Coated metal plate

The painted metal plate enhances photocatalytic effects by optimizing light reflection and incorporating chemical conversion layers, addressing inefficiencies in existing technologies to achieve cost-effective antiviral and sterilizing performance.

JP2024159944AActive Publication Date: 2024-11-08NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024148217
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-06-25
Filing Date
2024-08-30
Publication Date
2024-11-08
Estimated Expiration
2042-06-06

AI Technical Summary

Technical Problem

Existing technologies for imparting antiviral properties to metal surfaces, such as those using photocatalysts, do not efficiently utilize incident light for photocatalytic reactions, leading to suboptimal photocatalytic effects and high running costs due to the need for periodic drug application.

Method used

A painted metal plate design that includes a photocatalytic layer with compounds like anatase titanium oxide, optimized thickness, and reflective properties to enhance light utilization, combined with chemical conversion layers for improved adhesion and corrosion resistance, allowing for enhanced photocatalytic effects while controlling costs.

Benefits of technology

The design significantly improves photocatalytic activity, providing effective antiviral and sterilizing properties with reduced costs by efficiently reflecting and utilizing incident light, maintaining high specular gloss, and ensuring robust adhesion and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159944000001_ABST
    Figure 2024159944000001_ABST
Patent Text Reader

Abstract

To further increase a photocatalytic effect while reducing a cost.SOLUTION: A coated metal plate is a metal plate having a film layer on at least one surface thereof, has: a first film layer, as the film layer, located on an outermost surface of the film layer on the at least one surface of the metal plate and at least containing a compound with photocatalytic activity (excluding the cases of a rutile-type titanium dioxide and a crystalline zirconium titanate); and a second film layer located under the first film layer and composed of an inorganic component having at least one element of Si and Zr. The first film layer has an average thickness of 0.05 to 5.00 μm, the second film layer has an average thickness of 0.10 to 5.00 μm, and a total thickness from the surface of the metal plate to the outermost surface of the film layer is 15.00 μm or less. The second film layer further contains an inorganic component having at least one element of P and V, and regarding the coated metal plate, 60° specular glossiness is 80% or more.SELECTED DRAWING: Figure 1B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated metal sheet. [Background technology]

[0002] Due to the impact of the novel coronavirus (COVID-19) over the past few years, there is an increasing need to impart antiviral properties to various items, and businesses that apply antiviral agents to the surfaces of various items are thriving. Applying antiviral agents can be applied to existing structures, but there are problems with the high labor costs required for application and the lack of durability of the agents, which requires regular application and results in high running costs.

[0003] Meanwhile, there is a known technique for imparting antiviral properties to steel materials in advance, as shown in, for example, the following Patent Document 1. This technique uses a coated steel material as a base, and forms a protective layer and a photocatalyst layer in this order on top of the coated steel material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-131960 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, as a result of investigations by the present inventors, it was found that in the technology using a photocatalyst as disclosed in the above Patent Document 1, there is room for further improvement in the photocatalytic effect achieved by the photocatalyst layer.

[0006] Based on this knowledge, an object of the present invention is to provide a coated metal sheet that can further improve the photocatalytic effect while suppressing costs. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors conducted intensive research and found that, in the conventional technology disclosed in Patent Document 1, only the light incident on the steel material contributes to the manifestation of the photocatalytic effect among the light incident on the surface of the steel material. Based on this finding, further research was conducted and it was found that if the incident light could be reflected more efficiently on the surface of the metal plate so that the reflected light could also contribute to the manifestation of the photocatalytic effect, it would be possible to further improve the photocatalytic effect, leading to the completion of the present invention. The gist of the present invention, which was completed based on these findings, is as follows.

[0008] (1) A coated metal sheet having a coating layer on at least one surface of the metal sheet, the coating layer comprising a first coating layer located on the outermost surface of the coating layer on at least one surface of the metal sheet and containing at least a compound having photocatalytic activity (excluding cases where the compound having photocatalytic activity is rutile-type titanium oxide and where the compound having photocatalytic activity is crystalline zirconium titanate), and a second coating layer located below the first coating layer and made of an inorganic component having at least one element of Si or Zr, the first coating layer has an average thickness of 0.05 to 5.00 μm, the second coating layer has an average thickness of 0.10 to 5.00 μm, the total thickness from the surface of the metal sheet to the outermost surface of the coating layer is 15.00 μm or less, and the second coating layer further contains an inorganic component having at least one element of P or V, and the coated metal sheet satisfies the requirements of JIS A coated metal sheet having a 60° specular gloss of 80% or more as specified in Z8741:1997. (2) The coated metal sheet according to (1), wherein the first coating layer further contains at least one of the elements Si and Zr, and the total concentration of the elements is 5 to 50 mass% in terms of silica for Si and zirconia for Zr. (3) The coated metal sheet according to (1) or (2), wherein the ratio of the average thickness of the second coating layer to the average thickness of the first coating layer is 0.3 to 12.0. (4) The coated metal sheet according to (1) or (2), wherein the second coating layer contains at least one of zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, sodium zirconium carbonate, or ammonium zirconium carbonate as the inorganic component containing Zr. (5) The coated metal sheet according to (1) or (2), wherein the second coating layer contains, as the inorganic component containing P, at least one of phosphoric acid, orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, tetraphosphoric acid and salts thereof, or ammonium dihydrogen phosphate. (6) The coated metal sheet according to (1) or (2), wherein the second coating layer contains, as the inorganic component containing V, at least one of ammonium metavanadate (V), potassium metavanadate (V), sodium metavanadate (V), or vanadyl sulfate (IV). (7) The coated metal sheet according to (1) or (2), wherein the total thickness from the surface of the metal sheet to the outermost surface of the first coating layer is 10.00 μm or less. (8) The coated metal sheet according to (1) or (2), wherein the compound having photocatalytic activity is anatase type titanium oxide. (9) The coated metal sheet according to (8), wherein the anatase type titanium oxide is a metal-supported type titanium oxide supported on at least one of Cu and Fe. (10) The coated metal sheet according to (8), wherein the concentration of the anatase type titanium oxide in the first coating layer is 50 to 95 mass % in terms of titania. (11) The coated metal sheet according to (8), wherein the anatase type titanium oxide has an average particle size of 5 to 200 nm. (12) The coated metal sheet according to (1) or (2), wherein the metal sheet is a zinc-aluminum alloy-plated steel sheet, a zinc-aluminum-magnesium alloy-plated steel sheet, an aluminum-plated steel sheet, a zinc-nickel alloy-plated steel sheet, a zinc-iron alloy-plated steel sheet, an aluminum sheet, or a stainless steel sheet. (13) A coated metal sheet according to (1) or (2), in which a hairline is present on the surface of the metal sheet along the rolling direction of the metal sheet. (14) The coated metal sheet according to (1) or (2), wherein a spangle pattern is present on the surface of the metal sheet. Effect of the Invention

[0009] As described above, according to the present invention, it is possible to further improve the photocatalytic effect while suppressing costs. [Brief description of the drawings]

[0010] [Figure 1A] 1 is an explanatory diagram showing a schematic example of a structure of a coated metal sheet according to an embodiment of the present invention; [Figure 1B] FIG. 4 is an explanatory diagram showing a schematic diagram of another example of the structure of the coated metal plate according to the embodiment. [Figure 1C] FIG. 4 is an explanatory diagram showing a schematic diagram of another example of the structure of the coated metal plate according to the embodiment. [Figure 2A] FIG. 4 is an explanatory diagram showing a schematic diagram of another example of the structure of the coated metal plate according to the embodiment. [Figure 2B] FIG. 4 is an explanatory diagram showing a schematic diagram of another example of the structure of the coated metal plate according to the embodiment. [Diagram 3] FIG. 2 is an explanatory diagram for explaining a coated metal plate according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.

