Toner, process cartridge, and electrophotographic image forming apparatus

The toner composition with carbon black, polyester resin, fumaric acid, and hydrotalcite particles addresses charge stability issues in high-temperature, high-humidity environments, ensuring consistent image quality.

JP2024160767APending Publication Date: 2024-11-15CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023076085
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing toners struggle to maintain stable charge build-up properties in high-temperature, high-humidity environments, leading to inconsistent image quality in copying machines and printers.

Method used

A toner composition comprising toner particles with carbon black and polyester resin, resin particles with specific brightness and size ranges, and the inclusion of fumaric acid, along with hydrotalcite particles as external additives, to enhance charge transfer and stability.

Benefits of technology

The toner achieves excellent charge build-up properties and stable image quality even in challenging environmental conditions, improving charging start-up and reducing density variations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160767000008
    Figure 2024160767000008
  • Figure 2024160767000009
    Figure 2024160767000009
  • Figure 2024160767000001
    Figure 2024160767000001
Patent Text Reader

Abstract

To provide a toner that has an excellent charging start-up property even in a high temperature and high humidity environment, and achieves stable image quality.SOLUTION: A toner contains toner particles and resin particles. The toner particles contain carbon black and a polyester resin. The toner particles have a luminance average value of 40-80 based on monochrome 256 gradations. The resin particles contain a polyester resin. The resin particles have a luminance average value of 90-120. The toner contains fumaric acid. The resin particles have an average equivalent circle diameter of 0.5-3.0 μm. The toner particles have an average equivalent circle diameter of 4.0-10.0 μm. When the number-based content of the resin particles in 100 toner particles is defined as b in the toner, the b is 5-30. When a content of the fumaric acid in the total mass of the toner is defined as a (mass ppm) in the toner, the a is 10-1200 mass ppm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner, a process cartridge, and an electrophotographic image forming apparatus used in an image forming method such as electrophotography. [Background technology]

[0002] In recent years, copying machines and printers have become faster and have improved environmental stability, and toners are being required to be charged quickly and provide stable image quality even in environments where charging is difficult, such as high temperature and humidity environments.

[0003] In order to improve the charge rising property in this high temperature and high humidity environment, a method of incorporating a charge control agent into the toner has been considered. For example, Patent Document 1 proposes a toner using a resin containing a sulfonic acid group as a charge control resin. It is said that this method produces a toner with stable charging characteristics with little change in charge amount due to environmental changes. Also, Patent Document 2 proposes a toner using a resin containing a carboxylic acid group as a charge control resin. It is said that this method produces a toner that exhibits good charge build-up even in a high-temperature, high-humidity environment and has excellent durability and stability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 03-056974 [Patent Document 2] JP 2014-098840 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, even when the measures described in the above-mentioned documents are used, there is still room for improvement in the rise of charging in high-temperature and high-humidity environments in high-speed copying machines and printers. The present disclosure provides a toner that has excellent charge build-up properties even in a high-temperature, high-humidity environment and achieves stable image quality. The present disclosure also provides a process cartridge and an electrophotographic image forming apparatus that include the toner. [Means for solving the problem]

[0006] The present disclosure provides a toner comprising toner particles and resin particles, the toner particles contain carbon black and a polyester resin; the toner particles have an average brightness of 40 to 80 based on monochrome 256 gradations; The resin particles contain a polyester resin, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations; The toner contains fumaric acid, The average equivalent circle diameter of the resin particles is 0.5 to 3.0 μm, the toner particles have an average equivalent circular diameter of 4.0 to 10.0 μm; the content of the resin particles in the toner based on the number of the resin particles per 100 toner particles is designated as b (pieces), the b being 5 to 30 pieces; The toner relates to a toner, wherein when the content of the fumaric acid in the toner with respect to the total mass of the toner is represented as a (ppm by mass), the a is from 10 to 1200 ppm by mass. Effect of the Invention

[0007] According to the present disclosure, the toner has excellent charge build-up properties even in a high-temperature, high-humidity environment, and is stable. It is possible to provide a toner that realizes image quality. Furthermore, according to the present disclosure, it is possible to provide a process cartridge and an electrophotographic image forming apparatus that include the toner. [Brief description of the drawings]

[0008] [Figure 1] Schematic diagram of EDS line analysis in STEM-EDS mapping analysis [Diagram 2]Example of a Faraday Cage DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.

[0010] The present disclosure provides a toner comprising toner particles and resin particles, the toner particles contain carbon black and a polyester resin; the toner particles have an average brightness of 40 to 80 based on monochrome 256 gradations; The resin particles contain a polyester resin, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations; The toner contains fumaric acid, The average equivalent circle diameter of the resin particles is 0.5 to 3.0 μm, the toner particles have an average equivalent circular diameter of 4.0 to 10.0 μm; the content of the resin particles in the toner based on the number of the resin particles per 100 toner particles is designated as b (pieces), the b being 5 to 30 pieces; The toner relates to a toner, wherein when the content of the fumaric acid in the toner with respect to the total mass of the toner is represented as a (ppm by mass), the a is from 10 to 1200 ppm by mass.

[0011] The present inventors believe that the reason why the above toner has excellent charge build-up properties even in a high-temperature, high-humidity environment and can realize stable image quality is as follows. Generally, in the electrophotographic image forming method, a photoconductive material is used to form an electric latent image on an electrostatic latent image carrier by various means, and the latent image is then developed into a toner image by a developing device to make it visible. If necessary, the toner image is transferred to a transfer material such as paper, and then fixed by heat, pressure, heat and pressure, or solvent vapor to obtain a toner image.

[0012] As a developing device for such an electrophotographic method, a device is generally known that has a configuration in which a rubber or metal toner regulating blade is contacted on the surface of a developing sleeve acting as a toner carrier to regulate the toner coat amount.

[0013] The friction between the toner regulating blade and the toner and / or the friction between the toner carrier and the toner gives the toner a positive or negative charge. Furthermore, a common method is to develop the toner by causing the toner carrier, on whose surface the toner is thinly applied, to fly and adhere to the electrostatic latent image on the surface of the electrostatic latent image carrier facing the toner carrier, using the toner regulating blade. The toner of the present disclosure is also preferably used in such a configuration.

[0014] In many cases, small particles, which are more susceptible to the influence of van der Waals forces than gravity, tend to adhere to the regulating blade, and the small particles that adhere to the blade retain a charge on their surface, allowing the toner particles to be quickly charged.

[0015] In the present disclosure, the toner particles have an average equivalent circular diameter of 4.0 to 10.0 μm, and the average brightness of the toner particles based on monochrome 256 gradations is 40 to 80. The toner contains resin particles having an average equivalent circular diameter of 0.5 to 3.0 μm and an average brightness of 90 to 120. The content of the resin particles in the toner is 5 to 30 per 100 toner particles.

[0016] The brightness of a toner is a value obtained by measuring the degree of light scattering of the toner using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the analytical conditions described below, and is an index representing the degree of light scattering of the toner. Generally, the brightness of a toner decreases when it contains a colorant.

[0017] When the average equivalent circle diameter of the resin particles is 3.0 μm or less, the resin particles are sufficiently small compared to the toner particles and therefore easily adhere to the regulating blade. When the average equivalent circle diameter of the resin particles is 0.5 μm or more, the resin particles can retain charge even when attached to the regulating blade. It is believed that when the average equivalent circle diameter of the resin particles is within the above range, the resin particles adhere to the regulating blade and easily transfer charge to the toner particles, as described below. As a result, it is believed that the charge rise property is improved and a decrease in density at the leading edge of the image can be suppressed. The average equivalent circular diameter of the resin particles is preferably 0.8 to 2.2 μm, and more preferably 1.0 to 2.0 μm, and the average equivalent circular diameter of the toner particles is preferably 5.0 to 9.0 μm, and more preferably 6.0 to 8.0 μm.

[0018] The average brightness value of the toner particles containing carbon black is 40 to 80. This range of brightness means that carbon black is sufficiently present in the toner particles. In contrast, the average brightness value of the resin particles is 90 to 120. The average brightness value is the average brightness value based on monochrome 256 gradations. An average brightness value of 90 or more means that there is little carbon black present in the resin particles. Since the resin particles attached to the regulating blade have a low content of conductive carbon black, it is considered that the charge is not released into the resin particles and the charge can be held on the surface of the resin particles. Therefore, it is considered that the charge is easily transferred to the toner particles, the charge rise property is improved, and the decrease in density at the tip of the image can be suppressed. The average brightness value of the resin particles is preferably 100 to 115. When the brightness average value of the toner particles exceeds 80, the amount of carbon black becomes insufficient, and the image density tends to decrease.

[0019] In addition, when the content of resin particles in the toner based on the number of particles per 100 toner particles is b (pieces) (hereinafter also referred to as the content b), the b is 5 to 30. When the content b of resin particles is 5 or more, the start of charging can be improved, and when it is 30 or less, a decrease in image density can be prevented. The content b is preferably 9 to 27 pieces, and more preferably 12 to 18 pieces.

[0020] The toner contains fumaric acid. By using specific toner particles and resin particles that satisfy the above-mentioned average brightness value, average equivalent circle diameter, etc., and by making the toner contain fumaric acid, charge transfer from the resin particles to the toner particles occurs, and the charge rise property is improved.

