Method for depositing hafnium lanthanum oxide film on substrate by circulation deposition process in reaction chamber
A cyclic deposition process for hafnium lanthanum oxide films addresses manufacturing challenges by alternating subcycles with specific precursors, achieving uniform and compositionally stable films for high-k dielectric applications in semiconductor devices.
Patent Information
- Application Number
- JP2024135191
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-14
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-02-14
AI Technical Summary
Existing deposition methods for hafnium lanthanum oxide films face challenges in achieving time-effective and cost-effective manufacturing with uniformity and control over electrical performance criteria, particularly in high-k dielectric applications for next-generation integrated circuits.
A cyclic deposition process involving alternating subcycles for hafnium and lanthanum oxide film deposition using specific vapor phase precursors and oxidants, such as hafnium chloride and water, and lanthanum precursors with molecular oxygen, in a controlled environment to achieve uniform and compositionally stable films.
The method enables the deposition of hafnium lanthanum oxide films with improved uniformity, controlled composition, and enhanced electrical properties, suitable for high-k dielectric applications in semiconductor devices.
Smart Images

Figure 2024159774000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates generally to methods for depositing lanthanum hafnium oxide films by a cyclic deposition process, and to a particular method for depositing lanthanum hafnium oxide films by a cyclic deposition process that includes a first sub-cycle and a second sub-cycle. [Background technology]
[0002] For many years, silicon dioxide (SiO2) has been used in semiconductor substrates for components such as transistor gate dielectrics and capacitor dielectrics. However, as circuit component dimensions shrink, the electrical performance characteristics of SiO2 result in undesirable effects such as increased leakage current. Controlling leakage current to maintain high speed and low power performance poses challenges when older generation dielectrics such as SiO2 are used in the manufacture of next generation integrated circuit geometries.
[0003] New processes, especially those using fabrication geometries below 65 nm, are beginning to include high dielectric constant ("high-k") insulators in semiconductor fabrication. Some chipmakers are relying on high-k dielectrics, especially for process geometries below 45 nm. Replacing SiO2 gate dielectrics with high-k dielectrics is critical to shrinking device geometries while controlling leakage and other electrical performance criteria.
[0004] While the use of high-k dielectrics enables finer scaling of integrated circuit components such as transistor gate dielectrics, new performance issues arise from their use. For example, when conventional gate electrodes are paired with high-k dielectrics such as HfO2, they can suffer from low yield and insufficient threshold voltage (V th ) control issues need to be addressed.
[0005] Research has been conducted into the benefits of using tertiary oxides in high-k dielectric applications. Specifically, hafnium lanthanum oxide (HfLaO xFilms fabricated from ) offer higher dielectric constant values, lower crystallization temperatures, improved yields, and lower threshold voltages (V th ) control. x or HfAlO x Unlike other Hf-based amorphous materials such as HfLaO x The dielectric constant of HfLaO remains high (>20). x The dielectric is desirable in terms of electrical performance criteria, but the HfLaO x Challenges arise in terms of time- and cost-effective manufacturing of the dielectric. Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, a method for depositing high-k hafnium lanthanum oxide films on a substrate would be highly desirable. [Means for solving the problem]
[0007] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description of exemplary embodiments of this disclosure. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
[0008] In some embodiments, a method is disclosed for depositing a hafnium lanthanum oxide film on a substrate by a cyclic deposition process in a reaction chamber. The method includes depositing a hafnium oxide film on a substrate using at least one deposition cycle of a first subcycle of the cyclic deposition process, the one deposition cycle of the first subcycle including contacting the substrate with a hafnium vapor phase precursor and contacting the substrate with a first oxidizer precursor comprising water (H2O). The method may also include depositing a lanthanum oxide film on a substrate using at least one deposition cycle of a second subcycle of the cyclic deposition process, the one deposition cycle of the second subcycle including contacting the substrate with a lanthanum vapor phase precursor and contacting the substrate with a second oxidizer precursor comprising water (O2).
[0009] For purposes of summarizing the invention and the advantages achieved over the prior art, certain objects and advantages of the invention are described herein above. Of course, it should be understood that not all such objects or advantages may be achieved by any particular embodiment of the invention. Thus, those skilled in the art will recognize that the invention may be embodied or carried out in a manner that achieves or optimizes, for example, one advantage or group of advantages as taught or suggested herein, without necessarily achieving other objects or advantages that may be taught or suggested herein.
[0010] All of these embodiments are intended to be within the scope of the invention disclosed herein. These and other embodiments will become readily apparent to those skilled in the art from the following detailed description of certain embodiments, taken in conjunction with the accompanying drawings, and the invention is not limited to any particular embodiment disclosed.
[0011] While the specification concludes with claims particularly pointing out and distinctly claiming what are regarded as embodiments of the present disclosure, the advantages of the embodiments of the present disclosure may be more readily ascertained from the following description of certain specific examples of embodiments of the present disclosure when read in conjunction with the accompanying drawings. [Brief description of the drawings]
[0012] [Figure 1] 1 illustrates a process flow depicting an overall supercycle of a cyclical deposition process according to an embodiment of the present disclosure. [Diagram 2] 1 shows a process illustrating a first sub-cycle of a cyclical deposition process according to an embodiment of the present disclosure. [Diagram 3] 1 shows a process illustrating a second sub-cycle of a cyclical deposition process according to an embodiment of the present disclosure. [Figure 4] 1 shows X-ray photoelectron spectroscopy (XPS) data illustrating the change in lanthanum composition of several exemplary hafnium lanthanum oxide films related to the ratio of lanthanum oxide deposition sub-cycles to hafnium oxide deposition sub-cycles according to embodiments of the present disclosure. [Diagram 5] 1 presents data showing the crystallization temperature of several exemplary lanthanum hafnium oxide films with increasing lanthanum composition, according to embodiments of the present disclosure. [Figure 6] 1 presents data showing the crystallization temperature of several exemplary lanthanum hafnium oxide films with increasing lanthanum composition (atomic %) at various film thicknesses according to embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Certain specific embodiments and examples are disclosed below, which are provided to illustrate the invention. It will be appreciated by those skilled in the art that the present invention extends beyond the illustrated embodiments and / or applications, and obvious modifications and equivalents thereof, and therefore it is not intended that the scope of the disclosed invention should be limited by the specific disclosed embodiments described below.
[0014] The figures shown herein are not meant to be actual illustrations of any particular materials, structures or devices, but merely idealized representations used to explain embodiments of the present disclosure.
[0015] As used herein, the term "cyclic deposition" refers to the sequential introduction of precursors (reactants) into a reaction chamber to deposit a film on a substrate, and includes deposition techniques such as atomic layer deposition and cyclic chemical vapor deposition.
[0016] As used herein, the term "cyclic chemical vapor deposition" can refer to any process in which a substrate is sequentially exposed to two or more volatile precursors that react and / or decompose on the substrate to produce a desired deposit.
[0017] The term "substrate" as used herein can refer to any underlying material or material(s) that can be used or upon which a device, circuit, or film can be formed.
[0018] The term "atomic layer deposition" (ALD) as used herein can refer to a vapor deposition process in which a deposition cycle, preferably multiple consecutive deposition cycles, are performed in a reaction chamber. Typically, during each cycle, a precursor chemisorbs to the deposition surface (e.g., the surface of a substrate or a surface of a previously deposited underlayer, such as a material deposited using a previous ALD cycle) and forms a monolayer or submonolayer that does not readily react with additional precursors (i.e., a self-limiting reaction). If necessary, a reactant (e.g., another precursor or reactant gas) can then be subsequently introduced into the process chamber for use in converting the chemisorbed precursor to the desired material on the deposition surface. Typically, this reactant can further react with the precursor. Additionally, a purge step can be utilized during each cycle to remove excess precursor from the process chamber after conversion of the chemisorbed precursor and / or to remove excess reactants and / or reaction by-products from the process chamber. Additionally, the term "atomic layer deposition" as used herein is also meant to include processes denoted by related terms, such as, for example, "chemical vapor deposition atomic layer deposition," "atomic layer epitaxy" (ALE), molecular beam epitaxy (MBE), gas source MBE, or metalorganic MBE, as well as chemical beam epitaxy when performed with alternating pulses of precursor composition(s), reactive gas, and purge (e.g., inert carrier) gas.
[0019] The term "film" as used herein can refer to any continuous or non-continuous structure and material(s) deposited by the methods disclosed herein. For example, a "film" can include 2D materials, nanorods, nanotubes, nanolaminates, or nanoparticles, or even partial or complete molecular layers, or partial or complete atomic layers, or clusters of atoms and / or molecules. A "film" can include material(s) or layer(s) that have pinholes, yet are at least partially continuous.
