Composite bearings having polyimide matrix

A composite bearing assembly using a polyimide matrix with dispersed fillers and thermoplastics addresses the challenge of balancing wear resistance and friction, achieving superior performance through a novel production method that enhances both characteristics.

JP2024160356AInactive Publication Date: 2024-11-13SAINT GOBAIN PERFORMANCE PLASTICS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024135692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2013-12-31
Filing Date
2024-08-15
Publication Date
2024-11-13
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 2024160356000001_ABST
    Figure 2024160356000001_ABST
Patent Text Reader

Abstract

To provide novel bearing and seal assemblies improved in both wear resistance and a coefficient of friction.SOLUTION: The present disclosure relates to bearing and seal assemblies comprising a composite structure which includes a substrate and a layer 30 deposited on the substrate 20. The layer deposited on the substrate contains a polyimide matrix and a filler dispersed within the polyimide matrix. The filler can be a thermoplastic polymer, such as PTFE, and / or an organic filler. The bearing assembly can exhibit synergistic improvement in wear resistance and a coefficient of friction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to composites, and more particularly to composites used to construct bearings and seals. Pertaining to the body. [Background technology]

[0002] Bearing and seal assemblies are widely used in industry at the interface between moving and stationary surfaces. Conventionally, it has been used to obtain a desirable low coefficient of friction and to improve wear resistance of the bearing assembly. However, most of the attempts to improve wear resistance have focused on the coefficient of friction. Thus, the composite has improved wear resistance. The company has developed a new bearing and seal assembly that exhibits both improved wear resistance and improved coefficient of friction. There is a need to issue

[0003] Additionally, composite bearings and particularly composite bearings incorporating a polyimide matrix There are drawbacks to the methods of producing polyimides, particularly in situ or continuous production. A method for forming a doped matrix is ​​desirable. In this way, the polyimide matrix with dispersed fillers or thermoplastics is The imidization and formation of tungsten has never been disclosed or suggested.

[0004] The present disclosure provides composite assemblies that meet these needs and other needs, which are described in detail below. Serve the buri. [Brief description of the drawings]

[0005] Embodiments are illustrated with reference to examples and not limitation in the accompanying figures.

[0006] [Figure 1]FIG. 1 is an illustration of a composite according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is an illustration of a composite according to another embodiment of the present disclosure. [Diagram 3] FIG. 3 is an illustration of a test assembly for testing wear rate and coefficient of friction according to ASTM G-77. [Figure 4] FIG. 4 is a trace of wear and temperature as a function of time for Sample 1. [Diagram 5] FIG. 5 is a plot of the coefficient of friction as a function of time for Sample 1. [Figure 6] FIG. 6 is a trace of wear and temperature as a function of time for Sample 2. [Figure 7] FIG. 7 is a plot of the coefficient of friction as a function of time for Sample 2. [Figure 8] FIG. 8 is a trace of wear and temperature as a function of time for Sample 3. [Figure 9] FIG. 9 is a plot of the coefficient of friction as a function of time for Sample 3. [Figure 10] FIG. 10 illustrates an SEM of Sample 1. [Figure 11] FIG. 11 illustrates an SEM of Sample 1. [Figure 12] FIG. 12 illustrates an SEM of Sample 2. [Figure 13] FIG. 13 illustrates an SEM of Sample 2. [Figure 14] FIG. 14 illustrates an SEM of Sample 3. [Figure 15] FIG. 15 illustrates an SEM of Sample 3. [Figure 16] FIG. 16 illustrates the dry coefficient of friction data for Example 3. [Figure 17] FIG. 17 illustrates the lubricated coefficient of friction data for Example 3. [Figure 18] FIG. 18 illustrates a bearing pre-composite according to one embodiment. [Figure 19]FIG. 19 illustrates a bearing pre-composite according to another embodiment. [Figure 20] FIG. 20 illustrates the bearing pre-composite of FIG. 19 with the release layer removed, according to one embodiment.

[0007] Those skilled in the art will appreciate that the elements in the figures are illustrated for simplicity and clarity, Please understand that the drawings are not necessarily to scale. For example, some elements in the figures may differ slightly from those shown. Dimensions may be exaggerated relative to other elements to facilitate understanding of embodiments of the present invention. It is possible that. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The following description is provided in conjunction with the figures to facilitate understanding of the teachings disclosed herein. The discussion focuses on specific implementations and embodiments of the teachings. This focus facilitates the explanation of the teachings. These are merely for illustrative purposes and should not be construed as limiting the scope and applicability of the teachings. However, other embodiments may be used based on the teachings disclosed herein.

[0009] As used herein, "comprises" and "compris "including", "including", "Has," "having," or other variations are non-exclusive. For example, a method, article, or apparatus that includes a set of features is intended to encompass the entire , but is not limited to, features not expressly recited or otherwise included in such It may include other features that are inherent to the method, article, or device. Further, unless expressly stated otherwise, and "or" refers to an inclusive "or" and not an exclusive "or." For example, Condition A or B is satisfied by one of the following: A is true (or exists) , B is wrong (or does not exist), A is wrong (or does not exist) and B is right (or exist) and both A and B are true (or exist).

[0010] Additionally, the use of "a" or "an" refers to any element or elements described herein. This is used merely for convenience and to give a general sense of the scope of the invention. This description is to be read to include one or at least one The singular includes the plural, unless it is clear that the plural should or should not be construed as meaning the opposite. For example, where an item is referred to in the singular, it is understood to mean two or more. Similarly, two or more items may be used in place of a singular item. When appearing in the specification, a single item may be substituted for two or more of its items. .

[0011] Unless otherwise defined, all technical and scientific terms used herein are defined by the principles of the present invention. The terms "materials, methods and experiments" have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure pertains. All examples are illustrative only and are not to be construed as limiting. Many details regarding materials and processing are conventional, and the composites, bearings and seals These techniques may be found in textbooks and other sources within the art.

[0012] The following disclosure relates to a polyimide matrix having a material such as a thermoplastic filled therein: A composite and specifically a composite bearing is described, comprising a polyimide precursor or The method comprises depositing a mixture containing an imide monomer on a substrate and imidizing the mixture on the substrate, thereby forming a composite. A method is also described. Thus, the polyimide matrix with the plastic material is imidized and formed in situ. The idea has never been disclosed or suggested in any way. Understanding will be facilitated with reference to illustrative, non-limiting embodiments.

[0013] FIG. 1 illustrates a composite 100 that includes a substrate 20 and a first layer 30 disposed on the substrate 20. As illustrated, the first layer 30 is adjacent to the substrate 20 so as to be in direct contact with the substrate 20. However, as discussed further below, the composite may be applied directly to the substrate and the first The present invention may include an intermediate layer(s) disposed between the first layer 30 and the second layer 30.

[0014] The substrate 20 may be constructed from any material that can be formed into a bearing or seal. In certain embodiments, the substrate is made of a material such as steel, aluminum, bronze, copper, and combinations thereof. The metal may include

[0015] The surface 22 of the substrate 20 adjacent the first layer 30 is mechanically treated to bond the substrate and the first layer 30 together. For example, mechanically treating the surface 22 of the substrate 20 may include: This may include blasting or mechanically etching the surface 22 of the substrate 20. Surface 22 of 20 may be mechanically treated to have an effective surface roughness.

[0016] Referring again to FIG. 1, adjacent to the substrate 20 may be a first layer 30. The first layer 30 may be formed from a combination of materials. In a specific embodiment, the first layer 30 is It may include a polyimide matrix and a filler dispersed in the polyimide matrix.

[0017] As used herein, a "polyimide matrix" refers to a crosslinked network of polyimides. The polyimide is at least about 25% by weight of the first layer 30 based on the total weight of the first layer. Weight percentages.