[0021] In the present disclosure, when the content of fumaric acid in the toner relative to the total mass of the toner is a (ppm by mass) (hereinafter also referred to as the content a), a must be 10 to 1200 ppm by mass. Since fumaric acid has a conjugated system and is highly hydrophobic, when the content a is 10 ppm by mass or more, the charge can be transferred from the resin particles attached to the regulating blade surface to the toner particles even in a high-temperature and high-humidity environment. In addition, when the content a is 1200 ppm by mass or less, it is possible to prevent a decrease in the total amount of charge that is generated.

[0022] In order to further enhance the above-mentioned effects, the content a of fumaric acid is preferably from 50 to 1000 ppm by mass, and more preferably from 150 to 800 ppm by mass.

[0023] The toner particles contain a polyester resin, and the resin particles contain a polyester resin. That is, it is necessary that both the toner particles and the resin particles contain polyester resin. It is considered that the inclusion of polyester resin in the toner particles and the resin particles facilitates interaction with fumaric acid, which has a similar structure, and facilitates the transfer of electric charges between the toner particles and the resin particles. Of the resin components contained in the toner particles and resin particles, the content of the polyester resin is preferably 50 to 100% by mass, more preferably 80 to 100% by mass, and further preferably 90 to 100% by mass.

[0024] The toner preferably contains 3 to 15% by mass, and more preferably 4 to 10% by mass, of carbon black based on the mass of the toner. When the carbon black content in the toner is 3% by mass or more, the image density can be increased, and when it is 15% by mass or less, the charge amount of the toner can be increased.

[0025] In addition, it is preferable that the content a (ppm by mass) of fumaric acid in the toner and the content b (number of resin particles) per 100 toner particles satisfy the following formula (1). 2≦a / b≦120 (1)

[0026] When a / b is 2 or more, the amount of fumaric acid relative to the resin particles is sufficient, improving the charge rise. When a / b is 120 or less, the amount of resin particles relative to the fumaric acid is sufficient, improving the charge rise. The ratio a / b is more preferably 3-120, and further preferably 20-60.

[0027] When the mass-based content of fumaric acid in the toner extracted by methanol from the toner is f1 (%), the f1 is preferably 0.0001 to 0.0120%, more preferably 0.0005 to 0.0100%, even more preferably 0.0010 to 0.0090%, and even more preferably 0.0020 to 0.0084%. Methanol hardly dissolves the binder resin in the toner particles, but can dissolve the fumaric acid contained in the surface vicinity of the toner. Therefore, f1 is an index of the content of fumaric acid contained in the surface vicinity of the toner. When f1 is in the above range, charge transfer between the resin particles and the toner particles occurs more easily, and the charge rise property is more easily improved.

[0028] The toner preferably contains hydrotalcite particles as an external additive. The hydrotalcite particles may be those represented by the following structural formula (2). M 2+ y M 3+ x (OH)2A n- (x / n) ·mH2O formula (2) where 0 <x≦0.5、y=1-x、m≧0である。 M 2+ , and M 3+ represent divalent and trivalent metals, respectively. M 2+ is preferably at least one divalent metal ion selected from the group consisting of Mg, Zn, Ca, Ba, Ni, Sr, Cu, and Fe. M 3+ is preferably at least one trivalent metal ion selected from the group consisting of Al, B, Ga, Fe, Co, and In. A n- is an n-valent anion, CO3 2- , O.H. - , Cl - , I - , F - , Br - , SO4 2- , HCO3 - , CH3COO- , and NO3 - These may be used alone or in combination.

[0029] Hydrotalcite particles are M 3+ At least Al is contained as M 2+ It is preferable that the A contains at least Mg. n- It is preferable that the hydrotalcite particles contain at least F. That is, it is preferable that the hydrotalcite particles contain magnesium and aluminum. It is also preferable that the hydrotalcite particles contain fluorine, aluminum and magnesium. The hydrotalcite particles, which act as a microcarrier and are positively charged, have the effect of imparting negative charging to the toner, thereby improving the rise of charging.

[0030] It is further preferred that the hydrotalcite particles contain fluorine inside. By containing fluorine inside, excessive positive charging of the hydrotalcite particles can be suppressed, and electrostatic aggregation between the hydrotalcite particles can be suppressed, while improving the rise of charging.

[0031] Specific examples of hydrotalcite particles include: Mg 4.3 Al2(OH) 12.6 CO3·mH2O, Mg 8.6 Al4(OH) 25.2 F2CO3·mH2O, Mg 12 Al4(OH) 32 Examples include F2CO3·mH2O. The hydrotalcite particles may be a solid solution containing a plurality of different elements, and may also contain a trace amount of a monovalent metal.

[0032] The ratio Mg / Al (element ratio) of the atomic concentration of magnesium to aluminum in the hydrotalcite particles, obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, is preferably 1.5 to 4.0, more preferably 1.6 to 3.8, and even more preferably 1.8 to 3.0.

[0033] The amount of fluorine in the hydrotalcite particles can be controlled by adjusting the concentration of fluorine during the production of the hydrotalcite. For example, it can be controlled by adjusting the amount of sodium fluoride added. In addition, the atomic concentration of fluorine in the hydrotalcite particles can be obtained from the main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner.

[0034] In line analysis in the STEM-EDS mapping analysis of the toner, it is preferable that fluorine and aluminum are present inside the hydrotalcite particles. By STEM-EDS, it can be confirmed that fluorine is intercalated between the layers of the layered structure of the hydrotalcite particles.

[0035] The ratio F / Al (element ratio) of the atomic concentration of fluorine to aluminum in the hydrotalcite particles, obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, is preferably 0.01 to 0.60, and more preferably 0.02 to 0.60.

[0036] By setting F / Al to 0.01 or more, aggregation of the hydrotalcite particles is suppressed, and the toner charge rise is improved. Also, by setting F / Al to 0.60 or less, excessive neutralization of the surface charge of the hydrotalcite particles is suppressed, and the charge amount can be stabilized.

[0037] From the viewpoint of stabilizing the charge property, it is preferable that the hydrotalcite particles have water in their molecules, and in formula (2), it is more preferable that 0.1 < m < 0.6.

[0038] The number average particle diameter of the primary particles of the hydrotalcite particles is preferably 50 to 1200 nm, more preferably 60 to 1000 nm, and even more preferably 100 to 800 nm.

[0039] The hydrotalcite particles may be hydrophobically treated with a surface treatment agent. As the surface treatment agent, higher fatty acids, coupling agents, esters, oils such as silicone oil can be used. Among them, higher fatty acids are preferably used, and specifically, stearic acid, oleic acid, and lauric acid are exemplified.

[0040] The content based on the mass of the hydrotalcite particles is not particularly limited, but it is preferably 0.01 to 3.00 parts by mass, more preferably 0.05 to 0.50 parts by mass, based on 100 parts by mass of the toner particles. The content of the hydrotalcite particles can be quantified using fluorescence X-ray analysis and a calibration curve prepared from a standard sample. The above content can be controlled by changing the addition amount of the hydrotalcite particles to the toner particles.

[0041] The toner particles and the resin particles need to contain a polyester resin. The toner particles contain, for example, a polyester resin as a binder resin. As the polyester resin, for example, a polycondensate of the following carboxylic acid component and alcohol component can be used. Examples of the carboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, fumaric acid, maleic acid, cyclohexanedicarboxylic acid, and trimellitic acid. Examples of the alcohol component include bisphenol A, hydrogenated bisphenol, ethylene oxide adduct of bisphenol A, propylene oxide adduct of bisphenol A, glycerin, trimethylolpropane, and pentaerythritol.

[0042] Among these, preferred acid monomer components include terephthalic acid, succinic acid, adipic acid, fumaric acid, trimellitic acid, pyromellitic acid, etc. Among these, preferred alcohol components include ethylene oxide adduct of bisphenol A, propylene oxide adduct of bisphenol A, glycerin, etc. In particular, it is preferred that the polyester resin contained in the resin particles contains a polyester resin having terephthalic acid and bisphenol A as its constituent elements, because the polyester resin is likely to maintain its hardness even after it is attached to the blade.

[0043] More preferably, the polyester resin is a condensation polymer of a monomer mixture containing an alkylene glycol having 2 to 12 carbon atoms, an alkylene oxide adduct of bisphenol A (the average number of moles added is preferably 1 to 5 mol), and terephthalic acid. The polyester resin is preferably an amorphous polyester resin.

[0044] The binder resin of the toner or the resin in the resin particles is not particularly limited, and known resins can be used in combination with polyester resins to the extent that the effects of the present disclosure are not impaired. Specifically, styrene-based copolymers such as polystyrene, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-octyl methacrylate copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-maleic acid copolymer, and styrene-maleic acid ester copolymer, polyacrylic acid ester, polymethacrylic acid ester, and polyvinyl acetate can be used, and a plurality of these can be used in combination.

[0045] The toner is characterized by containing resin particles having an average equivalent circular diameter of 0.5 μm to 3.0 μm and an average brightness value of 90 to 120 inclusive, within the above content b.

[0046] There is no particular restriction on the means for making the resin particles exist in the toner. For example, when toner particles are produced by a pulverization method, a suspension polymerization method, or an emulsion aggregation method, the resin particles can be present in the toner by mixing the resin particles with the toner particles before the external addition step. Preferably, the toner contains the resin particles as an external additive. That is, the toner preferably has toner particles and resin particles on the surfaces of the toner particles.

