Low-carbon emission ore-molded product material, method for producing the same, and equipment containing low-carbon emission ore-molded product

A low carbon emission ore molding material, using silicates and aggregates, is cast at room temperature to address energy-intensive metal casting emissions, achieving reduced carbon footprints and superior mechanical properties.

JP2024159403AActive Publication Date: 2024-11-08WINSON MASCH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023140249
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-08-30
Publication Date
2024-11-08
Estimated Expiration
2043-08-30

AI Technical Summary

Technical Problem

Conventional metal casting methods produce significant carbon emissions due to the energy-intensive process of heating metals to a molten state, which is inconsistent with environmental protection trends.

Method used

A low carbon emission ore molding material composed of a binder, first aggregate with a particle diameter of 15 mm or less, and additives, which can be cast at room temperature without heating, using silicates, aluminates, or iron aluminates as binders, and aggregates like gabbro and sandy materials.

Benefits of technology

The method reduces carbon emissions by eliminating the need for heating, saves energy, and produces moldings with excellent mechanical properties and low thermal conductivity, suitable for applications requiring heat insulation and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159403000001_ABST
    Figure 2024159403000001_ABST
Patent Text Reader

Abstract

To provide a low-carbon emission ore-molded product material, a method for producing the same, and equipment containing a low-carbon emission ore-molded product.SOLUTION: A low-carbon emission ore-molded product material includes a binder, a primary aggregate, and an additive. The binder includes one or more of a silicate, an aluminate, or an iron aluminate. The primary aggregate has a primary particle diameter of 15 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to low carbon emission ore molding materials and methods for their manufacture and equipment containing low carbon emission ore moldings. [Background technology]

[0002] Generally, casting technology for industrial parts mainly involves heating metals, but in the current trend of environmental protection, this manufacturing method emits a large amount of carbon dioxide and brings a large carbon footprint to the product.

[0003] Furthermore, traditional metal casting methods require molten metal to be poured into a mold and cooled to solidify before forming a casting, however, those skilled in the art will appreciate that heating metal to a molten state requires the consumption of large amounts of energy, resulting in increased carbon emissions.

[0004] Furthermore, the production of metal materials, such as smelting, requires a large amount of carbon emissions, so that each step in the production process of casting products generates a large amount of carbon emissions, which is very inconsistent with the current trend of environmental protection. Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, there is a need for low carbon emission ore molding materials and methods of making same to overcome the known problems discussed above. [Means for solving the problem]

[0006] In accordance with the above objectives, the present invention provides a low carbon emission ore molding material comprising a binder, a first aggregate and an additive, the binder comprising one or more of a silicate, an aluminate or an iron aluminate, and the first aggregate having a first particle size of 15 mm or less.

[0007] Preferably, in one embodiment, the first particle size of the first aggregate is between 3 mm and 5 mm.

[0008] Preferably, in one embodiment, the first aggregate is an air-dried hard stone material, which is air-dried, dust-free, and angular.

[0009] Preferably, in one embodiment, the first aggregate is one or more of gabbro, granite, basalt, andesite, conglomerate, sandstone, shale, diabase, pyroxene, and quartz.

[0010] Preferably, in one embodiment, the composition further comprises a second aggregate, the second aggregate having a second particle size of less than 3 mm.

[0011] Preferably, in one embodiment, the second aggregate is an air-dried, dust-free, angular, sandy material.

[0012] Preferably, in one embodiment, the silicate is one or more of tricalcium silicate, dicalcium silicate, the aluminate is tricalcium aluminate, and the iron aluminate is tetracalcium iron aluminate.

[0013] Preferably, the additives include cement modifiers and shrinkage reducing agents for concrete.

[0014] Preferably, in one embodiment, the thermal conductivity of the low carbon emission ore molding material is 2 to 7 W·m -1 K -1 and the specific heat capacity is 0.7 to 1.5 kJ kg -1 K -1 and the linear thermal expansion coefficient is 5 to 15 × 10 -6 / K, compressive strength greater than 125 MPa, flexural strength greater than 15 MPa, Young's modulus greater than 40000 MPa, and density 2-3 g cm -3 It is.

