondensing them, adding resol, which is a condensate of phenol, to the benzene ring contained in the rosin skeleton, or by carrying out a Diels-Alder reaction with maleic anhydride or maleic acid, which is a dienophile, to add maleic acid or maleic anhydride skeleton. Various types of such rosin-modified resins are commercially available, and it is also possible to obtain and use them.

[0024] Examples of the rosin modified resin include rosin ester resin, maleic rosin, fumarated rosin resin, rosin modified maleic acid resin, rosin modified fumaric acid resin, rosin modified phenolic resin, rosin modified alkyd resin, rosin modified polyester resin, etc. In the present invention, any of the rosin modified resins may be used, but among these, rosin ester resins are preferably used.

[0025] The rosin-modified resin used in the present invention is preferably one having a hydroxyl value of 10 mgKOH / g or more. By including such a rosin-modified resin having a high hydroxyl value in the ink composition of the present invention, the transferability of the ink composition during printing can be improved, and the polarity of the composition itself becomes high, so that the affinity with the aqueous OP varnish, which also has a high polarity, is increased, and even if the ink composition is applied wet-on-wet, repelling is suppressed. The hydroxyl value of the rosin-modified resin is more preferably 15 mgKOH / g or more, and even more preferably 20 mgKOH / g or more. The upper limit of the hydroxyl value of the rosin-modified resin is not particularly limited, but an example is about 200 mgKOH / g, preferably about 150 mgKOH / g, and more preferably about 100 mgKOH / g.

[0026] Although not particularly limited, the acid value of the rosin-modified resin is preferably 100 mgKOH / g or less. The acid value of the rosin-modified resin is preferably 100 mgKOH / g or less, since it is possible to suppress repelling when the aqueous OP varnish is applied wet-on-wet, and to achieve printability such as suppressing misting and bubbly. The acid value of the rosin-modified resin is more preferably 80 mgKOH / g or less, and even more preferably 50 mgKOH / g or less.

[0027] The rosin-modified resin is used in a state in which it is dissolved or dispersed by heating together with a solvent described later to form a varnish. The rosin-modified resin may be used as a dissolved varnish in a state in which it is dissolved or dispersed in a solvent, or may be used in a state in which a divalent or higher metal alkoxy compound is added as a gelling agent to the dissolved varnish obtained by dissolving the resin when preparing the varnish, and the resin is used in a gelled varnish. Among these, it is preferable to prepare a dissolved varnish from the rosin-modified resin and use this to prepare the ink composition, since this can improve the transferability of the ink composition during printing. In addition, by preparing a gelled varnish from the rosin-modified resin and using this to prepare the ink composition, the ink composition is given an appropriate viscoelasticity, which can improve the flowability and reduce misting, and can form a tougher cured coating.

[0028] The content of the rosin-modified resin in the ink composition is preferably 5 to 50 mass% relative to the entire composition, more preferably 5 to 25 mass% relative to the entire composition, and even more preferably 7 to 20 mass% relative to the entire composition.

[0029] [Alkyd resin] The ink composition of the present invention contains an alkyd resin in addition to the rosin-modified resin. The alkyd resin is a condensation polymer of a polyhydric alcohol and a polybasic acid, and is a type of polyester. It can also be prepared by condensation polymerization with animal and vegetable oils and / or their fatty acids. At this time, the animal and vegetable oils are transesterified with the polyhydric alcohol to become fatty acids, which are incorporated into the structure of the alkyd resin. The proportion of fatty acids derived from the animal and vegetable oils in the alkyd resin is called the oil length, and the oil length of the alkyd resin used in the present invention is preferably 20 to 50 mass%.

[0030] The alkyd resin used in the present invention has a phthalic acid skeleton in the molecule. Such an alkyd resin is prepared by using phthalic acid or phthalic anhydride as a polybasic acid. By using such an alkyd resin, the transferability of the ink is improved, and the whiteness of the white ink can be further increased. The alkyd resin of the present invention may be prepared by using other polybasic acids in addition to phthalic acid or phthalic anhydride. In the present invention, the term "phthalic acid" refers to phthalic acid in the narrow sense having two carboxy groups at the ortho positions of the benzene ring, and does not refer to terephthalic acid or isophthalic acid.