[0047] In the suspension polymerization method, it is possible to form resin particles by generating small particles that do not contain pigments, for example by increasing the rotation speed during suspension, while in the emulsion aggregation method, it is possible to form resin particles by generating small particles that do not contain pigments, for example by using a resin with a high acid value during aggregation.

[0048] The toner is characterized by containing fumaric acid. The mass-based content of fumaric acid in the toner can be measured by the method described below. The means for making the toner contain fumaric acid is not particularly limited, and known means can be used. For example, fumaric acid can be made to be contained in the toner particles. That is, it is preferable that the toner particles contain fumaric acid. For example, when producing toner particles by a pulverization method, a method can be used in which fumaric acid is incorporated into the raw material resin in advance, or fumaric acid can be added when the raw material is melted and kneaded to incorporate it into the toner particles. When toner particles are produced by a wet production method such as a suspension polymerization method or an emulsion aggregation method, a method of incorporating fumaric acid in the raw material or a method of adding fumaric acid via an aqueous medium during the production process can be used. Further, it is also possible to use a method of externally adding fumaric acid to toner particles by using a known external addition method.

[0049] The toner may contain a charge control agent. As the charge control agent, an organic metal complex compound and a chelate compound are effective, and examples thereof include monoazo metal complex compounds, acetylacetone metal complex compounds, and metal complex compounds of aromatic hydroxycarboxylic acid or aromatic dicarboxylic acid. Specific examples of commercially available products include Spilon Black TRH, T-77, and T-95 (Hodogaya Chemical Co., Ltd.), and BONTRON (registered trademark) S-34, S-44, S-54, E-84, E-88, and E-89 (Orient Chemical Co., Ltd.).

[0050] The toner particles may contain a release agent as necessary to improve fixability. The resin particles may or may not contain wax. As the release agent, a known release agent can be used. Specific examples include petroleum waxes such as paraffin wax, microcrystalline wax, petroleum waxes and derivatives thereof, montan wax and derivatives thereof, hydrocarbon waxes and derivatives thereof produced by the Fischer-Tropsch process, polyolefin waxes such as polyethylene and polypropylene and derivatives thereof, natural waxes such as carnauba wax and candelilla wax and derivatives thereof, ester waxes, etc. Here, the derivatives include oxides, block copolymers with vinyl monomers, and graft modified products. As the ester wax, in addition to monofunctional ester wax and difunctional ester wax, polyfunctional ester wax such as tetrafunctional and hexafunctional ester wax can be used.

[0051] The toner may contain, in addition to hydrotalcite, silica fine particles, inorganic external additives, etc. Examples of inorganic external additives include strontium titanate, fatty acid metal salts, alumina, and metal oxide fine particles (inorganic fine particles) such as titanium oxide, zinc oxide fine particles, cerium oxide fine particles, and calcium carbonate fine particles. As the external additive, composite oxide fine particles using two or more kinds of metals can be used, and two or more kinds selected from these fine particle groups in any combination can be used.

[0052] Furthermore, resin fine particles and organic-inorganic composite fine particles of resin fine particles and inorganic fine particles can also be used. The external additive may be hydrophobized with a hydrophobizing agent.

[0053] Examples of the hydrophobic treatment agent include chlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, phenyltrichlorosilane, diphenyldichlorosilane, t-butyldimethylchlorosilane, and vinyltrichlorosilane; Tetramethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, o-methylphenyltrimethoxysilane, p-methylphenyltrimethoxysilane, n-butyltrimethoxysilane, i-butyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, dodecyltrimethoxysilane, tetraethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, i-butyl alkoxysilanes such as ethyltriethoxysilane, decyltriethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane; silazanes such as hexaethyldisilazane, hexapropyldisilazane, hexabutyldisilazane, hexapentyldisilazane, hexahexyldisilazane, hexacyclohexyldisilazane, hexaphenyldisilazane, divinyltetramethyldisilazane, and dimethyltetravinyldisilazane; Silicone oils such as dimethyl silicone oil, methyl hydrogen silicone oil, methyl phenyl silicone oil, alkyl modified silicone oil, chloroalkyl modified silicone oil, chlorophenyl modified silicone oil, fatty acid modified silicone oil, polyether modified silicone oil, alkoxy modified silicone oil, carbinol modified silicone oil, amino modified silicone oil, fluorine modified silicone oil, and terminal reactive silicone oil; Siloxanes such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, and octamethyltrisiloxane; Examples of fatty acids and their metal salts include long-chain fatty acids such as undecylic acid, lauric acid, tridecylic acid, dodecylic acid, myristic acid, palmitic acid, pentadecylic acid, stearic acid, heptadecylic acid, arachidic acid, montanic acid, oleic acid, linoleic acid, and arachidonic acid, and salts of the above fatty acids with metals such as zinc, iron, magnesium, aluminum, calcium, sodium, and lithium.

[0054] Among these, alkoxysilanes, silazanes, and silicone oils are preferably used because they are easy to carry out hydrophobic treatment. These hydrophobic treatment agents may be used alone or in combination of two or more kinds. The content of the external additive is preferably 0.05 parts by mass or more and 20.0 parts by mass or less with respect to 100 parts by mass of the toner particles.

[0055] The method for producing the toner particles is not particularly limited, and any known method can be used. For example, a method for producing a toner directly in a hydrophilic medium, such as an emulsion aggregation method, a dissolution suspension method, or a suspension polymerization method, can be used. A pulverization method can also be used, and the toner obtained by the pulverization method can be thermally spheronized.

[0056] Hereinafter, a detailed description will be given of a method for producing toner particles by an emulsion aggregation method. (Dispersion liquid preparation process) The binder resin particle dispersion liquid is prepared, for example, as follows: For example, a polyester resin is used as the binder resin. Polyester resin and fumaric acid are mixed into an aqueous medium in which an ionic surfactant or a polymer electrolyte is dissolved. Thereafter, this solution is heated to a temperature equal to or higher than the melting point or softening point of the resin to dissolve it, and a dispersion liquid in which the binder resin particles are dispersed in the ionic surfactant is prepared using a dispersing machine with strong shear force such as a homogenizer.

[0057] When the binder resin contains a homopolymer or copolymer of a vinyl monomer (vinyl resin), the vinyl monomer is subjected to emulsion polymerization or seed polymerization in an ionic surfactant to prepare a dispersion in which vinyl resin particles are dispersed in the ionic surfactant. The means for dispersion is not particularly limited, and examples thereof include known dispersion devices such as a rotary shear homogenizer, a ball mill having media, a sand mill, and a dyno mill.

[0058] A phase inversion emulsification method may also be used as a method for preparing the dispersion liquid. In the phase inversion emulsification method, a binder resin is dissolved in an organic solvent, a neutralizer and a dispersion stabilizer are added as necessary, and an aqueous solvent is dropped under stirring to obtain emulsified particles, and then the organic solvent in the resin dispersion liquid is removed to obtain an emulsion liquid. In this case, the order of adding the neutralizer and the dispersion stabilizer may be changed. The number average particle diameter of the binder resin particles is usually 1 μm or less, and is preferably 0.01 μm to 1.00 μm. When the number average particle diameter is 1.00 μm or less, the particle size distribution of the toner finally obtained is suitable, and the generation of free particles can be suppressed. In addition, when the number average particle diameter is within the above range, uneven distribution between toner particles is reduced, dispersion in the toner is improved, and the variation in performance and reliability is reduced.

[0059] In the emulsion aggregation method, a colorant particle dispersion can be used. Carbon black is used as the colorant. The colorant particle dispersion is prepared by dispersing at least colorant particles in a dispersant. The number average particle diameter of the colorant particles is preferably 0.5 μm or less, more preferably 0.2 μm or less. When the number average particle diameter is 0.5 μm or less, diffuse reflection of visible light can be prevented, and the binder resin particles and the colorant particles can be easily aggregated in the aggregation process. When the number average particle diameter is within the above range, uneven distribution between toner particles is reduced, dispersion in the toner is improved, and variations in performance and reliability are reduced.

[0060] In the emulsion aggregation method, a wax particle dispersion can be used as necessary. The wax particle dispersion is prepared by dispersing at least wax particles in a dispersant. The number-average particle diameter of the wax particles is preferably 2.0 μm or less, more preferably 1.0 μm or less. When the number-average particle diameter is 2.0 μm or less, the wax content is less uneven between toner particles, and the image stability over a long period of time is improved. When the number-average particle diameter is within the above range, uneven distribution between toner particles is reduced, dispersion in the toner is improved, and the variation in performance and reliability is reduced.

[0061] The combination of colorant particles, binder resin particles, and wax particles is not particularly limited and can be freely selected according to the purpose. In addition to the above dispersion, other particle dispersions obtained by dispersing appropriately selected particles in a dispersant may be further mixed. The particles contained in the other particle dispersions are not particularly limited and can be appropriately selected according to the purpose, and examples thereof include internal additive particles, charge control agent particles, inorganic particles, and abrasive particles. These particles may be dispersed in the binder resin particle dispersion or the colorant particle dispersion.

[0062] Examples of dispersants contained in binder resin particle dispersions, colorant particle dispersions, wax microdispersions, and other particle dispersions include aqueous media containing polar surfactants. Examples of aqueous media include water such as distilled water and ion-exchanged water, and alcohols. These may be used alone or in combination of two or more. The content of the polar surfactant cannot be generally specified, and may be appropriately selected depending on the purpose.

