Method of recycling urethane foam, method of manufacturing regenerated flexible urethane foam, and method of manufacturing regenerated amine-based polyol

By mixing urethane foam with diethanolamine and separating the reaction products, the method addresses the moldability issues of recycled polyol, enabling the production of flexible urethane foam with desired hardness and properties.

JP2024159620APending Publication Date: 2024-11-08SANYO CHEM IND LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024069612
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for recycling soft urethane resin result in recycled polyol with high hydroxyl and total amine values, leading to poor moldability and difficulty in achieving desired hardness during urethane resin production.

Method used

A method involving mixing urethane foam with diethanolamine at specific ratios, heating the mixture, and separating the resulting liquid into upper and lower layers through centrifugation to obtain a recycled polyol suitable for producing flexible urethane foam with desired hardness.

Benefits of technology

The method enables the production of recycled polyol with improved moldability, allowing the reformulation of urethane foam with desired hardness and properties, facilitating a resource circulation system for urethane foam.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159620000001
    Figure 2024159620000001
  • Figure 2024159620000002
    Figure 2024159620000002
  • Figure 2024159620000003
    Figure 2024159620000003
Patent Text Reader

Abstract

To provide a method of recycling a urethane foam, in which the urethane foam is easy to decompose, has a low hydroxy value and total amine value in an upper layer liquid obtained from the decomposed product, and has good moldability when using this upper layer liquid in a manufacture of urethane resin, and can be reformed into a urethane foam with desired hardness.SOLUTION: There is provided a method of recycling a urethane foam comprising: a mixing step of mixing a urethane foam and a urethane foam decomposing agent including diethanolamine at a weight ratio (urethane foam: decomposing agent) of 1:1 to 1:5; a urethane foam decomposing step of heating the mixture obtained in the mixing step to 100 to 200°C; and a separation step of centrifuging the liquid decomposed product obtained in the urethane foam decomposing step at 60 to 120°C to separate the liquid decomposed product into an upper layer liquid and a lower layer liquid, wherein weight of the diethanolamine contained in the urethane foam decomposing agent is 20 to 100 wt.% based on the weight of the urethane foam decomposing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recycling urethane foam. [Background technology]

[0002] Urethane resins are widely used as cushioning materials for automobile seats, furniture, mattresses, etc., as insulation materials, structural materials, and paving materials. The polyurethane foams used are produced and processed by methods such as slab production, on-site injection method, spray method, and panel molding method, and a large amount of foam waste (foam waste) is generated during the production and processing. Even after the product is used, it may be considered foam waste (so-called industrial waste). These foam wastes are difficult to recycle because they are thermosetting resins with a three-dimensional mesh structure, and currently they are disposed of by landfilling or incineration, so there is a need to develop effective reuse methods. Methods for recycling rigid polyurethane foam have been proposed in the past, such as a method in which polyurethane foam is decomposed using polyol and aminoethanol as decomposing agents and then regenerated as an adhesive assistant (Patent Document 1), and a method in which polyurethane foam is decomposed using an amine compound such as alkanolamine, and then the decomposed product is separated and recovered (Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 6-184513 [Patent Document 2] Patent No. 3242723 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the above-mentioned recycling method is applied to the decomposition of a flexible urethane resin, the hydroxyl value and total amine value of the resulting recycled polyol are high, and therefore, when used, the moldability during the production of the urethane resin is poor, making it difficult to obtain a urethane foam having the desired hardness. The present invention aims to provide a resource circulation system for urethane foam, which has good moldability during the production of urethane resin when recycled polyol obtained by decomposing urethane foam is used, and which can re-form urethane foam having the desired hardness. [Means for solving the problem]

[0005] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. That is, the present invention relates to a method for recycling urethane foam, the method including a mixing step of mixing urethane foam with a urethane foam decomposer containing diethanolamine in a weight ratio (urethane foam:decomposer) of 1:1 to 1:5, a urethane foam decomposition step of heating the mixture obtained in the mixing step to 100 to 200°C, and a separation step of centrifuging the liquid decomposition product obtained in the urethane foam decomposition step at 60 to 120°C to separate it into an upper layer liquid and a lower layer liquid, the weight of diethanolamine contained in the urethane foam decomposer being 20 to 100% by weight based on the weight of the urethane foam decomposer; a method for recycling urethane foam using the lower layer liquid separated in the separation step as the urethane foam decomposer; a method for producing recycled flexible urethane foam using the upper layer liquid separated in the separation step and polyisocyanate as essential monomers; and a method for producing recycled amine-based polyol using the lower layer liquid separated in the separation step and an alkylene oxide having 2 to 4 carbon atoms. Effect of the Invention

[0006] By using the recycling method of the present invention, a resource circulation system for urethane foam can be constructed, which can obtain recycled polyol that has good moldability during the production of urethane resin and can regenerate urethane foam having the desired hardness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The method for recycling urethane foam of the present invention includes a mixing step of mixing urethane foam with a urethane foam decomposer containing diethanolamine in a weight ratio (urethane foam:decomposer) of 1:1 to 1:5. The polyurethane foam decomposition agent contains diethanolamine, which allows the decomposition reaction to proceed without a catalyst and under mild conditions. Furthermore, diethanolamine is difficult to dissolve in the recycled polyol obtained by decomposing the polyurethane foam, which makes it easy to separate the polyol in the separation step described below, and allows the production of a recycled polyol with high purity.

