Toner

A toner with a specific fumaric acid to fatty acid metal salt ratio crosslinks to enhance abrasion resistance, addressing the issue of image slipperiness loss during rubbing, thereby maintaining image integrity.

JP2024160756APending Publication Date: 2024-11-15CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023076059
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing toners fail to maintain image slipperiness when rubbed for a long time, leading to image loss and decreased intensity.

Method used

A toner formulation containing binder resin and fatty acid metal salt particles, with a controlled molar ratio of fumaric acid to fatty acid metal salt, which crosslinks to enhance abrasion resistance and maintain slipperiness.

Benefits of technology

The toner effectively prevents image loss and maintains slipperiness even after prolonged rubbing, ensuring high scratch resistance and image integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160756000001
    Figure 2024160756000001
  • Figure 2024160756000002
    Figure 2024160756000002
  • Figure 2024160756000003
    Figure 2024160756000003
Patent Text Reader

Abstract

To provide a toner that can maintain slidability of an image even when the image is rubbed for a long period and can prevent omission of an image.SOLUTION: A toner has toner particles containing a binder resin, and an external additive. The external additive includes particles of a fatty acid metal salt. The toner contains fumaric acid. When the content of the fumaric acid in the toner is defined as a (mol / g), and the content of the particles of the fatty acid metal salt in the toner as b (mol / g), the following formula (1) is satisfied. (1) 0.50≤a / b≤70.00.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners for use in recording methods utilizing electrophotography, electrostatic recording, and toner jet recording. [Background technology]

[0002] In recent years, the fields in which electrophotographic image formation is used have become more diverse, ranging from printers and copiers to commercial printing machines, and the applications of images obtained by electrophotography have become more diverse. In the midst of this, the use of electrophotographic images is expanding to the exterior packaging of products, etc., and there is a problem in that images can be lost due to rubbing during stacking and transportation in logistics. To deal with such image defects, measures have been taken to increase the strength of the image surface and to improve the slipperiness of the image surface.

[0003] Patent Document 1 discloses a toner containing toner particles containing an amorphous polyester resin synthesized using fumaric acid as a monomer, a crystalline polyester resin, and fatty acid metal salt particles. On the other hand, Patent Document 2 discloses a toner in which the content of a monomer having a carboxylic acid group in the toner is specified in order to improve the low-temperature fixing property, heat-resistant storage property, charge stability (charge rise property), and contamination resistance of the toner and to suppress the occurrence of toner scattering inside the machine and background scumming. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-052627 [Patent Document 2] JP 2016-173396 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors have studied that an image formed using the toner described in Patent Document 1 has excellent surface slippage due to the lubricant action of fatty acid metal salt particles. However, it has become clear that when the surface of an image formed using the toner described in Patent Document 1 is rubbed for a long time, the slippage of the image gradually decreases. As a result, there is a problem that the image strength decreases, and it has been found that improvement is necessary. Moreover, the toner of Patent Document 2 has no effect of improving the slipperiness of the image surface. As described above, conventional studies have not yielded a toner that can maintain the slipperiness of the image surface when rubbed for a long period of time and can suppress image loss, and it has been found that improvements are necessary.

[0006] The present disclosure solves the above problems and provides a toner that can maintain the slipperiness of an image and suppress image loss even when the image is rubbed for a long period of time, i.e., a toner that has high image resistance to rub-off. [Means for solving the problem]

[0007] The present disclosure relates to A toner having toner particles containing a binder resin and an external additive, the external additive comprises particles of a fatty acid metal salt; The toner contains fumaric acid, The content of the fumaric acid in the toner is represented by a (mol / g), When the content of the fatty acid metal salt particles in the toner is b (mol / g), The toner satisfies the following formula (1). 0.50≦a / b≦70.00 (1) Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a toner that can maintain the slipperiness of an image even when the image is rubbed for a long period of time, and can suppress image loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. The term "monomer unit" refers to the reacted form of a monomer substance in a polymer. For example, one section of carbon-carbon bond in the main chain of a polymer in which a polymerizable monomer is polymerized is considered to be one unit. The polymerizable monomer can be represented by the following formula (C). [ka]

[0010] In formula (C), R A represents a hydrogen atom or an alkyl group (preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group); R B represents an optional substituent.

[0011] The present disclosure relates to A toner having toner particles containing a binder resin and an external additive, the external additive comprises particles of a fatty acid metal salt; The toner contains fumaric acid, The content of the fumaric acid in the toner is represented by a (mol / g), When the content of the fatty acid metal salt particles in the toner is b (mol / g), The toner satisfies the following formula (1). 0.50≦a / b≦70.00 (1)

[0012] The present inventors speculate as follows about the reason why the toner of the present disclosure can maintain the slipperiness of an image even when the image is rubbed for a long period of time. One of the reasons why the slipperiness of an image obtained using a toner having fatty acid metal salt particles as an external additive is reduced when the image is rubbed for a long time is believed to be that the fatty acid metal salt particles present on the image surface are detached by rubbing. That is, the image after image formation has fatty acid metal salt particles acting as a lubricant on the image surface, so that the image has high slipperiness and image loss can be suppressed. On the other hand, when the image is rubbed for a long time, the fatty acid metal salt particles acting as a lubricant are detached, and the slipperiness of the image is reduced. As a result, the strength of the image is reduced and image loss occurs. Therefore, the present inventors considered that in order to solve the problems of the present disclosure, it is necessary to suppress the detachment of fatty acid metal salt particles from an image.

[0013] The reason why the fatty acid metal salt particles are detached by rubbing is thought to be because fatty acid metal salts are low molecular weight compounds and have high molecular mobility. In order to suppress this, it was thought that it would be effective to crosslink fatty acid metal salts to each other and increase the apparent molecular weight. As a result of extensive research based on the above considerations, the inventors have discovered that by incorporating fumaric acid in the toner and controlling the molar ratio of the content of fumaric acid in the toner to the content of fatty acid metal salt particles in the toner, it is possible to suppress the detachment of fatty acid metal salt particles due to rubbing of the image, and therefore it is possible to suppress image loss after rubbing. This is believed to be because, in the fixing step during the image formation process, fumaric acid molecules crosslink between metal atoms in fatty acid metal salt molecules, improving the apparent molecular weight of the fatty acid metal salt molecules. Fumaric acid has a double bond and a trans-type molecular structure, so it is likely to have a linear structure. Furthermore, the molecular size of fumaric acid is close to the distance between metal atoms in fatty acid metal salts. For these reasons, fumaric acid is suitable for crosslinking between metal atoms in fatty acid metal salts. Therefore, fumaric acid is believed to have superior crosslinking properties between fatty acid metal salt molecules compared to other dicarboxylic acids.

[0014] The present disclosure will now be described in detail. The toner has toner particles containing a binder resin and an external additive. The external additive contains particles of a fatty acid metal salt. The toner contains fumaric acid. When the content of fumaric acid in the toner is a (mol / g) and the content of fatty acid metal salt particles in the toner is b (mol / g), the toner satisfies the following formula (1). 0.50≦a / b≦70.00 (1)

[0015] In the above formula (1), a / b represents the molar ratio of the content of fumaric acid in the toner to the content of fatty acid metal salt particles in the toner. Here, the content b (mol / g) of fatty acid metal salt particles in the toner is obtained by dividing the content (g) of fatty acid metal salt particles in the toner by the molecular weight of the fatty acid metal salt to obtain the content (number of moles) of fatty acid metal salt particles in the toner, and further converting the content (number of moles) into a value based on the toner mass (g). A specific method for measuring b will be described later. By satisfying the above formula (1), the ratio of the number of fumaric acid to the number of fatty acid metal salts in the toner becomes optimal. As a result, the degree of crosslinking between fatty acid metal salt molecules becomes optimal, and the abrasion resistance of the image is improved. In addition, the crosslinking speed between fatty acid metal salt molecules in the fixing process becomes appropriate, so the fixing temperature does not increase. If a / b is less than 0.50, the degree of crosslinking between fatty acid metal salt molecules becomes insufficient, and the effect of suppressing image dropout may be poor. On the other hand, if a / b is more than 70.00, the content of fumaric acid is too high compared to the content of fatty acid metal salt particles in the toner, and crosslinking may proceed in the early stage of the fixing process. Therefore, it is considered that the fixing temperature may increase. a / b is calculated from the values ​​obtained by measuring a and b using the method described below. a / b is more preferably from 1.20 to 70.00, further preferably from 1.50 to 70.00, even more preferably from 1.50 to 60.00, particularly preferably from 2.00 to 50.00, and even more preferably from 2.00 to 30.00.

[0016] The content of fumaric acid in the toner (mol / g) is 8.60×10-7 ~1.25×10 -5 mol / g, preferably 8.60×10 -7 ~1.05×10 -5 mol / g is more preferable. By satisfying the above conditions, the content of fumaric acid in the toner becomes more appropriate. Fumaric acid has chargeability and hygroscopicity. Therefore, by adjusting the content of fumaric acid appropriately, it is possible to achieve both the charge amount and charge rise in a high-temperature, high-humidity environment, and it is possible to suppress a decrease in image density in a high-temperature, high-humidity environment. A method for measuring the content a of fumaric acid in the toner will be described later. Measuring a by the method described later indicates that fumaric acid is present in a free state in the toner. In addition, the content of fumaric acid in the toner The value of a can be adjusted by changing the amount of fumaric acid added during toner production.

[0017] The means for making the toner contain fumaric acid is not particularly limited, and known means can be used. For example, fumaric acid can be made to be contained in the toner particles. That is, it is preferable that the toner particles contain fumaric acid. Specifically, when producing toner particles by a pulverization method, a method can be used in which fumaric acid is incorporated into the raw material resin in advance, or a method can be used in which fumaric acid is added when the raw material is melted and kneaded so that it is incorporated into the toner particles. When toner particles are produced by a wet production method such as a suspension polymerization method or an emulsion aggregation method, a method of incorporating fumaric acid in the raw material or a method of adding fumaric acid via an aqueous medium during the production process can be used. Further, it is also possible to use a method of externally adding fumaric acid to toner particles by using a known external addition method.