[0012] (About painted metal sheets) <Structure of painted metal plate> Hereinafter, first, the structure of a coated metal sheet according to an embodiment of the present invention will be described with reference to Figures 1A to 2B. Figure 1A is an explanatory diagram that shows a schematic example of the structure of a coated metal sheet according to this embodiment. Figures 1B to 2B are explanatory diagrams that show a schematic example of another example of the structure of a coated metal sheet according to this embodiment.

[0013] As shown in Fig. 1A, the coated metal sheet 1 according to the embodiment of the present invention has a coating layer on at least one surface of the metal sheet, and has at least a metal sheet 10 as a base material and a photocatalytic layer 20 as an example of a first coating layer. It may be considered that a hard resin substrate such as melamine resin may be used as the substrate instead of a metal sheet. However, it is important to use a substrate that can be subjected to various processes, and in this embodiment, a metal sheet is used as the substrate.

[0014] [Regarding metal plate 10] In the coated metal sheet 1 according to this embodiment, various metal sheets can be used as the base material, that is, the metal sheet 10. Examples of such metal sheets include zinc-plated steel sheets, zinc-aluminum alloy-plated steel sheets, zinc-aluminum-magnesium alloy-plated steel sheets, aluminum-plated steel sheets, zinc-nickel alloy-plated steel sheets, zinc-iron alloy-plated steel sheets, aluminum sheets, stainless steel sheets, and the like.

[0015] By using such a metal sheet, it becomes possible to efficiently reflect light (particularly light in the ultraviolet to visible light range) incident on the coated metal sheet 1 on the surface of the metal sheet 10. As a result, in the coated metal sheet 1 according to this embodiment, it becomes possible to utilize the reflected light reflected on the surface of the metal sheet 10 for a photocatalytic reaction, as described later. Among the above metal sheets, zinc-aluminum-magnesium alloy plated steel sheets, stainless steel sheets, aluminum plated steel sheets, zinc plated steel sheets, zinc-aluminum alloy plated steel sheets, etc. are particularly suitable because they can efficiently reflect incident light. In addition, those having designs such as hairlines or spangle patterns on the plated surface are suitable because they can be used as exterior parts.

[0016] Here, the thickness of the metal plate 10 as described above is not particularly limited, and may be set appropriately depending on the mechanical strength (e.g., tensile strength, etc.) and processability required for the painted metal plate 1 in this embodiment.

[0017] Furthermore, the surface of the metal sheet 10 (when a metal sheet having various platings is used as the metal sheet 10, the surface of the plating) may have various patterns such as a hairline pattern or a spangle pattern along the rolling direction of the metal sheet. The provision of such patterns makes it possible to further improve the design of the coated metal sheet 1. Furthermore, the design processing for providing such patterns on the surface of the metal sheet 10 itself contributes to further improving the 60° specular gloss, as described below.

[0018] For example, let us focus on a plated metal sheet 10. In general, when plating the surface of a metal substrate, an electroplating method or a hot-dip plating method can be adopted. Depending on the plating method adopted, fine particles are generated on the plated surface, and as a result, the glossiness of the surface of the plated metal sheet 10 (i.e., the glossiness of the plated surface) may decrease. However, by applying a hairline finish to such a plated surface, the plated surface is scraped, and the light reflectance of the plated surface is improved, making it possible to improve the glossiness of the surface. In addition, as a result of plating to form a spangle pattern, the crystal orientation of the plating that is more reflective of light appears on the surface, and the light reflectance of the plated surface is improved, making it possible to improve the glossiness of the surface.

[0019] As described in detail below, in the coated metal sheet 1, the thickness of the photocatalytic layer 20 as the first coating layer and the total thickness from the surface of the metal sheet 10 to the outermost surface of the photocatalytic layer 20 as the first coating layer are controlled to be in a specific state. In addition, by applying a design process such as the hairline pattern or spangle pattern described above, the design process also acts to further improve the 60° specular gloss as described below. As a method for forming such a pattern, various known processing methods can be appropriately used.

[0020] [About the photocatalyst layer 20] In the coated metal plate 1 according to the present embodiment, the photocatalyst layer 20 as an example of the first coating layer is a layer located on the outermost surface of the coating layer on at least one side of the metal plate 10 as shown in FIG. 1A, and contains at least a compound having photocatalytic activity (hereinafter, sometimes abbreviated as "photocatalytic compound"). When the photocatalyst layer 20 contains a compound having photocatalytic activity, the compound having photocatalytic activity causes a photocatalytic reaction by light (particularly, light in the ultraviolet to visible light range) incident on the photocatalyst layer 20. As a result, various photocatalytic effects, including an antiviral effect and a bactericidal effect, are expressed in the photocatalyst layer 20 according to the present embodiment. As a result, the coated metal plate 1 according to the present embodiment can realize various properties, including an antiviral effect and a bactericidal effect.

[0021] Compounds having such photocatalytic activity include compounds that exhibit photocatalytic activity mainly by reacting with light in the ultraviolet band (more specifically, by being excited by light in the ultraviolet band), and compounds that exhibit photocatalytic activity mainly by reacting with light in the visible band (more specifically, by being excited by light in the visible band).

[0022] Examples of compounds that react with ultraviolet light to exhibit photocatalytic activity include metal oxides such as titanium oxide (more specifically, anatase-type titanium oxide), zinc oxide, cerium oxide, tin oxide, bismuth oxide, zirconium oxide, tungsten oxide, chromium oxide, molybdenum oxide, iron oxide, nickel oxide, ruthenium oxide, cobalt oxide, copper oxide, manganese oxide, germanium oxide, lead oxide, cadmium oxide, vanadium oxide, niobium oxide, tantalum oxide, rhodium oxide, and rhenium oxide, metal sulfides such as cadmium sulfide and zinc sulfide, and titanium compounds such as strontium titanate and barium titanate. Among these, anatase-type titanium oxide, zinc oxide, tin oxide, zirconium oxide, tungsten oxide, iron oxide, niobium oxide, and strontium titanate are particularly preferably used as compounds that react with ultraviolet light to exhibit photocatalytic activity, and anatase-type titanium oxide is more preferably used.

[0023] Examples of compounds that react with light in the visible light range to exhibit photocatalytic activity include metal-supported titanium oxide (more specifically, anatase-type titanium oxide) supported on at least one of Cu and Fe, anatase-type titanium oxide supported on Cr, V, Mn, Ni, and Pt, anatase-type titanium oxide doped with anions such as nitrogen and sulfur, and a solid solution of AgNbO3 and SrTiO3. Among these, anatase-type titanium oxide supported on at least one of Cu and Fe is particularly preferably used.