[0031] In the present invention, a coconut oil-modified alkyd resin is preferably used as the alkyd resin, which is preferable in that the dispersion stability of the ink composition is improved and a good hue with high transparency can be obtained by using a coconut oil-modified alkyd resin as the alkyd resin.

[0032] An alkyd resin having a phthalic acid skeleton in the molecule can be obtained, for example, as a condensation polymer of an acid component consisting of a fatty acid and a polybasic acid including at least phthalic acid or phthalic anhydride, and a polyhydric alcohol. Next, a method for preparing such an alkyd resin will be described.

[0033] Fatty acids are obtained by hydrolysis of natural fats and oils such as vegetable oils and animal oils, and have one carboxyl group, so that they can form esters with polyhydric alcohols, which will be described later. By introducing such fatty acids into the alkyd resin, it is possible to improve the transferability of the ink composition using the alkyd resin and to increase the ratio of biomass-derived components. From this viewpoint, it is preferable to use an amount of fatty acid such that the oil length, which is the ratio (mass%) of the mass of the fatty acid portion to the mass of the entire resin, is about 20 to 50 mass%. As described above, coconut oil-modified alkyd resin is preferably used as the alkyd resin in the present invention, and in order to obtain such an alkyd resin, coconut oil fatty acid may be used as one of the fatty acids. Of course, in this case, other fatty acids may be used in addition to coconut oil fatty acid.

[0034] The polybasic acid is a compound having multiple carboxy groups, and is a component for polycondensation with a polyhydric alcohol to be described later to obtain a high molecular weight. As a compound having multiple carboxy groups, phthalic acid or phthalic anhydride is essential as described above, and in addition, any compound that has been used in the synthesis of an alkyd resin can be used without limitation.

[0035] Examples of such polybasic acids include isophthalic acid, terephthalic acid, adipic acid, trimellitic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexenedicarboxylic acid, 1,4-cyclohexenedicarboxylic acid, hexahydrophthalic anhydride, 5-sodiosulfoisophthalic acid, fumaric acid, benzoic acid, tert-butylbenzoic acid, tetrahydrophthalic anhydride, maleic anhydride, succinic acid, succinic anhydride, fumaric acid, sebacic acid, azelaic acid, tetrabromophthalic anhydride, methylhimic anhydride, tetrachlorophthalic anhydride, hexahydrophthalic anhydride, pyromellitic anhydride, trimellitic anhydride, methylcyclohexenedicarboxylic anhydride, etc. These can be used alone or in combination of two or more together with phthalic acid or phthalic anhydride, which is the essential component.

[0036] The polyhydric alcohol forms an ester with the above-mentioned acid component, and increases the molecular weight of these components. As the polyhydric alcohol, any of those that have been used in the synthesis of alkyd resins so far can be used without limitation, and examples of such polyhydric alcohol include compounds having two or more hydroxyl groups.

[0037] Such compounds include ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, diethylene glycol, triethylene glycol, polyethylene glycol, dipropylene glycol, 1,3-butanediol, neopentyl glycol, spiro glycol, dioxane glycol, adamantanediol, 3-methyl-1,5-pentanediol, methyloctanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 2-methylpropanediol 1,3, 3-methylpentanediol 1,5, hexamethylene glycol, and the like. Examples of the polyether polyol include ethylene glycol, octylene glycol, 9-nonanediol, 2,4-diethyl-1,5-pentanediol, ethylene oxide modified compounds of bifunctional phenols such as bisphenol A, propylene oxide modified compounds of bifunctional phenols such as bisphenol A, ethylene oxide and propylene oxide copolymer modified compounds of bisphenol A, copolymer polyether polyols of ethylene oxide and propylene oxide, polycarbonate diols, adamantane diols, polyether diols, polyester diols, polycaprolactone diols, etc. These may be used alone or in combination of two or more.