[0018] The content b (mol / g) of fatty acid metal salt particles in the toner is 1.55×10 -7 ~7.90×10 -6mol / g is more preferable. By satisfying the above conditions, the content of fatty acid metal salt particles in the toner becomes appropriate. Therefore, it is possible to further improve the abrasion resistance of the image. In addition, fatty acid metal salt acts as a lubricant. Therefore, by adjusting the content of fatty acid metal salt particles appropriately, it is possible to improve the slippage between the cleaning blade and the photoreceptor in a system that employs a blade cleaning method. As a result, it is possible to improve the cleaning performance of the external additive that has migrated from the toner to the photoreceptor. A method for measuring the content b of fatty acid metal salt particles in the toner will be described later. In addition, the value of the content b of fatty acid metal salt particles in the toner can be adjusted by changing the amount of fatty acid metal salt particles added during toner production.

[0019] Next, materials that can be used in the toner of the present disclosure will be described in detail below.

[0020] <Fatty acid metal salts> The toner contains an external additive, and the external additive contains particles of a fatty acid metal salt. As the fatty acid metal salt, any known fatty acid metal salt can be used without any particular limitation. The fatty acid metal salt is preferably a salt of a polyvalent metal having a valence of 2 or more, more preferably a salt of at least one metal selected from the group consisting of zinc, barium, aluminum, magnesium, and calcium. Among them, from the viewpoint of crosslinkability with fumaric acid, zinc salt is more preferable. Zinc salt has high crosslinkability with fumaric acid, and is more likely to improve the friction resistance.

[0021] The fatty acid of the fatty acid metal salt is not particularly limited, but may be an unsaturated fatty acid, and is preferably a saturated fatty acid. The fatty acid may be linear or branched, but is preferably linear. The fatty acid preferably has 10 to 24 carbon atoms, more preferably 12 to 22. When the carbon number of the fatty acid is within the above range, the formation of a crosslinked structure between fumaric acid and the metal atom of the fatty acid metal salt is not inhibited, and the abrasion resistance of the image can be further improved. In addition, the heat resistance of the image is improved by the crosslink between the metal atoms of the fatty acid metal salt, so that the abrasion resistance of the image can be maintained even when the image is placed under high temperatures. Furthermore, the excellent slipperiness further improves the cleaning property of the external additive. The fatty acid may be at least one selected from the group consisting of octanoic acid, nonanoic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and montanic acid. At least one selected from the group consisting of lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid is preferred. More preferably, it is arachidonic acid.

[0022] Specific examples of fatty acid metal salts include zinc stearate, zinc montanate, zinc behenate, zinc laurate, aluminum stearate, aluminum octylate, barium stearate, barium ricinoleate, etc. Among these, zinc stearate, aluminum stearate, and barium stearate are preferred. Zinc stearate is more preferred.

[0023] Solubility parameter SPf((J / cm 3 ) 1 / 2 ) is not particularly limited, but is preferably 18.00 to 21.00 ((J / cm 3 ) 1 / 2 ) is preferable, and 18.50 to 20.50 ((J / cm 3 ) 1 / 2 ) is more preferable, and 18.50 to 19.50 ((J / cm 3 ) 1 / 2 When SPf is in the above range, it becomes easier to control ΔSPfw, which will be described later, within a preferred range.

[0024] The volumetric median diameter of the fatty acid metal salt particles is preferably 0.15 to 2.0 μm, more preferably 0.3 to 1.5 μm, and even more preferably 0.3 to 1.0 μm. When the volumetric median diameter is within the above range, it is possible to achieve excellent abrasion resistance and cleaning properties even when the fatty acid metal salt particle content is small.

[0025] <Binding resin> The toner includes toner particles, and the toner particles contain a binder resin. The binder resin may be any known binder resin without any particular limitations. Specific examples include polyester resin, vinyl resin, polyurethane resin, polyamide resin, etc. The binder resin preferably contains a polyester resin, and more preferably contains a polyester resin having a monomer unit corresponding to fumaric acid, since this makes it easier to retain fumaric acid in the toner. As the polyester resin, it is preferable to use at least one selected from the group consisting of an amorphous polyester resin and a crystalline polyester resin.

[0026] The polyester resin can be obtained by combining suitable compounds selected from polyvalent carboxylic acids, polyols, hydroxycarboxylic acids, etc., and synthesizing the compounds using a known method such as an ester exchange method or a polycondensation method. Polycarboxylic acids are compounds containing two or more carboxy groups in one molecule. Among them, dicarboxylic acids are compounds containing two carboxy groups in one molecule and are preferably used.

[0027] Examples of dicarboxylic acids include fumaric acid, oxalic acid, succinic acid, glutaric acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-carboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, suberic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylenediacetic acid, m-phenylenediacetic acid, o-phenylenediacetic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracenedicarboxylic acid, and cyclohexanedicarboxylic acid. As described above, it is preferable to contain fumaric acid as the dicarboxylic acid, and it is more preferable to use fumaric acid in combination with an aromatic dicarboxylic acid.

[0028] Examples of polycarboxylic acids other than dicarboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tetracarboxylic acid, and pyrene tetracarboxylic acid. Examples of the succinic acid include tricarboxylic acid, pyrenetetracarboxylic acid, itaconic acid, glutaconic acid, n-dodecylsuccinic acid, n-dodecenylsuccinic acid, isododecylsuccinic acid, isododecenylsuccinic acid, n-octylsuccinic acid, and n-octenylsuccinic acid. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0029] A polyol is a compound containing two or more hydroxyl groups in one molecule. Among them, a diol is a compound containing two hydroxyl groups in one molecule, and is preferably used. Specifically, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanediol, dipropylene glycol, Examples of the bisphenols include propylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-butenediol, neopentyl glycol, 1,4-cyclohexanediol, polytetramethylene glycol, hydrogenated bisphenol A, bisphenol A, bisphenol F, bisphenol S, and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols are particularly preferred.

[0030] Examples of trivalent or higher polyols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, tetraethylolbenzoguanamine, sorbitol, trisphenol PA, phenol novolac, cresol novolac, and alkylene oxide adducts of the above-mentioned trivalent or higher polyphenols. The polyols may be used alone or in combination of two or more kinds. Solubility parameter of polyester resin SPp((J / cm 3 ) 1 / 2 ) is not particularly limited, but is preferably 19.00 to 22.50 (J / cm 3 ) 1 / 220.00 to 21.30 (J / cm 3 ) 1 / 2 Also, 20.50 to 21.30 (J / cm 3 ) 1 / 2 It is preferable that the refractive index is 21.10 to 21.30 (J / cm 3 ) 1 / 2 When the solubility parameter of the polyester resin is within the above range, it becomes easy to adjust the value of the product of the square of ΔSP and the molecular weight of the release agent, which will be described later, to the range described later. The solubility parameter, also known as the SP value, is a number used as an index of solubility or affinity, indicating how much a substance dissolves in another substance. The type of binder resin can be measured by a known method such as NMR.

[0031] The content of the binder resin relative to 100 parts by mass of the toner particles is not particularly limited, but may be 50.0 to 98.0 parts by mass, or 60.0 to 95.0 parts by mass.

[0032] The peak molecular weight (Mp) of the binder resin is not particularly limited, but is preferably 5000 to 10000, more preferably 5000 to 8000. When the peak molecular weight of the binder resin is within the above range, the mobility of fumaric acid and fatty acid metal salt during fixing is increased, so that fumaric acid can crosslink fatty acid metal salt molecules more efficiently. Therefore, it is possible to further improve the abrasion resistance of the image. When a polyester resin is used as the binder resin, for example, the peak molecular weight of the binder resin can be controlled by a known method such as controlling the reaction time.

[0033] <Release agent> The toner particles preferably contain a release agent. By containing the release agent, a release agent layer is formed on the image surface, thereby improving the strength of the image surface. As the releasing agent, there are no particular limitations and known waxes, silicone oils, etc. can be used. Among them, it is preferable to use wax. Specific examples of waxes include paraffin wax, microcrystalline wax, petroleum-based hydrocarbon waxes such as petrolatum and derivatives thereof, montan wax and derivatives thereof, and Fischer-Tropsch hydrocarbon waxes and derivatives thereof. monofunctional ester waxes, such as behenyl behenate, stearyl stearate, and palmityl palmitate, typified by esters of monohydric alcohols and aliphatic carboxylic acids, or esters of monohydric carboxylic acids and aliphatic alcohols; bifunctional ester waxes, such as esters of dihydric alcohols and aliphatic carboxylic acids, or esters of dihydric carboxylic acids and aliphatic alcohols, such as ethylene glycol distearate, dibehenyl sebacate, and hexanediol dibehenate; trifunctional ester waxes, such as esters of trihydric alcohols and aliphatic carboxylic acids, such as glycerol tribehenate, or esters of trihydric carboxylic acids and aliphatic alcohols; tetrafunctional ester waxes, such as esters of tetrahydric alcohols and aliphatic carboxylic acids, or esters of tetrahydric carboxylic acids and aliphatic alcohols, such as pentaerythritol tetrastearate and pentaerythritol tetrapalmitate; hexafunctional ester waxes, such as esters of hexahydric alcohols and aliphatic carboxylic acids, or esters of hexahydric carboxylic acids and aliphatic alcohols, e.g., dipentaerythritol hexastearate and dipentaerythritol hexapalmitate; Esters of polyhydric alcohols and aliphatic carboxylic acids, such as polyglycerol behenate, or esters of polyhydric carboxylic acids and aliphatic alcohols; Natural ester waxes such as carnauba wax and rice wax; Ester waxes, such as Examples of the wax include polyolefin-based hydrocarbon waxes such as polyethylene and polypropylene and their derivatives, and natural waxes such as carnauba wax and candelilla wax and their derivatives. The derivatives include oxides, block copolymers with vinyl monomers, and graft modified products. Other examples include alcohols such as higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid or their acid amides, esters, and ketones, hydrogenated castor oil and its derivatives, vegetable waxes, and animal waxes. These can be used alone or in combination of two or more kinds.

