Polyethylene resin composition, film, sheet, and solar cell sealing sheet
A polyethylene resin composition with ethylene-α-olefin copolymers and additives addresses the need for high heat resistance and transparency, particularly in solar cell encapsulants.
Patent Information
- Application Number
- JP2024059289
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-02
- Publication Date
- 2024-11-08
AI Technical Summary
There is a need for polyethylene resin compositions that offer high heat resistance and transparency for applications beyond traditional uses, particularly in encapsulants for solar cells.
A polyethylene resin composition containing 100 parts by mass of an ethylene polymer with a Vicat softening point of 50°C to 88°C and 0.01 to 0.4 parts by mass of a compound represented by structural formula (I), which includes ethylene-α-olefin copolymers and specific additives to enhance heat resistance and transparency.
The composition provides a polyethylene resin with improved heat resistance and transparency, suitable for use in solar cell encapsulants and other applications.
Smart Images

Figure 2024159538000001 
Figure 2024159538000002 
Figure 2024159538000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene resin composition, a film, a sheet, and a solar cell encapsulant sheet. [Background technology]
[0002] 2. Description of the Related Art Ethylene-based polymers have conventionally been used in food packaging materials, pharmaceutical packaging materials, electronic component packaging materials, surface protective materials, insulators and sheaths for electric wires and cables, and the like.
[0003] For example, Patent Document 1 describes an ethylene-α-olefin copolymer that is excellent in moldability and low smoke generation during melt processing, and describes the use of the ethylene-α-olefin copolymer as a food packaging material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-106264 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the use of ethylene-based polymers as encapsulants for solar cells has been considered. The encapsulant is required to have high heat resistance and high transparency, and the development of polyethylene resin compositions capable of forming such encapsulants has been promoted. In addition, high heat resistance and high transparency may also be required for applications other than encapsulants.
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polyethylene resin composition having relatively excellent heat resistance and transparency, and a film, a sheet, and a solar cell encapsulant sheet each using the polyethylene resin composition. [Means for solving the problem]
[0007] The polyethylene resin composition according to the present invention contains 100 parts by mass of an ethylene polymer having a Vicat softening point of 50° C. or more and 88° C. or less, and 0.01 part by mass or more and 0.4 part by mass or less of a compound represented by structural formula (I).
[0008] [ka]
[0009] [wherein n is 0, 1 or 2, A is a non-hydrogen group, and R 1 ~R 10 are each independently a hydrogen atom, a halogen atom, a phenyl group, an alkyl group, an alkenyl group, an alkoxy group, or an acyl group, and a hydrogen atom in the phenyl group, the alkyl group, the alkenyl group, the alkoxy group, and the acyl group may be substituted with a halogen atom, and any two adjacent groups may form a cyclic group.
[0010] The film or sheet according to the present invention comprises the above-mentioned polyethylene resin composition.
[0011] The solar cell encapsulant sheet according to the present invention contains the above-mentioned polyethylene resin composition. Effect of the Invention
[0012] According to the present invention, it is possible to provide a polyethylene resin composition having relatively excellent heat resistance and transparency, and a film, a sheet, and a solar cell encapsulant sheet each using the polyethylene resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. In addition, hereinafter, the "solar cell encapsulant sheet" may be simply referred to as the "encapsulant sheet".
[0014] [Polyethylene resin composition] The polyethylene resin composition according to the present embodiment contains an ethylene-based polymer and a compound represented by the following structural formula (I).
[0015] [ka]
[0016] [wherein n is 0, 1 or 2, A is a non-hydrogen group, and R 1 ~R 10 are each independently a hydrogen atom, a halogen atom, a phenyl group, an alkyl group, an alkenyl group, an alkoxy group, or an acyl group, and a hydrogen atom in the phenyl group, the alkyl group, the alkenyl group, the alkoxy group, and the acyl group may be substituted with a halogen atom, and any two adjacent groups may form a cyclic group.
[0017] <Ethylene-based polymer> The ethylene-based polymer is a polymer containing more than 50% by mass of monomer units based on ethylene. Examples of the ethylene-based polymer include ethylene-α-olefin copolymer, high-pressure low-density polyethylene (ethylene homopolymer), and ethylene-unsaturated ester copolymer. From the viewpoint of improving moisture resistance and flexibility, the ethylene-based polymer is preferably an ethylene-α-olefin copolymer. The above ethylene-based polymers may be used alone or in combination of two or more kinds.
[0018] The ethylene polymer according to the present embodiment has a Vicat softening point of 50°C or more and 88°C or less. From the viewpoint of improving heat resistance and flexibility, the Vicat softening point of the ethylene polymer is preferably 52°C or more and 87°C or less, more preferably 54°C or more and 86°C or less. The Vicat softening point can be adjusted by adjusting the content of monomer units based on α-olefin or unsaturated ester in the ethylene polymer. Specifically, the higher the content of monomer units based on α-olefin in the ethylene-α-olefin copolymer, the lower the Vicat softening point. The higher the content of monomer units based on unsaturated ester in the ethylene-unsaturated ester copolymer, the lower the Vicat softening point.
[0019] The Vicat softening point (unit: ° C.) of the ethylene polymer is measured by the following method.
[0020] (Method of measuring Vicat softening point (unit: °C)) A sample of an ethylene-based polymer is pressed by a hot press to form a sheet having a thickness of about 5 mm. The obtained sheet is measured according to the A50 method specified in JIS K7206-1999.
[0021] The melt flow rate (hereinafter sometimes referred to as "MFR") of the ethylene polymer is preferably 0.10 g / 10 min or more and 30.00 g / 10 min or less, more preferably 0.20 g / 10 min or more and 10.00 g / 10 min or less, from the viewpoint of improving extrusion processability. The MFR is measured using a sample of the ethylene polymer according to Method A specified in JIS K7210-1995, under conditions of a temperature of 190°C and a load of 2.16 kg.
[0022] The density of the ethylene polymer is preferably 940 kg / m from the viewpoint of increasing the mechanical strength of the extrusion molded product. 3 More preferably, it is 930 kg / m or less. 3 More preferably, it is 920 kg / m or less. 3 or less, and particularly preferably 910 kg / m 3From the viewpoint of improving the heat resistance of the extrusion molded product, the density of the ethylene polymer is preferably 880 kg / m 3 More preferably, it is 890 kg / m or more. 3 The density is measured according to the method specified in JIS K7112-1980.
[0023] In one embodiment, the density of the ethylene-based polymer is 880 kg / m 3 More than 910kg / m 3 The following is the result.
[0024] <Ethylene-α-olefin copolymer> The ethylene-α-olefin copolymer is an ethylene-α-olefin copolymer obtained by copolymerizing ethylene with an α-olefin having 3 to 20 carbon atoms. Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 4-methyl-1-pentene, 4-methyl-1-hexene, and the like, and preferably 1-butene, 1-hexene, 4-methyl-1-pentene, or 1-octene. The above α-olefin having 3 to 20 carbon atoms may be used alone or in combination of two or more.