[0020] As used herein, the term "hafnium lanthanum oxide film" may refer to a film that includes a hafnium component, a lanthanum component, and an oxygen component.
[0021] As used herein, the term "subcycle" may refer to a cyclic deposition process that includes one or more unit cycles repeated a predetermined number of times. A combination of two or more subcycles may constitute an overall cyclic deposition process. This combination of two or more subcycles may be referred to as a cyclic deposition supercycle.
[0022] As used herein, the terms "metal organic" or "organometallic" are used interchangeably and may refer to organic compounds that contain a metal species. Organometallic compounds may be considered a subclass of organometallic compounds that have a direct metal-carbon bond.
[0023] As used herein, the terms "contact" or "expose" are used interchangeably and can refer to the interaction between the surface of the substrate (and any deposited film) and one or more precursors or reactants.
[0024] It should be noted that many example materials are provided throughout the embodiments of this disclosure, and the chemical formulas provided for each of the example materials should not be construed as limiting, nor should the non-limiting example materials provided be limited by certain example stoichiometries.
[0025] A wide variety of methods and associated equipment exist for depositing high dielectric constant films on substrates such as semiconductors. Some methods utilize surface reactions on the semiconductor to form thin films on the substrate, such as vacuum deposition, molecular beam epitaxy, various variants of chemical vapor deposition (CVD) (such as low pressure CVD, metalorganic CVD, plasma enhanced CVD, etc.), and atomic layer deposition (ALD).
[0026] ALD is a method of depositing a film on the surface of a substrate through the sequential introduction of various precursor species. A conventional ALD apparatus may include a reactor chamber, a substrate holder, a gas flow system including gas inlets for providing precursors and reactants to the substrate surface, and an exhaust system for removing spent gases. The growth mechanism relies on the adsorption of the precursors to active sites on the substrate, and conditions are preferably maintained such that a monolayer does not form on the substrate, thereby making the process self-terminating. Exposing the substrate to the first precursor is typically followed by a purge stage or other removal process (e.g., evacuation or "pump-down") to remove any excess amounts of the first precursor and any reaction by-products from the reaction chamber. A second reactant or precursor is then introduced into the reaction chamber, at which point it reacts with the first precursor, and this reaction creates the desired film on the substrate. The reaction is terminated when all of the available first precursor species adsorbed on the substrate have reacted with the second precursor. A second purge or other removal stage is then performed, whereby the remaining second precursor and possible reaction by-products are removed from the reaction chamber. This cycle can be repeated to grow the film to a desired thickness.
[0027] One of the recognized advantages of ALD over other deposition processes is that as long as the temperature is within the ALD window (above the condensation temperature of the precursor and below the pyrolysis temperature), it is self-saturating and uniform, and each pulse provides a sufficient amount of reactant to saturate the surface. Thus, the temperature or gas delivery may not need to be perfectly uniform to obtain a uniform deposition.
[0028] Different dielectric films have been deposited using ALD processes. Known dielectric films deposited utilizing ALD processes can include binary oxides such as Al2O3, HfO2, ZrO2, La2O3, and Ta2O5. Tertiary oxides are also materials that can be deposited by ALD and can include, for example, HfZrO, HfAlO, and HfLaO. Selection of an appropriate material for use in high-k dielectric applications requires consideration of the effects of the deposition material on the particular substrate and circuit environment.
[0029] For the ALD of hafnium lanthanum oxide, the hafnium vapor-phase precursor can include, for example, hafnium tetrachloride (HfCl4) and the lanthanum vapor-phase precursor can include La(THD)3. Due to the hygroscopic nature of La2O3, ozone (O3) is often used instead of H2O as the oxidant in conventional processes, but unfortunately, both the HfCl4 / O3 and La(THD)3 / O3 processes are extremely sensitive to even small changes in the amount of ozone present. Thus, it is difficult to achieve a repeatable process with conventional ALD processes.
[0030] Thus, the present disclosure includes methods that can be used for the deposition of hafnium lanthanum oxide films by a cyclic deposition process. The cyclic deposition process can include a cyclic deposition supercycle that includes at least a first subcycle that is utilized for the deposition of a hafnium oxide film, and a second subcycle that is utilized for the deposition of a lanthanum oxide film. The hafnium lanthanum oxide film can be deposited by repeating the cyclic deposition supercycle one or more times such that alternating films of hafnium oxide and lanthanum oxide are deposited on the substrate. In some applications, the alternating films of hafnium oxide and lanthanum oxide can be deposited to a thickness such that the resulting film includes either a substantially compositionally uniform hafnium lanthanum oxide film, or alternatively a nanolaminate structure that includes a hafnium lanthanum oxide film that includes distinguishable alternating layers of hafnium oxide and lanthanum oxide.
[0031] The present disclosure overcomes prior art limitations in the ALD of hafnium lanthanum oxide films by utilizing mixed oxidant precursors, i.e., a first oxidant precursor can be utilized during a first sub-cycle to deposit a hafnium oxide film, and a second oxidant precursor (different from the first oxidant precursor) can be utilized during a second sub-cycle to deposit a lanthanum oxide film.
[0032] Thus, the cyclic deposition process disclosed herein can deposit hafnium lanthanum oxide films with superior characteristics to those deposited by previous deposition processes. In addition, the cyclic deposition process disclosed herein can deposit HfLaO x Precise control of the composition of the film, as well as HfLaO x Lanthanum hafnium oxide films can be deposited with improved uniformity of the film's composition.
[0033] Thus, a method is disclosed for depositing a hafnium lanthanum oxide film on a substrate by a cyclic deposition process in a reaction chamber. In some embodiments, the cyclic deposition process may include depositing a hafnium oxide film on a substrate using at least one deposition cycle of a first subcycle of the cyclic deposition process, the one deposition cycle of the first subcycle including contacting the substrate with a hafnium vapor phase precursor and contacting the substrate with a first oxidizer precursor comprising water (H2O). The disclosed method may also include depositing a lanthanum oxide film on a substrate using at least one deposition cycle of a second subcycle of the cyclic deposition process, the one deposition cycle of the first subcycle including contacting the substrate with a lanthanum vapor phase precursor and contacting the substrate with a second oxidizer precursor comprising water (O2).
[0034] Non-limiting exemplary embodiments of cyclic deposition processes include atomic layer deposition (ALD), which is based on a typically self-limiting reaction whereby sequential and alternating pulses of reactants are used to deposit approximately one atomic (or molecular) monolayer of material per deposition cycle. Deposition conditions and precursors are typically selected to provide a self-saturating reaction, such that an adsorbed layer of one reactant leaves a surface termination unreactive with the gas-phase reactant of the same reactant. The substrate is then contacted with a different reactant that reacts with the previous termination, allowing successive depositions. Thus, alternating Each cycle of alternating pulses typically leaves about one monolayer or less of the desired material, although one of skill in the art will recognize that, as noted above, more than one monolayer of material can be deposited in one or more ALD cycles, e.g., if some gas-phase reactions occur despite the alternating nature of the process.
[0035] A cyclical deposition process for depositing hafnium lanthanum oxide films may include two or more subcycles, with each subcycle including an ALD-type process for depositing two or more films, such as, for example, a hafnium oxide film and a lanthanum oxide film. In some embodiments, a first subcycle may include an ALD-type process for depositing a hafnium oxide film, with one deposition cycle, i.e., a unit deposition cycle, including exposing a substrate to a first precursor, removing unreacted first precursor and reaction by-products from the reaction chamber, and exposing the substrate to a second precursor, followed by a second removal step. In some embodiments, the first precursor of the first subcycle may include a hafnium vapor-phase precursor ("hafnium precursor") and the second precursor of the first subcycle may include a first oxidizer precursor. In some embodiments, the second subcycle can also include an ALD-type process for depositing a lanthanum oxide film, where one deposition cycle, or unit deposition cycle, can include exposing the substrate to a first precursor, removing unreacted first precursor and reaction by-products from the reaction chamber, and exposing the substrate to a second precursor, followed by a second removal step. In some embodiments, the first precursor of the second subcycle can include a lanthanum vapor-phase precursor ("lanthanum precursor"), and the second precursor of the second subcycle can include a second oxidizer precursor.