[0008] The weight of diethanolamine contained in the urethane foam decomposer is 20 to 100% by weight, and more preferably 50 to 100% by weight, based on the weight of the urethane foam decomposer. If the weight of diethanolamine contained in the decomposition agent is less than 20% by weight, the decomposition reaction does not proceed sufficiently.

[0009] The urethane foam to be decomposed is not particularly limited, but examples include foam scraps generated during the manufacturing process (foam generated by trimming, burrs, foam leaking from air vent holes, free-expanded foam for quality control, defective products, etc.) and recovered foam recovered from various used industrial products (industrial equipment, furniture, building materials, etc.).

[0010] Urethane foam can be broadly divided into three types depending on the foaming method: rigid, semi-rigid, and soft. "Soft" polyurethane foam has interconnected cells that are soft and resilient, while "rigid" polyurethane foam has closed cells that are hard and lack resilience. "Semi-rigid" polyurethane foam is somewhere in between. Among these, in the urethane foam recycling method of the present invention, it is preferable to use a flexible urethane foam, which has good separability between the upper layer liquid and diethanolamine in the separation step described below, and can reduce the amount of amine components contained in the upper layer liquid, so that the upper layer liquid can be used to regenerate a urethane foam with good moldability and desired hardness.

[0011] The shape of the urethane foam to be used for decomposition is not particularly limited, and for example, foam scraps or recovered foam may be used as is, or foam that has been further shredded using a pelletizer equipped with a cutter blade, a cutter mill, a sentry cutter, a single-shaft crusher, a biaxial crusher, or the like may be used.

[0012] The urethane foam and the urethane foam decomposer containing diethanolamine can be mixed using a known mixing method, such as mixing in a reaction vessel equipped with a heating device and a stirring device for carrying out the decomposition step described below.

[0013] In the mixing step of the urethane foam recycling method of the present invention, the urethane foam and a urethane foam decomposition agent containing diethanolamine are mixed in a weight ratio (urethane foam:decomposition agent) of 1:1 to 1:5. If the weight ratio of urethane foam to the urethane foam decomposer containing diethanolamine is less than 1:1, the decomposition reaction does not proceed sufficiently, and if it exceeds 1:5, there is a problem that it becomes difficult to separate and purify the liquid decomposition product. The weight ratio of the urethane foam to the urethane foam decomposer containing diethanolamine (urethane foam:decomposer) is preferably 1:1.5 to 1:4.5, and more preferably 1:2 to 1:4.

[0014] The method for recycling urethane foam of the present invention includes a urethane foam decomposition step of heating the mixture obtained in the mixing step to 100 to 200° C. By carrying out the urethane foam decomposition step, the urethane foam reacts with the diethanolamine contained in the urethane foam decomposition agent, and the urethane foam is decomposed into a liquid decomposition product. The heating temperature in the decomposition step is more preferably 130 to 170° C. If the temperature is less than 100° C., the reaction does not proceed sufficiently, whereas if the temperature exceeds 200° C., there is a problem that the upper layer liquid becomes colored and cannot be reused in the production of a flexible polyurethane foam, and there is also a problem that a large amount of energy is consumed.

[0015] The reaction time in the decomposition step is preferably 2 to 48 hours, and more preferably 4 to 24 hours. With the reaction time in the above range, the reaction proceeds sufficiently without problems such as coloration, and furthermore, energy loss is small.

[0016] The urethane foam decomposition process can be carried out in a known reaction vessel equipped with a heating device and a stirring device.

[0017] The method for recycling urethane foam of the present invention includes a separation step in which the liquid decomposition product obtained in the above decomposition step is centrifuged at 60 to 120° C. to separate it into an upper layer liquid and a lower layer liquid. The temperature in the separation step is 60 to 120° C., and more preferably 80 to 100° C. If the temperature is less than 60° C., separation is insufficient, whereas if the temperature exceeds 120° C., there is a problem that the upper layer becomes colored.

[0018] Examples of the centrifugation method include a method using a decanter type centrifuge equipped with a screw conveyor or a disk type centrifuge equipped with a plurality of disks stacked in an umbrella shape. Of these, the method using a disk type centrifuge is preferred from the viewpoint of productivity.

[0019] The centrifugal force in the separation step is preferably 500 to 20,000 G, and more preferably 1,000 to 15,000 G. With the above centrifugal force, separation can be carried out efficiently.

[0020] The separation time in the separation step is preferably 0.1 to 60 minutes, and more preferably 0.1 to 30 minutes. With the above separation time, separation can be performed without problems such as coloring, and further energy loss is small.

