Standing pouch and packaging article

The standing pouch design with higher crystallinity in the bottom film and specific polyethylene content addresses manufacturing defects and falling resistance, ensuring robustness and reliability.

JP2024159957AInactive Publication Date: 2024-11-08TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024150326
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Standing pouches during manufacturing are prone to defects and have poor resistance to the contents falling, especially when filled with large volumes, leading to potential damage to the bottom film.

Method used

The standing pouch is designed with a pair of main body films and a bottom film, where the crystallinity of the second base layer in the bottom film is significantly higher than the first base layer in the main body films, with a difference of 15 points or more, and both films contain polyethylene, ensuring a polyethylene content of 90% by mass or more, and include additional layers like intermediate and protective layers to enhance strength and resistance.

Benefits of technology

The design reduces manufacturing defects and enhances the pouch's resistance to falling, particularly when filled with large volumes, by minimizing warping and improving impact resistance, thus maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159957000001_ABST
    Figure 2024159957000001_ABST
Patent Text Reader

Abstract

To provide a standing pouch which hardly causes defects in manufacture, and is excellent in falling resistance of a packaging article filled with a content.SOLUTION: A standing pouch 110 includes a pair of body films 111A and 111B, and a bottom film 112, wherein each of the pair of body films includes a first base material layer containing polyethylene, and a first sealant layer which is provided on the first base material layer and contains polyethylene, the bottom film includes a second base material layer containing polyethylene and a second sealant layer which is provided on the second base material layer and contains polyethylene, and degrees of crystallization of the second base material layers are large compared to degrees of crystallization of the first base material layers of each of the pair of body films, and a difference therebetween is 15 points or more.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stand-up pouch. [Background technology]

[0002] A packaged article obtained by filling a content into a standing pouch can stand on its own. Therefore, such a packaged article can be stored in a box in a self-supporting state, for example, and can be easily packed. Furthermore, such a packaged article can be easily arranged on a shelf in a store in a good appearance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2001-206384 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a standing pouch which is less susceptible to defects during production and which provides excellent drop resistance for a packaged article filled with contents. [Means for solving the problem]

[0005] According to one aspect of the present invention, there is provided a standing pouch comprising a pair of main films and a bottom film, each of the pair of main films comprising a first base layer containing polyethylene and a first sealant layer comprising polyethylene provided on the first base layer, the bottom film comprising a second base layer containing polyethylene and a second sealant layer comprising polyethylene provided on the second base layer, the crystallinity of the second base layer being greater than the crystallinity of the first base layer of each of the pair of main films, the difference between them being 15 points or more.

[0006] According to another aspect of the present invention, there is provided a standing pouch according to the above aspect, comprising a pair of main films and a bottom film, each of the pair of main films comprising a first base layer containing polyethylene and a first sealant layer comprising polyethylene and provided on the first base layer, the bottom film comprising a second base layer containing polyethylene and a second sealant layer comprising polyethylene and provided on the second base layer, the crystallinity of the second base layer being in the range of 35% to 95%, and the crystallinity of the first base layer of each of the pair of main films being in the range of 5% to 35%.

[0007] According to yet another aspect of the present invention, there is provided a standing pouch relating to any of the above aspects, wherein each of the pair of main films further includes a first intermediate layer interposed between the first base layer and the first sealant layer and containing polyethylene.

[0008] According to yet another aspect of the present invention, there is provided a standing pouch according to any of the above aspects, wherein the bottom film further comprises a second intermediate layer interposed between the second base layer and the second sealant layer and comprising polyethylene.

[0009] According to yet another aspect of the present invention, there is provided a standing pouch relating to any of the above aspects, wherein each of the pair of main films further includes a first protective layer as an outermost layer facing the first sealant layer with the first base material layer sandwiched therebetween.

[0010] According to yet another aspect of the present invention, there is provided the standing pouch according to the above aspect, wherein the first protective layer contains a cured product of a thermosetting resin.

[0011] According to yet another aspect of the present invention, there is provided a standing pouch relating to any of the above aspects, wherein the bottom film further includes a second protective layer as an outermost layer facing the second sealant layer with the second base layer sandwiched therebetween.

[0012] According to yet another aspect of the present invention, there is provided the standing pouch according to the above aspect, wherein the second protective layer contains a cured product of a thermosetting resin.

[0013] According to yet another aspect of the present invention, there is provided a standing pouch relating to any of the above aspects, wherein each of the pair of main films further includes a first gas barrier layer interposed between the first base layer and the first sealant layer.

[0014] According to yet another aspect of the present invention, there is provided a standing pouch according to any of the above aspects, wherein the bottom film further includes a second gas barrier layer interposed between the second base layer and the second sealant layer.

[0015] According to yet another aspect of the present invention, there is provided a standing pouch according to any one of the above aspects, wherein each of the pair of main films and the bottom film has a polyethylene content of 90% by mass or more.

[0016] According to yet another aspect of the present invention, there is provided a stand-up pouch according to any of the above aspects for containing contents having a volume within the range of 0.2L to 4.0L.

[0017] According to yet another aspect of the present invention, there is provided a packaging article comprising the stand-up pouch according to any one of the above aspects and contents accommodated in the stand-up pouch.

[0018] According to yet another aspect of the present invention, there is provided a packaging article according to the above aspect, wherein the volume of the contents is within the range of 0.2L to 4.0L. Effect of the Invention

[0019] According to the present invention, there is provided a standing pouch which is less prone to defects during production and which provides excellent drop resistance for a packaged article filled with contents. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a front view of a packaging article according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a portion of the package shown in FIG. [Diagram 3] FIG. 3 is an enlarged cross-sectional view showing a part of a standing pouch used in producing the packaged article of FIG. [Figure 4] FIG. 4 is a cross-sectional view showing an example of a laminate that can be used as the main body film of the standing pouch of FIG. [Diagram 5] FIG. 5 is a cross-sectional view showing an example of a laminate that can be used as the bottom film of the standing pouch of FIG. [Figure 6] FIG. 6 is a front view of a packaged article according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0022] The embodiments described below are merely examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of ​​the present invention within the technical scope defined by the claims.

[0023] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.

[0024] <1> Stand-up pouches and packaging articles Fig. 1 is a front view of a packaging article according to one embodiment of the present invention. Fig. 2 is a cross-sectional view showing an enlarged portion of the packaging article shown in Fig. 1. Fig. 3 is a cross-sectional view showing an enlarged portion of a standing pouch used in producing the packaging article of Fig. 1.

[0025] Here, the cross section in Fig. 2 is a portion near the bottom of a cross section perpendicular to the width direction of the packaged article 100 shown in Fig. 1 and passing through the center of the width. The cross section in Fig. 3 corresponds to the portion of the cross section of the standing pouch 110 depicted in Fig. 2. Note that the standing pouch 110 has a folded, flat bottom immediately after production, but in Fig. 3, the bottom is slightly expanded to make it easier to understand.

[0026] The packaged article 100 shown in Figs. 1 and 2 includes a standing pouch 110 which is a package, and contents 120 contained therein.

[0027] The standing pouch 110 includes a pair of main body films 111A and 111B and a bottom film 112, as shown in FIGS.

[0028] Each of the main films 111A and 111B and the bottom film 112 is a laminate including a base material layer and a sealant layer provided thereon, as described below.

[0029] In the standing pouch 110 before being filled with the content 120, the main films 111A and 111B are arranged so that their sealant layers face each other, as shown in Fig. 3. The bottom film 112 is folded in half so as to form a mountain fold when viewed from the sealant layer side, and is sandwiched between the main films 111A and 111B at one end thereof so that the mountain fold MF faces the other end of the main films 111A and 111B.

[0030] The edges of the main body films 111A and 111B are heat-sealed to each other from the position of the mountain fold MF of the bottom film 112 to the other ends of the main body films 111A and 111B. As a result, the main body films 111A and 111B form heat-sealed parts HS1 shown in FIG. 1 on both sides thereof.

[0031] The bottom film 112 is heat-sealed to the main film 111A and 111B except for its central portion. Specifically, one of the two portions of the bottom film 112 defined by the mountain fold MF is heat-sealed to the main film 111A at a position other than the central portion of the bottom film 112, forming the heat-sealed portion HS2A shown in Figs. 1 to 3. The other of the two portions of the bottom film 112 defined by the mountain fold MF is heat-sealed to the main film 111B at a position other than the central portion of the bottom film 112, forming the heat-sealed portion HS2B shown in Figs. 2 and 3. The outer surfaces of these two portions of the bottom film 112 are bonded to each other at both sides of the bottom of the standing pouch 110.

[0032] The heat-sealed portions HS1 and HS4 shown in Fig. 1 are portions heat-sealed by a side seal and a point seal, respectively, which will be described later. The heat-sealed portion HS2A shown in Figs. 1 to 3 and the heat-sealed portion HS2B shown in Figs. 2 and 3 are portions heat-sealed by a bottom seal, which will be described later.

[0033] In the packaged article 100 in which the content 120 is accommodated in the standing pouch 110, the main body films 111A and 111B are further heat-sealed at the other ends thereof, so that the main body films 111A and 111B form the heat-sealed portion HS3 shown in FIG.

[0034] The standing pouch 110 is formed so that its upper corner can be used as a mouth after opening. An easy-to-open structure can be provided at the position of this corner. The easy-to-open structure is, for example, a notch.

[0035] The standing pouch 110 may be formed so that a portion other than the upper corners can be used as a mouth portion after opening. For example, the standing pouch 110 may be formed so that an upper central portion can be used as a mouth portion after opening. The standing pouch 110 may further include a mouth member and a lid body at its upper portion. For example, as in the standing pouch 110 of the packaged article 100A shown in FIG. 6, a spout 113 which is a member for extracting the contents may be interposed between the main body films 111A and 111B at the upper position of the standing pouch 110 and welded thereto, and a cap 114 which is a member for sealing the spout 113 may be fitted or screwed to the mouth portion of the spout 113.

[0036] The contents 120 may be, for example, a liquid or a mixture of a liquid and a solid, such as food or medicine.