[0018] As will be discussed in more detail below, the polyimide matrix is ​​based on a polyimide precursor. The polyimide precursor can be formed by depositing it on a material and imidizing it. For example, poly(amide) acid (PAA) can be mentioned. Poly(amide) acid (PAA) is a It may be the reaction product of a monomer mixture containing at least two different monomers. In an embodiment, the at least two different monomers are: pyromellitic dianhydride (PMDA ), 3,3'-4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2- Bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 2,2'-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'- Oxydianiline (ODA) or m-phenylenediamine (m-PDA), 4,4'-di Aminophenylsulfone (4,4'-DDS), p-phenylenediamine (p-PDA) and methylenedianiline (MDA). In the form, the polyimide matrix is ​​made of at least two different types of polyimide listed above. It may be a reaction product of crosslinking monomers. In a specific embodiment, a polyimide matrix The matrix may be a pure polyimide matrix. The phrase "polyimide copolymers" refers to polyimide copolymers that are essentially free of copolymers having imide monomers. That is, in certain embodiments, the polyimide matrix can be , may be essentially free of non-imide monomers.

[0019] Further, in certain embodiments, the polyamic acid is a copolymer of a first monomer and a second monomer. The first monomer can be derived from pyromellitic dianhydride (PMDA), 3,3'-4, 4'-Biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3,4-diphenyltetracarboxylic dianhydride) 2,2'-bis[4 -(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), benzophenone tetracarboxylic dianhydride (BTDA) and any combination thereof The second monomer may be selected from the group consisting of 4,4'-oxydianiline (ODA) or m-Phenylenediamine (m-PDA), 4,4'-diaminophenylsulfone (4, 4'-DDS), p-phenylenediamine (p-PDA), methylenedianiline (MDA ) and any combination thereof.

[0020] In a specific embodiment, the polyimide matrix may be derived from a polyamic acid salt. For example, polyamic acid is dissolved in a solvent such as N-methylpyrrolidone and reacted with a tertiary amine, for example. The polyamic acid salt solution can then be filled in the reaction vessel. Since the polyamic acid salt solution is water-miscible, the polyimide This can produce a more uniform dispersion of the filler in the trick. Then, as imide bonds are formed during curing, the salt moieties of the polyamic acid salt volatilize. The sexual material appears in the first layer.

[0021] As mentioned above, the first layer 30 may also include a filler dispersed in the polyimide matrix. Fillers include, but are not limited to, carbon graphite, grapheme , carbon nanotubes, econoline, glass fibers, and thermoplastics. The compounds may include organic compounds, inorganic compounds, or combinations thereof.

[0022] In certain embodiments, the filler may be a thermoplastic material. The polymeric material may be a fluoropolymer, such as a perfluoropolymer. In an embodiment, the thermoplastic material is PTFE, PVF, PVDF, PCTFE, PFA, FEP , ETFE, or a combination thereof. In a more specific embodiment, the thermoplastic The material may include PTFE or may consist essentially of PTFE. Such thermoplastics may be regrind thermoplastics.

[0023] In another particular embodiment, the filler can be an organic filler. For example, in a particular embodiment, The organic fillers are aromatic polyester, recycled polyimide, polyamide ether imide , polyamide-imide, PEEK, PEEK-like polymers of the polyaryl family, liquid crystal polymers The polymer may include a polybenzimidazole (LCP), a polybenzimidazole, or a combination thereof.

[0024] The filler is 0% by weight based on the combined weight of the thermoplastic material, polyimide precursor, and filler. The filler may be present in the mixture in an amount of from greater than 80% by weight. The agent is at least 1% by weight, at least 3% by weight, at least 5% by weight, at least 7% by weight, at least 8% by weight, at least 10% by weight, at least 12% by weight, at least 14% by weight, at least 16% by weight, at least 18% by weight, at least 20% by weight, at least 22% by weight %, at least 24%, at least 26%, at least 28%, or less by weight. In particular embodiments, the filler may be present in the mixture in an amount of up to 30% by weight. The filler is 80% by weight based on the combined weight of the thermoplastic material, polyimide precursor, and filler. % or less, 78% by weight or less, 76% by weight or less, 74% by weight or less, 72% by weight or less, 70% by weight % or less, 68% by weight or less, 66% by weight or less, 64% by weight or less, 62% by weight or less, or 60 % or even less by weight. Further, in specific embodiments, the filler is 1 to 80% by weight based on the combined weight of the thermoplastic material, the polyimide precursor, and the filler. %, or even within 10-70% by weight of any of the above minimum and maximum ranges. may be present in the mixture.

[0025] It is to be understood that the mixture may include any combination of the above fillers. In embodiments, the mixture may include a thermoplastic filler and an organic filler.

[0026] The first layer 30 may include any desired additives. For example, some additives may be The additives may include thickening agents or stabilizers. For example, the stabilizer may be a perfluoroalcohol. Examples of thickening agents include surfactants such as alkoxy compounds, thickeners, etc. Additives may include glycols and glycols or combinations thereof. The active ingredient may be added in any amount desired to produce the desired effect.

[0027] In a specific embodiment, the first layer 30 is about 1 mm or less, about 800 microns or less, about 5 00 microns or less, about 300 microns or less, about 250 microns or less, about 200 microns or less or even less than about 175 microns. The first layer 30 may be at least about 0.01 microns, at least about 1 micron, at least about The first layer 30 may have a thickness of 50 microns or even at least about 100 microns. It should be understood that the first layer 30 may include one or more layers. may include two or more layers formed through multiple coating operations.

[0028] The first layer 30 may have a particular porosity. For example, in certain embodiments, the first layer 30 is at least about 0.01%, at least about 0.05% microns or at least about 0.1 % porosity.

[0029] In certain embodiments, as specifically illustrated in FIG. 2, one or more additional intermediate layers 4 0 may be applied between the substrate 20 and the first layer 30. The intermediate layer 40 may be, for example, a 0 and the substrate 20. As will be appreciated by those skilled in the art, The specific selection of layer 40 may vary depending on the composition of substrate 20 and first layer 30. In some embodiments, the intermediate layer 40 may include zinc or a zinc-containing compound. Alternatively to or in lieu of the mechanical treatment of the surface 22 of the substrate 20 described above, It may be provided in addition to the treatment.

[0030] The specific effects of the present invention are the average friction coefficient, the average abrasion resistance, and the laminator adhesion test. The achievement of certain performance characteristics, such as the ability to pass the Erichsen The manner in which the above-mentioned performance characteristics, and in particular combinations of the above-mentioned performance characteristics, are achieved is known. It has not been done.

[0031] One characteristic that quantifies the performance of a bearing can be its average coefficient of friction (COF) Average Coefficient of Friction (COF) is an industry standard term measured according to ASTM G-77 It can be done.

[0032] In certain embodiments, bearings according to the present disclosure have a tensile strength measured in accordance with ASTM G-77. , about 1 or less, about 0.8 or less, about 0.7 or less, about 0.6 or less, about 0.5 or less, about 0. 4 or less, about 0.3 or less, about 0.25 or less, about 0.2 or less, about 0.18 or less, about 0.15 or less or even about 0.12 or less. In one embodiment, a bearing according to the present disclosure has a rolling resistance of about 0.05 mm, as measured according to ASTM G-77. An average coefficient of friction (COF) of .001 or greater, about 0.01 or greater, or even about 0.05 or greater Moreover, in a specific embodiment, a bearing according to the present disclosure may have a 0.001 Within any of the minimum and maximum ranges above, such as ~1 or even a range of 0.01 to 0.7 It may have an average coefficient of friction.

[0033] Another characteristic by which the performance of a bearing can be quantified is its average wear resistance. of material removed from bearings during wear testing conducted in accordance with ASTM G-77 It is a measurement of quantity.

