Carbon dioxide absorption material, carbon dioxide absorption method, carbon dioxide absorption device, and recycling method of carbon dioxide absorption material
The composite metal oxide Na A Ti B M C O D addresses the inefficiencies of conventional carbon dioxide absorbents by providing high absorption capacity and low-temperature regeneration, improving thermal efficiency and safety in carbon dioxide removal processes.
Patent Information
- Application Number
- JP2023075983
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-15
AI Technical Summary
Conventional carbon dioxide absorbents, such as amine liquids and sodium ferrites, pose safety and handling issues, and require high-temperature regeneration, which is inefficient in terms of thermal energy use.
A composite metal oxide represented by the formula Na A Ti B M C O D, where 5≦A≦11, 4≦B≦6, 0≦C≦2, 10.5≦D≦17.5, and M is any metal, exhibits high carbon dioxide absorption capacity and can be regenerated at low temperatures (400°C or lower) using air, inert gas, or vacuum.
The composite metal oxide achieves equivalent carbon dioxide absorption to sodium ferrite while allowing for efficient regeneration at lower temperatures, enhancing thermal efficiency and enabling recycling with reduced energy consumption.
Smart Images

Figure 2024160738000004 
Figure 2024160738000005 
Figure 2024160738000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon dioxide gas absorbent using a composite metal oxide, a carbon dioxide gas absorbing method, a carbon dioxide gas absorbing device, and a method for regenerating the carbon dioxide gas absorbent. [Background technology]
[0002] In the past, in consideration of social issues such as the reduction of greenhouse gases, the practical application of a technology for recovering carbon dioxide from a gas containing carbon dioxide has been proposed. For example, a carbon dioxide absorption technology using an organic absorbing liquid such as an amine liquid has a high reactivity with gas and has been put to practical use in factories and the like. However, the amine liquid has problems such as toxicity to the human body, and since it is a liquid, it is necessary to fill it in a closed space such as a container, which limits the manner of use. Furthermore, in recent years, there has been a demand for innovative technology that can reduce (beyond zero) the amount of carbon dioxide (carbon dioxide) emitted into the atmosphere in the past, but conventional carbon dioxide absorbents were not able to efficiently absorb carbon dioxide, which is present in low concentrations in the atmosphere.
[0003] Therefore, the present inventors have been working on the development of inorganic absorbents, and have previously proposed a technology relating to a carbon dioxide gas absorbent using α-sodium ferrites (hereinafter, also referred to as Prior Art 1) (Patent Document 1 below). Sodium ferrite is safe and has a high carbon dioxide gas absorption rate, and can be handled as a powder, making it suitable for various usage modes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2016-3156 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in order to reuse α-sodium ferrites that have absorbed carbon dioxide as carbon dioxide absorbents, a regeneration reaction must be carried out by heating at high temperatures of over 400°C, which poses an issue in terms of thermal efficiency.
[0006] The present invention has been made in consideration of the above-mentioned background, and specifically proposes a carbon dioxide absorbent that has a good carbon dioxide absorption rate and enables regeneration of the carbon dioxide absorbent after use at a low temperature of 400°C or less, a carbon dioxide absorption method and carbon dioxide absorption device that use the carbon dioxide absorbent, and a method for regenerating the carbon dioxide absorbent. [Means for solving the problem]
[0007] The first carbon dioxide absorbent of the present invention is characterized by containing a composite metal oxide represented by the following formula (1) (wherein, in formula (1), 5≦A≦11, 4≦B≦6, 0≦C≦2, 10.5≦D≦17.5, and M is any metal). [Formula 1] Na A Ti B M C O D ...(1)
[0008] The second carbon dioxide absorbent of the present invention contains a composite metal oxide containing sodium, titanium, and oxygen, and is characterized in that, in a powder X-ray diffraction pattern using CuKα radiation, the composite metal oxide exhibits peaks at diffraction angles 2θ in the ranges of 12.049°±0.5° and 12.616°±0.5°, and one or two peaks in the range from 39.110°±0.5° to 41.007°±0.5°.
[0009] The carbon dioxide absorption method of the present invention includes a storage step of storing the carbon dioxide absorbent of the present invention in a reaction vessel, a reaction step of introducing a carbon dioxide-containing gas into the reaction vessel and bringing the carbon dioxide-containing gas into contact with the composite metal oxide to cause a reaction, and a discharge step of discharging the gas that has undergone the reaction step from the reaction vessel.
[0010] The carbon dioxide absorption device of the present invention is characterized by comprising a storage section for storing the carbon dioxide absorbent of the present invention, a gas inlet for allowing a carbon dioxide-containing gas to flow into the storage section, and a gas outlet for discharging the gas from the storage section to the outside.