[0025] The content of the ethylene-based monomer unit in the ethylene-α-olefin copolymer is preferably more than 50% by mass and not more than 99.5% by mass, based on the total mass (100% by mass) of the ethylene-α-olefin copolymer, from the viewpoint of achieving a higher conversion efficiency of the solar cell and more effectively preventing cracking of the solar cell element during sealing. The content of the ethylene-α-olefin-based monomer unit having 3 to 20 carbon atoms in the ethylene-α-olefin copolymer is preferably 0.5% by mass or more and less than 50% by mass, based on the total mass (100% by mass) of the ethylene-α-olefin copolymer. When the ethylene-α-olefin copolymer has monomer units based on two or more kinds of α-olefins, the content of the α-olefin-based monomer unit is the total amount of the monomer units based on each α-olefin in the ethylene-α-olefin copolymer. The content of the ethylene-based monomer unit and the content of the α-olefin-based monomer unit are measured by infrared spectroscopy (IR method).
[0026] Examples of the ethylene-α-olefin copolymer include ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-4-methyl-1-pentene copolymer, ethylene-1-octene copolymer, ethylene-1-butene-1-hexene copolymer, ethylene-1-butene-4-methyl-1-pentene copolymer, ethylene-1-butene-1-octene copolymer, ethylene-1-hexene-1-octene copolymer, etc., and preferably ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-4-methyl-1-pentene copolymer, ethylene-1-butene-1-hexene copolymer, ethylene-1-butene-1-octene copolymer, or ethylene-1-hexene-1-octene copolymer. These ethylene-α-olefin copolymers may be used alone or in combination of two or more.
[0027] The density of the ethylene-α-olefin copolymer is preferably 940 kg / m from the viewpoint of increasing the mechanical strength of the extrusion molded product. 3 More preferably, it is 930 kg / m or less. 3More preferably, it is 920 kg / m or less. 3 or less, and particularly preferably 910 kg / m 3 The density of the ethylene-α-olefin copolymer is preferably 880 kg / m or less from the viewpoint of improving the heat resistance of the extrusion molded product. 3 More preferably, it is 890 kg / m or more. 3 The density is measured according to Method A described in JIS K7112-1980. The density can be adjusted by adjusting the content of monomer units based on ethylene in the ethylene-α-olefin copolymer.
[0028] The melt flow rate of the ethylene-α-olefin copolymer is, for example, preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, from the viewpoint of reducing the extrusion load during the production of the encapsulating sheet. The melt flow rate of the ethylene-α-olefin copolymer is, for example, preferably 100 g / 10 min or less, more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and particularly preferably 10 g / 10 min or less, from the viewpoint of achieving higher mechanical strength of the encapsulating sheet. The MFR is measured by the method A specified in JIS K7210-1995 at a temperature of 190° C. and a load of 2.16 kg. The MFR can be adjusted, for example, by adjusting the hydrogen concentration or polymerization temperature during the production of the ethylene-α-olefin copolymer by polymerization, and the higher the hydrogen concentration and polymerization temperature, the higher the MFR of the ethylene-α-olefin copolymer.
[0029] In one embodiment, from the viewpoint of improving heat resistance, flexibility, and extrusion processability, the ethylene-α-olefin copolymer satisfies all of the following requirements (i) and (ii): (i) Vicat softening point is 50°C or higher and 85°C or lower. (ii) A melt flow rate of 0.10 g / 10 min or more and 30.00 g / 10 min or less.
[0030] Examples of methods for producing ethylene-α-olefin copolymers include a method of copolymerizing ethylene and an α-olefin in the presence of a polymerization catalyst that uses as catalyst components a solid particulate cocatalyst component (hereinafter sometimes referred to as "component (A)") in which a cocatalyst component such as an organoaluminum compound, an organoaluminum oxy compound, a boron compound, or an organozinc compound is supported on a particulate carrier, and a metallocene complex (hereinafter sometimes referred to as "component (B)") having a ligand having a structure in which two cyclopentadienyl-type anion skeletons are bonded via a bridging group such as an alkylene group or a silylene group.
[0031] Examples of the solid particulate promoter component include a component in which methylalumoxane is mixed with porous silica, and a component in which diethylzinc, water, and fluorinated phenol are mixed with porous silica.
[0032] A specific example of the solid particulate promoter component is a promoter support component (i) obtained by contacting component (a) diethylzinc, component (b) fluorinated phenol, component (c) water, component (d) porous silica, and component (e) trimethyldisilazane (((CH3)3Si)2NH).
[0033] Examples of the fluorinated phenol of component (b) include pentafluorophenol, 3,5-difluorophenol, 3,4,5-trifluorophenol, and 2,4,6-trifluorophenol. From the viewpoint of increasing the flow activation energy (Ea) and molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, it is preferable to use two types of fluorinated phenols having different numbers of fluorine atoms. In this case, the molar ratio of the phenol having a larger number of fluorine atoms to the phenol having a smaller number of fluorine atoms is usually 20 / 80 or more and 80 / 20 or less. The molar ratio is preferably 30 / 70 or more and 70 / 30 or less.
[0034] Regarding the amounts of the components (a), (b) and (c) used, when the molar ratio of the amounts of the components used is component (a):component (b):component (c)=1:y:z, it is preferable that y and z satisfy the following formula:
[0035] |2-y-2z|≦1 In the above formula, y is preferably a number of 0.01 or more and 1.99 or less, more preferably a number of 0.10 or more and 1.80 or less, even more preferably a number of 0.20 or more and 1.50 or less, and particularly preferably a number of 0.30 or more and 1.00 or less.
[0036] The amount of component (d) used relative to component (a) is preferably an amount such that the number of moles of zinc atoms contained in the particles obtained by contacting component (a) with component (d) is 0.1 mmol or more, more preferably 0.5 mmol or more and 20 mmol or less per 1 g of the particles. The amount of component (e) used relative to component (d) is preferably an amount such that the number of moles of component (e) is 0.1 mmol or more, more preferably 0.5 mmol or more and 20 mmol or less per 1 g of component (d).
[0037] Examples of the metallocene complex include a zirconocene complex in which two indenyl groups are bonded with an ethylene group, a dimethylmethylene group, or a dimethylsilylene group, a zirconocene complex in which two methylindenyl groups are bonded with an ethylene group, a dimethylmethylene group, or a dimethylsilylene group, a zirconocene complex in which two methylcyclopentadienyl groups are bonded with an ethylene group, a dimethylmethylene group, or a dimethylsilylene group, and a zirconocene complex in which two dimethylcyclopentadienyl groups are bonded with an ethylene group, a dimethylmethylene group, or a dimethylsilylene group. Examples of the metal atom of component (ii) include zirconium and hafnium, and examples of the remaining substituents that the metal atom has include a diphenoxy group and a dialkoxy group. Component (ii) is preferably ethylenebis(1-indenyl)zirconium diphenoxide.
[0038] In the polymerization catalyst using the above-mentioned solid particulate cocatalyst component and metallocene complex, an organoaluminum compound may be used in combination as a catalyst component, as appropriate. Examples of the organoaluminum compound include triisobutylaluminum and tri-normal-octylaluminum.