[0063] Examples of polar surfactants include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; and cationic surfactants such as amine salts and quaternary ammonium salts. Specific examples of anionic surfactants include sodium dodecylbenzenesulfonate, sodium dodecylsulfate, sodium alkylnaphthalenesulfonate, and sodium dialkylsulfosuccinate. Specific examples of cationic surfactants include alkylbenzenedimethylammonium chloride, alkyltrimethylammonium chloride, and distearylammonium chloride. These may be used alone or in combination of two or more.

[0064] These polar surfactants can also be used in combination with non-polar surfactants, such as polyethylene glycol-based, alkylphenol ethylene oxide adduct-based, polyhydric alcohol-based, and other non-ionic surfactants.

[0065] The content of the colorant such as carbon black in the toner is preferably 0.1 to 30 parts by mass with respect to 100 parts by mass of the binder resin. In addition to carbon black, a known colorant may be used in combination with the toner particles. The content of the wax is preferably from 0.5 to 25 parts by mass, and more preferably from 5 to 20 parts by mass, relative to 100 parts by mass of the binder resin.

[0066] Furthermore, in order to more precisely control the chargeability of the resulting toner, charge control particles and binder resin particles may be added after the aggregated particles are formed. The particle sizes of the binder resin particles, colorant particles, and other particles are measured using a laser diffraction / scattering type particle size distribution measuring device LA-960V2 manufactured by Horiba, Ltd.

[0067] (Agglutination process) The aggregation step of forming aggregated particles is a step of forming aggregated particles containing binder resin particles, and, if necessary, colorant particles, wax particles, etc., which are added as necessary, in an aqueous medium containing binder resin particles, and, if necessary, colorant particles, wax particles, etc.

[0068] The aggregated particles can be formed in an aqueous medium by, for example, adding a pH adjuster, an aggregate agent, and a stabilizer to the aqueous medium and mixing the mixture, and then appropriately applying temperature, mechanical power, and the like. Examples of pH adjusters include alkalis such as ammonia and sodium hydroxide, and acids such as nitric acid and citric acid. Examples of flocculants include monovalent metal salts such as sodium and potassium, divalent metal salts such as calcium and magnesium, trivalent metal salts such as iron and aluminum, and alcohols such as methanol, ethanol, and propanol.

[0069] The stabilizer mainly includes a polar surfactant itself or an aqueous medium containing the same, etc. For example, when the polar surfactant contained in each particle dispersion is anionic, a cationic stabilizer can be selected.

[0070] The addition and mixing of the flocculant and the like is preferably carried out at a temperature equal to or lower than the glass transition temperature of the resin contained in the aqueous medium. When mixing is carried out under this temperature condition, the flocculation proceeds in a stable state. Mixing can be carried out using, for example, a known mixing device, homogenizer, mixer, etc. Cut.

[0071] In the aggregation step, a dispersion liquid containing a polyester resin is applied to the surface of the aggregated particles to form a coating layer (shell layer), thereby obtaining toner particles having a core / shell structure in which a shell layer is formed on the surface of the core particles. The aggregation step may be repeated several times in stages. In this case, it is preferable that the resin of the shell layer contains fumaric acid.

[0072] (fusion process) The fusion process is a process in which the obtained aggregated particles are heated and fused. Before the fusion process, a pH adjuster, a polar surfactant, a non-polar surfactant, etc. can be appropriately added to prevent fusion between toner particles. The heating temperature may be from the glass transition temperature of the resin contained in the aggregated particles (when there are two or more types of resin, the glass transition temperature of the resin having the highest glass transition temperature) to the decomposition temperature of the resin. Therefore, the heating temperature differs depending on the type of resin of the binder resin particles and cannot be generally specified, but is generally from the glass transition temperature of the resin contained in the aggregated particles to 140°C. The heating can be performed using a heating device or tool known per se.

[0073] The fusion time is short if the heating temperature is high, and long if the heating temperature is low. In other words, the fusion time depends on the heating temperature and cannot be specified in general, but it is generally between 30 minutes and 10 hours. The toner particles obtained through the above steps can be separated into solid and liquid in accordance with a known method, and the toner particles can be recovered, and then washed, dried, etc. under appropriate conditions.

[0074] The method for producing the toner preferably includes the following steps. (1) a dispersion step of preparing a dispersion of binder resin particles containing a polyester resin and binder resin fine particles containing fumaric acid; (2) an aggregation step of aggregating the binder resin fine particles (and, if necessary, colorant fine particles) contained in the binder resin fine particle dispersion to form aggregates; (3) a fusion step of heating the aggregates to fuse them together to form fused particles; The resulting fused particles can be cooled to obtain toner particles.

[0075] (External addition process) It is preferable to obtain a toner by adding resin particles, and further, if necessary, hydrotalcite particles and silica particles to the obtained toner particles. If necessary, other external additives may be added. From the viewpoint of dispersibility of the external additives, the mixing time in the external addition step is preferably adjusted to a range of 5 minutes or more and 30 minutes or less, and more preferably adjusted to a range of 8 minutes or more and 20 minutes or less. The method for producing toner particles preferably includes, for example, a step of mixing toner particles having the above average luminance value and average equivalent circular diameter with resin particles having the above average luminance value and average equivalent circular diameter.

[0076] (Method of producing resin particles) The resin particles are preferably produced by the emulsion aggregation method, as in the case of the toner particles. The binder resin particle dispersion liquid containing the polyester resin and, if necessary, the colorant particle dispersion liquid are aggregated to obtain the resin particles. The aggregation time may be controlled so that the above-mentioned average equivalent circle diameter is obtained by the same means as in the case of the production of the toner particles. The resin particles may contain a colorant. The resin particles preferably contain carbon black. The content of carbon black in the resin particles is preferably 0.01 to 0.30 parts by mass, more preferably 0.04 to 0.18 parts by mass, based on 100 parts by mass of the polyester resin. It is a department.

[0077] The toner can be used in an electrophotographic image forming apparatus or a process cartridge that is detachable from an electrophotographic image forming apparatus. Such a process cartridge and electrophotographic image forming apparatus may be any known one. The electrophotographic image forming apparatus includes a process cartridge.

[0078] For example, the process cartridge is The toner, A frame body, a cylindrical toner carrier that is rotatably supported by the frame and carries the toner; a regulating member having an abutment portion, one end of which is fixed to the frame and the other end of which is in contact with the toner carrier to form a contact nip between the toner carrier and the abutment portion; It is preferable that the regulating member is a toner regulating blade having a metal blade. The regulating member regulates the toner coat amount at the contact nip.

[0079] The toner regulating blade is preferably a metal blade because it can increase the amount of charge on the toner. More specifically, it is preferably made of a stainless steel (SUS) plate, a phosphor bronze plate, an aluminum plate, or the like.

[0080] A blade whose surface is covered with urethane rubber, urethane resin, polyamide resin, polyamide elastomer, silicone rubber, silicone resin or the like may also be used, but from the viewpoint of the amount of charge, a metal blade with an uncovered surface is more preferable.

[0081] Next, the methods for measuring the various toner properties will be described. <Method for measuring the content a of fumaric acid in toner> Dissolve 0.1 g of toner in 1 ml of chloroform. Drop 20 ml of methanol into the obtained sample solution to precipitate the resin in the solution, then remove the solids by centrifugation (HITACHI himac CR22G, 12000 rpm, 10 minutes). Remove the solvent from the obtained solution under reduced pressure, and dry for 4 hours under reduced pressure in a 60°C atmosphere. Add 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile to the obtained sample, and heat to 80°C for 1 hour to perform a silylation treatment. Analyze the obtained sample by GC-MS (gas chromatography mass spectrometry).

[0082] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0083] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is present. On the other hand, prepare several samples (e.g., 100 ng, 200 ng, 300 ng) of fumaric acid alone, and measure them under the above analytical conditions before measuring the samples obtained from the toner. After the measurement, a calibration curve is created from the amount of fumaric acid charged and the peak area value of fumaric acid. The content a (mass ppm) of fumaric acid in the toner is obtained by converting the area value of the fumaric acid component of the toner based on this calibration curve into the mass of fumaric acid, and then converting it into an amount based on the toner mass.

[0084] <Method for measuring the mass-based content f1 (mass%) of fumaric acid in toner extracted with methanol> 0.5 g of toner is placed in 20 ml of methanol and dispersed for 30 minutes. Then, solids are removed by centrifugation (HITACHI himac CR22G, 12000 rpm, 10 minutes). The solvent is removed from the resulting solution by vacuum distillation, and the solution is further dried for 4 hours under reduced pressure in a 60°C atmosphere. 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile are added to the resulting sample, which is then heated at 80°C for 1 hour to perform a silylation treatment. The resulting sample is analyzed by GC-MS (gas chromatography mass spectrometry).

[0085] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0086] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is contained. On the other hand, prepare several samples (e.g., 100 ng, 200 ng, 300 ng) of fumaric acid alone, and measure each of them under the above analytical conditions before measuring the samples. Then, create a calibration curve from the amount of fumaric acid added and the fumaric acid peak area value. The content ratio f1 (mass %) of fumaric acid in the toner that is extracted with methanol is obtained by converting the area value of the fumaric acid component of the sample based on this calibration curve into the mass of fumaric acid, and then converting it into an amount based on the toner mass.