[0024] Among these photocatalytic compounds, the average particle size (primary particle size) of anatase type titanium oxide (including those in a metal-supported state) is preferably 5 nm or more. By making the average particle size (primary particle size) of anatase type titanium oxide 5 nm or more, it becomes possible to disperse anatase type titanium oxide more uniformly in the photocatalytic layer 20. The average particle size (primary particle size) of anatase type titanium oxide is more preferably 20 nm or more. In addition, the average particle size (primary particle size) of anatase type titanium oxide (including those in a metal-supported state) is preferably 200 nm or less. By making the average particle size (primary particle size) of anatase type titanium oxide 200 nm or less, it becomes possible to disperse anatase type titanium oxide more uniformly in the photocatalytic layer 20 while suppressing excessive aggregation of anatase type titanium oxide in the photocatalytic layer 20. The average particle size (primary particle size) of anatase type titanium oxide is more preferably 100 nm or less.

[0025] Here, the average particle size of the anatase type titanium oxide can be measured, for example, by a dynamic light scattering method using a laser beam. This method makes it possible to easily obtain highly accurate measured values. However, when the anatase type titanium oxide particles are aggregated to a certain extent, it is possible to measure the size of the aggregates (aggregated particle size), so it is preferable to also directly confirm the primary particle size by a transmission electron microscope (TEM). When the presence of aggregated particles is confirmed as a result of TEM observation, it is preferable to change the dispersion conditions and measure again by a dynamic light scattering method. In addition, when it is difficult to completely disperse the particles to the level of primary particles, it is also possible to use the size of the primary particles observed and measured by TEM as the primary particle size. In this case, the inventor's experience has shown that a value representative of the entire particles can be obtained by measuring approximately 100 or more particles selected at random.

[0026] In addition, when measuring the average particle size of anatase-type titanium oxide contained in the photocatalyst layer 20 of a coated metal plate 1 on which a photocatalyst layer 20 has already been formed, the following procedure may be followed. That is, the cross section of the photocatalyst layer 20 cut along the thickness direction can be observed or analyzed using a transmission electron microscope (TEM). By using a TEM, the primary particle size of the photocatalyst compound can be measured. Furthermore, by performing an EDS analysis in combination with a TEM, the elements contained in the photocatalyst compound can be measured. Furthermore, the crystal structure of the photocatalyst compound (for example, whether it is anatase-type or rutile-type in the case of titanium oxide) can be known by electron beam diffraction. In the inventor's experience, it has been found that a value representative of the entire particles can be obtained by measuring approximately 100 or more particles selected at random.

[0027] Here, the concentration of anatase type titanium oxide (including that in a state in which a metal is supported) in the photocatalyst layer 20 is preferably 50% by mass or more in titania conversion. When the concentration of anatase type titanium oxide in the photocatalyst layer 20 is 50% by mass or more, it is possible to reliably exhibit various photocatalytic effects including an antiviral effect. The concentration of anatase type titanium oxide in the photocatalyst layer 20 is more preferably 60% by mass or more in titania conversion. In addition, the concentration of anatase type titanium oxide (including that in a state in which a metal is supported) in the photocatalyst layer 20 is preferably 95% by mass or less in titania conversion. When the concentration of anatase type titanium oxide in the photocatalyst layer 20 is 95% by mass or less, it is possible to suppress an increase in manufacturing costs while exhibiting various photocatalytic effects including an antiviral effect. The concentration of anatase type titanium oxide in the photocatalyst layer 20 is more preferably 80% by mass or less in titania conversion.

[0028] Similarly, photocatalytic compounds other than anatase type titanium oxide preferably have an average particle size of 5 to 200 nm and a concentration of 50 to 95% by mass.

[0029] In addition, the photocatalytic compounds represented by the above-mentioned anatase type titanium oxide can be used, if necessary, in the form of not only particulate substances but also sol-like substances that cannot be considered particulate, substances produced by heating metal complexes, and the like.

[0030] The photocatalyst layer 20 further contains at least one of Si and Zr, and the total concentration of the elements is preferably 5% by mass or more in terms of silica for Si and zirconia for Zr. In other words, the photocatalyst layer 20 is an inorganic coating having a skeleton of inorganic components in a three-dimensional mesh structure containing at least one of Si and Zr, and impurities in some cases, and the total concentration of at least one of Si and Zr is preferably 5% by mass or more in terms of silica for Si and zirconia for Zr. By containing at least one of Si and Zr at the above concentration, it is possible to realize a photocatalyst layer 20 with better corrosion resistance. The total content of at least one of Si and Zr is more preferably 10% by mass or more. The photocatalyst layer 20 further contains at least one of the elements Si and Zr, and the total concentration of such elements is preferably 50 mass% or less in terms of silica for Si and zirconia for Zr. By containing at least one of the elements Si and Zr at the above concentrations, it is possible to realize a photocatalyst layer 20 with better corrosion resistance. The total content of at least one of the elements Si and Zr is more preferably 40 mass% or less. Here, the contained Si or Zr is preferably an inorganic component that is excellent in light transmittance and is less susceptible to decomposition by photocatalysis. Examples of such inorganic components containing Si and Zr include silica and zirconia.

[0031] The photocatalyst layer 20 containing the above-mentioned photocatalyst compound may contain an antibacterial agent or an adsorbent such as activated carbon or zeolite, if necessary, within a range that does not impair the effects of the present invention.

[0032] The average thickness d1 of the photocatalyst layer 20 (in the case of the layer structure shown in FIG. 1A ) is the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalyst layer 20 (which can also be regarded as the outermost surface of the coating layer). T ) is 0.05 μm or more. If the average thickness d1 of the photocatalyst layer 20 is less than 0.05 μm, it is difficult to uniformly form the photocatalyst layer 20 as described above, and the obtained photocatalytic effect will be uneven, which is not preferable. By setting the average thickness d1 to 0.05 μm or more, it is possible to uniformly achieve the desired photocatalytic effect throughout the photocatalyst layer 20. On the other hand, the average thickness d1 of the photocatalyst layer 20 (in the case of the layer structure shown in FIG. 1A, the total thickness d T ) is 5.00 μm or less. When the average thickness d1 of the photocatalyst layer 20 exceeds 5.00 μm, the obtained photocatalytic effect is saturated while the manufacturing cost increases, which is not preferable. In addition, since the photocatalyst layer is an inorganic film, its processability decreases. By setting the average thickness d1 to 5.00 μm or less, it is possible to suppress the increase in manufacturing cost and the decrease in processability, while uniformly expressing the desired photocatalytic effect throughout the photocatalyst layer 20.

[0033] Usually, there is a certain probability that light passes through the photocatalyst layer 20 without hitting the photocatalyst compound. Conventionally, such light that does not interact with the photocatalyst compound is light that does not provide a photocatalytic effect. In this embodiment, such light is reflected on the surface of the metal plate 10, thereby making it possible to increase the probability that the light incident on the photocatalyst layer 20 will hit the photocatalyst compound. This makes it possible to further improve the photocatalytic effect in this embodiment. In the case of the layer structure shown in FIG. 1A, the total thickness d from the surface of the metal plate 10 to the outermost surface of the photocatalyst layer 20 is 100 μm. T Naturally, since the thickness is 15.00 μm or less, it is possible to utilize the reflected light from the surface of the metal plate 10 (in other words, the interface between the metal plate 10 and the photocatalytic layer 20) for the photocatalytic reaction caused by the photocatalytic compound, thereby making it possible to further improve the photocatalytic effect while suppressing costs.