[0011] The method for regenerating a carbon dioxide gas absorbent of the present invention is characterized in that the reaction product, which is the carbon dioxide gas absorbent, after the carbon dioxide gas absorption reaction is heated at a temperature of 400° C. or lower in air, an inert gas or a vacuum. Effect of the Invention
[0012] The carbon dioxide gas absorbent of the present invention exhibits a carbon dioxide gas absorption capacity equal to or greater than that of a carbon dioxide gas absorbent using sodium ferrite, and can be regenerated after carbon dioxide gas absorption at a low temperature of 400° C. or less. Therefore, the carbon dioxide gas absorbent of the present invention can be recycled with good thermal efficiency, and the series of processes from carbon dioxide gas absorption to recycling greatly contributes to environmental issues. The carbon dioxide gas absorbing method and the carbon dioxide gas absorbing device of the present invention also benefit from the effects of the carbon dioxide gas absorbent of the present invention. For example, the carbon dioxide gas absorbing method and the carbon dioxide gas absorbing device of the present invention can absorb carbon dioxide gas in a temperature range from room temperature to a relatively low temperature. Furthermore, the method for regenerating a carbon dioxide gas absorbent of the present invention can regenerate a used carbon dioxide gas absorbent at a lower temperature and has superior thermal efficiency, as compared with conventional carbon dioxide gas absorbents containing sodium ferrite. [Brief description of the drawings]
[0013] [Figure 1] Graph (1A) shows the weight increase rate at room temperature during a carbon dioxide absorption reaction, as determined by thermogravimetry (TG), of one embodiment of the carbon dioxide absorbent of the present invention (Na8Ti5O14) and sodium titanate (Na4Ti5O12), a comparative example having a similar composition but a different composition ratio. Graph (1B) shows the amount of carbon dioxide and moisture absorbed by the reaction shown in (1A). [Diagram 2] This is basic data showing the powder X-ray diffraction pattern of Na8Ti5O14 using CuKα radiation. [Diagram 3] FIG. 1 is a process diagram showing an example of a method for producing Na8Ti5O14. [Figure 4] FIG. 1 is an explanatory diagram showing one embodiment of a carbon dioxide gas absorbing device of the present invention. [Diagram 5] 1 is a chart showing powder X-ray diffraction patterns using CuKα radiation for Examples 1 to 5 before carbon dioxide gas absorption. [Figure 6] 2 is a chart showing powder X-ray diffraction patterns using CuKα radiation for Examples 1 to 5 after carbon dioxide gas absorption. [Figure 7] 1 is a chart showing a powder X-ray diffraction pattern using CuKα radiation of Example 1-1 after regeneration. [Figure 8] 1 is a graph showing the results of simultaneous differential thermal analysis and thermogravimetry (TG-DTA) during the regeneration reaction of Example 1-1 after carbon dioxide gas absorption. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The first carbon dioxide gas absorbent, the second carbon dioxide gas absorbent, the carbon dioxide gas absorption method, the carbon dioxide gas absorption device, and the method for regenerating a used carbon dioxide gas absorbent of the present invention will be described in order below. In the following description, the first carbon dioxide gas absorbent and the second carbon dioxide gas absorbent of the present invention may be collectively referred to as the carbon dioxide gas absorbent of the present invention. The present invention encompasses a carbon dioxide gas absorbent containing a composite metal oxide that has both the characteristics of the composite metal oxide in the first carbon dioxide gas absorbent and the characteristics of the composite metal oxide in the second carbon dioxide gas absorbent. In addition, in the present invention, absorbing carbon dioxide means that the carbon dioxide absorbent absorbs at least a part of the carbon dioxide contained in the gas to be reacted, thereby reducing the concentration of carbon dioxide in the gas after the reaction. In addition, in the present invention, the used carbon dioxide absorbent used in the carbon dioxide absorption reaction may be called the reaction product.
[0015] [The first carbon dioxide absorbent] The first carbon dioxide gas absorbent of the present invention contains a composite metal oxide represented by the following formula (1), where M is any metal, the number of sodium atoms is 5≦A≦11, the number of titanium atoms is 4≦B≦6, the number of atoms of any metal M is 0≦C≦2, and the number of oxygen atoms is 10.5≦D≦17.5. [Formula 2] Na A Ti B M C O D ...(1)
[0016] The composite metal oxide represented by formula (1) was discovered by the present inventors as a sodium titanate with high carbon dioxide absorption capacity. For example, as shown in FIG. 1A, the weight gain rate at room temperature due to a contact reaction with air is 1.0 g / mol / L, which is one of the composite metal oxides of the present invention. 14 However, other complex metal oxides with similar composition but different composition ratios, Na4Ti5O 12 As shown in Figure 1B, the amount of CO2 and H2O absorbed per 1 g of the sample (composite metal oxide) 18 hours after the start of contact with air in the above contact reaction was confirmed. 14 is Na4Ti5O 12 It was confirmed that the composite metal oxide shown in the above formula (1) absorbed a large amount of CO2 compared to the above, and that the ratio of CO2 to the total of absorbed CO2 and H2O exceeded 50%. In other words, the composite metal oxide shown in the above formula (1) has a significantly higher carbon dioxide absorption capacity than other sodium titanates. The carbon dioxide absorption reaction shown in Figure 1 will be described in detail in the Examples below.
[0017] From the viewpoint of providing a composite metal oxide having a higher carbon dioxide gas absorption capacity, the amount A of sodium atoms in the above formula (1) is preferably 6≦A≦10, and more preferably 7≦A≦9. From the same viewpoint, the composition ratios in the above formula (1) are preferably A=8, 4.5≦B≦5.5, 0≦C≦1, and D are values that make the charge in formula (1) ±0, and more preferably A=8, 4.5≦B≦5.0, 0≦C≦0.5, and D are values that make the charge in formula (1) ±0. From the same viewpoint, when C in the above formula (1) is more than 0 and is 1 or less, M is preferably Si, Zr, Mn, Fe, etc., among which Si, Zr, Mn, etc. showing a tetravalent positive charge are more preferable. In formula (1), C=0, Na8Ti5O 14 It is particularly preferred that:
[0018] A preferred example of the first carbon dioxide gas absorbent of the present invention is, for example, Na8Ti5O 14 , Na8Ti 4.75 S 0.25 O 14 , Na8Ti 4.75 Zr 0.25 O 14 , Na8Ti 4.75 Mn 0.25 O 14 , Na8Ti 4.75 Fe 0.25 O 14 A more preferred example is Na8Ti5O 14 , Na8Ti 4.75 S 0.25 O 14 , Na8Ti 4.75 Zr 0.25 O 14 , Na8Ti 4.75 Mn 0.25 O 14 , among which Na8Ti5O 14 is particularly preferred because it exhibits high carbon dioxide gas absorption capacity.