[0036] The precursors may be separated by an inert gas, such as argon (Ar) or nitrogen (N2), to prevent gas-phase reactions between the precursors and to allow self-saturating surface reactions. However, in some embodiments, the substrate may be moved to contact the first and second gas-phase reactants separately. Since the reaction is self-saturating, strict temperature control of the substrate and precise dosage control of the precursors may not be necessary. However, the substrate temperature is preferably such that the incident gas species do not condense into a monolayer and do not decompose at the surface. Before contacting the substrate with the next reactive chemical, excess chemicals and reaction by-products, if any, are removed from the substrate surface, for example by purging the reaction space or by moving the substrate. Undesired gas molecules can be effectively evacuated from the reaction space with an inert purge gas. A vacuum pump can be used to facilitate purging.
[0037] Reactors that can be used to deposit hafnium lanthanum oxide films can be used for the cyclic deposition process described herein. Such reactors include ALD reactors configured to deliver precursors as well as CVD reactors. According to some embodiments, showerhead reactors can be used. According to some embodiments, cross-flow, batch, mini-batch, or spatial ALD reactors can be used.
[0038] In some embodiments of the present disclosure, a batch reactor may be used. In some embodiments, a vertical batch reactor may be utilized. In other embodiments, the batch reactor comprises a mini-batch reactor configured to accommodate 10 or less wafers, 8 or less wafers, 6 or less wafers, 4 or less wafers, or 2 or less wafers. In some embodiments where a batch reactor is used, the wafer-to-wafer non-uniformity is less than 3% (1 sigma), less than 2%, less than 1% or even less than 0.5%.
[0039] The deposition processes described herein can optionally be carried out in reactors or reaction chambers that are coupled to a cluster tool. In a cluster tool, each reaction chamber has one Since the reaction chambers in each module are dedicated to a specific type of process, the temperature of the reaction chambers in each module can be kept constant, improving throughput compared to reactors that heat the substrate to a process temperature before each run. Additionally, the cluster tool allows for a shorter time to evacuate the reaction chambers to the desired process pressure level between substrates. In some embodiments of the present disclosure, the deposition process may be performed in a cluster tool that includes multiple reaction chambers, each individual reaction chamber may be used to expose the substrate to an individual precursor gas, and the substrate may be transported between the different reaction chambers to expose the substrate to the multiple precursor gases, with the substrate transport being performed under a controlled ambient environment to avoid oxidation / contamination of the substrate. In some embodiments of the present disclosure, the deposition process may be performed in a cluster tool with multiple reaction chambers, each individual reaction chamber may be configured to perform a different sub-cycle of the overall cyclical deposition process, i.e., a cyclical deposition super-cycle. For example, a first reaction chamber of the cluster tool may be configured to perform a first sub-cycle and a second reaction chamber of the cluster tool may be configured to perform a second sub-cycle, and the substrate may be moved between the first and second reaction chambers under a controlled environment to prevent unwanted contamination of the substrate and the oxide film thereon.
[0040] In certain embodiments, the reactor or reaction chamber may comprise a stand-alone reactor equipped with a load lock, in which case there is no need to cool the reaction chamber between runs. In some embodiments, the deposition process for deposition of lanthanum hafnium oxide films may include multiple deposition cycles, i.e., multiple unit cycles, such as ALD cycles or cyclic CVD cycles.
[0041] In some embodiments, one or more cyclic deposition processes are used to deposit the HfLaO of the present disclosure onto a substrate. x A film may be deposited. In some embodiments, the cyclic deposition process may include one or more ALD type processes. In some embodiments, the cyclic deposition process may include one or more hybrid ALD / CVD or one or more cyclic CVD processes. For example, in some embodiments, the growth rate of an ALD process may be low compared to a CVD process. One approach to increase the growth rate may be to operate at a higher substrate temperature than typically used in an ALD process, resulting in at least a portion of the deposition provided by a chemical vapor deposition type process, but still with the advantage of sequential introduction of precursors. Such a process may be referred to as a cyclic CVD process. In some embodiments, the cyclic CVD process may include the introduction of two or more precursors into the reaction chamber, with periods of overlap between the two or more precursors in the reaction chamber resulting in both the ALD component of the deposition and the CVD component of the deposition. For example, the cyclic CVD process may include a continuous flow of one precursor into the reaction chamber, and periodic pulsed injection of a second precursor.
[0042] In some embodiments, a cyclic deposition process may be utilized to deposit a hafnium lanthanum oxide film, non-limiting examples of such cyclic deposition processes may be understood with reference to FIGS. 1-3, where FIG. 1 illustrates an exemplary overall cyclic deposition process including a cyclic deposition supercycle, FIG. 2 illustrates an exemplary first subcycle for depositing a hafnium oxide film, and FIG. 3 illustrates an exemplary second subcycle for depositing a lanthanum oxide film.
[0043] More specifically, FIG. 1 shows HfLaO xAn exemplary overall cyclical deposition process 100 is shown that includes a cyclical deposition supercycle 150 that includes a first subcycle 120 and a second subcycle 130 that are utilized to deposit a film. More specifically, the cyclical deposition process 100 can begin with a process 110 that includes providing a substrate into a reaction chamber and heating the substrate to a desired deposition temperature.
[0044] In some embodiments of the present disclosure, the substrate may include a planar substrate or a patterned substrate including high aspect ratio features, such as trench structures and / or fin structures. The substrate may include one or more materials including, but not limited to, silicon (Si), germanium (Ge), germanium tin (GeSn), silicon germanium (SiGe), silicon germanium tin (SiGeSn), silicon carbide (SiC), or III-V semiconductor materials, such as gallium arsenide (GaAs), gallium phosphide (GaP), or gallium nitride (GaN). In some embodiments of the present disclosure, the substrate may comprise an engineered substrate, where a surface semiconductor layer is disposed on a bulk support with an intervening buried oxide (BOX) disposed therebetween.
[0045] The patterned substrate may comprise a substrate that may include semiconductor device structures formed in or on a surface of the substrate, for example, the patterned substrate may include partially fabricated semiconductor device structures, such as transistors and / or memory elements. In some embodiments, the substrate may include one or more secondary surfaces that may include a single crystal surface and / or a non-single crystal surface, such as a polycrystalline surface and / or an amorphous surface. The single crystal surface may include, for example, one or more of silicon (Si), silicon germanium (SiGe), germanium tin (GeSn), or germanium (Ge). The polycrystalline or amorphous surface may include a dielectric material, such as an oxide, oxynitride, or nitride, such as silicon oxide and silicon nitride.
[0046] The reaction chamber utilized for deposition may be an atomic layer deposition reaction chamber, or a chemical vapor deposition reaction chamber, or any of the reaction chambers as previously described herein. In some embodiments of the present disclosure, the substrate may be heated to a desired deposition temperature during the cyclical deposition process. For example, the substrate may be heated to a substrate temperature of less than about 750°C, or less than about 650°C, or less than about 550°C, or less than about 450°C, or less than about 350°C, or less than about 300°C, or less than about 250°C, or less than about 150°C. In some embodiments of the present disclosure, the substrate temperature during the cyclical deposition process may be between 100°C and 400°C, or between 150°C and 350°C, or between 200°C and 300°C.
[0047] 1 may continue with a cyclical deposition supercycle 150, which includes one or more repetitions of depositing a hafnium oxide film utilizing at least one deposition cycle of a first subcycle and depositing a lanthanum oxide film utilizing at least one deposition cycle of a second subcycle. The cyclical deposition supercycle 150 may begin with process block 120, which includes depositing a hafnium oxide film utilizing at least one deposition cycle of a first subcycle.
[0048] 2 illustrates in more detail the first subcycle 120 and its constituent subprocesses. For example, the first subcycle 120 may begin by subprocess block 210, which includes contacting or exposing a substrate with a hafnium vapor-phase reactant (a "hafnium precursor").
[0049] In some embodiments, the hafnium precursor may include at least one of a hafnium halide precursor, a hafnium organometallic precursor, or an organometallic hafnium precursor.
[0050] As described later herein, in some embodiments, the hafnium halide precursor may include at least one halogen ligand, while the remaining ligands, e.g., metallo-organic or organometallic ligands, are different. In some embodiments, the hafnium halide precursor includes one, two, three, or four halide ligands, e.g., chloride ligands. That's fine too.
[0051] In some embodiments, the hafnium halide precursor may include at least one of hafnium chloride, hafnium iodide, or hafnium bromide. In some embodiments, the hafnium chloride may include hafnium tetrachloride (HfCl4). In some embodiments, the hafnium iodide may include hafnium tetraiodide (HfI4). In some embodiments, the hafnium bromide may include hafnium tetrabromide (HfBr4).
