Hard coat film for folding type display and use of the same

The hard coat film for foldable displays addresses image distortion and cracking issues by using a controlled refractive index and simplified structure, ensuring durability and visibility in foldable displays.

JP2024160329AActive Publication Date: 2024-11-13TOYOBO CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024133957
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2024-08-09
Publication Date
2024-11-13
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

Conventional hard coat films for foldable displays suffer from image distortion, creases, and cracks due to repeated folding, and they fail to effectively suppress iris-like colors (interference spots) caused by reflected light, while also being unsuitable for mass production and requiring complex antireflection layers.

Method used

A hard coat film with a specific configuration on a polyester film, including an easily adhesive resin layer made of titanium or zirconium compounds, with controlled refractive indices in different directions to prevent cracking and distortion, and a simplified structure to reduce interference spots, ensuring durability and visibility.

Benefits of technology

The film maintains image quality without distortion or cracking, supports mass production, and reduces iris-like colors, enhancing the functionality and portability of foldable displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160329000001_ABST
    Figure 2024160329000001_ABST
Patent Text Reader

Abstract

To provide a hard coat film for a folding type display which prevents a folding crease and a crack in a folding part, is affected by a fine crack of an easily adhesive resin layer, and is excellent in suppressing iris-like color (interference spot).SOLUTION: A hard coat film for a folding type display has an easily adhesive resin layer and a hard coat layer on at least one surface of a polyester film having a thickness of 10 to 80 μm in this order, wherein the easily adhesive resin layer is obtained by curing a composition containing at least one kind of compound selected from a titanium compound and a zirconium compound, and a polyester resin, and has the easily adhesive resin layer, and the polyester film before the hard coat layer is laminated satisfies a characteristic within a specific range.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hard coat film for a foldable display, a foldable display, and a mobile terminal device, and more particularly to a foldable display and a mobile terminal device that are less susceptible to image distortion due to deformation of the film even when folded repeatedly, and the hard coat film for the foldable display. [Background technology]

[0002] As mobile terminal devices become thinner and lighter, smartphones and other mobile terminal devices are becoming more and more popular. While mobile terminal devices are required to have a variety of functions, they are also required to be convenient. For this reason, the mobile terminal devices that are currently in use must be able to perform simple operations with one hand, and must have a small screen size of around 6 inches, since they are assumed to be stored in a pocket or similar.

[0003] On the other hand, tablet devices with screen sizes of 7 to 10 inches are highly functional and can be used not only for video content and music, but also for business purposes, drawing, reading, etc. However, they cannot be operated with one hand, are less portable, and have issues with convenience.

[0004] To achieve these goals, a method has been proposed of connecting multiple displays together to make them more compact (see Patent Document 1), but this method has not become widespread because it leaves a bezel, which means the image is cut off and visibility is reduced.

[0005] In recent years, mobile terminals incorporating flexible displays and foldable displays have been proposed, which provide a large-screen display without interruption to the image and are convenient to carry around.

[0006] Here, in the case of conventional displays and mobile terminal devices that do not have a folding structure, the surface of the display can be protected by a non-flexible material such as glass, but in the case of a folding display, when a one-sided display is formed through a folding part, it is necessary to use a hard coat film that is flexible and can protect the surface. However, in a folding display, the part corresponding to a certain folding part is repeatedly folded, so that the film in that part deforms over time, causing problems such as distorting the image displayed on the display. In addition to the surface protection film, films are used in various parts of the folding display, such as polarizing plates, retardation plates, touch panel substrates, substrates of display cells such as organic EL, and protective members on the back surface, and durability against repeated folding is also required for these films.

[0007] As a method for improving durability, a method for partially changing the film thickness has been proposed (see Patent Document 2), but this method has a problem of poor mass productivity.

[0008] A method of adjusting the refractive index in the bending direction of a polyester film has also been proposed (see Patent Document 3), but as the refractive index in the bending direction is reduced, the pencil hardness when a hard coat is applied decreases, resulting in a problem of reduced surface protection function for displays. In addition, lowering the refractive index in one direction improves deformation when folded, but increases uniaxial orientation in the folding direction, resulting in problems such as cracks or breakage at the folded portion.

[0009] On the other hand, the hard coat film is also required to have visibility and design. Therefore, in order to suppress glare and iridescent color (interference pattern) caused by reflected light when viewed from any angle, it is common to provide an anti-reflection layer with a multi-layer structure in which a high refractive index layer and a low refractive index layer are alternately laminated on the upper layer of the hard coat layer. However, in recent years, three-wavelength fluorescent lamps have become mainstream in order to reproduce daylight color, making interference patterns caused by reflected light more visible. Furthermore, there is an increasing demand for cost reduction by simplifying the anti-reflection layer. Therefore, there is a demand for a hard coat film alone without adding an anti-reflection layer that suppresses interference patterns as much as possible.

[0010] As described above, a method of providing one or two optical adjustment layers with adjusted refractive index on a polyester film has been proposed as a method of suppressing interference patterns, but the durability of polyester films against repeated folding must be considered. For example, an optical adjustment layer containing excessive metal fine particles generates interference patterns due to microcracks originating from the fine particles, so a fully satisfactory one has not been obtained. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2010-228391 A [Patent Document 2] JP 2016-155124 A [Patent Document 3] International Publication No. 2018 / 150940 Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention seeks to solve the problems associated with conventional display components as described above, and to provide a foldable display that is easy to mass-produce and has no risk of distortion of the image displayed at the folded portion after repeated folding, and a mobile terminal device equipped with such a foldable display. The present invention seeks to provide a hard coat film for a foldable display that does not cause fold marks or cracks in the folded portion and can effectively suppress iridescent colors (interference patterns) affected by fine cracks in an easy-adhesive resin layer, etc. [Means for solving the problem]

[0013] That is, the present invention comprises the following: 1. A hard coat film for folding displays, comprising an easy-adhesion resin layer and a hard coat layer, in that order, on at least one surface of a polyester film having a thickness of 10 to 80 μm, the easy-adhesion resin layer being formed by curing a composition containing at least one compound selected from titanium compounds and zirconium compounds, and a polyester resin, and the polyester film having the easy-adhesion resin layer and prior to lamination of the hard coat layer satisfies the following conditions (1) to (4): (1) The refractive index in the bending direction is 1.590 to 1.620 (2) The refractive index in the direction of the fold is 1.670 to 1.700 (3) Refractive index in the thickness direction is 1.520 or less (4) Density is 1.380 g / cm 3 End (Here, the bending direction refers to the direction perpendicular to the fold when folding the polyester film.) 2. The hard coat film for folding displays described in 1 above, wherein the refractive index of the easy-adhesion resin layer is lower than the refractive index in the bending direction of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer, and the refractive index in the direction of the fold, and is higher than the refractive index of the hard coat layer. 3. The polyester film for a folding display according to the above 1 or 2, wherein the refractive index of the easy-adhesion resin layer satisfies the following conditions (5) and (6): (5) The refractive index of the easy-adhesion resin layer is lower than the refractive index of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer in the bending direction, and the difference in the refractive index is greater than 0 and less than or equal to 0.07. (6) The refractive index of the easy-adhesion resin layer is lower than the refractive index of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer in the direction of the folded portion, and the difference in the refractive index is 0.080 or more and 0.150 or less. 4. The polyester film for a folding display according to any one of claims 1 to 3, wherein the polyester resin contained in the easy-adhesion resin layer is a polyester resin containing a naphthalene dicarboxylic acid component as at least a part of the dicarboxylic acid component among the dicarboxylic acid component and diol component constituting the polyester resin. 5. A hard coat film for a folding display according to any one of claims 1 to 4 above, wherein the polyester film having the easy-adhesion resin layer and before laminating a hard coat layer has a total light transmittance of 85% or more, a haze of 3% or less, and a maximum heat shrinkage of 6% or less. 6. The hard coat film for a folding display according to any one of the above items 1 to 5, wherein the hard coat layer has a thickness of 1 to 50 μm. 7. A foldable display in which the hard coat film for a foldable display according to 6 above is arranged as a surface protective film so that the hard coat layer is positioned on the surface, and a single continuous hard coat film is arranged through the folding portion of the foldable display. 8. A mobile terminal device having the foldable display described in claim 7. Effect of the Invention

[0014] A folding display using the hard coat film for folding displays of the present invention maintains mass productivity, and the hard coat film does not crack at the folding portion and does not deform after repeated folding. Furthermore, cracks at the folding portion, lifting at the interface between the hard coat and the easy-adhesion resin layer, lifting at the interface between the easy-adhesion resin layer and the polyester film, and iridescent colors (interference patterns) caused by fine cracks can be effectively suppressed, and image distortion does not occur at the folding portion of the display. A mobile terminal device equipped with a folding display using such a hard coat film provides beautiful images, is highly functional, and has excellent convenience such as portability. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a schematic diagram showing the bending radius when the foldable display of the present invention is folded. [Diagram 2] FIG. 2 is a schematic diagram showing the bending direction of a polyester film constituting the hard coat film for a foldable display in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] (display) The display in the present invention generally refers to a display device, and the types of displays include LCD, organic EL display, inorganic EL display, LED, FED, etc., but LCD, organic EL, and inorganic EL having a bendable structure are preferred. In particular, organic EL and inorganic EL, which can reduce the layer structure, are more preferred, and organic EL, which has a wide color gamut, is even more preferred.

[0017] (Foldable display) A folding display is a single continuous display that can be folded in half or the like when carried. By folding, the size can be halved, improving portability. The bending radius of a folding display is preferably 5 mm or less, and more preferably 3 mm or less. If the bending radius is 5 mm or less, it can be made thin when folded. It can be said that the smaller the bending radius, the better, but the smaller the bending radius, the more likely it is to leave creases. The bending radius is preferably 0.1 mm or more, but may be 0.5 mm or more, or may be 1 mm or more. Even if the bending radius is 1 mm, it is possible to achieve a practically sufficient thinness when carried. The bending radius when folded is measured at the location of the symbol 11 in the schematic diagram of FIG. 1, and means the radius of the inside of the folded part when folded. The surface protective film described later may be located on the outside or inside of the folded folding display. Furthermore, the foldable display may be folded in three or four, or may be a rollable type, all of which are considered to fall within the scope of the foldable display of the present invention.

[0018] The hard coat film for folding displays of the present invention may be used in any part as long as it is a component of a folding display. Below, a typical configuration of a folding display and the part where the hard coat film of the present invention can be used will be described using an organic EL display as an example. Hereinafter, the hard coat film for folding displays of the present invention may be simply referred to as the hard coat film of the present invention.

[0019] (Foldable OLED display) The essential component of a folding organic EL display is an organic EL module, and further includes a circular polarizing plate, a touch panel module, a front protective film, a back protective film, and the like, as required. (Organic LED module) The general structure of an organic EL module is composed of an electrode / electron transport layer / light-emitting layer / hole transport layer / transparent electrode.

[0020] (Touch panel module) It is preferable that the mobile terminal device has a touch panel. When an organic EL display is used, it is preferable that a touch panel module is disposed on the top of the organic EL display or between the organic EL module and the circular polarizing plate. The touch panel module has a transparent substrate such as a film and a transparent electrode disposed thereon. The hard coat film of the present invention can be used as this transparent substrate. When used as a transparent substrate for a touch panel, it is preferable to provide a refractive index adjustment layer.

[0021] (Circular polarizing plate) The circular polarizing plate suppresses deterioration of image quality due to reflection of external light by members inside the display. The circular polarizing plate has a linear polarizing plate and a retardation plate. The linear polarizing plate has a protective film on at least the viewing side surface of the polarizer. The polarizer may also have a protective film on the surface opposite to the viewing side, or the retardation plate may be directly laminated on the polarizer. The retardation plate is a resin film having a retardation such as polycarbonate or cyclic olefin, or a resin film provided with a retardation layer made of a liquid crystal compound. The hard coat film of the present invention can be used as a polarizer protective film. In these cases, when the base film of the hard coat film of the present invention is a polyester film, it is preferable that the slow axis direction of the polyester film is parallel or perpendicular to the absorption axis direction of the polarizer. Incidentally, a deviation of 10 degrees, preferably 5 degrees, from this parallel or perpendicular direction is permitted.

[0022] (Surface protection film) When an impact is applied to a display from above, the circuits of an organic EL module or a touch panel module may be broken, so a surface protective film is often provided. The hard coat film of the present invention is used as this surface protective film. Surface protective films include those called cover windows that are incorporated into the outermost surface of a display, and those called afters that can be attached, peeled off, and replaced by the user himself, but the hard coat film of the present invention is used in either case. The hard coat layer is provided on the surface of a folding display with the hard coat layer on the viewing side. The hard coat layer may be provided on both sides.

[0023] (Back protection film) It is also preferable that a protective film is provided on the back side of the display, and the hard coat film of the present invention can be used as the protective film on the back side.