[0034] Among them, at least one selected from the group consisting of hydrocarbon waxes and ester waxes is preferred, and at least one selected from the group consisting of Fischer-Tropsch hydrocarbon waxes, tetrafunctional ester waxes and hexafunctional ester waxes is more preferred. These waxes have high crystallinity and therefore tend to form a uniform release agent layer on the image surface, and are excellent in terms of the effect of increasing the strength of the image surface.

[0035] The content of the release agent is preferably 1.0 to 30.0 parts by mass, and more preferably 5.0 to 20.0 parts by mass, relative to 100.0 parts by mass of the binder resin. The melting point of the release agent is preferably 60 to 120° C., more preferably 70 to 120° C., and even more preferably 80 to 120° C. By using a release agent having a melting point in the above range, the heat resistance of the image is further improved. Solubility parameter of release agent SPw((J / cm 3 ) 1 / 2 ) is, but is not limited to, 16.50 to 19.00 (J / cm 3 ) 1 / 2 17.00 to 18.50 ( J / cm 3 ) 1 / 2 When SPw is in the above range, the value of the product of the square of ΔSPpw and the molecular weight of the release agent described below can be easily adjusted to the above range. The molecular weight of the release agent is not particularly limited, but may be 500 to 1800, and preferably 700 to 1500. When the molecular weight of the release agent is in the above range, the value of the product of the square of ΔSPpw and the molecular weight of the release agent described below can be easily adjusted to the below range.

[0036] <Relationship between the solubility parameter of polyester resin and the solubility parameter and molecular weight of release agent> In a toner in which the binder resin contained in the toner particles contains a polyester resin and the toner particles contain a release agent, the solubility parameter of the polyester resin is SPp((J / cm 3 ) 1 / 2 ), and the solubility parameter of the release agent is SPw((J / cm 3 ) 1 / 2 ), and the difference between SPp and SPw is ΔSPpw, the product of the square of ΔSPpw and the molecular weight of the release agent is 10000.00 (J / cm 3 ) or more, and preferably 11000.00 (J / cm 3 ) or more, and more preferably 12000.00 (J / cm 3 ) or more. The upper limit is not particularly limited, but is preferably 20,000.00 (J / cm 3 ) or less, and 15000.00 or less (J / cm 3 ). For example, it is preferably 10000.00 to 20000.00 (J / cm 3 ), 11000.00~15000.00(J / cm 3 ), 12000.00~15000.00(J / cm 3 ), etc. The product of the square of ΔSPpw and the molecular weight of the release agent represents the ease of separation of the resin and the release agent. If it is 10,000 or more, the release agent is quickly separated in the fixing process and a strong release agent layer is formed on the image surface. As a result, the surface of the fixed image is protected. Therefore, in addition to the improvement in slipperiness due to the fatty acid metal salt, the strength of the fixed image can be further increased, and the taping resistance of the image when taping the image and the abrasion resistance of the image are improved. The method for calculating the solubility parameter and the method for calculating the molecular weight of the release agent will be described later.

[0037] <Relationship between the solubility parameter of fatty acid metal salt and the solubility parameter of release agent> In toner particles containing a release agent, the solubility parameter of the fatty acid metal salt is SPf((J / cm3 ) 1 / 2 ), and the solubility parameter of the release agent is SPw((J / cm 3 ) 1 / 2 ), and the difference between SPf and SPw is ΔSPfw, ΔSPfw is 0.00 to 3.00 ((J / cm 3 ) 1 / 2 ), and preferably 0.20 to 1.60 ((J / cm 3 ) 1 / 2 ), and more preferably 0.30 to 0.80 ((J / cm 3 ) 1 / 2 ) is more preferable. When ΔSPfw is within the above range, it is possible to increase the dispersibility of the fatty acid metal salt particles on the fixed image surface, and improve the uniformity of the image surface, so that it is possible to obtain an image with higher gloss even after rubbing.

[0038] <How to calculate solubility parameter (SP value)> The solubility parameter SPf of the fatty acid metal salt, the solubility parameter SPp of the polyester resin, and the solubility parameter SPw of the release agent are determined as follows in accordance with the calculation method proposed by Fedors. SP value of fatty acid metal salt (SPf) (J / cm 3 ) 1 / 2 and the SP value of the release agent (SPw) (J / cm 3 ) 1 / 2 When calculating the above, the evaporation energy (Δei) (J / mol) and molar volume (Δvi) (cm) are calculated for the atoms or atomic groups in the molecular structures of the fatty acid metal salt and the release agent from the table in "Polym. Eng. Sci., 14(2), 147-154 (1974)". 3 / mol) and calculate using the following formula. (ΣΔei / ΣΔvi) 1 / 2

[0039] SP value of polyester resin (SPp) (J / cm 3 ) 1 / 2When calculating the SP value of the repeating unit constituting the polyester resin, first, the SP value of the repeating unit constituting the polyester resin is calculated as follows. It refers to the molecular structure of the part separated by tert-butyl bonds. For example, the SP value (σm) of the repeating unit (J / cm 3 ) 1 / 2 When calculating the vaporization energy (Δei) (J / mol) and molar volume (Δvi) (cm) for the atom or atomic group in the molecular structure of the repeating unit, refer to the table in "Polym. Eng. Sci., 14(2), 147-154 (1974)". 3 / mol) and calculate using the following formula. σm=(ΣΔei / ΣΔvi) 1 / 2 The SP value (SPp) of a polyester resin is calculated by calculating the evaporation energy (Δei) and molar volume (Δvi) of each repeating unit constituting the resin for each repeating unit, calculating the product of each repeating unit and the molar ratio (j) of each repeating unit in the resin, and dividing the sum of the evaporation energies of each repeating unit by the sum of the molar volumes, using the following formula: σp={(Σj×ΣΔei) / (Σj×ΣΔvi)} 1 / 2

[0040] For example, assuming that a polyester resin is composed of two types of repeating units, X and Y, the composition ratios of the repeating units are Wx and Wy (mass%), the molecular weights are Mx and My, the evaporation energies are Δei(X) and Δei(Y), and the molar volumes are Δvi(X) and Δvi(Y), respectively. Then, the molar ratios (j) of the repeating units are Wx / Mx and Wy / My, respectively, and the solubility parameter (SPp) of this resin is given by the following formula. SPp=[{(Wx / Mx)×Δei(X)+Wy / My×Δei(Y)} / {(Wx / Mx)×Δvi(X)+Wy / My×Δvi(Y)}] 1 / 2 When multiple types of polyester resins are mixed, the SP value of the mixture is defined as SPp. The SP value of the mixture (σM) is calculated as the product of the mass composition ratio of the mixture (Wi) and the SP value of each resin (σi), as shown in the following formula. σM = Σ(Wi × σi)

[0041] <Plasticizer> The toner particles may contain a plasticizer. The plasticizer is not particularly limited, and the waxes listed in the section on the release agent can be used.

[0042] <Coloring agent> The toner particles may contain a colorant. As the colorant, known pigments and dyes of black, yellow, magenta, cyan, and other colors, magnetic materials, and the like can be used without any particular limitation. Black colorants include black pigments such as carbon black.

[0043] Examples of yellow colorants include yellow pigments and yellow dyes such as monoazo compounds, disazo compounds, condensed azo compounds, isoindolinone compounds, benzimidazolone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include CI Pigment Yellow 74, 93, 95, 109, 111, 128, 155, 174, 180, and 185, and CI Solvent Yellow 162.

[0044] Examples of magenta colorants include magenta pigments and magenta dyes such as monoazo compounds, condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specifically, CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 238, 254, 269 , CI Pigment Violet 19, etc.

[0045] Examples of cyan colorants include cyan pigments and cyan dyes such as copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Specifically, examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66.

[0046] The content of the colorant is preferably 1.0 to 20.0 parts by mass with respect to 100.0 parts by mass of the binder resin.

[0047] It is also possible to make the toner magnetic by incorporating a magnetic material in the toner particles. In this case, the magnetic material can also serve as a colorant. Examples of magnetic materials include iron oxides such as magnetite, hematite, and ferrite; metals such as iron, cobalt, and nickel; and alloys of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, beryllium, bismuth, cadmium, calcium, manganese, selenium, titanium, tungsten, and vanadium, and mixtures thereof. When a magnetic material is used as the colorant, the content of the magnetic material is preferably 20.0 to 120.0 parts by mass with respect to 100.0 parts by mass of the binder resin.