[0019] [Second carbon dioxide absorbent] The second carbon dioxide gas absorbent of the present invention relates to sodium titanate having high carbon dioxide gas absorption capacity like the first carbon dioxide gas absorbent described above. The second carbon dioxide gas absorbent is specified by a large peak appearing in a predetermined range of diffraction angle 2θ in a powder X-ray diffraction pattern using CuKα radiation. That is, the second carbon dioxide absorbent of the present invention contains a composite metal oxide containing sodium, titanium, and oxygen, and in a powder X-ray diffraction pattern using CuKα radiation, the composite metal oxide exhibits peaks in the diffraction angle 2θ ranges of 12.049°±0.5° and 12.616°±0.5°, and one or two peaks in the range from 39.110°±0.5° to 41.007°±0.5°. From the viewpoint of providing a carbon dioxide absorbent with higher carbon dioxide absorption capacity, the second carbon dioxide absorbent of the present invention preferably contains a composite metal oxide which shows peaks in the ranges of diffraction angles 2θ of 12.049°±0.5° and 12.616°±0.5°, and one peak each in the ranges of 39.110°±0.5° and 41.007°±0.5°, in a powder X-ray diffraction pattern using CuKα radiation.
[0020] To explain the second carbon dioxide absorbent, Na8Ti5O 14 The basic data of the powder X-ray diffraction pattern using CuKα radiation is shown in Figure 2. 14 As shown in Fig. 2, the carbon dioxide gas absorbent shows large peaks at diffraction angles 2θ of 12.049°, 12.616°, 39.110° and 41.007°. The second carbon dioxide gas absorbent of the present invention contains a composite metal oxide having a composition in which, in addition to sodium, titanium and oxygen, an arbitrary metal is further substituted for a part of the titanium, and the powder X-ray diffraction pattern of the composite metal oxide using CuKα radiation shows a pattern roughly similar to the four large peaks shown in Fig. 2. Here, roughly similar pattern includes a pattern having a large peak detected at a diffraction angle 2θ of about ±0.5° of the four large peaks shown in Fig. 2 and a pattern showing one or two large peaks in the diffraction angle 2θ range of 39.110°±0.5° to 41.007°±0.5° among the four large peaks in Fig. 2.
[0021] The first carbon dioxide gas absorbent and the second carbon dioxide gas absorbent of the present invention both contain sodium titanate, which is a composite metal oxide that satisfies certain conditions, and are excellent in carbon dioxide gas absorption. The carbon dioxide gas absorbent of the present invention can absorb carbon dioxide gas not only from a gas with a high carbon dioxide gas concentration, but also from a gas with a low carbon dioxide gas concentration. More specifically, the carbon dioxide gas absorbent of the present invention can absorb carbon dioxide gas not only from a gas with a carbon dioxide gas ratio of more than 10% and not more than 100%, but also from a gas with a carbon dioxide gas ratio of 10% or less, and furthermore can absorb carbon dioxide gas well from air with a carbon dioxide gas ratio of about 0.04%. The reason why the carbon dioxide gas absorbent of the present invention has excellent absorption ability for low concentrations of carbon dioxide gas is not clear, but it is presumed that the composite metal oxide contained in the carbon dioxide gas absorbent of the present invention contains a large number of sodium atoms, and as a result, can efficiently absorb carbon dioxide gas even from gases with low carbon dioxide concentrations, such as air.
[0022] Furthermore, the first and second carbon dioxide gas absorbents of the present invention have an advantageous property of being regenerated at a low temperature after the carbon dioxide gas absorption reaction, as compared with conventional carbon dioxide gas absorbents using sodium ferrite. More specifically, for example, at a low temperature of 400°C or less, the carbon dioxide gas absorbent of the present invention after carbon dioxide gas absorption can be desorbed and regenerated to a degree that allows it to be reused as a carbon dioxide gas absorbent. The lower limit of the temperature during regeneration is not particularly limited, but from the viewpoint of rapid regeneration, it is preferably 200°C or more. Therefore, the carbon dioxide gas absorbent of the present invention has good thermal efficiency for recycling. The regeneration of the used composite metal oxide can be confirmed by performing a carbon dioxide gas absorption reaction again using a sample after the regeneration reaction, or by confirming the powder X-ray diffraction pattern using CuKα radiation of the sample after the regeneration reaction and confirming the above-mentioned second feature of the present invention.
[0023] Incidentally, currently, there are established uses for waste heat above the mid-range (over 400°C) generated in factories. On the other hand, there are no established uses for waste heat below the mid-range (below 400°C, or even below 350°C), and proposals for effective uses are being sought. For this reason, using waste heat from exhaust gases and the like discharged from factories as a heat source for the regeneration reaction of the carbon dioxide absorbent of the present invention is desirable from the perspective of energy recycling, and we also propose a new use for waste heat below the mid-range or even lower temperature range from factories.
[0024] Although the reason why the carbon dioxide gas absorbent of the present invention can be regenerated at a lower temperature than conventional carbon dioxide gas absorbents is not clear, the carbon dioxide gas absorbent of the present invention tends to absorb less water together with carbon dioxide gas than sodium ferrite, which is a conventional carbon dioxide gas absorbent. Therefore, when the absorbed carbon dioxide gas is separated from the carbon dioxide gas absorbent, less energy is required to evaporate the water that is generated at the same time, which is presumably one of the reasons why low-temperature regeneration is possible.
[0025] The following further describes common points between the composite metal oxide in the first carbon dioxide gas absorbent and the second carbon dioxide gas absorbent of the present invention. The carbon dioxide gas absorbent of the present invention contains the composite metal oxide in the first carbon dioxide gas absorbent and / or the composite metal oxide in the second carbon dioxide gas absorbent described above, but may further contain any optional component within the scope of the present invention, or the carbon dioxide gas absorbent of the present invention may be substantially composed of only the composite metal oxide described above. In this specification, preferred numerical ranges of the present invention may be shown as appropriate. In this case, preferred ranges, more preferred ranges, and particularly preferred ranges regarding the upper and lower limits of the numerical ranges can be determined from all combinations of the upper and lower limits.
