Laminate board, multilayer board, and manufacturing method of laminate board
A liquid crystal polymer film with a melting point of 345°C or higher, composed of specific monomers, addresses the issue of metal wiring deformation and impedance errors in multilayer boards, ensuring high-quality circuit integrity during thermocompression bonding.
Patent Information
- Application Number
- JP2023171246
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-10
- Filing Date
- 2023-10-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-10-02
AI Technical Summary
Existing laminates with poor heat resistance in multilayer boards lead to metal wiring deformation and impedance errors, increasing signal transmission loss and cross-talk between wiring lines during thermocompression bonding.
Utilizing a liquid crystal polymer film with a melting point of 345°C or higher, composed of specific monomers such as aromatic dicarboxylic acids, hydroxycarboxylic acids, and diols, with a metal layer attached, to prevent metal wiring deformation and maintain circuit integrity during thermocompression bonding.
The high heat resistance of the liquid crystal polymer film ensures that metal wiring does not fall into the film, maintaining circuit integrity and preventing impedance errors and signal loss, resulting in a high-quality multilayer board.
Smart Images

Figure 2024160919000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to laminates, multi-layer boards, and methods for making laminates. [Background technology]
[0002] A laminate typically includes an insulating substrate and metal wiring. When stacking multiple layers of a laminate and then thermocompression bonding, if the insulating substrate has poor heat resistance, the metal wiring may easily sink or deform into the insulating substrate. This can lead to impedance errors in the circuit design, and can also increase signal transmission loss and crosstalk between wiring. In view of this, there is an urgent need to develop a solution that can overcome the above problems. Summary of the Invention
[0003] The present disclosure provides a laminate comprising: a liquid crystal polymer film having a melting point of 345°C or greater, the liquid crystal polymer being polymerized by a reactant comprising a plurality of first monomers which are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or combinations thereof; a plurality of second monomers which are aromatic hydroxycarboxylic acids; a plurality of third monomers which are aromatic diols, aliphatic diols, or combinations thereof; a plurality of fourth monomers which are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or combinations thereof; and at least one metal layer attached to a surface of the liquid crystal polymer film.
[0004] In some embodiments, the liquid crystal polymer is polymerized with an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid.
[0005] In some embodiments, the liquid crystal polymer is polymerized with an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aromatic hydroxyamine.
[0006] In some embodiments, the liquid crystal polymer is polymerized with an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aliphatic diol.
[0007] In some embodiments, the liquid crystal polymer comprises a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. each first monomer unit [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] and each fourth monomer unit is [ka] It is.
[0008] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 14 mol % to 16 mol %, the third monomer units are 5 mol % to 13 mol %, and the fourth monomer units are 5 mol % to 13 mol %.
[0009] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 16 mol % to 18 mol %, the third monomer units are 9 mol % to 12 mol %, and the fourth monomer units are 9 mol % to 12 mol %.
[0010] In some embodiments, the liquid crystal polymer comprises a plurality of first monomer units and a plurality of second monomer units, each of the first monomer units being [ka] and each second monomer unit is [ka] %, the first monomer units are present in an amount of 70 mol % to 85 mol %, and the second monomer units are present in an amount of 15 mol % to 30 mol %.
[0011] In some embodiments, the liquid crystal polymer comprises a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units, each of the first monomer units being [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] %, wherein the first monomer units are 55 mol % to 65 mol %, the second monomer units are 15 mol % to 25 mol %, and the third monomer units are 15 mol % to 25 mol %.
[0012] The present disclosure provides a multilayer board including at least one single-sided board or at least one double-sided board, and a laminate board described in any one of the above embodiments bonded to the at least one single-sided board or at least one double-sided board.
[0013] The present disclosure provides a method for producing a laminate, comprising the steps of: preparing a liquid crystal polymer film from a liquid crystal polymer having a melting point of 345°C or greater, the liquid crystal polymer being polymerized by a reactant comprising a plurality of first monomers which are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or combinations thereof, a plurality of second monomers which are aromatic hydroxycarboxylic acids, a plurality of third monomers which are aromatic diols, aliphatic diols or combinations thereof, a plurality of fourth monomers which are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids or combinations thereof, or combinations thereof; and forming at least one metal layer adhered to a surface of the liquid crystal polymer film.
[0014] In some embodiments, the liquid crystal polymer is polymerized with an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid.
[0015] In some embodiments, the liquid crystal polymer comprises a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units, each of the first monomer units being [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] and each fourth monomer unit is [ka] It is.
[0016] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 14 mol % to 16 mol %, the third monomer units are 5 mol % to 13 mol %, and the fourth monomer units are 5 mol % to 13 mol %.
[0017] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 16 mol % to 18 mol %, the third monomer units are 9 mol % to 12 mol %, and the fourth monomer units are 9 mol % to 12 mol %.