[0048] <Charge control agent> The toner may contain a charge control agent. As the charge control agent, any known charge control agent can be used without any particular limitation. Specifically, examples of negative charge control agents include metal compounds of aromatic carboxylic acids such as salicylic acid, alkylsalicylic acid, dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids, or polymers or copolymers having metal compounds of the aromatic carboxylic acids; polymers or copolymers having a sulfonic acid group, a sulfonate salt group, or a sulfonate ester group; metal salts or metal complexes of azo dyes or azo pigments; boron compounds, silicon compounds, and calixarenes. On the other hand, examples of the positive charge control agent include quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains, guanidine compounds, nigrosine compounds, imidazole compounds, and the like. Examples of polymers or copolymers having a sulfonate group or a sulfonate ester group that can be used include homopolymers of sulfonate group-containing vinyl monomers such as styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, and methacrylsulfonic acid, and copolymers of other known vinyl monomers and the above-mentioned sulfonate group-containing vinyl monomers. The content of the charge control agent is preferably 0.01 parts by mass or more and 5.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0049] <External additives> The toner has an external additive. The external additive contains particles of a fatty acid metal salt. The external additive may contain, in addition to the particles of a fatty acid metal salt, an external additive other than the particles of a fatty acid metal salt. As the external additive, any known external additive can be used without any particular limitation. Specific examples include raw silica fine particles such as wet-process silica and dry-process silica, or surface-treated silica fine particles obtained by subjecting such raw silica fine particles to a surface treatment with a treating agent such as a silane coupling agent, a titanium coupling agent, or silicone oil; and resin fine particles such as vinylidene fluoride fine particles and polytetrafluoroethylene fine particles. The content of the external additive is preferably 0.1 to 5.0 parts by mass with respect to 100.0 parts by mass of the toner particles.

[0050] Next, a method for obtaining the toner of the present disclosure will be described in detail below.

[0051] <Method of manufacturing toner particles> The method for producing the toner particles is not particularly limited, and may be an emulsion aggregation method, a suspension polymerization method, a dissolution suspension method, a pulverization method, or the like. Among them, it is preferable to use the emulsion aggregation method. That is, it is preferable that the toner particles are emulsion aggregation toner particles. The emulsion aggregation toner particles have a suitable unevenness on the surface, and therefore have excellent cleaning properties and transfer properties. In addition, it is easy to increase the dispersibility of the fatty acid metal salt particles. In the emulsion aggregation method, a dispersion of fine particles of a binder resin is first prepared, and then dispersions of other materials such as a colorant and a release agent are prepared as necessary. The obtained dispersions of the materials are dispersed and mixed by adding a dispersion stabilizer as necessary. Then, an aggregating agent is added to aggregate the particles to the desired toner particle size, and then or simultaneously with the aggregation, the resin fine particles are fused together. If necessary, the shape is controlled by heat to form toner particles.

[0052] The method for producing the toner preferably includes the following steps. (1) A dispersion and mixing step of preparing a binder resin particle dispersion liquid (and, if necessary, a colorant particle dispersion liquid, etc.) containing a binder resin and fumaric acid, and mixing them to obtain a mixed dispersion liquid; (2) an aggregation step of aggregating the binder resin fine particles (and colorant fine particles, if necessary) contained in the obtained mixed dispersion to form aggregates; and (3) a fusion step of heating the aggregates to fuse them together to form fused particles; The resulting fused particles can be cooled to obtain toner particles.

[0053] It is preferable to have the following step (4) during the above step (3) or after the above steps (1) to (3). (4) A spheronization step in which the agglomerates are heated at a higher temperature. Furthermore, it is more preferable to have the following steps (5) and (6) in this order after the above step (4). (5) A cooling step of cooling the aggregate at a cooling rate of 0.1° C. / min or more. (6) an annealing step of heating and holding the temperature at or above the crystallization temperature or the glass transition temperature of the binder resin after the cooling step;

[0054] Here, the binder resin particles may be composite particles formed of two or more layers of resins having different compositions, and may be produced by at least one method selected from the group consisting of emulsion polymerization, mini-emulsion polymerization, and phase inversion emulsification.

[0055] When an internal additive is contained in the toner particles, the internal additive may be contained in the resin fine particles, or a dispersion liquid of internal additive fine particles containing the internal additive may be prepared separately, and the internal additive fine particles may be aggregated together with the resin fine particles when the internal additive fine particles are aggregated. In addition, toner particles having layer structures with different compositions can be produced by adding resin fine particles with different compositions at different times during aggregation and aggregating them. That is, toner particles having a core-shell structure can be produced. After aggregating resin fine particles containing a binder resin to form a core portion, resin fine particles containing a shell resin can be added at different times and aggregating them to form a shell portion. The shell resin may be the same as or different from the binder resin. For example, the shell resin may contain fumaric acid. The resin fine particles containing the shell resin may contain fumaric acid. The amount of the shell resin added (shell content) is preferably 1.0 to 10.0 parts by mass, more preferably 2.0 to 7.0 parts by mass, based on 100 parts by mass of the binder resin contained in the core particles.

[0056] In the case of producing toner particles having a core-shell structure, the method for producing the toner preferably includes the following steps in the following order. (1) A dispersion step of preparing a dispersion of binder resin particles containing a binder resin and fumaric acid (and, if necessary, a colorant particle dispersion) and mixing the mixture to obtain a mixed dispersion; (2) an aggregation step of aggregating the binder resin particles (and, if necessary, colorant particles) contained in the obtained mixed dispersion to form aggregates; (3) a shell formation step of further adding resin fine particles containing a resin for a shell to the dispersion containing the aggregates, and aggregating the resin fine particles to form aggregates having a shell; and (4) a fusion step of heating the aggregates to fuse them together to form fused particles;

[0057] In addition, it is preferable to have the following step (5) during the above step (4) or after the above steps (1) to (4). (5) A spheronization step in which the agglomerates are heated at a higher temperature. It is more preferable to have the following steps (6) and (7) after the above step (5). (6) A cooling step of cooling the aggregate at a cooling rate of 0.1° C. / sec or more. (7) an annealing step of heating and holding the temperature at or above the crystallization temperature or the glass transition temperature of the binder resin after the cooling step;

[0058] The amount of fumaric acid added is not particularly limited, but is preferably 0.006 to 0.500 parts by mass, more preferably 0.006 to 0.400 parts by mass, and even more preferably 0.006 to 0.200 parts by mass, relative to 100 parts by mass of the binder resin. By being in the above range, the content a of fumaric acid in the toner can be easily and suitably adjusted. The amount of fatty acid metal salt particles added is not particularly limited, but is preferably 0.003 to 0.700 parts by mass, more preferably 0.005 to 0.600 parts by mass, and even more preferably 0.005 to 0.500 parts by mass, relative to 100 parts by mass of toner particles. By being in the above range, it becomes easy to suitably adjust the fatty acid metal salt particle content b in the toner.

[0059] The following can be used as the dispersion stabilizer. As the dispersion stabilizer, a surfactant can be used, including known cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of inorganic dispersion stabilizers include tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Examples of the organic dispersion stabilizer include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch. These can be used alone or in combination of two or more.

[0060] As the flocculant, in addition to a surfactant having a polarity opposite to that of the surfactant used in the above-mentioned dispersion stabilizer, an inorganic salt or a divalent or higher inorganic metal salt can be suitably used. In particular, an inorganic metal salt is preferred because it is easy to control the flocculation property and the toner charge property by ionizing a polyvalent metal element in an aqueous medium. Specific examples of preferred inorganic metal salts include metal salts of calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, iron chloride, aluminum chloride, and aluminum sulfate, as well as polyiron chloride, polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. Among these, aluminum salts and their polymers are particularly preferred. These can be used alone or in combination of two or more. In general, in order to obtain a sharper particle size distribution, the valence of the inorganic metal salt is preferably divalent rather than monovalent, and more preferably trivalent or more than divalent. Furthermore, even if the valence is the same, an inorganic metal salt polymer is more suitable.

[0061] From the viewpoint of high definition and high resolution of images, the weight average particle size (D4) of the toner particles is preferably 3.0 to 10.0 μm. In addition, from the viewpoint of the balance between the developability, the transferability, and the cleanability, the average circularity of the toner particles may be 0.940 to 0.980, preferably 0.950 to 0.980, and more preferably 0.955 to 0.970. By controlling the average circularity within the above range, the fatty acid metal salt is easily distributed uniformly on the toner. Therefore, the uniformity of the image surface after the image is rubbed is improved, and an image with higher gloss can be obtained even after the image is rubbed. In addition, the fatty acid metal salt is stably supplied from the toner to the cleaning blade, and the cleanability of the external additive is further improved.

[0062] <Toner manufacturing method> The toner particles obtained above can be mixed with an external additive containing fatty acid metal salt particles and attached to the surface of the toner particles to produce a toner. That is, the toner manufacturing method includes an external addition step of externally adding an external additive containing fatty acid metal salt particles to the toner particles. At this time, an external additive other than the fatty acid metal salt particles may be added as necessary. The mixer for adding the external additive to the toner particles is not particularly limited, and any known mixer can be used, regardless of whether it is a dry or wet type. Examples include FM Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (manufactured by Kawata Corporation), Nobilta (manufactured by Hosokawa Micron Corporation), and Hybridizer (manufactured by Nara Machinery Co., Ltd.). In order to control the coating state of the external additive, the toner can be prepared by adjusting the rotation speed, processing time, and water temperature and amount of water in the jacket of the external addition device. In addition, sieving devices used to sift out coarse particles after external addition include Ultrasonic (manufactured by Koei Sangyo Co., Ltd.); Resonaseave, Gyroshifter (Tokuju Kogyo Co., Ltd.); Vibrasonic System (manufactured by Dalton Co., Ltd.); Soniclean (manufactured by Shinto Kogyo Co., Ltd.); Turbo Screener (manufactured by Turbo Kogyo Co., Ltd.); Microshifter (manufactured by Makino Sangyo Co., Ltd.), etc.

[0063] The methods for measuring the physical properties of the toner and each material will be described below.

[0064] <Method for measuring the content a (mol / g) of fumaric acid in toner> 0.1 g of toner is dissolved in 1 ml of chloroform. 20 ml of methanol is dropped into the obtained sample solution to precipitate the resin in the solution, and then the solid matter is removed by centrifugation (HITACHI himac CR22G, 12000 rpm, 10 minutes). The solvent is removed from the obtained solution by vacuum distillation, and the solution is further dried under reduced pressure in a 60°C atmosphere for 4 hours. 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile are added to the obtained sample, and the sample is heated at 80°C for 1 hour to perform a silylation treatment. The obtained sample is analyzed by GC-MS (gas chromatography mass spectrometry).