[0015] Based on the above object, the present invention further provides a method for manufacturing a low-carbon discharge ore molding material, including: crushing raw ore to form a plurality of crushed raw ore; screening the plurality of crushed raw ore according to a first particle size to obtain a first aggregate; and mixing the first aggregate, a binder, an additive and water to form a low-carbon discharge ore molding material. The binder includes tricalcium silicate, dicalcium silicate, tricalcium aluminate and tetracalcium aluminoferrite. The first particle size of the first aggregate is 15mm or less, and the low-carbon discharge ore molding material can be poured at room temperature, and is filled into a mold under gravity flow, and then solidified to form a low-carbon discharge ore molding.

[0016] Based on the above objective, the present invention further provides a low-carbon emission ore molding-containing apparatus, including a low-carbon emission ore molding and a working machine. The low-carbon emission ore molding is made of the low-carbon emission ore molding material of any of the above-mentioned embodiments. The working machine is connected to the low-carbon emission ore molding. Effect of the Invention

[0017] The present invention provides a low-carbon ore molding material and a manufacturing method thereof. The processing of ores can obviously reduce carbon emissions compared to the manufacturing of metal materials, so it is economical and environmentally friendly. In addition, the low-carbon ore molding material of the present invention does not need to be heated to a molten state during the molding process, so it is possible to further save energy and effectively reduce the carbon emissions of the final product. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a first schematic diagram of a low carbon emission ore molding material according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a second schematic diagram of a low carbon emission ore molding material according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a comparison diagram of material properties between the low carbon emission ore molding material according to the embodiment of the present invention and other materials. [Figure 4]FIG. 4 is a schematic diagram of an apparatus including low carbon emission ore moldings according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In order to allow the examiner to understand the technical features, contents and advantages of the present invention, as well as the effects that can be achieved by them, the present invention will be described in detail as follows in the form of an embodiment with reference to the drawings. However, the drawings used therein are only for the purpose of schematic and auxiliary explanation, and may not necessarily represent the true proportion and accurate layout of the present invention after it is implemented. Therefore, the proportion and layout relationship of the attached drawings should not be used to interpret or limit the scope of rights in the actual implementation of the present invention, which is explained in advance here.

[0020] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In order to facilitate understanding, the same elements in the following embodiments will be denoted by the same reference numerals.

[0021] As shown in Fig. 1, the low carbon emission ore molding material of the present invention includes a binder 11, a first aggregate 12, and an additive 14. Furthermore, after the binder 11, the first aggregate 12, and the additive 14 are mixed and stirred, the low carbon emission ore molding material of the present invention can be injected into a mold and solidified without heating to form a molding, which can be used in particular for moldings such as bases, beds, cross beams, columns, axle heads, fuselages, and tables of machine tools or other equipment.

[0022] Additionally, the binder 11 can include one or more of a silicate, an aluminate, or a ferroaluminate. In some examples, the silicate can be one or more of tricalcium silicate, dicalcium silicate, the aluminate can be tricalcium aluminate, and the ferroaluminate can be tetracalcium aluminate, but is not limited thereto.

[0023] In a preferred embodiment, the binder 11 may include silicates, aluminates, and ferroaluminates, where the silicates may be tricalcium silicate and dicalcium silicate, the aluminates may be tricalcium aluminate, and the ferroaluminates may be tetracalcium aluminate.

[0024] Furthermore, the first particle size of the first aggregate 12 is 15mm or less, and in one embodiment, in order to further strengthen the structure, the low carbon emission ore molding material of the present invention may further include a second aggregate 13, and the second particle size of the second aggregate 13 is smaller than the first particle size of the first aggregate 12. That is, since the particle sizes of the first aggregate 12 and the second aggregate 13 in the low carbon emission ore molding material of the present invention are both small, the different particle sizes of the constituent materials of the low carbon emission ore molding material of the present invention can form close packing in an optimal ratio, and the molding formed later has excellent physical and mechanical properties.