[0021] The lower layer obtained in the separation step contains diethanolamine and by-products. The lower layer liquid can be used as a urethane foam decomposing agent in the above-mentioned urethane foam recycling method. That is, the second invention is a method for recycling urethane foam, comprising a mixing step of mixing urethane foam with a urethane foam decomposer containing diethanolamine in a weight ratio (urethane foam:decomposer) of 1:1 to 1:5, a urethane foam decomposition step of heating the mixture obtained in the mixing step to 100 to 200°C, and a separation step of centrifuging the liquid decomposition product obtained in the urethane foam decomposition step at 60 to 120°C to separate it into an upper layer liquid and a lower layer liquid, wherein the urethane foam decomposer contains the lower layer liquid separated in the separation step in the urethane foam recycling method of the first invention.

[0022] The upper layer liquid obtained in the separation step preferably has a hydroxyl value of 20 mgKOH / g to 200 mgKOH / g, more preferably 50 mgKOH / g to 130 mgKOH / g. The upper layer liquid obtained in the separation step preferably has a total amine value of 0 to 100 mgKOH / g, more preferably 0 to 60 mgKOH / g. The upper layer liquid obtained in the separation step preferably contains 60% by weight or more of the polyol constituting the urethane foam, and may additionally contain diethanolamine and by-products. The hydroxyl value in this specification is measured by the method specified in JIS K0070 (1995 edition). The total amine value in this specification can be measured by a method in accordance with ASTM D2074. Moreover, the upper layer liquid obtained in the separation step is preferably pale yellow to brown in color.

[0023] A flexible urethane foam can be produced by using the upper layer liquid and polyisocyanate as essential monomers. That is, the method for producing a recycled flexible urethane foam according to the third invention is a method for producing a recycled flexible urethane foam by using the upper layer liquid and polyisocyanate separated in the separation step in the method for recycling urethane foam according to the first invention as essential monomers. The method for producing the recycled flexible polyurethane foam is not limited except for using the above-mentioned upper layer liquid and polyisocyanate, and all methods conventionally used in the production of polyurethane can be applied. For example, a method is exemplified in which the mixture (premix resin) in which the above-mentioned upper layer liquid, catalyst, foam stabilizer, additives, and foaming agent are mixed in advance, and polyisocyanate is stirred and mixed by hand mixing at 1000 to 10000 rpm, and foamed in a specific container.

[0024] When the recycled flexible polyurethane foam is produced using the upper layer liquid and polyisocyanate as essential monomers, other polyols may be used in addition to the upper layer liquid. The other polyols are not particularly limited, and known polyols may be used.

[0025] The polyisocyanate used in the method for producing recycled flexible polyurethane foam may be any known organic polyisocyanate used in polyurethane foam. Examples include aromatic polyisocyanates, aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, modified polyisocyanates (modified products containing urethane groups, carbodiimide groups, allophanate groups, urea groups, biuret groups, isocyanurate groups, and oxazolidone groups, etc.) that are modified products of these, and mixtures of two or more of these.

[0026] The blowing agent may be any known blowing agent used in polyurethane foams, such as water, liquefied carbon dioxide gas, and low-boiling compounds having a boiling point of -5 to 70°C.

[0027] As the catalyst, a known catalyst used for polyurethane foams can be used.

[0028] As the foam stabilizer, known foam stabilizers (such as silicone-based foam stabilizers and non-silicone-based foam stabilizers) used in the production of polyurethane foams can be used, and examples thereof include commercially available foam stabilizers such as "SZ-1959", "SF-2904", "SZ-1142", "SZ-1720", "SZ-1675t", "SF-2936F", "SZ-3601", "SRX-294A", and "SH-193" manufactured by Dow Corning Toray Co., Ltd., "L-540" and "L-3601" manufactured by Nippon Unicar Co., Ltd., "L-595", "L-598", and "L-626" manufactured by Momentive Performance Materials, Inc., and "B8715 LF2" manufactured by Evonik Degussa Japan Ltd.

[0029] Examples of the additives include known additives such as colorants (dyes and pigments), plasticizers (phthalates, adipates, and the like), organic fillers (synthetic short fibers, hollow microspheres made of thermoplastic or thermosetting resins, and the like), flame retardants (phosphate esters, halogenated phosphate esters, and the like), age resistors (triazoles, benzophenones, and the like), and antioxidants (hindered phenols, hindered amines, and the like).

[0030] The lower layer liquid obtained in the separation step contains diethanolamine and by-products. By adding alkylene oxide to the diethanolamine contained in the lower layer liquid, a regenerated amine-based polyol can be obtained.

[0031] The fourth invention relates to a method for producing a regenerated amine-based polyol using the lower layer liquid and an alkylene oxide having a carbon number of 2 to 4. The regenerated amine-based polyol obtained by this method can be used to produce a regenerated urethane foam. Examples of alkylene oxides having 2 to 4 carbon atoms include ethylene oxide (hereinafter sometimes abbreviated as EO), 1,2- or 1,3-propylene oxide (hereinafter sometimes abbreviated as PO), and 1,2-, 1,3-, 1,4- or 2,3-butylene oxide, etc. Among these, it is preferable to use EO and / or PO from the viewpoint of reactivity.