[0052] In some embodiments, the hafnium organometallic precursor can include at least one of a hafnium alkylamide precursor, a hafnium cyclopentadienyl ligand-containing precursor, or other organometallic hafnium precursor.
[0053] In some embodiments, the hafnium alkylamide precursor may be selected from the group including tetrakis(ethylmethylamido)hafnium (Hf(NEtMe)4), tetrakis(dimethylamido)hafnium (Hf(NMe2)4), or tetrakis(diethylamido)hafnium (Hf(NEt2)4).
[0054] In some embodiments of the present disclosure, the hafnium cyclopentadienyl ligand-containing precursor may be selected from the group including (tris(alkylamido)cyclopentadienylhafnium, such as (tris(dimethylamido)cyclopentadienylhafnium HfCp(NMe2)3, or bis(methylcyclopentadienyl)methoxymethylhafnium (MeCp)2Hf(CH)3(OCH3) or derivatives thereof, such as those having one or more hydrocarbon groups, such as alkyl, or other alkyl groups of the alkylamido ligands, bonded to the cyclopentadienyl ligands of the precursors.
[0055] In some embodiments, the hafnium precursor has the formula: HfL1L2L3L4 In the formula, each of the L ligands L1 to L4 is a) a halide, such as chloride, bromide, or iodide; b) alkylamides, such as dimethylamide (-NMe2), diethylamide (-NEt2), ethylmethylamide (-NEtMe); c) amidinates, such as N,N'-dimethylformamidinate; d) guanidinates, such as N,N'-diisopropyl-2-ethylmethylamidoguanidinate; e) cyclopentadienyl or derivatives thereof, such as cyclopentadienyl or methylcyclopentadienyl or other alkyl substituted cyclopentadienyl ligands; f) cycloheptadienyl or cycloheptatrienyl systems, for example cycloheptatrienyl or cycloheptadienyl g) alkyl, e.g. C1-C5 alkyl, e.g. mostly methyl in the case of heteroleptic precursors; h) Alkoxides, such as methoxide (-OMe), ethoxide (-OEt), isopropoxide (-O i Pr), n-butoxide (-OBu) or tert-butoxide (-O t Bu) i) beta-diketonates, such as (2,2,6,6-tetramethyl-3,5-heptanedionate) (THD), and / or j) a donor functionalized alkoxide, for example dimethylethanolamine.
[0056] In some embodiments of the present disclosure, the hafnium precursor comprises nitrogen and / or oxygen atoms. In some embodiments, the hafnium precursor comprises one or more bidentate ligands bonded to Hf through nitrogen, oxygen, and / or carbon.
[0057] In some embodiments of the present disclosure, the hafnium precursor does not include a plasma-excited precursor, i.e., the hafnium oxide film is deposited without plasma excitation of the precursor, in other words, the hafnium oxide film is deposited in a plasma-free environment.
[0058] In some embodiments of the present disclosure, contacting the substrate with a hafnium vapor phase precursor may include pulsing the hafnium precursor into the reaction chamber, followed by contacting the hafnium precursor with the substrate for a time period of about 0.01 seconds to about 60 seconds, or about 0.05 seconds to about 10 seconds, or about 0.1 seconds to about 5.0 seconds. In addition, during the pulsing of the hafnium precursor, the flow rate of the hafnium precursor can be less than 2000 sccm, or less than 500 sccm, or even less than 100 sccm. In addition, during the pulsing of the hafnium precursor onto the substrate, the flow rate of the hafnium precursor can range from about 1 to 2000 sccm, or from about 5 to 1000 sccm, or from about 10 to about 500 sccm.
[0059] The exemplary subcycle 120 of FIG. 2 can be continued by purging the reaction chamber. For example, excess rhenium precursor and reaction by-products (if any) can be removed from the surface of the substrate, for example, by evacuating with an inert gas. In some embodiments of the present disclosure, the purge process can include a purge cycle, where the substrate surface is purged for a time period of less than about 5.0 seconds, or less than about 3.0 seconds, or even less than about 2.0 seconds. Excess hafnium gas-phase reactant, and any possible reaction by-products, can be removed using a vacuum generated by a pump system in fluid communication with the reaction chamber.
[0060] Upon purging the reaction chamber with the purge cycle, the exemplary cyclical deposition subcycle 120 may continue with subprocess block 220, which includes contacting or exposing the substrate to a first oxidant precursor, in particular a first oxidant precursor comprising water (H2O). In alternative embodiments, the first oxidant precursor comprises at least one of hydrogen peroxide (H2O2), ozone (O3), or nitrogen oxides, such as nitric oxide (NO), nitrous oxide (N2O), or nitrogen dioxide (NO2). In some embodiments of the present disclosure, the oxidant precursor may comprise an organic alcohol, such as isopropyl alcohol.
[0061] In some embodiments of the present disclosure, the first oxidizer precursor does not include a plasma-excited precursor, i.e., the hafnium oxide film is deposited without plasma excitation of the precursor, in other words, in certain embodiments, the hafnium oxide film is deposited in a plasma-free environment.
[0062] In some embodiments of the present disclosure, contacting the substrate with the first oxidant precursor may include pulsing the first oxidant precursor, such as water (HO), into the reaction chamber, followed by contacting the substrate with the first oxidant precursor for a time period of about 0.01 seconds to about 60 seconds, or about 0.05 seconds to about 10 seconds, or about 0.1 seconds to about 5.0 seconds. In addition, during the pulsing of the first oxidant precursor, the flow rate of the first oxidant precursor can be less than 2000 sccm, or less than 500 sccm, or even less than 100 sccm. In addition, during the pulsing of the first oxidant precursor onto the substrate, the flow rate of the first oxidant precursor can range from about 1 to 2000 sccm, or from about 5 to 1000 sccm, or from about 10 to about 500 sccm.
[0063] In embodiments where the first oxidant precursor comprises water (HO), the purity of the water can be determined by its electrical resistivity For example, a higher electrical resistivity of water may indicate a higher purity and therefore reduce unwanted contaminants in the deposited film. In some embodiments, the first oxidizer precursor may include water (H2O) having an electrical resistivity of greater than 5 MΩ·cm, or greater than 10 MΩ·cm, or greater than 15 MΩ·cm, or greater than 20 MΩ·cm. In some embodiments of the present disclosure, the electrical resistivity of water utilized in the deposition of the hafnium oxide film may be between 5 MΩ·cm and 20 MΩ·cm.
[0064] The exemplary subcycle 120 of FIG. 2 can be continued by purging the reaction chamber. For example, excess first oxidant precursor and reaction by-products (if any) can be removed from the surface of the substrate, for example, by evacuating with an inert gas. In some embodiments of the present disclosure, the purge process can include a purge cycle, where the substrate surface is purged for a time period of less than about 5.0 seconds, or less than about 3.0 seconds, or even less than about 2.0 seconds. Excess first oxidant precursor, for example water and possible reaction by-products, can be removed using a vacuum generated by a pump system in fluid communication with the reaction chamber.
[0065] Subcycle 120 of FIG. 2 may continue with subprocess block 230, which includes a decision gate, which depends on the thickness of the hafnium oxide film deposited by the exemplary first subcycle 120. If the hafnium oxide film is of insufficient thickness for subsequent process steps, cyclic subcycle 120 may return to subprocess block 210 and contact the substrate with a hafnium vapor phase precursor (subprocess block 210) and a first oxidizer precursor (subprocess block 220). For example, a single deposition cycle, or unit deposition cycle, of first subcycle 120 may include contacting the substrate with a hafnium precursor, purging the reaction chamber, contacting the substrate with water, and purging the reaction chamber again. To deposit a hafnium oxide film to a desired thickness, subcycle 120 may be repeated one or more times until the desired thickness of the hafnium oxide film is deposited, at which point the exemplary first subcycle may be terminated via subprocess block 240.
[0066] It should be appreciated that in some embodiments of the present disclosure, the order of contacting the substrate with the hafnium precursor and the first oxidizer precursor may be such that the substrate is first contacted with the first oxidizer precursor and then with the hafnium precursor. Additionally, in some embodiments, the cyclical deposition subcycle 120 may include contacting the substrate with the hafnium precursor one or more times before contacting the substrate with the first oxidizer precursor one or more times. Additionally, in some embodiments, the cyclical deposition subcycle 120 may include contacting the substrate with the first oxidizer precursor one or more times before contacting the substrate with the hafnium precursor one or more times.