[0024] The hard coat film of the present invention may be any other than those described above, so long as it is used in a portion of a folding display that is to be folded. Among these, the hard coat film of the present invention is preferably used as a cover window surface protection film, an after-surface protection film, a base film of a touch panel module, or a back surface protection film, and more preferably used as a cover window surface protection film or an after-surface protection film.

[0025] In addition, the hard coat film of the present invention does not necessarily have to be used for all of the above applications of the folding display. In the folding display, a hard coat film based on a polyester film, a polyimide film, a polyamide film, a polyamideimide film, a polycarbonate film, an acrylic film, a triacetyl cellulose film, a cycloolefin polymer film, a polyphenylene sulfide film, a polymethylpentene film, etc. can be used appropriately according to suitability.

[0026] When the substrate film constituting the hard coat film of the present invention is a polyester film, it may be a single-layer film made of one or more types of polyester resin, or when two or more types of polyester are used, it may be a multilayer structure film or a super multilayer laminate film with a repeating structure.

[0027] Examples of polyester resins used in the polyester film, which is the base film of the hard coat film, include polyester films made of polyethylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, or copolymers mainly composed of the constituent components of these resins. Among these, stretched polyethylene terephthalate films are particularly preferred in terms of mechanical properties, heat resistance, transparency, cost, etc.

[0028] When a polyester copolymer is used for the polyester film, which is the base film of the hard coat film, examples of the dicarboxylic acid component of the polyester include aliphatic dicarboxylic acids such as adipic acid and sebacic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid; and polyfunctional carboxylic acids such as trimellitic acid and pyromellitic acid. Examples of the glycol component include fatty acid glycols such as ethylene glycol, diethylene glycol, 1,4-butanediol, propylene glycol, and neopentyl glycol; aromatic glycols such as p-xylene glycol; alicyclic glycols such as 1,4-cyclohexanedimethanol; and polyethylene glycols having an average molecular weight of 150 to 20,000. The mass ratio of the copolymerization components of the preferred copolymer is less than 20% by mass. When it is less than 20% by mass, it is preferable because the film strength, transparency, and heat resistance are maintained.

[0029] In addition, in the production of the polyester film, which is the base film of the hard coat film, the intrinsic viscosity of at least one type of resin pellet is preferably in the range of 0.50 to 1.0 dl / g. When the intrinsic viscosity is 0.50 dl / g or more, the impact resistance of the obtained film is improved, and disconnection of the internal circuit of the display due to external impact is less likely to occur, which is preferable. On the other hand, when the intrinsic viscosity is 1.00 dl / g or less, the filtration pressure of the molten fluid does not increase too much, which makes it easier to operate the film production stably, which is preferable.

[0030] The thickness of the polyester film, which is the base film of the hard coat film, is preferably 10 to 80 μm, and more preferably 25 to 75 μm. A thickness of 10 μm or more improves the pencil hardness and impact resistance, while a thickness of 80 μm or less is advantageous for weight reduction and is excellent in flexibility, processability, handleability, etc.

[0031] The surface of the hard coat film of the present invention may be smooth or uneven, but since it is used for display surface covering, the deterioration of optical properties due to unevenness is not preferable. The haze in the state before laminating the easy-adhesion resin layer on the polyester film and laminating the hard coat layer is preferably 3% or less, more preferably 2% or less, and most preferably 1% or less. If the haze is 3% or less, the visibility of the image can be improved. The lower limit of the haze is better, but from the viewpoint of stable production, it is preferably 0.1% or more, and may be 0.3% or more.

[0032] As described above, in order to reduce haze, it is preferable that the unevenness of the film surface is not too large. However, in order to provide a certain degree of slipperiness from the viewpoint of ease of handling, unevenness can be formed by blending particles into the base polyester film or by coating the base polyester film with a coating layer containing particles as an easy-adhesion resin layer during the film formation process.

[0033] The method of blending particles into the base polyester film can be a known method. For example, it can be added at any stage of polyester production, but preferably it can be added as a slurry dispersed in ethylene glycol or the like at the stage of esterification, or after the completion of transesterification reaction and before the start of polycondensation reaction, and polycondensation reaction can be carried out. It can also be carried out by a method of blending a slurry of particles dispersed in ethylene glycol or water with polyester raw material using a vented kneading extruder, or a method of blending dried particles with polyester raw material using a kneading extruder.

[0034] Among them, a method is preferred in which aggregated inorganic particles are homogeneously dispersed in a monomer liquid that will become a part of the polyester raw material, and then the filtered product is added to the remainder of the polyester raw material before, during, or after the esterification reaction. According to this method, since the monomer liquid has a low viscosity, homogeneous dispersion of the particles and highly accurate filtration of the slurry can be easily performed, and when added to the remainder of the raw material, the dispersibility of the particles is good and new aggregates are unlikely to be generated. From this viewpoint, it is particularly preferred to add to the remainder of the raw material in a low temperature state before the esterification reaction.

[0035] In addition, the number of protrusions on the film surface can be further reduced by a method in which, after obtaining a polyester containing particles in advance, the pellets are mixed and extruded with pellets not containing particles (master batch method).

[0036] The polyester film substrate may contain various additives, such as antistatic agents, UV absorbers, and stabilizers, within a range that maintains a preferred range of total light transmittance.

[0037] The total light transmittance of the polyester film having an easy-adhesion resin layer and no hard coat layer is preferably 85% or more, more preferably 87% or more. With a transmittance of 85% or more, visibility can be sufficiently ensured. The total light transmittance of the polyester film is preferably 85% or more in order to increase the total light transmittance of the hard coat film described below. The higher the total light transmittance of the polyester film, the better, but from the viewpoint of stable production, it is preferably 99% or less, and may be 97% or less.

[0038] The maximum heat shrinkage rate of the polyester film having an easy-adhesive resin layer and not having a hard coat layer after heat treatment at 150°C for 30 minutes is preferably 6% or less, more preferably 5% or less. If the heat shrinkage rate is 6% or less, flatness defects such as curling and undulation during HC processing can be suppressed. The lower the maximum heat shrinkage rate, the better, but it is preferably -1% or more, and more preferably 0% or more. Here, minus means that the film expanded after heating, and -1% or more is preferable because the flatness is good.

[0039] In order to provide the hard coat film for folding displays of the present invention with sufficient pencil hardness, it is preferable that the polyester film has an easy-adhesion resin layer and has the following properties in a state in which it does not have a hard coat layer. It is considered that the pencil hardness of the conventional base polyester film is reduced due to deformation of the film in the thickness direction in the pencil hardness evaluation of the hard coat film after laminating a hard coat layer. In the present invention, it is preferable to set the indentation depth after unloading the test force in the thickness direction of the base polyester film in the above state by the dynamic ultra-microhardness meter described later to a specific range. In the pencil hardness evaluation of the hard coat film using the base polyester film, it is preferable that a high hardness can be achieved. The indentation depth in the thickness direction of the base polyester film in the above state after unloading the test force is preferably 1.5 μm or less, more preferably 1.4 μm or less, and even more preferably 1.3 μm or less. If the indentation depth after the test force is removed (final deformation amount under load) is 1.5 μm or less, the film is less likely to deform in the thickness direction in the pencil hardness evaluation of the hard coat film after laminating the hard coat layer, and the pencil hardness can be increased. If the pencil hardness of the hard coat film can be increased, scratches and dents are less likely to occur on the display surface, improving the visibility of the display. It can be said that the lower the indentation depth after the test force is removed, the better, but from the viewpoints of stable production and saturation of the effect, 0.3 μm or more is preferable, and more preferably 0.5 μm or more is more preferable.

[0040] In order to reduce the indentation depth after the test force is removed, it is effective to adjust the refractive index in the thickness direction of a polyester film having an easy-adhesion resin layer and no hard coat layer to 1.520 or less. As a means for adjusting the refractive index to 1.520 or less, as described later, examples of conditions include adjusting the stretch ratio in the bending direction or folding direction to a high value, setting the stretching temperature in the bending direction or folding direction to a low value, and setting the heat setting temperature to a high value, within a range in which other physical properties and the refractive index in the bending direction or folding direction can be controlled to a preferred range.

[0041] The non-hard-coated surface of the hard-coated film of the present invention may be coated with an adhesive or subjected to a treatment for improving adhesion to the hard-coat layer.

[0042] Examples of the surface treatment method include roughening treatment using sandblasting or solvent treatment, and oxidation treatment such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone or ultraviolet irradiation treatment, flame treatment, chromic acid treatment, or hot air treatment, and any of these methods can be used without any particular limitation.

[0043] It is also preferable to improve the adhesion by using an adhesion improving layer such as an easy-adhesion resin layer. The easy-adhesion resin layer can be made of any resin such as an acrylic resin, a polyester resin, a polyurethane resin, or a polyether resin, without any particular limitation, and can be formed by a general coating method, preferably a so-called in-line coating method.

[0044] The polyester film described above can be produced, for example, through a polymerization step in which inorganic particles are homogeneously dispersed in a monomer liquid that becomes a part of the polyester raw material, the dispersion is filtered, and then the dispersion is added to the remainder of the polyester raw material to polymerize the polyester, and a film formation step in which the polyester is melt-extruded through a filter into a sheet, which is cooled and stretched to form a base film.

[0045] Next, a method for producing a polyester film as a substrate will be described in detail using an example in which polyethylene terephthalate (hereinafter, sometimes referred to as PET) pellets are used as the raw material for the substrate film, but the present invention is not limited to this. In addition, the number of layers, such as a single layer structure or a multilayer structure, is not limited.

[0046] After mixing and drying PET pellets in a predetermined ratio, the mixture is fed to a known melt lamination extruder, extruded from a slit die into a sheet, and cooled and solidified on a casting roll to form an unstretched film. In the case of a single layer, one extruder is sufficient, but in the case of producing a film with a multilayer structure, two or more extruders, two or more manifolds or merging blocks (e.g., merging blocks having a rectangular merging portion) are used to laminate multiple film layers constituting each outermost layer, and a sheet of two or more layers is extruded from a die and cooled on a casting roll to form an unstretched film.

[0047] In this case, it is preferable to perform high-precision filtration to remove foreign matter contained in the resin at any location where the molten resin is kept at about 280° C. during melt extrusion. The filter material used for high-precision filtration of the molten resin is not particularly limited, but a filter material made of sintered stainless steel is preferable because it has excellent performance in removing aggregates and high-melting organic matter mainly composed of Si, Ti, Sb, Ge, and Cu.

[0048] Furthermore, the filtration particle size (initial filtration efficiency 95%) of the filter medium is preferably 20 μm or less, particularly preferably 15 μm or less. If the filtration particle size (initial filtration efficiency 95%) of the filter medium exceeds 20 μm, foreign matter with a size of 20 μm or more cannot be sufficiently removed. By using a filter medium with a filtration particle size (initial filtration efficiency 95%) of 20 μm or less to perform high-precision filtration of molten resin, productivity may decrease, but it is preferable to obtain a film with few protrusions due to coarse particles.

[0049] (Refractive index in bending direction) In the present invention, the refractive index in at least one of the longitudinal direction (machine flow direction) and the width direction of the polyester film having an easy-adhesion resin layer and before laminating the hard coat layer is preferably 1.590 to 1.620, more preferably 1.591 to 1.600. The refractive index in the bending direction of the polyester film having an easy-adhesion resin layer and before laminating the hard coat layer is preferably 1.590 to 1.620, more preferably 1.591 to 1.600. Here, the bending direction refers to the direction perpendicular to the folding part (reference number 21) assumed in the use of a folding display, as shown by reference number 22 on the polyester film (reference number 2) in FIG. 2. When the refractive index in at least one of the longitudinal direction and the width direction is 1.590 to 1.620, there is little deformation when repeatedly folded, and there is no risk of deteriorating the image quality of the folding display, which is preferable. The refractive index is more preferably 1.591 to 1.600. Of course, the direction is preferably the bending direction. If the refractive index is 1.590 or more, there is no risk of cracks occurring in the direction of the folded portion after the bending test described below, and of course no breakage occurs, so that the visibility of the display can be maintained good. The refractive index of the polyester film can be effectively adjusted by adjusting the stretching ratio and stretching temperature. In addition, a relaxation process in the stretching direction and multi-stage stretching may be used to adjust the refractive index. When multi-stage stretching is performed, it is preferable to make the stretching ratio in the second stage and thereafter higher than the stretching ratio in the first stage. The difference in refractive index between the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer and the polyester film alone not having the easy-adhesion resin layer is negligibly small.

[0050] By controlling the refractive index in at least one of the longitudinal direction (machine flow direction) and the width direction of the polyester film having an easy-adhesion resin layer and before laminating the hard coat layer within the above range, and more preferably by controlling the refractive index in the bending direction within the above range, fatigue due to the compressive stress applied to the inside of the fold when folded can be reduced. It is believed that fatigue due to compressive stress occurs mainly in the crystalline portion, and fatigue is less likely to occur when there are fewer crystals in the bending direction. Therefore, it is believed that the amount of oriented crystals in the bending direction is reduced by lowering the refractive index, and compression fatigue is suppressed.