[0039] The amount of the metallocene complex used is preferably 5×10 -6 mol or more 5×10 -4 The amount of the organoaluminum compound used is preferably an amount such that the amount of aluminum atoms in the organoaluminum compound is 1 mol or more and 2000 mol or less per 1 mol of metal atoms in the metallocene complex.
[0040] In the polymerization catalyst using the above-mentioned solid particulate cocatalyst component and the metallocene complex, an electron donor compound may be used as a catalyst component. Examples of the electron donor compound include triethylamine and tri-n-octylamine.
[0041] When two types of fluorinated phenols having different numbers of fluorines are used as the fluorinated phenol of the above component (b), an electron donating compound is preferably used.
[0042] The amount of the electron donor compound used is usually 0.1 mol% or more and 10 mol% or less based on the number of moles of aluminum atoms in the organoaluminum compound used as the catalyst component. From the viewpoint of increasing the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, the amount used is preferably 0.2 mol% or more and 5 mol% or less based on the number of moles of aluminum atoms in the organoaluminum compound used as the catalyst component.
[0043] More specifically, the method for producing an ethylene-α-olefin copolymer includes a method of copolymerizing ethylene with an α-olefin having 3 to 20 carbon atoms in the presence of a catalyst obtained by contacting the cocatalyst support component (a), a crosslinked bisindenyl zirconium complex, and an organoaluminum compound.
[0044] The polymerization method may be, for example, a continuous polymerization method involving the formation of particles of an ethylene-α-olefin copolymer. The continuous polymerization method may be, for example, continuous gas phase polymerization, continuous slurry polymerization, or continuous bulk polymerization, with continuous gas phase polymerization being preferred. The gas phase polymerization reactor is usually an apparatus having a fluidized bed reactor, and is preferably an apparatus having a fluidized bed reactor with an enlarged section. The apparatus having a fluidized bed reactor may have an agitator installed in the reactor.
[0045] The method for supplying each component of the polymerization catalyst used in the production of ethylene-α-olefin copolymer to a reaction vessel usually includes a method of supplying the components in a moisture-free state using an inert gas such as nitrogen or argon, hydrogen, ethylene, etc., or a method of supplying each component in a solution or slurry state by dissolving or diluting it in a solvent. Each component of the polymerization catalyst may be supplied separately, or any component may be contacted in advance in any order and then supplied.
[0046] Also, a prepolymerization may be carried out before carrying out the main polymerization. The prepolymerized prepolymerization catalyst component is preferably used as a catalyst component or catalyst for the main polymerization. Different α-olefins may be used in the main polymerization and the prepolymerization. The α-olefin to be prepolymerized with ethylene is preferably an α-olefin having 4 to 12 carbon atoms, more preferably an α-olefin having 6 to 8 carbon atoms.
[0047] The polymerization temperature is usually lower than the temperature at which the ethylene-α-olefin copolymer melts, and is preferably from 0° C. to 150° C., more preferably from 30° C. to 100° C., and even more preferably from 50° C. to 90° C. In addition, from the viewpoint of broadening the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, the polymerization temperature is preferably from 60° C. to 85° C.
[0048] The polymerization time (average residence time in the case of a continuous polymerization reaction) is usually 1 hour or more and 20 hours or less. From the viewpoint of widening the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, the polymerization time (average residence time) is preferably 2 hours or more and 10 hours or less.
[0049] In addition, for the purpose of adjusting the melt fluidity of the ethylene-α-olefin copolymer, hydrogen may be added to the polymerization reaction gas as a molecular weight regulator, or an inert gas may be allowed to coexist in the polymerization reaction gas. The molar concentration of hydrogen in the polymerization reaction gas relative to the molar concentration of ethylene in the polymerization reaction gas is usually 0.1 mol% or more and 3 mol% or less, where the molar concentration of ethylene in the polymerization reaction gas is taken as 100 mol%. In addition, from the viewpoint of widening the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, the molar concentration of hydrogen in the polymerization reaction gas is preferably 0.2 mol% or more and 2.5 mol% or less, where the molar concentration of ethylene in the polymerization reaction gas is taken as 100 mol%.
[0050] <Ethylene homopolymer> The ethylene homopolymer is preferably an ethylene homopolymer obtained by polymerizing ethylene by a high-pressure method, for example, an ethylene homopolymer produced by polymerizing ethylene in the presence of a radical generator using a tank reactor or a tubular reactor at a polymerization pressure of 140 MPa or more and 300 MPa or less and a polymerization temperature of 200° C. or more and 300° C. or less.
[0051] The density of the ethylene homopolymer is preferably 920 kg / m from the viewpoint of improving heat resistance. 3 More preferably, 925 kg / m 3More preferably, it is 928 kg / m 3 The density of the ethylene homopolymer is preferably 935 kg / m from the viewpoint of improving transparency. 3 More preferably, it is 933 kg / m or less. 3 The density is measured according to the method A specified in JIS K7112-1980 after annealing as specified in JIS K6760-1995.
[0052] <Ethylene-unsaturated ester copolymer> The ethylene-unsaturated ester copolymer is a copolymer having a monomer unit based on ethylene and a monomer unit based on an unsaturated ester. The unsaturated ester is a compound having a vinyl group and an ester bond in the molecule, and examples of the unsaturated ester include vinyl carboxylate, unsaturated alkyl carboxylate, and unsaturated glycidyl carboxylate, and preferably at least one selected from the group consisting of vinyl carboxylate and unsaturated alkyl carboxylate. Examples of the vinyl carboxylate include vinyl acetate and vinyl propionate. Examples of the unsaturated alkyl carboxylate include methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate. Examples of the unsaturated glycidyl carboxylate include glycidyl acrylate and glycidyl methacrylate. The above unsaturated esters may be used alone or in combination of two or more.
[0053] Examples of the ethylene-unsaturated ester copolymer include ethylene-vinyl acetate copolymer, ethylene-vinyl propionate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-glycidyl methacrylate copolymer, ethylene-vinyl acetate-methyl methacrylate copolymer, etc. The above ethylene-unsaturated ester copolymers may be used alone or in combination of two or more kinds.
[0054] The content of the monomer unit based on ethylene in the ethylene-unsaturated ester copolymer is, for example, from the viewpoint of achieving better peelability from the roll of the sheet-forming material during the production of the encapsulating sheet and from the viewpoint of achieving higher conversion efficiency of the solar cell, preferably 65% by mass or more and 80% by mass or less, more preferably 67% by mass or more and 77% by mass or less, and even more preferably 68% by mass or more and 75% by mass or less, based on the total mass (100% by mass) of the ethylene-unsaturated ester copolymer, from the viewpoint of achieving better peelability from the roll of the sheet-forming material during the production of the encapsulating sheet and from the viewpoint of achieving higher conversion efficiency of the solar cell. The content of the monomer unit based on the unsaturated ester in the ethylene-unsaturated ester copolymer is, for example, from the viewpoint of achieving better peelability from the roll of the sheet-forming material during the production of the encapsulating sheet and from the viewpoint of achieving higher conversion efficiency of the solar cell, preferably 20% by mass or more and 35% by mass or less, more preferably 23% by mass or more and 33% by mass or less, and even more preferably 25% by mass or more and 32% by mass or less, based on the total mass (100% by mass) of the ethylene-unsaturated ester copolymer. In addition, when the ethylene-unsaturated ester copolymer has monomer units based on two or more kinds of unsaturated esters, the content of the monomer units based on the unsaturated ester is the total amount of the monomer units based on each unsaturated ester in the ethylene-unsaturated ester copolymer. The content of the monomer units based on the ethylene and the content of the monomer units based on the unsaturated ester are measured by infrared spectroscopy (IR method).