[0037] Although there is no limit to the volume of the contents 120, the technology described here is particularly useful when the volume of the contents 120 is large. In this respect, the volume of the contents 120 is preferably within the range of 0.2 to 4.0 L. More preferably, the volume of the contents 120 is 0.8 L or more. Moreover, the volume of the contents 120 is more preferably 3.0 L or less.

[0038] <2> Main body film FIG. 4 is a cross-sectional view showing an example of a laminate that can be used as the main body film of the standing pouch of FIG.

[0039] The laminate 10 shown in Fig. 4 can be used for the main films 111A and 111B. As described later, various modifications of the laminate 10 are possible. The laminates according to these modifications can also be used for the main films 111A and 111B.

[0040] The laminate 10 includes a protective layer 16, a substrate layer 11, a printed layer 14, an adhesive layer 13A, an intermediate layer 18, an inorganic compound layer 15, a coating layer 17, an adhesive layer 13B, and a sealant layer 12, in this order.

[0041] As described below, the base layer 11, the intermediate layer 18, and the sealant layer 12 contain polyethylene. The laminate 10 preferably contains polyethylene at a rate of 90% by mass or more. Here, the rate of polyethylene in the laminate means the rate of the total amount of polyethylene in the total amount of resin material in each layer constituting the laminate. By making the rate of polyethylene 90% by mass or more, high recyclability can be achieved.

[0042] <2.1> Base material layer The base layer 11 is a first base layer. The base layer 11 contains polyethylene. Preferably, the base layer 11 is made of polyethylene.

[0043] The crystallinity of the base layer 11 is smaller than that of the base layer 21 of the bottom film 112, which will be described later. That is, the crystallinity of the base layer 21 of the bottom film 112 is larger than that of each of the base layers 11 of the main films 111A and 111B. The difference between these crystallinities is 15 points or more, preferably 20 points or more. The difference between these crystallinities is, for example, 70 points or less. Drop resistance is required for the base layer 21. If a crystallinity that satisfies this requirement is selected for the base layer 21 and the crystallinity of the base layer 11 is brought close to this crystallinity, even if a standing pouch is to be manufactured, the film will curl significantly and it will not be possible to manufacture the pouch. Therefore, it is preferable that the crystallinity of the base layer 11 is somewhat lower than that of the base layer 21. Specifically, it is preferable that the crystallinity is 15 points or more lower.

[0044] The crystallinity of the base layer 11 is preferably within a range of 5% to 35%. More preferably, the crystallinity of the base layer 11 is 10% or more. Moreover, the crystallinity of the base layer 11 is more preferably 30% or less.

[0045] Here, the "crystallinity" is the ratio of the crystalline peak area to the total peak area measured by the parallel beam method of X-ray diffraction in the diffraction angle range of 10° to 30°. The method for measuring the crystallinity will be described in detail later.

[0046] As described later, the standing pouch 110 having such a configuration is less likely to have defects during its manufacture. Also, as described later, the packaged article 100 obtained by filling the contents 120 into the standing pouch 110 having such a configuration has excellent drop resistance.

[0047] The polyethylene contained in the base layer 11 may be a homopolymer of ethylene or a copolymer of ethylene and another monomer. When the polyethylene is a copolymer of ethylene and another monomer, the proportion of ethylene in the copolymer is, for example, 80 mol % or more.

[0048] The other monomer is, for example, an α-olefin. According to one example, the α-olefin has a carbon number in the range of 3 to 20. Such an α-olefin is, for example, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, or 6-methyl-1-heptene.

[0049] The polyethylene may be a copolymer of ethylene and one of vinyl acetate and acrylic ester, or a copolymer of ethylene and vinyl acetate, a completely or partially saponified product thereof, (meth)acrylic acid, or an esterified product or an ionically crosslinked product thereof.

[0050] The substrate layer 11 is, for example, high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), or very low density polyethylene (VLDPE).

[0051] Here, high density polyethylene has a density of 0.942 g / cm 3 and medium density polyethylene has a density of 0.930 g / cm 3 More than 0.942g / cm 3 and low density polyethylene has a density of 0.910 g / cm 3 More than 0.930g / cm 3 Linear low density polyethylene has a density of 0.910 g / cm 3 More than 0.930cm 3 and ultra-low density polyethylene has a density of 0.910 g / cm 3 is less than. The density is a value obtained by a method in accordance with JIS K7112:1999.

[0052] The polyethylene contained in the base material layer 11 may be polyethylene derived from biomass. As the polyethylene derived from biomass, for example, Green Polyethylene (manufactured by Braskem) can be used.

[0053] Alternatively, the polyethylene contained in the base layer 11 may be polyethylene recycled by mechanical recycling. Here, mechanical recycling refers to decontaminating the polyethylene film by crushing collected polyethylene films and the like, washing the crushed films with an alkali to remove dirt and foreign matter on the film surface, and then drying the films at high temperature and reduced pressure to diffuse contaminants remaining inside the films.

[0054] Alternatively, the polyethylene contained in the base layer 11 may be polyethylene recycled by chemical recycling.

[0055] The melting point of the base layer 11 is preferably within a range of 100° C. to 140° C., and more preferably within a range of 120° C. to 140° C. The melting point is a value obtained by a method in accordance with JIS K7121-1987.

[0056] The substrate layer 11 may be a non-stretched film or a stretched film. The substrate layer 11 is preferably a non-stretched film. When the substrate layer 11 has a lower crystallinity than the substrate layer 21 of the bottom film 112 and is a non-stretched film, the laminate 10 used as the main films 111A and 111B during the manufacture of the standing pouch 110 can be more reliably prevented from warping due to heat. When the substrate layer 11 is a stretched film, the substrate layer 11 may be a uniaxially stretched film or a biaxially stretched film. In this specification, the term "film" does not include the concept of thickness.

[0057] In this specification, whether a stretched film is a uniaxially stretched film or a biaxially stretched film can be determined by performing in-plane measurement using wide-angle X-ray diffraction, as described below. The X-ray diffraction pattern obtained by this measurement contains information about the degree of orientation of molecular chains present on the film surface.

[0058] When a polymer film is uniaxially stretched, a higher-order structure called a shish-kebab structure appears. The shish-kebab structure consists of a shish structure, which is an extended chain crystal, and a kebab structure, which is a lamellar crystal. In a uniaxially stretched film, this higher-order structure is arranged with a high degree of order, and therefore the X-ray diffraction pattern obtained by the above measurement of the uniaxially stretched film contains a sharp diffraction peak. That is, when the above measurement is performed on a uniaxially stretched film, a clear diffraction peak appears. Note that a "clear diffraction peak" means a diffraction peak with a half-width of less than 10°.

[0059] In contrast, in the manufacture of biaxially stretched films, the film is stretched in a specific direction, and then stretched in a direction perpendicular to the first direction. Therefore, although the first stretching produces the above-mentioned high-order structure, this high-order structure is disturbed by the second stretching. Therefore, when the above-mentioned measurements are performed on a biaxially stretched film, the diffraction peaks in the resulting X-ray diffraction pattern are broad. In other words, when the above-mentioned measurements are performed on a biaxially stretched film, no clear diffraction peaks appear.

[0060] As described above, the X-ray diffraction patterns obtained by the above-mentioned measurements are different between uniaxially stretched films and biaxially stretched films, and therefore it is possible to determine whether a stretched film is a uniaxially stretched film or a biaxially stretched film based on the X-ray diffraction patterns.

[0061] The film can be produced by known methods such as a casting method, an inflation method, etc. Also, a multilayer polyethylene film obtained by co-extruding polyethylenes having different densities can be used as the base layer 11. The stretched film can be obtained, for example, by stretching a film obtained by forming a polyethylene film by a T-die method or an inflation method, etc.

[0062] The haze of the base layer 11 is preferably 20% or less, and more preferably 10% or less. The haze is a value obtained by a method in accordance with JIS K7136:2000.

[0063] The thickness of the base layer 11 is preferably in the range of 10 μm to 200 μm. The thickness of the base layer 11 is, for example, in the range of 10 μm to 50 μm, or in the range of 15 μm to 50 μm, or in the range of 12 μm to 35 μm. If the base layer 11 is too thin, the strength of the laminate 10 is likely to be reduced. If the base layer 11 is too thick, the processability of the laminate 10 is likely to be reduced.

[0064] The substrate layer 11 is preferably surface-treated. This treatment can improve the adhesion between the substrate layer 11 and the layer adjacent to the substrate layer 11.

[0065] The method of the surface treatment is not particularly limited, and examples of the surface treatment include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, and chemical treatments such as oxidation treatment using chemicals.

[0066] The base layer 11 may further contain additives, such as a crosslinking agent, an antioxidant, an antiblocking agent, a slip agent, an ultraviolet absorbing agent, a light stabilizer, a filler, a reinforcing agent, an antistatic agent, a pigment, and a modifying resin.

[0067] The proportion of polyethylene in the base layer 11 is preferably 50% by mass or more, and more preferably 80% by mass or more. According to one example, the base layer 11 is made of polyethylene. According to another example, the base layer 11 is made of polyethylene and an additive.

[0068] The substrate layer 11 may be colored, for example, white.

[0069] As described above, the base layer 11 has a lower degree of crystallinity than the base layer 21. In the case of such a base layer 11, the laminate 10 used as the main films 111A and 111B during the production of the standing pouch 110 is not significantly warped by heat. Therefore, in the case of such a base layer 11, defects such as defective products and troubles with the production equipment are unlikely to occur during the production of the standing pouch 110. From this viewpoint, it is preferable that the crystallinity of the base layer 11 is within the above-mentioned range.

[0070] The crystallinity of the base layer 11 can be adjusted by controlling the degree of stretching of the polyethylene film used in the base layer 11, or the thermal history during or after the production of the film. For example, the crystallinity increases when the film is slowly cooled after production, and decreases when it is rapidly cooled. It is also possible to improve the crystallinity by adding an additive such as a crystal nucleating agent.

[0071] <Method for measuring crystallinity> The crystallinity of the substrate layer 11 is measured by X-ray diffraction using a parallel beam method. An example of a method for measuring the crystallinity will be described below.