[0051] Furthermore, the creep phenomenon caused by tensile stress applied to the outside of the fold when the material is folded can be suppressed by reducing the refractive index. Fatigue caused by tensile stress is thought to occur mainly in the amorphous portion, and the repeated application of stress causes molecular chains to align, resulting in deformation. It can be assumed that the fewer molecular chains aligned in the bending direction, the less deformation caused by alignment. Furthermore, since fatigue caused by tension can be suppressed with fewer amorphous portions, a higher degree of crystallinity, i.e., a higher density, is preferable.

[0052] In the present invention, the stretching ratio of the unstretched polyester sheet in at least one of the longitudinal direction (machine flow direction) and the width direction is preferably 1.2 to 2.0 times, more preferably 1.7 to 2.0 times. The stretching direction is preferably the bending direction. A stretching ratio of 1.2 times or more is preferable because there is no deformation during post-processing such as hard coat coating, and a stretching ratio of 2.0 times or less is preferable because thickness unevenness of the film does not occur. The stretching temperature is preferably 75 to 120°C, more preferably 75 to 105°C. The heating method during stretching can be a conventionally known method such as hot air heating method, roll heating method, and infrared heating method. By setting the stretching temperature to 75 to 120°C, it is possible to prevent large thickness unevenness due to stretching at the above stretching ratio. In addition, by stretching at a temperature as low as possible within a range in which large thickness unevenness does not occur as described above, the refractive index in the thickness direction can be reduced.

[0053] (Refractive index in the direction of the fold) The refractive index in the direction perpendicular to the direction in which the refractive index of the polyester film having the above-mentioned easy-adhesion resin layer and before laminating the hard coat layer is 1.590 to 1.620 is preferably 1.670 to 1.700. That is, the refractive index in the direction perpendicular to the bending direction (direction of the folded part) is preferably 1.670 to 1.700. By making it 1.670 to 1.700, it is possible to reduce deformation when folded in the bending direction. By making it 1.700 or less, it is possible to suppress cracks and breakage in the direction of the folded part. By making it 1.670 or more, it is possible to improve the flexibility in the bending direction and improve the surface hardness. It is more preferable that it is 1.680 to 1.695. Methods for adjusting the refractive index in the direction perpendicular to the bending direction include the stretching ratio, stretching preheating temperature, stretching temperature, multi-stage stretching, and film relaxation. The stretching ratio is preferably 4.0 to 6.0 times, more preferably 4.4 to 6.0 times. The preheating temperature for stretching in the direction perpendicular to the bending direction is preferably 70 to 110° C. When multi-stage stretching is performed in the direction perpendicular to the bending direction, it is preferable to set the stretch ratio higher in the second and subsequent stages than in the first stage. The film may be relaxed by 1 to 10% in either the machine flow direction (longitudinal direction) or the perpendicular direction (width direction).

[0054] (Refractive index in the thickness direction) The refractive index in the thickness direction of the polyester film having an easy-adhesion resin layer and before laminating the hard coat layer is preferably 1.520 or less. By making it 1.520 or less, even if the refractive index in the bending direction is designed to be low, the decrease in hardness of the film surface can be suppressed, and both flexibility and surface hardness can be achieved. By making it 1.520 or less, the indentation depth after unloading the test force in the thickness direction is reduced, and the hardness of the film surface, particularly the pencil hardness of the hard coat film after lamination of the hard coat layer, can be improved. More preferably, it is 1.515 or less, even more preferably 1.510 or less, particularly preferably 1.505 or less, and most preferably 1.500 or less. The refractive index in the thickness direction is preferably low, but is preferably 1.3 or more in terms of stable production, and may even be 1.4 or more. Particularly preferably, it is 1.410 or more. It can be said that the above range can be achieved by increasing the stretch ratio in both the bending direction and the folding direction. However, in order to control the refractive index in the thickness direction after controlling the refractive index in the bending direction and width direction within preferred ranges, it is preferable to set the conditions while checking the balance of the conditions for each process in the film formation process.

[0055] The method of controlling the refractive index in the thickness direction to the above range includes the preheating temperature, stretching temperature, and stretching ratio in the bending direction, the preheating temperature, stretching temperature, multi-stage stretching, high-ratio stretching, or heat fixing temperature setting in the folding direction. The preheating temperature in the bending direction is preferably 70°C to 110°C. The stretching temperature in the bending direction is preferably 75°C to 120°C. The stretching ratio in the bending direction is preferably 1.2 to 2.0 times, more preferably 1.7 to 2.0 times. By lowering the stretching temperature and stretching at a low stretching ratio, the refractive index in the thickness direction can be effectively reduced while maintaining the flexibility in the bending direction. The preheating temperature in the folding direction is also preferably 75°C to 110°C. The stretching temperature is preferably 75°C to 120°C. The stretching ratio in the folding direction is preferably 4.0 to 6.0 times, more preferably 4.4 to 6.0 times. The refractive index in the thickness direction can be effectively reduced while maintaining or reducing the refractive index in the bending direction. Multi-stage stretching may be used as a method of high-ratio stretching. In this case, it is preferable to set the stretching ratio in the second stage higher than that in the first stage, since this allows for effective control of the refractive index. A method of stretching again after the crystallization step may also be used. Accelerated stretching, in which the stretching speed is increased from the initial stage to the latter stage of stretching, may also be used. The heat setting temperature is preferably 180 to 240° C. By carrying out heat setting, oriented crystallization in the stretching direction advances, and the refractive index in the thickness direction can be reduced. The reason why lowering the refractive index in the thickness direction improves the hardness of the film surface is not entirely clear, but it is thought that aromatic groups such as benzene rings in the molecular chain are oriented in the plane direction, which has the effect of suppressing deformation due to stress applied in the thickness direction.

[0056] (Regarding density of polyester film) The density of the polyester film having an easy-adhesion resin layer and before laminating the hard coat layer is 1.380 g / cm 3 It is preferable that the density is 1.383 g / cm or more. 3 More preferably, it is 1.380 g / cm or more. 3By setting the density to 1.40 g / cm or more, it is possible to improve the flexibility and the film surface hardness, particularly the pencil hardness of the hard coat film after laminating the hard coat layer. The higher the density, the better. Although it depends somewhat on the presence or absence of particles in the film, it is preferable to set the density to 1.40 g / cm or more. 3 It is preferable that the temperature is 180 to 240° C. or less. By setting the heat setting temperature during film formation to 180 to 240° C., crystallization can be promoted and the density can be effectively increased. The density of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer is negligibly small compared to the density of the polyester film alone not having the easy-adhesion resin layer.

[0057] The bending direction of the polyester film is preferably set to correspond to the longitudinal direction (machine flow direction). This makes it easier to reduce the refractive index in the bending direction by biaxial stretching and improve the flexibility. That is, a polyester film is preferably obtained by stretching an unstretched polyester sheet in the longitudinal direction at a stretching ratio of 1.2 to 2.0 times, more preferably 1.7 to 2.0 times. In addition, it can be said that a preferred embodiment is to stretch the polyester sheet in the transverse direction at a stretching ratio of 4.0 to 6.0 times, more preferably 4.4 to 6.0 times.

[0058] In the present invention, the polyester film has an easily adhesive resin layer and is not laminated with the hard coat layer. (1) The refractive index in the bending direction is 1.590 to 1.620 (2) The refractive index in the direction of the fold is 1.670 to 1.700 (3) Refractive index in the thickness direction is 1.520 or less (4) Density is 1.380 g / cm 3 End It is particularly preferable to have the above four characteristics simultaneously, but even if the combination is within the above-mentioned preferred manufacturing conditions, it may not necessarily be possible to obtain a film that satisfies all four characteristics simultaneously if the combination is not the best within each preferred manufacturing condition range, for example, a combination of a stretch ratio in the bending direction of 1.4 times or less, a stretch ratio in the folding direction of less than 4.4 times, and a heat setting temperature of 220° C. or less. In this case, the above four characteristics can be simultaneously satisfied by fine-tuning any of the conditions or a combination of them, such as increasing the stretch ratio in the bending direction to 1.7 times or more, increasing the stretch ratio in the folding direction to 4.4 times or more, increasing the heat setting temperature to about 230° C., or lowering the stretching temperature in the bending direction and / or the folding direction.

[0059] In order to adjust the film formability, film strength, thermal dimensional stability, and appearance defects, any film forming method such as stretching, relaxation, heat setting, and surface treatment may be used, but it can be said that a particularly preferred embodiment of the present invention is to control the refractive index and density of the film within the above-mentioned preferred ranges. By controlling the refractive index and density within the preferred ranges, it is possible to provide a polyester film suitable for a folding display, which has superior flex resistance and surface hardness compared to conventional films, particularly high pencil hardness of the hard coat film after laminating a hard coat layer.

[0060] Specifically, for example, PET pellets are thoroughly vacuum-dried, then fed to an extruder, melt-extruded into a sheet at about 280°C, and cooled and solidified to form an unstretched PET sheet. The unstretched sheet obtained is stretched 1.2 to 2.0 times, more preferably 1.7 to 2.0 times, in the longitudinal direction with a roll heated to 75 to 120°C to obtain a uniaxially oriented PET film. Furthermore, the end of the film is held by a clip and introduced into a hot air zone heated to 75 to 120°C, and after drying, is stretched 4.0 to 6.0 times, more preferably 4.4 to 6.0 times, in the transverse direction. Subsequently, the film can be introduced into a heat treatment zone at 180 to 240°C and heat-treated for 1 to 60 seconds. During this heat treatment process, a relaxation treatment of 0 to 10% may be performed in the transverse or longitudinal direction as necessary.

[0061] The intrinsic viscosity of the polyester film is preferably in the range of 0.50 to 1.0 dl / g. When the intrinsic viscosity is 0.50 dl / g or more, the impact resistance is improved and disconnection of the internal circuit of the display due to external impact is less likely to occur, which is preferable. On the other hand, when the intrinsic viscosity is 1.00 dl / g or less, the increase in the filtration pressure of the molten fluid is not too large, which is preferable because film production is stable.

[0062] (Easy adhesive resin layer) In the present invention, in order to improve the adhesion between the polyester film and the hard coat layer, etc., it is preferable to laminate an easy-adhesion resin layer on the polyester film. The easy-adhesion resin layer can be obtained by so-called in-line coating, in which a coating liquid for forming the easy-adhesion resin layer is applied to one or both sides of an unstretched or uniaxially stretched film in the longitudinal direction, and then heat-treated and dried as necessary, and further stretched in at least one direction that is not stretched. Heat treatment can also be performed after biaxial stretching. The final coating amount of the easy-adhesion layer is 0.005 to 0.20 g / m 2 It is preferable to control the coating amount to 0.005 g / m 2 On the other hand, if the coating amount is 0.20 g / m or more, adhesiveness is obtained, which is preferable. 2 If it is not more than this, blocking resistance can be obtained, which is preferable.

[0063] Resins contained in the coating liquid used for laminating the easy-adhesion layer include, for example, polyester resins, polyether polyurethane resins, polyester polyurethane resins, polycarbonate polyurethane resins, acrylic resins, etc., and can be used without any particular limitation. However, in terms of high adhesion to polyester films and refractive index, it is preferable to contain a polyester resin. Furthermore, among the dicarboxylic acid components and diol components constituting the polyester resin, a polyester resin composed of a naphthalene dicarboxylic acid component that can increase the refractive index of the easy-adhesion resin layer is preferably used as at least a part of the dicarboxylic acid component. In addition, in order to improve the adhesion durability of these easy-adhesion resin layers, a crosslinked structure may be formed in the binder resin contained in the easy-adhesion resin layer. Examples of crosslinking agents contained in the coating liquid for forming the easy-adhesion layer include melamine compounds, isocyanate compounds, oxazoline compounds, epoxy compounds, carbodiimide compounds, etc., and self-crosslinking polyurethane resins and the like can also be blended. The crosslinking agents can be used in a mixture of two or more types. Due to the nature of the in-line coating, these are preferably coated with a water-based coating liquid, and the resins and crosslinking agents are preferably water-soluble or water-dispersible resins or compounds.

[0064] The polyester resin contained in the easy-adhesion resin layer is preferably a linear polyester having a dicarboxylic acid component and a diol component (glycol component) as constituent components.

[0065] Examples of the dicarboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4-diphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, adipic acid, sebacic acid, phenylindanedicarboxylic acid, and dimer acid. Two or more of these components can be used. Furthermore, together with these components, small proportions of unsaturated polybasic acids such as maleic acid, fumaric acid, and itaconic acid, and hydroxycarboxylic acids such as p-hydroxybenzoic acid and p-(β-hydroxyethoxy)benzoic acid can be used. The proportion of the unsaturated polybasic acid component and the hydroxycarboxylic acid component is 10 mol % or less, preferably 5 mol % or less.

[0066] By including a component derived from naphthalenedicarboxylic acid as the dicarboxylic acid component of the polyester resin, the refractive index increases, and it becomes easier to control the iridescent color under fluorescent light. It is also possible to improve the wet heat resistance. Of course, the polymerization process and copolymerization process for including a naphthalenedicarboxylic acid component in a polyester may be a so-called direct polymerization method or an ester exchange method, and the dicarboxylic acid component such as a naphthalenedicarboxylic acid component may be introduced in the form of its ester derivative.