[0067] In some embodiments of the present disclosure, an exemplary cyclic first subcycle 120 may alternately contact a substrate with a hafnium precursor and a first oxidizer precursor to deposit a hafnium oxide film on a surface of the substrate by reaction of the hafnium precursor with the first oxidizer precursor, e.g., water.
[0068] In some embodiments of the present disclosure, the exemplary cyclic deposition subcycle 120 cannot be repeated, and only one deposition cycle of the deposition process can be performed. For example, the substrate can be contacted with a hafnium precursor and subsequently with a first oxidizer precursor to deposit a single monolayer or less than a single monolayer of a hafnium oxide film, i.e., in some embodiments, the hafnium oxide film comprises a single monolayer or less than a single monolayer. In such embodiments where one deposition cycle is utilized to deposit the hafnium oxide film, the hafnium oxide film can have a thickness of less than 5 angstroms, or less than 2 angstroms, or even less than 1 angstrom. In some embodiments, In some embodiments, the hafnium oxide film does not include a continuous film, but may include a plurality of separate regions of hafnium oxide disposed on the substrate.
[0069] In some embodiments of the present disclosure, the exemplary cyclical deposition subcycle 120 can be repeated one or more times to deposit a hafnium oxide film to a desired thickness. In some embodiments of the present disclosure, a unit deposition cycle of the first subcycle 120 can include contacting the substrate with a hafnium precursor, purging the reactants, contacting the substrate with a first oxidizer precursor, and purging the reaction chamber again. In some embodiments of the present disclosure, a unit deposition cycle of the subcycle 120 can be performed more than two times, or more than four times, or more than six times, or more than eight times, or more than ten times, or more than fifteen times, or more than twenty times. In some embodiments, the unit deposition cycle can be repeated to deposit a hafnium oxide film to a thickness of less than 3 nanometers, or less than 2 nanometers, or less than 1 nanometer, or less than 5 angstroms, or even less than 2 angstroms. In some embodiments, the hafnium oxide film does not include a continuous film, but rather includes multiple separate regions of hafnium oxide disposed on the substrate.
[0070] Upon completion of process block 120, i.e., the first subcycle, the cyclical deposition supercycle 150 (FIG. 1) may continue with process block 130, which includes depositing a lanthanum oxide film utilizing at least one deposition cycle of the second subcycle.
[0071] FIG. 3 shows the second subcycle 130 and its constituent subprocesses in more detail, and the second subcycle 130 may begin with subprocess block 310, which includes contacting or exposing a substrate with a lanthanum vapor phase precursor ("lanthanum precursor").
[0072] In some embodiments of the present disclosure, the lanthanum precursor may include an amidinate-based precursor, such as, for example, lanthanum formamidinate (La(FAMD)3), or tris(N,N'-diisopropylacetaminato)lanthanum (La(iPrAMD)3). In some embodiments, the lanthanum precursor may include a diketonate precursor, such as, for example, (La(THD)3). In some embodiments, the lanthanum precursor may include a Cp (cyclopentadienyl)-based precursor, such as, for example, tris(isopropyl-cyclopentadienyl)lanthanum (La(iPrCp)3). In some embodiments, the lanthanum precursor may include an amide-based chemistry, such as, for example, tris(bistrimethylsilylamido)lanthanum (La[N(SiMe3)2]3).
[0073] In some embodiments, the lanthanum precursor may include a hybrid combination of the above. In other embodiments, the lanthanum precursor may include a lanthanum precursor having a nitrogen bond, such as, for example, lanthanum amidinate. The amidinate compound may include delocalized electrons resulting in a bond between nitrogen and lanthanum. In other embodiments, the lanthanum precursor may include a lanthanum precursor having a carbon bond, such as, for example, lanthanum cyclopentadienyl. In such embodiments, the lanthanum precursor may include a delocalized electron that is considered to be a compound in which a bond between carbon and lanthanum is formed. In other embodiments, the lanthanum precursor may include a lanthanum precursor having both nitrogen and carbon bonds, such as, for example, lanthanum amidinate and lanthanum cyclopentadienyl.
[0074] In some embodiments of the present disclosure, the lanthanum precursor does not include a plasma-excited precursor, i.e., the lanthanum oxide film may be deposited without plasma excitation of the precursor, in other words, the lanthanum oxide film may be deposited in a plasma-free environment.
[0075] In some embodiments, contacting the substrate with the lanthanum gas-phase reactant may include pulsing the lanthanum precursor into the reaction chamber, followed by contacting the lanthanum precursor with the substrate for a time period of about 0.01 seconds to about 60 seconds, or about 0.05 seconds to about 10 seconds, or about 0.1 seconds to about 5.0 seconds. In addition, during the pulsing of the lanthanum precursor into the reaction chamber, the flow rate of the lanthanum precursor can be less than 2000 sccm, or less than 500 sccm, or even less than 100 sccm. In addition, during the pulsing of the lanthanum precursor onto the substrate, the flow rate of the lanthanum precursor can range from about 1 to 2000 sccm, or from about 5 to 1000 sccm, or from about 10 to about 500 sccm.
[0076] The exemplary subcycle 130 of FIG. 3 can be continued by purging the reaction chamber. For example, excess lanthanum gas-phase reactant and reaction by-products (if any) can be removed from the surface of the substrate, for example, by evacuating with an inert gas. In some embodiments of the present disclosure, the purging process can include a purge cycle, where the substrate surface is purged for a time period of less than about 5.0 seconds, or less than about 3.0 seconds, or even less than about 2.0 seconds. Excess lanthanum precursor and possible reaction by-products can be removed using a vacuum generated by a pump system in fluid communication with the reaction chamber.
[0077] Upon purging the reaction chamber with the purge cycle, the exemplary cyclical deposition subcycle 130 may continue with subprocess block 320, which includes contacting or exposing the substrate to a second oxidant precursor, particularly a second oxidant precursor comprising molecular oxygen (O2). In alternative embodiments, the second oxidant precursor may comprise water (H2O), hydrogen peroxide (H2O2), ozone (O3), or nitrogen oxides, such as nitric oxide (NO), nitrous oxide (N2O), or nitrogen dioxide (NO2). In some embodiments of the present disclosure, the oxidant precursor may comprise an organic alcohol, such as isopropyl alcohol.
[0078] In some embodiments of the present disclosure, the second oxidant precursor, e.g., molecular oxygen (O2), does not include a plasma-excited precursor, i.e., the lanthanum oxide film is deposited without plasma excitation of the precursor, in other words, the lanthanum oxide film is deposited in a plasma-free environment.
[0079] In embodiments in which the second oxidant precursor comprises molecular oxygen (O2), a high purity source of molecular oxygen (O2) may be utilized to substantially prevent unwanted contamination of the deposited lanthanum oxide film. Thus, in some embodiments, the molecular oxygen (O2) may have a purity of greater than 99.99%, or greater than 99.999%, or greater than 99.9999%, or greater than 99.99999%.
[0080] In some embodiments of the present disclosure, contacting the substrate with a second oxidant precursor, such as molecular oxygen (O2), may include pulsing the second oxidant precursor into the reaction chamber, followed by contacting the substrate with the second oxidant precursor for a time period of about 0.01 seconds to about 60 seconds, or about 0.05 seconds to about 10 seconds, or about 0.1 seconds to about 5.0 seconds. In addition, during the pulsing of the second oxidant precursor into the reaction chamber, the flow rate of the second oxidant precursor can be less than 2000 sccm, or less than 500 sccm, or even less than 100 sccm. In addition, during the pulsing of the second oxidant precursor onto the substrate, the flow rate of the second oxidant precursor can range from about 1 to about 2000 sccm, or from about 5 to about 1000 sccm, or from about 10 to about 500 sccm.
[0081] 3 can be continued by purging the reaction chamber. For example, excess second oxidant precursor and reaction by-products (if any) can be removed from the surface of the substrate, for example, by purging with an inert gas. In some embodiments of the present disclosure, the purging process may include a purge cycle. The substrate surface is purged for a time period of less than about 5.0 seconds, or less than about 3.0 seconds, or even less than about 2.0 seconds. Excess second oxidant precursor and possible reaction by-products may be removed using a vacuum generated by a pump system in fluid communication with the reaction chamber.