[0038] The alkyd resin can be prepared by adding a small amount of a solvent such as xylene to a reaction vessel containing the acid component and polyhydric alcohol, heating the vessel while injecting an inert gas such as nitrogen gas, and removing the water by azeotropy with the condensed water. Alternatively, an alkyd resin that provides a highly crosslinked and tough cured coating can be obtained by carrying out a condensation polymerization reaction of the acid component and polyhydric alcohol as the first step, and a condensation polymerization using a polybasic acid having three or more functional groups such as trimellitic acid as the second step. The reaction temperature can be about 170 to 250°C, and the reaction time can be about 5 to 25 hours, but is not particularly limited. The end of the reaction can be determined by monitoring the acid value of the reaction mixture as the reaction time elapses. That is, the reaction can be completed when the decrease in the acid value of the reaction mixture accompanying the condensation polymerization stops. The condensation polymerization reaction can be carried out in a shorter time by distilling the water generated by the condensation polymerization out of the system or by using a reaction catalyst. Examples of the reaction catalyst include tetrabutyl zirconate, monobutyltin oxide, zirconium naphthate, and tetrabutyl titanate.

[0039] The weight average molecular weight of the alkyd resin is preferably 10,000 or less, more preferably 7,000 or less, and even more preferably 5,000 or less.

[0040] The content of the alkyd resin in the ink composition is preferably from 10 to 40 mass % relative to the entire composition, and more preferably from 10 to 35 mass % relative to the entire composition.

[0041] In addition to the above-mentioned rosin-modified resin or alkyd resin, the ink composition of the present invention can also contain resins that have been used in the preparation of conventional ink compositions for metal printing. That is, known resins that are compatible with the above-mentioned rosin-modified resin or alkyd resin can be used alone or in combination depending on the required performance such as printability and coating film properties. Examples of such resins include polyester resins, petroleum resins, epoxy resins, ketone resins, amino resins, and benzoguanamine resins.

[0042] [solvent] The solvent used in the ink composition of the present invention is a solvent that has been used in the field of ink for metal printing. Examples of such solvents include, without particular limitation, those that have been used. Examples of such solvents include aliphatic hydrocarbons, alicyclic hydrocarbons, alkylbenzenes, polyalkylene glycols, etc., each having a boiling point range of about 230 to 400°C. Among these, preferred examples include those selected from the group consisting of compounds represented by the following general formula (1). Hereinafter, the solvent selected from the group consisting of compounds represented by the following general formula (1) is also referred to as a specific solvent.

[0043] [ka]

[0044] In the above general formula (1), each A is independently determined and is an alkylene group having 2 to 4 carbon atoms which may have a branch. Examples of such an alkylene group include an ethylene group [-(CH2)2-], a propylene group [-CH2(CH3)-CH2- or -CH2CH2(CH3)-], a trimethylene group [-(CH2)3-], and an isopropylidene group [-C(CH3)2-].

[0045] In the above general formula (1), R is an alkyl group having 1 to 13 carbon atoms, which may have a branched and / or cyclic structure. This alkyl group may be not only an aliphatic group but also an alicyclic group. Examples of such an alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a hexyl group, a 2-ethylhexyl group, an octyl group, a decyl group, and a cyclohexyl group.

[0046] In the above general formula (1), n ​​is an integer of 2 to 8. When n is 2 or more, a sufficient boiling point of the specific solvent can be secured to provide stability to the ink composition on a printing machine, which is preferable, and when n is 8 or less, a viscosity suitable for the solvent of the ink composition can be achieved.

[0047] Examples of the compound represented by the above general formula (1) include dipropylene glycol monomethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monooctyl ether, dipropylene glycol tridecyl ether, tripropylene glycol monobutyl ether, tripropylene glycol monodecyl ether, tetrapropylene glycol monohexyl ether, pentapropylene glycol monobutyl ether, and hexapropylene glycol monomethyl ether.