[0067] As the above-mentioned naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid is preferred. The ratio of the above-mentioned naphthalenedicarboxylic acid component to the total dicarboxylic acid components constituting the polyester resin is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 50 mol% or more, and even more preferably 60 mol% or more. If it is 20 mol% or more, the effect of increasing the refractive index of the easy-adhesion resin layer is remarkable, which is preferable. The ratio of the above-mentioned naphthalenedicarboxylic acid component to the total dicarboxylic acid components constituting the polyester resin may be 100 mol%, but it is more preferable that it is 95 mol% or less in view of the flexibility of the easy-adhesion resin layer.

[0068] As long as the effects of the present invention are achieved, the glycol component in the polyester resin may further include ethylene glycol, 1,3-propane glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, 1,4-cyclohexanedimethanol, xylene glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, poly(ethyleneoxy)glycol, poly(tetramethyleneoxy)glycol, and alkylene oxide adducts of bisphenol A, and two or more of these may be used.

[0069] In addition, when the weight of the crosslinking agent in the easy-adhesion resin layer is taken into consideration, flexibility is likely to be lost, and there is a possibility that cracks may occur in the easy-adhesion resin layer after a bending test. In such a case, it is preferable that the polyester resin contains a dicarboxylic acid component represented by the following formula (1) and / or a diol component represented by the following formula (2). (1) HOOC-(CH)-COOH (wherein n is an integer of 4≦n≦10) (2) HO-(CH2)n-OH (wherein n is an integer of 4≦n≦10)

[0070] In this way, by containing a dicarboxylic acid component and / or a diol component having a carbon component of a specific length, flexibility is imparted to the polyester resin, making it easier to maintain a coating film even after a bending test, and cracks originating from particle aggregates can be suppressed. Examples of the dicarboxylic acid component of formula (1) include adipic acid, sebacic acid, azelaic acid, etc. Examples of the diol component of formula (2) include 1,4-butanediol, 1,6-hexanediol, etc.

[0071] The polyester resin can be used in the form of a solution or dispersion in water, a water-soluble organic solvent (e.g., an aqueous solution containing less than 50% by mass of alcohol, alkyl cellosolve, ketone, or ether), or an organic solvent (e.g., toluene, ethyl acetate, etc.).

[0072] When a polyester resin is used as a water-based coating liquid, a water-soluble or water-dispersible polyester resin is used. In order to make the polyester resin water-soluble or water-dispersible, it is preferable to copolymerize a compound containing a sulfonate group or a compound containing a carboxylate group.

[0073] The number average molecular weight of the polyester resin is preferably 5,000 to 40,000 from the standpoint of coating film strength, ease of water dispersion, etc., more preferably 10,000 to 30,000, and particularly preferably 12,000 to 25,000.

[0074] The solid content of the polyester resin in the solid content of the easy-adhesion resin layer is preferably 20% by mass or more and 90% by mass or less in terms of adhesion and refractive index adjustment. More preferably, it is 30% by mass or more and 80% by mass or less. The polyester resin may be a single one or a blend of two or more kinds. In the case of a blend of two or more kinds, the total of the polyester resin components is preferably the above composition.

[0075] (urethane resin) The urethane resin that can be used for the easy-adhesion resin layer contains at least a polyol component and a polyisocyanate component as constituents, and further contains a chain extender as necessary. The above-mentioned urethane resin is a polymer compound in which these constituents are copolymerized mainly by urethane bonds. Inclusion of polycarbonate polyol as a constituent of the urethane resin is one of the preferred forms because it can provide flexibility to the coating film. The constituents of these urethane resins can be identified by nuclear magnetic resonance analysis or the like.

[0076] (Polyurethane resin with polycarbonate skeleton) The diol component, which is a constituent of the polyurethane resin having a polycarbonate skeleton, preferably contains an aliphatic polycarbonate polyol having excellent heat resistance and hydrolysis resistance. In the optical applications of the present invention, it is preferable to use an aliphatic polycarbonate polyol from the viewpoint of preventing yellowing.

[0077] Examples of the aliphatic polycarbonate polyol include aliphatic polycarbonate diol and aliphatic polycarbonate triol, and preferably aliphatic polycarbonate diol can be used. Examples of the aliphatic polycarbonate diol that is a component of the urethane resin of the present invention include aliphatic polycarbonate diols obtained by reacting one or more diols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,8-nonanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol with carbonates such as dimethyl carbonate, diphenyl carbonate, ethylene carbonate, and phosgene.

[0078] Examples of polyisocyanates that are components of the urethane resin of the present invention include aromatic aliphatic diisocyanates such as xylylene diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanatomethyl)cyclohexane, aliphatic diisocyanates such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate, and polyisocyanates in which one or more of these compounds are added to trimethylolpropane or the like in advance. The above-mentioned polyisocyanates are preferable for optical applications that require no yellowing problem and high transparency. In addition, such polyisocyanates are preferable because the coating film does not become too hard, the stress caused by the shrinkage and swelling of photocurable resins and the like can be alleviated, and adhesion is maintained.

[0079] To impart water solubility to urethane resins, sulfonic acid (salt) groups or carboxylic acid (salt) groups can be introduced (copolymerized) into the urethane molecular structure. Sulfonic acid (salt) groups are strongly acidic, and their moisture absorption properties can make it difficult to maintain moisture resistance, so it is preferable to introduce weakly acidic carboxylic acid (salt) groups. Nonionic groups such as polyoxyalkylene groups can also be introduced.

[0080] In order to introduce a carboxylic acid (salt) group into a urethane resin, for example, a polyol compound having a carboxylic acid group, such as dimethylolpropionic acid or dimethylolbutanoic acid, is introduced as a copolymerization component as a polyol component, and neutralized with a salt-forming agent. Specific examples of salt-forming agents include ammonia, trialkylamines such as trimethylamine, triethylamine, triisopropylamine, tri-n-propylamine, and tri-n-butylamine, N-alkylmorpholines such as N-methylmorpholine and N-ethylmorpholine, and N-dialkylalkanolamines such as N-dimethylethanolamine and N-diethylethanolamine. These can be used alone or in combination of two or more kinds.

[0081] When a polyol compound having a carboxylic acid (salt) group is used as a copolymerization component to impart water solubility, the molar composition ratio of the polyol compound having a carboxylic acid (salt) group in the urethane resin is preferably 3 to 60 mol%, and more preferably 5 to 40 mol%, when the total polyol components of the urethane resin are taken as 100 mol%. When the molar composition ratio is 3 mol% or more, water dispersibility is good, which is preferable. Also, when the molar composition ratio is 60 mol% or less, water resistance and moist heat resistance are maintained, which is preferable.

[0082] The glass transition temperature of the urethane resin in the present invention is preferably less than 0° C., and more preferably less than −5° C. When the glass transition temperature is less than 0° C., it is preferred since suitable flexibility is easily achieved in terms of stress relaxation of the coating layer.

[0083] In order to form a crosslinked structure in the easy-adhesion resin layer, the easy-adhesion resin layer may be formed by including a crosslinking agent. By including a crosslinking agent, it is possible to further improve adhesion under high temperature and high humidity. Specific examples of crosslinking agents include urea-based, epoxy-based, melamine-based, isocyanate-based, oxazoline-based, and carbodiimide-based crosslinking agents. Among these, melamine-based, isocyanate-based, oxazoline-based, and carbodiimide-based crosslinking agents are preferred in terms of the stability over time of the coating liquid and the effect of improving adhesion under high temperature and high humidity treatment. In addition, a catalyst or the like can be appropriately used as necessary to promote the crosslinking reaction.

[0084] When the crosslinking agent is contained in the easy-adhesion resin layer, the content of the crosslinking agent is preferably 5% by mass or more and 50% by mass or less in the total solid components of the coating layer. More preferably, it is 10% by mass or more and 40% by mass or less. If it is 10% by mass or more, the strength of the resin of the easy-adhesion resin layer is maintained and the adhesion under high temperature and high humidity is good, and if it is 40% by mass or less, the flexibility of the resin of the coating layer is maintained and the adhesion after repeated folding tests at room temperature and under high temperature and high humidity is maintained, which is preferable.

[0085] The easy-adhesion resin layer in the present invention preferably contains at least one compound selected from titanium compounds and zirconium compounds. It is said that the iridescent color (interference pattern) of the hard coat film occurs due to a large difference between the refractive index (e.g., 1.62 to 1.65) of the polyester film substrate and the refractive index (e.g., 1.52) of the hard coat layer made of acrylic resin or the like. In order to prevent the occurrence of interference patterns by reducing the refractive index difference between the laminated layers, it is important to control the refractive index of the easy-adhesion resin layer so as to reduce the refractive index difference between the polyester film and the easy-adhesion resin layer, and the refractive index difference between the easy-adhesion resin layer and the hard coat layer. When controlling the refractive index of the easy-adhesion resin layer made of the binder resin or particles as the main component, the control becomes easier by including the above-mentioned compound having a high refractive index. Examples of titanium compounds include water-soluble titanium chelate compounds, water-soluble titanium acylate compounds, titanium oxide, titanium chloride, etc., and among them, titanium dioxide (titania) is preferably used. Examples of the zirconium compound include water-soluble zirconium chelate compounds, water-soluble zirconium acylate compounds, zirconium acetate, zirconium hydroxide, zirconium oxide, etc., and among these, zirconium dioxide (zirconia) is preferably used. It is also preferable that the compound with a high refractive index is in the form of particles.

[0086] The average particle size of the metal oxide particles such as zirconium dioxide is preferably 5 nm to 150 nm, more preferably 10 nm to 100 nm, and even more preferably 30 nm to 70 nm.

[0087] By designing the average particle size of the metal oxide particles to be within the above range, the film haze can be reduced. In addition, the particulate metal compound is desirably designed to have a particle size smaller than the film thickness of the easy-adhesion resin layer in order to obtain a cushioning effect when repeatedly folded, and the particle size is preferably such that particle aggregation is unlikely to occur. Suppressing particle aggregation is preferable because it does not become the starting point of cracks in the easy-adhesion resin layer when folded.

[0088] The amount of particulate metal compound added is preferably designed to be 0.1% by mass or more and less than 15% by mass with respect to the adhesion resin layer, so as to provide a cushioning effect when the adhesion resin layer is folded, and also to prevent the adhesion resin layer from becoming a starting point for cracks due to particle aggregation. More preferably, the amount is 0.5% by mass or more and 14% by mass or less, and more preferably, the amount is 1% by mass or more and 13% by mass or less. When particles are added within this range, aggregated particles are unlikely to occur in the adhesion resin layer, and the adhesion resin layer does not crack when repeatedly folded due to the aggregated particles, so that interference spots are unlikely to occur even after a folding test, which is preferable.

[0089] It is preferable that the particulate metal compound in the easy-adhesion resin layer is present in a smaller proportion in the direction of the folded parts than in the bending direction. Since fine cracks that occur during repeated folding are likely to occur in the direction of the folded parts where load is applied in the thickness direction, it is believed that the occurrence of cracks can be suppressed by reducing the particle frequency in the direction of the folded parts. It is believed that the particle aggregation rate and the frequency of crack propagation can be reduced by reducing the particle frequency. The particle presence rate in each direction can be confirmed by observing the cross section with a transmission electron microscope (TEM), etc.

[0090] As a method for changing the ratio of the particulate metal compound in each direction in the easy-adhesion resin layer, formation by an in-line coating method is preferable. In the in-line coating method, since there is a process of stretching a coating liquid containing an easy-adhesion resin material in at least one direction after coating, it is considered that the ratio of the particles in the easy-adhesion resin layer can be changed by adjusting the stretching ratio.

[0091] A dispersant may be used in combination with the particulate metal compound to prevent aggregation. The dispersant used in the present invention may be a polymer compound capable of maintaining the binder resin in the emulsion, dissolving or dispersing the crosslinking agent described below, and dispersing the metal oxide fine particles.

[0092] Specifically, known polymer dispersants such as polyvinyl, polyacrylic acid, polycarboxylic acid, polyurethane, etc. can be used. More specifically, as the polyvinyl polymer, polyvinyl alcohol, polyvinylpyrrolidone, polyvinyl acetate, polyvinyl ester, etc. and copolymers thereof can be used; as the polyacrylic acid polymer, polyacrylic acid, sodium polyacrylate, ammonium polyacrylate, etc. and copolymers thereof can be used; as the polycarboxylic acid polymer, polycarboxylic acid, sodium polycarboxylate, ammonium polycarboxylate, etc. and copolymers thereof can be used; as the polyurethane polymer, polyurethane, etc. and copolymers thereof can be used; and also, copolymers of these and copolymers with sulfonic acid polymers can be used. Among these, acrylic resins such as polyacrylic acid polymers are preferable as dispersants for metal fine particles.