[0032] The method for producing the regenerated amine polyol of the present invention can be carried out by mixing the lower layer liquid and an alkylene oxide having 2 to 4 carbon atoms and reacting them by heating. For example, the lower layer liquid and the catalyst are put into an autoclave, and while controlling the reaction temperature to be kept at 125 to 135°C, an alkylene oxide having 2 to 4 carbon atoms is dropped, and then the mixture is aged at 130°C, cooled to 60°C, and the catalyst is removed. This method allows the alkylene oxide to be added to the diethanolamine contained in the lower layer liquid to obtain a regenerated amine polyol. Catalysts for use in the process for producing regenerated amine-based polyol of the present invention include potassium hydroxide and sodium hydroxide. The catalyst can be removed by adsorption onto an adsorbent. Examples of the adsorbent include silicates such as aluminum silicate and magnesium silicate, activated clay, acid clay, and silica gel. Examples of commercially available adsorbents that can be used include silicates such as Kyoward 600 and 700 (trade names: Kyowa Chemical Industry Co., Ltd.), Mizuka Life P-1, P-1S, P-1G, and F-1G (trade names: Mizusawa Chemical Industry Co., Ltd.), and Tomita AD600 and 700 (trade names: Tomita Pharmaceutical Co., Ltd.). Only one of these adsorbents may be used, or two or more of them may be used in combination.

[0033] In the method for producing the regenerated amine polyol of the present invention, the weight ratio of the lower layer liquid to the alkylene oxide having 2 to 4 carbon atoms is preferably 1:1 to 1:100, more preferably 1:2 to 1:60. If the weight ratio of the lower layer liquid to the alkylene oxide having 2 to 4 carbon atoms is less than 1:1, the hydroxyl value and total amine value of the obtained regenerated amine polyol are high, and when it is used, the moldability during the production of urethane resin may be poor, and it may be difficult to obtain a urethane foam with the desired hardness. If it exceeds 1:100, the viscosity becomes high, and it may be impossible to produce a urethane foam using it. EXAMPLES

[0034] The present invention will be further described below with reference to examples, but the present invention is not limited to these. In the examples, the parts are parts by weight.

[0035] <Production Example 1> According to the formulation shown in Table 1, a polyol was mixed with a blowing agent, a catalyst, and a foam stabilizer, and then an organic polyisocyanate was mixed to obtain a mixture (H). The obtained mixture (H) was foamed under the foaming conditions described below to produce a polyurethane foam (X-1). The obtained polyurethane foam (X-1) was allowed to stand for 24 hours at a temperature of 25°C and a humidity of 50%, and then the 25% compression hardness, 40% compression hardness, rebound elasticity, tensile strength, elongation, tear strength and dry heat compression set of each polyurethane foam (X-1) were measured, and the results are shown in Table 1. The organic polyisocyanate was used in an amount such that the isocyanate index in the compounding recipe would be the isocyanate index shown in Table 1.

[0036] <Foaming conditions> Mold size: 250mm x 250mm x 250mm Material: wood Mixing method: Hand mixing (after placing the required amount of the required reagent in a designated container, insert the stirring blade into the container and stir at 3000 rpm for 6 to 20 seconds) Mixing time: 5 to 20 seconds Agitator rotation speed: 3000 rpm

[0037] [Table 1]

[0038] <Example 1> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and the liquid decomposition product of the polyurethane foam (X-1) was separated and collected into an upper layer liquid (Y-1) and a lower layer liquid (Z-1). The resulting upper layer liquid (Y-1) had a hydroxyl value of 80 mgKOH / g, a total amine value of 20 mgKOH / g, and a viscosity (25°C) of 810 mPa·s. The resulting lower layer liquid (Z-1) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1020 mPa·s. The amount of diethanolamine contained in the lower layer liquid (Z-1) was 79% by weight. The amount of diethanolamine was measured by liquid chromatography mass spectrometry (LCMS). The centrifuge (A-1) has a centrifuge tube capacity of 200 ml, a maximum centrifugal acceleration of 32,870 G, and a heating function. In addition, the viscosity (mPa·s) of the upper layer liquid (Y-1) and the lower layer liquid (Z-1) was measured by placing them in glass bottles, sealing them, and regulating the temperature at 25°C for 24 hours, and then using a B-type viscometer with rotor No. 3 or 4.

[0039] <Liquid chromatography mass spectrometry (LCMS) measurement conditions> Equipment: LCMS-8030 (Shimadzu Corporation) Column: Inert Sustain (particle size 2.0 μm, inner diameter 2.1 mm, length 10 cm) Mobile phase: A / B=15 / 85(v / v) A: 10 mM ammonium acetate aqueous solution / methanol = 80 / 20 (v / v) B: Methanol Flow rate: 0.1mL / min Sample preparation: Dilute with methanol to 1-100 ppm and filter through a 0.45 μm PTFE filter. Sample injection volume: 0.1 μL Oven temperature: 40℃ Detector: Mass spectrometer Ion source: ESI Mode:Negative Measured mass number: m / z 20-2000

[0040] <Example 2> A mixing step was carried out by charging 5.0 kg of diethanolamine as a urethane foam decomposition agent and 5.0 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 24 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and the liquid decomposition product of the polyurethane foam (X-1) was separated into an upper layer liquid (Y-2) and a lower layer liquid (Z-2) and collected. The resulting upper layer (Y-2) had a hydroxyl value of 110 mgKOH / g, a total amine value of 46 gKOH / g, and a viscosity (25°C) of 820 mPa s. The lower layer (Z-2) had a hydroxyl value of 1480 mgKOH / g, a total amine value of 505 mgKOH / g, and a viscosity (25°C) of 1080 mPa s.