[0034] The average thickness d1 of the photocatalyst layer 20 is preferably 0.10 μm or more, more preferably 0.15 μm or more. The average thickness d1 of the photocatalyst layer 20 is preferably 2.00 μm or less, more preferably 1.00 μm or less.

[0035] [60° specular gloss] In the coated metal sheet 1 having the layer structure shown in FIG. 1A, the 60° specular gloss of the coated metal sheet 1 measured from the side where the photocatalyst layer 20 is provided is 80% or more, as defined in JIS Z8741:1997, due to the reflection of light by the metal sheet 10 and the photocatalyst layer 20 having the average thickness d1 as described above. In other words, the coated metal sheet 1 according to this embodiment has a 60° specular gloss of 80% or more as described above, which makes it possible to effectively utilize the reflected light generated at the interface between the metal sheet 10 and the photocatalyst layer 20, and exhibits excellent antiviral performance. Note that light that collides with the photocatalyst is not detected as reflected light, but in the film structure of the present invention, such light is only a small part of the whole. Therefore, even when the reduction due to the photocatalyst is taken into consideration, it can be determined that the coated metal sheet 1 has excellent antiviral properties by satisfying that the 60° specular gloss of 80% or more as defined in the present invention. In the coated metal sheet 1 according to this embodiment, the 60° specular gloss is preferably 90% or more, more preferably 130% or more. Although the upper limit of the 60° specular gloss is not particularly specified, it is difficult to exceed 200%, and this value is considered to be the practical upper limit. The 60° specular gloss can be measured using a gloss meter conforming to the above JIS standard.

[0036] <Modification> The coated metal sheet 1 according to this embodiment, which has a layer structure as shown in Fig. 1A, may have an additional coating layer functioning as a chemical conversion coating layer between the metal sheet 10 and the photocatalyst layer 20. By providing a chemical conversion coating layer between the metal sheet 10 and the photocatalyst layer 20, it is possible to further improve the adhesion between the metal sheet 10 and the photocatalyst layer 20. Furthermore, it is also possible to further improve the corrosion resistance, etc. of the coated metal sheet 1 according to this embodiment.

[0037] In the case where a chemical conversion coating layer is further provided in the coated metal sheet 1 according to this embodiment, it is preferable to realize the following two types of layer configurations according to the types of compound components that constitute the chemical conversion coating layer. Hereinafter, the layer configuration of the coated metal sheet having the chemical conversion coating layer will be described in detail with reference to Figs. 1B to 3. 1B to 2 are explanatory diagrams that show a schematic diagram of another example of the structure of the coated metal sheet according to the present embodiment. FIG 3 is an explanatory diagram for explaining the coated metal sheet according to the present embodiment.

[0038] [When applying an inorganic conversion coating layer] 1B and 1C are schematic diagrams showing the layer structure of a coated metal sheet 1 when an inorganic chemical conversion treatment coating layer made of an inorganic component is provided as the chemical conversion treatment coating layer. In such a case, the coated metal sheet 1 according to this embodiment has an inorganic chemical conversion coating layer 30, which is an example of a second coating layer, between the metal sheet 10 and the photocatalyst layer 20 as described above.

[0039] Photocatalytic compounds such as anatase titanium oxide have extremely excellent oxidizing properties, so when a coating layer is provided below the layer containing the photocatalytic compound, a protective layer is often formed to protect the coating layer. However, as described below, by forming the chemical conversion coating layer from inorganic components, it becomes possible to arrange the chemical conversion coating layer without providing a protective layer.

[0040] The inorganic chemical conversion coating layer 30 is formed by chemical conversion treatment after removing impurities such as oil and surface oxides adhering to the surface of the metal sheet 10 by a known degreasing process and cleaning process. The inorganic chemical conversion coating layer 30 is preferably made of an inorganic component having at least one of the elements Si and Zr. The inorganic chemical conversion coating layer 30 may further contain an inorganic component having at least one of the elements P and V.

[0041] The inorganic chemical conversion coating layer 30 contains inorganic components having the elements as described above, which improves the film-forming properties after application of the chemical conversion treatment liquid, the barrier properties (density) of the coating against corrosive factors such as moisture and corrosive ions, and the adhesion of the coating to the metal sheet surface, thereby contributing to improving the corrosion resistance of the coating.

[0042] Here, examples of inorganic components containing Si include γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, etc. Examples of inorganic components containing Zr include zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, sodium zirconium carbonate, ammonium zirconium carbonate, etc.

[0043] Examples of inorganic components containing P include phosphoric acids such as phosphoric acid, orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, tetraphosphoric acid, and salts thereof, ammonium dihydrogen phosphate, etc. Examples of inorganic components containing V include ammonium metavanadate (V), potassium metavanadate (V), sodium metavanadate (V), vanadyl sulfate (IV), etc.

[0044] In the inorganic conversion coating layer 30 according to this embodiment, the various inorganic components as described above can be used alone or in combination. The contents of the various inorganic components as described above can also be appropriately adjusted.

[0045] The average thickness d2 of the inorganic chemical conversion coating layer 30 is preferably 0.10 μm or more, and more preferably 0.20 μm or more. This allows the inorganic chemical conversion coating layer 30 to be uniformly formed on the surface of the metal sheet 10 while stably achieving the various effects achieved by providing the above-mentioned chemical conversion coating layer. The average thickness d2 of the inorganic chemical conversion coating layer 30 is preferably 5.00 μm or less, and more preferably 1.00 μm or less. This allows the inorganic chemical conversion coating layer 30 to be uniformly formed on the surface of the metal sheet 10 while stably achieving the various effects achieved by providing the above-mentioned chemical conversion coating layer.

[0046] In addition, the ratio (d2 / d1) of the average thickness d2 of the inorganic chemical conversion coating layer 30 to the average thickness d1 of the photocatalyst layer 20 is preferably 0.3 or more, and more preferably 0.5 or more. This makes it possible to further improve the processing adhesion. In addition, the ratio (d2 / d1) of the average thickness d2 of the inorganic chemical conversion coating layer 30 to the average thickness d1 of the photocatalyst layer 20 is preferably 12.0 or less, and more preferably 5.0 or less. This makes it possible to further improve the processing adhesion.

[0047] Furthermore, as shown in FIG. 1C, the coated metal sheet 1 according to this embodiment may further have various known layers between the photocatalyst layer 20 and the inorganic chemical conversion coating layer 30, including, for example, a colored layer containing various color pigments.

[0048] Here, even in the cases shown in FIG. 1B and FIG. 1C, the total thickness d from the surface of the metal plate 10 to the outermost surface of the coating layer (which is also the outermost surface of the photocatalyst layer 20) T(=d1+d2+α) is set to 15.00 μm or less. As a result, as shown in FIG. 3, it becomes possible to utilize the reflected light, which is the incident light reflected on the surface of the metal plate 10 (in other words, the interface between the metal plate 10 and the photocatalytic layer 20), for the photocatalytic reaction by the photocatalytic compound, thereby making it possible to further improve the photocatalytic effect while suppressing an increase in costs. The total thickness d from the surface of the metal plate 10 to the outermost surface of the coating layer is T (=d1+d2+α) is preferably 10.00 μm or less, and more preferably 7.00 μm or less.