[0018] The present disclosure relates to a liquid crystalline polymer having a melting point of less than 345° C. and polymerized by reactants including a plurality of first monomers that are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or combinations thereof, a plurality of second monomers that are aromatic hydroxycarboxylic acids, a plurality of third monomers that are aromatic diols, aliphatic diols, or combinations thereof, a plurality of fourth monomers that are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or combinations thereof, and m and a heating temperature of T m -40℃~T m and forming at least one metal layer attached to a surface of the second liquid crystal polymer film.
[0019] In some embodiments, the liquid crystal polymer is polymerized with an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aromatic hydroxyamine.
[0020] In some embodiments, the liquid crystal polymer is polymerized with an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aliphatic diol.
[0021] In some embodiments, the liquid crystal polymer comprises a plurality of first monomer units and a plurality of second monomer units, each of the first monomer units being [ka] and each second monomer unit is [ka] %, the first monomer units are present in an amount of 70 mol % to 85 mol %, and the second monomer units are present in an amount of 15 mol % to 30 mol %.
[0022] In some embodiments, the liquid crystal polymer comprises a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units, each of the first monomer units being [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] %, wherein the first monomer units are 55 mol % to 65 mol %, the second monomer units are 15 mol % to 25 mol %, and the third monomer units are 15 mol % to 25 mol %. [Brief description of the drawings]
[0023] A more complete understanding of the present disclosure can be obtained by reading the following detailed description of the embodiments and by referring to the drawings, in which: [Figure 1]1A-1D are cross-sectional schematic diagrams of multilayer boards according to various embodiments of the present disclosure. [Diagram 2] 1A-1D are cross-sectional schematic diagrams of multilayer boards according to various embodiments of the present disclosure. [Diagram 3] 1A-1D are cross-sectional schematic diagrams of multilayer boards according to various embodiments of the present disclosure. [Figure 4] 1A-1D are cross-sectional schematic diagrams of multilayer boards according to various embodiments of the present disclosure. [Diagram 5] FIG. 1 is a schematic diagram of performing thermal shock testing according to various embodiments of the present disclosure. [Figure 6] FIG. 2 is a schematic bottom view of a laminate according to various embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The following embodiments are disclosed in detail with reference to the drawings. For clarity, many practical details are described together in the following description. However, it should be understood that these practical details are not intended to limit the present disclosure. That is, in some embodiments of the present disclosure, these practical details are not necessary. In addition, in order to simplify the drawings, some known structures and elements are shown in the drawings in a schematic manner.
[0025] Although the methods disclosed herein are described below as a series of operations or steps, the order in which these operations or steps are presented should not be construed as limiting the disclosure. For example, some operations or steps may be performed in different orders and / or simultaneously with other steps. Also, not all illustrated operations, steps and / or features must be performed to achieve embodiments of the disclosure. Also, each operation or step described herein may include multiple sub-steps or actions.
[0026] The present disclosure provides a laminate including a liquid crystal polymer film and at least one metal layer attached to a surface of the liquid crystal polymer film. The liquid crystal polymer film has a melting point of 345°C or higher. In some embodiments, the melting point is 345°C to 400°C, such as 345, 350, 355, 360, 365, 370, 375, 385, 390, 395, or 400°C. The liquid crystal polymer film includes a liquid crystal polymer polymerized by a reactant. The reactant includes a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers, or a combination thereof. The first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or a combination thereof, the second monomers are aromatic hydroxycarboxylic acids, the third monomers are aromatic diols, aliphatic diols, or a combination thereof, and the fourth monomers are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or a combination thereof. Because the liquid crystal polymer film has good heat resistance, the laminate can withstand a thermal shock test at 250°C to 320°C, and in particular, the metal layer does not collapse or deform into the liquid crystal polymer film during the thermal shock test.
[0027] The present disclosure provides a multilayer board including at least one single-sided board or at least one double-sided board and the laminate. The laminate is attached to at least one single-sided board or at least one double-sided board. More specifically, the laminate is pressed against at least one single-sided board or at least one double-sided board. Since the laminate of the present disclosure has good heat resistance, when the multilayer board is formed by thermocompression bonding the multilayer laminate of the present disclosure, it is possible to avoid the metal wiring from falling into the liquid crystal polymer film, and therefore problems such as impedance error of the circuit due to deformation of the wiring, increased transmission loss, and increased crosstalk between wiring can be avoided. Therefore, the multilayer board can have good quality after thermocompression bonding.
[0028] FIG. 1 is a cross-sectional schematic diagram of a multilayer board according to various embodiments of the present disclosure. As shown in FIG. 1, the multilayer board ML1 includes a laminate board 110 and a laminate board 120. The laminate board 110 and the laminate board 120 each include a liquid crystal polymer film having a melting point of 345° C. or more, and at least one metal layer (not shown) attached to the surface of the liquid crystal polymer film. Since the liquid crystal polymer film has a high melting point, when the laminate board 110 and the laminate board 120 are pressed (thermocompression) together to form the multilayer board ML1, the metal layer does not fall into the liquid crystal polymer film and is not deformed. This allows the multilayer board ML1 to have good quality after pressing. In some embodiments, the laminate board 110 and the laminate board 120 are independently single-sided or double-sided boards.