[0087] <Measurement of average brightness and average equivalent circle diameter of toner particles and resin particles> The average brightness value and average circle equivalent diameter of the toner particles and resin particles are measured using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions during the calibration work. The brightness is based on monochrome 256 gradations (0 to 255) (brightness 0: dark, brightness 255: light). The specific measurement method is as follows. First, 20 mL of ion-exchanged water from which impurities such as solids have been removed is placed in a glass container. 0.2 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant. 0.02 g of the measurement sample is then added, and the dispersion is treated for 2 minutes using an ultrasonic disperser to obtain a dispersion for measurement. The dispersion is then appropriately cooled so that the temperature is between 10°C and 40°C. A tabletop ultrasonic cleaner disperser "VS-150" (manufactured by Vervoclear Co., Ltd.) with an oscillation frequency of 50 kHz and an electrical output of 150 W is used as the ultrasonic disperser, and a specified amount of ion exchange water is placed in the water tank. Add replacement water and add 2 mL of the above Contaminon N to this tank.

[0088] For the measurement, the flow type particle image analyzer equipped with "LUCPLFLN" (magnification 20x, numerical aperture 0.40) is used as the objective lens, and particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid. The dispersion liquid prepared according to the above procedure is introduced into the flow type particle image analyzer, and 2000 toner particles and resin particles are measured in HPF measurement mode and total count mode. From the results, the average brightness value and average circle equivalent diameter of the toner particles and resin particles are calculated.

[0089] When toner particles or resin particles are available as the measurement sample, they can be measured separately. When toner is used as the measurement sample, measurements can be made as follows. The average brightness of toner particles can be obtained by setting the range of equivalent circle diameters in analysis mode to the range of equivalent circle diameters of toner particles (for example, 4.0 μm to 10.0 μm). The average brightness of resin particles can be obtained by setting the range of equivalent circle diameters in analysis mode to the range of equivalent circle diameters of resin particles (for example, 0.5 μm to 3.0 μm). The average equivalent circular diameter of the toner particles can be obtained by setting the range of the average brightness in the analysis mode to the range of the brightness of the toner particles (for example, 40 to 80). The average equivalent circular diameter of the resin particles can be obtained by setting the range of the average brightness in the analysis mode to the range of the brightness of the resin particles (for example, 90 to 120). The range of the equivalent circular diameter and the range of brightness of the toner particles and the range of the equivalent circular diameter and the range of brightness of the resin particles can be understood, for example, from the particle size distribution and brightness of the toner particles and the resin particles measured from the toner.

[0090] <Measurement of resin particle number-based content b> The content b of the resin particles in the toner based on the number of the resin particles per 100 toner particles can be measured by the following method. In the measurement of the average equivalent circle diameter of the resin particles using the toner as the measurement sample, a frequency table is displayed, and the count number A of the particles included in the range of the equivalent circle diameter of the resin particles (e.g., 0.5 μm to 3.0 μm) and the range of the brightness of the resin particles (e.g., 90 to 120) is measured. Furthermore, the count number B of all the particles is measured, and BA is defined as the count number of the toner particles. The content b can be calculated from the obtained count numbers of the resin particles and the count numbers of the toner particles.

[0091] Before starting the measurement, automatic focus adjustment is performed using standard latex particles (Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5100A" diluted with ion-exchanged water). After that, it is preferable to perform focus adjustment every 2 hours from the start of the measurement. In this case, the flow-type particle image analyzer used has been calibrated by Sysmex Corporation and has a calibration certificate issued by Sysmex Corporation.

[0092] <Method for identifying hydrotalcite particles> The hydrotalcite particles, which are external additives, can be identified by a combination of shape observation using a scanning electron microscope (SEM) and elemental analysis using energy dispersive X-ray analysis (EDS). Using a scanning electron microscope "S-4800" (product name; manufactured by Hitachi), the toner is observed at a maximum magnification of 50,000 times. The focus is adjusted to the surface of the toner particles, and the external additive to be identified is observed. An EDS analysis is performed on the external additive to be identified, and the hydrotalcite particles can be identified from the type of element peak. As the element peak, at least one metal element peak selected from the group consisting of Mg, Zn, Ca, Ba, Ni, Sr, Cu, and Fe, which are metals that can constitute hydrotalcite particles, is When an element peak of at least one metal selected from the group consisting of Al, B, Ga, Fe, Co, and In is observed, the presence of hydrotalcite particles containing the two metals can be inferred. A specimen of the hydrotalcite particles estimated by EDS analysis is prepared separately, and its shape is observed by SEM and analyzed by EDS. The analysis results of the specimen are compared to the analysis results of the particles to be identified to see if they match, and it is determined whether or not they are hydrotalcite particles.

[0093] <Method for measuring the mass content (%) of hydrotalcite particles in toner> The mass content (%) of hydrotalcite particles in the toner can be quantified using fluorescent X-ray analysis and a calibration curve created from a standard sample. It conforms to K 0119-1969, but specifically as follows: The measurement equipment used is a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. In addition, a proportional counter (PC) is used to measure light elements, and a scintillation counter (SC) is used to measure heavy elements.

[0094] The measurement sample is prepared by putting 4 g of toner into a dedicated aluminum ring for pressing, flattening it, and pressing it at 20 MPa for 60 seconds using a tablet press to form pellets with a thickness of 2 mm and a diameter of 39 mm. The tablet press used is the "BRE-32" manufactured by Mayekawa Test Machinery Co., Ltd.

[0095] Measurements are performed under the above conditions, and elements are identified based on the peak positions of the obtained X-rays, and their concentrations are calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time. A separately prepared sample of hydrotalcite particles is added to 100 parts by mass of toner particles so that the amount is 0.10 parts by mass, and the mixture is thoroughly mixed using a coffee mill. Similarly, 0.20 parts by mass and 0.50 parts by mass of hydrotalcite particles are mixed with the toner particles, respectively, to prepare samples for the calibration curve.

[0096] For each sample, the count rate (unit: cps) derived from the metal elements in the hydrotalcite is measured. In this case, the acceleration voltage and current value of the X-ray generator are 24 kV and 100 mA, respectively. A linear calibration curve is obtained by plotting the obtained X-ray count rate on the vertical axis and the amount of hydrotalcite particles added in each calibration curve sample on the horizontal axis. Next, the toner to be analyzed is pelletized as described above using a tablet molding compressor, and the counting rate derived from the metal elements in the hydrotalcite is measured. Then, the mass-based content (%) of the hydrotalcite particles in the toner is calculated from the calibration curve.

[0097] <Method for measuring the element ratio of hydrotalcite particles> The element ratios of hydrotalcite particles are measured by EDS mapping of the toner using a scanning transmission electron microscope (STEM). In EDS mapping measurements, spectrum data is obtained for each pixel in the analysis area. By using a silicon drift detector with a large detection element area, EDS mapping can be measured with high sensitivity. By performing statistical analysis on the spectral data for each pixel obtained by EDS mapping measurement, it is possible to obtain a principal component mapping that extracts pixels with similar spectra, making it possible to map specific components.

[0098] The observation sample is prepared according to the following procedure. 0.5 g of the toner is weighed out, and placed in a cylindrical mold with a diameter of 8 mm and left to stand for 2 minutes under a load of 40 kN using a Newton press to prepare a cylindrical toner pellet with a diameter of 8 mm and a thickness of approximately 1 mm. A 200 nm-thick slice is prepared from the toner pellet using an ultramicrotome (Leica, FC7).

[0099] The STEM-EDS analysis is carried out using the following equipment and conditions. Scanning transmission electron microscope: JEM-2800 manufactured by JEOL Ltd. EDS detector: JED-2300T Dry SD100GV detector (detector area: 100 mm 2 ) EDS analyzer: Thermo Fisher Scientific NORAN System 7

[0100] [Conditions for STEM-EDS] STEM accelerating voltage: 200kV ·Magnification: 20,000x Probe size 1nm STEM image size: 1024 x 1024 pixels (EDS element mapping images are acquired at the same position.) EDS mapping size: 256 x 256 pixels, Dwell Time: 30 μs, Integration count: 100 frames The ratio of each element in the hydrotalcite particles is calculated based on the multivariate analysis as follows.

[0101] The EDS mapping is obtained by the STEM-EDS analysis device. Next, the collected spectral mapping data is subjected to multivariate analysis using the COMPASS (PCA) mode in the measurement command of the NORAN System 7 described above, and a principal component map image is extracted. In this case, the setting values ​​are as follows: Kernel size: 3×3 Quantitative map setting: High (slow) Filter Fit Type: High Precision (Slow) At the same time, this operation calculates the area ratio of each extracted principal component in the EDS measurement field of view. Quantitative analysis is performed on the EDS spectrum of each obtained principal component mapping by the Cliff-Lorimer method.

[0102] The toner particle portion and the hydrotalcite particles are distinguished based on the quantitative analysis results of the obtained STEM-EDS main component mapping. The particles can be identified as hydrotalcite particles based on the particle size, shape, content of polyvalent metals such as aluminum and magnesium, and the amount ratio thereof. Moreover, whether or not fluorine and aluminum are present inside the hydrotalcite particles can be determined by the following means.