[0034] In certain embodiments, bearings according to the present disclosure have a tensile strength measured in accordance with ASTM G-77. Approximately 10 mm 3 Below, approximately 8mm 3 Below, 5mm 3 Below, approximately 4mm 3 Below, approximately 3mm 3 Below, approximately 2.9mm 3 Below, approximately 2mm 3 Below, approximately 1.5mm 3 Below, approximately 1.3mm 3 Below Bottom, approx. 1.1mm 3 Below, approximately 1mm 3 Below, approximately 0.8mm 3 Below, approximately 0.6mm 3 below, Approximately 0.5mm 3 Below, approximately 0.3mm 3 Less than or equal to 0.2 mm 3 Average wear resistance of even less than Additionally, in certain embodiments, bearings according to the present disclosure may have an ASTM G Measured according to -77, approximately 0.001mm 3 Above 0.01mm 3 More than or about 0.05mm 3 In particular embodiments, the abrasion resistance of the sintered body may be greater than or equal to 100%. Bearings according to the present disclosure have a diameter of 0.001 mm 3 ~10mm 3 or 0.01 mm 3 ~4m m 3 The wear resistance is within the range of any of the minimum and maximum values ​​above, such as even obtain.

[0035] The third characteristic that can quantify the performance of a bearing is the laminator adhesion test (Erich sen) is the ability of the bearing to pass the laminator adhesion test. This is a measure of the adhesion of a first layer to a second layer in a tubular membrane, and is well known in the art. It is being done.

[0036] In certain embodiments, bearings according to the present disclosure are tested using a laminator adhesion test (Eric hsen) can be passed through.

[0037] According to another aspect of the present disclosure, a method of forming a composite sheet and forming a composite bearing is described. In one embodiment, the method includes: Preparing; Preparing the filler; Preparing the solvent; Filler, solvent and polyimide mixing the imide precursor or imide monomer to form a mixture; depositing the mixture on a substrate; and heat curing the substrate and the applied mixture. To form, the method further includes forming a composite bearing from the composite sheet. That's fine too.

[0038] In certain embodiments, the formation of the complex may be a continuous process. For example, imide The polymerization is carried out by mixing a polyimide precursor or a mixture of monomer and filler and applying it to the substrate, followed by The imidization may be performed in situ, such as by in situ imidization after deposition on a substrate.

[0039] The method can produce bearings having the above-mentioned coefficients of friction and wear resistance. In an exemplary embodiment, the method includes providing a coefficient of friction of less than about 1 and a friction coefficient of less than about 2.9 mm 3 Wear resistance less than A bearing having the following structure may be formed.

[0040] The polyimide precursor may include uncrosslinked polyimide or imide monomers. The polyimide precursor may include a poly(amide) acid. The poly(amide) acid may include at least two In a specific embodiment, the polymer may be derived from the reaction of at least two different monomers. The monomers are: pyromellitic dianhydride (PMDA), 3,3'-4,4'-biphenyl Bis(2,2-dicarboxyphenyl)tetraanhydride (BPDA), 2,2'-bis[4-(3,4-difluoropropane dianhydride (6FDA)] Carboxyphenoxy)phenyl]propane dianhydride (BPADA), benzophenone tetrahydrate Tricarboxylic dianhydride (BTDA) and 4,4'-oxydianiline (ODA) or m -phenylenediamine (m-PDA), 4,4'-diaminophenylsulfone (4,4' -DDS), p-phenylenediamine (p-PDA) and methylenedianiline (MDA) is selected from the group consisting of:

[0041] In a more specific embodiment, the first monomer is pyromellitic dianhydride (PMDA ), 3,3'-4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2- Bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 2,2'-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), benzophenonetetracarboxylic dianhydride (BTDA) and the second monomer may comprise a monomer selected from the group consisting of 4,4 '-Oxydianiline (ODA) or m-Phenylenediamine (m-PDA), 4,4' -Diaminophenylsulfone (4,4'-DDS), p-phenylenediamine (p-PD A), methylenedianiline (MDA), and any combination thereof. The monomer may include a monomer that is

[0042] In specific embodiments, the poly(amide) acid may be in the form of a salt, as detailed above. Thus, in a specific embodiment, the method includes providing a poly(amic acid salt); For example, in certain embodiments, the polyamic acid may be dissolved in water. can be combined in a solvent and reacted, for example, with a tertiary amine, to form a water-soluble polyamic acid salt mixture. The aqueous dispersion containing the filler can then be added to the polyamic acid salt mixture, Since the compound is water soluble, the filler disperses uniformly in the polyamic acid salt and converts to imide during curing. The homogeneous dispersion can be maintained after the polymerization.

[0043] In a specific embodiment, the polyimide precursor is a combination of a thermoplastic and a polyimide precursor. The mixture may be present in an amount of 20 to 99% by weight based on the combined weight of the particular In an embodiment, the polyimide precursor is a thermoplastic material and a polyimide precursor. At least 20% by weight, at least 22% by weight, at least 24% by weight, At least 26% by weight, at least 28% by weight, at least 30% by weight, at least 32% by weight , at least 34% by weight, at least 36% by weight, at least 38% by weight, at least 4 0% by weight of the polyimide precursor. is 99% by weight or less, 97% by weight or less based on the combined weight of the filler and the polyimide precursor Below, 95% by weight or less, 93% by weight or less, 91% by weight or less, 99% by weight or less, 99% by weight Hereinafter, it may be present in the mixture in an amount up to 99% by weight, up to 99% by weight, up to 99% by weight.

[0044] As described above, the method includes providing a filler, incorporating the filler in a mixture, imidizing and The method may include retaining the polyimide within the polyimide matrix during curing.

[0045] As noted above, the filler can be a number of different materials, and in a specific embodiment, is a thermoplastic The thermal expansion coefficient may include, for example, 0.1 to 0.5, and may include, for example, 0.1 to 0.5. When using a combination of fillers, such as plastic fillers and / or organic fillers, they should be combined with other ingredients. The fillers may be combined together prior to combining.

[0046] In a specific embodiment, the filler may be in particulate form prior to being mixed into the solvent. In such embodiments, the filler, particularly a thermoplastic filler, and even more particularly PTFE At least about 1 micron, at least about 3 microns, at least about 5 microns, At least about 10 microns, at least about 15 microns, or even at least about 20 microns. Average particle size (D 50 In addition, in certain embodiments, the filler may have about 1000 microns or less, about 500 microns or less, about 50 microns or less, about 30 microns or less, about 2 0 microns or even about 10 microns or less average particle size (D 50 ). The filler may be about 1 micron to 50 microns, about 3 microns to about 30 microns, or about 5 Within the range between any of the maximum and minimum values ​​above, such as from about 20 microns to about 30 microns The average particle size (D 50 ).

[0047] Additionally, the filler may be premixed prior to being combined with the polyimide precursor or imide monomer, e.g. It may be in powder form, or in other embodiments, it may be a dispersed phase in a solvent, such as water. In some embodiments, the mixture may be formed with both powdered filler and filler dispersed in a solvent. do.

[0048] In certain embodiments, the filler, such as a thermoplastic filler, is a filler and a polyimide precursor. may be present in the mixture in an amount of from greater than 0% to 80% by weight based on the combined weight of In a specific embodiment, the filler is, based on the combined weight of the filler and the polyimide precursor, At least 1% by weight, at least 3% by weight, at least 5% by weight, at least 7% by weight %, at least 8% by weight, at least 10% by weight, at least 12% by weight, at least 1 4% by weight, at least 16% by weight, at least 18% by weight, at least 20% by weight, at least 22% by weight, at least 24% by weight, at least 26% by weight, at least 28% by weight % or even at least 30% by weight of the mixture. In the form, the filler is 80% by weight based on the combined weight of the filler and the polyimide precursor. 78% by weight or less, 76% by weight or less, 74% by weight or less, 72% by weight or less, 70% by weight 68% by weight or less, 66% by weight or less, 64% by weight or less, 62% by weight or less, or 60% by weight or less % or even less than 50% by weight of the filler. and the polyimide precursor, Any of the above minimum and maximum ranges may be present in the mixture, such as within the ranges.