[0093] It is more preferable that the metal oxide particles have a dispersant on a part or all of their surface. By containing a dispersant, the effect of suppressing the aggregation of metal oxide particles can be obtained. By containing such particles in the easy-adhesion resin layer, stress relaxation during repeated folding tests can be expected while maintaining the transparency of the coating film. By containing a dispersant, it is preferable that the aggregation of metal oxide particles is unlikely to occur in the easy-adhesion resin layer and cracks are unlikely to occur depending on the coating film formation process.

[0094] The method for surface treating the metal oxide particles with the acrylic resin is not particularly limited, but specific examples include a method in which a mixture of the metal oxide particles and the acrylic resin is added to a solvent and then dispersed, and a method in which the metal oxide particles and the acrylic resin are added in sequence to a solvent and then dispersed.

[0095] Apparatuses that can be used to carry out the dispersion include a dissolver, a high-speed mixer, a homomixer, a meader, a ball mill, a roll mill, a sand mill, a paint shaker, an SC mill, an annular mill, and a pin mill.

[0096] The amount of dispersant added to the metal oxide particles is preferably 5% by mass or more and less than 40% by mass based on the mass of the metal oxide particles. When the amount of dispersant added is 5% by mass or more, it is preferable because a good dispersion state of the metal oxide particles can be obtained in the easy-adhesion resin layer. When the amount of dispersant added is less than 40% by mass, it is preferable because it is easy to adjust the refractive index of the easy-adhesion resin layer by making use of the characteristics of the metal oxide particles. Furthermore, an amount of 10% by mass or more and less than 30% by mass is more preferable.

[0097] In the present invention, the refractive index of the easy-adhesive resin layer is designed to be within a certain range, and the thin film interference principle is satisfied, thereby reducing the iridescent color (interference pattern). Furthermore, by filling the easy-adhesive resin layer with a certain amount of the metal compound used for adjusting the refractive index, it is believed that the easy-adhesive resin layer has the effect of buffering damage to the easy-adhesive resin layer when repeatedly folded.

[0098] The thickness of the adhesive resin layer capable of suppressing iridescent colors (interference patterns) may be adjusted to satisfy the formula 2nd=λb / 4, where n is the refractive index of the adhesive resin layer, d is the thickness of the adhesive resin layer, and λb is the bottom wavelength of the reflection spectrum, which can be appropriately set within the range of 450 to 650 nm.

[0099] The polyester film having an easy-adhesion resin layer in the present invention is designed to have different refractive indices in the bending direction and in the direction of the folded portion, so it is preferable to control the refractive index of the easy-adhesion resin layer taking each direction into consideration.

[0100] It is desirable to control the refractive index of the easy-adhesion resin layer low with respect to the refractive index in the bending direction of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer. The range of the refractive index difference between the easy-adhesion resin layer and the bending direction is preferably greater than 0 and less than 0.070. More preferably, it is 0.005 or more and 0.065 or less. More preferably, it is 0.010 or more and 0.060 or less. If the refractive index of the easy-adhesion resin layer is lower than the bending direction of the polyester film, the refractive index difference with the laminated hard coat layer becomes small, and iridescent color (interference pattern) is effectively suppressed, which is preferable. In addition, if the refractive index difference is 0.070 or less, the refractive index difference with the polyester film does not become too large, and iridescent color (interference pattern) can be effectively suppressed, which is preferable. The bending direction is preferably designed with a resin component having more amorphous structure than a resin component having more crystalline structure, since compressive stress is applied when the easy-adhesion resin layer is bent inward, and tensile stress is applied when it is bent outward, and it is preferable to add an appropriate amount of a metal compound to compensate for the refractive index.

[0101] It is desirable to control the refractive index of the easy-adhesion resin layer low with respect to the refractive index in the direction of the folded part of the polyester film having the easy-adhesion resin layer before laminating the hard coat layer. The range of the difference in refractive index between the easy-adhesion resin layer and the folded part is preferably 0.080 or more and 0.150 or less. It is more preferably 0.085 or more and 0.14 or less. It is even more preferably 0.090 or more and 0.13 or less. If the refractive index is lower than the folded part direction of the polyester film, the refractive index difference with the laminated hard coat layer becomes small, and iridescent color (interference pattern) is effectively suppressed, which is preferable. In addition, if the refractive index difference is 0.150 or less, the refractive index difference with the polyester film does not become too large, and iridescent color (interference pattern) can be effectively suppressed, which is preferable.

[0102] It is preferable to add particles to the easy-adhesion layer to give it easy slipperiness. The average particle size of the fine particles is preferably 2 μm or less. If the average particle size of the particles exceeds 2 μm, the particles are likely to fall off from the easy-adhesion layer. Examples of particles to be contained in the easy-adhesion layer include inorganic particles such as titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, and calcium fluoride, and organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles. These may be added to the easy-adhesion layer alone, or two or more types may be added in combination. In order to give the coating layer appropriate slipperiness, silica particles having an average particle size of 200 nm to 700 nm are particularly preferably used.

[0103] The amount of particles added to impart slipperiness is preferably less than 1% by weight relative to the adhesive resin layer. If the amount is less than 1% by weight, the adhesive resin layer contains a small number of particles larger than the thickness of the adhesive resin layer, which is preferable because cracks are less likely to propagate when folded. Furthermore, a more preferable embodiment is 0.5% by weight or less.

[0104] The coating liquid can be applied by a known method, similar to the coating layer described above, such as reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, wire bar coating, and pipe doctor coating, which can be used alone or in combination.

[0105] (Hard coat layer) When the polyester film of the present invention is used as a surface protection film for protecting a folding display by placing it on the surface of the display, it is preferable that the polyester film has a hard coat layer on at least one surface. The hard coat layer is preferably placed on the display surface side of the polyester film and used in the display. The resin for forming the hard coat layer can be siloxane-based, inorganic hybrid-based, acrylic-based, urethane acrylate-based, polyester acrylate-based, epoxy-based, or the like, without any particular limitation. In addition, two or more types of materials can be mixed and used, or particles such as inorganic filler or organic filler can be added.

[0106] Examples of the resin forming the hard coat layer include compounds having a (meth)acrylate functional group, such as polyester (meth)acrylate, urethane (meth)acrylate, epoxy (meth)acrylate, and silicone (meth)acrylate, and compounds having a functional group having an unsaturated double bond, such as an allyl group or a vinyl group. In addition, a polyfunctional monomer may be used in combination to increase the hardness of the hard coat layer. Examples of the polyfunctional monomer include trimethylolpropane tri(meth)acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate. The above materials may be used alone or in combination of two or more materials.

[0107] When the active energy ray for curing the hard coat layer is ultraviolet light, it is preferable to add a photopolymerization initiator. The photopolymerization initiator may be a radical polymerization system, a cationic polymerization system, or a mixed system of cationic polymerization and radical polymerization, but the radical polymerization system is particularly preferable because it has a high reaction rate and excellent productivity. Examples of ultraviolet radical polymerization initiators include alkylphenones, benzoins, benzophenones, phosphine oxides, ketals, anthraquinones, thioxanthones, azo compounds, peroxides, 2,3-dialkyldione compounds, disulfide compounds, fluoroamine compounds, aromatic sulfonium compounds, titanocenes, and oxyphenyl acetates, which may be used alone or in combination of two or more. Further specific examples include carbonyl compounds such as acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, Michler's ketone, benzil, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, methylbenzoyl formate, p-isopropyl-α-hydroxyisobutylphenone, α-hydroxyisobutylphenone, 2,2-dimethoxy-2-phenylacetophenone, and 1-hydroxycyclohexyl phenyl ketone; sulfur compounds such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone; and peroxide compounds such as benzoyl peroxide and di-t-butyl peroxide. The amount of the photopolymerization initiator added can be in the range of 0.1 parts by mass or more, more preferably 1 part by mass or more, and 30 parts by mass or less, more preferably 20 parts by mass or less, based on 100 parts by mass of the active energy ray curable resin. When the amount added is 0.1 parts by mass or more, the hardness of the hard coat layer can be increased, which is preferable. When the amount added is 30 parts by mass or less, there is no risk of the hard coat layer turning yellow, and the hard coat layer is sufficiently cured, which is preferable.

[0108] Furthermore, various additives may be contained within a range that does not impair the performance of the hard coat, such as a polymerization inhibitor, a crosslinking agent, an antistatic agent, an adhesion improver, an antioxidant, a leveling agent, a coupling agent, an antifoaming agent, a filler, a solvent, an antiglare agent, an antireflection agent, an inorganic filler, an organic filler, etc.

[0109] The refractive index of the hard coat layer is preferably smaller than that of the easy-adhesion resin layer in order to suppress iridescent coloring (interference patterns) of the hard coat film.

[0110] (Thickness of hard coat layer) The thickness of the hard coat layer is preferably 1 to 50 μm. If it is 1 μm or more, it can be cured sufficiently. In order to increase the pencil hardness, it is more preferably 5 μm or more. Furthermore, by making the thickness 50 μm or less, curling due to cure shrinkage of the hard coat can be suppressed, and the handling properties of the film can be improved.

[0111] (Application method) The hard coat layer can be applied by any method including, but not limited to, a Mayer bar, a gravure coater, a die coater, a knife coater, etc., and can be appropriately selected depending on the viscosity and film thickness.

[0112] (Curing conditions) The hard coat layer can be cured by energy rays such as ultraviolet rays and electron beams, or by heat, and is preferably cured by ultraviolet rays or electron beams in order to reduce damage to the film.

[0113] (Pencil hardness) The pencil hardness of the hard coat layer is preferably 3H or more, more preferably 4H or more. If the hard coat layer has a pencil hardness of 3H or more, it is not easily scratched and does not reduce visibility. In general, the pencil hardness of the hard coat layer is preferably high, but it may be 9H or less, 8H or less, or even 6H or less can be used without any practical problems.

[0114] (Characteristics of hard coat layer) The hard coat layer in the present invention can be used for the purpose of protecting a display by increasing the pencil hardness of the surface as described above, and preferably has a high transmittance. The transmittance of the hard coat film is preferably 85% or more, more preferably 87% or more, and even more preferably 88% or more. If the transmittance is 85% or more, sufficient visibility can be obtained. The total light transmittance of the hard coat film is generally preferably as high as possible, but is preferably 99% or less from the viewpoint of stable production, and may be 97% or less. In addition, the haze of the hard coat film is generally preferably low, and is preferably 3% or less. The haze of the hard coat film is more preferably 2% or less, and most preferably 1% or less. If the haze is 3% or less, the visibility of the image can be improved. The lower the haze, the better, but is generally preferably 0.1% or more from the viewpoint of stable production, and may be 0.3% or more.

[0115] The hard coat layer may further have other functions added thereto. For example, a hard coat layer having the above-mentioned functions such as an antiglare layer having a certain pencil hardness, an antiglare antireflection layer, an antireflection layer, a low reflection layer, and an antistatic layer is preferably used in the present invention.

[0116] A hard coat layer may also be provided when used as a substrate film of a touch panel module. When an ITO layer is used as a transparent electrode layer of a touch panel module, it is preferable to provide a refractive index adjustment layer between the substrate film and the transparent electrode layer to make the electrode pattern less visible. In this case, the hard coat layer itself may also serve as a refractive index adjustment layer, or a separate layer for refractive index adjustment may be laminated. EXAMPLES

[0117] Next, the present invention will be described with reference to examples and comparative examples. First, the methods for evaluating the properties of the polyester film of the present invention will be described below.

[0118] (1) Intrinsic viscosity The film or polyester resin was crushed and dried, and then dissolved in a mixed solvent of phenol / tetrachloroethane = 60 / 40 (mass ratio). After the solution was centrifuged to remove inorganic particles, the flow time of the solution with a concentration of 0.4 (g / dl) at 30°C and the flow time of the solvent alone were measured using an Ubbelohde viscometer, and the intrinsic viscosity was calculated from the ratio of these times using the Huggins equation and assuming that the Huggins constant is 0.38.

[0119] (2) Density The density was measured according to the method compliant with JIS K7112:1999 (density gradient tube method). (Unit: g / cm 3 ). (3) Average particle size of particles in the polyester film or the easily adhesive resin layer The particles on the cross section of the film are observed with a scanning electron microscope, 50 particles are observed, and the average of the observed particles is taken as the average particle size. The particle size of particles that are not spherical and have an irregular shape can be calculated as the equivalent circle diameter. The equivalent circle diameter is calculated by dividing the area of ​​the observed particle by pi (π), calculating the square root, and multiplying it by 2. (The unit used depends on the average particle size, but nm is mainly used.)

[0120] (4) Refractive index of a polyester film having an easily adhesive resin layer and before laminating a hard coat layer In accordance with JIS K7142:2008 "Method of measuring refractive index of plastics (Method A)" Using an Abbe refractometer (Atago Co., Ltd., NAR-4T, measurement wavelength 589 nm), the refractive index in the longitudinal direction, the refractive index in the width direction, and the refractive index in the thickness direction of the polyester film having an easy-adhesion resin layer and before laminating the hard coat layer were determined.