[0103] (Method for analyzing fluorine and aluminum in hydrotalcite particles) Based on the mapping data obtained by the above-mentioned method using STEM-EDS mapping analysis, the fluorine and aluminum in the hydrotalcite particles are analyzed. Specifically, EDS line analysis is performed in the normal direction to the outer periphery of the hydrotalcite particle, and the fluorine and aluminum present inside the particle are analyzed. A schematic diagram of the line analysis is shown in Figure 1(a). For a toner particle 1 and a hydrotalcite particle 3 adjacent to a toner particle 2, a line analysis is performed in the normal direction to the outer periphery of the hydrotalcite particle 3, i.e., in the direction of 5. Note that 4 indicates the boundary of the toner particle. The area in the acquired STEM image where hydrotalcite particles exist is selected using the rectangular selection tool, and line analysis is performed under the following conditions. Line analysis conditions STEM magnification: 800,000x Line length: 200nm Line width: 30nm Number of line divisions: 100 points (intensity measurement every 2 nm)

[0104] When the elemental peak intensity of fluorine or aluminum in the EDS spectrum of the hydrotalcite particle is 1.5 times or more the background intensity, and when the elemental peak intensity of fluorine or aluminum at both ends of the hydrotalcite particle in the line analysis (points a and b in FIG. 1(a)) does not exceed 3.0 times the peak intensity at point c, the element is determined to be contained inside the hydrotalcite particle. Point c is the midpoint of the line segment ab (i.e., the midpoint of the both ends). Examples of X-ray intensities of fluorine and aluminum obtained by line analysis are shown in Figures 1(b) and 1(c). When hydrotalcite particles contain fluorine and aluminum inside, the graph of X-ray intensity normalized by peak intensity shows a shape as shown in Figure 1(b). When hydrotalcite particles contain fluorine derived from a surface treatment agent, the graph of X-ray intensity normalized by peak intensity has peaks near the points a and b at both ends of the fluorine graph, as shown in Figure 1(c). By checking the X-ray intensities derived from fluorine and aluminum in the line analysis, it can be confirmed that the hydrotalcite particles contain fluorine and aluminum inside.

[0105] (Calculation method of the ratio of the atomic concentration of fluorine to aluminum in hydrotalcite particles (element ratio) F / Al) The atomic concentration ratio (element ratio) F / Al of fluorine to aluminum in the hydrotalcite particles obtained from the main component mapping derived from the hydrotalcite particles by the above-mentioned STEM-EDS mapping analysis is obtained in multiple fields of view, and the arithmetic average is taken for 100 or more relevant particles to obtain the atomic concentration ratio (element ratio) F / Al of fluorine to aluminum in the hydrotalcite particles.

[0106] (Method of calculating the ratio of the atomic concentration of magnesium to aluminum in hydrotalcite particles (element ratio) Mg / Al) The same method as for calculating the atomic concentration ratio (element ratio) F / Al of fluorine to aluminum in the hydrotalcite particles described above is performed for magnesium and aluminum to calculate the atomic concentration ratio (element ratio) Mg / Al of magnesium to aluminum in the hydrotalcite particles.

[0107] <Measurement of carbon black content> The carbon black content in the toner was measured using a TGA (TA-Instruments, Inc., Model 2950 high resolution automatic type). The toner was heated to 800°C in a nitrogen stream and maintained at that temperature for 30 minutes to remove the resin content of the toner. The weight of the resulting residue was taken as the carbon black content.

[0108] <Method of measuring weight average particle size (D4) of toner> The weight-average particle diameter (D4) of the toner is calculated as follows. The measurement device used is a precision particle size distribution measurement device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (Beckman Coulter, Inc.). The measurement will be performed using an effective number of measurement channels of 25,000. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter). Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm. The specific measurement method is as follows.

[0109] (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) About 30 ml of the electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and about 0.3 ml of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) with two built-in oscillators with an oscillation frequency of 50 kHz and a phase difference of 180 degrees, and an electrical output of 120 W. Pour about 3.3 L of ion-exchanged water into the water tank of the ultrasonic disperser, and add about 2 ml of Contaminon N to the water tank. (4) Set the beaker from (2) in the beaker fixing hole of the ultrasonic disperser, and operate the ultrasonic disperser. Then, adjust the height position of the beaker so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, add the electrolytic solution (5) in which the toner has been dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4). EXAMPLES

[0110] The present invention will be described in more detail below with reference to Production Examples and Examples, which are not to be construed as limiting the present invention in any way. Note that the numbers of parts in the following formulations all refer to parts by mass.

[0111] <Production Example of Polyester Resin 1> Into a reaction vessel equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dehydration tube, and a pressure reducing device, 1.0 mol of terephthalic acid, 0.65 mol of a propylene oxide 2-mol adduct of bisphenol A, and 0.35 mol of ethylene glycol were added, and the mixture was heated to 130° C. with stirring. After that, 0.52 parts of tin di(2-ethylhexanoate) was added as an esterification catalyst relative to 100.0 parts of the total amount of the monomers, and the temperature was raised to 200° C., and polycondensation was carried out until the desired molecular weight was reached. Furthermore, 0.03 mol parts of trimellitic anhydride was added, and the reaction was continued for 1 hour to obtain amorphous polyester resin 1.

[0112] <Production Example of Polyester Resin 2> Fumaric acid: 24.61 parts (50.0 mol%) Bisphenol A-propylene oxide 2.2 mole adduct: 75.39 parts (50.0 mole%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted for 1 hour under reduced pressure of 60 to 70 mmHg to obtain amorphous polyester resin 2. In this specification, the reaction rate refers to the value of the amount of reaction water produced (mol) / theoretical amount of water produced (mol)×100.

[0113] <Production Example of Polyester Resin 3> 1,6 Hexanediol: 48.96 parts (50.0 mol%) Fumaric acid: 36.10 parts (37.5 mol%) Adipic acid: 14.94 parts (12.5 mol%) Dibutyltin oxide: 0.1 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted in a nitrogen atmosphere at 160°C for 5 hours, then heated to 200°C and reacted for 1 hour. The reaction was further carried out for 1 hour under a reduced pressure of 60 to 70 mmHg to obtain polyester resin 3, which is a crystalline polyester.

[0114] <Production example of binder resin 1> The polyester monomers were mixed in the following ratios: Cyclohexanedicarboxylic acid: 0.650mol Hexane diacid: 0.200mol Adipic acid: 0.100mol Dodecenyl succinic anhydride: 0.050mol Fumaric acid: 0.008mol Cyclohexanedimethanol: 0.690mol Propylene glycol: 0.300mol Ethylene glycol: 0.090mol To the above material, 0.1 mass % of tetrabutyl titanate as a catalyst and 0.01 mass % of magnesium acetate as a co-catalyst were added, and condensation polymerization was carried out at 240° C. to obtain an unsaturated polyester resin (Tg=53° C., main peak molecular weight=5800).

[0115] The unsaturated polyester resin: 75 parts by mass, styrene: 18 parts by mass as vinyl monomers, n-butyl acrylate: 6.5 parts by mass, mono n-butyl maleate: 0.5 parts by mass, paraffin wax (Mn450, Mw520, main peak molecular weight 500, DSC peak temperature 75.0 ° C): 2 parts by mass, and 2,5-dimethyl-2,5-bis (t-butylperoxy) hexyne-3 (10-hour half-life temperature 128 ° C): 0.08 parts by mass as an initiator were mixed. This vinyl monomer / polyester resin mixture was polymerized at 120 ° C for 20 hours until the polymerization conversion rate of the vinyl monomer reached 98%, and then the temperature was further raised to 150 ° C and maintained for 5 hours to polymerize the unreacted vinyl monomer, thereby obtaining binder resin 1.

[0116] <Preparation of Polyester Resin Particle Dispersion 1> Polyester resin 1: 200 parts Ion-exchanged water: 500 parts Fumaric acid: 0.170 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining polyester resin particle dispersion 1. The particle size distribution of this polyester resin particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0117] <Preparation of Polyester Resin Particle Dispersions 2 to 12> Polyester resin particle dispersions 2 to 12 were obtained in the same manner as in Production Example of Polyester Resin Particles 1, except that the amount of fumaric acid added was changed to the amount shown in Table 1. [Table 1]

[0118] <Preparation of Polyester Resin Particle Dispersion 13> Polyester resin 1: 200 parts Ion-exchanged water: 500 parts Phthalic acid: 0.17 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium hydrogen carbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining polyester resin particle dispersion 13. The particle size distribution of this polyester resin particle dispersion 13 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0119] <Preparation of Polyester Resin Particle Dispersion 14> Polyester resin 2: 200 parts Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, melted, and thoroughly stirred at 7800 rpm using a homogenizer (IKA Ultra Turrax T50) while adding 0.1 mol / L sodium bicarbonate to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining polyester resin particle dispersion 14. The particle size distribution of this polyester resin particle dispersion 14 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0120] <Preparation of Polyester Resin Particle Dispersion 15> Polyester resin 1: 160 parts Polyester resin 3: 40 parts Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium hydrogen carbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining polyester resin particle dispersion 15. The particle size distribution of this polyester resin particle dispersion 15 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0121] <Preparation of Resin Particle Dispersion 16> Binder resin 1: 200 parts Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining a resin particle dispersion 16. The particle size distribution of this resin particle dispersion 16 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0122] <Preparation of vinyl resin dispersion> Polystyrene resin: 200 parts (product name: TSK Standard Polystyrene F-2, Tosoh Corporation) -Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 100°C in a hot bath, and melted. While thoroughly stirring at 7800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to make the pH greater than 8.5. After that, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining a vinyl resin dispersion.