[0048] The content of the solvent in the ink composition of the present invention is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, based on the entire composition. Among the solvents, the content of the specific solvent is preferably 5% by mass or more based on the entire composition, which is preferable because it can increase the compatibility of the rosin-modified resin in the ink composition and can effectively suppress repelling when a water-based OP varnish is applied wet-on-wet after printing.

[0049] Here, the above-mentioned rosin-modified resin is preferably one that gives a dissolved varnish with an n-hexane tolerance of more than 50 g / 5 g when 70 g of the resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130° C. by stirring for 60 minutes. Since the measurement of n-tolerance is not particularly time-consuming as described later, this selection process does not require excessive trial and error. By using a rosin-modified resin that satisfies these conditions, the compatibility of the rosin-modified resin in the ink composition can be improved, and the transferability of the ink composition during printing can be further improved. Moreover, the above-mentioned tripropylene glycol monobutyl ether is an ether of tripropylene glycol and butanol formed by polymerization of three molecules of propylene oxide, and is one of the specific solvents in the present invention.

[0050] Next, the method for measuring the n-hexane tolerance of a resin in the present invention will be described. First, 70 g of the rosin-modified resin to be measured is prepared, and this is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130° C. by stirring for 60 minutes to prepare a dissolved varnish. The obtained dissolved varnish is allowed to cool to room temperature, and then 5 g is collected in a beaker. While maintaining the liquid temperature in the beaker at 25° C., n-hexane is added to the dissolved varnish in the beaker little by little while stirring, and the mass (g) of n-hexane required until the liquid in the beaker starts to become cloudy is obtained. The mass (g) of n-hexane obtained is the n-hexane tolerance (g / 5g). This measurement is so sensitive that the solution immediately begins to become cloudy when only one drop of n-hexane is added to the solution just before it becomes cloudy, so measurement errors due to the difference in judgment of cloudiness caused by differences in the measurer are not particularly problematic.

[0051] [Coloring pigments] The color pigment is a component for imparting coloring power to the ink composition. Examples of the color pigment include, without particular limitation, organic and / or inorganic pigments that have been conventionally used in printing ink compositions.

[0052] Examples of such color pigments include yellow pigments such as disazo yellow (pigment yellow 12, pigment yellow 13, pigment yellow 17, pigment yellow 1) and Hansa Yellow, magenta pigments such as brilliant carmine 6B, lake red C, and watching red, cyan pigments such as phthalocyanine blue, phthalocyanine green, and alkali blue, black pigments such as carbon black, white pigments such as titanium oxide, and fluorescent pigments. Metal powder pigments for imparting metallic colors such as gold and silver to the ink composition are also treated as color pigments in the present invention. Examples of such metal powder pigments include gold powder, bronze powder, aluminum paste obtained by processing aluminum powder into a paste, and mica powder.

[0053] The amount of the color pigment added is, for example, about 5 to 50% by mass relative to the entire ink composition, but is not particularly limited. When preparing a yellow ink composition using a yellow pigment, a magenta ink composition using a magenta pigment, a cyan ink composition using a cyan pigment, or a black ink composition using a black pigment, it is also possible to use a pigment of another color in combination or add an ink composition of another color as a complementary color.

[0054] [Other ingredients] To the ink composition of the present invention, known curing agents, pigment dispersants, waxes, silica particles, stabilizers and the like can be added as other components, if necessary.

[0055] As the curing agent, for example, an amino resin such as a melamine resin or a benzoguanamine resin can be used.

[0056] Silica particles are commercially available as SiO2 powder, and are easily available in the form of hydrophilic particles that have not been surface-treated or that have been hydrophilized, or hydrophobic particles that have been hydrophobized. Among these silica particles, hydrophilic silica particles are preferably used in the ink composition of the present invention. By using hydrophilic silica particles, the transferability of the ink composition during printing can be improved, and the fluidity of the ink composition can be increased, which is preferable. The content of silica particles in the ink composition is preferably 0.5 to 15% by mass, and more preferably 5 to 10% by mass.