[0121] (5) Refractive index of easy-adhesive resin layer The refractive index of the easy-adhesion resin layer can be calculated by fitting the reflection spectrum measured using a spectrophotometer (product name "UV-3150", manufactured by Shimadzu Corporation) with the reflection spectrum calculated from an optical model of a thin film using Fresnel coefficients. The refractive index of the PET substrate is measured on the opposite side to the surface on which the easy-adhesion resin layer is formed (the back surface, or the surface of the easy-adhesion resin layer on the side on which the refractive index is not measured when the easy-adhesion resin layer is formed on both sides), and then the measurement is performed after attaching a black vinyl tape (for example, product name "Yamato Vinyl Tape NO200-38-21", manufactured by Yamato Co., Ltd., 38 mm wide) having a width larger than the measurement spot area to prevent back reflection.

[0122] (6) Bending resistance of polyester film sample (bending radius 1.5 mm) A polyester film sample with a size of 20 mm in the width direction × 110 mm in the flow direction is prepared. Using a no-load U-shaped stretch tester (Yuasa System Co., Ltd., DLDMLH-FS), the bending radius is set to 1.5 mm, and the sample is bent 200,000 times at a speed of 1 time / second. At that time, the sample is fixed at a position 10 mm from both ends of the long side, and the bending portion is 20 mm × 90 mm. Here, FIG. 1 is a schematic diagram for showing the bending radius when a folding display is folded, and considering the case where a polyester film is arranged on the inner surface of the folded state, a bending test is performed as a model with the portion indicated by the symbol 11 in FIG. 1 set to 1.5 mm. After the bending process, the sample was placed on a flat surface with the inner side of the bend facing down, and visual observation was performed. ○: No cracks or deformations were observed in the sample. ×: The sample had a crack or crease, and when placed horizontally, the maximum floating height was 5 mm or more.

[0123] (7) Bending resistance of polyester film sample (bending radius 0.5 mm) In the same manner as in the bending test, the bending radius was set to 0.5 mm and the display was bent 200,000 times at a speed of 1 time / second. Here, FIG. 1 is a schematic diagram showing the bending radius when the foldable display is folded, and considering the case where a polyester film is arranged on the inner surface of the folded state, a bending test was performed as a model with the portion indicated by reference numeral 11 in FIG. 1 set to 0.5 mm. The film surface on the outer side of the bent portion was observed at 700 times magnification with a digital microscope (HIROX RH8800) to observe the presence or absence of wrinkles (cracks). In addition to the above-mentioned visual bending resistance test with a bending radius of 1.5 mm, this test was performed with the bending radius reduced to 0.5 mm, with the intention of evaluating the display in a state close to the actual use state of the foldable display in which a hard coat layer or other members are laminated or attached. In addition to the visual observation with a bending radius of 1.5 mm, this test is for detecting minute defects that are difficult to detect by visual inspection, such as defects that are prone to breakage or cracking. ○: No defects on the film surface on the outer side of the bend. ×: Broken or wrinkles (cracks) were observed on the film surface on the outer side of the bend.

[0124] (8) Indentation depth after removing the test force The sample was cut into approximately 2 cm squares and fixed on a micro cover glass 18 × 18 mm (manufactured by Matsunami Glass Co., Ltd.) with an adhesive (Cemedine (registered trademark) High Super 30) on the surface opposite to the measurement surface. After adhesion and fixing, it was left at room temperature for 12 hours or more, and then the indentation depth (μm) after removing the test force was measured using a dynamic ultra-microhardness tester "DUH-211" (manufactured by Shimadzu Corporation) under the following conditions. <Measurement conditions> Test mode: Load-unload test Indenter used: 115 degree ridge angle, triangular pyramid indenter Indenter elastic modulus: 1.140×10 6 N / mm 2 Indenter Poisson's ratio: 0.07 Test force: 50mN Load speed: 4.44mN / sec Load holding time: 2sec Unloading holding time: 0sec

[0125] (9) Total light transmittance, haze The polyester film having the easy-adhesive resin layer laminated thereon was used as a sample, and the haze was measured using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0126] (10) Maximum heat shrinkage rate A sample film of polyester film laminated with an easy-adhesion resin layer was cut to 10 mm vertical x 250 mm horizontal, and marks were made at 200 mm intervals along the long side in the direction to be measured, and the distance A between the marks was measured under a constant tension of 5 g. The sample film was then left in an oven at an atmosphere of 150°C for 30 minutes without load, and then removed from the oven and cooled to room temperature. The distance B between the marks was then measured under a constant tension of 5 g, and the thermal shrinkage rate (%) was calculated using the following formula. The thermal shrinkage rate was measured at three equal positions in the width direction of the sample film, and the average value of the three points was taken as the thermal shrinkage rate (%). Heat shrinkage rate (%) = [(AB) x 100] / A The sample film is cut so that the length and width of the sample differ in both the bending direction and the folding direction, and measurements are taken. The data in the direction where the measured value is greater is regarded as the maximum heat shrinkage rate (%).

[0127] (11) Refractive Index of Hard Coat Layer The refractive index of the hard coat layer can be calculated by fitting the reflection spectrum measured using a spectrophotometer (product name "UV-3150", manufactured by Shimadzu Corporation) with the reflection spectrum calculated from an optical model of a multilayer thin film using Fresnel coefficients. The reflectance of the hard coat layer is measured after applying a hard coat composition to a 50 μm thick polyethylene terephthalate (PET) substrate on which an easy-adhesive resin layer is not applied, curing the composition to form a hard coat layer having a thickness of 1 to 10 μm, and attaching a black vinyl tape (for example, product name "Yamato Vinyl Tape NO200-38-21", manufactured by Yamato Co., Ltd., 38 mm wide) having a width larger than the measurement spot area to prevent backside reflection on the surface (backside) of the PET substrate opposite to the surface on which the hard coat layer is formed.

[0128] (12) Improvement of interference patterns of hard coat film (iris-like color) The hard-coated film was cut into an area of ​​50 mm (film width direction) × 110 mm (film length direction) to prepare a sample film. A black glossy tape (Nitto Denko, vinyl tape No. 21; black) was attached to the opposite side of the obtained sample film from the hard-coated layer. The hard-coated surface of this sample film was placed on top, and a three-wavelength neutral white light (National Pallook, FL 15EX-N 15W) was used as a light source, and the sample film was observed from above at an angle where the strongest reflection was observed (40 to 60 cm from the light source, 15 to 45° angle to the film surface).

[0129] The results of visual observation are ranked according to the following criteria. The observation is performed by five people familiar with the evaluation, and the most common rank is the evaluation rank. If there are two ranks with the same number of people, the center of the three ranks is adopted. For example, if there are two people who have ◎ and ○ and one person who has △, the middle of the three ranks is adopted. If there is one person who has ◎ and two people who have ○ and △, the middle of the three ranks is adopted. If there are two people who have ◎ and △ and one person who has ○, the middle of the three ranks is adopted. ◎: No iridescent color is observed from any angle ○: Slight iridescent coloring is visible at certain angles △: Slight iridescent coloring is observed ×: Clear iridescent color is observed

[0130] (13) Bending test properties of hard coat film A sample film was prepared by cutting out a hard-coated film into a size of 50 mm in the width direction × 110 mm in the machine direction. The obtained sample film was folded in the same manner as in the bending test method described above, with the easy-adhesion resin layer and the hard-coat layer facing inward, and a bending radius of 3.0 mm was set, and a bending test was performed 200,000 times at a speed of 1 time / second. After the test, the bent portion of the sample film was placed on a flat surface with the inner side of the bend facing down, and visually observed. ○: No cracks or deformations were observed in the sample. ×: Cracks or creases were observed in the sample.

[0131] (14) Observation of interference patterns (iris-like color) after bending test of hard coat film The bent portion of the sample film after the bending test of the hard-coated film described above was observed in the same manner as in the case of interference pattern improvement. Specifically, a black glossy tape (Nitto Denko, vinyl tape No. 21; black) was attached to the opposite side of the hard-coated layer of the obtained sample film. The hard-coated surface of the sample film was placed on top, and the sample film was observed from above at an angle with a three-wavelength daylight white light (National Pallook, FL 15EX-N 15W) as a light source, at a position where the strongest reflection was observed visually (40 to 60 cm from the light source, 15 to 45° angle with respect to the film surface). The results of the visual observation were ranked according to the following criteria. The observation was performed by five people familiar with the evaluation, and the most common rank was determined as the evaluation rank. If the number of people with two ranks was the same, the center of the three ranks was adopted. For example, if there are 2 ◎s and 2 ○s and 1 △, then ○ will be selected; if there is 1 ◎ and 2 ○s and 2 △s, then ○ will be selected; and if there are 2 ◎s and 2 △s and 1 ○, then ○ will be selected. ◎: No iridescent color is observed from any angle ○: Slight iridescent coloring is visible at certain angles △: Slight iridescent coloring is observed ×: Clear iridescent color is observed

[0132] This test is conducted to evaluate interference patterns and detect interference patterns caused by minute adhesion defects such as interfacial peeling and cracks between the hard coat layer and the highly adhesive resin layer and polyester film layer.

[0133] (15) Pencil hardness The pencil hardness of the hard coat film sample was measured at a load of 750 g and a speed of 1.0 mm / s in accordance with JIS K 5600-5-4: 1999. In the present invention, a value of 3H or more was considered to be acceptable.

[0134] (Preparation of polyethylene terephthalate pellets (R1)) A continuous esterification reactor consisting of a three-stage complete mixing tank having an agitator, a partial condenser, a raw material inlet, and a product outlet was used as the esterification reactor, and the slurry was continuously fed to the first esterification reactor of the esterification reactor with TPA at 2 tons / hr, EG at 2 moles per mole of TPA, and antimony trioxide at an amount such that Sb atoms were 160 ppm relative to the produced PET, and reacted at normal pressure for an average residence time of 4 hours at 255°C. Next, the reaction product in the first esterification reactor was continuously taken out of the system and fed to the second esterification reactor, and EG distilled from the first esterification reactor was fed to the second esterification reactor at 8% by mass relative to the produced polymer (produced PET), and further, an EG solution containing magnesium acetate in an amount such that Mg atoms were 65 ppm relative to the produced PET and an EG solution containing TMPA in an amount such that P atoms were 20 ppm relative to the produced PET were added, and reacted at normal pressure for an average residence time of 1.5 hours at 260°C. Next, the reaction product in the second esterification reactor was continuously taken out of the system and fed to a third esterification reactor, and an EG solution containing TMPA in an amount such that the P atom was 20 ppm relative to the produced PET was added, and the reaction was carried out at normal pressure for an average residence time of 0.5 hours at 260° C. The esterification reaction product produced in the third esterification reactor was continuously fed to a three-stage continuous polycondensation reactor to carry out polycondensation, and further filtered with a stainless steel sintered filter medium (nominal filtration accuracy of 90% cut of 5 μm particles) to obtain polyethylene terephthalate pellets (R1) with an intrinsic viscosity of 0.62 dl / g.

[0135] (Preparation of polyethylene terephthalate pellets (R2)) Polyethylene terephthalate pellets (R2) were obtained by adjusting the intrinsic viscosity to 0.580 dl / g in the same manner as in the production process of polyethylene terephthalate pellets (R1), except that the residence time of the third esterification reaction was adjusted.

[0136] (Preparation of polyethylene terephthalate pellets (R3)) The polyethylene terephthalate pellets (R1) were subjected to solid-phase polymerization at 220°C under a reduced pressure of 0.5 mmHg for various times using a rotary vacuum polymerization apparatus to produce polyethylene terephthalate pellets (R3) with an intrinsic viscosity of 0.75 dl / g.

[0137] (Polymerization of Copolymerized Polyester Resin) The copolymerization of the polyester resins (a1) to (a3) ​​for forming the easy-adhesion resin layer was carried out as follows. In a stainless steel autoclave equipped with a stirrer, a thermometer, and a partial reflux condenser, 410.3 parts by mass of dimethyl 2,6-naphthalenedicarboxylate, 46.3 parts by mass of sebacic acid, 42.5 parts by mass of dimethyl sodium 5-sulfoisophthalate, 175.6 parts by mass of ethylene glycol, 29.2 parts by mass of diethylene glycol, 204.2 parts by mass of 1,6-hexanediol, and 0.5 parts by mass of tetra-n-butyl titanate were charged, and an ester exchange reaction was carried out from 160°C to 220°C over 4 hours. The temperature was then raised to 255°C, and the reaction system was gradually reduced in pressure, and then the reaction was carried out under a reduced pressure of 30 Pa for 1 hour and 30 minutes to obtain a copolymer polyester resin (a1). The obtained copolymer polyester resin was pale yellow and transparent. The composition of the copolymer polyester resin (a1) is shown in Table 1.

[0138] In addition, by changing the raw materials, copolymer polyester resins (a2) and (a3) ​​having the compositions shown in Table 1 were obtained in the same manner. The compositions and weight average molecular weights of these copolymer polyester resins were measured by 1H-NMR, and the results are shown in Table 1.