[0065] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0066] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is contained. On the other hand, several samples of fumaric acid alone (e.g., 100 ng, 200 ng, and 300 ng) are precisely weighed and prepared, and before measuring the sample obtained from the toner, each sample is measured under the above-mentioned analytical conditions, and then a calibration curve is created from the amount of fumaric acid added and the fumaric acid peak area value. The content a (mol / g) of fumaric acid in the toner is obtained by converting the area value of the fumaric acid component of the toner based on this calibration curve into the mass of fumaric acid, and then converting it into the number of moles based on the toner mass.

[0067] <Method for identifying fatty acid metal salt particles> The fatty acid metal salt can be identified by a combination of shape observation using a scanning electron microscope (SEM) and elemental analysis using energy dispersive X-ray analysis (EDS). Using a scanning electron microscope "S-4800" (product name; manufactured by Hitachi, Ltd.), the toner is observed in a field of view magnified up to 50,000 times. The focus is adjusted to the surface of the toner particles, and the external additive to be identified is observed. An EDS analysis is performed on the external additive to be identified, and the fatty acid metal salt can be identified based on the presence or absence of an element peak. When an element peak of at least one metal selected from the group consisting of metals that can constitute fatty acid metal salts, such as Mg, Zn, Ca, Al, Na, and Li, is observed, the presence of fatty acid metal salts can be inferred. A sample of the fatty acid metal salt inferred by EDS analysis is prepared separately, and its shape is observed by SEM and analyzed by EDS. The analysis results of the sample are compared to the analysis results of the particles to be identified to determine whether they match, and the fatty acid metal salt is identified.

[0068] <Method of measuring the fatty acid metal salt particle content b (mol / g) in toner> The amount of the metal observed in the identification method of the fatty acid metal salt (hereinafter, also referred to as the metal to be measured) is measured using a wavelength dispersive X-ray fluorescence analyzer. Specifically, 4 g of the following toner is prepared, pelletized, and the content of the metal to be measured is determined. First, the following operation is carried out to separate the metals to be measured into those derived from the particles of fatty acid metal salts externally added to the toner and those derived from the toner particles. First, (1) the toner as is, (2) the toner passed through a sieve with 38 μm (400 mesh) openings five times, and (3) the toner passed through a sieve with 38 μm (400 mesh) openings 20 times are prepared. Then, each of the toners (1), (2), and (3) is measured using a wavelength dispersive X-ray fluorescence analyzer as follows. When the toner passes through the sieve, the fatty acid metal salt particles added to the toner peel off, and the more the toner passes through the sieve, the more fatty acid metal salt particles peel off. Therefore, the metal content in the toner (2) is less than that in (1), and the metal content in the toner (3) is less than that in (2). The metal content derived from the toner particles can be determined by creating a graph using the method described below and extrapolating. Note that if the metal is only contained in the fatty acid metal salt particles, it can be calculated only from the measurement value of (1) above.

[0069] The measurement using a wavelength dispersive X-ray fluorescence analyzer conforms to JIS K 0119-1969, and specifically, is as follows. The measurement equipment used was a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "Sup The X-ray tube anode is Rh, the measurement atmosphere is vacuum, and the measurement diameter (collimator mask diameter) is 27 mm. The measurement uses the Omnian method to measure the range of elements F to U, and detects light elements with a proportional counter (PC) and heavy elements with a scintillation counter (SC). The acceleration voltage and current of the X-ray generator are set to an output of 2.4 kW. For the measurement sample, 4 g of the above toner sample is placed in a dedicated aluminum ring for pressing, flattened, and pressed at 20 MPa for 60 seconds using a tablet molding compression machine "BRE-32" (Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of 2 mm and a diameter of 39 mm.

[0070] Measurements are performed under the conditions described above, and each element is identified based on the peak position of the obtained X-rays. The mass ratio of each element is then calculated from the count rate (unit: cps), which is the number of X-ray photons per unit time. The analysis uses the FP (Fundamental Parameter) quantitative method to calculate the mass ratio of all elements contained in the sample and determine the metal content in the toner. In the FP quantitative method, the balance is set according to the binder resin of the toner. Regarding the metals in the toner determined by fluorescent X-rays, for each of the toners (1), (2), and (3) above, a graph is created with the quantitative value of (1) as A, the quantitative value of (2) as B, and the quantitative value of (3) as C, with the horizontal axis representing the ratio of each measured value to A and the vertical axis representing each measured value. That is, (horizontal axis, vertical axis) = (A / A = 1, A), (B / A, B), and (C / A, C) are plotted, and an approximate line is created by the least squares method. The intercept of the approximate line is considered to be the metal derived from the toner particles, and the content of the metal derived from the fatty acid metal salt particles externally added to the toner can be determined by taking the difference between the value of A and the value of the intercept of the approximate line. The metal content thus measured is used as the metal that is the main component of the fatty acid metal salt, such as metal stearate, to determine the fatty acid metal salt particle content (g) in the toner. Specifically, the measured content (g) is divided by the molecular weight of the fatty acid metal salt identified by the fatty acid metal salt particle identification method described above to convert it into the content (mol). The content b (mol / g) of the fatty acid metal salt particles in the toner is obtained by converting the obtained content (mol) into an amount based on the toner mass (g). In addition, a / b is calculated using the values ​​of a and b obtained above.

[0071] <Identification of release agent in toner> (1) Method for separating release agent from toner First, the melting point of the release agent in the toner is measured using a thermal analyzer (DSC Q2000, manufactured by TA Instruments Japan, Inc.). Put 3.0 mg of the toner sample into a sample container in an aluminum pan (KIT NO. 0219-0041), place the sample container on a holder unit, and set it in an electric furnace. In a nitrogen atmosphere, heat from 30°C to 200°C at a temperature increase rate of 10°C / min, measure the DSC curve with a differential scanning calorimeter (DSC), and calculate the melting point of the release agent in the toner sample. Next, the toner is dispersed in ethanol, which is a poor solvent for the toner, and the temperature is raised to a temperature above the melting point of the release agent. At this time, pressure may be applied if necessary. This operation melts the release agent, which has exceeded its melting point, and it is extracted into the ethanol. The release agent can be separated from the toner by heating and, if pressure is applied, by performing solid-liquid separation while still under pressure. Next, the extracted liquid is dried and solidified to obtain the release agent.

[0072] (2) Identification of release agents by pyrolysis GCMS The specific conditions for identifying the release agent by pyrolysis GCMS are shown below. Mass spectrometer: ThermoFisherScinetific ISQ GC equipment: ThermoFisher Scientific FocusGC Ion source temperature: 250℃ Ionization method: EI Mass range: 50-1000m / z Column: HP-5MS [30m] Pyrolysis equipment: Japan Analytical Industry Co., Ltd. JPS-700

[0073] The release agent separated by the extraction operation is added to tetramethylammonium hydroxide (TMAH) at 1 mass% to prepare a measurement sample on a 590°C pyrofoil. Pyrolysis GCMS measurement is performed on 1 μL of the prepared sample under the above conditions to obtain a peak derived from the release agent. When the release agent is an ester compound, peaks are obtained for the alcohol component and the carboxylic acid component. The alcohol component and the carboxylic acid component are detected as methylated products due to the action of the methylating agent TMAH. The obtained peaks can be analyzed to identify the structure of the release agent. Furthermore, by identifying the structure of the release agent, the molecular weight of the release agent can also be obtained. When the release agent has a molecular weight distribution, such as a hydrocarbon wax, the component that is most frequently detected is taken as the molecular weight of the wax.

[0074] <Melt point measurement method> The melting point of a crystalline material (a release agent such as a crystalline resin or wax) is measured under the following conditions using a differential scanning calorimeter (DSC) Q2000 (manufactured by TA Instruments). Heating rate: 10℃ / min Measurement start temperature: 20℃ End of measurement temperature: 180℃ The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction. Specifically, 5 mg of the sample is weighed out and placed in an aluminum pan, and a measurement is performed once. An empty aluminum pan is used as a reference. The peak temperature of the maximum endothermic peak at that time is taken as the melting point.

[0075] <Method for measuring the glass transition temperature (Tg) of binder resin> The glass transition temperature (Tg) of the binder resin is measured using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments) in accordance with ASTM D3418-82. The melting points of indium and zinc are used for temperature correction of the device detection unit, and the heat of fusion of indium is used for heat correction. Specifically, 5 mg of binder resin is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference. The measurement range is 30 to 200°C, and the temperature rise rate is 1°C / min. During this temperature rise process, the specific heat change is obtained in the temperature range of 40°C to 100°C. The intersection point between the line at the midpoint of the baseline before and after the specific heat change appears and the differential heat curve is taken as the glass transition temperature (Tg) of the binder resin.

[0076] <Method for measuring average circularity> The average circularity of the toner and toner particles is measured and analyzed under the following conditions using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation). The specific measurement method is as follows. First, 20 mL of ion-exchanged water from which solids and other impurities have been removed is placed in a glass container. 0.2 mL of a solution prepared by diluting "Contaminon N" (a 10% by weight aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water is added as a dispersant. 0.02 g of the measurement sample is then added, and the solution is dispersed in an ultrasonic disperser. The dispersion is cooled appropriately so that the temperature of the dispersion is 10 to 40°C. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser ("VS-150" (manufactured by Velvoclear)) with an oscillation frequency of 50 kHz and an electrical output of 150 W was used. A predetermined amount of ion-exchanged water was placed in the water tank, and approximately 2 mL of the Contaminon N was added to the water tank. For the measurement, the flow type particle image analyzer equipped with "UPlanApro" (magnification 10x, numerical aperture 0.40) as the objective lens is used, and particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid.