[0049] 1B and 1C, the 60° specular gloss of the coated metal sheet 1 measured from the side on which the photocatalytic layer 20 is provided is 80% or more as specified in JIS Z8741:1997. T If the reflectance is 15.00 μm or less and the 60° specular gloss is 80% or more, it can be considered that the reflected light of the incident light reflected on the surface of the metal plate 10 is utilized for the photocatalytic reaction by the photocatalytic compound.

[0050] [When an organic conversion coating layer is applied] 2A and 2B are schematic diagrams showing the layer structure of a coated metal sheet 1 when an organic chemical conversion treatment film layer containing an organic component is provided as the chemical conversion treatment film layer. In such a case, the painted metal sheet 1 of this embodiment has, between the metal sheet 10 and the photocatalyst layer 20 as described above, an organic chemical conversion coating layer 40 as an example of a third coating layer, and a protective layer 50 as an example of a fourth coating layer.

[0051] <Organic conversion coating layer 40> The organic chemical conversion coating layer 40 is a layer located below the photocatalyst layer 20 (more specifically, on the surface of the metal plate 10), and is formed by chemical conversion treatment after impurities such as oil and surface oxides adhering to the surface of the metal plate 10 are removed by known degreasing and cleaning processes.

[0052] The organic chemical conversion coating layer 40 according to this embodiment may contain, for example, any one or more selected from the group consisting of resins, silane coupling agents, zirconium compounds, silica, phosphoric acid and its salts, fluorides, vanadium compounds, and tannin or tannic acid. The inclusion of these substances further improves the film-forming properties after application of the chemical conversion coating solution, the barrier properties (density) of the coating against corrosive factors such as moisture and corrosive ions, and the coating adhesion to the surface of the metal sheet, thereby contributing to raising the corrosion resistance of the coating.

[0053] In particular, when the organic chemical conversion coating layer 40 contains one or more of a silane coupling agent or a zirconium compound, a cross-linked structure is formed within the organic chemical conversion coating layer 40, and the bond with the metal sheet surface is also strengthened, making it possible to further improve the adhesion and barrier properties of the coating.

[0054] Furthermore, when the organic chemical conversion coating layer 40 contains one or more of silica, phosphoric acid and its salts, fluorides, and vanadium compounds, these function as inhibitors and form a precipitated film or a passive film on the surface of the metal sheet, thereby making it possible to further improve corrosion resistance.

[0055] In the following, the components that may be contained in the organic chemical conversion coating layer 40 as described above will be described in detail with reference to examples.

[0056] [resin] As the resin, for example, known organic resins such as polyester resin, polyurethane resin, epoxy resin, phenol resin, acrylic resin, polyolefin resin, etc. can be used. In order to further increase the adhesion to the metal plate, it is preferable to use at least one resin having a forced site or a polar functional group in the molecular chain (polyester resin, urethane resin, epoxy resin, acrylic resin, etc.). The resin may be used alone or in combination of two or more kinds.

[0057] The resin content in the organic chemical conversion coating layer 40 is, for example, preferably 0 mass % or more, and more preferably 1 mass % or more, relative to the solid content of the coating. This can improve corrosion resistance. Also, the resin content in the organic chemical conversion coating layer 40 is, for example, preferably 85 mass % or less, more preferably 60 mass % or less, and even more preferably 40 mass % or less, relative to the solid content of the coating. By setting the resin content to 85 mass % or less, the corrosion resistance of the coating can be improved while ensuring the performance required of the coating other than corrosion resistance.

[0058] [Silane coupling agents] Examples of the silane coupling agent include γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltriethoxy ...triethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysil Dipropylmethyldiethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltriethoxy Silane, gamma-glycidoxypropylmethyldiethoxysilane, gamma-mercaptopropyltrimethoxysilane, gamma-mercaptopropylmethyldimethoxysilane, gamma-mercaptopropyltriethoxysilane, gamma-mercaptopropylmethyldiethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, vinyltriacetoxysilane, gamma-chloropropyltrimethoxysilane, gamma-chloropropylmethyldimethoxysilane, gamma-chloropropyltriethoxysilane, gamma-chloropropyl dimethyldiethoxysilane, hexamethyldisilazane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-anilinopropyltriethoxysilane, γ-anilinopropylmethyldiethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyltriethoxysilane, vinylmethyldiethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldimethoxysilyl)propyl]ammonium chloride,Examples of suitable silane coupling agents include octadecyldimethyl[3-(triethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldiethoxysilyl)propyl]ammonium chloride, γ-chloropropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, and trimethylchlorosilane. The amount of silane coupling agent added in the chemical conversion coating agent for forming the organic chemical conversion coating layer 40 can be, for example, 2 to 80 g / L. By adding 2 g / L or more of the silane coupling agent, it is possible to improve the adhesion to the metal sheet surface and improve the processing adhesion of the coating film. In addition, by adding 80 g / L or less of the silane coupling agent, it is possible to maintain the cohesive force of the chemical conversion coating film and improve the processing adhesion of the coating film. The silane coupling agents exemplified above may be used alone or in combination of two or more.

[0059] [Zirconium compounds] Examples of the zirconium compound include zirconium normal propylate, zirconium normal butylate, zirconium tetraacetylacetonate, zirconium monoacetylacetonate, zirconium bisacetylacetonate, zirconium monoethylacetoacetate, zirconium acetylacetonate bisethylacetoacetate, zirconium acetate, zirconium monostearate, zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate. The amount of the zirconium compound added to the chemical conversion coating agent for forming the organic chemical conversion coating layer 40 can be, for example, 2 to 80 g / L. By setting the amount of the zirconium compound to 2 g / L or more, it is possible to improve the adhesion to the metal sheet surface and improve the processing adhesion of the coating film. In addition, by setting the amount of the zirconium compound to 80 g / L or less, it is possible to maintain the cohesive force of the chemical conversion coating film and improve the processing adhesion of the coating film. Such zirconium compounds may be used alone or in combination of two or more kinds.

[0060] [silica] As the silica, for example, commercially available silica gel such as "Snowtex N", "Snowtex C", "Snowtex UP", and "Snowtex PS" manufactured by Nissan Chemical Industries, Ltd., "Adelite AT-20Q" manufactured by ADEKA Corporation, or powdered silica such as Aerosil #300 manufactured by Nippon Aerosil Co., Ltd. can be used. The silica can be appropriately selected according to the required performance of the coated metal sheet. The amount of silica added in the chemical conversion coating agent for forming the organic chemical conversion coating layer 40 is preferably 1 to 40 g / L. By adding 1 g / L or more of silica, it is possible to improve the processing adhesion of the coating film. In addition, by adding 40 g / L or less of silica, it is possible to achieve both the effects of processing adhesion and corrosion resistance while suppressing the increase in cost.