[0072] First, the X-ray diffraction pattern of the base layer 11 is obtained by out-of-plane measurement using a wide-angle X-ray diffractometer manufactured by Rigaku Corporation, scanning the diffraction angle range of 10° to 30° with 2θ / θ. The characteristic X-ray CuKα is used as the X-ray, and the X-ray is collimated by a multilayer mirror and made incident on the base layer 11. A scintillation detector equipped with a flat collimator is used as the light receiving unit.

[0073] From the obtained X-ray diffraction pattern, the peak area of ​​the crystalline component and the halo pattern area of ​​the amorphous component are determined, and the ratio of the peak area of ​​the crystalline component to the total area is calculated as the degree of crystallinity. When the base layer 11 has a plurality of layers, the crystallinity of one of the outermost surfaces of the base layer 11 is measured.

[0074] When the base layer 11 is a polyethylene film, scanning at a diffraction angle range of 10° to 30° reveals two sharp crystalline component peaks corresponding to the (110) and (200) planes, and a broad amorphous component halo pattern. These are separated and analyzed, and the areas of the crystalline component peaks and the amorphous component halo pattern are calculated, and the degree of crystallinity can be calculated from the following formula (1).

[0075] Crystallinity = crystalline component peak area / (crystalline component peak area + amorphous component halo pattern area) ... (1) The focusing method is known as an X-ray diffraction method other than the parallel beam method, but in the case of samples with uneven surfaces such as resin films, the focusing method is prone to affecting the measurement results, such as peak broadening due to misalignment of the measurement surface. In contrast, in the case of parallel beam method, misalignment of the measurement surface has little effect on the measurement results, even in the case of samples with uneven surfaces.

[0076] On the other hand, the base layer 11 is preferably a non-stretched film, but may be a uniaxially stretched film or a biaxially stretched film, and as described above, the in-plane method using X-ray diffraction can be used to distinguish between them. This in-plane method fixes the X-ray incidence angle θ and the angle 2θ at which the diffracted X-rays are detected by the detector to the angles θ and 2θ at which a diffraction peak corresponding to a specific crystal plane is detected in the out-of-plane method, for example, the diffraction peak corresponding to the (110) plane of a polyethylene film, respectively, and in this state, the film to be measured is scanned in the in-plane direction to obtain a diffraction pattern.

[0077] When in-plane measurements are performed on a uniaxially stretched film that has been uniaxially stretched in the machine direction (MD), a diffraction pattern can be obtained that has a sharp diffraction peak corresponding to the (110) plane at an angle 2θ of about ±90°, assuming that the MD direction is defined as 0°. On the other hand, in the case of a biaxially stretched film, the high-order structure obtained by uniaxial stretching is disturbed by the second stretching, and the anisotropy is reduced, so a diffraction pattern having a sharp diffraction peak corresponding to this (110) plane cannot be obtained. Therefore, in-plane measurements can be cited as one method for distinguishing uniaxially stretched films from biaxially stretched films.

[0078] <2.2> Sealant layer The sealant layer 12 is a first sealant layer. The sealant layer 12 faces the base layer 11. The sealant layer 12 contains polyethylene. Preferably, the sealant layer 12 is made of polyethylene. For example, the polyethylene contained in the base layer 11 may be any of those described above. The sealant layer 12 is preferably low density polyethylene (LDPE), linear low density polyethylene (LLDPE), or very low density polyethylene (VLDPE), and more preferably linear low density polyethylene.

[0079] From the viewpoint of environmental load, the polyethylene is preferably biomass-derived polyethylene or recycled polyethylene.

[0080] The sealant layer 12 may further include the additives described above. The proportion of polyethylene in the sealant layer 12 is preferably 50% by mass or more, and more preferably 80% by mass or more. In one example, the sealant layer 12 is made of polyethylene. In another example, the sealant layer 12 is made of polyethylene and an additive.

[0081] The sealant layer 12 may be transparent or opaque. In the latter case, the sealant layer 12 may be white, black, gray, sepia, or the like. In the sealant layer 12, these opaque layers may be used alone, may form a multilayer structure including two or more of these, or may be combined with a transparent sealant. When the laminate 10 has a transparent sealant layer 12 and is used as the main body films 111A and 111B of the standing pouch 110, the contents 120 are easily visible. When the laminate 10 has an opaque sealant layer 12 and is used as the main body films 111A and 111B of the standing pouch 110, the contents 120 do not interfere with the visibility of the image displayed by the printing layer 14. In particular, the white sealant layer 12 improves the visibility of the image displayed by the printing layer 14.

[0082] The sealant layer can be colored white, gray, black, or the like by mixing a pigment or the like into the material resin. For example, the sealant layer will be white if titanium oxide is mixed into the material resin, black if carbon black is mixed into the material resin, and gray if both are mixed into the material resin. If the sealant layer is required to have light-shielding properties, it is preferably black, gray, or sepia. The light-shielding sealant contains, for example, carbon black.

[0083] The thickness of the sealant layer 12 can be appropriately set in consideration of the shape of the packaging bag to be manufactured, the mass of the contents to be contained, etc., but is preferably 30 μm or more, and more preferably 60 μm or more from the viewpoint of content retention. Also, the thickness of the sealant layer 12 is preferably 300 μm or less, more preferably 200 μm or less, from the viewpoint of bag manufacturing efficiency and cost.

[0084] The sealant layer 12 is, for example, a non-oriented polyethylene resin film, or a layer formed by melt extrusion of polyethylene.

[0085] <2.3>Printing layer The printed layer 14 is a first printed layer. The printed layer 14 is provided on the surface of the base layer 11 facing the sealant layer 12, i.e., on the back surface of the base layer 11. The position at which the printed layer 14 is provided is not limited. That is, the printed layer 14 may be provided on the surface of the base layer 11, or may be provided at any position between the base layer 11 and the sealant layer 12. For example, the printed layer 14 may be provided on any surface of the intermediate layer 18. The laminate 10 may also include multiple printed layers. The printed layer 14 may be omitted.

[0086] The printing ink used for the printing layer 14 is not particularly limited as long as it has adhesion to polyethylene. The printing layer 14 is composed of ink in which additives such as various pigments, extender pigments, plasticizers, drying agents, and stabilizers are added to conventionally used ink binder resins such as urethane-based, acrylic-based, nitrocellulose-based, rubber-based, and vinyl chloride-based inks. It is preferable to use ink derived from biomass as the printing ink. As the printing method, for example, well-known printing methods such as offset printing, gravure printing, flexographic printing, and silk screen printing, and well-known coating methods such as roll coating, knife edge coating, and gravure coating can be used. In addition, light-shielding inks can also be preferably used. As the light-shielding inks, for example, white ink, black ink, silver ink, and sepia ink can be mentioned.

[0087] <2.4> Middle class The intermediate layer 18 is a first intermediate layer. The intermediate layer 18 is provided between the base material layer 11 and the sealant layer 12. Here, the intermediate layer 18 is provided between the base material layer 11 and the sealant layer 12 such that the printed layer 14 is interposed between the base material layer 11 and the intermediate layer 18. The intermediate layer 18 may be omitted.

[0088] The intermediate layer 18 contains polyethylene. As the polyethylene, for example, the polyethylene contained in the base layer 11 described above can be used.

[0089] The polyethylene contained in the intermediate layer 18 may be the same as or different from the polyethylene contained in the base layer 11. In addition, the intermediate layer 18 may further contain the additives described above.

[0090] The proportion of polyethylene in the intermediate layer 18 is preferably 50% by mass or more, and more preferably 80% by mass or more. In one example, the intermediate layer 18 is made of polyethylene. In another example, the intermediate layer 18 is made of polyethylene and an additive.

[0091] According to one example, the intermediate layer 18 has a crystallinity of less than 35%. By using a film with a low crystallinity as the intermediate layer 18, the strength of the laminate 10 can be improved, and in particular, damage (bag breakage) caused by dropping the packaged article 100 can be made less likely to occur. From this perspective, the intermediate layer 18 is preferably a non-oriented film.

[0092] In another example, the intermediate layer 18 has a crystallinity of preferably 35% or more, more preferably 40% or more, and even more preferably 50% or more. In one example, the crystallinity of the intermediate layer 18 is 75% or less.

[0093] Using a film with a high degree of crystallinity as the intermediate layer 18 increases the strength of the laminate 10, particularly the puncture strength. A laminate with a high proportion of polyethylene is weaker than other laminates, and is therefore frequently folded when used as a packaging material. Frequent folding increases the likelihood of pinholes occurring, but the laminate 10, which has excellent puncture strength, is less likely to develop pinholes. From this perspective, it is preferable that the intermediate layer 18 is a stretched film.

[0094] The melting point of the intermediate layer 18 is preferably within the range of 100°C to 140°C, and more preferably within the range of 120°C to 140°C.

[0095] The thickness of the intermediate layer 18 is preferably in the range of 10 μm to 200 μm, and more preferably in the range of 15 μm to 50 μm.

[0096] The intermediate layer 18 may be colored, for example, white.

[0097] The intermediate layer 18 can be produced by a known production method such as a casting method or an inflation method. It is also possible to use a multilayer polyethylene film obtained by co-extruding polyethylenes having different densities as the intermediate layer 18. The stretched film can be obtained, for example, by stretching a film obtained by forming a polyethylene film by a T-die method or an inflation method.

[0098] <2.5>Inorganic compound layer The inorganic compound layer 15 is a first inorganic compound layer. The inorganic compound layer 15 is provided on one surface of the intermediate layer 18. Here, the inorganic compound layer 15 is provided on the surface of the intermediate layer 18 facing the sealant layer 12. The inorganic compound layer 15 may be provided on the surface of the intermediate layer 18 facing the base material layer 11. The inorganic compound layer 15 may be provided on the surface of the base material layer 11 facing the sealant layer 12, here between the base material layer 11 and the printed layer 14. The inorganic compound layer 15 may be provided on the surface of the base material layer 11 opposite to the sealant layer 12, here as the outermost layer of the laminate. The inorganic compound layer 15 may be omitted.

[0099] The inorganic compound layer 15 is a thin film made of an inorganic compound, for example, an inorganic oxide such as aluminum oxide or silicon oxide, and functions as a gas barrier layer or a part thereof that suppresses the transmission of oxygen and water vapor. The inorganic compound layer 15 may be formed by coating or by vapor deposition of an inorganic compound.