[0049] In certain embodiments, the solvent is mixed with the filler, polyimide precursor, or imide monomer. The fillers and polyimide precursors may be added separately to these components. The solvent may be added after the combination of the copolymer or imide monomer. The filler may be mixed with the solvent prior to mixing with the imide precursor or imide monomer. may be added to the mixture. In a specific embodiment, the solvent is N-methyl-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, diglyme, dimethylsulfate The polyvinyl chloride may include dimethyl ether, diphenyl ether, ...

[0050] In specific embodiments, the solvent may include an aqueous component. may contain at least water and NMP.

[0051] As described above, the method includes the steps of: The method may include mixing an optional solvent to form a mixture.

[0052] In certain embodiments, the components are mixed for at least about 1 minute, at least about 5 minutes, or at least Mixing may be carried out for as long as about 15 minutes.

[0053] As described above, the method can include depositing the mixture on a substrate. It can be any material, specifically, steel, aluminum, bronze, copper and the like. It may be a metal such as a combination.

[0054] The mixture can be applied to a substrate in any suitable manner. For example, in specific embodiments, The mixture can be applied by dip coating, spray coating, knife coating or It may be deposited on the substrate by any other useful method. The composition may be deposited on the substrate by dip coating. The first layer 30 may be formed through two or more coating operations. It is understood that the mixture may include layers, and the mixture may be heat cured between the layers.

[0055] A particular advantage of certain embodiments of the present invention is that instead of, for example, skiving or extrusion processes, The first layer 30 can be formed by a coating operation. Conventional sliding layers formed from such materials cannot achieve the performance characteristics described herein. By using a coating operation, the filler material, such as a thermoplastic material, is dispersed in the form of a filler. Unlike extraction or skiving operations that affect the .

[0056] The mixture can be applied so that the first layer 30 has a desired thickness. For example, The thickness of layer 30 can be any of the thicknesses described above. The method includes adjusting the viscosity of the mixture to produce a desired thickness of the mixture when coated onto a substrate. For example, in some embodiments, the viscosity of the mixture can be determined by mixing the components By varying the percentage of and / or adding a viscosity modifier, can be adjusted as desired.

[0057] After deposition of the first layer, the method includes depositing a polyimide precursor or imide monomer, a thermoplastic The method may further include thermally curing the deposited mixture of the agent and the solvent. While being removed, the formation of polyimide (if an imide monomer is used) and polyimide pre- In certain embodiments, the heat curing includes a step heat curing process. For example, a staged heat cure may include multiple stages lasting between about 10 minutes and 6 hours. The stage has a temperature increase between the subsequent stages of between about 10° C. and 50° C. In an embodiment, the temperature during any and / or all steps is from about 80° C. to about 450° C. or higher. It can be between the following.

[0058] Heat curing can be performed to provide the first layer 30 with a desired porosity. The curing may be carried out such that the porosity of the first layer 30 is at least about 0.1%.

[0059] In certain embodiments, the method includes applying an intermediate layer 40 between the substrate and the first layer 30. For example, the intermediate layer 40 may further include a step of improving adhesion between the first layer 30 and the substrate. As will be appreciated by those skilled in the art, the particular selection of intermediate layer 40 will depend on the underlying The material and composition of the first layer 30 can vary. In a specific embodiment, the intermediate layer 40 is zinc or may include a zinc-containing compound.

[0060] In certain embodiments, the method further comprises the steps of: Such an embodiment may include mechanically treating the surface of the substrate adjacent to layer 30. In the present embodiment, the substrate may be directly contacted with the first layer 30. Mechanically treating the surface of the substrate may include: For example, this may involve blasting or mechanically etching the surface of the substrate. In particular, the specific advantages of certain embodiments of the present invention are as described herein, specifically Excellent adhesion between the substrate, which may be a metal substrate such as steel, and the first layer. For example, Adhesion was thought to be difficult due to differences in thermal expansion of the layers and the substrate. Without wishing to be limiting, the inventors carefully adjusted the curing conditions to achieve in situ and continuous The continuous composite formation process produces a composite with excellent adhesion between the substrate and the first layer. was created.

[0061] In certain embodiments, the method includes providing a catalyst and mixing the catalyst with other components in a mixture. In a specific embodiment, the catalyst is first combined with the thermoplastic material. The catalyst may be an isomer of polyamic acid. It can promote midification.

[0062] In a specific embodiment, the catalyst is, for example, 1,4-diazabicyclo[2.2.2 ]octane (DABCO); 4.0]undec-7-ene (DBU); nitrogenous bases; phenols; or amphoteric materials. It can be said.

[0063] The method can include providing and mixing a desired additive into the mixture. For example, some additives may include thickeners or stabilizers.

[0064] In a particular embodiment, and with particular reference to FIG. 18, a polyimide layer is formed and is separate from the substrate. The laminate may be cured and then laminated onto a substrate with a lamination adhesive. For example, as illustrated in FIG. The composite precursor 100 includes a first substrate 105, such as a release layer, and a first substrate 105. 19, the cured polyimide-based layer 110 may be disposed adjacent to the The composite precursor 101 includes an adhesion layer 120 disposed adjacent to a polyimide-based layer 100. Then, a second substrate 130, such as a metal substrate, more specifically a steel substrate, is attached to the adhesive layer. 120. A polyimide-based layer 110 is then deposited adjacent to the composite 10 shown in FIG. The release layer may be removed from the composite to form an outer major surface of 0.

[0065] In a specific embodiment, the release layer can be a film, such as a Kapton film. The delamination may be treated, such as by ionization with UV light.

[0066] The polyimide precursor solution is then applied, for example, by spray coating or dip coating. , knife coating, roll coating or a combination thereof. can be applied to.

[0067] The coated release layer is then cured to form the polyimide precursor and filler mixture. It can be made into a digital format.

[0068] An adhesive layer may then be applied to the exposed polyimide layer or substrate, and the cured coated A release layer may be laminated to the substrate. Adhesive layers include, for example, modified ETFE films and epoxy resins. or combinations thereof.

[0069] In a specific embodiment, the adhesive layer is a film, such as a modified ETFE film. The laminate may be laminated and bonded into a composite by a lamination method such as heat and pressure.

[0070] A particular advantage of certain embodiments of the present invention is the formation of polyimide layers that are essentially crack-free. For example, some processes for forming composite bearings The process involves depositing the uncured solution directly onto the substrate and curing it on the substrate. The coefficient of thermal expansion of the adhesive is significantly different from that of typical metal substrates, making it difficult to apply directly to the substrate. During curing, the polyimide layer shrinks and cracks. In contrast, The polyimide is formed and cured on a release liner to produce a composite material, which is then laminated to a metal substrate. By producing a composite material by applying This produces a composite that is essentially free of delamination.

[0071] To form a composite bearing from the composite sheet material, the sheet material is at least partially The laminate may be cut and turned separately to form an inner layer (substrate) and an outer layer (first layer 30).

[0072] The present disclosure departs from the prior art, in particular by virtue of the performance characteristics described herein, and Specifically, forming a composite bearing that provides the combination of performance characteristics described herein. For example, the present disclosure relates to a method for producing a crosslinked polyimide matrix and , specific fillers, such as thermoplastic or organic fillers, dispersed in the polyimide matrix. Illustrated are various bearings, seals, etc., having the same adhesive material. Such structures provide unexpected and significantly superior coefficient of friction values ​​and wear resistance values ​​that were previously unattainable. It was found to show the wear rate.