[0061] [Phosphoric acid and its salts] Examples of phosphoric acid and its salts include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and their salts, ammonium salts such as triammonium phosphate and diammonium hydrogen phosphate, phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and their salts, and organic phosphoric acids such as phytic acid and their salts. Examples of phosphoric acid salts other than ammonium salts include metal salts with Na, Mg, Al, K, Ca, Mn, Ni, Zn, Fe, and the like. Phosphoric acid and its salts may be used alone or in combination of two or more.

[0062] The content of phosphoric acid and its salts is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The content of phosphoric acid and its salts is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By making the content of phosphoric acid and its salts 20% by mass or less, embrittlement of the coating can be prevented, and a decrease in the processing adhesion of the coating when forming the coated metal sheet can be prevented.

[0063] [Fluoride] Examples of the fluoride include ammonium zirconate fluoride, ammonium silicofluoride, ammonium titanium fluoride, sodium fluoride, potassium fluoride, calcium fluoride, lithium fluoride, titanium hydrofluoric acid, zirconate hydrofluoric acid, etc. Such fluorides may be used alone or in combination of two or more.

[0064] The fluoride content is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The fluoride content is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By making the fluoride content 20% by mass or less, embrittlement of the coating can be prevented, and a decrease in the processing adhesion of the coating when forming the coated metal sheet can be prevented.

[0065] [Vanadium compounds] Examples of vanadium compounds include vanadium compounds obtained by reducing pentavalent vanadium compounds such as vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, and vanadium oxytrichloride to divalent to tetravalent vanadium compounds with a reducing agent, vanadium trioxide, vanadium dioxide, vanadium oxysulfate, vanadium oxyoxalate, vanadium oxyacetylacetonate, vanadium acetylacetonate, vanadium trichloride, phosphovanadomolybdic acid, vanadium sulfate, vanadium dichloride, and vanadium oxide, and other vanadium compounds having an oxidation number of 4 to 2. Such vanadium compounds may be used alone or in combination of two or more.

[0066] The content of the vanadium compound is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The content of the vanadium compound is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By making the content of the vanadium compound 20% by mass or less, it is possible to prevent embrittlement of the coating and to prevent a decrease in the processing adhesion of the coating when forming the coated metal sheet.

[0067] [Tannin or tannic acid] The tannin or tannic acid may be either hydrolyzable tannin or condensed tannin. Examples of tannin and tannic acid include hammeta tannin, Chinese gall tannin, gall tannin, myrobalan tannin, dividivi tannin, algarovila tannin, baronia tannin, and catechin. The amount of tannin or tannic acid added to the chemical conversion coating agent for forming the organic chemical conversion coating layer 40 may be 2 to 80 g / L. By setting the amount of tannin or tannic acid to 2 g / L or more, the adhesion to the metal sheet surface can be improved, and the processing adhesion of the coating film can be improved. In addition, by setting the amount of tannin or tannic acid added to 80 g / L or less, the cohesive force of the chemical conversion coating film can be maintained, and the processing adhesion of the coating film can be improved.

[0068] Furthermore, an acid, an alkali, or the like may be added to the chemical conversion treatment agent for forming the organic chemical conversion coating layer 40 in order to adjust the pH, within a range in which performance is not impaired.

[0069] The average thickness d3 of the organic chemical conversion coating layer 40 is preferably 0.10 μm or more, more preferably 0.20 μm or more, and even more preferably 0.30 μm or more. This makes it possible to stably achieve the various effects of providing the above-mentioned chemical conversion coating layer while uniformly forming the organic chemical conversion coating layer 40 on the surface of the metal sheet 10. The average thickness d3 of the organic chemical conversion coating layer 40 is preferably 5.00 μm or less, more preferably 4.00 μm or less, and even more preferably 3.00 μm or less. This makes it possible to stably achieve the various effects of providing the above-mentioned chemical conversion coating layer while uniformly forming the organic chemical conversion coating layer 40 on the surface of the metal sheet 10.

[0070] In addition, the ratio (d3 / d1) of the average thickness d3 of the organic chemical conversion coating layer 40 to the average thickness d1 of the photocatalyst layer 20 is preferably 0.5 or more, and more preferably 2.0 or more. This makes it possible to further improve the adhesion to the processed part. In addition, the ratio (d3 / d1) of the average thickness d3 of the organic chemical conversion coating layer 40 to the average thickness d1 of the photocatalyst layer 20 is preferably 20.0 or less, and more preferably 10.0 or less. This makes it possible to further improve the adhesion to the processed part.

[0071] ≪Protective layer 50≫ The protective layer 50 is a layer provided between the photocatalyst layer 20 and the organic chemical conversion coating layer 40 (more preferably, directly below the photocatalyst layer 20) and is provided to protect layers located below the photocatalyst layer 20 from the oxidizing power of the photocatalyst compound contained in the photocatalyst layer 20.

[0072] Here, the protective layer 50 may contain various known components. Examples of such components include inorganic oxides such as silica and zirconia. The specific content of such components may be appropriately adjusted.

[0073] In addition, the protective layer 50 is also preferably excellent in light transmittance, similar to the photocatalyst layer 20. In order to realize a protective layer 50 having excellent light transmittance, for example, it is possible to use the same components as those in the photocatalyst layer 20 other than the photocatalyst compound.

[0074] The average thickness d4 of the protective layer 50 is preferably 0.05 μm or more, and more preferably 0.20 μm or more. This makes it possible to reliably protect the layers located below the protective layer 50 from the oxidizing power of the photocatalytic compound while suppressing a decrease in processability. The average thickness d4 of the protective layer 50 is preferably 5.00 μm or less, and more preferably 0.60 μm or less. This makes it possible to reliably protect the layers located below the protective layer 50 from the oxidizing power of the photocatalytic compound while suppressing a decrease in processability.

[0075] Moreover, the ratio (d4 / d1) of the average thickness d4 of the protective layer 50 to the average thickness d1 of the photocatalyst layer 20 is preferably 0.3 or more, and more preferably 1.0 or more. This makes it possible to reliably suppress decomposition of the organic chemical conversion coating layer 40 by the photocatalyst layer 20. Moreover, the ratio (d4 / d1) of the average thickness d4 of the protective layer 50 to the average thickness d1 of the photocatalyst layer 20 is preferably 20.0 or less, and more preferably 3.0 or less. This makes it possible to reliably suppress decomposition of the organic chemical conversion coating layer 40 by the photocatalyst layer 20.

[0076] Furthermore, as shown in FIG. 2B, the coated metal sheet 1 according to this embodiment may further include various known layers between the photocatalyst layer 20 and the protective layer 50 and the organic chemical conversion coating layer 40, such as colored layers containing various color pigments.

[0077] Here, even in the case shown in FIG. 2A and FIG. 2B, the total thickness d from the surface of the metal plate 10 to the outermost surface of the coating layer (which is also the outermost surface of the photocatalyst layer 20) T(=d1+d3+d4+α) is set to 15.00 μm or less. As a result, as shown in FIG. 3, it becomes possible to utilize the reflected light, which is the incident light reflected on the surface of the metal plate 10 (in other words, the interface between the metal plate 10 and the photocatalytic layer 20), for the photocatalytic reaction by the photocatalytic compound, thereby making it possible to further improve the photocatalytic effect while suppressing costs. The total thickness d from the surface of the metal plate 10 to the outermost surface of the coating layer is T (=d1+d3+d4+α) is preferably 10.00 μm or less, and more preferably 7.00 μm or less.