[0055] The melt flow rate of the ethylene-unsaturated ester copolymer is preferably 50 g / 10 min or less, more preferably 40 g / 10 min or less, from the viewpoint of achieving better peelability from the roll of the sheet-forming material during the production of the encapsulating sheet. The melt flow rate of the ethylene-unsaturated ester copolymer is preferably 4 g / 10 min or more, more preferably 5 g / 10 min or more, from the viewpoint of reducing the extrusion load during the production of the encapsulating sheet. The MFR is measured at a temperature of 190° C. and a load of 2.16 kg according to the method specified in JIS K7210-1995. The MFR can be adjusted, for example, by adjusting the polymerization pressure and / or polymerization temperature during the production of the ethylene-unsaturated ester copolymer.
[0056] The ethylene-unsaturated ester copolymer can be produced by copolymerizing ethylene with an unsaturated ester in the presence of a known radical generator.
[0057] The above-mentioned ethylene-based polymer can use, as the monomer such as ethylene, propylene, 1-butene, or 1-hexene, a monomer derived from a plant, a monomer derived from a fossil resource, or a monomer obtained by chemical recycling.
[0058] The plant-derived monomers are derived from carbon circulating on the earth's surface as plants and animals, and generally contain a certain percentage of carbon-14 (14C). Methods for producing plant-derived monomers include known methods, such as cracking bionaphtha, vegetable oil, animal oil, etc., dehydrogenation of biopropane, a method of separating alcohol from fermented products such as sugar extracted from plant raw materials such as sugarcane and corn, and subjecting it to a dehydration reaction, and a method of subjecting ethylene obtained from plant-derived ethanol to a metathesis reaction with n-butene.
[0059] The fossil resource-derived monomers are derived from underground carbon resources such as petroleum, coal, and natural gas, and generally contain almost no carbon-14 (14C). Methods for producing fossil resource-derived monomers include known methods, such as cracking of petroleum-derived naphtha and ethane, and dehydrogenation of ethane and propane to produce olefins.
[0060] The monomers obtained by chemical recycling are derived from carbon generated by decomposition and combustion of waste, and the carbon-14 (14C) content varies depending on the waste. Methods for producing monomers obtained by chemical recycling include known methods, such as a method of pyrolyzing waste plastics, a method of cracking waste vegetable oils and waste animal oils, and a method of gasifying, converting to alcohol, and dehydrating waste such as food waste, biomass waste, food waste, waste oil, waste wood, waste paper, and waste plastics.
[0061] The plant-derived monomer, the fossil resource-derived monomer, and the monomer obtained by chemical recycling may be used in combination of two or more kinds. For example, combinations such as fossil resource-derived ethylene / plant-derived ethylene / chemically recycled ethylene, fossil resource-derived ethylene / plant-derived ethylene / chemically recycled ethylene / fossil resource-derived 1-hexene / plant-derived 1-hexene / chemically recycled 1-hexene, etc. may be used. In this case, the plant-derived monomer, the fossil resource-derived monomer, and the monomer obtained by chemical recycling may be used in combination of two or more kinds of monomers produced individually, or may be used in combination of two or more kinds of monomers produced by mixing the respective raw materials, intermediates, etc.
[0062] In the ethylene-based polymer according to this embodiment, the carbon atoms constituting the ethylene-based polymer may be plant-derived carbon (14C), may be fossil resource-derived carbon, or may be composed of both.
[0063] The concentration of carbon-14 (14C) contained in ethylene-based polymers is calculated as pMC (percentage of modern carbon: unit %) using the AMS (Accelerator mass spectrometry) method specified in ISO 16620-2:2019.
[0064] From the viewpoint of reducing the environmental load, the carbon-14 (14C) concentration in the ethylene polymer is preferably 0.2 pMC(%) or more, more preferably 0.5 pMC(%) or more, even more preferably 1 pMC(%) or more, particularly preferably 5 pMC(%) or more, and most preferably 10 pMC(%) or more. From the viewpoint of reducing costs, the carbon-14 (14C) concentration is preferably 99 pMC(%) or less, more preferably 95 pMC(%) or less, even more preferably 90 pMC(%) or less, particularly preferably 70 pMC(%) or less, and most preferably 50 pMC(%) or less.
[0065] The carbon-14 (14C) concentration in the ethylene polymer can be adjusted by changing the ratio of the plant-derived monomer, the fossil resource-derived monomer, and the monomer obtained by chemical recycling used in the production of the ethylene polymer. More specifically, carbon-14 (14C) is contained at a certain ratio in carbon dioxide in the atmosphere, and it is known that plants that grow by absorbing carbon dioxide from the atmosphere, such as corn and trees, contain 14C. On the other hand, it is also known that fossil resources such as petroleum, which are thought to have been stored underground for a long time, contain almost no carbon-14 (14C). Therefore, carbon-14 (14C) can be contained in the constituent elements of the ethylene polymer by using a plant-derived substance as a raw material for the monomer used in the production of the ethylene polymer.
[0066] As the ethylene polymer containing carbon 14 (14C), commercially available ethylene polymers can be used, such as the "I'M GREEN" (green polyethylene) series manufactured by Braskem, the "TRUCIRCLE" series manufactured by SABIC, and the "CirculenRenew" series manufactured by LyondellBasell.
[0067] <Compound represented by structural formula (I)> In the above structural formula (I), n is 0, 1 or 2.
[0068] A represents a non-hydrogen group. The non-hydrogen group A is -CH3, -CH2CH3, -CH2CH2CH3, -CH2CH2CH2CH3, -CH2CH=CH2, -CH(CH3)CH=CH2, -CH2CH-X-CH2-X', -CH2CH-X''-CH2-CH3, -CH2CH-X'''-CH2OH, or -CH-OH-CH-OH-CH2-OH. Here, X, X', X'' and X''' are halogen atoms or halogenated hydrocarbon groups such as halogenated alkyl groups, preferably fluorine, chlorine or bromine atoms, or halogenated alkyl groups containing fluorine, chlorine or bromine atoms.
[0069] R 1 ~R 10 are each independently a hydrogen atom, a halogen atom, a phenyl group, or an alkyl group, an alkenyl group, an alkoxy group, or an acyl group having 1 to 20 carbon atoms, and the hydrogen atom in the phenyl group, the alkyl group, the alkenyl group, the alkoxy group, and the acyl group may be substituted with a halogen atom. The halogen atom is preferably a fluorine atom.
[0070] R 1 ~R 10 In the above formula, any two adjacent groups may together form a cyclic group.