[0026] (Porosity of Complex Metal Oxides) The porosity of the composite metal oxide used in the present invention is not particularly limited, but from the viewpoint of providing a carbon dioxide gas absorbent that has better carbon dioxide gas absorption, the porosity is preferably 39.0% or more, more preferably 39.1% or more, even more preferably 39.2% or more, and even more preferably 39.3% or more. On the other hand, the upper limit of the porosity is preferably 41.5% or less, and more preferably 41.0% or less. It is presumed that a composite metal oxide having a large amount of sodium atoms in its composition, a moderately high porosity as described above, and a sparse unit lattice structure of the compound, is likely to easily absorb carbon dioxide gas from a gas containing low concentrations of carbon dioxide gas, and also to realize good regeneration at low temperatures. Specifically, the large amount of sodium atoms in the composition means 5≦A≦11, more preferably 6≦A≦10, and even more preferably 7≦A≦9, as shown in the above formula (1).
[0027] The porosity of the composite metal oxide is calculated using the following formula (2). [Number 1] Porosity (%) = 100 - [(sum of the sphere volumes of all ions contained in the unit cell) / unit cell volume) × 100] (2) Here, the spherical volume of an ion refers to the volume of a sphere calculated from the radius of the atomic sphere, assuming that the atomic sphere of each atom is a non-deformable sphere.
[0028] (Form of complex metal oxide) The shape of the composite metal oxide used in the present invention is not particularly limited, and may be, for example, a powder or a porous body bound with a binder. A powder composite metal oxide is preferable from the viewpoint of increasing the absorption rate of carbon dioxide gas because the total area in contact with gas is large. A porous composite metal oxide is also preferable from the viewpoint of excellent handling. Methods for forming a composite metal oxide into a porous body include, but are not limited to, granulation and extrusion methods. The porous body may be adjusted to have an average particle size of, for example, about 0.1 mm to 10.0 mm, and various shapes such as granular, cylindrical, disc, honeycomb, etc. may be adopted.
[0029] When forming the composite metal oxide into the porous body, a binder material (binding agent) for binding the powdered composite metal oxide can be used. The binder material can be either an inorganic material or an organic material. Examples of the inorganic material include clay, minerals, milk of lime, etc. Examples of the organic material include starch, methyl cellulose, polyvinyl alcohol, paraffin, etc.
[0030] (Method of producing composite metal oxide) The method for producing the composite metal oxide used in the present invention is not particularly limited, and can conform to a general method for producing composite metal oxides. An example of a method for producing a composite metal oxide used in the present invention will be described with reference to FIG. 3. Specifically, in FIG. 14 1 shows the steps of a manufacturing method. First, sodium carbonate and titanium dioxide are mixed to obtain a mixture. The mixing ratio is adjusted so that it is the same as the composition ratio of sodium and titanium in the composite metal oxide finally obtained. Next, ion-exchanged water is poured into the mixture, and then the mixture is mixed for 1 hour using an ultrasonic stirrer. After stirring, the mixture is heated at 80°C and evaporated to dryness until no moisture is visible in the container or mixture, and then dried overnight in a thermostatic bath adjusted to 120°C. The dried product obtained is ground and mixed for 30 minutes using an agate mortar to obtain a mixed powder. The mixed powder is placed in a tubular furnace, heated at 700°C for 5 hours under air flow, and then cooled naturally to 100°C or less under argon gas flow to obtain powdered Na8Ti5O 14 is obtained.
[0031] Na8Ti5O 14When producing a composite metal oxide in which part of the titanium is replaced by another metal (M in the above formula (1)), sodium carbonate, titanium dioxide, and metal M are mixed to obtain a blend. The blending ratio is adjusted, as described above, so as to be the same as the composition ratio of sodium, titanium, and metal M in the composite metal oxide finally obtained. The blend thus obtained is used to produce Na A Ti B M C O D can be manufactured.
[0032] [Carbon dioxide absorption method] The carbon dioxide gas absorbent of the present invention described above reacts with a gas containing carbon dioxide gas upon contact with the gas, and absorbs the carbon dioxide gas in the gas. As a preferred example of a method for absorbing carbon dioxide gas using the carbon dioxide gas absorbent of the present invention, the carbon dioxide gas absorbing method of the present invention will be described below.
[0033] The carbon dioxide absorption method of the present invention includes a storage step of storing the carbon dioxide absorbent of the present invention in a reaction vessel, a reaction step of introducing a carbon dioxide-containing gas into the reaction vessel and bringing the carbon dioxide-containing gas into contact with the composite metal oxide to cause a reaction, and a discharge step of discharging the gas that has undergone the reaction step from the reaction vessel. The carbon dioxide gas absorption method of the present invention can absorb carbon dioxide gas in a very simple manner and can discharge a gas having a lower carbon dioxide gas concentration than before the reaction. The carbon dioxide gas absorption method of the present invention may further include a recovery step of recovering the gas having a lower carbon dioxide gas concentration discharged from the discharge step.
[0034] The carbon dioxide gas absorption method of the present invention enjoys the effects of the carbon dioxide gas absorbent of the present invention described above. Therefore, carbon dioxide gas can be absorbed not only from a gas having a high carbon dioxide gas concentration, but also from a gas having a low carbon dioxide gas concentration. For example, in the carbon dioxide absorption method of the present invention, the carbon dioxide concentration of the carbon dioxide-containing gas introduced into the reaction vessel in the above-mentioned reaction step may be 10% or less, 1% or less, 0.1% or less, or 0.05% or less.