[0078] 2A and 2B, the 60° specular gloss measured from the side where the photocatalytic layer 20 is provided, as defined in JIS Z8741:1997, is 80% or more. T If the reflectance is 15.00 μm or less and the 60° specular gloss is 80% or more, it can be considered that the reflected light of the incident light reflected on the surface of the metal plate 10 is utilized for the photocatalytic reaction by the photocatalytic compound.

[0079] 1A to 3 show the case where the photocatalytic layer 20 and other layers are provided on one side of the metal plate 10, but the photocatalytic layer 20 and other layers may be provided on both sides of the metal plate 10. In this case, the total thickness d from the surface of the metal plate 10 to the surface of the photocatalytic layer 20 is T is set to 15.00 μm or less on each surface of the coated metal sheet 1. In addition, the 60° specular gloss is set to 80% or more on each surface of the coated metal sheet 1. Furthermore, when the inorganic conversion coating layer 30 described above is provided, the protective layer 50 as described above may be formed.

[0080] The coated metal sheet according to this embodiment has been described in detail above with reference to FIGS. 1A to 3.

[0081] <Method for measuring the average thickness of each layer> Here, the average thickness of each layer including the photocatalyst layer can be measured by observing the layer of interest from the cross-sectional direction with a microscope. As a method for preparing a sample to be observed from the cross-sectional direction, for example, a method of embedding in resin and polishing the observation surface, a method of FIB processing, a microtome method, or other known methods can be used. In addition, as a type of microscope, known devices such as SEM and TEM can be used.

[0082] (About the manufacturing method of painted metal sheets) The coated metal sheet according to the present embodiment as described above can be produced by subjecting the surface of a base metal sheet to various pretreatments, such as cleaning, as necessary, and then applying a photocatalyst treatment agent for forming a photocatalyst layer, a chemical conversion treatment agent for forming a chemical conversion coating layer, or a protective treatment agent for forming a protective layer to the desired layer configuration, followed by drying and baking.

[0083] Here, the coating of various coating materials can be performed by a generally known coating method, such as roll coating, curtain flow coating, air spray, airless spray, immersion, bar coating, brush coating, etc. In particular, roll coating, which is a feature of the present product and can be stably applied in a thin film, is preferred.

[0084] The drying and baking conditions are not particularly limited and may be appropriately set depending on the paint used, etc. EXAMPLES

[0085] The coated metal sheet according to the present invention will be specifically described below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the coated metal sheet according to the present invention, and the coated metal sheet according to the present invention is not limited to the following examples.

[0086] Eight types of metal sheets shown in Table 1 below were prepared as base metal sheets. In Table 1, the six types of metal sheets shown as SD, ZL, GI, GL, AL, and GA are various types of plated steel sheets using steel sheets as the base material. The thickness of each metal sheet, as well as the plating composition and coating weight / standard of each plated steel sheet, are as shown in Table 1 below.

[0087] [Table 1]

[0088] As compounds having photocatalytic activity (photocatalytic compounds), seven types of compounds shown in Table 2 below were prepared. All photocatalytic compounds used were commercially available. The supported metals and average particle diameters are also shown in Table 2.

[0089] [Table 2]

[0090] <Inorganic / organic conversion coating agents> The raw materials of the water-based paint (chemical conversion coating agent) used to form the inorganic conversion coating and the organic conversion coating, and the concentrations in the dried coating are shown in Table 3 below. The amount of each component added was adjusted so that the concentration of each component was a predetermined concentration in the dried coating. Ion-exchanged water was added to adjust the solids concentration of the treatment agent to 10 mass% for the inorganic conversion coating and 20 mass% for the organic conversion coating. Each treatment agent was applied to the dried film thickness shown in Tables 4-1 and 4-2 below. Thereafter, the metal plate was dried in an induction heating furnace so that the temperature reached by the metal plate was 150°C, and then water-cooled with a spray.

[0091] [Table 3]

[0092] <Photocatalytic treatment agents, protective treatment agents> The photocatalytic treatment agent used and the method for preparing the protective treatment agent will be described below. The protective treatment agent was adjusted to have a solid content concentration of 8 mass % in consideration of storage stability. The concentration was adjusted by diluting with n-butanol. The photocatalytic treatment agent was prepared by adding a predetermined amount of the compound shown in Table 2 to the following protective treatment agent. The solid content concentration of the photocatalytic compound is as shown in Tables 4-1 and 4-2 below.

[0093] (1) Protective film treatment agent (Si-based): Tetraethoxysilane (22.5 parts by mass), methacryloxypropyltrimethoxysilane (2.8 parts by mass), and n-butanol (26 parts by mass) were mixed and stirred at 60°C for 2 hours. While stirring this mixture, a mixture of 26% by mass hydrochloric acid (3 parts by mass) and n-butanol (26 parts by mass) was added dropwise at 1 drop / second. After that, the mixture was kept stirred at 60°C for 2 hours to obtain a treatment agent. A series of operations was carried out in a nitrogen atmosphere.

[0094] (2) Protective film treatment agent (Zr-based): Zirconium n-butoxide (34.5 parts by mass), n-butanol (11.6 parts by mass), 1,5-diaminopentane (0.5 parts by mass), and yttrium nitrate (2.8 parts by mass) were mixed and stirred for 1 hour. Then, glacial acetic acid (4.8 parts by mass) was added and stirred for 40 hours. Then, concentrated nitric acid (0.6 parts by mass) was added dropwise at 1 drop / second, and the mixture was stirred for 2 hours to obtain a treatment agent. The series of operations was carried out in a nitrogen atmosphere.

[0095] Using the metal sheets and photocatalytic compounds described above, coated metal sheets having the configurations shown in Tables 4-1 and 4-2 below were manufactured by roll coating. Each layer was formed on one side of the metal sheet. For some of the coated metal sheets, a design was applied to the surface of the metal sheet to form a hairline pattern. For some of the coated metal sheets, a hot-dip galvanizing bath containing 0.1 mass % Sb and 0.2 mass % Al was used, and a plated steel sheet on which a spangle pattern was formed by adjusting the solidification rate of the hot-dip galvanizing was used as the substrate.

[0096] The average thickness of each layer in the coated metal plate was measured by embedding the coated metal plate in resin, polishing the cross section, and observing the observation surface with a microscope. The 60° specular gloss was measured with a gloss meter (UGV-6P manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS Z8741:1997.

[0097] The obtained coated metal sheets were evaluated from the viewpoints of antiviral properties, adhesion properties during processing, and corrosion resistance. The detailed evaluation methods are as follows.