[0071] In the structural formula (I), from the viewpoint of improving transparency, n is preferably 0, 1 or 2, and R 1 , R2 , R 4 , R 5 , R 6 , R 7 , R 9 and R 10 are hydrogen atoms, and R 3 , R 8 and A are each an alkyl group having from 1 to 20 carbon atoms.
[0072] The polyethylene resin composition according to the present embodiment contains 0.01 to 0.4 parts by mass of a compound represented by structural formula (I) relative to 100 parts by mass of an ethylene polymer having a Vicat softening point of 50 to 88° C. From the viewpoint of improving transparency, the polyethylene resin composition contains preferably 0.025 to 0.3 parts by mass, more preferably 0.05 to 0.2 parts by mass, of the compound represented by structural formula (I) relative to 100 parts by mass of the ethylene polymer.
[0073] From the viewpoint of improving heat resistance and flexibility, the Vicat softening point of the polyethylene resin composition is preferably 50°C or more and 90°C or less, more preferably 52°C or more and 89°C or less, and even more preferably 54°C or more and 88°C or less.
[0074] The polyethylene resin composition may contain additives as necessary, such as organic peroxides, hindered amine light stabilizers, crosslinking assistants, ultraviolet absorbers, and silane coupling agents.
[0075] (organic peroxide) An organic peroxide can be blended into the polyethylene resin composition. The organic peroxide is mainly used to crosslink the ethylene polymer. As the organic peroxide, an organic peroxide having a decomposition temperature (temperature at which the half-life is 1 hour) of 70°C or more and 180°C or less, particularly 90 to 160°C, can be used. Examples of such organic peroxides include t-butylperoxyisopropyl carbonate, t-butylperoxy-2-ethylhexyl carbonate, t-butylperoxyacetate, t-butylperoxybenzoate, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3,1,1-di(t-butylperoxy)-3,4 ... ,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy)cyclohexane, methyl ethyl ketone peroxide, 2,5-dimethylhexyl-2,5-diperoxybenzoate, t-butyl hydroperoxide, p-menthane hydroperoxide, benzoyl peroxide, p-chlorobenzoyl peroxide, t-butyl peroxyisobutyrate, hydroxyheptyl peroxide, dicyclohexanone peroxide, etc.
[0076] The content of the organic peroxide is preferably 0.2 parts by mass or more and 5 parts by mass or less, more preferably 0.5 parts by mass or more and 3 parts by mass or less, and even more preferably 1 part by mass or more and 2 parts by mass or less, based on 100 parts by mass of the ethylene-based polymer. When the blending ratio of the organic peroxide is within the above range, the crosslinking of the ethylene-based polymer is sufficiently and uniformly carried out.
[0077] (Hindered amine light stabilizer) The polyethylene resin composition may contain a hindered amine-based light stabilizer. The hindered amine-based light stabilizer captures radical species harmful to the polymer and prevents new radicals from being generated. There are many types of hindered amine-based light stabilizers, ranging from low molecular weight compounds to high molecular weight compounds, and any conventionally known compounds may be used without any particular limitation.
[0078] Low molecular weight hindered amine light stabilizers include a mixture of 70% by weight of decanedioic acid bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidinyl) ester, 1,1-dimethylethyl hydroperoxide, and octane (molecular weight 737) and 30% by weight of polypropylene; bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (molecular weight 685); a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl-1,2,2,6,6-pentamethyl-4-piperidylsebacate (molecular weight 509); and bis(2,2,6,6-tetramethyl-4-piperidyl). tetrakis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (molecular weight 481); tetrakis(1,2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butane tetracarboxylate (molecular weight 791); tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butane tetracarboxylate (molecular weight 847); a mixture of 2,2,6,6-tetramethyl-4-piperidyl-1,2,3,4-butane tetracarboxylate and tridecyl-1,2,3,4-butane tetracarboxylate (molecular weight 900); a mixture of 1,2,2,6,6-pentamethyl-4-piperidyl-1,2,3,4-butane tetracarboxylate and tridecyl-1,2,3,4-butane tetracarboxylate (molecular weight 900), and the like.
[0079] Examples of high molecular weight hindered amine light stabilizers include poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}] (molecular weight 2,000 to 3,100); polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol (molecular weight 3,100 to 4,000); N,N',N",N"'-tetrakis-(4,6-bis a mixture of -(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazin-2-yl)-4,7-diazadecane-1,10-diamine (molecular weight 2,286) and the polymer of the above dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol; a polymer of dibutylamine-1,3,5-triazine-N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine Condensates (molecular weight 2,600 to 3,400), as well as 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-acryloyloxy-1-ethyl-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-1-propyl-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-1-butyl-2,2,6,6-tetramethylpiperidine, 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine, 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine, and copolymers of cyclic aminovinyl compounds and ethylene such as 4-methacryloyloxy-1,2,2,6,6-pentamethylperidine, 4-methacryloyloxy-1-ethyl-2,2,6,6-tetramethylpiperidine, 4-methacryloyloxy-1-butyl-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, and 4-crotonoyloxy-1-propyl-2,2,6,6-tetramethylpiperidine. The above hindered amine light stabilizers may be used alone or in combination of two or more.
[0080] Among these, preferred examples of the hindered amine-based light stabilizer include poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}] (molecular weight 2,000 to 3,100); polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol (molecular weight 3,100 to 4,000); and N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazin-2-yl)-4,7-diazadecane-1,10-diamine. (molecular weight 2,286) and a polymer of the above-mentioned dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol; a polycondensate of dibutylamine-1,3,5-triazine-N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine (molecular weight 2,600 to 3,400); or a copolymer of a cyclic aminovinyl compound and ethylene. This is because bleeding out of the hindered amine light stabilizer over time during use of the product is prevented. Moreover, from the viewpoint of ease of preparation of the polyethylene resin composition, the hindered amine light stabilizer preferably has a melting point of 60°C or higher.
[0081] In the polyethylene resin composition, the content of the hindered amine-based light stabilizer relative to 100 parts by mass of the ethylene-based polymer is preferably 0.01 part by mass or more and 2.5 parts by mass or less, more preferably 0.01 part by mass or more and 1.0 part by mass or less, even more preferably 0.01 part by mass or more and 0.5 parts by mass or less, particularly preferably 0.01 part by mass or more and 0.2 parts by mass or less, and most preferably 0.03 part by mass or more and 0.1 part by mass or less.
[0082] By setting the content of the hindered amine light stabilizer at 0.01 parts by mass or more, a sufficient stabilizing effect can be obtained, and by setting it at 2.5 parts by mass or less, discoloration of the resin due to excessive addition of the hindered amine light stabilizer can be suppressed. In addition, in the polyethylene resin composition, the mass ratio of the organic peroxide to the hindered amine light stabilizer is preferably 1:0.01 or more and 1:10 or less, more preferably 1:0.02 or more and 1:6.5 or less. This makes it possible to significantly suppress yellowing of the polyethylene resin composition.