[0035] In the carbon dioxide gas absorption method of the present invention, the reaction step can be carried out at a high temperature or at about room temperature. More specifically, the temperature environment of the reaction step is preferably 5° C. or higher, more preferably 15° C. or higher, and even more preferably 25° C. or higher, from the viewpoint of better absorption of carbon dioxide gas. Also, from the viewpoint of exhibiting good thermal efficiency, the temperature is preferably 250° C. or lower, more preferably 200° C. or lower, even more preferably 100° C. or lower, and particularly preferably 50° C. or lower. For example, air at room temperature can be directly subjected to the reaction step, and carbon dioxide gas can be absorbed from the air. Alternatively, relatively high-temperature exhaust gas discharged from a factory can be directly subjected to the reaction step. In addition, a heating step for raising the temperature of the carbon dioxide gas-containing gas to be reacted with the carbon dioxide gas absorbent in the reaction step to a predetermined temperature in advance can be carried out before or during the reaction step.
[0036] The atmospheric gas in the reaction step is not particularly limited, but may be, for example, air or an inert gas such as nitrogen or argon.
[0037] The carbon dioxide absorption rate of the carbon dioxide absorbent of the present invention can be improved by increasing the humidity of the carbon dioxide-containing gas to be reacted. Therefore, a "humidity adjustment step" for increasing the humidity of the carbon dioxide-containing gas to be reacted may be carried out before the reaction step. The humidity adjustment step can be carried out appropriately within a range in which the humidity of the carbon dioxide-containing gas can be increased, and for example, it can be carried out by preparing an environment with a humidity relatively higher than the humidity of the carbon dioxide-containing gas to be introduced and passing the carbon dioxide-containing gas under the environment. More specifically, for example, a water tank is placed in the flow path of the carbon dioxide-containing gas to pass the carbon dioxide-containing gas through the water, or the carbon dioxide-containing gas is brought into contact with the water surface, but this is not limited thereto. From the viewpoint of increasing the absorption rate of carbon dioxide gas, the humidity of the carbon dioxide gas-containing gas subjected to the reaction step is preferably a relative humidity (RH) of 18% or more, more preferably a relative humidity (RH) of 40% or more, even more preferably a relative humidity (RH) of 60% or more, and even more preferably a relative humidity (RH) of 70% or more.
[0038] The flow rate and pressure of the carbon dioxide-containing gas passing through the reaction step are not particularly limited. For example, the flow rate can be adjusted to about 50 ml / min to 200 ml / min. The pressure can be adjusted to 0.1 MPa or more or 0.1 MPa or less. The carbon dioxide-containing gas introduced into the reaction vessel may be continuously discharged from the reaction vessel, or may be discharged after being stored in the reaction vessel for a predetermined time.
[0039] [Carbon dioxide absorption device] Next, the carbon dioxide gas absorbing device of the present invention will be described. Fig. 4 shows a carbon dioxide gas absorbing device 100 according to one embodiment of the present invention. In the description of the carbon dioxide gas absorbing device 100, the upstream side and downstream side refer to the upstream side and downstream side of the gas flow from an arbitrary position in the gas flow in the device. The carbon dioxide gas absorbing device 100 includes a storage section 10 that stores the above-described carbon dioxide gas absorbent 20 of the present invention, a gas inlet 30 that allows a carbon dioxide-containing gas to flow into the storage section 10, and a gas outlet 40 that discharges the gas from the storage section 10 to the outside. In this embodiment, the gas inlet 30 and the gas outlet 40 are provided on both ends of the tubular storage section 10. The carbon dioxide gas absorbing device 100 can enjoy the effect of the carbon dioxide gas absorbent of the present invention, absorb carbon dioxide gas well, and discharge gas with a reduced carbon dioxide gas concentration. Although not shown, a recovery section for recovering the discharged gas may be provided downstream of the gas discharge port 40.
[0040] In this embodiment, the carbon dioxide-containing gas introduced into the storage section 10 is shown as air with a low carbon dioxide concentration, but the present invention is not limited to this and a carbon dioxide-containing gas with a high carbon dioxide concentration can be introduced into the storage section 10 and the carbon dioxide can be absorbed by the carbon dioxide absorbent 20 stored in the storage section 10.
[0041] The carbon dioxide gas absorbing device 100 according to this embodiment is provided with a humidity adjusting section 50 upstream of the gas inlet 30. The humidity adjusting section 50 is a means for increasing the relative humidity of the carbon dioxide gas-containing gas introduced into the storage section 10, and its configuration is not particularly limited as long as it can increase the relative humidity of the carbon dioxide gas-containing gas. The humidity adjusting section 50 in this embodiment shown in Fig. 4 increases the humidity of the carbon dioxide gas-containing gas by passing the carbon dioxide gas-containing gas below the water surface 58 or by bringing the carbon dioxide gas-containing gas into contact with the water surface 58. More specifically, the container 52 in this embodiment is provided with a first inlet passage 32 for introducing external gas into the container 52, and a second inlet passage 34 for introducing gas in the container 52 into the storage unit 10. The gas introduced into the container 52 through the first inlet passage 32 passes through an inlet pipe 54 provided inside the container 52 and is discharged from a downstream opening 321 of the inlet pipe 54. The discharged gas comes into contact with water, and is introduced to the outside through an outlet pipe 56 provided inside the container 52, and is introduced into the storage unit 10 through a second inlet passage 34 connected thereto. At this time, the humidity of the carbon dioxide-containing gas can be adjusted, for example, by adjusting the distance between the downstream opening 321 of the inlet pipe 54 and the water surface 58. That is, when the downstream opening 321 is located below the water surface 58, the carbon dioxide-containing gas passes through the water, and the humidity of the carbon dioxide-containing gas can be sufficiently increased. In addition, by arranging the downstream opening 321 above the water surface 58, the increase in humidity of the carbon dioxide-containing gas can be kept relatively small. The humidity can also be adjusted by adjusting the flow rate of the carbon dioxide-containing gas passing through the container 52 .