[0025] In one embodiment, the first particle size of the first aggregate 12 is 5 mm to 12 mm, and may be, for example, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, or 12 mm, or any particle size within these ranges, but is not limited thereto. In one embodiment, the particle size of the first aggregate 12 is preferably 5 mm to 10 mm.

[0026] Furthermore, in another embodiment, the first aggregate 12 is an air-dried hard stone material, and the first aggregate 12 is one or more of gabbro, granite, basalt, andesite, conglomerate, sandstone, shale, diabase, pyroxene, and quartz. In other words, the first aggregate 12 made of one or more types of hard stone material can be selected.

[0027] In one embodiment, the first aggregate 12 may be naturally dried or air-dried in other ways. In another embodiment, the first aggregate 12 is a dust-free, angular hard stone. That is, in the present invention, the first aggregate 12 can be obtained by only passing through a flow of drying, crushing, dust removal, washing, particle size sorting (the order can be adjusted according to actual needs, but is not limited thereto). The shape of the first aggregate 12 is not limited, so the processing process of the aggregate shape can be omitted.

[0028] In one embodiment, the second particle size of the second aggregate 13 is less than 3 mm, and may be, for example, 1 mm, 2 mm, 3 mm, or any particle size between 0 mm and 3 mm. Preferably, the second aggregate 13 may be an air-dried, dust-free, angular sandy material. Furthermore, in one embodiment, the second aggregate 13 may be natural sand or artificial sand whose main material is silica.

[0029] In other embodiments, the second aggregate 13 may include other materials, for example, the second aggregate 13 may include one or more of slag, sea sand, and coral gravel, that is, one or more of slag, sea sand, and coral gravel may replace some or all of the silica-based sandy material.

[0030] In one embodiment, the additive 14 may include one or more of a cement modifier and a shrinkage reducing agent for concrete. For example, the cement modifier may be a high performance water reducing agent, and the shrinkage reducing agent for concrete may be a magnesium oxide expanding agent, a high performance concrete expanding agent, and the like.

[0031] In one embodiment, the content of the first aggregate 12 and the second aggregate 13 in the low carbon emission ore molded material is 0-80% by weight. Preferably, the low carbon emission ore molded material of the present invention may be calculated in terms of weight percentage, with the binder 11 being 35-45% by weight, the first aggregate 12 and the second aggregate 13 being 35-45% by weight, the water being 5-12% by weight, and the additive being 2-8% by weight. Furthermore, in a preferred embodiment, the first aggregate 12 and the second aggregate 13 may be approximately 50% by weight.

[0032] The present invention relates to comminuting the ore feedstock to form a plurality of comminuted ore feedstocks; sorting the plurality of crushed raw ore materials based on a first particle size to obtain a first aggregate (12); De-dusting and cleaning the first aggregate 12; Providing a second aggregate 13; A step of de-dusting and purifying the second aggregate 13; mixing the first aggregate 12, the second aggregate 13, the binder 11, the additive 14 and water to form the low carbon emission ore molded material.

[0033] The low carbon emission ore molding material is then injected into a mold to form a molding. Furthermore, since the low carbon emission ore molding material of the present invention does not contain a resin material such as an epoxy resin, it may have excellent fluidity, at least higher than molding materials containing a resin material. The low carbon emission ore molding material of the present invention has excellent fluidity, and its performance is sufficient to fill every corner of the mold before solidification. That is, the low carbon emission ore molding material of the present invention can be cast at room temperature (e.g., -5°C to 50°C, preferably 15°C to 35°C, more preferably 20°C to 30°C), and after filling the mold under gravity flow, it is solidified to form a low carbon emission ore molding. Therefore, the material can be smoothly and reliably filled in the mold without the need for a vibration device or other external force means. It should also be noted that the low carbon emission ore molding material of the present invention can also be cast at extremely low room temperature below 0°C.

[0034] In another embodiment, in the production of the low carbon emission ore molding material of the present invention, the second aggregate 13 may not be used, and only the first aggregate 12 made of ore may be used as the main aggregate of the molding.