[0073] These and other unexpected and superior features are illustrated in the following examples, which are exemplary of the present invention. and is not limited in any way to the embodiments described herein. EXAMPLES

[0074] Example 1 A 2-liter flask equipped with a mechanical stirrer, thermocouple, Dean-Stark adapter, and reflux condenser was used. Into a 1000 cc reactor was added the filler F4PN40 and xylene (425 g). The mixture was stirred at 60°C and 150 rpm to obtain a dispersion in which PTFE was uniformly dispersed in the xylene solvent. Then, oxydianiline (ODA, 70 g, 0.350 mol) and N-methyl NMP (433 g) was added. The solution mixture was stirred (150 rpm). Heat to 160 °C under nitrogen gas and dissolve the residual water in a Dean-Star azeotrope with xylene. The mixture was cooled to 60°C and pyromelodipine was removed using a capillary adapter. PMDA (76.9 g, 0.353 mol) was added to the ODA / PMDA ratio. The mixture was added until the ratio of the two was 1.0000:1.0085. The mixture was heated to about 89°C, and the viscosity increased considerably. The increase in temperature resulted in the formation of poly(amic acid) The exothermic nature of the product is noted. The reaction mixture is stirred and heated at 70°C for 2 hours, and the stirring is continued for 6 hours. The rpm was then slowed to 0 and the solution was allowed to cool to room temperature. Thus, a 15% solution of poly(amic acid) was obtained. The solution was stored in a clean, pre-dried glass bottle.

[0075] The poly(amic acid) solution was heated to 60° C. and stirred at 12 rpm. The coated substrate was heated at 70°C for 1 hour. 100℃ for 1 hour, 120℃ for 1 hour, 140℃ for 1 hour, 160℃ for about 30 minutes, and 2 Heat cure in a vacuum oven under nitrogen flow at 50°C overnight. The composite sheet is then left for approximately 6 hours. Allow to cool gradually and remove from oven.

[0076] Three samples were prepared and tested for friction coefficient and wear rate. Sample 1 was 30% by weight The coating was formed as described above with a PTFE loading of about 175 microns. Sample 2 has a PTFE loading of 50% by weight and a coating thickness of approximately 70 microns. The rest of the sample was formed in the same manner as sample 1. Sample 3 had a coating thickness of about 285 microns. It was formed similarly to sample 2, except that: Comparison samples 4–6 obtained from the ation were also prepared and tested.

[0077] Each sample was tested for wear rate and coefficient of friction according to ASTM G-77. A schematic diagram of the method is illustrated in Figure 3. During the test, the sliding wear of the plastic material was determined. To achieve this, a block-on-ring configuration was used. The stationary test block was rotated from the axis of rotation of the ring. The block and ring were pressed against the test rotating ring at a 90 degree angle with a constant force. Friction between the sliding surfaces of the two specimens results in the removal of material from both specimens. The temperature of each sample is calculated using the decrease in the volume of the block and the decrease in the weight of the ring. The temperature was measured and showed the increase in temperature during the test. The results of the test are shown below and in Figures 4 to 9. Figure 4 shows FIG. 5 illustrates the wear and temperature records as a function of time for sample 1; FIG. 6 illustrates the friction coefficient as a function of time for Sample 1. FIG. FIG. 7 illustrates the wear and temperature records as a function of time for sample 2; FIG. 8 illustrates the coefficient of friction as a function of time for sample 3. FIG. 9 illustrates the wear and temperature records obtained by the present invention; FIG. 10 illustrates the friction coefficient as a function of time for sample 3. Illustrate the recording of numbers.

[0078] Samples 1 to 3 were also observed under a microscope and their microstructures were evaluated using a SEM. The results are shown in Figure 1. 10 and 11 illustrate SEMs of sample 1; Figures 14 and 15 illustrate SEMs of Sample 2 and Sample 3. The images illustrate the non-homogeneous distribution of the PTFE filler in all three samples.

[0079] [Table 1]

[0080] As shown in the results in Table 1, samples 1 to 3 exhibited the following characteristics in terms of the combination of wear volume and friction coefficient: The wear volume and wear rate shown in Samples 1 to 3 were significantly improved. It has not been previously known how to make a bearing having such a good combination of friction coefficients.

[0081] Example 2 - Polyamic acid salt Three samples were prepared and tested for friction coefficient and wear rate under dry and lubricated conditions. No. 10001 available from Gobain Performance Plastics The three samples according to certain embodiments of the present disclosure were compared to the rglide material: It was prepared as follows:

[0082] ODA was dissolved in a mixture of NMP and xylene. With stirring, an equal molar amount of PMD A was added to the ODA solution at 60°C, and after 2 hours, a polyamic acid solution was obtained. Triethylamine was slowly added to the polyamic acid solution to obtain a homogeneous viscous polyamic acid salt. A quantity of the PTFE suspension was mixed with the polyamic acid salt solution to form a substrate. Successful.

[0083] The coefficient of friction (COF) test was performed on a print tester, which is a ball-on-flat sliding test. Also known as dynamic testing. The tests were performed under two different conditions: lubricated and dry. In the lubricated test, the samples are in an oil bath at room temperature throughout the test. The coating is supported without any lubrication other than that provided by the coating itself. Three samples according to certain embodiments of the present disclosure have the following characteristics: Distinguished by:

[0084] 25% PTFE and approximately 50 micron coating thickness, prepared with the following composition:

[0085] [Table 2]

[0086] 35% PTFE and coating thickness of approximately 90 microns, prepared with the following composition:

[0087] [Table 3]

[0088] 45% PTFE and a coating thickness of approximately 130 microns, prepared with the following composition:

[0089] [Table 4]

[0090] The vibration frequency of the ball is 0.11Hz, the distance traveled in a given period is 3cm (round trip), The load was 25N and the test time was 5 minutes. The pressure applied to the coating during the test The force should be 53 MPa, which is the same as the situation listed in test 1. The area of ​​contact between the ring and the ball is 5.10-5 m 2 Therefore, the pressure (load of 25N at ) was close to 50 MPa.

[0091] In lubrication testing, all PTFE / PI samples exhibited approximately the same properties as shown in Table 8 below. All PTFE / PI samples had a lower COF than Norglide. stomach.

[0092] Table 8. Results of print tests under lubricated conditions

[0093] [Table 8]

[0094] In the dry test, the COF values ​​showed more differences, indicating that the PTFE in the coating The results show that the PTFE / PI samples are all N Better than orglide material.

[0095] Table 9: Results of print tests under dry conditions

[0096] [Table 9]

[0097] Many different aspects and embodiments are possible. Some of these aspects and embodiments are Upon reading this specification, those skilled in the art will recognize these aspects and embodiments as exemplary and It is understood that the above is merely an example and does not limit the scope of the present disclosure. Any one or more of the items may follow.

[0098] Example 3: Lamination Kapton® corona treated 25% PTFE blend described in Example 2 A release film was coated and cured to prepare a sample according to certain embodiments of the present disclosure. The coating had a thickness of about 70-130 um. The composite was then Instead of coating directly onto the steel substrate as in Example 2, zinc was plated onto the In one embodiment, the modified ETFE film was laminated onto a cured steel substrate. The coated layer was then placed in direct contact with the modified ETFE film and cured with the steel substrate. In another embodiment, an epoxy layer was applied between the steel substrate and the cured composite. The bearing samples were then hot pressed to bond the modified ETFE layer or the epoxy layer. The COF was then measured under dry conditions as described above during the print test. The parameters were as follows:

[0099] The ball has a vibration frequency of 5Hz, the distance traveled in a given period is 3cm (round trip), and the load is 8 The pressure applied to the coating during the test was 2N and the test time was 18 minutes. , should be 53 MPa, the same as the conditions listed in Test 1. Coating The area of ​​contact between the ball and the -5 m 2 Therefore, the pressure (load of 82N) ) was close to 53 MPa.