[0042] Although not shown, the carbon dioxide gas absorbing device 100 may be provided with a heating means on the upstream side of the storage section 10 or in the storage section 10, and the carbon dioxide gas-containing gas and the carbon dioxide gas absorbent 20 may be reacted in a temperature environment higher than room temperature. The storage section 10 may be heated by a heating means provided outside the storage section 10, and the carbon dioxide gas-containing gas and the carbon dioxide gas absorbent 20 may be reacted. The carbon dioxide gas absorbent 20 may be filled entirely into the internal space of the storage section 10.
[0043] [How to regenerate carbon dioxide absorbents] The carbon dioxide gas absorbent of the present invention can be regenerated into a state capable of absorbing carbon dioxide gas again by desorbing the absorbed carbon dioxide gas through heating. A suitable example of such a regeneration method is the carbon dioxide absorbent regeneration method of the present invention, in which the reaction product after the carbon dioxide absorption reaction (used carbon dioxide absorbent) is heated at a temperature of 400°C or lower in the presence of air or an inert gas. The method for regenerating a carbon dioxide gas absorbent of the present invention can regenerate a used carbon dioxide gas absorbent at a temperature significantly lower than the conventional regeneration temperature for sodium ferrite, and has good thermal efficiency.
[0044] The reason why the carbon dioxide absorbent can be regenerated at low temperatures in the carbon dioxide absorbent regeneration method of the present invention is not clear, but the following factors are thought to be the cause: The first factor is that the composite metal oxide used in the present invention tends to have a large sodium composition ratio and a large porosity in the unit lattice, the second factor is that the reactivity of the titanium compound in the used carbon dioxide absorbent of the present invention is higher than the reactivity of the iron oxide in used conventional sodium ferrite, and the third factor is that the composite metal oxide used in the present invention absorbs less water simultaneously with carbon dioxide during the absorption reaction than sodium ferrite, so that less energy (calorie) is required to be input when desorbing carbon dioxide and water during the regeneration reaction.
[0045] In the carbon dioxide gas absorbent regeneration method of the present invention, the heating temperature is preferably 350° C. or lower from the viewpoint of economic efficiency, more preferably 300° C. or lower, and even more preferably 270° C. or lower. Moreover, from the viewpoint of rapid regeneration, the lower limit of the heating temperature is preferably 200° C. or higher, more preferably 220° C. or higher, and even more preferably 230° C. or higher.
[0046] In the carbon dioxide absorbent regeneration method of the present invention, for example, a used carbon dioxide absorbent is placed in a container filled with air or an inert gas such as argon or nitrogen, and heated at the temperature range described above for about 12 to 24 hours. This causes carbon dioxide and moisture to be desorbed from the used carbon dioxide absorbent (particularly the composite metal oxide), and a reusable carbon dioxide absorbent is obtained. The desorbed carbon dioxide may be recovered and provided for industrial use. EXAMPLES
[0047] The present invention will be described in detail below with reference to examples. Table 1 shows the conditions for producing the carbon dioxide gas absorbent in each example and comparative example. However, the present invention is not limited to the examples described below.
[0048] [Example 1] A mixed powder was obtained by adjusting the molar ratio of sodium carbonate (Na2CO3) and titanium dioxide (TiO2) to Na:Ti = 8:5. 100 ml of ion-exchanged water was added to the mixed powder and stirred for 1 hour with an ultrasonic stirrer, then evaporated to dryness on a hot stirrer, and the dried mixed powder was placed in a thermostatic bath at 120°C and dried overnight. The mixed powder removed from the thermostatic bath was ground and mixed in an agate mortar for 30 minutes, and the ground mixture thus obtained was heated in a tubular furnace under air circulation at 700°C for 5 hours. After heating, argon gas was circulated while the temperature was lowered to room temperature, whereby Na8Ti5O 14 This was obtained as Example 1.
[0049] [Examples 2 to 5, Comparative Example 1] Examples 2 to 5 and Comparative Example 1 were produced in the same manner as in Example 1 described above, except that the carbon dioxide gas absorbent production conditions were changed as shown in Table 1.
[0050] [Comparative Example 2] Sodium nitrate (NaNO3) and iron oxide (Fe2O3) were used, and the molar ratio Na:Fe was adjusted to 1:1 to obtain a mixed powder. 100 ml of ion-exchanged water was added to the mixed powder, which was then stirred for 1 hour with an ultrasonic stirrer, and then evaporated to dryness on a hot stirrer. The dried mixed powder was placed in a thermostatic bath at 120°C and dried overnight. The mixed powder removed from the thermostatic bath was ground and mixed in an agate mortar for 30 minutes, and the ground mixture thus obtained was heated in a tubular furnace under air circulation at 800°C for 15 hours. After the heating was completed, argon gas was circulated when the temperature was lowered to room temperature, thereby obtaining β-NaFeO2, which was designated as Comparative Example 2.
[0051] [Comparative Example 3] Sodium nitrate (NaNO3) and manganese nitrate (Mn(NO3)2) were used and adjusted to a molar ratio of Na:Mn = 0.70:1 to obtain a mixed powder. 100 ml of ion-exchanged water was added to the above mixed powder and stirred with an ultrasonic stirrer for 1 hour, then evaporated to dryness on a hot stirrer, and the dried mixed powder was placed in a thermostatic bath at 120°C and dried overnight. The mixed powder removed from the thermostatic bath was ground and mixed in an agate mortar for 30 minutes, and the ground mixture thus obtained was heated in a tubular furnace under air circulation at 650°C for 3 hours, and after heating, argon gas was circulated while the temperature was lowered to room temperature, whereby Na 0.7 MnO 2.05 This was designated as Comparative Example 3.