[0041] <Example 3> A mixing step was carried out by charging 6.0 kg of diethanolamine as a urethane foam decomposition agent and 4.0 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 16 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and the liquid decomposition product of polyurethane foam (X-1) was separated into an upper layer liquid (Y-3) and a lower layer liquid (Z-3), which were then collected. The resulting upper layer (Y-3) had a hydroxyl value of 103 mgKOH / g, a total amine value of 38 mgKOH / g, and a viscosity (25°C) of 820 mPa s. The lower layer (Z-3) had a hydroxyl value of 1490 mgKOH / g, a total amine value of 510 mgKOH / g, and a viscosity (25°C) of 1060 mPa s.

[0042] <Example 4> A mixing step was carried out by charging 8.33 kg of diethanolamine as a urethane foam decomposition agent and 1.67 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and the liquid decomposition product of polyurethane foam (X-1) was separated into an upper layer liquid (Y-4) and a lower layer liquid (Z-4) and collected. The resulting upper layer (Y-4) had a hydroxyl value of 70 mgKOH / g, a total amine value of 11 mgKOH / g, and a viscosity (25°C) of 810 mPa s. The lower layer (Z-4) had a hydroxyl value of 1580 mgKOH / g, a total amine value of 530 mgKOH / g, and a viscosity (25°C) of 980 mPa s.

[0043] <Example 5> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 135°C for 16 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and the liquid decomposition product of polyurethane foam (X-1) was separated into an upper layer liquid (Y-5) and a lower layer liquid (Z-5) and collected. The resulting upper layer (Y-5) had a hydroxyl value of 80 mgKOH / g, a total amine value of 20 mgKOH / g, and a viscosity (25°C) of 820 mPa s. The lower layer (Z-5) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1010 mPa s.

[0044] <Example 6> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 120°C for 32 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and the liquid decomposition product of polyurethane foam (X-1) was separated into an upper layer liquid (Y-6) and a lower layer liquid (Z-6) and collected. The resulting upper layer (Y-6) had a hydroxyl value of 80 mgKOH / g, a total amine value of 20 mgKOH / g, and a viscosity (25°C) of 830 mPa s. The lower layer (Z-6) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1000 mPa s.

[0045] <Example 7> A mixing step was carried out by charging 12.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 100°C for 32 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), to separate and recover an upper layer liquid (Y-7) and a lower layer liquid (Z-7) of the liquid decomposition product of polyurethane foam (X-1). The resulting upper layer (Y-7) had a hydroxyl value of 70 mgKOH / g, a total amine value of 11 mgKOH / g, and a viscosity (25°C) of 810 mPa s. The lower layer (Z-7) had a hydroxyl value of 1580 mgKOH / g, a total amine value of 530 mgKOH / g, and a viscosity (25°C) of 980 mPa s.

[0046] <Example 8> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 200°C for 4 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and an upper layer liquid (Y-8) and a lower layer liquid (Z-8) of the liquid decomposition product of polyurethane foam (X-1) were separated and collected. The resulting upper layer (Y-8) had a hydroxyl value of 90 mgKOH / g, a total amine value of 30 mgKOH / g, and a viscosity (25°C) of 810 mPa s. The lower layer (Z-8) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1000 mPa s.

[0047] <Example 9> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 60°C, and then centrifuged at 60°C and 1000G for 22.5 minutes using a centrifuge (A-1), and an upper layer liquid (Y-9) and a lower layer liquid (Z-9) of the liquid decomposition product of the polyurethane foam (X-1) were separated and collected. The resulting upper layer (Y-9) had a hydroxyl value of 80 mgKOH / g, a total amine value of 20 mgKOH / g, and a viscosity (25°C) of 810 mPa s. The lower layer (Z-9) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1020 mPa s.

[0048] <Example 10> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 120°C, and then centrifuged at 1000G at 120°C for 7.5 minutes using a centrifuge (A-1), to separate and recover an upper layer liquid (Y-10) and a lower layer liquid (Z-10) of the liquid decomposition product of polyurethane foam (X-1). The resulting upper layer (Y-10) had a hydroxyl value of 80 mgKOH / g, a total amine value of 20 mgKOH / g, and a viscosity (25°C) of 810 mPa s. The lower layer (Z-7) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1020 mPa s.

[0049] <Example 11> A mixing step was carried out by charging 150 kg of diethanolamine as a urethane foam decomposition agent and 50 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 140°C for 13 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-2), and the upper layer liquid (Y-11) and lower layer liquid (Z-11) of the liquid decomposition product of polyurethane foam (X-1) were separated and collected. The resulting upper layer (Y-11) had a hydroxyl value of 82 mgKOH / g, a total amine value of 22 mgKOH / g, and a viscosity (25°C) of 800 mPa s. The lower layer (Z-11) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1030 mPa s. The centrifuge (A-2) is an industrial decanter centrifuge with a capacity of 300 L and a maximum centrifugal acceleration of 1000 G.