[0100] Examples of the inorganic compound contained in the inorganic compound layer 15 include metal oxides such as aluminum oxide, silicon oxide, magnesium oxide, and tin oxide. The inorganic compound layer 15 is preferably a vapor deposition film made of a metal oxide. From the viewpoint of transparency and barrier properties, the metal oxide may be selected from the group consisting of aluminum oxide, silicon oxide, and magnesium oxide. Considering the cost, the metal oxide is preferably selected from aluminum oxide and silicon oxide. From the viewpoint of excellent tensile elongation during processing, it is preferable to use silicon oxide as the metal oxide. By making the inorganic compound layer 15 a vapor deposition film made of a metal oxide, high barrier properties can be obtained with a very thin layer within a range that does not affect the recyclability of the laminate 10.

[0101] A vapor-deposited film made of a metal oxide has the advantage of being transparent, and therefore less likely to cause a user holding a packaging material made of a laminate to mistakenly believe that a metal foil is used, compared to a vapor-deposited film made of a metal.

[0102] The thickness of the vapor-deposited film made of aluminum oxide is preferably 5 nm or more and 30 nm or less. When the thickness is 5 nm or more, sufficient gas barrier properties can be obtained. Furthermore, when the thickness is 30 nm or less, cracks caused by deformation due to internal stress of the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that, when the thickness exceeds 30 nm, the cost is likely to increase due to an increase in the amount of material used and a prolonged film formation time, and is therefore not preferable from an economical point of view. From the same viewpoint as above, the thickness of the vapor-deposited film made of aluminum oxide is more preferably 7 nm or more and 15 nm or less.

[0103] The thickness of the vapor-deposited film made of silicon oxide is preferably 10 nm or more and 50 nm or less. When the thickness is 10 nm or more, sufficient gas barrier properties can be obtained. Furthermore, when the thickness is 50 nm or less, the occurrence of cracks due to deformation caused by internal stress in the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that, when the thickness exceeds 50 nm, the cost is likely to increase due to an increase in the amount of material used and a prolonged film formation time, and is therefore not preferable from an economical point of view. From the same viewpoint as above, the thickness of the vapor-deposited film made of silicon oxide is more preferably 20 nm or more and 40 nm or less.

[0104] The inorganic compound layer 15 can be formed by, for example, vacuum film formation. For the vacuum film formation, physical vapor deposition or chemical vapor deposition can be used. Examples of physical vapor deposition include, but are not limited to, vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition include, but are not limited to, thermal CVD (Chemical Vapor Deposition), plasma CVD, and photo CVD.

[0105] In the vacuum film formation, resistance heating vacuum deposition, EB (Electron Beam) heating vacuum deposition, induction heating vacuum deposition, sputtering, reactive sputtering, dual magnetron sputtering, plasma enhanced chemical vapor deposition (PECVD), etc. are particularly preferably used. In terms of productivity, the vacuum deposition is currently the most excellent. As a heating means for the vacuum deposition, it is preferable to use any one of the electron beam heating method, the resistance heating method, and the induction heating method.

[0106] Metal vapor deposition films such as aluminum are suitable for disposal. If the required light-shielding and barrier properties are satisfied, an aluminum vapor deposition film can be used instead of the inorganic compound layer 15. The thickness of the aluminum vapor deposition layer is preferably 40 nm to 80 nm. The aluminum vapor deposition layer can be provided on the intermediate layer 18, the base layer 11, or the sealant layer 12. When the aluminum vapor deposition layer is provided on the sealant layer 12, it preferably has a thickness of about 40 nm, and when the aluminum vapor deposition layer is provided on the intermediate layer 18 or the base layer 11, it preferably has a thickness of about 80 nm.

[0107] <2.6> Covering layer The coating layer 17 is a first coating layer. The coating layer 17 coats the inorganic compound layer 15. A laminate of the inorganic compound layer 15 and the coating layer 17 constitutes a first gas barrier layer that improves the oxygen barrier property and water vapor barrier property of the laminate 10. The first gas barrier layer may include only the inorganic compound layer 15, or may include only the coating layer 17. The laminate 10 may not include the first gas barrier layer.

[0108] The coating layer 17 can be formed, for example, by coating. For this coating, a coating liquid containing a resin such as polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, polyvinylidene chloride, polyacrylonitrile, or epoxy resin can be used. Additives such as organic or inorganic particles, layered compounds, and curing agents may be added to this coating liquid.

[0109] The coating layer 17 may be an organic-inorganic composite layer containing at least one of a metal alkoxide, a hydrolysate of a metal alkoxide, and a reaction product of a metal alkoxide or a hydrolysate of a metal alkoxide, and a water-soluble polymer. This organic-inorganic composite layer may further contain at least one of a silane coupling agent, a hydrolysate of a silane coupling agent, and a reaction product of a silane coupling agent or a hydrolysate of a silane coupling agent.

[0110] Examples of metal alkoxides and their hydrolysates include those represented by the general formula M(OR), such as tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3]. n and hydrolysates thereof. One of these may be used alone, or two or more may be used in combination.

[0111] The total content of the metal alkoxide, its hydrolysate or their reaction products in the coating liquid used for forming the organic-inorganic composite layer may be, for example, 40% by mass or more, 50% by mass or more, or 65% by mass or more from the viewpoint of oxygen barrier property. The total content of the metal alkoxide, its hydrolysate or their reaction products in the coating liquid may be, for example, 70% by mass or less.

[0112] The water-soluble polymer contained in the organic-inorganic composite layer is not particularly limited, and examples thereof include polyvinyl alcohol-based polymers, polysaccharides such as starch, methyl cellulose, and carboxymethyl cellulose, and hydroxyl-containing polymers such as acrylic polyol-based polymers. From the viewpoint of further improving the oxygen gas barrier property, the water-soluble polymer preferably includes a water-soluble polymer of polyvinyl alcohol-based polymer. The number-average molecular weight of the water-soluble polymer is, for example, within the range of 40,000 to 180,000.

[0113] The polyvinyl alcohol-based water-soluble polymer contained in the organic-inorganic composite layer can be obtained, for example, by saponifying polyvinyl acetate (including partial saponification). This water-soluble polymer may have several tens of percent of acetate groups remaining, or may have only a few percent of acetate groups remaining.

[0114] The content of the water-soluble polymer in the coating liquid used to form the organic-inorganic composite layer may be, for example, 15% by mass or more, or 20% by mass or more, from the viewpoint of oxygen barrier property. Also, the content of the water-soluble polymer in the coating liquid may be, for example, 50% by mass or less, or 45% by mass or less, from the viewpoint of oxygen barrier property.

[0115] The silane coupling agent used in the organic-inorganic composite layer includes a silane coupling agent having an organic functional group. Such silane coupling agents include ethyltrimethoxysilane, vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, and γ-methacryloxypropylmethyldimethoxysilane. The silane coupling agent selected from these, its hydrolyzate, and their reaction product can be used alone or in combination of two or more.

[0116] It is preferable to use a silane coupling agent having an epoxy group as an organic functional group. Examples of silane coupling agents having an epoxy group include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Silane coupling agents having an epoxy group may have an organic functional group different from the epoxy group, such as a vinyl group, an amino group, a methacryl group or a ureyl group, or an isocyanate group. These may also be derivatives, polyfunctionalized, or composites. The silane coupling agents selected from these, their hydrolyzates, and their reaction products may be used alone or in combination of two or more.

[0117] A silane coupling agent having an organic functional group, its hydrolysate, or a reaction product thereof can further improve the oxygen barrier property of the coating layer 17 and the adhesion to adjacent layers by interaction between the organic functional group and the hydroxyl group of the water-soluble polymer. In particular, when the silane coupling agent, its hydrolysate, or a reaction product thereof has an epoxy group and the water-soluble polymer is polyvinyl alcohol (PVA), the oxygen barrier property and the adhesion to adjacent layers can be further improved by interaction between the epoxy group and the hydroxyl group of the PVA.

[0118] The total content of the silane coupling agent, its hydrolysate and their reaction products in the coating liquid used for forming the organic-inorganic composite layer may be, for example, 1% by mass or more, or 2% by mass or more, from the viewpoint of oxygen barrier property. Also, the total content of the silane coupling agent, its hydrolysate and their reaction products in the coating liquid may be, for example, 15% by mass or less, or 12% by mass or less, from the viewpoint of oxygen barrier property.

[0119] The thickness of the coating layer 17 is preferably 50 nm or more and 1000 nm or less, and more preferably 100 nm or more and 500 nm or less. When the thickness of the coating layer 17 is 50 nm or more, high gas barrier properties tend to be obtained, and when it is 1000 nm or less, sufficient flexibility tends to be maintained.

[0120] <2.7>Adhesive layer The adhesive layer 13A bonds the base material layer 11, on which the printing layer 14 is provided, to the intermediate layer 18. The adhesive layer 13B bonds the intermediate layer 18, on which the inorganic compound layer 15 and the coating layer 17 are provided, to the sealant layer 12. When the intermediate layer 18 is omitted, one of the adhesive layers 13A and 13B can be omitted.

[0121] The adhesive layers 13A and 13B are made of at least one type of adhesive. The adhesive may be a one-component curing adhesive, a two-component curing adhesive, or a non-curing adhesive. The adhesive may be a solventless adhesive, or a solvent-based adhesive.

[0122] Examples of the adhesive include epoxy adhesives such as polyether adhesives, polyester adhesives, silicone adhesives, and polyamine adhesives, urethane adhesives, rubber adhesives, vinyl adhesives, silicone adhesives, epoxy adhesives, phenol adhesives, and olefin adhesives. Adhesives containing biomass components can also be used preferably. The adhesive is preferably a polyamine adhesive or a urethane adhesive having gas barrier properties. Specific examples of gas barrier adhesives include "Maxive" manufactured by Mitsubishi Gas Chemical Company, Inc. and "Paslim" manufactured by DIC Corporation.