[0083] (Crosslinking aid) A crosslinking aid can be blended into the polyethylene resin composition. The crosslinking aid is effective in promoting the crosslinking reaction and increasing the degree of crosslinking of the ethylene-based polymer. Specific examples of the crosslinking aid include polyallyl compounds and poly(meth)acryloxy compounds. More specifically, examples of the crosslinking aid include polyallyl compounds such as triallyl isocyanurate, triallyl cyanurate, diallyl phthalate, diallyl fumarate, and diallyl maleate, poly(meth)acryloxy compounds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, and trimethylolpropane trimethacrylate, and divinylbenzene. The crosslinking aid can be blended in a ratio of more than 0 parts by mass and not more than 5 parts by mass with respect to 100 parts by mass of the ethylene-based polymer according to the present embodiment.
[0084] (UV absorber) The polyethylene resin composition may contain an ultraviolet absorbing agent, such as benzophenone-based, benzotriazole-based, triazine-based, salicylic acid ester-based, or other types of ultraviolet absorbing agent.
[0085] Examples of benzophenone-based ultraviolet absorbers include 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-n-octadecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone, 2-hydroxy-5-chlorobenzophenone, 2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, and 2,2',4,4'-tetrahydroxybenzophenone.
[0086] Benzotriazole-based ultraviolet absorbers include hydroxyphenyl-substituted benzotriazole compounds, such as 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-t-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dimethylphenyl)benzotriazole, 2-(2-methyl-4-hydroxyphenyl)benzotriazole, 2-(2-hydroxy-3-methyl-5-t-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-t-amylphenyl)benzotriazole, and 2-(2-hydroxy-3,5-di-t-butylphenyl)benzotriazole. In addition, triazine-based ultraviolet absorbers include 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)phenol, and the like. Examples of the salicylic acid ester include phenyl salicylate, p-octylphenyl salicylate, etc. The content of these ultraviolet absorbents is preferably 2.0 parts by mass or less, more preferably 0.05 parts by mass or more and 2.0 parts by mass or less, even more preferably 0.1 parts by mass or more and 1.0 parts by mass or less, particularly preferably 0.1 parts by mass or more and 0.5 parts by mass or less, and most preferably 0.2 parts by mass or more and 0.4 parts by mass or less, relative to 100 parts by mass of the ethylene polymer.
[0087] (Silane coupling agent) A silane coupling agent can be used in the polyethylene resin composition for the purpose of modifying the resin. Examples of the silane coupling agent used in the polyethylene resin composition include γ-chloropropyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyl-tris-(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-acryloxypropyltrimethoxysilane. The silane coupling agent is preferably vinyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, or 3-acryloxypropyltrimethoxysilane. The amount of these silane coupling agents used is preferably more than 0 parts by mass and not more than 5 parts by mass, more preferably 0.01 parts by mass or more and not more than 4 parts by mass, even more preferably 0.01 parts by mass or more and not more than 2 parts by mass, and particularly preferably 0.05 parts by mass or more and not more than 1 part by mass, relative to 100 parts by mass of the ethylene-based polymer.
[0088] (Other added ingredients) The polyethylene resin composition may contain other optional additional components within the scope of the present invention, such as antioxidants, crystal nucleating agents, clarifying agents, lubricants, colorants, dispersants, fillers, fluorescent whitening agents, ultraviolet absorbers, light stabilizers, etc., which are commonly used in polyolefin resin materials.
[0089] Furthermore, in order to impart flexibility and the like to the polyethylene resin composition, 3 parts by mass or more and 75 parts by mass or less of a rubber-based compound such as a lubricating oil, a crystalline ethylene-α-olefin copolymer polymerized by a Ziegler or metallocene catalyst and / or an ethylene-α-olefin elastomer such as EBR or EPR, or a styrene-based elastomer such as SEBS or a hydrogenated styrene block copolymer may be blended into the polyethylene resin composition, within a range that does not impair the object of the present invention.
[0090] Examples of the method for blending the polyethylene resin composition with other optional additional components include known melt-kneading methods, such as a method of dry blending using a tumbler blender, a Henschel mixer, or the like, followed by melt-kneading using a single-screw extruder, a multi-screw extruder, or the like, and a method of melt-kneading using a kneader, a Banbury mixer, or the like.
[0091] The polyethylene resin composition according to the present embodiment is used for, for example, sheets, containers, insulators such as electric wires and cables, sheaths, solar cell encapsulant, etc. As the solar cell encapsulant, the polyethylene resin composition in the form of pellets or sheets can be used.
[0092] The polyethylene resin composition according to the present embodiment can be molded into various molded articles by known molding methods, such as extrusion molding and covering extrusion molding for covering electric wires and pipes.
[0093] [Films and Sheets] The film or sheet according to the present embodiment contains the above-mentioned polyethylene resin composition.
[0094] The polyethylene resin composition according to the present embodiment can be used as a material for forming various films or sheets. The film formed using the polyethylene resin composition according to the present embodiment can be suitably used as a packaging material for food, medicine, daily necessities, etc., for example. The sheet formed using the polyethylene resin composition according to the present embodiment can be suitably used as an encapsulating sheet for solar cells, for example. In this specification, the film thickness of the film or sheet is not particularly limited, but for example, according to JIS Z 0108-2012, the film has a thickness of less than 250 μm, and the sheet has a thickness of 250 μm or more.
[0095] The method for producing the film or sheet is not particularly limited, and examples thereof include known film or sheet production methods, such as an inflation method using an inflation film production apparatus and an extrusion molding method such as a T-die method using a T-die cast film production apparatus.
[0096] [Solar cell encapsulant sheet] The solar cell encapsulant sheet according to this embodiment contains the above-mentioned polyethylene resin composition.
[0097] The polyethylene resin composition according to the present embodiment can be used as a material for forming a solar cell encapsulant sheet. The solar cell encapsulant sheet formed using the polyethylene resin composition according to the present embodiment may be a multilayer sheet having a skin layer-core layer-skin layer configuration. The skin layer is formed on the outermost surface of the solar cell encapsulant sheet, and is preferably a layer having a relatively low density and a low melting point. The core layer is preferably a layer having a relatively high density and a high melting point. The polyethylene resin composition according to the present embodiment may be used in the skin layer or the core layer of the solar cell encapsulant sheet. The polyethylene resin composition according to the present embodiment may be used in both the skin layer and the core layer.
[0098] When the solar cell encapsulant sheet is a multi-layer sheet having a skin layer-core layer-skin layer structure, the core layer does not need to contain a crosslinking agent and a crosslinking assistant.
[0099] The thickness of the core layer in the solar cell encapsulant sheet is preferably 0.2 mm or more and 0.4 mm or less, more preferably 0.25 mm or more and 0.35 mm or less. The thickness of each layer of the skin is preferably 0.03 mm or more and 0.1 mm or less, more preferably 0.035 mm or more and 0.080 mm or less. The total thickness of the two skin layers laminated on both sides of the core layer is preferably 1 / 20 to 1 / 3 of the total thickness of the solar cell encapsulant sheet, more preferably 1 / 15 to 1 / 4. By setting the thickness of each layer of the solar cell encapsulant sheet in such a range, the heat resistance and molding properties of the solar cell encapsulant sheet can be maintained in a good range.