[0035] In this embodiment, the binder may include tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium aluminate, silica fume, and other materials that may provide added strength and durability. In a preferred embodiment, the tricalcium silicate, dicalcium silicate, tricalcium aluminate, and tetracalcium aluminate comprise about 50% by weight of the binder.

[0036] In one embodiment, as shown in FIG. 2, the other material capable of increasing the strength and durability may be reinforcing fiber 15, steel fiber, HPP fiber, plastic fiber (polyethylene, polypropylene), etc. The length may be 3 mm to 10 mm, preferably 4 to 6 mm. In one embodiment, the content of reinforcing fiber 15 is less than 1 weight % in the binder. In addition, since the low carbon emission ore molding material of the present invention has low thermal conductivity, even if plastic fiber or other reinforcing fiber 15 that is weak in high temperature resistance is added, the characteristics of the reinforcing fiber 15 are not easily affected by high temperature. In another embodiment, the other material capable of increasing the strength and durability, such as reinforcing fiber 15, may be omitted, and for example, a binder 11 containing only mineral components is used.

[0037] In addition, in a preferred embodiment, tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium ferroaluminate, and silica fume (quartz powder) are all nano-sized powders, so that a dense structure is formed.

[0038] In addition, silica fume, in the process of formation, due to the action of surface tension in the formation process of phase change, becomes amorphous phase under the action of surface tension, and the surface becomes smooth. Part of silica fume is an aggregate of multiple spherical particles attached together. Silica fume is a material with very high surface area and high activity. Silica fume has a fineness of less than 1000 nanometers, an average particle size of 100-300 nanometers, and a particle size of 20-28 m. 2 / g. Its fineness and specific surface area are about 80-100 times that of cement and about 50-70 times that of fly ash, so it is very suitable for bonding other substrates.

[0039] In a preferred embodiment, the silica fume is mostly silica powder, and has a particle size of 7 nanometers to 40 nanometers, such as 10 nanometers to 20 nanometers, which is advantageous for forming a dense structure. In other embodiments, the silica powder may have other particle sizes less than 300 nanometers. In a preferred embodiment, the silica fume may be composed of one or more of the following by weight percentage: 75% to 98% silica, 1.0±0.2% alumina, 0.9±0.3% iron trioxide, 0.7±0.1% magnesium oxide, 0.3±0.1% calcium oxide, and 1.3±0.2% Na2O. The bulk density is about 320 to 700 kg / m 3 It is.

[0040] In one embodiment, when silica fume reacts with silicate, a hydration reaction occurs to produce hydrated calcium silicate and calcium hydroxide. The hydrated calcium silicate may have the effect of binding other substances. Silica fume, calcium hydroxide and water can further react to produce more calcium silicate gel polymer, and the content of calcium hydroxide decreases, which can be shown by the following chemical reaction:

[0041] Calcium hydroxide + silica fume + water → calcium silicate hydrate Ca(OH)2 + SiO2 + H2O → CSH

[0042] The calcium silicate gel polymer helps to increase matrix adhesion and reduce permeability within the casting, and since calcium hydroxide is reduced in the reaction, it can also improve the durability of the overall structure.

[0043] In summary, silica fume particles are so small that it can be used as a filler and gel material, it can fill the gaps between particles of various substrates, especially between aggregates, and silica fume can also bond with calcium hydroxide, making the structure of the moldings denser, more robust and less permeable.

[0044] In one embodiment, the components of the binder 11 further include calcium oxide. The particle size of the finely divided calcium oxide in the calcium oxide may be 0.7 to 100 microns, preferably 20 to 80 microns. The finely divided calcium oxide accounts for 90% to 99% by weight of the calcium oxide.

[0045] In one embodiment, the binder 11 includes cement, silica, and calcium oxide. The cement includes ordinary cement and ultrafine cement. The particle size of the ultrafine cement is 2 to 20 microns, and the weight percentage of the ordinary cement to the ultrafine cement is 3:1 to 5:1.

[0046] In one embodiment, the silica may have two forms, which are fumed silica and precipitated silica, respectively, and the ratio of the weight percentage of both may be 1:1 to 1:50.