[0123] The adhesive layers 13A and 13B may be a cured product of a resin composition containing a polyester polyol and an isocyanate compound, or may be a cured product of a resin composition further containing a phosphoric acid-modified compound as necessary. Among the resin compositions used for the adhesive layers 13A and 13B, for example, a polyol as a main agent and an isocyanate compound as a curing agent, or a polyamine resin as a main agent and an epoxy compound as a curing agent, it is preferable that either one or both of the main agent and the curing agent have not only a straight-chain structure but also a bent structure, or contain a unit that can form such a structure. For example, by incorporating a compound having a substituent at the ortho-position or meta-position of an aromatic ring into these structures, it is possible to form not only a straight-chain crosslink but also a bent crosslinked structure in the cured coating. This bent crosslinked structure controls the orientation of the molecules, and thus can contribute to the oxygen barrier property and water vapor barrier property. If necessary, an inorganic compound such as an inorganic layered compound may be blended into the resin composition to further improve the barrier property. This can further improve the oxygen barrier property and water vapor barrier property of the laminate 10.

[0124] The thickness of each of the adhesive layers 13A and 13B is preferably in the range of 0.1 μm to 20 μm, more preferably in the range of 0.5 μm to 10 μm, and even more preferably in the range of 1 to 5 μm.

[0125] The adhesive layers 13A and 13B can be formed by applying and drying onto the intermediate layer 18 or the sealant layer 12 using a conventional method such as a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fontaine method, or a transfer roll coating method.

[0126] <2.8>Protective layer The protective layer 16 is a first protective layer. The protective layer 16 is the outermost layer of the laminate 10, and covers the back surface of the base layer 11 opposite to the sealant layer 12. The protective layer 16 may be omitted.

[0127] The protective layer 16 contains a cured product of a thermosetting resin. The thermosetting resin is not particularly limited as long as it produces a cured product having heat resistance, and examples thereof include polyurethane resin, polyester resin, polyamide resin, polyamideimide resin, acrylic resin, epoxy resin, and water-soluble polymer. The protective layer 16 may contain one type of cured product of a thermosetting resin, or may contain two or more types of cured products of a thermosetting resin. An inorganic filler may be blended into the protective layer 16, for example, for the purpose of improving heat resistance.

[0128] In one embodiment, the protective layer 16 preferably contains a water-soluble polymer, and more preferably is an organic-inorganic composite layer that further contains an organometallic compound.

[0129] Examples of the water-soluble polymer include polyvinyl alcohols, polysaccharides such as starch, methyl cellulose, and carboxymethyl cellulose, and hydroxyl-containing polymers such as acrylic polyols. In one embodiment, the protective layer 16 preferably contains a polyvinyl alcohol-based hydroxyl-containing polymer that the coating layer 17 may contain.

[0130] The protective layer 16 preferably contains at least one of a metal alkoxide, a hydrolysate of a metal alkoxide, and a reaction product of a metal alkoxide or a hydrolysate of a metal alkoxide as an organometallic compound. Examples of the metal alkoxide include tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3], which have the general formula M(OR). n Examples of the above-mentioned are represented by the following formula:

[0131] Moreover, the protective layer 16 preferably further contains, as the organometallic compound, at least one of a silane coupling agent, a hydrolysate of a silane coupling agent, and a reaction product of a silane coupling agent or a hydrolysate of a silane coupling agent.

[0132] In one embodiment, the protective layer 16 can be formed using a coating liquid for forming the coating layer 17. When the laminate 10 includes the coating layer 17, the protective layer 16 may be a layer formed using the same coating liquid as the coating liquid used to form the coating layer 17. The protective layer 16 is not limited to the method using the above-mentioned coating liquid, and can also be formed by co-extrusion of the polyethylene resin constituting the base layer 11 or the base layer 21 and a thermoplastic resin having a high melting point and heat resistance. In this case, resins having a high melting point such as polyester resin, polyamide resin, polypropylene resin, and polymethylpentene resin can be used as the thermoplastic resin having a high melting point. At this time, an adhesive resin can be interposed between the polyethylene resin constituting the base layer 11 or the base layer 21 and the thermoplastic resin having a high melting point and heat resistance, taking into consideration the adhesiveness between them.

[0133] The protective layer 16 reduces thermal damage to the surface of the laminate 10 during heat sealing. By providing the protective layer 16, which has excellent heat resistance, as the outermost layer of the laminate 10, heat sealability and productivity are ensured even though the laminate 10 uses polyethylene resin, which has poor heat resistance, as a base material.

[0134] The thickness of the protective layer 16 is preferably within the range of 0.3 μm to 3 μm. If the protective layer 16 is too thin, it tends to be difficult to achieve high heat resistance. If the protective layer 16 is too thick, it tends to be difficult to sufficiently dry the cured resin film during the manufacturing process of the laminate 10.

[0135] Furthermore, the protective layer 16 is expected to not only prevent defects during bag making by imparting heat resistance to the base layer 11, but also to prevent pinholes during transportation.

[0136] <2.9> Other layers The laminate 10 may further include one or more other layers. For example, the laminate 10 may further include an anchor coat layer covering the surface of the intermediate layer 18 on which the inorganic compound layer 15 is formed. Alternatively, the laminate 10 may further include an anchor coat layer covering the surface of the base layer 11 facing the adhesive layer 13A. Alternatively, the laminate 10 may further include an anchor coat layer covering the surface of the intermediate layer 18 on which the inorganic compound layer 15 is formed, and an anchor coat layer covering the surface of the base layer 11 facing the adhesive layer 13A.

[0137] The anchor coat layer can be formed using a known anchor coat agent. This can improve the adhesion between layers, for example, between the intermediate layer 18 and the inorganic compound layer 15 made of a metal oxide. Examples of the anchor coat agent include polyester polyurethane resin and polyether polyurethane resin. In addition, as the anchor coat layer, a polyurethane cured coating film in which an isocyanate compound is reacted with various hydroxyl group-containing polymers such as polyester polyol, polyether polyol, and acrylic polyol can be provided. In addition, in order to improve the adhesion between the substrate and the layer formed by vapor deposition, the above-mentioned various silane coupling agents can be blended into the anchor coat agent. From the viewpoint of heat resistance and interlayer adhesive strength, the anchor coat agent is preferably a polyester polyurethane resin.

[0138] <3> Bottom film FIG. 5 is a cross-sectional view showing an example of a laminate that can be used as the bottom film of the standing pouch of FIG.

[0139] 5 can be used for the bottom film 112. As described below, various modifications of the laminate 20 are possible. The laminates according to these modifications can also be used for the bottom film 112.

[0140] The laminate 20 includes a protective layer 26, a base layer 21, a printed layer 24, an adhesive layer 23A, an intermediate layer 28, an inorganic compound layer 25, a coating layer 27, an adhesive layer 23B, and a sealant layer 22, in this order.

[0141] As described below, the base layer 21, the intermediate layer 28, and the sealant layer 22 contain polyethylene. The laminate 20 preferably contains polyethylene at a rate of 90% by mass or more. By containing polyethylene at a rate of 90% by mass or more, high recyclability can be achieved.

[0142] <3.1> Base material layer The base layer 21 is a second base layer. The base layer 21 contains polyethylene. Preferably, the base layer 21 is made of polyethylene.

[0143] As described above, the crystallinity of the base layer 21 is greater than that of the base layer 11. The crystallinity of the base layer 21 is preferably within a range of 35% to 95%. The crystallinity of the base layer 21 is more preferably 40% or more, and further preferably 50% or more. Moreover, the crystallinity of the base layer 21 is more preferably 90% or less.

[0144] The base material layer 21 may be a non-stretched film or a stretched film. The base material layer 21 is preferably a stretched film. When the base material layer 21 is a stretched film, the base material layer 21 may be a uniaxially stretched film or a biaxially stretched film. When the base material layer 21 has a higher crystallinity than the base material layers 11 of the main body films 111A and 111B and is a stretched film, the laminate 20 including such a base material layer 21 has a particularly high impact strength when used as the bottom film 112 of the standing pouch 110.

[0145] As described above, the base layer 21 has a higher degree of crystallinity than the base layer 11. The laminate 20 including such a base layer 21 has high impact resistance when used as the bottom film 112 of the standing pouch 110, and has excellent drop resistance when filled with the contents 120 to form the packaged article 100. The laminate 20 including such a base layer 21 also has excellent puncture strength. From these viewpoints, the crystallinity of the base layer 21 is preferably within the above-mentioned range.

[0146] Polyethylene is a crystalline polymer, and therefore has both crystalline and amorphous parts. Polyethylene with a high degree of crystallinity has a high ratio of crystalline parts. This crystalline part controls the elastic part in the viscoelastic behavior of the resin, so a high degree of crystallinity improves the rigidity of the film.

[0147] Due to the influence of this viscoelastic behavior, in films with high crystallinity, the strain associated with the plastic deformation of the resin is also large. As a result, the effect of suppressing the deformation of the resin against the strain generated by the instantaneous impact applied to the film is obtained, and breakage is less likely to occur. Therefore, the laminate 20 having the base layer 21 containing polyethylene and having high crystallinity can have high puncture strength.

[0148] The polyethylene constituting the base layer 21 is preferably an ethylene-α-olefin copolymer copolymerized with an α-olefin. The reason for this is that when the crystallinity of the base layer 21 of the base material is adjusted to 35% or more, tie molecules are likely to form between the crystals. Not only is improved crystallinity imparting rigidity, but the formation of tie molecules is also expected to improve toughness, and when such a base layer 21 is used for the bottom film, a standing pouch with particularly excellent drop resistance can be realized. In this case, the ethylene-α-olefin copolymer in the base layer 21 may be used alone or in a mixture with other polyethylenes.

[0149] Except for the above, the base material layer 21 may have the same configuration as that described above for the base material layer 11.

[0150] <3.2> Sealant layer The sealant layer 22 is a second sealant layer. The sealant layer 22 faces the base layer 21. The sealant layer 22 contains polyethylene. Preferably, the sealant layer 12 is made of polyethylene. The sealant layer 22 may have the same structure as that described above for the sealant layer 12.