[0057] The ink composition of the present invention can be prepared by mixing the various components, such as the color pigment, resin, and solvent containing the specific solvent, in a conventional manner using a roll mill, ball mill, bead mill, etc. The viscosity of the ink composition can be, for example, 10 to 70 Pa s at 25°C measured with a Raleigh viscometer, but is not particularly limited.

[0058] The metal for use in metal printing in the ink composition of the present invention is not particularly limited, but examples thereof include galvanized or tinned iron plate, aluminum plate, and metal cans made of these metal materials.

[0059] As the aqueous OP varnish to be applied onto the printed ink composition, any commonly used one can be used, and specific examples thereof include those using an aqueous acrylic resin, an aqueous polyester resin, an aqueous alkyd resin, an aqueous epoxy resin, or a modified resin of two or more of these as a binder in combination with an amino resin as a curing agent.

[0060] When printing on the surface of a metal material using the ink composition and aqueous OP varnish, first, printing is performed using the ink composition of the present invention with a dry offset printing machine, offset printing machine, or the like, and then, while the ink composition is still in a wet state (wet-on-wet), the aqueous OP varnish is overcoated with a coater or the like, and then baking is performed at 150 to 280°C for a few seconds to a few minutes. EXAMPLES

[0061] The ink composition of the present invention will be explained in more detail below by showing examples, but the present invention is not limited to the following examples in any way.

[0062] [Synthesis of alkyd resin 1] 5.98 parts by mass of neopentyl glycol, 8.53 parts by mass of pentaerythritol, 11.00 parts by mass of coconut oil fatty acid, 7.30 parts by mass of isophthalic acid, and 6.50 parts by mass of phthalic anhydride were reacted at 220°C under a nitrogen atmosphere until the acid value of the mixture reached 7mgKOH / g to perform the first stage of esterification, and then 0.70 parts by mass of trimellitic anhydride was added and heated at 165°C for 30 minutes under a nitrogen atmosphere to perform the second stage of esterification. These esterification reactions were carried out according to a conventional method to obtain an alkyd resin with a weight average molecular weight of 4450 and a number average molecular weight of 2007. 15.0 parts by mass of tripropylene glycol monobutyl ether (which corresponds to the above-mentioned specific solvent) was added to this alkyd resin to obtain alkyd resin varnish 1.

[0063] [Synthesis of alkyd resin 2] 5.98 parts by mass of neopentyl glycol, 8.53 parts by mass of pentaerythritol, 10.10 parts by mass of coconut oil fatty acid, 11.95 parts by mass of isophthalic acid, and 2.48 parts by mass of terephthalic acid were reacted at 220 ° C. under a nitrogen atmosphere until the acid value of the mixture reached 7 mg KOH / g to perform the first stage esterification, and then 0.70 parts by mass of trimellitic anhydride was added and heated at 165 ° C. for 30 minutes under a nitrogen atmosphere to perform the second stage esterification. These esterification reactions were carried out according to a conventional method to obtain an alkyd resin with a weight average molecular weight of 15303 and a number average molecular weight of 1454. 21.8 parts by mass of tripropylene glycol monobutyl ether and 2.0 parts by mass of triethanolamine were added to this alkyd resin to obtain alkyd resin varnish 2.

[0064] [Preparation of rosin-modified resin varnish] 63.2 parts by mass of rosin ester resin (hydroxyl value 20-30 mgKOH / g, acid value <10 mgKOH / g, weight average molecular weight 632, number average molecular weight 565) and 35.9 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, to obtain a rosin modified resin varnish. This rosin modified resin varnish is a dissolved varnish containing rosin ester resin (hydroxyl value 20-30 mgKOH / g). The n-hexane tolerance of the rosin ester resin used in the preparation of the rosin modified resin varnish was determined according to the procedure specified in the present invention, and was found to be 50 <g / 5gだった。