[0082] 3 may continue with sub-process block 330, which includes a decision gate that depends on the thickness of the lanthanum oxide film deposited by the exemplary second sub-cycle 130. If the lanthanum oxide film is of insufficient thickness for subsequent process steps, the cyclic sub-cycle 130 may return to sub-process block 310 and contact the substrate with a lanthanum precursor (sub-process block 310) and a second oxidant precursor, such as molecular oxygen (O2), (sub-process block 320). For example, a single deposition cycle, or unit deposition cycle, of the second sub-cycle 130 may include contacting the substrate with a lanthanum vapor phase precursor, purging the reaction chamber, contacting the substrate with a second oxidant precursor, and purging the reaction chamber again. To deposit a lanthanum oxide film to a desired thickness, subcycle 130 may be repeated one or more times until the desired thickness of lanthanum oxide film has been deposited on the substrate, at which point the exemplary second subcycle 130 may be terminated via sub-process block 340.
[0083] It should be understood that in some embodiments of the present disclosure, the order of contacting the substrate with the lanthanum precursor and the second oxidant precursor may be such that the substrate is first contacted with the second oxidant precursor and then with the lanthanum precursor. Additionally, in some embodiments, the second subcycle 130 of the cyclical deposition may include contacting the substrate with the lanthanum precursor one or more times before contacting the substrate with the second oxidant precursor one or more times. Additionally, in some embodiments, the second subcycle 130 of the cyclical deposition may include contacting the substrate with the second oxidant precursor one or more times before contacting the substrate with the lanthanum precursor one or more times.
[0084] In some embodiments of the present disclosure, an exemplary circulating subcycle 130 may alternately contact a substrate with a lanthanum precursor and a second oxidant precursor to deposit a lanthanum oxide film on the substrate by reaction between the lanthanum precursor and the second oxidant precursor.
[0085] In some embodiments of the present disclosure, the subcycle 130 of the exemplary cyclic deposition cannot be repeated, and only a unit cycle, i.e., one deposition cycle of the deposition process, can be performed. For example, the substrate can be contacted with a lanthanum precursor and subsequently with a second oxidant precursor to deposit a single monolayer or less than a single monolayer of a lanthanum oxide film, i.e., in some embodiments, the lanthanum oxide film comprises a single monolayer or less than a single monolayer. In such embodiments where one deposition cycle is utilized to deposit the lanthanum oxide film, the lanthanum oxide film can have a thickness of less than 5 angstroms, or less than 2 angstroms, or even less than 1 angstrom. In some embodiments, the lanthanum oxide film does not include a continuous film, but rather includes multiple separate regions of lanthanum oxide disposed on the substrate.
[0086] In some embodiments of the present disclosure, the exemplary cyclical deposition subcycle 130 can be repeated one or more times to deposit a lanthanum oxide film to a desired thickness. In some embodiments of the present disclosure, a unit deposition cycle of the second subcycle 130 can include contacting the substrate with a lanthanum precursor, purging the reactants, contacting the substrate with a second oxidant precursor, and purging the reaction chamber again. In some embodiments of the present disclosure, a unit deposition cycle of the subcycle 130 can be performed more than two times, or more than four times, or more than six times, or more than eight times, or more than ten times, or more than fifteen times, or more than twenty times, or even more. In some embodiments of the present disclosure, the unit deposition cycle of the subcycle 130 can be performed more than two times, or more than four times, or more than six times, or more than eight times, or more than ten times, or more than fifteen times, or more than twenty times, or even more. In some embodiments, the unit deposition cycle may be repeated to deposit the lanthanum oxide film to a thickness of less than 3 nanometers, or less than 2 nanometers, or less than 1 nanometer, or less than 5 Angstroms, or even less than 2 Angstroms. In some embodiments, the lanthanum oxide film does not include a continuous film, but rather can include multiple separate regions of lanthanum oxide disposed on the substrate.
[0087] Upon completion of the second subcycle 130, the exemplary cyclical deposition process 100 of FIG. 1 may continue with a process block 140 that includes a decision gate that depends on the total thickness of the hafnium lanthanum oxide film deposited by the first subcycle and the second subcycle. If the total thickness of the hafnium lanthanum oxide film is insufficient for the desired semiconductor device application, then the cyclical deposition supercycle 150 may be repeated by returning to process block 120 and depositing a hafnium oxide film utilizing at least one deposition cycle of the first subcycle, followed by depositing a lanthanum oxide film utilizing at least one deposition cycle of the second subcycle, utilizing process block 130, thereby depositing alternating layers of hafnium oxide and lanthanum oxide. Thus, the cyclical deposition supercycle 150 may be repeated one or more times until the desired thickness of the hafnium lanthanum oxide film is deposited on the substrate. Once a desired thickness of the lanthanum hafnium oxide film is achieved, the exemplary cyclic deposition process 100 terminates via process block 160, and the substrate having the lanthanum hafnium oxide film disposed thereon may be subjected to further semiconductor device fabrication processes.
[0088] It will be appreciated that in some embodiments of the present disclosure, the order of depositing hafnium oxide and lanthanum oxide films on a substrate may be such that the cyclical deposition supercycle 150 first deposits a lanthanum oxide film, followed by deposition of a hafnium oxide film, and then optionally repeating the lanthanum oxide deposition and hafnium oxide deposition steps to result in deposition of a hafnium lanthanum oxide film.
[0089] In some embodiments of the present disclosure, a method of depositing a hafnium lanthanum oxide film includes both a deposition process to deposit a hafnium oxide film or component (e.g., one or more first subcycles) and a deposition process to deposit a lanthanum oxide film or component (e.g., one or more second subcycles). For example, a method of depositing a hafnium lanthanum oxide film encompassed by the present disclosure includes a deposition process to deposit one or more hafnium oxide (HfO x) deposition subcycle and one or more lanthanum oxide (LaO x ) deposition sub-cycles.
[0090] In some embodiments, the specific properties of the deposited hafnium lanthanum oxide film are determined by the first sub-cycle (HfO x subcycle) and the number of second subcycles (LaO x The deposition rate can be controlled by varying the ratio of the number of first sub-cycles (HfO) performed per supercycle. In other words, the exemplary cyclic deposition process 100 can include a ratio of first sub-cycles performed to second sub-cycles performed per supercycle. Alternatively, the exemplary cyclic deposition process 100 can include a ratio of second sub-cycles performed to first sub-cycles performed per supercycle. In some embodiments, the deposition rate can be controlled by varying the ratio of the number of first sub-cycles (HfO) performed per supercycle. x The second subcycle (LaO x The ratio of (subcycles) is less than 0.50, or less than 0.40, or less than 0.30, or less than 0.20, or less than 0.15, or less than 0.10, or even less than 0.05.
[0091] In some embodiments, the first subcycle (LaO x One or more deposition parameters of a first subcycle (LaO) may vary from another first subcycle (LaO) within a given supercycle or between successive supercycles. x subcycle) may be different from that of the second subcycle (HfO x One or more deposition parameters of the sub-cycle are Within a given supercycle or between consecutive supercycles, another second subcycle (HfO xIn some embodiments, the deposition parameters of the first subcycle or the second subcycle may be substantially the same throughout the deposition process, i.e., over one or more successive supercycles.
[0092] In some embodiments of the present disclosure, the first sub-cycle (HfO x The second subcycle (LaO x The ratio of the lanthanum oxide deposition subcycles (subcycles) can be utilized to control the composition of the hafnium lanthanum oxide film, such as the lanthanum composition (atomic %) in the hafnium lanthanum oxide film. More specifically, Figure 4 shows X-ray photoelectron spectroscopy (XPS) data illustrating the change in lanthanum composition (atomic %) of several exemplary hafnium lanthanum oxide films related to the ratio of lanthanum oxide deposition subcycles to hafnium oxide deposition subcycles according to embodiments of the present disclosure. Examination of Figure 4 shows that the exemplary HfLaO x LaO present in the film x :HfO x It shows a clear relationship between the subcycle ratio and the lanthanum content (at.%). For example, LaO x :HfO x As the subcycle ratio decreases, the exemplary HfLaO x The lanthanum composition in the film is also reduced. Thus, embodiments of the present disclosure can provide a method to tightly control the composition of the deposited hafnium lanthanum oxide film. For example, hafnium lanthanum oxide films deposited according to embodiments of the present disclosure can have a lanthanum composition of less than 10 atomic %, or less than 7 atomic %, or less than 5 atomic %, or less than 3 atomic %, or less than 2 atomic %, or even 1 atomic % or less. In some embodiments, the lanthanum composition in hafnium lanthanum films deposited according to embodiments of the present disclosure can be between 0.5 atomic % and 3 atomic %, or between 1.0 atomic % and 2.5 atomic %.