[0050] <Example 12> A mixing step was carried out by charging 150 kg of diethanolamine as a urethane foam decomposition agent and 50 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 140°C for 13 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 10,000G for 0.75 minutes using a centrifuge (A-3), and an upper layer liquid (Y-12) and a lower layer liquid (Z-12) of the liquid decomposition product of polyurethane foam (X-1) were separated and collected. The resulting upper layer (Y-12) had a hydroxyl value of 82 mgKOH / g, a total amine value of 22 mgKOH / g, and a viscosity (25°C) of 800 mPa s. The lower layer (Z-12) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1030 mPa s. The centrifuge (A-3) is a continuous disk-type centrifuge with a maximum centrifugal acceleration of 10,000G.

[0051] <Example 13> A mixing step was carried out by charging 7.5 kg of the lower layer liquid (Z-1) obtained in Example 1 and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 as a polyurethane foam decomposition agent into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 1000G for 7.5 minutes using a centrifuge (A-1), to obtain an upper layer liquid (Y-13) and a lower layer liquid (Z-13) of the liquid decomposition product of the polyurethane foam (X-1). The resulting upper layer liquid (Y-13) had a hydroxyl value of 118 mg KOH / g, a total amine value of 54 mg KOH / g, and a viscosity (25°C) of 820 mPa·s. The lower layer liquid (Z-13) had a hydroxyl value of 1540 mg KOH / g, a total amine value of 530 mg KOH / g, and a viscosity (25°C) of 1040 mPa·s. The amount of diethanolamine contained in the lower layer liquid (Z-13) calculated by analysis in the same manner as in Example 1 was 50% by weight.

[0052] <Example 14> A mixing step was carried out by charging 7.5 kg of the lower layer liquid (Z-13) obtained in Example 13 and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 as a polyurethane foam decomposition agent into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 16 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), to obtain an upper layer liquid (Y-14) and a lower layer liquid (Z-14) of the liquid decomposition product of the polyurethane foam (X-1). The resulting upper layer liquid (Y-14) had a hydroxyl value of 162 mgKOH / g, a total amine value of 96 mgKOH / g, and a viscosity (25°C) of 830 mPa·s. The lower layer liquid (Z-14) had a hydroxyl value of 1530 mgKOH / g, a total amine value of 530 mgKOH / g, and a viscosity (25°C) of 1090 mPa·s. The amount of diethanolamine contained in the lower layer liquid (Z-14) calculated by analysis in the same manner as in Example 1 was 20% by weight.

[0053] <Example 15> A mixing step was carried out by charging 7.5 kg of the lower layer liquid (Z-14) obtained in Example 14 and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 as a polyurethane foam decomposition agent into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 32 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), to obtain an upper layer liquid (Y-15) and a lower layer liquid (Z-15) of the liquid decomposition product of the polyurethane foam (X-1). The resulting upper layer liquid (Y-15) had a hydroxyl value of 203 mgKOH / g, a total amine value of 150 mgKOH / g, and a viscosity (25°C) of 900 mPa·s. The lower layer liquid (Z-15) had a hydroxyl value of 1530 mgKOH / g, a total amine value of 530 mgKOH / g, and a viscosity (25°C) of 1090 mPa·s. The amount of diethanolamine contained in the lower layer liquid (Z-15) calculated by analysis in the same manner as in Example 1 was 10% by weight.

[0054] [Table 2]

[0055] [Table 3]

[0056] <Comparative Example 1> A mixing process was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposer and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and after replacing the inside of the reactor with nitrogen, the reactor was heated at 80°C for 48 hours to carry out a decomposition process, but the urethane foam did not decompose and no liquid decomposition product was obtained.

[0057] <Comparative Example 2> A mixing step was carried out by charging 3.33 kg of diethanolamine as a urethane foam decomposer and 6.67 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and after replacing the inside of the reactor with nitrogen, the reactor was heated at 145°C for 48 hours to carry out a decomposition step, but the urethane foam did not decompose completely, and no liquid decomposition product was obtained.

[0058] <Comparative Example 3> A mixing step was carried out by charging 7.5 kg of the lower layer liquid (Z-15) obtained in Example 15 as a polyurethane foam decomposition agent and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and after replacing the inside of the reactor with nitrogen, the reactor was heated at 145°C for 48 hours to carry out a decomposition step, and a liquid decomposition product was obtained. The liquid decomposition product was cooled to 25°C, and then centrifuged at 25°C and 1000G for 60 minutes using a centrifuge (A-1), but the liquid decomposition product could not be separated into an upper layer liquid and a lower layer liquid.

[0059] <Comparative Example 4> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposer and 2.5 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 25°C, and then centrifuged at 25°C and 1000G for 60 minutes using a centrifuge (A-1), but the liquid decomposition product could not be separated into an upper layer liquid and a lower layer liquid.