[0139] [Table 1]

[0140] (Preparation of aqueous dispersion of copolymerized polyester resin) In a reactor equipped with a stirrer, a thermometer and a reflux device, 25 parts by mass of copolymerized polyester resin (a1) and 15 parts by mass of ethylene glycol t-butyl ether were placed, and the mixture was heated to 110°C and stirred to dissolve the resin. After the resin was completely dissolved, 60 parts by mass of water was gradually added to the polyester solution while stirring. After the addition, the liquid was cooled to room temperature while stirring to prepare an aqueous dispersion (Aw-1) of a milky white copolymerized polyester with a solid content of 25% by mass. Similarly, aqueous dispersions were prepared using copolymerized polyester resins (a2) to (a3) ​​instead of copolymerized polyester resin (a1), and these were named aqueous dispersions (Aw-2) to (Aw-3).

[0141] (Polymerization of urethane resin) Into a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, 72.96 parts by mass of 1,3-bis(isocyanatemethyl)cyclohexane, 12.60 parts by mass of dimethylolpropionic acid, 11.74 parts by mass of neopentyl glycol, 112.70 parts by mass of polycarbonate diol having a number average molecular weight of 2000, and 85.00 parts by mass of acetonitrile and 5.00 parts by mass of N-methylpyrrolidone were added, and the mixture was stirred for 3 hours at 75°C under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, after lowering the temperature of this reaction liquid to 40°C, 9.03 parts by mass of triethylamine was added to obtain a polyurethane prepolymer solution. Next, 450g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the mixture was adjusted to 25°C and stirred for 2000min. -1 While stirring and mixing at 40° C., the isocyanate-terminated prepolymer was added and dispersed in water. Then, acetonitrile and a part of the water were removed under reduced pressure to prepare a water-soluble polyurethane resin (B-1) with a solid content of 35% by mass.

[0142] (Preparation of self-crosslinking polyurethane resin aqueous solution) 100 parts by mass of polyester diol (OHV: 2000eq / ton) composed of adipic acid, 1,6-hexanediol, and neopentyl glycol (molar ratio: 4 / 2 / 3) was mixed with 41.4 parts by mass of xylylene diisocyanate, and reacted at 80-90°C for 1 hour under a nitrogen stream, then cooled to 60°C, and dissolved by adding 70 parts by mass of tetrahydrofuran to obtain a urethane prepolymer solution (NCO / OH ratio: 2.2, free isocyanate group: 3.30% by mass). The urethane prepolymer solution was then heated to 40°C, and then 45.5 parts by mass of a 20% by mass aqueous sodium bisulfite solution was added and reacted at 40-50°C for 30 minutes while stirring vigorously. After confirming the disappearance of the free isocyanate group content (converted into solid content), the solution was diluted with emulsified water to obtain a self-crosslinking polyurethane resin aqueous solution (B-2) containing isocyanate groups blocked with sodium bisulfite and having a solid content of 20% by mass.

[0143] (Polymerization of blocked isocyanate compounds) A flask equipped with a stirrer, a thermometer, and a reflux condenser was charged with 100 parts by mass of a polyisocyanate compound having an isocyanurate structure made from hexamethylene diisocyanate (Asahi Kasei Chemicals, Duranate TPA), 55 parts by mass of propylene glycol monomethyl ether acetate, and 30 parts by mass of polyethylene glycol monomethyl ether (average molecular weight 750), and the mixture was kept at 70°C for 4 hours under a nitrogen atmosphere. Thereafter, the reaction liquid temperature was lowered to 50°C, and 47 parts by mass of methyl ethyl ketoxime was added dropwise. The infrared spectrum of the reaction liquid was measured to confirm that the absorption of the isocyanate group had disappeared, and a blocked polyisocyanate liquid with a solid content of 75% by mass was obtained.

[0144] (Adjustment of water-dispersible blocked isocyanate) Water was added to the blocked polyisocyanate liquid obtained above to obtain a blocked polyisocyanate aqueous dispersion (C-1) having a solid content of 40 mass %.

[0145] (Polymerization of Water-soluble Carbodiimide Compounds) In a flask equipped with a thermometer, a nitrogen gas inlet tube, a reflux condenser, a dropping funnel, and a stirrer, 200 parts by mass of isophorone diisocyanate and 4 parts by mass of 3-methyl-1-phenyl-2-phospholene-1-oxide as a carbodiimide catalyst were added, and the mixture was stirred for 10 hours at 180°C under a nitrogen atmosphere to obtain isocyanate-terminated isophorone carbodiimide (polymerization degree = 5). Next, 111.2 g of the obtained carbodiimide and 80 g of polyethylene glycol monomethyl ether (molecular weight 400) were reacted at 100°C for 24 hours. Water was gradually added to the mixture at 50°C to obtain a yellow, transparent, water-soluble carbodiimide compound (C-2) with a solid content of 40% by mass.

[0146] (Melamine-based crosslinking agent) As the melamine-based crosslinking agent, Beckamin (registered trademark) M-3 (solid content concentration 60%) manufactured by DIC Corporation was used (melamine-based crosslinking agent (C-3)).

[0147] (Polymerization of oxazoline-based crosslinking agents) A mixture of 58 parts by mass of ion-exchanged water and 58 parts by mass of isopropanol as an aqueous medium, and 4 parts by mass of a polymerization initiator (2,2'-azobis(2-amidinopropane) dihydrochloride) were placed in a flask equipped with a thermometer, a nitrogen gas inlet tube, a reflux condenser, a dropping funnel, and a stirrer. Meanwhile, a mixture of 16 parts by mass of 2-isopropenyl-2-oxazoline as a polymerizable unsaturated monomer having an oxazoline group, 32 parts by mass of methoxypolyethylene glycol acrylate (average number of moles of ethylene glycol added: 9 moles, Shin-Nakamura Chemical Co., Ltd.), and 32 parts by mass of methyl methacrylate were placed in the dropping funnel, and added dropwise at 70°C for 1 hour under a nitrogen atmosphere. After the dropwise addition was completed, the reaction solution was stirred for 9 hours and cooled to obtain a water-soluble resin (C-4) having an oxazoline group with a solid content concentration of 40% by mass.

[0148] (zirconia particles) In a 3-liter glass container, 2283.6 g of pure water and 403.4 g of oxalic acid dihydrate were added and heated to 40°C to prepare a 10.72 mass% oxalic acid aqueous solution. While stirring this aqueous solution, 495.8 g of zirconium oxycarbonate powder (ZrOCO3, manufactured by AMR International Corp., containing 39.76 mass% in terms of ZrO2) was gradually added and mixed for 30 minutes, and then heated at 90°C for 30 minutes. Next, 1747.2 g of a 25.0 mass% aqueous tetramethylammonium hydroxide solution (manufactured by Tama Chemicals Co., Ltd.) was gradually added over 1 hour. At this point, the mixture was in a slurry state, and ZrO2 The content was 4.0% by mass in terms of ZrO2. The slurry was transferred to a stainless steel autoclave container and subjected to hydrothermal treatment at 145°C for 5 hours. The product after this hydrothermal treatment was completely solated with no undissolved matter. The obtained sol contained 4.0% by mass as ZrO2, had a pH of 6.8, and an average particle size of 19 nm. The transmittance measured by adjusting the sol to a ZrO2 concentration of 2.0% by mass with pure water was 88%. When the particles were observed with a transmission electron microscope, most of the particles were aggregated particles of ZrO2 primary particles of about 7 nm. 4000 g of zirconia sol with a ZrO2 concentration of 4.0% by mass obtained by the above hydrothermal treatment was washed and concentrated using an ultrafiltration device while gradually adding pure water, and 953 g of zirconia sol with a ZrO2 concentration of 13.1% by mass, pH 4.9, and transmittance of 76% at a ZrO2 concentration of 13.1% by mass was obtained.

[0149] 300g of zirconia sol with a ZrO2 concentration of 13.1% by mass obtained by the above washing and concentration was added with 3.93g of 20% by mass citric acid aqueous solution and 11.0g of 25% by mass tetramethylammonium hydroxide aqueous solution, and then concentrated by ultrafiltration to obtain 129g (D-1) of a high concentration of ZrO2 concentration of 30.5% by mass. The obtained high concentration zirconia sol had a pH of 9.3 and an average particle size of 19 nm. In addition, this zirconia sol had no precipitate and was stable for more than one month under conditions of 50°C.

[0150] (Zirconia water dispersion) The zirconia sol obtained above was mixed with a polyacrylic acid dispersant (Aron A-30SL, manufactured by Toa Gosei Co., Ltd.) to prepare a zirconia aqueous dispersion having a solid content concentration of 13% by mass. A zirconia aqueous dispersion D-1 was obtained in which the solid content concentration was 3% by mass of the dispersant and 10% by mass of zirconia.

[0151] (Titania particles) 12.09 kg of titanium tetrachloride aqueous solution containing 7.75 mass% titanium tetrachloride (manufactured by Osaka Titanium Technologies Co., Ltd.) in terms of TiO2 was mixed with 4.69 kg of ammonia water containing 15 mass% ammonia (manufactured by Ube Industries, Ltd.) to prepare a white slurry liquid with a pH of 9.5. Next, the slurry was filtered and washed with pure water to obtain 9.87 kg of hydrous titanic acid cake with a solid content of 10 mass%. Next, 11.28 kg of hydrogen peroxide water containing 35 mass% hydrogen peroxide (manufactured by Mitsubishi Gas Chemical Co., Ltd.) and 20.00 kg of pure water were added to the cake, and the mixture was heated at a temperature of 80°C for 1 hour under stirring, and 57.52 kg of pure water was added to obtain 98.67 kg of a titanic acid peroxide aqueous solution containing 1 mass% titanic acid in terms of TiO2. This titanic acid peroxide aqueous solution was transparent yellow-brown and had a pH of 8.5.

[0152] Next, 98.67 kg of the titanic acid peroxide aqueous solution was mixed with 4.70 kg of a cation exchange resin (manufactured by Mitsubishi Chemical Corporation), and 12.33 kg of a potassium stannate aqueous solution containing 1 mass % of potassium stannate (manufactured by Showa Kako Co., Ltd.) calculated as SnO2 was gradually added thereto under stirring. Next, the cation exchange resin that had taken in potassium ions and the like was separated, and then placed in an autoclave (manufactured by Taiatsu Glass Industry Co., Ltd., 120 L) and heated at a temperature of 165°C for 18 hours.

[0153] Next, the obtained mixed aqueous solution was cooled to room temperature, and then concentrated with an ultrafiltration membrane device (ACV-3010, manufactured by Asahi Kasei Corporation) to obtain 9.90 kg (D-2) of a water-dispersed sol containing titanium-based fine particles with a solid content of 10% by mass. When the solid matter contained in the sol thus obtained was measured by the above method, it was found to be titanium-based fine particles (primary particles) made of a composite oxide containing titanium and tin having a rutile crystal structure. Furthermore, when the content of metal components contained in the titanium-based fine particles was measured, it was found to be TiO2 87.2% by mass, SnO2 11.0% by mass, and K2O 1.8% by mass, calculated based on the oxide of each metal component. In addition, the pH of the mixed aqueous solution was 10.0. Furthermore, the water-dispersed sol containing the titanium-based fine particles was transparent and milky white, the average particle diameter of the titanium-based fine particles contained in this water-dispersed sol was 35 nm, and the distribution frequency of coarse particles having a particle diameter of 100 nm or more was 0%. Furthermore, the refractive index of the obtained titanium-based particles was deemed to be 2.42.

[0154] (Titania water dispersion) The titanium-based fine particles obtained above were mixed with a polyacrylic acid dispersant (Aron A-30SL, manufactured by Toa Gosei Co., Ltd.) to prepare a titania aqueous dispersion with a solid content concentration of 13% by mass. Titania aqueous dispersion D-2 was obtained, in which 3% by mass of the solid content was the dispersant and 10% was titania.

[0155] (zirconia / titania mixed dispersion) The zirconia sol obtained above was mixed with titania-based fine particles and a polyacrylic acid dispersant (Aron A-30SL, manufactured by Toa Gosei Co., Ltd.) to prepare a zirconia / titania mixed aqueous dispersion with a solid concentration of 13% by mass. Mixed dispersion D-3 was obtained, in which 3% by mass of the solid concentration was the dispersant, 7.5% was zirconia, and 2.5% was titania.

[0156] (Silica particles) As the silica particles, colloidal silica having a particle diameter of 40 nm and a solid content concentration of 30 mass % was used as D-4.

[0157] (Silica particles) In order to impart slipperiness, silica particles having a particle diameter of 450 nm and a solid content concentration of 40 mass % were used as D-5.

[0158] (Surfactant) In order to improve the leveling properties of the coating film when forming the highly adhesive resin layer, a silicone-based surfactant having a solid content concentration of 100% by mass was used as E-1.