[0100] The solar cell encapsulant sheet can be manufactured by a known sheet molding method using a T-die extruder, a calendar molding machine, or the like. The molded sheet is wound up on a paper tube for easy storage and transportation, but at this time, the sheets may adhere to each other (blocking may occur). If blocking occurs, the sheet cannot be stably unwound when it is unwound for use in the next process, resulting in reduced productivity. For this reason, it is common to avoid blocking by roughening the sheet surface or creating an uneven structure.
[0101] The present invention includes the following aspects. [1] A polyethylene resin composition comprising 100 parts by mass of an ethylene polymer having a Vicat softening point of 50°C or more and 88°C or less, and 0.01 part by mass or more and 0.4 part by mass or less of a compound represented by structural formula (I). [ka] [wherein n is 0, 1 or 2, A is a non-hydrogen group, and R 1 ~R 10are each independently a hydrogen atom, a halogen atom, a phenyl group, an alkyl group, an alkenyl group, an alkoxy group, or an acyl group, and a hydrogen atom in the phenyl group, the alkyl group, the alkenyl group, the alkoxy group, and the acyl group may be substituted with a halogen atom, and any two adjacent groups may form a cyclic group. [2] The polyethylene resin composition according to the above [1], wherein the Vicat softening point of the polyethylene resin composition is 50°C or higher and 90°C or lower. [3] The polyethylene resin composition according to the above [1] or [2], wherein the ethylene polymer has a Vicat softening point of 54°C or higher and 86°C or lower. [4] The polyethylene resin composition according to any one of the above [1] to [3], wherein the polyethylene resin composition has a Vicat softening point of 53°C or higher and 87°C or lower. [5] The density of the ethylene polymer is 880 kg / m 3 More than 910kg / m 3 The polyethylene resin composition according to any one of the above [1] to [4], which is: [6] The density of the ethylene polymer is 880 kg / m 3 More than 900kg / m 3 The polyethylene resin composition according to any one of the above [1] to [5], which is: [7] The polyethylene resin composition according to any one of the above [1] to [6], wherein the ethylene-based polymer is an ethylene-α-olefin copolymer. [8] The polyethylene resin composition according to the above [7], wherein the ethylene-α-olefin copolymer satisfies all of the following requirements (i) and (ii): (i) Vicat softening point is 50°C or higher and 85°C or lower. (ii) A melt flow rate of 0.10 g / 10 min or more and 30.00 g / 10 min or less. [9] A film or sheet comprising the polyethylene resin composition according to any one of the above [1] to [8].
[10] A solar cell encapsulant sheet comprising the polyethylene resin composition according to any one of the above [1] to [8]. EXAMPLES
[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The measured values of each item in the detailed description of the invention, examples, and comparative examples were measured by the following methods.
[0103] (1) Density (unit: kg / m 3 ) Measurement method After carrying out the annealing treatment described in JIS K6760-1995, the measurement was carried out by Method A according to the method specified in JIS K7112-1980.
[0104] (2)Melt flow rate (MFR, unit: g / 10 min) measurement method The measurement was performed according to Method A specified in JIS K7210-1995, at a temperature of 190°C and a load of 2.16 kg.
[0105] (3) Haze (unit: %) measurement method The polyethylene resin composition was preheated for 5 minutes in a hot press at 150°C, pressed for 5 minutes at a pressure of 5 MPa, and then cooled for 15 minutes in a laboratory atmosphere (about 23°C) to form a sheet having a thickness of 0.5 mm. The haze of the formed sheet was measured according to ASTM1003 using a direct-reading haze meter (manufactured by Toyo Seiki Seisakusho Co., Ltd.).
[0106] (4) Tensile impact strength (unit: kJ / m 2 ) Measurement method The polyethylene resin composition was preheated for 5 minutes in a hot press at 150°C, pressed for 5 minutes at a pressure of 5 MPa, and then cooled for 15 minutes in a laboratory atmosphere (about 23°C) to form a sheet. The tensile impact strength of the formed sheet was measured by a tensile impact test in a 23°C atmosphere in accordance with ASTM-D1822.
[0107] (5) Measurement method for volume resistivity (unit: Ω cm) A sheet having a thickness of 0.5 mm was molded by a heat press. The molded sheet was placed on a large-diameter electrode for flat plate samples SME-8310 (manufactured by Hioki E.E. Corporation), and a voltage of 500 V was applied at 23° C. After 1 minute, the resistance was measured with a digital insulation meter SM-7110 (manufactured by Hioki E.E. Corporation), and the volume resistivity was calculated based on the resistance in accordance with JIS-K-6911.
[0108] (6) Measurement method for Vicat softening point (VSP) (unit: °C) The ethylene polymer or polyethylene resin composition was pressed by a hot press to form a sheet having a thickness of about 5 mm. The Vicat softening point of the obtained sheet was measured according to the A50 method specified in JIS K7206-1999.
[0109] The materials used in the examples and comparative examples are as follows.
[0110] [Production Example of Ethylene Polymer A-1] (1) Production of component (H) Component (H) was produced in the same manner as in the preparation of component (A) in Examples 1(1) and (2) described in JP 2009-79180 A. Elemental analysis revealed that Zn was 11% by mass and F was 6.4% by mass.
[0111] (2) Preparation of prepolymerized catalyst component 41 liters of butane was added to a 210 liter autoclave equipped with a stirrer, which had been replaced with nitrogen in advance, and then 60.9 mmol of racemic ethylene bis(1-indenyl)zirconium diphenoxide was added. The autoclave was heated to 50°C and stirred for 2 hours. Next, 0.60 kg of the component (H) obtained above was added to the autoclave. The autoclave was then cooled to 31°C, and after the system was stabilized, 0.1 kg of ethylene and 0.1 liters of hydrogen (normal temperature and normal pressure) were added to the autoclave, followed by the addition of 240 mmol of triisobutylaluminum to initiate prepolymerization. Ethylene and hydrogen (normal temperature and normal pressure) were fed to the autoclave at 0.5 kg / hr and 1.1 liters / hr, respectively, for 30 minutes, and then the temperature was raised to 50°C, and ethylene and hydrogen (normal temperature and normal pressure) were fed to the autoclave at 2.7 kg / hr and 8.2 liters / hr, respectively. Prepolymerization was carried out for a total of 10.0 hours. After the completion of the prepolymerization, ethylene, butane, hydrogen, etc. were purged, and the remaining solid was vacuum dried at room temperature to obtain a prepolymerization catalyst component containing 4.14 g of polyethylene per 1 g of component (H). The [η] of the polyethylene was 1.26 dl / g.
[0112] (3) Production of ethylene polymer A-1 In the presence of the prepolymerized catalyst component obtained in (2) above, copolymerization of ethylene and 1-hexene was carried out in a continuous fluidized bed gas phase polymerization apparatus to obtain a powder of an ethylene-1-hexene copolymer (hereinafter referred to as ethylene polymer A-1). The polymerization conditions were as follows: polymerization temperature: 72°C; polymerization pressure: 2.0MPa; molar ratio of hydrogen to ethylene: 0.49%; molar ratio of 1-hexene to the total of ethylene and 1-hexene: 2.2%. Ethylene, 1-hexene and hydrogen were continuously supplied during polymerization to maintain a constant gas composition.