[0065] [Examples 1 to 3, Comparative Examples 1 to 2] Each ink composition of Examples 1 to 3 and Comparative Examples 1 and 2 was prepared by mixing each component according to the formulation in Table 1 and kneading the resulting mixture with a three-roll mill. In Table 1, "white pigment" is titanium oxide, "hydrophilic silica" is surface-untreated silica particles (manufactured by Tokuyama Corporation, product name Reolosil CP102), "clay" is organophilic bentonite (manufactured by BYK, product name CRAYTONE-APA), and "solvent" is tripropylene glycol monobutyl ether. The numerical values ​​of each blend amount in Table 1 mean parts by mass.

[0066] [Metastatic] The ink compositions of Examples 1 to 3 and Comparative Examples 1 to 2 were evaluated for transferability by the following procedure. First, 0.15 cc of the ink composition was spread on a blanket (Airtack FS, Kinyosha Co., Ltd.) using a 4-split roll of an RI tester (Akira Manufacturing Co., Ltd.), and left for 10 or 20 minutes. After that, an aluminum plate to be printed was attached to the spread blanket, and when pressure was applied, whether the spread ink composition was transferred to the aluminum plate and the degree of transfer was visually judged to evaluate the transferability of the ink composition. The evaluation criteria were as follows, and the results are shown in the "Transferability Evaluation" column in Table 1. ○: Good transfer even after leaving for 20 minutes △~◯: When left for 20 minutes, the transfer was slightly insufficient, but when left for 10 minutes, the transfer was good. △: No transfer when left for 20 minutes, but good transfer when left for 10 minutes ×: No transfer even after leaving for 10 minutes

[0067] [Whiteness] For each of the ink compositions of Examples 1 to 3 and Comparative Examples 1 and 2, 0.1 cc of the ink composition was spread on an aluminum plate using a 4-split roll of an RI tester (manufactured by Mei Seisakusho Co., Ltd.), and the resulting spread piece was heated at 200°C for 2 minutes in an electric oven by applying a water-based OP varnish onto the coating film. The spread piece was then returned to room temperature, and the whiteness was measured using eXact Advance (manufactured by X-Rite Inc.). The whiteness thus determined is shown in the "Whiteness" column of Table 1.

[0068] [Table 1]

[0069] Comparing the ink compositions of Examples 1 to 3 with the ink compositions of Comparative Examples 1 and 2, it can be seen that by containing the ink compositions containing the alkyd resin and rosin-modified resin specified in the present invention, the transferability of the ink composition can be improved and the whiteness of the white ink can be improved.

Claims

1. An ink composition for metal printing comprising a color pigment, a rosin-modified resin, an alkyd resin and a solvent, 1. An ink composition for metal printing, wherein the alkyd resin has a phthalic acid skeleton in its molecule.

2. 2. The ink composition for metal printing according to claim 1, wherein the alkyd resin has an oil length of 20 to 50 mass %.

3. 2. The ink composition for metal printing according to claim 1, wherein the weight average molecular weight of the alkyd resin is 10,000 or less.

4. 2. The ink composition for metal printing according to claim 1, wherein the rosin-modified resin has a hydroxyl value of 10 mgKOH / g or more.

5. 2. The ink composition for metal printing according to claim 1, characterized in that the solvent contains at least one compound selected from the group consisting of compounds represented by the following general formula (1): 【Chemistry 1】 (In the above general formula (1), each A is independently an alkylene group having 2 to 4 carbon atoms which may have a branch, R is an alkyl group having 1 to 13 carbon atoms which may have a branched and / or cyclic structure, and n is an integer of 2 to 8.)

6. 2. The ink composition for metal printing according to claim 1, wherein the rosin-modified resin is a rosin ester resin.

Citation Information

Patent Citations

  • Printing ink for metal

    JP1989060670A

  • Automatic register method for parts data base

    JP1993040791A

  • Electronic card arranging book

    JP1993040792A

  • Semiconductor device

    JP1993075031A

  • Printing ink composition for seamless can

    JP2009249435A