[0077] The dispersion liquid prepared according to the above procedure is introduced into the flow type particle image analyzer, and 3000 toner particles are measured in HPF measurement mode and total count mode.Then, the binarization threshold during particle analysis is set to 85%, and the analyzed particle diameter is limited to a circle equivalent diameter of 1.985 μm or more and less than 39.69 μm, and the average circularity of the toner particles is obtained. Before starting the measurement, automatic focus adjustment is performed using standard latex particles (Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water).

[0078] <Method of measuring weight average particle size (D4)> The weight average particle diameter (D4) of the toner or toner particles (hereinafter, also referred to as toner, etc.) is calculated as follows. The measuring device used is a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000 channels. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1.0%, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter, Inc.). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0079] The specific measurement method is as follows. (1) Pour 200.0 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "Aperture tube flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Place 30.0 mL of the electrolyte solution in a 100 mL flat-bottom glass beaker. Add 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water as a dispersant. (3) Two oscillators with an oscillation frequency of 50 kHz are built in with a phase difference of 180 degrees. Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) with an electric power of 120 W. Place 3.3 L of ion-exchanged water in the water tank of the ultrasonic disperser, and add 2.0 mL of Contaminon N to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is being irradiated with ultrasonic waves, 10 mg of toner or the like is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted so that it is between 10°C and 40°C. (6) Using a pipette, drip the electrolytic solution (5) in which the toner or the like has been dispersed into the round-bottom beaker (1) placed in the sample stand to adjust the measurement concentration to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) Analyze the measurement data using the dedicated software that comes with the device to calculate the weight-average particle size (D4). Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).

[0080] <Measurement of the median particle size of fatty acid metal salts> The volume-based median diameter of fatty acid metal salt particles is measured in accordance with JIS Z8825-1 (2001), specifically as follows. The measurement device used is a laser diffraction / scattering particle size distribution analyzer "LA-920" (manufactured by HORIBA, Ltd.). The measurement conditions are set and the measurement data is analyzed using the dedicated software "HORIBA LA-920 for Windows (registered trademark) WET (LA-920) Ver. 2.02" that comes with the LA-920. The measurement solvent is ion-exchanged water from which impurities such as solids have been removed in advance.

[0081] The measurement procedure is as follows. (1) Attach the batch type cell holder to the LA-920. (2) A specified amount of ion-exchanged water is placed in a batch cell, and the batch cell is set in the batch cell holder. (3) Stir inside the batch cell using a dedicated stirrer tip. (4) Click the "Refractive Index" button on the "Display Condition Setting" screen and select the file "110A000I" (relative refractive index 1.10). (5) On the "Display Condition Setting" screen, set the particle size standard to the volume standard. (6) After warming up for at least one hour, adjust the optical axis, fine-tune the optical axis, and perform a blank measurement. (7) About 60 ml of ion-exchanged water is placed in a 100 ml flat-bottom glass beaker, and about 0.3 ml of a solution obtained by diluting "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made from a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) about 3 times by weight with ion-exchanged water is added as a dispersant. (8) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetora 150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add approximately 2 ml of Contaminon N to this tank. (9) The beaker of (7) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the aqueous solution in the beaker is maximized. (10) About 1 mg of fatty acid was added to the aqueous solution in the beaker of (9) while irradiating it with ultrasound. Metal salt particles are added little by little to the aqueous solution in the beaker and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. Note that during this process, the fatty acid metal salt may form lumps and float on the surface of the liquid. In this case, the lumps are submerged in the water by shaking the beaker, and ultrasonic dispersion is then continued for 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be between 10°C and 40°C. (11) The aqueous solution in which the fatty acid metal salt particles prepared in (10) are dispersed is immediately added to the batch cell in small amounts while being careful not to introduce air bubbles, and the transmittance of the tungsten lamp is adjusted to 90% to 95%. Then, the particle size distribution is measured. The 50% cumulative diameter is calculated based on the obtained volume-based particle size distribution data.

[0082] <Identification and quantification of binder resin> A pyrolysis gas chromatography mass spectrometer (hereinafter also referred to as "pyrolysis GC / MS") and NMR are used to identify the type and ratio of monomer units in the binder resin. Pyrolysis GC / MS is used to analyze the types of constituent compounds of the resin. The type of monomer unit is identified by analyzing the mass spectrum of the components of the resin decomposition products generated when the resin is pyrolyzed at 550°C to 700°C. The specific measurement conditions are as follows:

[0083] (Measurement conditions for pyrolysis GC / MS) Pyrolysis device: JPS-700 (Japan Analysis Industry) Decomposition temperature: 590℃ GC / MS equipment: Focus GC / ISQ (Thermo Fisher) Column: HP-5MS, length 60 m, inner diameter 0.25 mm, film thickness 0.25 μm Inlet temperature: 200℃ Flow pressure: 100kPa Split: 50mL / min MS ionization: EI Ion source temperature: 200℃ Mass Range 45-650 Next, the ratio of the monomer units of the identified binder resin is 1 The structure was determined using a FT-NMR apparatus JNM-EX400 (manufactured by JEOL Ltd.) 1 H-NMR 400 MHz, CDCl3, room temperature (25 °C)].

[0084] ( 1 H-NMR measurement conditions) Measurement frequency: 400MHz Pulse condition: 5.0μs Frequency range: 10500Hz Number of times of accumulation: 1024 times Measurement temperature: 25℃ Sample: 50 mg of the measurement sample is placed in a sample tube with an inner diameter of 5 mm, deuterated chloroform (CDCl3) is added as a solvent, and this is dissolved in a constant temperature bath at 40°C to prepare the sample. The molar ratio of each monomer unit is determined from the integral value of the obtained spectrum, and the ratio (mass %) of each monomer unit is calculated based on this.

[0085] <Method of measuring peak molecular weight (Mp)> The peak molecular weight (Mp) of the binder resin is measured using gel permeation chromatography (GPC) as follows. First, the sample to be measured is dissolved in tetrahydrofuran (THF) at room temperature. If it is difficult to dissolve, heat it to a temperature of 35°C or less. The obtained solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: High-speed GPC equipment "HLC-8220GPC" [Tosoh Corporation] Column: 2 columns of LF-604 [Showa Denko Co., Ltd.] Eluent:THF Flow rate: 0.6mL / min Oven temperature: 40℃ Sample injection volume: 0.020mL In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (product names: "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used. EXAMPLES

[0086] The present disclosure will be specifically described with reference to the following examples. However, these are not intended to limit the present disclosure in any way. "Parts" and "%" are all by mass unless otherwise specified.

[0087] [Production example of polyester resin] <Polyester resin 1> Fumaric acid: 10.6 parts (23 mol%) Terephthalic acid: 8.5 parts (13 mol%) Trimellitic acid: 3.3 parts (4 mol%) Bisphenol A-ethylene oxide 2-mol adduct: 47.6 parts (38 mol%) Bisphenol A-propylene oxide 2-mol adduct: 30.0 parts (22 mol%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted under a reduced pressure of 60 to 70 mmHg until the peak molecular weight reached 6,000, thereby obtaining amorphous polyester resin 1. The acid value of the obtained polyester resin 1 was 20.3 mgKOH / g, the peak molecular weight (Mp) was 6000, the glass transition temperature was 54.6°C, and the solubility parameter was 21.01 ((J / cm 3 ) 1 / 2 ) was.

[0088] <Polyester resin 2> Terephthalic acid: 22.6 parts (36 mol%) Trimellitic acid: 3.2 parts (4 mol%) Bisphenol A-ethylene oxide 2-mol adduct: 45.5 parts (38 mol%) Bisphenol A-propylene oxide 2-mol adduct: 28.7 parts (22 mol%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted for 1 hour under a reduced pressure of 60 to 70 mmHg to obtain amorphous polyester resin 2. The acid value of the obtained polyester resin 1 was 20.1 mgKOH / g, the peak molecular weight (Mp) was 6000, the glass transition temperature was 59.4°C, and the solubility parameter was 21.28 ((J / cm 3 ) 1 / 2 ) was.

[0089] <Polyester resin 3> Amorphous polyester resin 3 was prepared in the same manner as in the preparation example of polyester resin 1, except that the reaction was continued until the peak molecular weight reached 12,000. obtained. The acid value of the obtained polyester resin 3 was 12.2 mgKOH / g, the peak molecular weight (Mp) was 12,000, the glass transition temperature was 55.2°C, and the solubility parameter was 21.01 ((J / cm 3 ) 1 / 2 ) was.

[0090] [Example of resin particle dispersion production] <Resin particle dispersion 1> 1,200 parts polyester resin -Ion-exchanged water 500 parts Fumaric acid 0.250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath to melt, and 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise, and emulsified and dispersed while stirring at 7800 rpm to obtain resin particle dispersion 1. The solid content concentration of resin particle dispersion 1 was 20%. The particle size distribution of the polyester resin 1 particles contained in the resin particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.). The number average particle size of the polyester resin 1 particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0091] <Resin particle dispersion 2~11> Resin particle dispersions 2 to 11 were produced in the same manner as in Production Example of Resin Particle Dispersion 1, except that the resin used and the amount of fumaric acid added were changed to those shown in Table 1. However, in Resin Particle Dispersion 9, fumaric acid was not added, and maleic acid was added in the amount shown in Table 1. In any case, coarse particles exceeding 1 μm were not observed. The number average particle size of the polyester resin particles in Resin Particle Dispersions 2 to 11 is also shown in Table 1.