[0100] The results of the drying test of the above two samples are shown in Figure 16. As shown, the same excellent CO F values ​​were obtained for both samples.

[0101] The modified ETFE-containing samples were then sold under the trademark Norglide T by a German company. Norglide® (available from Saint-Gobain Pampus, Germany) glide material and JBT samples. The results are shown in Figure 17. As shown, However, samples according to certain embodiments of the present disclosure outperformed the Norglide samples. It was significantly better and essentially comparable to the JBT sample.

[0102] The above Example 3 is at least a coating on a release film, curing, and then a substrate. By laminating the coating on the steel substrate, shrinkage caused by differences in thermal expansion between the steel substrate and the coating is eliminated. This demonstrates that samples can be prepared without any adverse effects, resulting in a better and more sustainable High bearing capacity can be obtained.

[0103] Item 1. Bearing: a. Substrate; and b. a layer deposited on the substrate, i. a polyimide matrix; and ii. a filler dispersed in said polyimide matrix, wherein the filler is a thermally and said layer comprising a plastic or organic filler.

[0104] Item 2. Bearing: a. Substrate; and b. a layer deposited on said substrate, said layer comprising: i. a polyimide matrix derived from a polyamic acid salt; and ii. a thermoplastic and / or organic filler dispersed in said polyimide matrix; the layer comprising; and the bearing comprising.

[0105] Item 3. Bearing: a. Substrate; and b. a first layer deposited on the substrate, the first layer comprising a polyimide matrix and the polyimide the first layer comprising a filler dispersed in an imide matrix; c. wherein the bearing has a coefficient of friction of less than about 1 and a 3 Wear resistance less than The bearing.

[0106] Item 4. A friction coefficient of less than about 1 and about 2.9 mm 3 Bearings with wear resistance of less than Guh.

[0107] Item 5. The bearing according to any one of items 1 to 3, wherein the substrate comprises a metal.

[0108] Item 6. The metal according to item 4, wherein the metal includes steel, aluminum, bronze or copper. Bearings on board.

[0109] Item 7. The bearing has a friction coefficient of about 1 or less, measured in accordance with ASTM G-77; About 0.8 or less, about 0.7 or less, about 0.6 or less, about 0.5 or less, about 0.4 or less, about 0.3 or less below, about 0.25 or less, about 0.2 or less, about 0.18 or less, about 0.15 or less, or about 0.12 The bearing according to any one of items 1 to 3, having an average coefficient of friction (COF) of less than or equal to the following: ng.

[0110] Item 8. The bearing has a surface roughness of about 0.00, as measured in accordance with ASTM G-77. having an average coefficient of friction (COF) of 1 or greater, about 0.01 or greater, or even about 0.05 or greater; The bearing according to any one of Items 1 to 3.

[0111] Item 9. The bearing has a diameter of about 10 mm, measured in accordance with ASTM G-77. 3 Below, approximately 8mm 3 Below, 5mm 3 Below, approximately 4mm 3 Below, approximately 3mm 3 Below, approximately 2.9m m 3Below, approximately 2mm 3 Below, approximately 1.5mm 3 Below, approximately 1.3mm 3 Below, approximately 1.1mm 3 Below, approximately 1mm 3 Below, approximately 0.8mm 3 Below, approximately 0.6mm 3 Below, approximately 0.5mm 3 below , about 0.3mm 3 Less than or equal to 0.2 mm 3 Items with even less than average wear resistance 4. The bearing according to any one of 1 to 3.

[0112] Item 10. The bearing has a surface roughness of about 0.0 mm, as measured in accordance with ASTM G-77. 01mm 3 Above 0.01mm 3 More than or equal to 0.05 mm 3 Even more wear-resistant 4. The bearing according to any one of items 1 to 3, comprising:

[0113] Item 11. The layer deposited on the substrate is tested by a laminator adhesion test (Erichse n) passing through a bearing according to any one of items 1 to 3.

[0114] Item 12. The layer deposited on the substrate is about 1 mm or less, about 800 microns or less; Approximately 500 microns or less, approximately 300 microns or less, approximately 250 microns or less, approximately 200 microns or less 175 microns or less, or even less than about 175 microns. Bearings on board.

[0115] Item 13. The layer deposited on the substrate is at least about 0.01 microns thick. At least about 1 micron, at least about 50 microns, or even at least about 100 microns. 4. The bearing according to any one of items 1 to 3, having a thickness.

[0116] Item 14. The layer deposited on the substrate comprises at least about 0.01%, at least about Any of items 1 to 3 having a porosity of 0.05% or even at least about 0.1%. Bearings as described above.

[0117] Item 15. The polyimide matrix comprises a crosslinked and imidized polyamic acid. 4. A bearing according to any one of items 1 to 3.

[0118] Item 16. The polyamic acid or polyamic acid salt is pyromellitic dianhydride (P MDA), 3,3'-4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2 ,2-Bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FD A), 2,2'-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane diamine Anhydride (BPADA), Benzophenonetetracarboxylic dianhydride (BTDA) and 4, 4'-oxydianiline (ODA) or m-phenylenediamine (m-PDA), 4,4 '-Diaminophenylsulfone (4,4'-DDS), p-phenylenediamine (pP Two different monoamines selected from the group consisting of methylenedianiline (MDA) and methylenedianiline (MDA) Item 15. A bearing according to item 14, comprising a reaction product of mer.

[0119] Item 17. The polyamic acid or polyamic acid salt is a first monomer different from each other. 15. The bearing of claim 14, comprising the reaction product of a first monomer and a second monomer.

[0120] Item 18. The first monomer is pyromellitic dianhydride (PMDA), 3,3 '-4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3, 4-Dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 2,2'- Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPAD A), benzophenonetetracarboxylic dianhydride (BTDA) and any combination thereof and wherein said second monomer comprises a monomer selected from the group consisting of 4,4'-oxo Dianiline (ODA) or m-phenylenediamine (m-PDA), 4,4'-diamine Nophenylsulfone (4,4'-DDS), p-phenylenediamine (p-PDA), A moiety selected from the group consisting of ethylenedianiline (MDA) and any combination thereof. Item 16. Bearings, including Nomar.

[0121] Item 19. The polyimide matrix is ​​derived from a polyamic acid salt. 19. A bearing according to any one of claims 1 to 18.

[0122] Item 20. The polyimide matrix is ​​an imidization reaction product of a polyamic acid salt. 20. A bearing as described in any one of items 1 to 19.

[0123] Item 21. Any of items 1 to 3, wherein the thermoplastic material comprises a fluoropolymer. Bearings as described above.

[0124] Item 22. The method according to item 18, wherein the thermoplastic material comprises a perfluoropolymer. Bearings.

[0125] Item 23. The bearing according to item 18, wherein the thermoplastic material comprises PTFE. .

[0126] Item 24. The method according to item 20, wherein the thermoplastic material comprises PTFE regrind. Bearings on board.

[0127] Item 25. The thermoplastic material is a composite of a thermoplastic material and a polyimide matrix. Items 1 to 3 are present in the layer in an amount of from greater than 0% to 80% by weight based on the weight of the layer. 2. A bearing as described in any one of claims 1 to 11.

[0128] Item 26. The polyimide matrix is ​​a thermoplastic and a polyimide matrix. The item is present in the layer in an amount of 20 to 100% by weight based on the combined weight of the material and the base. 4. The bearing according to any one of 1 to 3.

[0129] Item 27. The layer deposited on the substrate further comprises an organic filler, items 1 to 3. 2. A bearing as described in any one of claims 1 to 11.