[0047] In one embodiment, the cement may include one or more of blast furnace slag, fly ash, silicon powder, pozzolan, calcium carbonate, silica, aluminum oxide (e.g., aluminum oxide), iron oxide (e.g., ferric oxide), and gypsum. Furthermore, the low carbon emission ore molding material of the present invention has excellent bleeding resistance and water absorption properties, and the water absorption properties are determined by factors such as the aggregate mixing ratio, the water-binder ratio, and the material components. The low carbon emission ore molding material of the present invention has a very low water absorption rate of less than about 0.1%. This is because the above-mentioned fine aggregate and powder materials make the microstructure of the molding more dense. In addition, the low carbon emission ore molding material of the present invention usually contains a high-performance water reducer and other additives to improve the fluidity and operating performance, which helps to reduce the water absorption of the final molding. The molding made of the low carbon emission ore molding material of the present invention also has excellent bleeding resistance and can maintain high bleeding resistance under water pressure.

[0048] Furthermore, the molding made of the low carbon emission ore molding material of the present invention, which contains or consists of the above-mentioned material, has a thermal conductivity of 1 to 8 W m -1 K -1 and the specific heat capacity is 0.7 to 1.5 kJ kg-1 K -1 and the linear thermal expansion coefficient is 1 to 15 × 10 -6 / K, compressive strength greater than 125 MPa, flexural strength greater than 15 MPa, Young's modulus greater than 40000 MPa, and density 2-3 g cm -3 It is.

[0049] In addition, moldings made of low carbon emission ore molding materials can withstand high temperatures, at least 450°C, and maintain excellent mechanical and physical properties. Compared to moldings containing resin materials, for example materials containing epoxy resins, the temperature that can be withstood in the present invention is at least 200°C higher (generally, the maximum temperature range of epoxy resins is about 150°C).

[0050] As shown in FIG. 3, in one embodiment, the molding made of the low carbon emission ore molding material of the first embodiment has a thermal conductivity of 2 to 5 W m -1 K -1 For example, 3.0 W m -1 K -1 and the specific heat capacity is 0.8 to 2.0 kJ kg -1 K -1 For example, 1.2 kJ kg -1 K -1 and the linear thermal expansion coefficient is 8 to 15 × 10 -6 / K, for example 12×10 -6 / K, the compressive strength is greater than 125 MPa, the flexural strength is greater than 15 MPa, the Young's modulus is 45000 MPa, and the density is 1.8 to 3.3 g cm -3 For example, 2.5 g cm -3 The logarithmic decay rate may be 0.02 to 0.04, for example, 0.03, and the decay rate may be 0.4 to 0.6, for example, 0.5.

[0051] In another embodiment, a molding made of the low carbon emission ore molding material of the second embodiment has a thermal conductivity of 3 to 9 W m -1 K -1 For example, 6.0 W m-1 K -1 and the specific heat capacity is 0.5 to 1.6 kJ kg -1 K -1 For example, 0.85 kJ kg -1 K -1 and the linear thermal expansion coefficient is 5 to 15 × 10 -6 / K, e.g. 7×10 -6 / K, the compressive strength is greater than 150 MPa, the flexural strength is greater than 20 MPa, the Young's modulus is 80000 MPa, and the density is 1.8 to 3.3 g cm -3 For example, 2.8 g cm -3 The logarithmic decay rate may be 0.01 to 0.03, for example, 0.021, and the decay rate may be 0.2 to 0.5, for example, 0.33.

[0052] Furthermore, epoxy resin mineral moldings have a thermal conductivity of 2.9 to 3.0 W m -1 K -1 and the specific heat capacity is 0.7 to 0.9 kJ kg -1 K -1 and the linear thermal expansion coefficient is 15×10 -6 / K, compressive strength is 110-150 MPa, flexural strength is 30-35 MPa, Young's modulus is 38-45000 MPa, and density is 2.3-2.4 g cm -3 It is.