[0159] (Preparation of Coating Solution for Forming Adhesion Layer) The following coating materials were mixed to prepare coating solution P-1. Water 47.52 parts by mass Isopropanol 25.00 parts by weight Polyester resin (Aw-1) 17.75 parts by mass Water-dispersible blocked isocyanate compound (C-1) 4.76 parts by mass Zirconia / titania mixed water dispersion (D-3) 4.88 parts by mass Silica particles (D-5) 0.06 parts by mass (Silica sol with average particle size of 450 nm, solid content concentration of 40% by mass) Silicone surfactant (E-1) 0.03 parts by mass (Silicone-based, solids concentration 100% by mass)

[0160] Similarly, coating solutions P-2 to P-14 were prepared by mixing the coating materials in the ratios shown in Table 2.

[0161] [Table 2]

[0162] Example 1 Pellets of polyethylene terephthalate (R1) were fed to an extruder and melted at 285°C. The polymer was filtered with a stainless steel sintered filter medium (nominal filtration accuracy 10μm particles 95% cut), extruded from a die in the form of a sheet, and then contacted with a casting drum with a surface temperature of 30°C using an electrostatic casting method to cool and solidify, producing an unstretched film. The unstretched film was uniformly heated to 75°C using a heating roll, heated to 85°C using a non-contact heater, and roll-stretched (longitudinal stretching) 1.4 times. The above-mentioned coating liquid (P-1) for forming an easy-adhesion resin layer was applied to both sides of the obtained uniaxially stretched film by a roll coating method, and then dried at 80°C for 20 seconds. The coating amount after the final (biaxial stretching) drying was 0.09g / m 2 The film was then introduced into a tenter, preheated at 105°C, transversely stretched 4.0 times at 95°C, fixed in width, heat-set at 230°C for 5 seconds, and further relaxed in the width direction by 4% at 180°C to obtain a polyethylene terephthalate film with a thickness of 50 μm.

[0163] A hard coat coating solution (H-1 below) was applied to one side of the polyethylene terephthalate film having the above-mentioned easy-adhesion resin layer using a Mayer bar so that the film thickness after drying would be 10 μm, and the film was dried at 80° C. for 1 minute, and then irradiated with ultraviolet light (accumulated light amount 200 mJ / cm 2 ) to obtain a hard coat film.

[0164] (Coating solution for forming hard coat layer: H-1) 95 parts by mass of a urethane acrylate hard coat agent (Beamset (registered trademark) 577, solids concentration 100%, manufactured by Arakawa Chemical Industries, Ltd.), 5 parts by mass of a photopolymerization initiator (Irgacure (registered trademark) 184, solids concentration 100%, manufactured by BASF Japan Ltd.), and 0.1 parts by mass of a leveling agent (BYK307, solids concentration 100%, manufactured by BYK Japan K.K.), were mixed and diluted with a solvent of toluene / MEK=1 / 1 to prepare a coating solution (H-1) for forming a hard coat layer with a solids concentration of 40%.

[0165] (Examples 2 to 3) A polyester film and a hard coat film were obtained in the same manner as in Example 1, except that the longitudinal stretching ratio was changed to the values ​​shown in Table 3.

[0166] Example 4 A polyester film and a hard coat film were obtained in the same manner as in Example 1, except that the stretching ratio in the width direction was changed to 5.5 times and the heat setting temperature was changed to 190°C.

[0167] (Examples 5 to 14) As shown in Table 3, the coating solutions for forming an easily adhesive resin layer were changed to P-2 to P-11, and the same procedure as in Example 1 was repeated to obtain polyester films and hard coat films.

[0168] (Examples 15 and 16) As shown in Table 4, a polyester film and a hard-coated film were obtained in the same manner as in Example 1, except that the hard-coat coating solution H-1 was changed to the following H-2 and H-3.

[0169] (Coating solution for forming hard coat layer: H-2) 30 parts by mass of pentaerythritol tri- and tetraacrylate (Toagosei Co., Ltd., Aronix (registered trademark) M-306, solid content concentration 100%), 65 parts by mass of polyester acrylate (Toagosei Co., Ltd., Aronix (registered trademark) M9050, solid content 100%), 5 parts by mass of photopolymerization initiator (BASF Japan, Ltd., Irgacure (registered trademark) 907, solid content concentration 100%), 0.1 parts by mass of leveling agent (BYK Japan, Ltd., BYK307, solid content concentration 100%) were mixed and diluted with a solvent of toluene / MEK = 1 / 1 to prepare a hard coat coating solution (H-2) with a concentration of 40% by mass.

[0170] (Coating solution for forming hard coat layer: H-3) To 100 parts by mass of a hard coat material (Opstar (registered trademark) Z7503, manufactured by JSR Corporation, concentration 75%), 0.1 parts by mass of a leveling agent (BYK307, manufactured by BYK Japan, concentration 100%) was added, and the mixture was diluted with methyl ethyl ketone to prepare a hard coat coating solution (H-3) with a solid content concentration of 40% by mass.

[0171] Comparative Example 1 A polyester film and a hard coat film were obtained in the same manner as in Example 1, except that the film was not stretched in the longitudinal direction but was stretched only in the width direction, that is, uniaxially stretched in the transverse direction.

[0172] Comparative Example 2 A polyester film and a hard coat film were obtained in the same manner as in Example 4, except that the film was not stretched in the longitudinal direction but was stretched only in the width direction, that is, uniaxially stretched in the transverse direction.

[0173] (Comparative Examples 3 to 7) A polyester film and a hard coat film were obtained in the same manner as in Example 1, except that the heat setting temperature was changed to 220° C., and the PET pellets and thicknesses were as shown in Table 1.

[0174] Comparative Example 8 A polyester film and a hard coat film were obtained in the same manner as in Example 1, except that the stretching ratio in the longitudinal direction was changed to 3.4 times.

[0175] (Comparative Examples 9 to 11) As shown in Table 3, polyester films and hard coat films were obtained in the same manner as in Example 1, except that the coating solutions were changed to P-12 to P-14.

[0176] The evaluation results are shown in Tables 3 and 4.

[0177] [Table 3]

[0178] [Table 4]

[0179] In the cases of Examples 1 to 16, in which the refractive index of the polyester film having an easy-adhesion layer was within a certain range, and a hard coat layer was provided on the easy-adhesion resin layer of the polyester film formed by curing a composition containing at least one compound selected from titanium compounds and zirconium compounds and a polyester resin, the pencil hardness of the hard coat was satisfactory, and the improvement in interference patterns after continuous bending tests was also good.

[0180] In each example, when the cross section was observed with a transmission electron microscope, it was found that the particles contained in the highly adhesive resin layer were present in a smaller proportion in the width direction, i.e., the direction of the fold, than in the longitudinal direction, i.e., the direction of bending.

[0181] In Comparative Examples 1 to 8, in which the film-forming conditions for the polyester film were changed, the refractive index of the polyester film having the easy-adhesion resin layer was not within the optimum range, and therefore the pencil hardness of the resulting hard coat film was not satisfactory.

[0182] In Comparative Example 9, in which the easy-adhesion resin layer was changed, neither titanium compound nor zirconia compound was contained, and the refractive index adjustment of the easy-adhesion resin layer was insufficient, so that no improvement in interference patterns was observed before the bending test of the hard coat film.In addition, the dispersibility of silica, which was used instead of the metal compound, was poor, and the interference patterns after the bending test were also deteriorated.

[0183] In Comparative Example 10, in which the easy-adhesion resin layer was changed, an improvement in the interference patterns before the bending test was observed, but the dispersibility of the silica, in which a titanium compound was used instead of a zirconia compound, was poor, and a deterioration in the interference patterns was observed after the bending test due to the occurrence of cracks in the easy-adhesion resin layer.

[0184] In Comparative Example 11, in which the easy-adhesion resin layer was changed, a large amount of titanium / zirconia mixed oxide had to be added to adjust the refractive index because the polyester resin was not included. As a result, the metal oxide in the coating film also aggregated, and the interference pattern after the bending test was deteriorated.

[0185] The hard coat film according to each Example and Comparative Example was attached to an organic EL module via a 25 μm thick adhesive layer, and a smartphone-type folding display that can be folded in half at the center of the entire display with a radius of 3 mm corresponding to the bending radius in FIG. 1 was created. The hard coat film was arranged on the surface of one continuous display through the folding portion, and the hard coat layer was arranged so as to be located on the surface of the display. The hard coat film of each Example was used to satisfy the operation and visibility as a smartphone that can be folded in half at the center and carried around. In addition, the surface was not dented by external force. On the other hand, the folding display using the hard coat film of each Comparative Example seemed to have generated image distortion at the folding portion of the display as the frequency of use increased, and also seemed to have deteriorated visibility due to the generation of interference spots, which was not very preferable. In addition, some of the displays had dents and scratches on the surface. [Industrial Applicability]

[0186] A folding display using the hard coat film for folding displays of the present invention maintains mass productivity, and the hard coat film located on the surface of the folding display does not deform after repeated folding, so that there is no distortion of the image at the folded part of the display. In particular, a mobile terminal device or image display device equipped with a folding display using the hard coat film of the present invention as a surface protective film provides beautiful images, is rich in functionality, and has excellent convenience such as portability. [Explanation of symbols]

[0187] 1: Foldable display 11: Bending radius 2: Polyester film for surface protection of folding displays 21: Folding section 22: Bending direction (direction perpendicular to the folding part)

Claims

1. A hard coat film for a folding display having an easy-adhesion resin layer and a hard coat layer in this order on at least one side of a polyester film having a thickness of 10 to 80 μm, the easy-adhesion resin layer is formed by curing a composition containing at least one compound selected from a titanium compound and a zirconium compound, a polyester resin, and a surfactant; At least one compound selected from the titanium compounds and zirconium compounds is The average particle size is 5 nm or more and 150 nm or less, The total amount of the titanium compound and the zirconium compound is, relative to the adhesive resin layer, A concentration of 0.1% by mass or more and less than 15% by mass, The intrinsic viscosity of the resin pellets forming the polyester film is more than 0.58 dl / g and less than 0.75 dl / g, In the film having the polyester film and the easy-adhesion resin layer, The adhesive resin layer has a coating amount after drying of 0.005 to 0.20 g / m 2 The refractive index and density of the layer formed so as to satisfy the following conditions: The refractive index in the bending direction is 1.590 to 1.

620. The refractive index in the direction of the fold is 1.670 to 1.700, The refractive index in the thickness direction is 1.520 or less, Density is 1.380 g / cm 3 That's all. (Here, the bending direction is a longitudinal direction of the film having the polyester film and the easy-adhesion resin layer, the direction of the folded portion is the width direction of the film having the polyester film and the easy-adhesion resin layer; The polyester resin in the easily adhesive resin layer contains a dicarboxylic acid component and a diol component, and the dicarboxylic acid component is at least a part of the polyester resin, and the polyester resin contains a naphthalene dicarboxylic acid component. Hard coat film for folding displays.

2. The refractive index of the easy-adhesion resin layer is lower than the refractive index in the bending direction of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer, and the refractive index in the direction of the folded portion, and is higher than the refractive index of the hard coat layer. The hard coat film for folding displays according to claim 1.

3. The hard coat film for a folding display according to claim 1, wherein the refractive index of the easy-adhesion resin layer satisfies the following condition: the refractive index of the easy-adhesion resin layer is lower than the refractive index in the bending direction of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer, and the difference between the refractive indices is greater than 0 and not greater than 0.07; The refractive index of the easy-adhesion resin layer is lower than the refractive index in the direction of the folded portion of the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer, and the difference in refractive index is 0.080 or more and 0.150 or less.

4. the polyester film having the easy-adhesion resin layer and before laminating the hard coat layer has a total light transmittance of 85% or more, a haze of 3% or less, and a maximum heat shrinkage of 6% or less; The maximum heat shrinkage rate is measured after leaving the sample film in an oven at 150° C. for 30 minutes without load and cooling it to room temperature. The hard coat film for a folding display according to claim 1 .

5. The composition for forming the easy-adhesion resin layer further contains a crosslinking agent, The content of the crosslinking agent is 5% by mass or more and 50% by mass or less based on the total solid content of the easy-adhesion resin layer. The hard coat film for a folding display according to claim 1 .

6. The hard coat film for folding displays according to claim 1, wherein the average particle size of the particles contained in the easy-adhesion resin layer is 200 nm or more and 700 nm or less.

7. The hard coat film for a folding display according to claim 1 , wherein the surfactant contained in the easy-adhesion resin layer is a silicone-based surfactant.

8. A foldable display in which the hard coat film for a foldable display according to claim 1 is arranged as a surface protective film so that the hard coat layer is positioned on the surface, and a single continuous hard coat film is arranged through the folding portion of the foldable display.

9. A mobile terminal device comprising the foldable display according to claim 8.

Citation Information

Patent Citations

  • Folding display and mobile terminal device

    JP2018072663A

  • Polyester film and applications thereof

    WO2018150940A1

  • Polyester film as surface protective film for foldable display and application thereof

    WO2018159285A1

  • Polyester film for surface protection film of foldable display and use thereof