[0098] <Antiviral> The antiviral properties were verified by measuring the virus infectivity in the following antiviral test in accordance with the antiviral standards stipulated by the Japan Antibacterial Product Technology Council. More specifically, each coated metal sheet was placed in a petri dish with the evaluation surface facing up, and a virus suspension containing influenza A virus was dropped onto the evaluation surface. After that, a film was placed on the coated metal sheet to bring the virus suspension into close contact with the entire evaluation surface, and the petri dish was then covered with a lid. The petri dish was left to stand for 24 hours in a room at 25°C with an illuminance of 1000 lux, simulating the interior of a typical office. The virus on the film surface and the evaluation surface was then washed away, and the virus infectivity (unit: PFU / cm) in the resulting washing solution was measured. 2 The PFU (Plaque Forming Units) was measured by plaque assay.

[0099] In addition to the painted metal plates, the same antiviral test was also carried out on each metal plate without a photocatalyst layer, and the extent to which the virus infectivity of the painted metal plate had decreased compared to the virus infectivity of the metal plate without a photocatalyst layer was evaluated as the activity value. 2 If the activity has decreased by more than 1×10 2 If the activity value is 1×10 or more, the use of the certification seal prescribed by the Japan Antibacterial Product Technology Council is permitted. 2 Those having the above value were judged to be acceptable. In addition, in the following Table 5, the obtained activity values ​​are shown in logarithm.

[0100] <Processing adhesion> The test material was subjected to 0T bending (180° bending), the coating on the outside of the bent part was peeled off with adhesive tape (Nichiban Cellotape (registered trademark), tape width 15 mm), and the state of adhesion of the coating to the tape side was observed. Then, the processing adhesion was evaluated according to the following evaluation criteria. In such adhesion test, the pass level was 3 or more. Specifically, a score of 4 or more was judged to be excellent in adhesion, and 3 or more was judged to be acceptable (pass level).

[0101] (Evaluation Criteria) 5: No coating on the tape side 4: Several points of coating peeling on the tape side, with the peeling length on the steel plate side being less than 5% of the total length of the processed area on one side of the test material 3: Several points of coating peeling on the tape side, with the peeled length on the steel plate side being 5% or more and less than 10% of the total length of the processed area on one side of the test material 2: Coating peeled off on the tape side, and the peeled length on the steel plate side was 10% or more but less than 20% of the total length of the processed area on one side of the test material. 1: Coating peeled off on the tape side, and the peeled length on the steel plate side was 20% or more of the total length of the processed part on one side of the test material.

[0102] <Corrosion resistance> The end faces of the test specimens were sealed with tape and subjected to a salt spray test (SST) for 72 hours in accordance with JIS Z 2371. After the test, the state of rust on the flat surface was observed and the corrosion resistance was evaluated according to the following evaluation criteria. A pass level was 3 or higher.

[0103] (Evaluation Criteria) 5: The area of ​​white rust is less than 1% of the total area on one side of the test material. 4: The area of ​​white rust is 1% or more and less than 5% of the total area on one side of the test material. 3: The area of ​​white rust is 5% or more and less than 10% of the total area on one side of the test material. 2: The area of ​​white rust is 10% or more and less than 30% of the total area on one side of the test material. 1: The area of ​​white rust is 30% or more of the total area on one side of the test material.

[0104] [Table 4-1]

[0105] [Table 4-2]

[0106] The results obtained are summarized in Table 5 below. As is clear from Table 5 below, the coated metal sheets corresponding to the examples of the present invention exhibited excellent antiviral properties, adhesion during processing, and corrosion resistance, while the coated metal sheets corresponding to the comparative examples of the present invention failed the evaluation results for antiviral properties or adhesion during processing.

[0107] [Table 5]

[0108] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. [Explanation of symbols]

[0109] 1. Painted metal plate 10 metal plate 20 Photocatalyst layer (first film layer) 30 Inorganic chemical conversion coating layer (second coating layer) 40 Organic conversion coating layer (third coating layer) 50 Protective layer (fourth coating layer)

Claims

1. A coated metal plate having a coating layer on at least one surface of the metal plate, The coating layer is located on the outermost surface of the coating layer on at least one surface of the metal plate, and comprises a compound having photocatalytic activity (excluding the cases where the compound having photocatalytic activity is rutile-type titanium oxide and the case where the compound having photocatalytic activity is crystalline zirconium titanate. and a second coating layer located below the first coating layer and made of an inorganic component having at least one element selected from the group consisting of Si and Zr. The first coating layer has an average thickness of 0.05 to 5.00 μm; The average thickness of the second coating layer is 0.10 to 5.00 μm; The total thickness from the surface of the metal plate to the outermost surface of the coating layer is 15.00 μm or less, The second coating layer further contains an inorganic component having at least one element of P or V, The coated metal sheet has a 60° specular gloss of 80% or more as defined in JIS Z8741:1997.

2. The first coating layer further contains at least one element of Si or Zr, The coated metal sheet according to claim 1, wherein the total concentration of the elements is 5 to 50 mass % in terms of silica for Si and zirconia for Zr.

3. 3. The coated metal sheet according to claim 1, wherein a ratio of an average thickness of the second coating layer to an average thickness of the first coating layer is 0.3 to 12.

0.

4. 3. The coated metal sheet according to claim 1, wherein the second coating layer contains at least one of zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, sodium zirconium carbonate, or ammonium zirconium carbonate as the inorganic component containing Zr.

5. 3. The coated metal sheet according to claim 1, wherein the second coating layer contains, as the inorganic component containing P, at least one of phosphoric acid, orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, tetraphosphoric acid, and salts thereof, or ammonium dihydrogen phosphate.

6. 3. The coated metal sheet according to claim 1, wherein the second coating layer contains at least one of ammonium metavanadate (V), potassium metavanadate (V), sodium metavanadate (V), or vanadyl sulfate (IV) as the inorganic component containing V.

7. The coated metal sheet according to claim 1 or 2, wherein a total thickness from the surface of the metal sheet to an outermost surface of the first coating layer is 10.00 μm or less.

8. 3. The coated metal sheet according to claim 1, wherein the compound having photocatalytic activity is anatase type titanium oxide.

9. 9. The coated metal sheet according to claim 8, wherein the anatase type titanium oxide is a metal-supported type titanium oxide supported on at least one of Cu and Fe.

10. 9. The coated metal sheet according to claim 8, wherein the concentration of the anatase type titanium oxide in the first coating layer is 50 to 95 mass % in terms of titania.

11. 9. The coated metal sheet according to claim 8, wherein the anatase type titanium oxide has an average particle size of 5 to 200 nm.

12. The coated metal sheet according to claim 1 or 2, wherein the metal sheet is a zinc-plated steel sheet, a zinc-aluminum alloy-plated steel sheet, a zinc-aluminum-magnesium alloy-plated steel sheet, an aluminum-plated steel sheet, a zinc-nickel alloy-plated steel sheet, a zinc-iron alloy-plated steel sheet, an aluminum sheet, or a stainless steel sheet.

13. The coated metal sheet according to claim 1 or 2, wherein a hairline is present on a surface of the metal sheet along a rolling direction of the metal sheet.

14. The coated metal sheet according to claim 1 or 2, wherein a spangle pattern is present on the surface of the metal sheet.

Citation Information

Patent Citations

  • Coated metal plate with excellent stain resistance and its manufacture

    JP1998264299A

  • Photocatalyst-bearing structure body, production method of the same, composition for intermediate layer

    JP2001286766A

  • Titanium oxide-based photocatalyst, process for preparing the same, and use thereof

    WO1998058736A1