[0151] <3.3>Printing layer The printed layer 24 is a second printed layer. The printed layer 24 is provided on the surface of the base layer 21 facing the sealant layer 22, i.e., on the back surface of the base layer 21. The position at which the printed layer 24 is provided is not limited. That is, the printed layer 24 may be provided on the surface of the base layer 21, or may be provided at any position between the base layer 21 and the sealant layer 22. For example, the printed layer 24 may be provided on any surface of the intermediate layer 28. The laminate 20 may also include multiple printed layers. The printed layer 24 may be omitted.

[0152] The printing layer 24 can be formed using the same ink as that described above for the printing layer 14. The printing layer 24 can be formed by the same method as that described above for the printing layer 14.

[0153] <3.4> Middle class The intermediate layer 28 is a second intermediate layer. The intermediate layer 28 is provided between the base material layer 21 and the sealant layer 22. Here, the intermediate layer 28 is provided between the base material layer 21 and the sealant layer 22 such that the printed layer 24 is interposed between the base material layer 21 and the intermediate layer 28. The intermediate layer 28 may be omitted.

[0154] The intermediate layer 28 contains polyethylene. As the polyethylene, for example, the polyethylene contained in the base layer 11 described above can be used.

[0155] The intermediate layer 28 may have the same configuration as that described above for the intermediate layer 18. The intermediate layer 28 may be manufactured by the same method as that described above for the intermediate layer 18.

[0156] <3.5>Inorganic compound layer The inorganic compound layer 25 is a second inorganic compound layer. The inorganic compound layer 25 is provided on one surface of the intermediate layer 28. Here, the inorganic compound layer 25 is provided on the surface of the intermediate layer 28 facing the sealant layer 22. The inorganic compound layer 25 may be provided on the surface of the intermediate layer 28 facing the base material layer 21. The inorganic compound layer 25 may be provided on the surface of the base material layer 21 facing the sealant layer 22, here between the base material layer 21 and the printed layer 24. The inorganic compound layer 25 may be provided on the surface of the base material layer 21 opposite to the sealant layer 22, here as the outermost layer of the laminate. The inorganic compound layer 25 may be omitted.

[0157] The inorganic compound layer 25 may have the same configuration as that described above for the inorganic compound layer 15. The inorganic compound layer 25 may be formed by the same method as that described above for the inorganic compound layer 15.

[0158] Metal vapor deposition films such as aluminum are suitable for disposal. If the required light-shielding and barrier properties are satisfied, an aluminum vapor deposition film can be used instead of the inorganic compound layer 25. The thickness of the aluminum vapor deposition layer is preferably 40 nm to 80 nm. The aluminum vapor deposition layer can be provided on the intermediate layer 28, the base layer 21, or the sealant layer 22. When the aluminum vapor deposition layer is provided on the sealant layer 22, it preferably has a thickness of about 40 nm, and when the aluminum vapor deposition layer is provided on the intermediate layer 28 or the base layer 21, it preferably has a thickness of about 80 nm.

[0159] <3.6> Covering layer The coating layer 27 is a second coating layer. The coating layer 27 coats the inorganic compound layer 25. A laminate of the inorganic compound layer 25 and the coating layer 27 constitutes a second gas barrier layer that improves the oxygen barrier property and water vapor barrier property of the laminate 20. The second gas barrier layer may include only the inorganic compound layer 25, or may include only the coating layer 27. The laminate 20 may not include the second gas barrier layer.

[0160] The covering layer 27 may have the same structure as that described above for the covering layer 17. The covering layer 27 may be formed by the same method as that described above for the covering layer 17.

[0161] <3.7>Adhesive layer The adhesive layer 23A bonds the base material layer 21, on which the printing layer 24 is provided, to the intermediate layer 28. The adhesive layer 23B bonds the intermediate layer 28, on which the inorganic compound layer 25 and the coating layer 27 are provided, to the sealant layer 22. When the intermediate layer 28 is omitted, one of the adhesive layers 23A and 23B can be omitted.

[0162] The adhesive layers 23A and 23B are made of the same adhesive as described above for the adhesive layers 13A and 13B. The adhesive layers 23A and 23B may have the same configuration as described above for the adhesive layers 13A and 13B. The adhesive layers 23A and 23B may be formed by the same method as described above for the adhesive layers 13A and 13B.

[0163] <3.8>Protective layer The protective layer 26 is a second protective layer. The protective layer 26 is the outermost layer of the laminate 20, and covers the back surface of the base layer 21 opposite to the sealant layer 22. The protective layer 26 may be omitted.

[0164] The protective layer 26 may have the same structure as that described above for the protective layer 16. The protective layer 26 may be formed by the same method as that described above for the protective layer 16.

[0165] <3.9> Other layers The laminate 20 may further include one or more other layers. For example, the laminate 20 may further include an anchor coat layer that covers the surface of the intermediate layer 28 on which the inorganic compound layer 25 is formed. Alternatively, the laminate 20 may further include an anchor coat layer that covers the surface of the base layer 21 facing the adhesive layer 23A. Alternatively, the laminate 20 may further include an anchor coat layer that covers the surface of the intermediate layer 28 on which the inorganic compound layer 15 is formed, and an anchor coat layer that covers the surface of the base layer 21 facing the adhesive layer 23A. The anchor coat layer can be formed using the anchor coat agent described above for the anchor coat layer of the laminate 10.

[0166] <4> effect The above-mentioned standing pouch 110 is less likely to have defects during its production, and the packaged article 100 obtained by filling it with the contents 120 has excellent drop resistance. This will be described below.

[0167] When a packaged article formed by filling a standing pouch 110 with contents 120 is dropped upright, the impact easily destroys the bottom film 112. In particular, when the volume of the contents 120 is large, the impact of dropping upright is large and the bottom film 112 is easily destroyed. In the above-mentioned packaged article 100, the crystallinity of the base material layer 21 of the bottom film 112 is sufficiently large compared with the crystallinity of each of the base material layers 11 of the main films 111A and 111B. Therefore, the impact resistance strength of the bottom film 112 is high, and the packaged article 100 has excellent drop resistance. This drop resistance effect is particularly noticeable when the volume of the contents 120 is large. In particular, when the base layer 21 of the bottom film 112 contains an ethylene-α-olefin copolymer, adjusting the crystallinity to 35% or more makes it easier for tie molecules to form between the crystals, and not only is improved crystallinity imparting rigidity, but the formation of tie molecules is also expected to improve toughness, thereby improving the drop resistance of the standing pouch through improved rigidity and toughness.

[0168] In manufacturing the standing pouch 110, the laminate 20 to be used as the bottom film 112 is folded in half. Then, the folded laminate 20 is sandwiched between a pair of laminates 10 to be used as the main body films 111A and 111B, and they are heat-sealed.

[0169] A bag making machine used to manufacture a standing pouch performs, for example, a heat sealing process and a cutting process in this order. In the heat sealing process, the laminate 20, which is folded in half so as to form a mountain fold when viewed from the sealant layer 22 during the conveying process, is sandwiched between a pair of laminates 10 conveyed so that the sealant layers 12 face each other, and these are heat sealed with a heat seal bar. Specifically, bottom sealing, point sealing, and side sealing are performed, thereby forming heat sealed parts HS1, HS4, HS2A, and HS2B. The length direction of the heat sealed part HS1 is perpendicular to the conveying direction. In the cutting process, the composite obtained by heat sealing is cut into individual standing pouches 110.

[0170] The packaged article 100 can be manufactured, for example, by using a filling machine that performs a filling step and a heat sealing step in this order. In the filling step, the content 120 is filled into the standing pouch 110. In the heat sealing step, the opening of the standing pouch 110 is heat sealed with a heat seal bar to form a heat sealed portion HS3. In this manner, the packaged article 100 is obtained.

[0171] A base layer having a high degree of crystallinity shrinks significantly due to the heat applied during heat sealing, etc. Therefore, a laminate including a base layer having a high degree of crystallinity is prone to warping when heat is applied.

[0172] If the base layer of the laminate used as the main film and the base layer of the laminate used as the bottom film have high crystallinity and all of these laminates are significantly warped by heat, the risk of defective products and troubles with the manufacturing equipment increases. In addition, if all of these laminates are prone to warping by heat, it becomes difficult to adjust the manufacturing conditions to prevent the above-mentioned problems.

[0173] In the above-mentioned standing pouch 110, the crystallinity of each of the base material layers 11 of the main body films 111A and 111B is sufficiently smaller than the crystallinity of the base material layer 21 of the bottom film 112. Therefore, in the manufacture of the standing pouch 110, the laminate 10 used as the main body films 111A and 111B does not warp significantly due to heat. Therefore, the standing pouch 110 is less likely to suffer from defects such as defective products and manufacturing equipment troubles during its manufacture.

[0174] Furthermore, in the standing pouch 110, the polyethylene content of each of the main films 111A and 111B and the bottom film 112 can be set to 90% by mass or more. Such a standing pouch 110 also has excellent recyclability. EXAMPLES

[0175] The results of tests carried out in relation to the present invention are described below.

[0176] (1) Manufacturing of standing pouches (1.1) Example 1 The standing pouch 110 described with reference to FIGS. 1 to 5 was manufactured by the following method.

[0177] (1.1.1) Manufacturing of laminates to be used as main film The laminate 10 used as the main films 111A and 111B was produced by the following method. Here, the printed layer 14 and the protective layer 16 were omitted.

[0178] A high-density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2% was used as the base layer 11. The crystallinity shown in this example and the examples and comparative examples described below was measured by the above-mentioned measurement method.

[0179] A non-oriented high-density polyethylene film having a thickness of 32 μm and having been subjected to a corona treatment on both sides was used as the intermediate layer 18. On one side of the intermediate layer 18, an anchor coat layer, an inorganic compound layer 15, and a coating layer 17 (not shown) were sequentially formed.

[0180] When forming the anchor coat layer, first, the anchor coat agent was prepared by the following method. That is, acrylic polyol and tolylene diisocyanate were mixed so that the number of NCO groups of tolylene diisocyanate was equal to the number of OH groups of acrylic polyol, and diluted with ethyl acetate so that the total solid content (total amount of acrylic polyol and tolylene diisocyanate) was 5 mass%. β-(3,4-epoxycyclohexyl)trimethoxysilane was further added to the diluted mixed liquid so that it was 5 mass parts per 100 mass parts of the total amount of acrylic polyol and tolylene diisocyanate, and these were mixed to prepare the anchor coat agent.