[0093] In some embodiments of the present disclosure, the hafnium lanthanum oxide film may be deposited with a low concentration of impurities. For example, the hafnium lanthanum oxide film may have a lanthanum composition of less than 10 atomic %, or less than 5 atomic %, or less than 2 atomic %, or less than 1 atomic %, or less than 0.5 atomic %, or even less than 0.2 atomic %. In some embodiments, the impurities in the hafnium oxide film include, but are not limited to, carbon. For example, the hafnium lanthanum oxide film may have a carbon concentration of less than 10 atomic %, or less than 5 atomic %, or less than 2 atomic %, or less than 1 atomic %, or less than 0.5 atomic %, or even less than 0.2 atomic %.
[0094] In some embodiments, due to the reduced hygroscopicity of the deposition process enabled by utilizing two different oxidizer precursors for the hafnium oxide and lanthanum oxide deposition subcycles, the methods of the present disclosure may deposit hafnium lanthanum oxide films with greater compositional uniformity. In some embodiments of the present disclosure, the uniformity of lanthanum composition in hafnium lanthanum oxide films deposited according to embodiments of the present disclosure may be less than 2 atomic % (1 sigma), or less than 0.5 atomic % (1 sigma), or less than 0.2 atomic % (1 sigma), or less than 0.1 atomic % (1 sigma). In some embodiments of the present disclosure, the uniformity of lanthanum composition in hafnium lanthanum oxide films deposited according to embodiments of the present disclosure may be between 2 atomic % (1 sigma) and 0.1 atomic % (1 sigma). In embodiments disclosed herein, the atomic concentration of the elements may be determined using Rutherford backscattering (RBS) or x-ray photoelectron spectroscopy (XPS).
[0095] In some embodiments, the hafnium lanthanum oxide deposited according to the methods disclosed herein may comprise a nanolaminate film. That is, in some embodiments, separate and distinct layers may be visible within the hafnium lanthanum oxide film. For example, the hafnium lanthanum oxide film may comprise a nanolaminate that includes alternating layers of hafnium oxide and lanthanum oxide.
[0096] In some embodiments, the hafnium lanthanum oxide deposited according to the methods disclosed herein is not a nanolaminate film, i.e., in some embodiments, it is not a nanolaminate film. and different layers may not be visible in hafnium lanthanum oxide films deposited according to embodiments of the present disclosure. For example, uniform or substantially compositionally uniform hafnium lanthanum oxide films may be deposited by the methods disclosed herein. In some embodiments, the hafnium lanthanum oxide film comprises a substantially compositionally uniform tertiary hafnium lanthanum oxide film.
[0097] More specifically, in some embodiments of the present disclosure, the hafnium lanthanum oxide film deposited by the cyclic deposition process described herein may comprise a substantially compositionally uniform hafnium lanthanum oxide film. For example, the cyclic deposition process described herein may deposit alternating hafnium oxide and lanthanum oxide films (or vice versa). However, in some embodiments, the hafnium oxide and lanthanum oxide films may be deposited to a thickness of less than 5 angstroms, such that the alternating layers interdiffuse to result in a substantially compositionally uniform hafnium lanthanum oxide film, i.e., there is no discernible distinction between the hafnium oxide and lanthanum oxide regions of the hafnium lanthanum oxide film.
[0098] In some embodiments, the hafnium lanthanum oxide films of the present disclosure may be deposited to a thickness of 20 nanometers to 0.5 nanometers, or 15 nanometers to 1 nanometer, or 10 nanometers to 1.5 nanometers. In some embodiments, the hafnium lanthanum oxide films of the present disclosure may be deposited to a thickness of less than 20 nanometers, or less than 15 nanometers, or less than 10 nanometers, or less than 8 nanometers, or even less than 5 nanometers.
[0099] In some embodiments, the growth rate of the hafnium lanthanum oxide film may be from about 0.1 Å / cycle to about 5 Å / cycle, or from 0.2 Å / cycle to 3 Å / cycle, or from 0.3 Å / cycle to 2.0 Å / cycle. In some embodiments, the growth rate of the hafnium lanthanum oxide film is greater than 0.3 Å / cycle, or greater than 0.5 Å / cycle, or greater than 0.8 Å / cycle, or greater than 1.0 Å / cycle, or greater than 1.2 Å / cycle. In some embodiments, the growth rate of the hafnium lanthanum oxide film is less than 1.5 Å / cycle, or less than 1.0 Å / cycle, or less than 0.5 Å / cycle, or less than 0.3 Å / cycle, or less than 0.2 Å / cycle. The growth rates cited herein are based on the growth rate of HfO x and LaO x Based on the number of bonds in both subcycles, i.e., the cycle is HfO x or LaO x It means subcycle.
[0100] The hafnium lanthanum oxide film deposited by the cyclic deposition process disclosed herein may be a continuous film. In some embodiments, the hafnium lanthanum oxide film may be continuous with a thickness of less than 100 nanometers, or less than 60 nanometers, or less than 50 nanometers, or less than 40 nanometers, or less than 30 nanometers, or less than 20 nanometers, or less than 10 nanometers, or less than 5 nanometers, or less than 2 nanometers, or less than 1 nanometer, or even less than 0.5 nanometers. The continuity referred to herein can be physical continuity or electrical continuity. In some embodiments of the present disclosure, the thickness at which the hafnium lanthanum oxide film may be physically continuous may not be the same as the thickness at which the film is electrically continuous, and vice versa.
[0101] In some embodiments of the present disclosure, lanthanum hafnium oxide films may be formed on substrates that include high aspect ratio features, such as three-dimensional, non-planar substrates. In some embodiments, lanthanum hafnium oxide films may be deposited on substrates that include one or more trench and / or fin structures with a ratio of greater than 10:1, or greater than 20:1, or greater than 30:1, or even greater than 50:1. In such embodiments deposited on a substrate including topomorphic features, the step coverage of the deposited film may be greater than about 90%, or greater than about 95%, or greater than about 99%, or even substantially equal to 100%.
[0102] In some embodiments of the present disclosure, the hafnium lanthanum oxide film deposited according to embodiments of the present disclosure can be subjected to one or more deposition processes to further improve the quality of the film, for example, to improve crystallinity or to concentrate the film. Thus, in some embodiments, the method of the present disclosure can further include thermally annealing the hafnium lanthanum oxide film after deposition. For example, the hafnium lanthanum oxide film can be thermally annealed at a temperature below 800°C, or below 700°C, or below 600°C, or below 500°C, or below 400°C, or even below 300°C, or at a temperature between 300°C and 800°C, or between 350°C and 750°C, or between 400°C and 600°C.
[0103] In some embodiments of the present disclosure, the post-deposition thermal annealing of the hafnium lanthanum oxide film may be performed in a reaction chamber under a controlled environment. For example, the thermal annealing of the hafnium lanthanum oxide film may be performed in an inert gas atmosphere, such as, for example, a noble gas (e.g., Ar, He, etc.) or nitrogen. In a further example, the thermal annealing of the hafnium lanthanum oxide film may be performed in a hydrogen-containing atmosphere, such as, for example, forming gas (H2 / N2). In a further example, the thermal annealing of the hafnium lanthanum oxide film may be performed in an oxygen-containing atmosphere, such as, for example, molecular oxygen (O2), water (H2O), ozone (O3), hydrogen peroxide (H2O2), etc.
[0104] In some embodiments of the present disclosure, thermally annealing the hafnium lanthanum oxide film further comprises at least partially crystallizing the hafnium lanthanum oxide film. In some embodiments, thermally annealing the deposited hafnium lanthanum oxide film may form a hafnium lanthanum oxide film comprising a predominantly orthorhombic crystal structure. In some embodiments, thermally annealing the hafnium lanthanum oxide film further comprises forming a substantially single crystalline hafnium lanthanum oxide film. In some embodiments, the substantially single crystalline hafnium lanthanum oxide film comprises a predominantly orthorhombic crystal structure. In some embodiments of the present disclosure, the hafnium lanthanum oxide film may be deposited in an amorphous state, and thermally annealing the hafnium lanthanum oxide film may be formed from a crystalline hafnium lanthanum oxide film comprising LaHfO x It may provide controlled crystallization of the film.
[0105] FIG. 5 illustrates exemplary data showing the crystallization temperatures of several exemplary hafnium lanthanum oxide films deposited according to embodiments of the present disclosure with various deposition temperatures and increasing lanthanum composition (atomic %). Inspection of FIG. 5 reveals that the crystallization temperature of the exemplary hafnium lanthanum oxide films decreases with decreasing lanthanum composition (atomic %) of the exemplary hafnium lanthanum oxide films. As a non-limiting example, the hafnium lanthanum oxide films may include a composition of 1 atomic % or less of lanthanum with a crystallization temperature less than 600° C. is. As a further non-limiting example, the hafnium lanthanum oxide films may include a composition of 1 atomic % or less of lanthanum with a crystallization temperature less than approximately 450° C.