[0113] The above prepolymerization catalyst components, triisobutylaluminum, and triethylamine were continuously fed to maintain a constant total powder mass of 80 kg in the fluidized bed. The amount of triisobutylaluminum relative to the ethylene polymer A-1 was 0.43 mmol / kg. The molar ratio of triethylamine to triisobutylaluminum was 3%. The average polymerization time was 5.0 hr. The obtained ethylene polymer A-1 powder was granulated using an extruder (LCM50 manufactured by Kobe Steel, Ltd.) under conditions of a feed rate of 50 kg / hr, a screw rotation speed of 338 rpm, a gate opening of 50%, a suction pressure of 0.1 to 0.2 MPa, and a resin temperature of 180 to 200°C, to obtain pellets of the ethylene polymer A-1 (VSP: 54°C, MFR: 0.43 g / 10 min, density: 890 kg / m 3 ) was obtained.
[0114] [Production Example of Ethylene Polymer A-2] The ethylene polymer A-2 was produced under the same conditions as those for the production of the ethylene polymer A-1, except that the polymerization temperature was 77°C, the molar ratio of hydrogen to ethylene was 0.81%, the molar ratio of 1-hexene to the total of ethylene and 1-hexene was 2.5%, the amount of triisobutylaluminum to the ethylene polymer A-2 was 0.38 mmol / kg, the molar ratio of triethylamine to triisobutylaluminum was 10%, and the average polymerization time was 4.1 hr. Pellets of the ethylene polymer A-2 (VSP: 65°C, MFR: 0.55 g / 10 min, density: 896 kg / m 3 ) was obtained.
[0115] [Ethylene-based polymer A-3] Ethylene-1-hexene copolymer (Japan Polyethylene Co., Ltd., VSP: 78°C, MFR: 2.2g / 10min, density: 902kg / m 3 ) was used.
[0116] [Ethylene-based polymer A-4] Ethylene-1-octene copolymer (Dow Chemical Company, VSP: 86°C, MFR: 3.0g / 10min, density: 902kg / m 3 ) was used.
[0117] [Ethylene-based polymer A-5] High-pressure low-density polyethylene (Sumitomo Chemical Co., Ltd., VSP: 90°C, MFR: 3.5g / 10min, density: 919kg / m 3 ) was used.
[0118] [Ethylene-based polymer A-6] Ethylene-1-hexene copolymer (Sumitomo Chemical Co., Ltd., VSP: 47°C, MFR: 8.0g / 10min, density: 880kg / m 3 ) was used.
[0119] [Ethylene-based polymer A-7] High-pressure low-density polyethylene (Sumitomo Chemical Co., Ltd., VSP: 84°C, MFR: 7.0g / 10min, density: 919kg / m 3 ) was used.
[0120] [Nucleating agent B-1] Nonitol, 1,2,3-trideoxy-4,6:5,7-bis-O-[(4-propylphenyl)methylene] (Milliken) was used.
[0121] [Nucleating agent B-2] Bis(3,4-dimethylbenzylidene)sorbitol (manufactured by New Japan Chemical Co., Ltd.) was used.
[0122] [Nucleating agent B-3] Adeka STAB NA-21 (ADEKA Corporation) was used.
[0123] [Nucleating agent B-4] Hyperform (registered trademark) HPN-20E (manufactured by Milliken) was used.
[0124] [Production Example of Polyethylene Resin Composition] [Example 1] Nucleating agent B-1 (0.1 parts by mass) was mixed with ethylene polymer A-1 (100 parts by mass). The resulting mixture (100.1 parts by mass) was kneaded using Labo Plastomill R-100 (manufactured by Toyo Seiki Seisakusho) at 150°C, a rotation speed of 50 rpm, and for 5 minutes to obtain polyethylene resin composition 1. The physical properties of the resulting polyethylene resin composition 1 were evaluated and are shown in Table 1.
[0125] [Examples 2 to 6] Polyethylene resin compositions 2 to 6 were obtained under the same conditions as in Example 1, except that the conditions were changed as shown in Table 1. The physical properties of the obtained polyethylene resin compositions 2 to 6 were evaluated and are shown in Table 1.
[0126] [Comparative Examples 1 to 11] Polyethylene resin compositions C1 to C11 were obtained under the same conditions as in Example 1, except that the conditions were changed as shown in Table 2. The physical properties of the obtained polyethylene resin compositions C1 to C11 were evaluated and are shown in Table 2.
[0127] [Table 1]
[0128] [Table 2]
[0129] From Tables 1 and 2, it was shown that the press sheets using the polyethylene resin compositions of Examples 1 to 6, which satisfy all the constituent requirements of the present invention, maintained heat resistance because they had relatively high Vicat softening points. In addition, it was shown that the press sheets using the polyethylene resin compositions of Examples 1 to 6, which satisfy all the constituent requirements of the present invention, had relatively low haze values, which indicated that transparency was improved. In other words, according to the present invention, a polyethylene resin composition having relatively excellent heat resistance and transparency can be provided.
Claims
1. A polyethylene resin composition comprising 100 parts by mass of an ethylene polymer having a Vicat softening point of 50° C. or more and 88° C. or less, and 0.01 part by mass or more and 0.4 part by mass or less of a compound represented by structural formula (I). [Formula 1] [wherein n is 0, 1 or 2, A is a non-hydrogen group, and R 1 ~R 10 are each independently a hydrogen atom, a halogen atom, a phenyl group, an alkyl group, an alkenyl group, an alkoxy group, or an acyl group, and a hydrogen atom in the phenyl group, the alkyl group, the alkenyl group, the alkoxy group, and the acyl group may be substituted with a halogen atom, and any two adjacent groups may form a cyclic group.
2. The polyethylene resin composition according to claim 1, wherein the Vicat softening point of the polyethylene resin composition is 50°C or higher and 90°C or lower.
3. The polyethylene resin composition according to claim 1, wherein the ethylene polymer has a Vicat softening point of 54°C or higher and 86°C or lower.
4. The polyethylene resin composition according to claim 1, wherein the Vicat softening point of the polyethylene resin composition is 53°C or higher and 87°C or lower.
5. The density of the ethylene polymer is 880 kg / m 3 More than 910kg / m 3 2. The polyethylene resin composition according to claim 1, wherein:
6. The density of the ethylene polymer is 880 kg / m 3 More than 900kg / m 3 2. The polyethylene resin composition according to claim 1, wherein:
7. The polyethylene resin composition according to claim 1, wherein the ethylene-based polymer is an ethylene-α-olefin copolymer.
8. The polyethylene resin composition according to claim 7, wherein the ethylene-α-olefin copolymer satisfies all of the following requirements (i) and (ii): (i) A Vicat softening point of 50°C or higher and 85°C or lower. (ii) A melt flow rate of 0.10 g / 10 min or more and 30.00 g / 10 min or less.
9. A film or sheet comprising the polyethylene resin composition according to any one of claims 1 to 8.
10. A solar cell encapsulant sheet comprising the polyethylene resin composition according to any one of claims 1 to 8.
Citation Information
Patent Citations
ETHYLENE-alpha-OLEFIN COPOLYMER AND FOOD PACKAGING MATERIAL
JP2008106264A