[0092] <Resin particle dispersion 12> A resin particle dispersion 12 in which a vinyl resin 1 was dispersed was produced by the emulsion aggregation method as described below. 78.0 parts of styrene and 22.0 parts of butyl acrylate were placed in a stainless steel container and mixed. An aqueous solution of 4.0 parts of sodium dodecylbenzenesulfonate mixed with 150 parts of ion-exchanged water was added to this solution and dispersed. An aqueous solution of 0.3 parts of potassium persulfate mixed with 10 parts of ion-exchanged water was added while slowly stirring for 10 minutes. After the stainless steel container was replaced with nitrogen, emulsion polymerization was performed at 70°C for 6 hours. After the polymerization was completed, the reaction solution was cooled to room temperature and ion-exchanged water was added to adjust the solid content concentration to 20.0% by mass. The particle size distribution of resin particle dispersion 12 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the particles of vinyl resin 1 was 0.25 μm, and no coarse particles exceeding 1 μm were observed. Vinyl resin 1 was separated from resin particle dispersion 11, and the physical properties of vinyl resin 1 were measured, and the acid value was 0.0 (mgKOH / g), the peak molecular weight was 20,000, and the glass transition temperature was 54.0° C. [Table 1] In the table, (maleic acid) indicates that no fumaric acid was added, but maleic acid was added in the amount shown in the table.

[0093] [Example of wax particle dispersion production] <Wax particle dispersion 1> -500 parts deionized water Wax (FNP0090 (manufactured by Nippon Seiro Co., Ltd.): Hydrocarbon wax produced by the Fischer-Tropsch method, melting point 90°C, molecular weight 771, solubility parameter: 17.16 (J / cm 3 ) 1 / 2 ) 200 copies The above materials were placed in a stainless steel container, heated to 95°C in a hot bath and melted, and 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 295 parts of ion-exchanged water was gradually added dropwise, and emulsified and dispersed while stirring at 7800 rpm to obtain wax particle dispersion 1. The solids concentration of wax particle dispersion 1 was 20%. The particle size distribution of the wax particles contained in wax particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the wax particles was 0.35 μm, and no coarse particles exceeding 1 μm were observed.

[0094] <Wax particle dispersions 2-6> Wax particle dispersions 2 to 6 were produced in the same manner as in Production Example of Wax Particle Dispersion 1, except that the wax used in Production Example of Wax Particle Dispersion 1 was changed to that shown in Table 2. [Table 2]

[0095] <Production Example of Colorant Particle Dispersion> Carbon black (Nipex35: Orion Engineered Carbons) 100 parts Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above materials were mixed and dispersed using a sand grinder mill to obtain a colorant particle dispersion. The solid content of the colorant particle dispersion was 20%. The particle size distribution of the colorant particles contained in this colorant particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0096] [Toner particle manufacturing example] <Toner particle 1> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 1 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion 1, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 1 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.960.

[0097] <Toner particles 2 to 18> Toner particles 2 to 18 were produced in the same manner as in the production example of toner particles 1, except that the resin particle dispersion and wax particle dispersion used in the production example of toner particles 1 were changed to those shown in Table 3.

[0098] <Toner particles 19> A ground toner was produced by the following method. Polyester resin 1: 100.0 parts Fumaric acid: 0.125 parts Release agent (FNP0090): 5.0 parts Colorant: Nipex35 (Orion Engineered Carbons carbon black) 5.0 copies The above materials were premixed in a Henschel mixer FM10C (Nippon Coke Engineering Co., Ltd. (formerly Mitsui Miike Chemical Engineering Co., Ltd.)), and then melt-kneaded using a twin-screw kneader (Ikegai Iron Works, Ltd., PCM-30 model) to obtain a kneaded mixture. The kneaded mixture was cooled, coarsely pulverized using a hammer mill (Hosokawa Micron Corporation), and then pulverized using a mechanical pulverizer (Turbo Kogyo, T-250) to obtain a finely pulverized powder. The finely pulverized powder was classified using a multi-division classifier (Nitetsu Mining Co., Ltd., EJ-L-3 model) that utilizes the Coanda effect, and toner particles 19 with a weight average particle size (D4) of 6.9 μm and an average circularity of 0.940 were obtained. [Table 3]

[0099] [Example of production of fatty acid metal salt particles] <Fatty acid metal salt particles 1> A receiving vessel equipped with an agitator was prepared, and the agitator was rotated at 350 rpm. 500 parts of 0.5% by mass sodium stearate aqueous solution was charged into the receiving vessel as a fatty acid source, and the liquid temperature was adjusted to 85°C. Next, 525 parts of 0.2% by mass zinc sulfate aqueous solution was dropped into the receiving vessel as a metal source over 15 minutes. After the entire amount was charged, the mixture was aged for 10 minutes at the reaction temperature to terminate the reaction. Next, the fatty acid metal salt slurry thus obtained was filtered and washed. The fatty acid metal salt cake obtained after washing was crushed roughly, and then dried at 105°C using a continuous instantaneous airflow dryer. Then, it was pulverized in a nano grinding mill [NJ-300] (manufactured by Sunrex Co., Ltd.) under conditions of an air volume of 6.0 m3 / min and a processing speed of 80 kg / h, and then reslurried and fine particles and coarse particles were removed using a wet centrifugal classifier. Then, it was dried at 80°C using a continuous instantaneous airflow dryer to obtain fatty acid metal salt particles 1. The median diameter (D50s) of the obtained fatty acid metal salt particles 1 on a volume basis was 0.45 μm.

[0100] <Fatty acid metal salt particles 2-8> Fatty acid metal salt particles 2 to 8 were produced in the same manner as in the fatty acid metal salt particle 1 production example, except that the fatty acid source and metal source in the fatty acid metal salt particle 1 production example were changed to those shown in Table 4. [Table 4]

[0101] [Toner manufacturing example] <Toner 1> Toner particles 1 100.0 parts 0.200 parts fatty acid metal salt particles 1 Silica particles (RX200: primary average particle size 12 nm, HMDS treatment, Nippon Aerosil Co., Ltd.) 1.5 parts The above materials were mixed by external addition using FM10C (manufactured by Nippon Coke & Engineering Co., Ltd.). The external addition conditions were as follows: the lower blade was set to A0 blade, the distance to the deflector wall was set to 20 mm, the amount of toner particles charged was 2.0 kg, and the rotation speed was 66.6 s. -1The external addition was performed for 10 minutes with cooling water at a temperature of 20° C. and a flow rate of 10 L / min. Thereafter, the mixture was sieved through a mesh having an opening of 37 μm to obtain Toner 1. The physical properties of Toner 1 thus obtained are shown in Tables 6 and 7.

[0102] <Toner 2-32> Toners 2 to 32 were produced in the same manner as in Production Example of Toner 1, except that in Production Example of Toner 1, the toner particles and fatty acid metal salt particles were changed to those shown in Table 5, and the amount of fatty acid metal salt particles was changed as shown in Table 5. The physical properties of the obtained Toners 2 to 32 are shown in Tables 6 and 7. [Table 5] [Table 6] In the table, a indicates the content (mol / g) of fumaric acid in the toner, and b indicates the content (mol / g) of fatty acid metal salt particles in the toner. For example, 8.62E-06 is 8.62×10 -6 Shows. [Table 7] In the table, "PES-containing" indicates the presence or absence of polyester resin in the binder resin, "Y" indicates that the binder resin contains polyester resin, and "N" indicates that the binder resin does not contain polyester resin. In addition, ΔSPpw indicates the difference between the solubility parameter SPp of the polyester resin and the solubility parameter SPw of the release agent, ΔSPfw indicates the difference between the solubility parameters SPf and SPw of the fatty acid metal salt, and the peak molecular weight indicates the peak molecular weight of the binder resin.

[0103] [Examples 1 to 27, Comparative Examples 1 to 5] The following evaluations were carried out using the above toners 1 to 32. The evaluation results are shown in Table 8.

[0104] The evaluation methods and evaluation criteria of the present disclosure are described below. The image forming apparatus used was a commercially available laser printer LBP-712Ci (Canon) modified to have a process speed of 200 mm / sec, and a commercially available process cartridge, toner cartridge 040H (black) (Canon). The product toner was removed from the inside of the cartridge, and after cleaning with an air blower, 165 g of the toner to be evaluated was filled. The product toner was removed from each of the yellow, magenta, and cyan stations, and the evaluation was performed by inserting a yellow cartridge, magenta cartridge, and cyan cartridge with the toner remaining amount detection mechanism disabled. In a normal temperature and humidity environment (25°C / 50% RH, hereafter referred to as N / N environment), BROCHURE PAPER 150g GLOSSY paper (HP: 150g / m 2 ) with a toner loading of 0.50 g / cm 2 Ten solid black images were printed.

[0105] (Image abrasion resistance and image gloss after abrasion) Of the obtained solid black images, the tenth sample was rubbed ten times with a rubbing tester at five points on the image (top left, top right, center, bottom left, and bottom right) with a load of 7.35 kPa, and it was confirmed that the image density did not change before and after rubbing. The same sample was then rubbed another 100 times with the rubbing tester, and the rub resistance of the image was confirmed from the change in density before and after rubbing. The image density was measured using a color reflection densitometer X-RITE 404A (manufactured by X-Rite Co.) to measure the relative density of the printout image of the white background part with an original density of 0.00, and the reduction rate of the image density after rubbing with respect to the image density before rubbing was calculated. The evaluation criteria were as follows. In addition, the gloss of the image after rubbing was measured using a handy gloss meter PG-3D (manufactured by Nippon Denshoku Industries Co., Ltd.) at a light incidence angle of 75°. The evaluation criteria were as follows. In this test, the image was sufficiently fixed on the paper because the density did not change before and after 10 rubbings. Therefore, if the density decreased after 100 rubbings, it was determined that image loss had occurred due to a decrease in the slipperiness of the image surface.