[0181] Next, the anchor coating agent prepared by the above method was applied by gravure coating to one side of the intermediate layer 18 that had been subjected to the corona treatment. This application was performed so that the thickness of the coating film in the dry state was 0.1 μm. In this way, an anchor coating layer was formed.

[0182] The inorganic compound layer 15 is a transparent silicon oxide (SiO x A vapor-deposited film having a thickness of 40 nm was formed on the anchor coat layer. The O / Si ratio of the vapor-deposited film was set to 1.8 by adjusting the type of material used for vapor deposition.

[0183] In forming the covering layer 17, first, a coating solution for forming the covering layer was prepared by the following method. That is, a coating liquid for forming a coating layer containing an organic / inorganic mixture (hereinafter, simply referred to as the "coating liquid") was prepared by mixing the following liquids A, B, and C in a mass ratio of 70 / 20 / 10, respectively. Liquid A: A hydrolysis solution with a solid content of 5 mass% (SiO2 equivalent) obtained by adding 72.1 g of 0.1N hydrochloric acid to 17.9 g of tetraethoxysilane (Si(OC2H5)4) and 10 g of methanol and stirring for 30 minutes. Liquid B: 5% by mass solution of polyvinyl alcohol in water / methanol (mass ratio of water:methanol is 95:5). Liquid C: A hydrolysis solution in which 1,3,5-tris(3-trialkoxysilylpropyl)isocyanurate was diluted with a mixture of water and isopropyl alcohol (water:isopropyl alcohol mass ratio 1:1) to a solid content of 5 mass%.

[0184] Next, the coating solution for forming a coating layer prepared as described above was applied to the inorganic compound layer 15 so that the thickness of the coating film in a dry state became 0.3 μm. In this manner, a coating layer 17 made of an organic-inorganic mixture was formed.

[0185] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate layer 18 opposite to the surface on which the inorganic compound layer 15 and the like were formed, to form an adhesive layer 13A. Next, the base material layer 11 and the intermediate layer 18 were bonded together with the adhesive layer 13A sandwiched therebetween.

[0186] A non-oriented linear low-density polyethylene film having a thickness of 120 μm was used as the sealant layer 12. A dry lamination adhesive (urethane adhesive) was applied to one surface of the sealant layer 12 to form an adhesive layer 13B. The sealant layer 12 was then attached to a composite including the base layer 11 and the intermediate layer 18 such that the sealant layer 12 and the coating layer 17 faced each other with the adhesive layer 13B sandwiched therebetween. In this manner, the laminate 10 was produced.

[0187] (1.1.2) Preparation of the laminate to be used as the bottom film The laminate 20 used as the bottom film 112 was manufactured by the following method. Here, the printing layer 24 and the protective layer 26 were omitted.

[0188] As the base layer 21, a linear low-density polyethylene film, which is an ethylene-α-olefin copolymer, having a thickness of 25 μm and a crystallinity of 54.1% was used.

[0189] The sealant layer 22 and intermediate layer 28 were made of the materials used as the sealant layer 12 and intermediate layer 18 in (1.1.1), respectively. The inorganic compound layer 25, coating layer 27, anchor coat layer, adhesive layer 23A and adhesive layer 23B were made of the materials used as the inorganic compound layer 15, coating layer 17, anchor coat layer, adhesive layer 13A and adhesive layer 13B in (1.1.1), respectively.

[0190] The laminate 20 was then produced in the same manner as described above for the laminate 10 in (1.1.1).

[0191] (1.1.3) Bag making Two rolls each made of laminate 10 and a roll made of laminate 20 were placed in a bag making machine. The bag making machine was then operated to produce a standing pouch 110 that was 240 mm long, 160 mm wide, had a seal width of 5 mm, and a bottom seal fold width of 40 mm, and was capable of containing 800 mL of contents.

[0192] The bag making machine used here performs the heat sealing process and the cutting process in this order. In the heat sealing process, the laminate 20, which has been folded in half so as to form a mountain fold when viewed from the sealant layer 22 during the conveying process, is sandwiched between a pair of laminates 10 conveyed so that the sealant layers 12 face each other, and these are heat sealed with a heat seal bar. Specifically, bottom sealing, point sealing, and side sealing are performed, thereby forming heat sealed parts HS1, HS4, HS2A, and HS2B. The length direction of the heat sealed part HS1 is perpendicular to the conveying direction. In the cutting process, the composite obtained by heat sealing is cut into individual standing pouches 110.

[0193] (1.2) Example 2 The standing pouch 110 described with reference to Figures 1 to 5 was manufactured by the following method. That is, in this example, instead of using a linear low-density polyethylene film having a thickness of 25 µm and a crystallinity of 54.1% as the base material layer 21 of the laminate 20, a high-density polyethylene film having a thickness of 25 µm and a crystallinity of 55.9% was used. Except for this point, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0194] (1.3) Example 3 The standing pouch 110 described with reference to Figures 1 to 5 was manufactured by the following method. That is, in this example, when manufacturing the bottom film laminate 20, the intermediate layer 28, the adhesive layer 23A, the anchor coat layer, the inorganic compound layer 25, and the coating layer 27 were omitted, and the base material layer 21 and the sealant layer 22 were bonded together via the adhesive layer 23B. In addition, when manufacturing the main film laminate 10, the intermediate layer 18 was left as it was, but the anchor coat layer, the inorganic compound layer 15, and the coating layer 17 were omitted. Except for these points, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0195] (1.4) Example 4 The standing pouch 110 described with reference to Figs. 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 20 as the bottom film, the anchor coat layer, the inorganic compound layer, and the coating layer similar to those formed on the intermediate layer 28 in Example 1 were sequentially formed on the base layer 21, while the intermediate layer 28 and the adhesive layer 23A, the anchor coat layer, the inorganic compound layer 25, and the coating layer 27 formed thereon were omitted, and the coating layer-forming surface of the base layer 21 was bonded to the sealant layer 22 via the adhesive layer 23B. In addition, instead of the unstretched linear low-density polyethylene film having a thickness of 120 μm, a unstretched linear low-density polyethylene film having a thickness of 150 μm was used as the sealant layer 22. Except for these points, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0196] (1.5) Example 5 The standing pouch 110 described with reference to Fig. 1 to Fig. 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, the anchor coat layer, the inorganic compound layer, and the coating layer were sequentially formed on the base layer 11, similar to those formed on the intermediate layer 18 in Example 1, while the intermediate layer 18 and the adhesive layer 13A, the anchor coat layer, the inorganic compound layer 15, and the coating layer 17 formed thereon were omitted, and the coating layer-forming surface of the base layer 11 was bonded to the sealant layer 12 via the adhesive layer 13B. For the laminate 20 as the bottom film, the anchor coat layer, the inorganic compound layer, and the coating layer were sequentially formed on the base layer 21, similar to those formed on the intermediate layer 28 in Example 1, while the intermediate layer 28 and the adhesive layer 23A, the anchor coat layer, the inorganic compound layer 25, and the coating layer 27 formed thereon were omitted, and the coating layer-forming surface of the base layer 21 was bonded to the sealant layer 22 via the adhesive layer 23B. Except for these points, in this example, the standing pouch 110 was produced in the same manner as in Example 1.

[0197] (1.6) Example 6 The standing pouch 110 described with reference to Figures 1 to 5 was manufactured by the following method. That is, in this example, instead of using a non-oriented high-density polyethylene film having a thickness of 32 μm and having been subjected to corona treatment on both sides as the intermediate layer 28 of the laminate 20 as the bottom film, a biaxially oriented linear low-density polyethylene film having a thickness of 25 μm was used. Except for this point, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0198] (1.7) Example 7 The standing pouch 110 described with reference to Figures 1 to 5 was manufactured by the following method. That is, in this example, instead of using a high density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2% as the base layer 11 of the main film, a high density polyethylene film having a thickness of 30 μm and a crystallinity of 27.6% was used. Except for this point, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0199] (1.8) Example 8 The standing pouch 110 described with reference to Figs. 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, the covering layer 17 was omitted, and an epoxy-amine-based gas barrier adhesive was used for the adhesive layer 13B instead of the dry lamination adhesive (urethane adhesive). Also, for the laminate 20 as the bottom film, the covering layer 27 was omitted, and an epoxy-amine-based gas barrier adhesive was used for the adhesive layer 23B instead of the dry lamination adhesive (urethane adhesive). Except for these points, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0200] (1.9) Example 9 The standing pouch 110 described with reference to Figs. 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, an anchor coat layer and an inorganic compound layer similar to those formed on the intermediate layer 18 in Example 1 were sequentially formed on the base material layer 11. Then, the intermediate layer 18 and the adhesive layer 13A, the anchor coat layer, the inorganic compound layer 15, and the coating layer 17 formed thereon were omitted, and instead of using an adhesive for dry lamination (urethane adhesive) for the adhesive layer 13B, an epoxy-amine gas barrier adhesive was used, which was applied on the inorganic compound layer to bond the inorganic compound layer-forming surface of the base material layer 11 to the sealant layer 12. For the laminate 20 as the bottom film, an anchor coat layer and an inorganic compound layer similar to those formed on the intermediate layer 28 in Example 1 were sequentially formed on the base material layer 21. Then, the intermediate layer 28 and the adhesive layer 23A, anchor coat layer, inorganic compound layer 25, and coating layer 27 formed thereon were omitted, and instead of using an adhesive for dry lamination (urethane adhesive) for the adhesive layer 23B, an epoxy-amine gas barrier adhesive was used, which was applied onto the inorganic compound layer to bond the inorganic compound layer-forming surface of the base material layer 21 to the sealant layer 22. Except for these points, in this example, a standing pouch 110 was produced by the same method as in Example 1.