[0106] Inspection of Figure 5 reveals that the crystallization temperature of the exemplary hafnium lanthanum oxide film decreases with increasing deposition temperature of the hafnium lanthanum oxide film. As a non-limiting example, the hafnium lanthanum oxide film may include a composition of 1 atomic % or less of lanthanum deposited at a deposition temperature less than 200°C and a corresponding crystallization temperature at a temperature less than 650°C, less than 600°C, less than 550°C, or between 550°C and 650°C. As a further non-limiting example, the hafnium lanthanum oxide film may include a concentration of 1 atomic % or less of lanthanum deposited at a deposition temperature less than 300°C and a corresponding crystallization temperature less than 550°C, or less than 500°C, or less than 450°C, or between 450°C and 550°C.
[0107] FIG. 6 illustrates exemplary data showing the crystallization temperatures of several exemplary hafnium lanthanum oxide films with increasing lanthanum composition (atomic %) at various film thicknesses. Inspection of FIG. 6 reveals that as the lanthanum content in the hafnium lanthanum oxide film decreases, as previously discussed, the crystallization temperature generally decreases. Further inspection of FIG. 6 reveals that as the thickness of the hafnium lanthanum oxide film increases, the crystallization temperature also decreases. For example, in some embodiments, the hafnium lanthanum oxide film may have a lanthanum composition of approximately 1.5 atomic % to 3 atomic % with a corresponding crystallization temperature of approximately 540° C. to 680° C. In some embodiments, the hafnium lanthanum oxide film may have a lanthanum composition of less than 1.5 atomic %, a film thickness of less than 3 nanometers, and a crystallization temperature of less than 650° C. In some embodiments, the hafnium lanthanum oxide film may have a lanthanum composition of less than 1.5 atomic %, a film thickness of less than 5 nanometers, and a crystallization temperature of less than 600° C. In some embodiments, the hafnium lanthanum oxide films can have a lanthanum composition of less than 1.5 atomic %, a thickness of less than 7 nanometers, and a crystallization temperature of less than 560° C. In some embodiments, the hafnium lanthanum oxide films can have a lanthanum composition of less than 1.5 atomic %, a thickness of less than 10 nanometers, and a crystallization temperature of less than 550° C.
[0108] The exemplary embodiments of the present disclosure described above are merely examples of embodiments of the present invention, as defined by the appended claims and their legal equivalents, and therefore do not limit the scope of the present invention. Any equivalent embodiments are intended to be within the scope of the present invention. Indeed, various modifications of the present disclosure in addition to those shown and described herein may become apparent to those skilled in the art from the description, such as alternative useful combinations of the described elements. Such modifications and embodiments are also intended to fall within the scope of the appended claims.
Claims
1. 1. A method for depositing a lanthanum hafnium oxide film on a substrate by a cyclic deposition process in a reaction chamber, comprising: Depositing a hafnium oxide film on the substrate using at least one deposition cycle of a first sub-cycle of the cyclical deposition process, the one deposition cycle of the first sub-cycle comprising: contacting the substrate with a hafnium vapor phase precursor; The substrate is dissolved in water (H 2 and contacting the first oxidant precursor comprising: depositing a lanthanum oxide film on the substrate using at least one deposition cycle of a second sub-cycle of the cyclic deposition process, the one deposition cycle of the second sub-cycle comprising: contacting the substrate with a lanthanum vapor phase precursor; The substrate is subjected to molecular oxygen (O 2 and contacting said first oxidant precursor with a second oxidant precursor comprising:
2. 10. The method of claim 1, wherein the hafnium vapor phase precursor comprises at least one of a hafnium halide precursor or a hafnium organometallic precursor.
3. The hafnium halide precursor is hafnium tetrachloride (HfCl 4 ), hafnium tetraiodide (HfI 4 ), or hafnium tetrabromide (HfBr 4 3. The method of claim 2, further comprising at least one of:
4. The hafnium organometallic precursor is tetrakis(ethylmethylamido)hafnium (Hf(NEtMe) 4 ), tetrakis(dimethylamido)hafnium (Hf(NMe 2 ) 4 ), tetrakis(diethylamido)hafnium (Hf(NEt 2 ) 4 ), (tris(dimethylamido)cyclopentadienyl hafnium HfCp(NMe 2 ) 3 , or bis(methylcyclopentadienyl)methoxymethylhafnium (MeCp) 2 Hf(CH) 3 (O.C.H. 3 3. The method of claim 2, further comprising at least one of:
5. 2. The method of claim 1, wherein the lanthanum vapor phase precursor comprises at least one of a lanthanum amidinate or a lanthanum cyclopentadienyl compound.
6. 10. The method of claim 1, wherein the substrate is heated to a temperature between 100° C. and 400° C. prior to depositing the hafnium oxide film on the substrate.
7. 2. The method of claim 1, wherein the uniformity of lanthanum composition in the hafnium lanthanum oxide film is less than 2 atomic % (1 sigma).
8. 2. The method of claim 1, wherein the lanthanum hafnium oxide film has a lanthanum composition of less than 10 atomic percent.
9. 9. The method of claim 8, wherein the lanthanum hafnium oxide film has a lanthanum composition of 1 atomic % or less.
10. The method of claim 1 , wherein the lanthanum hafnium oxide film has a thickness of less than 20 nanometers.
11. The hafnium lanthanum oxide film has a thickness of 3 nanometers to 10 nanometers. The method according to claim 10.
12. The second oxidant precursor is molecular oxygen (O 2 ) having a purity of greater than 99.999%. 2 2. The method of claim 1 , comprising:
13. The method of claim 1 , wherein the first oxidant precursor comprises water having an electrical resistivity greater than 5 MΩ·cm.
14. The method of claim 1 , wherein the hafnium oxide film is deposited to a thickness of less than 3 nanometers.
15. The method of claim 1 , wherein the lanthanum oxide film is deposited to a thickness of less than 3 nanometers.
16. The method of claim 1 , wherein the lanthanum hafnium oxide film comprises a ternary lanthanum hafnium oxide film.
17. The method of claim 1 , wherein the lanthanum hafnium oxide film comprises a nanolaminate.
18. 2. The method of claim 1 , wherein the cyclical deposition process includes varying a ratio of a number of first sub-cycles performed to a number of second sub-cycles performed, and the ratio of second sub-cycles performed to first sub-cycles performed per supercycle is less than 0.
2.
19. 20. The method of claim 18, wherein the cyclical deposition process comprises a ratio of second sub-cycles performed to first sub-cycles that is less than 0.
1.
20. 10. The method of claim 1, wherein the lanthanum hafnium oxide film comprises a carbon content of less than 2 atomic percent.
21. 10. The method of claim 1, further comprising thermally annealing the hafnium lanthanum oxide film following deposition of the hafnium lanthanum oxide film.
22. 22. The method of claim 21, wherein the lanthanum hafnium oxide film is thermally annealed at a temperature less than 800°C.
23. 22. The method of claim 21, wherein thermally annealing the lanthanum hafnium oxide film further comprises at least partially crystallizing the lanthanum hafnium oxide film.
24. 24. The method of claim 23, wherein the lanthanum hafnium oxide film comprises a composition of less than or equal to 1 atomic % lanthanum having a crystallization temperature less than about 600°C.
25. 24. The method of claim 23, wherein the lanthanum hafnium oxide film comprises a composition of less than or equal to 1 atomic % lanthanum having a crystallization temperature less than about 450°C.
26. 24. The method of claim 23, wherein the at least partially crystallized lanthanum hafnium oxide film comprises a predominantly orthorhombic crystal structure.
27. The method of claim 1 , wherein the first sub-cycle and the second sub-cycle comprise an atomic layer deposition process.
28. 2. The method of claim 1 , wherein the cyclical deposition process comprises one or more repeated supercycles, each supercycle comprising depositing the hafnium oxide film on the substrate and depositing the lanthanum oxide film on the substrate.
29. 29. The method of claim 28, wherein the second subcycle is executed before the first subcycle within a unit supercycle.
Citation Information
Patent Citations
Method and apparatus for optical excitation of chemicals for atomic layer deposition of dielectric films
JP2009536267A
Capacitor with hafnium, lanthanum and oxygen mixed dielectric and method for fabricating the same
US20050139965A1
Atomic layer deposition of hafnium lanthanum oxides
US20100270626A1