[0123] <Preparation of Wax Particle Dispersion> -500 parts deionized water Wax (hydrocarbon wax; maximum endothermic peak temperature 77°C) 250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7,800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to adjust the pH to greater than 7.0. Thereafter, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 245 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the wax particles. The particle size distribution of the wax particles contained in this wax particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the wax particles contained was 0.35 μm, and no coarse particles exceeding 1 μm were observed.

[0124] <Preparation of Colorant Particle Dispersion 1> Carbon black Nipex 35 (Orion Engineered Carbons) 100 parts Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above was mixed and dispersed using a sand grinder mill to obtain a colorant particle dispersion. The particle size distribution of the colorant particles contained in this colorant particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0125] <Preparation of Colorant Particle Dispersions 2 to 6> Colorant particle dispersions 2 to 6 were obtained in the same manner as in the production example of colorant particle dispersion 1, except that the amount of carbon black Nipex 35 added was changed to the amount shown in Table 2. [Table 2]

[0126] <Production Example of Toner Particle 1> Polyester resin particle dispersion 1: 500 parts Colorant particle dispersion 1: 50 parts Wax particle dispersion: 50 parts Ion-exchanged water: 160 parts The above materials were put into a round stainless steel flask and mixed. Then, the homogenizer Ultra Turrax T50 (IKA) was used to disperse the mixture at 5000 r / min for 10 minutes. After adding a 1.0% aqueous nitric acid solution and adjusting the pH to 3.0, the mixture was heated to 58°C in a heating water bath using a stirring blade while appropriately adjusting the rotation speed so that the mixture was stirred. The formed aggregated particles were appropriately confirmed using a Coulter Multisizer III, and when aggregated particles with a weight average particle size (D4) of 7.2 μm were formed, the pH was adjusted to 9.0 using a 5% aqueous sodium hydroxide solution.

[0127] After that, while continuing stirring, the mixture was heated to 75°C. The mixture was then held at 75°C for 1 hour to fuse the aggregated particles. The mixture was then cooled to 50°C and held for 3 hours to promote crystallization of the resin. The mixture was then cooled to 25°C, filtered and separated into solid and liquid, and washed with ion-exchanged water. After washing, the mixture was dried using a vacuum dryer to obtain toner particles 1 having a weight average particle size (D4) of 7.2 μm.

[0128] <Production Example of Resin Particle 1> Polyester resin particle dispersion 1: 500 parts Colorant particle dispersion 1: 0.10 parts Ion-exchanged water: 160 parts The above materials were put into a round stainless steel flask and mixed. Then, the materials were dispersed for 10 minutes at 5000 r / min using a homogenizer Ultra Turrax T50 (manufactured by IKA). After adding a 1.0% nitric acid aqueous solution and adjusting the pH to 3.0, the mixture was heated to 58°C in a heating water bath using a stirring blade while appropriately adjusting the rotation speed so that the mixture was stirred. The formed aggregated particles were appropriately confirmed using a Coulter Multisizer III, and when aggregated particles with a weight average particle size (D4) of 1.5 μm were formed, the pH was adjusted to 9.0 using a 5% sodium hydroxide aqueous solution.

[0129] Then, while continuing stirring, the mixture was heated to 75°C. The mixture was then held at 75°C for 1 hour to fuse the aggregated particles. The mixture was then cooled to 50°C and held for 3 hours to promote crystallization of the resin. The mixture was then cooled to 25°C, filtered and separated into solid and liquid, and washed with ion-exchanged water. After washing, the mixture was dried using a vacuum dryer to obtain resin particles 1 having a weight average particle size (D4) of 1.5 μm.

[0130] <Production Examples of Resin Particles 2 to 6> Resin particles 2 to 6 were obtained in the same manner as in the production example of resin particles 1, except that the added amount of polyester resin dispersion 1 and the added amount of colorant particle dispersion were changed to the amounts shown in Table 3. The physical properties of the obtained resin particles 2 to 6 are shown in Table 3. [Table 3]

[0131] <Production Example of Hydrotalcite Particle 1> Hydrotalcite particles 1 were produced as follows. A mixed aqueous solution of 1.03 mol / L magnesium chloride and 0.239 mol / L aluminum sulfate (Liquid A), a 0.753 mol / L aqueous solution of sodium carbonate (Liquid B), and a 3.39 mol / L aqueous solution of sodium hydroxide (Liquid C) were prepared. Next, liquid A, liquid B, and liquid C were poured into the reaction tank using a metering pump at a flow rate that gave a volume ratio of liquid A:liquid B of 4.5:1, and the pH value of the reaction solution was maintained in the range of 9.3 to 9.6 with liquid C, and the reaction temperature was 40°C to generate a precipitate. After filtration and washing, the precipitate was re-emulsified in ion-exchanged water to obtain a raw material hydrotalcite slurry. The hydrotalcite in the obtained hydrotalcite slurry had a concentration of 5.6 mass%. The obtained hydrotalcite slurry was vacuum dried overnight at 40°C. NaF was dissolved in ion-exchanged water to a concentration of 100mg / L, and a solution was prepared by adjusting the pH to 7.0 using 1mol / L HCI or 1mol / L NaOH, to which the dried hydrotalcite was added to a concentration of 0.1% (w / v%). The mixture was stirred at a constant speed for 48 hours using a magnetic stirrer so as not to cause precipitation. The mixture was then filtered through a membrane filter with a pore size of 0.5μm and washed with ion-exchanged water. The obtained hydrotalcite was vacuum dried overnight at 40°C, and then crushed. The composition of the obtained hydrotalcite particles 1 is shown in Table 4.

[0132] <Production Examples of Hydrotalcite Particles 2 to 5> Except for appropriately adjusting the concentrations of the solutions A, B and the NaF aqueous solution, hydrotalcite particles 2 to 11 were obtained in the same manner as in the production example of the hydrotalcite particles 1. The compositions of the obtained hydrotalcite particles 2 to 5 are shown in Table 4. In the hydrotalcite particles 1 to 5, fluorine and aluminum were present inside the hydrotalcite particles.

[0133] <Production Example of Hydrotalcite Particle 6> Hydrotalcite particles 6 were obtained in the same manner as in Production Example of Hydrotalcite Particles 1, except that ion-exchanged water was used instead of the NaF aqueous solution in Production Example of Hydrotalcite Particles 1. The composition of the obtained hydrotalcite particles 6 is shown in Table 4. [Table 4]

[0134] <Production of Toner 1> Using an FM mixer ("FM-10B" manufactured by Nippon Coke and Engineering Co., Ltd.), 1:100 parts of toner particles, 1:2.0 parts of resin particles, 1:0.2 parts of hydrotalcite particles, 1.4 parts of silica fine particles, and 0.2 parts of titanium oxide particles (number average particle size 1.2 μm) were mixed for 180 seconds at a rotation speed of 3500 rpm to obtain a toner mixture. Thereafter, coarse particles were removed using a 300 mesh (48 μm opening) sieve to obtain Toner 1. The production conditions and physical properties are shown in Table 5.

[0135] <Production of toners 2 to 21> Toners 2 to 21 were produced in the same manner as in the production example of Toner 1, except that the type of colored particle dispersion, type of polyester resin dispersion, type of resin particle dispersion, amount of resin particle dispersion added, type of hydrotalcite, equivalent circle diameter of toner particles, and equivalent circle diameter of resin particles in Toner 1 were changed as shown in Table 5. The production conditions are shown in Table 5, and the physical properties are shown in Table 6.

[0136] <Production of Comparative Toners 1 to 15> Comparative toners 1 to 15 were produced in the same manner as in the production example of toner 1, except that in toner 1, the type of colorant particle dispersion, type of polyester resin dispersion, type of resin particles, amount of resin particles added, type of hydrotalcite particles, equivalent circle diameter of toner particles, and equivalent circle diameter of resin particles were changed as shown in Table 5. The production conditions are shown in Table 5, and the physical properties are shown in Table 6.

[0137] In addition, in each of the toners using hydrotalcite particles 1 to 5, fluorine and aluminum were present inside the hydrotalcite particles, and the same F / Al ratio as in Table 4 was confirmed. [Table 5]

[0138] [Table 6] In the table, the content b is the content of the resin particles in the toner based on the number of particles per 100 toner particles. The CB amount indicates the carbon black content (mass%) based on the mass of the toner. The brightness is the average brightness value.