[0060] <Comparative Example 5> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was heated to 160°C, and then centrifuged at 1000G at 160°C for 7.5 minutes using a centrifuge (A-1), and the upper layer liquid (Y-16) and lower layer liquid (Z-16) of the liquid decomposition product of polyurethane foam (X-1) were separated and collected. The resulting upper layer liquid (Y-16) had a hydroxyl value of 80 mgKOH / g, a total amine value of 20 mgKOH / g, and a viscosity (25°C) of 810 mPa·s. It was a black liquid and could not be reused for recycled flexible polyurethane foam. The lower layer liquid (Z-16) had a hydroxyl value of 1540 mgKOH / g, a total amine value of 520 mgKOH / g, and a viscosity (25°C) of 1020 mPa·s. It was a black liquid and could not be reused as a polyurethane foam decomposer or used to produce recycled amine-based polyol.

[0061] <Comparative Example 6> A mixing step was carried out by charging 7.5 kg of diethanolamine as a urethane foam decomposition agent and 2.5 kg of polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 250°C for 4 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 7.5 minutes using a centrifuge (A-1), and an upper layer liquid (Y-17) and a lower layer liquid (Z-17) of the liquid decomposition product of polyurethane foam (X-1) were separated and collected. The resulting upper layer liquid (Y-17) had a hydroxyl value of 91 mgKOH / g, a total amine value of 30 mgKOH / g, and a viscosity (25°C) of 960 mPa·s. It was a black liquid and could not be reused for recycled flexible polyurethane foam. The lower layer liquid (Z-17) had a hydroxyl value of 1530 mgKOH / g, a total amine value of 530 mgKOH / g, and a viscosity (25°C) of 1160 mPa·s. It was a black liquid and could not be reused as a polyurethane foam decomposer or used to produce recycled amine-based polyol.

[0062] <Comparative Example 7> A mixing step was carried out by charging 8.57 kg of diethanolamine as a urethane foam decomposer and 1.43 kg of the polyurethane foam (X-1) obtained in Production Example 1 into a reactor, and the inside of the reactor was replaced with nitrogen, and then the reactor was heated at 145°C for 8 hours to carry out a decomposition step, thereby obtaining a liquid decomposition product. The liquid decomposition product was cooled to 90°C, and then centrifuged at 90°C and 1000G for 60 minutes using a centrifuge (A-1), but the liquid decomposition product could not be separated into an upper layer liquid and a lower layer liquid.

[0063] [Table 4]

[0064] <Examples 16 to 19> According to the formulation shown in Table 5, a polyol was mixed with a blowing agent, a catalyst, and a foam stabilizer, and then an organic polyisocyanate was mixed to obtain a mixture (H). The obtained mixture (H) was foamed under the foaming conditions described above to produce a polyurethane foam (P). The obtained polyurethane foams (P) were allowed to stand for 24 hours at a temperature of 25°C and a humidity of 50%, and then the 25% compression hardness, 40% compression hardness, rebound elasticity, tensile strength, elongation, tear strength and dry heat compression set of each polyurethane foam (P) were measured, and the results are shown in Table 5. Regarding the organic polyisocyanate, an amount of organic polyisocyanate such that the isocyanate index in the compounding recipe would be the isocyanate index shown in Table 5 was used.

[0065] <Comparative Example 8> According to the formulation shown in Table 5, a polyol was mixed with a blowing agent, a catalyst, and a foam stabilizer, and then an organic polyisocyanate was mixed to obtain a mixture (H). The obtained mixture (H) was foamed under the foaming conditions described above to produce a polyurethane foam (P-8). The obtained polyurethane foam (P-8) was allowed to stand for 24 hours at a temperature of 25°C and a humidity of 50%, and then the 25% compression hardness, 40% compression hardness, rebound elasticity, tensile strength, elongation, tear strength and dry heat compression set of each polyurethane foam (P-8) were measured, and the results are shown in Table 5. The organic polyisocyanate was used in an amount such that the isocyanate index in the compounding recipe would be the isocyanate index shown in Table 1.

[0066] The density, 25% compression hardness, 40% compression hardness, rebound elasticity, tensile strength, elongation, tear strength and dry heat compression set of the polyurethane foam were measured by the methods described below.

[0067] <density> Density (kg / m2) based on JIS K6400 3 ) was measured.

[0068] <Compression hardness> The 25% compression hardness and 40% compression hardness were measured in accordance with JIS K6400 using polyurethane foam that had been kept at a temperature of 25°C (unit: N / 314 cm 2 ).

[0069] <Rebound elasticity> The impact resilience was measured according to a method in accordance with JIS K6400. Urethane foam with a rebound elasticity of 15% or less is considered low rebound.

[0070] <Tensile strength> The tensile strength was measured by a method in accordance with JIS K6400.

[0071] <Stretch> The elongation was measured by a method in accordance with JIS K6400.

[0072] <Tear strength> The tear strength was measured by a method in accordance with JIS K6400.

[0073] <Dry heat compression set> The dry heat compression set was measured according to a method in accordance with JIS K6400.