[0130] Item 28. The organic filler comprises a thermoplastic material, a polyimide matrix and an organic filler. The ink is present in the layer in an amount of from greater than 0% to 80% by weight based on the combined weight of the filler. The bearing described in Item 24.

[0131] Item 29. The bearing further comprises an intermediate layer disposed between the substrate and the layer. 4. The bearing according to any one of items 1 to 3,

[0132] Item 30. The method according to item 26, wherein the intermediate layer comprises zinc or a zinc-containing compound. bearing.

[0133] Item 31. A method of forming a composite bearing, comprising: a. providing a polyimide precursor or imide monomer; b. Preparing a thermoplastic material; c. Mixing the thermoplastic material, the polyimide precursor or imide monomer, and a solvent. forming a mixture; d. depositing the mixture onto a substrate; e. heat-curing the substrate and applied mixture, thereby converting the polyimide precursor into an indium ion. and forming a composite sheet.

[0134] Item 32. A method of forming a composite bearing, comprising: a. providing a polyimide precursor or imide monomer; b. Preparing an organic filler; c. Mix the filler, the polyimide precursor or imide monomer, and a solvent. To form a compound; d. depositing the mixture onto a substrate; e. heat-curing the substrate and applied mixture, thereby converting the polyimide precursor into an indium ion. midization to form a composite sheet; f. forming a bearing from said composite sheet.

[0135] Item 33. A method of forming a composite bearing, comprising: a. providing a polyimide precursor or imide monomer; b. Providing an organic filler and / or a thermoplastic; c. The organic filler and / or thermoplastic material, the polyimide precursor or imide monomer and a solvent to form a mixture; d. depositing the mixture onto a substrate; e. heat-curing the substrate and applied mixture, thereby converting the polyimide precursor into an indium ion. midization to form a composite sheet; and f. forming a bearing from the composite sheet; g. the bearing has a coefficient of friction of less than about 1 and a 3 Has abrasion resistance of less than The method.

[0136] Item 34. Any of Items 28 to 30, in which the heat curing includes a step heat curing process. The method according to any one of the preceding claims.

[0137] Item 35. The step heat cure may include multiple steps, each step lasting between about 10 minutes and 6 hours. Each stage has a temperature increase of between about 10°C and 50°C between the next successive stages. Item 32. The method according to item 31.

[0138] Item 36. The solvent is N-methyl-pyrrolidone (NMP), dimethylformamide dimethylacetamide, diglyme, dimethylsulfoxide, xylene or any of these The method according to any one of items 28 to 30, including any combination thereof.

[0139] Item 37. The method according to any one of items 28 to 30, wherein the polyimide precursor comprises a polyamic acid. Any method as described above.

[0140] Item 38. The method according to any one of items 1 to 37, wherein the polyimide precursor comprises a polyamic acid salt. Any method as described above.

[0141] Item 39. The polyamic acid or polyamic acid salt is pyromellitic dianhydride (P MDA), 3,3'-4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2 ,2-Bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FD A), 2,2'-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane diamine Anhydride (BPADA), Benzophenonetetracarboxylic dianhydride (BTDA) and 4, 4'-oxydianiline (ODA) or m-phenylenediamine (m-PDA), 4,4 '-Diaminophenylsulfone (4,4'-DDS), p-phenylenediamine (pP At least two selected from the group consisting of methylenedianiline (MDA) and methylenedianiline (MDA). Item 35. The method according to item 34, which is derived from different monomers.

[0142] Item 40. The polyamic acid or polyamic acid salt is a first monomer different from each other. and a second monomer.

[0143] Item 41. The first monomer is pyromellitic dianhydride (PMDA), 3,3 '-4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3, 4-Dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 2,2'- Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPAD A), benzophenonetetracarboxylic dianhydride (BTDA) and any combination thereof and wherein said second monomer comprises a monomer selected from the group consisting of 4,4'-oxo Dianiline (ODA) or m-phenylenediamine (m-PDA), 4,4'-diamine Nophenylsulfone (4,4'-DDS), p-phenylenediamine (p-PDA), A moiety selected from the group consisting of ethylenedianiline (MDA) and any combination thereof. Item 36. Bearings as described in item 36, including Nomar.

[0144] Item 42. Any of items 28 to 30, wherein the thermoplastic material comprises a fluoropolymer. Any method according to the present invention.

[0145] Item 43. The thermoplastic material of items 28 to 30, wherein the thermoplastic material comprises a perfluoropolymer. 2. The method according to claim 1 ,

[0146] Item 44. Any of Items 28 to 30, wherein the thermoplastic material comprises PTFE. The method described.

[0147] Item 45. The thermoplastic material comprises PTFE regrind material, items 28 to 30. 2. The method according to claim 1 ,

[0148] Item 46. The thermoplastic material has a thickness of at least about 1 micron, at least about 3 microns. lon, at least about 5 microns, at least about 10 microns, at least about 15 microns Or even at least about 20 microns average particle size (D 50 ) and items 28-3 10. The method according to claim 1, wherein

[0149] Item 47. The thermoplastic material has a thickness of about 50 microns or less, about 30 microns or less, about 2 0 microns or even about 10 microns or less average particle size (D 50 ) items 28. A method according to any one of claims 28 to 30.

[0150] Item 48. The thermoplastic material has a thickness of about 1 micron and 50 microns, about 3 microns to 50 microns. Average particle size (D) in the range of about 30 microns or even between about 5 microns and about 20 microns 50 31. The method according to any one of Items 28 to 30, comprising the steps of:

[0151] Item 49. Any of items 28 to 30, wherein the thermoplastic material is in powder form. The method described.

[0152] Item 50. The method according to any one of Items 28 to 30, wherein the thermoplastic material is a dispersed phase. Method of posting.

[0153] Item 51. The thermoplastic material has a particle size of at least 0.05 microns, at least about 0. 28 to 30, having an average particle size of 1 micron or even at least about 2 microns. Any method as described above.

[0154] Item 52. The thermoplastic material has a thickness of about 1000 microns or less, about 500 microns or less or even less than about 100 microns. The method described.

[0155] Item 53. Adjusting the viscosity of the mixture to obtain a desired viscosity of the mixture deposited on the substrate. The method according to any one of items 28 to 30, wherein the thickness is formed.

[0156] Item 54. The thermoplastic material is a polymer of a thermoplastic material and a polyimide precursor. Item 28 to 3, which are present in the mixture in an amount of from more than 0% to 80% by weight, based on the amount of 10. The method according to claim 1, wherein

[0157] Item 55. The polyimide precursor is a combination of a thermoplastic material and a polyimide precursor. Item 2. The method according to claim 1, wherein the amount of the component (I) is from 20% to 100% by weight of the mixture. A method according to any one of 8 to 30.

[0158] Item 56. Providing an organic filler and mixing the organic filler with the thermoplastic material. The method according to any one of Items 28 to 30, further comprising:

[0159] Item 57. The organic filler comprises a thermoplastic material, a polyimide precursor and an organic filler. The item is present in the mixture in an amount of from greater than 0% to 80% by weight based on the combined weight. The method according to claim 52.

[0160] Item 58. The method of any of Items 28 to 30, wherein the substrate comprises a metal.

[0161] Item 59. The metal is steel, aluminum, bronze or copper or a combination thereof. Item 55. The method according to item 54,

[0162] Item 60. Treating the substrate prior to applying the mixture onto the substrate to form a mixture to be applied. 31. The method of claim 28, further comprising improving adhesion between the composition and a substrate. Method of posting.

[0163] Item 61. Chemically treating the surface of the substrate adjacent to the layer prior to applying the mixture onto the substrate. Item 57. The method according to item 56, wherein the processing includes automatically processing the

[0164] Item 62. Chemically treating the surface of the substrate with zinc or a zinc-containing compound. 58. The method according to item 57, comprising coating.