[0053] Furthermore, ordinary concrete has a thermal conductivity of 2 W m -1 K -1 and the specific heat capacity is 1 kJ kg -1 K -1 and the linear thermal expansion coefficient is 10~11×10 -6 / K, compressive strength is 5-55 MPa, flexural strength is 0-5 MPa, Young's modulus is 22000-35000 MPa, and density is 2.3 g cm -3 It is.

[0054] Furthermore, natural hard stone has a thermal conductivity of 1.7 W·m -1 K -1 and the specific heat capacity is 0.85 kJ kg-1 K -1 and the linear thermal expansion coefficient is 5.5 to 7.5 × 10 -6 / K, compressive strength is 280-360 MPa, flexural strength is 13-35 MPa, Young's modulus is 90000-120000 MPa, and density is 2.9-3.0 g cm -3 It is.

[0055] Furthermore, cast iron has a thermal conductivity of 29 to 54 W·m -1 K -1 and the specific heat capacity is 0.46 to 0.63 kJ kg -1 K -1 and the linear thermal expansion coefficient is 9.5 to 10.5 × 10 -6 / K, bending strength is 100-800 MPa, Young's modulus is 80-185000 MPa, and density is 7.2-7.4 g cm -3 , where the logarithmic decay rate is 0.003 and the decay rate is 0.05.

[0056] In addition, S235 series steel has a thermal conductivity of 50 W·m -1 K -1 and the specific heat capacity is 0.45 kJ kg -1 K -1 and the linear thermal expansion coefficient is 12×10 -6 / K, bending strength is 340-470MPa, Young's modulus is 210000MPa, and density is 7.8g cm -3 where the logarithmic decay rate is 0.001 and the decay rate is 0.02.

[0057] Furthermore, aluminum has a thermal conductivity of 130 to 220 W·m -1 K -1 and the specific heat capacity is 0.9 kJ kg -1 K -1 and the linear thermal expansion coefficient is 23 to 24 × 10 -6 / K, bending strength is 120-500MPa, Young's modulus is 70000MPa, and density is 2.7g cm -3 It is.

[0058] In addition, stainless steel has a thermal conductivity of 15 W·m -1K -1 and the specific heat capacity is 0.5 kJ kg -1 K -1 and the linear thermal expansion coefficient is 10~16×10 -6 / K.

[0059] Furthermore, the aluminum alloy has a logarithmic decrement of 0.01 to 0.15 and a decrement of 0.01 to 0.05.

[0060] From the above, it can be seen that the vibration damping performance of the molding made of the low carbon emission ore molding material of the present invention is about 10 times that of cast iron (gray cast iron), has a lower thermal conductivity than cast iron, has better heat resistance and Young's modulus than epoxy resin ore moldings, and has a low thermal expansion coefficient. In other words, the molding made of the low carbon emission ore molding material of the present invention has effects such as heat resistance, low thermal conductivity, low expansion coefficient, and high vibration damping performance.

[0061] In one embodiment, a molding made of the low carbon emission ore molding material of the present invention has a width of about 3 meters, a height of about 2 to 4 meters, and a length of about 4 meters, and therefore, at least the molding of this embodiment can have various effects of each of the above embodiments.

[0062] As shown in Figure 4, the present invention further provides a system 10 including a low carbon emission ore molding, the system including a low carbon emission ore molding 100 and a working machine 200. The low carbon emission ore molding 100 is made of the low carbon emission ore molding material in any of the above-mentioned embodiments, and a working machine 200 is connected to the low carbon emission ore molding.

[0063] Further, in one embodiment, the low carbon emission ore molding 100 may be a base, bed, cross beam, column, arbor, body, table, etc. of a machine tool or other equipment. The work machine 200 may be a work table or a work table, such as a three-axis work table, a five-axis work table, a cutter, a motor, etc.

[0064] Moldings made from the low-carbon emission ore molding material of the present invention have low thermal conductivity, sufficient compressive strength, bending strength and Young's modulus compared to other materials, particularly conventional cast iron and concrete, and are therefore suitable for equipment such as machine tools that require excellent insulation and impact resistance.