[0074] [Table 5]

[0075] <Example 20> In an autoclave, 100 parts by weight of the lower layer liquid (Z-1) obtained in Example 1 and 0.4 parts by weight of potassium hydroxide were added, and 285 parts by weight of 1,2-propylene oxide (hereinafter sometimes abbreviated as PO) was added dropwise while controlling the reaction temperature to be kept at 125 to 135° C., and then the mixture was aged for 2 hours at 130° C. After cooling to 60° C., 7.7 parts by weight of Kyoward 600 (manufactured by Kyowa Chemical Industry Co., Ltd.) and 7.7 parts by weight of water were added, and the mixture was treated at 90° C. for 1 hour to adsorb potassium hydroxide, filtered, and dehydrated under reduced pressure. The compound thus obtained had a hydroxyl value of 400 mgKOH / g and a total amine value of 135 mgKOH / g. The compound thus obtained was subjected to gel permeation chromatography (GPC) measurement, and it was found to contain a glycerin-PO adduct.

[0076] <Example 21> Into an autoclave, 100 parts by weight of the lower layer liquid (Z-1) obtained in Example 1 and 9 parts by weight of potassium hydroxide were charged, and 2650 parts by weight of 1,2-propylene oxide was added dropwise while controlling the reaction temperature to be maintained at 125 to 135° C., and then the mixture was aged for 2 hours at 130° C. After cooling to 60° C., 55 parts by weight of Kyoward 600 (manufactured by Kyowa Chemical Industry Co., Ltd.) and 55 parts by weight of water were charged, and the mixture was treated at 90° C. for 1 hour to adsorb potassium hydroxide, filtered, and dehydrated under reduced pressure. The compound thus obtained had a hydroxyl value of 56 mgKOH / g and a total amine value of 20 mgKOH / g. The compound thus obtained was subjected to gel permeation chromatography (GPC) measurement, and it was found to contain a glycerin-PO adduct.

[0077] <Gel Permeation Chromatography (GPC)> Equipment (example): Tosoh Corporation HLC-8120 Column (example): 2 TSK GEL GMH6 [Tosoh Corporation] Measurement temperature: 40℃ Sample solution: 0.25% by weight in THF Solution injection volume: 10μL Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) manufactured by Tosoh Corporation (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) For the measurement of molecular weight, a sample was dissolved in THF to a concentration of 0.25% by weight, and the insoluble matter was filtered off using a glass filter to obtain a sample solution.

[0078] From the examples, it can be seen that the urethane foam recycling method of the present invention can decompose soft urethane foam, the hydroxyl value and total amine value of the resulting upper layer liquid are low, and when used to produce urethane resin, the moldability is good and urethane foam with the desired hardness can be re-formed. [Industrial Applicability]

[0079] The upper layer liquid obtained by the urethane foam recycling method of the present invention has a low hydroxyl value and a low total amine value, and when used, it has good moldability during the production of urethane resin, and can regenerate urethane foam with the desired hardness. By adding an alkylene oxide having 2 to 4 carbon atoms to the upper layer liquid obtained by the urethane foam recycling method of the present invention, a polyol can be obtained, and further, urethane foam can be regenerated. Therefore, the present invention is effective in reducing the burden of waste disposal of urethane foam.

Claims

1. The method includes a mixing step of mixing urethane foam with a urethane foam decomposer containing diethanolamine in a weight ratio (urethane foam:decomposer) of 1:1 to 1:5, a urethane foam decomposition step of heating the mixture obtained in the mixing step to 100 to 200°C, and a separation step of centrifuging the liquid decomposition product obtained in the urethane foam decomposition step at 60 to 120°C to separate it into an upper liquid and a lower liquid, A method for recycling urethane foam, wherein the weight of diethanolamine contained in the urethane foam decomposer is 20 to 100% by weight based on the weight of the urethane foam decomposer.

2. 2. The method for recycling urethane foam according to claim 1, wherein the urethane foam is a soft urethane foam.

3. 2. The method for recycling urethane foam according to claim 1, wherein a disk-type centrifuge is used in the separation step.

4. A method for recycling urethane foam, comprising: a mixing step of mixing urethane foam with a urethane foam decomposer containing diethanolamine in a weight ratio (urethane foam:decomposer) of 1:1 to 1:5; a urethane foam decomposition step of heating the mixture obtained in the mixing step to 100 to 200°C; and a separation step of centrifuging the liquid decomposition product obtained in the urethane foam decomposition step at 60 to 120°C to separate it into an upper layer liquid and a lower layer liquid, wherein the urethane foam decomposer contains the lower layer liquid separated in the separation step according to claim 1.

5. A method for producing a recycled flexible polyurethane foam, comprising using the upper layer liquid separated in the separation step according to claim 1 and a polyisocyanate as essential monomers.

6. A method for producing a regenerated amine-based polyol, which uses the lower layer liquid separated in the separation step according to claim 1 and an alkylene oxide having 2 to 4 carbon atoms.

Citation Information

Patent Citations

  • Production of assistant for epoxy adhesive, and epoxy adhesive

    JP1994184513A

  • Method for decomposing and recycling rigid polyurethane foam waste

    JP3242723B2