[0106] (Image abrasion resistance) [Evaluation Criteria] A: Concentration reduction rate is less than 1% B: Concentration reduction rate is 1% or more but less than 3% C: Concentration reduction rate is 3% or more but less than 10% D: Concentration decrease rate is 10% or more <Gloss of the image after rubbing> [Evaluation Criteria] A: Image gloss is 70 or more B: Image gloss is between 60 and 70 C: Image gloss is between 50 and 60 D: Image gloss is less than 50

[0107] <Heat resistance of image> Of the obtained solid black images, the 8th sample and the 9th sample were stacked so that the image surfaces were in contact, and a load of 7.35 kPa was applied and left to stand at 50°C for 24 hours. The heat resistance of the images was evaluated based on the state of adhesion after standing. The evaluation criteria were as follows. [Evaluation Criteria] A: No sticking is observed B: There is a slight adhesion, but no trace is left when removed. C: Sticking is observed, and when peeled off, there is a small amount of image loss. D: The sticker is noticeably stuck, and when peeled off, the image is noticeably missing.

[0108] (Image taping resistance) Of the obtained solid black images, Mylar tape (manufactured by Nitto Denko Corporation) was applied to the center of the image of the seventh sample with a load of 7.35 kPa. The applied tape was then slowly peeled off, and the image's taping resistance was evaluated based on the state of image loss using the following criteria. The evaluation criteria were as follows. High taping resistance of the image indicates high strength of the image surface. [Evaluation Criteria] A: The tape is not sticking. B: The image sticks slightly to the tape, but the image is not lost. C: The image is slightly missing. D: Image loss is noticeable

[0109] Image density and image density unevenness The image forming apparatus was left in a high temperature and high humidity environment (30°C / 80% RH, hereinafter also referred to as H / H environment) for 24 hours. After that, in the H / H environment, a Canon color laser copier paper (A4: 81.4 g / m 2 ) with a toner load of 0.50g / cm 2 A solid black image with a print rate of 1% was output on one sheet, which was used as an initial image sample. Then, 5,000 sheets of horizontal line images with a print rate of 1% were output continuously. Then, immediately after the 5,000 sheets were output continuously, and after the 5,000 sheets were output continuously and left for 60 hours, the toner amount was measured. 2 Solid black image printed on Canon Color Laser Copier Paper (A4: 81.4g / m 2 ) one sheet each was printed. The density of the obtained images was measured, and the rate of change in density relative to the initial image sample was confirmed. The sample with the largest rate of change between the sample immediately after 5,000 continuous prints and the sample left stationary for 60 hours after 5,000 continuous prints was regarded as the image density change rate of the sample, and was evaluated according to the following criteria. Furthermore, for the initial image sample, the image density was measured at five points on the same image, and the change in image density from the point with the lowest image density to the point with the highest image density was evaluated as image density unevenness according to the following criteria: Specifically, the five measurement points were point A 3 cm from the left edge and 3 cm from the top edge of the image, point B 3 cm from the left edge and 3 cm from the bottom edge of the image, point C 3 cm from the right edge and 3 cm from the top edge of the image, point D 3 cm from the right edge and 3 cm from the bottom edge of the image, and point E in the center of the image.

[0110] Image Density [Evaluation Criteria] A: Image density change is less than 3% B: Image density change is 3% or more but less than 5% C: Image density change is 5% or more but less than 10% D: Image density change is 10% or more (Image Density Unevenness) [Evaluation Criteria] A: Image density change is less than 3% B: Image density change is 3% or more but less than 5% C: Image density change is 5% or more but less than 10% D: Image density change is 10% or more

[0111] <Charging roller contamination> The image forming apparatus was left in a low temperature and low humidity environment (15°C / 10% RH, hereinafter also referred to as L / L environment) for 24 hours. After that, in the L / L environment, Canon color laser copier paper (A4: 81.4 g / m 2 ), a horizontal line image with a print rate of 1% was printed on 5,000 sheets in succession. Then, Canon Color Laser Copier Paper (A4: 81.4 g / m 2 ) with a toner load of 0.20 g / cm 2 After that, the cartridge was disassembled and the surface of the charging roller (charging member) was observed. [Evaluation Criteria] A: No streaks are visible on the charged member. B: Slight streaks are visible on the charged member, but no streaks are visible on the image. C: Streaks are visible on the charged member, and slight streaks are also visible on the image. D: Streaks are clearly visible on the image. [Table 8]

[0112] The present disclosure relates to the following configurations. (Configuration 1) A toner having toner particles containing a binder resin and an external additive, the external additive comprises particles of a fatty acid metal salt; The toner contains fumaric acid, The content of the fumaric acid in the toner is represented by a (mol / g), When the content of the fatty acid metal salt particles in the toner is b (mol / g), A toner characterized by satisfying the following formula (1): 0.50≦a / b≦70.00 (1) (Configuration 2) The toner according to embodiment 1, which satisfies the following formula (2): 1.20≦a / b≦70.00 (2) (Configuration 3) The toner according to configuration 2, which satisfies the following formula (3): 1.50≦a / b≦70.00 (3) (Configuration 4) The content a (mol / g) of the fumaric acid in the toner is 8.60×10 -7 ~1.05×10 -5 4. The toner according to any one of configurations 1 to 3, wherein the molecular weight is 1 / mol / g. (Configuration 5) The content b (mol / g) of the fatty acid metal salt particles in the toner is 1.55×10 -7 ~7.90×10 -6 5. The toner according to any one of configurations 1 to 4, wherein the molecular weight is 1 / mol / g. (Configuration 6) The fatty acid metal salt is a metal salt of a saturated fatty acid having 12 to 22 carbon atoms. The toner according to any one of the preceding claims. (Configuration 7) 7. The toner according to configuration 6, wherein the fatty acid metal salt is a metal salt of stearic acid. (Configuration 8) The toner according to any one of configurations 1 to 7, wherein the fatty acid metal salt is a zinc salt. (Configuration 9) 9. The toner according to claim 8, wherein the fatty acid metal salt is zinc stearate. (Configuration 10) The toner according to any one of configurations 1 to 9, wherein the toner particles contain a release agent. (Configuration 11) 11. The toner according to embodiment 10, wherein the release agent has a melting point of 70 to 120° C. (Configuration 12) 12. The toner according to claim 11, wherein the release agent has a melting point of 80 to 120° C. (Configuration 13) 13. The toner according to any one of configurations 1 to 12, wherein the binder resin contains a polyester resin. (Configuration 14) the toner particles contain a release agent, The solubility parameter of the polyester resin is SPp((J / cm 3 ) 1 / 2 ), and the solubility parameter of the release agent is SPw((J / cm 3 ) 1 / 2 ) and the difference between SPp and SPw is ΔSPpw, The product of the square of the ΔSPpw and the molecular weight of the release agent is 10000.00 (J / cm 3 14. The toner according to claim 13, wherein (Configuration 15) The solubility parameter of the fatty acid metal salt is SPf((J / cm 3 ) 1 / 2 ), and the solubility parameter of the release agent is SPw((J / cm 3 ) 1 / 2 ) and the difference between SPf and SPw is ΔSPfw, 15. The toner according to any one of configurations 10 to 14, wherein the ΔSPfw is 0.20 to 1.60. (Configuration 16) 15. The toner according to any one of configurations 1 to 14, wherein the binder resin has a peak molecular weight (Mp) of 5,000 to 10,000.

Claims

1. A toner having toner particles containing a binder resin and an external additive, the external additive comprises particles of a fatty acid metal salt; The toner contains fumaric acid, The content of the fumaric acid in the toner is represented by a (mol / g), When the content of the fatty acid metal salt particles in the toner is b (mol / g), A toner characterized by satisfying the following formula (1): 0.50≦a / b≦70.00 (1)

2. The toner according to claim 1 , which satisfies the following formula (2): 1.20≦a / b≦70.00 (2)

3. The toner according to claim 2 , which satisfies the following formula (3): 1.50≦a / b≦70.00 (3)

4. The content a (mol / g) of the fumaric acid in the toner is 8.60×10 -7 ~1.05 x 10 -5 4. The toner according to claim 1, wherein the toner has a molecular weight of 1.0 to 1.0 mol / g.

5. The content b (mol / g) of the fatty acid metal salt particles in the toner is 1.55×10 -7 ~7.90 x 10 -6 4. The toner according to claim 1, wherein the toner has a molecular weight of 1.0 to 1.0 mol / g.

6. 4. The toner according to claim 1, wherein the fatty acid metal salt is a metal salt of a saturated fatty acid having 12 to 22 carbon atoms.

7. 7. The toner according to claim 6, wherein the fatty acid metal salt is a metal salt of stearic acid.

8. 4. The toner according to claim 1, wherein the fatty acid metal salt is a zinc salt.

9. 9. The toner of claim 8, wherein the fatty acid metal salt is zinc stearate.

10. The toner according to any one of claims 1 to 3, wherein the toner particles contain a release agent.

11. The toner according to claim 10, wherein the release agent has a melting point of 70 to 120°C.

12. The toner according to claim 11, wherein the release agent has a melting point of 80 to 120°C.

13. The toner according to any one of claims 1 to 3, wherein the binder resin contains a polyester resin.

14. the toner particles contain a release agent, The solubility parameter of the polyester resin is SPp ((J / cm 3 ) 1/2 ), and the solubility parameter of the release agent is SPw ((J / cm 3 ) 1/2 ) and the difference between SPp and SPw is ΔSPpw, The product of the square of the ΔSPpw and the molecular weight of the release agent is 10000.00 (J / cm 3 14. The toner according to claim 13, wherein the toner is at least 100% by weight.

15. The solubility parameter of the fatty acid metal salt is SPf ((J / cm 3 ) 1/2 ), and the solubility parameter of the release agent is SPw ((J / cm 3 ) 1/2 ) between SPf and SPw When the difference is ΔSPfw, 11. The toner according to claim 10, wherein the ΔSPfw is from 0.20 to 1.

60.

16. 4. The toner according to claim 1, wherein the binder resin has a peak molecular weight (Mp) of 5,000 to 10,000.

Citation Information

Patent Citations

  • Toner, developer, process cartridge, and image forming apparatus

    JP2016173396A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2022052627A