[0201] (1.10) Example 10 The standing pouch 110 described with reference to Figs. 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, the anchor coat layer, the inorganic compound layer 15, and the coating layer 17 were omitted, and an epoxy-amine-based gas barrier adhesive was used instead of a dry lamination adhesive (urethane adhesive) for the adhesive layer 13B. Also, for the laminate 20 as the bottom film, the anchor coat layer, the inorganic compound layer 25, and the coating layer 27 were omitted, and an epoxy-amine-based gas barrier adhesive was used instead of a dry lamination adhesive (urethane adhesive) for the adhesive layer 23B. Except for these points, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0202] (1.11) Example 11 The standing pouch 110 described with reference to Figs. 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, a protective layer 16 having a thickness of 1 µm was formed on the opposite side of the intermediate layer bonding surface of the base material layer 11 using an organic solvent solution of polyamideimide resin (non-volatile component concentration of 5% by mass). For the laminate 20 as the bottom film, a protective layer 26 having a thickness of 1 µm was formed on the opposite side of the intermediate layer bonding surface of the base material layer 21 using an organic solvent solution of polyamideimide resin (non-volatile component concentration of 5% by mass). Except for these points, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0203] (1.12) Example 12 The standing pouch 110 described with reference to Figures 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, an aluminum vapor deposition layer having a thickness of 40 nm was provided instead of the inorganic compound layer 15. For the laminate 20 as the bottom film, an aluminum vapor deposition layer having a thickness of 40 nm was provided instead of the inorganic compound layer 25. Except for these points, in this example, the standing pouch 110 was manufactured by the same method as in Example 1.

[0204] (1.13) Example 13 The standing pouch 110 described with reference to Figs. 1 to 5 was manufactured by the following method. That is, in this example, for the laminate 10 as the main film, the intermediate layer 18 and the adhesive layer 13A, anchor coat layer, inorganic compound layer 15, and coating layer 17 formed thereon were omitted. Then, an aluminum vapor deposition layer having a thickness of 80 nm was formed on one side of the sealant layer 12, and the aluminum vapor deposition layer formed surface was bonded to the substrate 11 via the adhesive layer 13B. For the adhesive layer 13B, a urethane-based gas barrier adhesive was used instead of a dry lamination adhesive (urethane-based adhesive). Also, for the laminate 20 as the bottom film, the intermediate layer 28 and the adhesive layer 23A, anchor coat layer, inorganic compound layer 25, and coating layer 27 formed thereon were omitted. Then, an aluminum vapor deposition layer having a thickness of 80 nm was formed on one side of the sealant layer 22, and the aluminum vapor deposition layer formed surface was bonded to the substrate 21 via the adhesive layer 23B. For the adhesive layer 23B, a urethane-based gas barrier adhesive was used instead of the dry lamination adhesive (urethane-based adhesive). Except for these points, in this example, the standing pouch 110 was produced in the same manner as in Example 1.

[0205] (1.14) Comparative Example 1 In the laminate 20 for forming the bottom film 112, a high-density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2% was used as the base layer 21 instead of a linear low-density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1%. Except for this, in this example, a standing pouch was manufactured in the same manner as in Example 1.

[0206] (1.15) Comparative Example 2 In the laminate 10 for forming the main films 111A and 111B, instead of using a high-density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2%, a linear low-density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1% was used as the base material layer 11. In addition, in the laminate 20 for forming the bottom film 112, instead of using a linear low-density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1%, a high-density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2% was used as the base material layer 21. Except for these points, in this example, a standing pouch was manufactured in the same manner as in Example 1.

[0207] (1.16) Comparative Example 3 In the laminate 10 for forming the main films 111A and 111B, instead of using a high density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2%, a high density polyethylene film having a thickness of 25 μm and a crystallinity of 55.9% was used as the base material layer 11. In addition, in the laminate 20 for forming the bottom film 112, instead of using a linear low density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1%, a high density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2% was used as the base material layer 21. Except for these points, in this example, a standing pouch was manufactured by the same method as in Example 1.

[0208] (1.17) Comparative Example 4 In the laminate 10 for forming the main films 111A and 111B, a linear low-density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1% was used as the base layer 11 instead of a high-density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2%. Except for this, in this example, a standing pouch was produced in the same manner as in Example 1.

[0209] (1.18) Comparative Example 5 In the laminate 10 for forming the main films 111A and 111B, instead of using a high density polyethylene film having a thickness of 30 μm and a crystallinity of 23.2%, a high density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1% was used as the base material layer 11. In addition, in the laminate 20 for forming the bottom film 112, instead of using a linear low density polyethylene film having a thickness of 25 μm and a crystallinity of 54.1%, a high density polyethylene film having a thickness of 25 μm and a crystallinity of 55.9% was used as the base material layer 21. Except for these points, in this example, a standing pouch was manufactured in the same manner as in Example 1.

[0210] (2) Evaluation method (2.1) Occurrence of defects during bag making The occurrence of defects during bag production was examined for each of Examples 1 to 13 and Comparative Examples 1 to 5. The occurrence of defects during bag production was evaluated based on the following criteria. A: Good product rate of 90% or more B: Good product rate: 80% or more - less than 90% C: Less than 80% good product rate a: There was no pseudo-fusion of the bottom film (high crystallinity of the bottom base layer) b: There was pseudo-fusion of the bottom film (low crystallinity of the bottom base layer)

[0211] (2.2) Drop test Each of the standing pouches of Examples 1 to 13 and Comparative Examples 1 to 5 was filled with 800 mL of cold water at 5°C to produce a packaged article. Thirty packaged articles were produced for each example. The packaged article was dropped from a height of 100 cm above the ground with the bottom film facing down (upright state). The percentage of the number of packaged articles whose bottom film was broken relative to the total number of packaged articles subjected to the drop test was calculated as the "probability of breakage."

[0212] (3) Results The evaluation results are shown in Tables 1 to 3 below.

[0213] [Table 1]

[0214] [Table 2]

[0215] [Table 3]

[0216] As shown in Tables 1 to 3, in Comparative Examples 1 to 5, the bottom film was easily broken when the packaged article was dropped, or defects occurred during bag making. In contrast, in Examples 1 to 11, the bottom film was not easily broken when the packaged article was dropped, and defects did not occur frequently during bag making. A base layer with a high degree of crystallinity shrinks greatly due to heating during bag making. If the crystallinity of the base layer of both the main film and the bottom film is 35% or more, each film curls due to the influence of heat near the heat seal unit where it is supplied to the bag making device, and the rate of quality bags decreases. More specifically, the rate of bags that do not become normal increases because the film is folded or shifted during the sealing process. The yield rate can be increased by adjusting the bag making equipment, such as by slowing down the bag making speed; however, if the crystallinity of the base layer of the main film is less than 15 points lower than the crystallinity of the base layer of the bottom film, or if the crystallinity of the base layer of the main film is less than 35%, no defects will occur during bag making even under normal bag making conditions, there will be no pseudo-fusion of the bottom film, and the bottom film will be less likely to be destroyed when dropped. [Explanation of symbols]

[0217] 10... laminate, 11... base material layer, 12... sealant layer, 13A... adhesive layer, 13B... adhesive layer, 14... printed layer, 15... inorganic compound layer, 16... protective layer, 17... coating layer, 18... intermediate layer, 20... laminate, 21... base material layer, 22... sealant layer, 23A... adhesive layer, 23B... adhesive layer, 24... printed layer, 25... inorganic compound layer, 26... protective layer, 27... coating layer, 28... intermediate layer, 100... packaging article, 100A... packaging article, 110... standing pouch, 111A... main body film, 111B... main body film, 112... bottom film, 113... spout, 114... cap, 120... contents, HS1... heat sealed portion, HS2A... heat sealed portion, HS2B... heat sealed portion, HS3... heat sealed portion, HS4... heat sealed portion, MF... mountain fold portion.

Claims

1. A pair of a main film and a bottom film is provided, Each of the pair of main films includes a first base layer containing polyethylene and a first sealant layer provided on the first base layer and containing polyethylene; The bottom film includes a second substrate layer including polyethylene, and a second sealant layer including polyethylene disposed on the second substrate layer, A standing pouch, wherein the crystallinity of the second base material layer is greater than the crystallinity of the first base material layer of each of the pair of main films, the difference therebetween being 15 points or more.

2. A pair of a main film and a bottom film is provided, Each of the pair of main films includes a first base layer containing polyethylene and a first sealant layer provided on the first base layer and containing polyethylene; The bottom film includes a second substrate layer including polyethylene, and a second sealant layer including polyethylene disposed on the second substrate layer, A standing pouch, wherein the crystallinity of the second base layer is in the range of 35% to 95%, and the crystallinity of the first base layer of each of the pair of main films is in the range of 5% to 35%.

3. 2. The standing pouch according to claim 1, wherein each of the pair of main films further includes a first intermediate layer containing polyethylene and interposed between the first base layer and the first sealant layer.

4. 2. The stand-up pouch of claim 1, wherein the bottom film further comprises a second intermediate layer interposed between the second substrate layer and the second sealant layer, the second intermediate layer comprising polyethylene.

5. The standing pouch according to claim 1 , wherein each of the pair of main films further includes a first protective layer as an outermost layer facing the first sealant layer with the first base material layer sandwiched therebetween.

6. The standing pouch according to claim 5 , wherein the first protective layer contains a cured product of a thermosetting resin.

7. The standing pouch according to claim 1 , wherein the bottom film further includes a second protective layer as an outermost layer facing the second sealant layer with the second base material layer sandwiched therebetween.

8. The standing pouch according to claim 7 , wherein the second protective layer contains a cured product of a thermosetting resin.

9. The standing pouch according to claim 1 , wherein each of the pair of main films further includes a first gas barrier layer interposed between the first base layer and the first sealant layer.

10. The standing pouch according to claim 1 , wherein the bottom film further comprises a second gas barrier layer interposed between the second substrate layer and the second sealant layer.

11. 2. The standing pouch according to claim 1, wherein each of the pair of main films and the bottom film has a polyethylene content of 90% by mass or more.

12. 10. The stand-up pouch of claim 1 for containing contents having a volume within the range of 0.2L to 4.0L.

13. A standing pouch according to any one of claims 1 to 12; The contents contained in the standing pouch; A packaging article comprising:

14. 14. The package of claim 13, wherein the content volume is in the range of 0.2L to 4.0L.

Citation Information

Patent Citations

  • Sealing form for bottom gusseted standing pouch and sealing method therefor

    JP2001206384A