[0139] The obtained toner was subjected to the following evaluations. [Charge rise property] <Evaluation of charging start> A solid image is output, and the machine is forcibly stopped during output of the first and 100th sheets, and the amount of charge of the toner on the developing roller immediately after it has passed the regulating blade is measured. The charge amount of the toner was measured using the following procedure using a Faraday cage 200 (suction type Faraday cage) shown in Figure 2. The Faraday cage is a metal double cylinder configured with the same axis, and the inner cylinder 201 and the outer cylinder 202 are insulated by an insulating member 203. When a charged body with a charge Q is placed inside this inner cylinder, electrostatic induction makes it seem as if a metal cylinder with a charge Q exists. First, the process cartridge is forcibly pulled out from the electrophotographic image forming apparatus during the operation of forming a solid white image, and the developing roller is stopped. Next, the toner 205 of the toner layer that has passed through the toner regulating member and is not yet in contact with the photosensitive member is sucked from the surface of the developing roller by air suction 206 with a Faraday filter. The toner particles are taken into the filter paper 204 installed in the inner cylinder of the cage. The amount of induced charge Q (μC) is measured with an electrometer (product name: 616 DIGITAL ELECTROMETER; manufactured by KEITHLEY) and divided by the weight M (g) of the toner particles held in the filter paper in the inner cylinder to obtain the amount of charge Q / M (μC / g). The charge rise rate was calculated using the following formula and evaluated according to the following ranks. (Charge rise rate) = (Q / M of 1st solid sheet) / (Q / M of 100th solid sheet) x 100

[0140] <Tip concentration evaluation> The image forming apparatus used was a modified laser printer (product name: LBP-9650Ci, manufactured by Canon Inc.) and a modified process cartridge (product name: Toner Cartridge 323, manufactured by Canon Inc.) The image forming apparatus was modified by changing the gear and software of the evaluation machine body to change the process speed to 350 mm / sec. The cartridge was modified by changing and adding gears inside the cartridge so that the toner supply member (toner supply roller) and the developing member (developing roller) move in the same direction at the contact point. When printing images, high white paper (product name: GF-C081, manufactured by Canon, 81.4 g / m 2 First, the toner was removed from the inside of the cartridge and the cartridge was cleaned with an air blower, and then 300 g of Toner 1 was filled into the cartridge. The toner cartridge and the modified machine were left for 24 hours in an environment with a temperature of 5.0°C and a relative humidity of 10.0%RH, and then installed in the black station of the printer under the same environment, while a dummy cartridge was installed in the other stations. A solid image was output in a high temperature and high humidity environment (30°C / 90%Rh), and the image density from the top of the solid image for one revolution of the developing roller and the image density from the second revolution onwards were measured with a color reflection densitometer (X-Rite404A), and the image density difference (tip density difference) at that time was evaluated as follows. A: The image density difference is 0.05 or less. B: The image density difference is greater than 0.05 and is 0.10 or less. C: The image density difference is greater than 0.10 and is 0.15 or less. D: The image density difference is greater than 0.15.

[0141] <Evaluation of image density> A solid image was printed using the above machine in a high temperature and high humidity environment (30°C / 90%Rh), and the image density was measured at five points using a color reflection densitometer (X-Rite404A) and the average value was calculated. The image density was evaluated according to the following criteria: A: 1.2 or higher B: 1.1 or more and less than 1.2 C: 1.0 or more and less than 1.1 D: Less than 1.0

[0142] [Examples 1 to 22] In Examples 1 to 21, the above evaluation was performed using Toners 1 to 21, respectively. In Example 22, Toner 1 was used, and the regulating blade was changed from SUS to urethane, and the evaluation was performed. The evaluation results are shown in Table 7.

[0143] [Comparative Examples 1 to 15] In Comparative Examples 1 to 15, the above evaluations were carried out using Comparative Toners 1 to 15, respectively. The evaluation results are shown in Table 7.

[0144] [Table 7]

[0145] In Examples 1 to 22, good results were obtained in all evaluation items. On the other hand, in Comparative Examples 1, 2, 4 to 8, and 10 to 15, the charge rise rate was low, and the evaluation item of low density at the leading edge was inferior to the Examples. In Comparative Examples 3 and 9, the charge rise was good, but the image density was inferior to the Examples.

[0146] As a result of the above, according to the present disclosure, it is possible to provide a toner that has excellent charge start-up properties even in a high-temperature and high-humidity environment and realizes stable image quality.

[0147] The present disclosure relates to the following configurations. (Configuration 1) A toner containing toner particles and resin particles, the toner particles contain carbon black and a polyester resin; the toner particles have an average brightness of 40 to 80 based on monochrome 256 gradations; The resin particles contain a polyester resin, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations; The toner contains fumaric acid, The average equivalent circle diameter of the resin particles is 0.5 to 3.0 μm, the toner particles have an average equivalent circular diameter of 4.0 to 10.0 μm; The content of the resin particles in the toner based on the number of the resin particles per 100 toner particles is represented by b (pieces), said b is 5 to 30 pieces, the content of the fumaric acid in the toner relative to the total mass of the toner is represented as a (ppm by mass), the content a is 10 to 1,200 ppm by mass; A toner characterized by: (Configuration 2) 2. The toner according to claim 1, wherein the toner contains the carbon black in an amount of 3 to 15% by mass based on the mass of the toner. (Configuration 3) 3. The toner according to configuration 1 or 2, wherein the a (ppm by mass) is 50 to 1000 ppm by mass. (Configuration 4) The toner according to any one of configurations 1 to 3, wherein the a (ppm by mass) and the b (pieces) satisfy the following formula (1): 2≦a / b≦120 (1) (Configuration 5) 5. The toner according to any one of configurations 1 to 4, wherein the toner contains hydrotalcite particles as an external additive. (Configuration 6) In a line analysis in the STEM-EDS mapping analysis of the toner, Fluorine and aluminum are present inside the hydrotalcite particles, The toner according to Configuration 5, wherein a value F / Al of a ratio of the atomic concentration of fluorine to that of aluminum in the hydrotalcite particles, obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, is 0.01 to 0.60. (Configuration 7) The toner according to any one of configurations 1 to 6, wherein the toner particles contain the fumaric acid. (Configuration 8) The toner according to any one of configurations 1 to 7, wherein when the mass-based content of fumaric acid in the toner that is extracted from the toner with methanol is defined as f1 (%), f1 is 0.0005 to 0.0100%. (Configuration 9) The resin particles contain carbon black, The toner according to any one of Configurations 1 to 8, wherein the content of the carbon black in the resin particles is preferably 0.01 to 0.30 parts by mass with respect to 100 parts by mass of the polyester resin. (Configuration 10) A process cartridge that is detachably mountable to an electrophotographic image forming apparatus, The process cartridge comprises: Toner; A frame body, a cylindrical toner carrier that is rotatably supported by the frame and carries the toner; a regulating member having an abutment portion, one end of which is fixed to the frame and the other end of which is in contact with the toner carrier to form a contact nip between the toner carrier and the abutment portion; Equipped with The toner is a toner according to any one of configurations 1 to 9, The process cartridge is characterized in that the regulating member is a toner regulating blade having a metal blade. (Configuration 11) 1. An electrophotographic image forming apparatus, comprising: The electrophotographic image forming apparatus includes a process cartridge, 11. An electrophotographic image forming apparatus, wherein the process cartridge is the process cartridge according to configuration 10. [Explanation of symbols]

[0148] 1: toner particle 1, 2: toner particle 2, 3: hydrotalcite particle, 4: boundary of toner particle, 5: analysis direction of line analysis

Claims

1. A toner containing toner particles and resin particles, the toner particles contain carbon black and a polyester resin; the toner particles have an average brightness value of 40 to 80 based on monochrome 256 gradations; The resin particles contain a polyester resin, the resin particles have an average brightness value of 90 to 120 based on monochrome 256 gradations; The toner contains fumaric acid, The resin particles have an average equivalent circular diameter of 0.5 to 3.0 μm, the toner particles have an average equivalent circular diameter of 4.0 to 10.0 μm; the content of the resin particles in the toner based on the number of the resin particles per 100 toner particles is designated as b (pieces), the b being 5 to 30 pieces; the content of the fumaric acid in the toner relative to the total mass of the toner is represented as a (ppm by mass), the content a is 10 to 1,200 ppm by mass; A toner characterized by:

2. 2. The toner according to claim 1, wherein the toner contains the carbon black in an amount of 3 to 15% by mass based on the mass of the toner.

3. 2. The toner according to claim 1, wherein the a (ppm by mass) is from 50 to 1000 ppm by mass.

4. The toner according to claim 1 , wherein the a (ppm by mass) and the b (pieces) satisfy the following formula (1): 2≦a / b≦120 (1)

5. The toner according to claim 1 , wherein the toner contains hydrotalcite particles as an external additive.

6. In a line analysis in the STEM-EDS mapping analysis of the toner, Fluorine and aluminum are present inside the hydrotalcite particles, 6. The toner according to claim 5, wherein a value F / Al of a ratio of atomic concentration of fluorine to aluminum in the hydrotalcite particles, obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, is 0.01 to 0.

60.

7. The toner of claim 1 , wherein said toner particles contain said fumaric acid.

8. 2. The toner according to claim 1, wherein when a mass-based content of fumaric acid in the toner that is extracted from the toner with methanol is defined as f1 (%), f1 is 0.0005 to 0.0100%.

9. The resin particles contain carbon black, 2. The toner according to claim 1, wherein the content of the carbon black in the resin particles is preferably 0.01 to 0.30 parts by mass with respect to 100 parts by mass of the polyester resin.

10. A process cartridge that is detachably mountable to an electrophotographic image forming apparatus, The process cartridge comprises: Toner; A frame body, a cylindrical toner carrier that is rotatably supported by the frame and carries the toner; a regulating member having an abutment portion, one end of which is fixed to the frame and the other end of which is in contact with the toner carrier to form a contact nip between the toner carrier and the abutment portion; Equipped with The toner is the toner according to any one of claims 1 to 9, The process cartridge is characterized in that the regulating member is a toner regulating blade having a metal blade.

11. 1. An electrophotographic image forming apparatus, comprising: The electrophotographic image forming apparatus includes a process cartridge, 11. An electrophotographic image forming apparatus, wherein the process cartridge is the process cartridge according to claim 10.

Citation Information

Patent Citations

  • Electrophotographic negatively chargeable toner

    JP1991056974A

  • Toner

    JP2014098840A