[0052] [Carbon dioxide absorption reaction] The carbon dioxide gas absorption reaction of the carbon dioxide gas absorbent of Example 1 obtained as described above was confirmed as follows using a carbon dioxide gas absorption device (100) shown in Figure 4. The reaction conditions for the carbon dioxide gas absorption reaction are shown in Table 2. Specifically, 100 mg of the carbon dioxide gas absorbent (20) of Example 1 was placed in a tubular furnace (accommodation section (10)) with a volume of about 0.2 L, and 1 ml of water was filled in a 200 ml Erlenmeyer flask (container (50)) in the humidity adjustment section (50). Then, at an ambient temperature of 25° C., air was introduced into the container (50) from the first inflow passage (32 (30)) at a flow rate of 100 ml / min, and the air was discharged into the container (50) from the downstream opening (321) of the introduction pipe (54). After the air and water were brought into contact with each other in the container (50), the air with increased humidity was discharged from the discharge pipe (56) and introduced into the tubular furnace (accommodation section (10)) from the second flow passage (34) connecting the container (50) and the tubular furnace (accommodation section (10)). The air that flowed into the tubular furnace (container (10)) came into contact with the carbon dioxide gas absorbent (20) and was then discharged to the outside through the gas outlet (40). The above-mentioned series of steps was carried out continuously for 18 hours.
[0053] In order to adjust the humidity of the air flowing into the tubular furnace (the storage section (10)), the distance between the downstream opening (321) of the inlet pipe (54) and the water surface (58) was adjusted. Specifically, in Example 1-1, the downstream opening (321) was positioned below the water surface (58) so that the air passed underwater, and thus the humidity was adjusted to a high humidity (RH 77%). In Example 1-2, the humidity (RH) was adjusted to 67% by circulating the air with the downstream opening (321) located closer to the water surface (18). In Example 1-3, the humidity (RH) was adjusted to 41% by circulating the air with the downstream opening (321) located further away from the water surface (58) than in Example 1-2.
[0054] [Analysis of carbon absorbent after reaction] After completing the series of steps as described above, elemental analysis was performed using 1 mg of the used carbon dioxide gas absorbent (reaction product) in the tubular furnace, and the carbon (C) content (mass%) and hydrogen (H) content (mass%) in 100 mass% of the sample were confirmed and shown in Table 1. The elemental analysis was performed using an elemental analyzer (trade name: FlashSmart) manufactured by Thermo Scientific. In addition, the amount of carbon dioxide and water actually absorbed was calculated from the carbon and hydrogen contents (mass%) confirmed by such elemental analysis and the amount of carbon dioxide gas absorbent set in the tubular furnace, and is shown in Table 2.
[0055] Carbon dioxide gas absorption reaction was carried out in the same manner as in Example 1, except that the carbon dioxide gas absorption reaction conditions were changed to those shown in Table 2, using Examples 2 to 5 and Comparative Examples 1 to 3 obtained as described above. In addition, in Examples 2 to 5 and Comparative Examples 1 to 3, the humidity was adjusted by adjusting the position of the downstream opening (321) of the inlet pipe (54) with respect to the water surface (58) in the same manner as in Examples 1-1 to 1-3. In Comparative Example 2, the carbon dioxide absorption reaction was carried out with air having a humidity (RH) of 76% in Comparative Example 2-1, and with air having a humidity (RH) of 39% in Comparative Example 2-2. In addition, for Examples 2 to 5 and Comparative Examples 1, 2-1, 2-2, and 3, which are reaction products after the absorption reaction, the carbon dioxide and moisture in the reaction products were analyzed in the same manner as in Example 1. The analysis results are shown in Table 2.
[0056] [Confirmation of crystal density, lattice volume, and porosity] For the above-mentioned Example 1 and Comparative Example 1, the crystal density (g / cm 3 ), unit cell volume (Å 3 ) was calculated. The unit cell volume (Å 3 The porosity (%) was calculated using the following formula (2). The crystal density, unit lattice volume, and porosity calculated as described above are all shown in Table 3. [Number 2] Porosity (%) = 100 - [(sum of the sphere volumes of all ions contained in the unit cell) / unit cell volume) × 100] (2) Here, the spherical volume of an ion refers to the volume of a sphere calculated from the radius of the atomic sphere, assuming that the atomic sphere of each atom is a non-deformable sphere.
[0057] [X-ray diffraction] Powder X-ray diffraction using CuKα radiation was performed on Examples 1 to 5 obtained as described above, and the differences in the XRD patterns were confirmed. The results are shown in FIG. 5. Similarly, changes in the XRD patterns were confirmed for Example 1-1 and Examples 2 to 5 that had been used after absorbing carbon dioxide gas. The results are shown in FIG. 6. For confirmation, FIG. 6 also shows basic data showing powder X-ray diffraction patterns using CuKα radiation of Na2CO3·H2O.
[0058] 5, it was confirmed that the diffraction angle 2θ of each of Examples 1 to 5 exhibits peaks in the ranges of 12.049°±0.5° and 12.616°±0.5°, and exhibits one or two peaks in the range of 39.110°±0.5° to 41.007°±0.5°. In particular, it was confirmed that the diffraction angle 2θ of each of Examples 1 to 4 exhibits peaks in the ranges of 12.049°±0.5° and 12.616°±0.5°, and exhibits peaks in the ranges of 39.110°±0.5° and 41.007°±0.5°. Furthermore, in the XRD pattern change in FIG. 6, a peak specific to Na2CO3·H2O was observed in all of Examples 1-1 to 5 after the carbon dioxide gas absorption reaction, confirming that carbon dioxide gas was absorbed by the carbon dioxide gas absorption reaction.
[0059] [Regeneration of carbon dioxide absorbents] The used Example 1-1 used in the carbon dioxide gas absorption reaction was regenerated as follows. 10 mg of the reaction product of Example 1-1 was used as a sample, and the sample was set in the sample chamber of a heating type X-ray diffraction device in air. The sample was left for 5 minutes in the sample chamber of the device at room temperature, 50°C, 100°C, 150°C, 200°C, 250°C, and 300°C, respectively, to carry out a regeneration reaction and obtain a regenerated product.