[0165] Item 63. Mechanically treating a surface of the substrate adjacent to the layer prior to applying the mixture onto the substrate. Item 57. The method according to item 56, wherein the processing includes automatically processing the

[0166] Item 64. Mechanically treating the surface of the substrate by sandblasting or mechanically 60. The method of claim 59, comprising etching.

[0167] Item 65. Forming two or more layers containing a polyimide matrix on the substrate. The method according to any one of Items 28 to 30, further comprising:

[0168] Item 66. The method of item 28, further comprising adding a second filler to the mixture. A method according to any one of claims 1 to 30.

[0169] Item 67. The second filler is carbon graphite, graphime, carbon nanotubes , Econol, glass fiber, polymer compounds, inorganic compounds and combinations thereof Item 63. The method according to item 62, selected from the group consisting of

[0170] Item 68. Heat curing is performed such that the composite has a porosity of at least about 0.1%. The method according to any one of items 28 to 30, comprising temperature regulation.

[0171] Item 69. The method of claim 69, further comprising providing a catalyst and mixing the catalyst with the thermoplastic material. The method according to any one of Items 28 to 30.

[0172] Item 70. The method according to item 65, wherein the catalyst promotes imidization of polyamic acid. method.

[0173] Item 71. The method of item 65, wherein the catalyst comprises a strong tertiary aliphatic base.

[0174] Item 72. The catalyst is 1,4-diazabicyclo[2.2.2]octane (DAB Strong tertiary aliphatic bases such as 1,8-diazabicyclo[5.4.0]undeca- 7-ene (DBU); nitrogenous base; phenol; or amphoteric material, see item 65. The method described.

[0175] Item 73. Any of Items 28 to 30, wherein the method is a continuous process. The method described.

[0176] Item 74. The method further includes at least partially cutting the coated substrate. The method according to any one of Items 28 to 30.

[0177] Item 75. The filler is an aromatic polyester, recycled polyimide, polyamide ethylene Thermoimides, polyamideimides, PEEK, PEEK-like polysulfides from the polyaryl family may include a polymer, a liquid crystal polymer (LCP), a polybenzimidazole, or a combination thereof. 75. A bearing or method according to any one of items 1 to 74.

[0178] Item 76. The organic filler is selected from the group consisting of aromatic polyester, recycled polyimide, polyamide. Doetherimide, polyamideimide, PEEK, PEEK-like from the polyaryl family Polymers, liquid crystal polymers (LCPs), polybenzimidazoles, or combinations thereof 76. A bearing or method according to any one of items 1 to 75.

[0179] Item 77. The substrate is a release film, and the method comprises: and hardening the resulting mixture on a steel substrate to form a composite. 2. The method according to claim 1 ,

[0180] Item 78. The method further comprises forming the composite with a second substrate, the hardened mixture being then forming an outer surface of the bearing. Item 77. The method according to item 77.

[0181] Item 79. The method of item 78, wherein the second substrate is a metal substrate.

[0182] Item 80. The method of item 79, wherein the second substrate comprises steel.

[0183] Item 81. The surface of the release film is treated prior to application of the mixture. The method according to any one of 1 to 80.

[0184] Item 82. The second substrate is a zinc-coated steel substrate. The method according to any one of items 1 to 81.

[0185] Not all of the activities or examples described above in the general description are required, and specific activities may not be required. may not be necessary and may benefit from one or more activities in addition to those listed above. Additionally, the order in which the activities are listed does not necessarily represent the order in which they should be performed.

[0186] The benefits, other advantages, and solutions to problems have been described above with reference to specific embodiments. The benefits, solutions to problems, and any other benefits, benefits or solutions that produce or make more clear Any feature or features may be deemed to be important, essential or essential features of any or all of the claims. are not interpreted as

[0187] The description and illustrations of the embodiments set forth herein are provided to provide a general understanding of the structure of the various embodiments. The description and examples are intended to provide an understanding of the present invention and are not intended to limit the scope of the invention. It is not intended to serve as an exhaustive or comprehensive description of all of the elements and features of the system. Separate embodiments may also be provided in combination in a single embodiment and conversely, for clarity, For the purposes of this disclosure, various features that are described in the context of a single embodiment may also be provided separately or in any subcombination. Further, when reference is made to values ​​stated in ranges, each and every value within that range is also included. Many other embodiments may become apparent to those of ordinary skill in the art upon reading this description. Structural, logical substitutions, and other changes may be made without departing from the scope of the present disclosure. As such, other embodiments may be used and derived from this disclosure. Accordingly, this disclosure is not intended to be limiting. It should be viewed as an illustrative example rather than a rigorous examination.

Claims

1. A bearing comprising: a. a substrate; and b. a first layer disposed on the substrate, i. a polyimide matrix; and ii. A filler dispersed in the polyimide matrix, wherein the filler is a thermally the first layer comprising a plastic material or an organic filler.

2. The bearing of claim 1 , wherein the substrate comprises a metal substrate.

3. The bearing of claim 1 , wherein the substrate comprises steel, aluminum, bronze or copper. .

4. The polyimide matrix is ​​a crosslinked and imidized polyamic acid or polyamic acid salt. The bearing of claim 1 , comprising:

5. The crosslinked and imidized polyamic acid or polyamic acid salt is pyromellitic dianhydride. (PMDA), 3,3'-4,4'-biphenyltetracarboxylic dianhydride (BPDA) , 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6 FDA), 2,2'-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane Benzophenone dianhydride (BPADA), Benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydianiline (ODA) or m-phenylenediamine (m-PDA), 4 , 4'-diaminophenylsulfone (4,4'-DDS), p-phenylenediamine (p -PDA) and methylenedianiline (MDA) 5. The bearing of claim 4 comprising a reaction product of monomers.

6. The bearing of claim 1 , wherein the filler comprises a thermoplastic fluoropolymer.

7. The bearing of claim 1 , wherein the filler comprises a thermoplastic perfluoropolymer.

8. The bearing of claim 1 , wherein the filler comprises PTFE.

9. The bearing of claim 1 , wherein the filler comprises an organic filler.

10. The bearing of claim 1 , wherein the filler comprises a thermoplastic filler and an organic filler.

11. The filler has a weight ratio of about 1:1 based on the combined weight of the filler and the polyimide matrix.

2. The bearing of claim 1, wherein the inorganic filler is present in the first layer in an amount of from greater than 0 to 80% by weight. .

12. a. the substrate comprises steel; b. The polyimide matrix is ​​a crosslinked and imidized polyamic acid or polyamide Contains acid salts, 3. The bearing of claim 1, wherein said filler material comprises PTFE.

13. A bearing comprising: a. a metal substrate; and b. A polyimide matrix and a filler dispersed in the polyimide matrix. a first layer comprising: c. wherein said bearing has a coefficient of friction of less than about 1 and a bearing radius of about 2.9 mm 3 Wear resistance less than The bearing.

14. The bearing further includes an adhesion layer disposed between the metal substrate and the first layer. The bearing of claim 13.

15. The bearing further includes a release layer disposed adjacent to the first layer, thereby 15. The method of claim 14, wherein the first layer and the adhesive layer are sandwiched between the release layer and the metal substrate. The bearing described in

Citation Information

Patent Citations

  • Polyimide composition with improved abrasion resistance

    JP1999510835A

  • Composition for slide member

    JP2007031501A

  • Polyimide resin, dry film using the same, metal laminate, and adhesive sheet

    JP2011102349A

  • Self-crosslinking polyamic acid, self-crosslinking polyimide, method of manufacturing self-crosslinking polyimide, and self-crosslinking polyimide film including the self-crosslinking polyimide

    US20100228002A1

  • bearings

    US20110317955A1