[0065] In addition to the above advantages, the moldings made of the low carbon emission ore molding material of the present invention have a lower density than cast iron and most metal materials, so the weight of the entire finished product can be significantly reduced. In other words, the moldings made of the low carbon emission ore molding material of the present invention not only have excellent mechanical properties, but also have the effect of reducing weight.

[0066] In summary, the present invention provides a low-carbon emission ore molding material and a manufacturing method thereof. The processing of ores can obviously reduce carbon emissions compared to the manufacturing of metal materials, so it is economical and environmentally friendly. In addition, the low-carbon emission ore molding material of the present invention does not need to be heated to a molten state during the molding process, so it can further save energy and effectively reduce the carbon emissions of the final product.

[0067] The above is merely illustrative and not limiting. Any equivalent modifications or variations made without departing from the spirit and scope of the present invention should be included in the appended claims. [Explanation of symbols]

[0068] 11 Binder 12 Primary aggregate 13 Secondary aggregate 14 Additives 15 Reinforced Fiber 10. Facilities that contain low carbon emission ore moldings 100 Low carbon emission ore moldings 200 Work Machine

Claims

1. 1. A low carbon emission ore molding material, comprising: a binder comprising one or more of a silicate, an aluminate, or an iron aluminate; A first aggregate having a first particle size of 15 mm or less; and an additive, The low carbon emission ore molding material is cast and solidified at room temperature to form a low carbon emission ore molding.

2. 2. The low carbon emission ore molding material according to claim 1, wherein the first particle size of the first aggregate is between 5 mm and 12 mm.

3. 3. The low carbon emission ore molding material of claim 2, wherein the first aggregate is one or more of gabbro, granite, basalt, andesite, conglomerate, sandstone, shale, diabase, pyroxene, and quartz.

4. 2. The low carbon emission ore molding material of claim 1, further comprising a second aggregate, the second aggregate having a second particle size of less than 3 mm and being a sandy material.

5. 2. The low carbon emission ore molding material of claim 1, wherein the first aggregate is an air-dried, dust-free, angular, hard stone material.

6. 2. The low carbon emission ore molding material of claim 1, wherein said silicate is one or more of tricalcium silicate, dicalcium silicate, said aluminate is tricalcium aluminate, and said ferroaluminate is tetracalcium aluminate.

7. 10. The low carbon emission ore molding material of claim 1, further comprising additives, said additives including cement modifiers and shrinkage reducing agents for concrete.

8. The moldings made of the low carbon emission ore molding material have a thermal conductivity of 2 to 7 W·m -1 K -1 and the specific heat capacity is 0.7 to 1.5 kJ kg -1 K -1 and the linear thermal expansion coefficient is 5 to 15×10 -6 / K, compressive strength is 125 MPa, bending strength is greater than 15 MPa, Young's modulus is greater than 40,000 MPa, and density is 2 to 3 g cm -3 2. The low carbon emission ore molding material of claim 1,

9. 1. A method for producing a low carbon emission ore molding material, comprising: comminuting the ore feedstock to form a plurality of comminuted ore feedstocks; sorting the plurality of crushed raw ore materials based on a first particle size to obtain a first aggregate; mixing the first aggregate, a binder, an additive, and water to form the low carbon emission ore molding material; The binder comprises tricalcium silicate, dicalcium silicate, tricalcium aluminate and tetracalcium aluminoferrite, the first aggregate has a first particle size of 15 mm or less, and the low-carbon emission ore molding material, when poured at room temperature, fills a mold under gravity flow and then solidifies to form a low-carbon emission ore molding.

10. 1. A system including low carbon emission ore moldings, comprising: A low carbon emission ore molding comprising the low carbon emission ore molding material according to claim 1; and a work machine coupled to the low carbon emission ore molds.

Citation Information

Patent Citations

  • Cementitious inductrial instrument

    JP1987119150A

  • Low environmental load type ultra high early strength concrete

    JP2001039758A

  • Concrete die for casting

    JP2002137043A

  • Method for producing high strength precast concrete

    JP2011195354A

  • Refractory cement composition

    JP2014076917A