[0060] The regenerated materials obtained at each temperature as described above were used as samples, and powder X-ray diffraction was performed using CuKα radiation to confirm the change in crystal phase due to the regeneration reaction. The powder X-ray diffraction pattern is shown in Figure 7. For confirmation, Figure 7 also shows basic data showing the powder X-ray diffraction pattern of Example 1 before the carbon dioxide absorption reaction, as well as basic data showing the powder X-ray diffraction patterns of Na2CO3·H2O and Na2CO3. As can be seen in boxes 60 and 62 in FIG. 7, in the regeneration reactions where the regeneration temperatures were 200° C., 250° C., and 300° C., Na8Ti5O 14 Four large peaks characteristic of the carbon dioxide absorbent were identified, confirming that the carbon dioxide absorbent had been regenerated.
[0061] In addition, Na8Ti5O 14 Approximately 5 mg of the reaction product was used as a sample, and the thermal decomposition behavior was observed by simultaneous differential thermal analysis and thermogravimetry (TG-DTA) while heating from room temperature to 300°C. The results of simultaneous differential thermal analysis and thermogravimetry are shown in Figure 8. It was presumed that the dehydration reaction of sodium carbonate hydrate occurred due to the endothermic reaction in box 64 shown in FIG. 8. By further heating to a high temperature, another endothermic reaction occurred in box 66, which resulted in the desorption of carbon dioxide and the dehydration of Na8Ti5O 14 It was confirmed that the video was played.
[0062] [Table 1]
[0063] [Table 2]
[0064] [Table 3]
[0065] The present invention described above encompasses the following technical ideas. (1) A carbon dioxide gas absorbent characterized by containing a composite metal oxide represented by the following formula (1) (wherein, in formula (1), 5≦A≦11, 4≦B≦6, 0≦C≦2, 10.5≦D≦17.5, and M is any metal). [Formula 3] Na A Ti B M C O D ...(1) (2) Contains a complex metal oxide containing sodium, titanium, and oxygen; The composite metal oxide has a powder X-ray diffraction pattern using CuKα radiation, A carbon dioxide absorbent characterized in that the diffraction angle 2θ exhibits peaks in the ranges of 12.049°±0.5° and 12.616°±0.5°, and exhibits one or two peaks in the range from 39.110°±0.5° to 41.007°±0.5°. (3) The carbon dioxide gas absorbent according to (1) or (2) above, wherein the composite metal oxide has a porosity of 39.0% or more. (4) The composite metal oxide is Na8Ti5O 14 The carbon dioxide gas absorbent according to (1) or (2) above, (5) a step of storing the carbon dioxide gas absorbent according to (1) or (2) above in a reaction vessel; a reaction step of introducing a carbon dioxide-containing gas into the reaction vessel and contacting the carbon dioxide-containing gas with the composite metal oxide to cause a reaction; and a discharge step of discharging the gas that has undergone the reaction step from the reaction vessel. (6) A storage section for storing the carbon dioxide gas absorbent according to (1) or (2) above; a gas inlet for introducing a carbon dioxide-containing gas into the storage section; a gas exhaust port for exhausting gas from the storage section to the outside; A carbon dioxide gas absorption device comprising: (7) A method for regenerating the carbon dioxide gas absorbent according to (1) or (2) above, The reaction product after the carbon dioxide absorption reaction is A method for regenerating a carbon dioxide gas absorbent, comprising heating the absorbent at a temperature of 400°C or lower in air, an inert gas or a vacuum. [Explanation of symbols]
[0066] 10...tubular furnace 20 Carbon dioxide absorbent 30 Gas inlet 32...first inflow path 321...Downstream opening 34...Second inflow channel 40...Gas outlet 50...Humidity adjustment section 52...container 54...Introduction pipe 56...Discharge pipe 58...Water surface 60, 62, 64, 66... frames 100 Carbon dioxide absorption device
Claims
1. A carbon dioxide gas absorbent characterized by containing a composite metal oxide represented by the following formula (1) (wherein, in formula (1), 5≦A≦11, 4≦B≦6, 0≦C≦2, 10.5≦D≦17.5, and M is any metal). [Formula 1] Na A Ti B 7. C 9 D ・・・・・(1)
2. It contains a complex metal oxide containing sodium, titanium, and oxygen, The composite metal oxide has a powder X-ray diffraction pattern using CuKα radiation, A carbon dioxide gas absorbent characterized in that the diffraction angle 2θ shows peaks in the ranges of 12.049°±0.5° and 12.616°±0.5°, and shows one or two peaks in the range from 39.110°±0.5° to 41.007°±0.5°.
3. 3. The carbon dioxide gas absorbent according to claim 1, wherein the composite metal oxide has a porosity of 39.0% or more.
4. The composite metal oxide is Na 8 Ti 5 O 14 The carbon dioxide gas absorbent according to claim 1 or 2, comprising:
5. A step of housing the carbon dioxide gas absorbent according to claim 1 or 2 in a reaction vessel; a reaction step of introducing a carbon dioxide-containing gas into the reaction vessel and contacting the carbon dioxide-containing gas with the composite metal oxide to cause a reaction; and a discharge step of discharging the gas that has undergone the reaction step from the reaction vessel.
6. A storage section for storing the carbon dioxide gas absorbent according to claim 1 or 2; a gas inlet for introducing a carbon dioxide-containing gas into the storage section; a gas exhaust port for exhausting gas from the storage section to the outside; A carbon dioxide gas absorption device comprising:
7. A method for regenerating the carbon dioxide gas absorbent according to claim 1 or 2, The reaction product after the carbon dioxide absorption reaction is A method for regenerating a carbon dioxide gas absorbent, comprising heating the absorbent at a temperature of 400° C. or less in air, an inert gas or a vacuum.
Citation Information
Patent Citations
Method for manufacturing α-sodium ferrite
JP2016003156A
Cited By
Carbon dioxide gas absorbing material, carbon dioxide gas absorbing method, carbon dioxide gas absorbing device, and method for regenerating carbon dioxide gas absorbing material
WO2026094252A1