[0029] FIG. 2 is a cross-sectional schematic diagram of a multilayer board according to various embodiments of the present disclosure. The multilayer board ML2 includes a laminate 210 and a laminate 220. The laminate 210 is a double-sided board, and the laminate 220 is a single-sided board. The laminate 210 includes a liquid crystal polymer film 212, a metal layer 214, and a metal layer 216, where the metal layer 214 and the metal layer 216 are attached to the upper surface S1 and the lower surface S2 of the liquid crystal polymer film 212, respectively. More specifically, the metal layer 214 is in direct contact with the upper surface S1, and the metal layer 216 is in direct contact with the lower surface S2. The laminate 220 includes a liquid crystal polymer film 222 and a metal layer 224. The metal layer 224 is attached to the upper surface S3 of the liquid crystal polymer film 222. More specifically, the metal layer 224 is in direct contact with the upper surface S3. Both of the liquid crystal polymer films 212 and 222 have a melting point of 345° C. or higher. As shown in FIG. 2, the metal layers 214, 216, 224 are metal wiring, which may be called patterned metal layers. The metal wiring is, for example, copper wiring. The method of forming the metal wiring includes forming a metal foil (for example, copper foil) on the surface of the liquid crystal polymer film, and then etching the metal foil to form the metal wiring. The method of forming the metal foil is, for example, a sputtering method, an electroless plating method, or an electrolytic plating method. In another embodiment, the metal wiring is directly formed on the surface of the liquid crystal polymer film by printing or electroplating. However, in other embodiments, the metal layers 214, 216, 224 may be unetched metal foil, so that the upper surfaces S1, S2, S3 are completely covered by the metal layers 214, 216, 224, respectively. In some embodiments, the liquid crystal polymer films 212, 222 are independently thermoplastic liquid crystal polymer films or thermotropic liquid crystal polymer films.
[0030] 2, the laminate 210 and the laminate 220 are stacked together, and the metal layer 214 is in contact with the lower surface S4 of the liquid crystal polymer film 222. Since the liquid crystal polymer film 212 has a high melting point, when the laminate 210 and the laminate 220 are pressed (thermocompression bonded) to form the multi-layer board ML2, the metal layer 214 will not be sunk into the liquid crystal polymer film 212, and will not be deformed by the pressing. Therefore, the distance between the metal layer 214 and the metal layer 216 can be matched with a predetermined circuit design. Based on the above, the pressing (thermocompression bonding) will not cause impedance errors in a predetermined circuit design, will not increase signal transmission loss, and will not increase crosstalk between wirings. The multi-layer board ML2 can have good quality.
[0031] FIG. 3 is a cross-sectional schematic diagram of a multilayer board according to various embodiments of the present disclosure. The multilayer board ML3 includes a laminate 310 and a laminate 320. The laminate 310 and the laminate 320 are both single-sided boards. The laminate 310 includes a liquid crystal polymer film 312 and a metal layer 314, where the metal layer 314 is attached to the top surface S5 of the liquid crystal polymer film 312, and the bottom surface S6 of the liquid crystal polymer film 312 is not covered by the metal layer. More specifically, the metal layer 314 is in direct contact with the top surface S5. The laminate 320 includes a liquid crystal polymer film 322 and a metal layer 324. The metal layer 324 is attached to the top surface S7 of the liquid crystal polymer film 322. More specifically, the metal layer 324 is in direct contact with the top surface S7. The liquid crystal polymer films 312, 322 have melting points of 345° C. or higher. 3, the metal layers 314, 324 are metal traces and may be referred to as patterned metal layers. However, in other embodiments, the metal layers 314, 324 may be unetched metal foils, such that the top surfaces S5, S7 are completely covered by the metal layers 314, 324, respectively.
[0032] 3, the laminate 310 and the laminate 320 are stacked together, and the metal layer 314 is in direct contact with the lower surface S8 of the liquid crystal polymer film 322. Since the liquid crystal polymer film 312 has a high melting point, when the laminate 310 and the laminate 320 are pressed (thermocompression bonded) to form the multi-layer board ML3, the metal layer 314 will not be tucked into the liquid crystal polymer film 312, and will not be deformed by the pressing. Therefore, the pressing (thermocompression bonding) will not cause impedance errors in a given circuit design, will not increase signal transmission loss, and will not increase crosstalk between wirings. The multi-layer board ML3 can have good quality.
[0033] 4 is a schematic cross-sectional view of a multilayer board according to various embodiments of the present disclosure. The multilayer board ML4 includes laminates 410, 420, 430, 440, 450, and 460, each of which includes a liquid crystal polymer film having a melting point of 345°C or higher. Each laminate may be a single-sided board or a double-sided board, and the embodiment of the single-sided board may refer to the embodiment of the laminate 220, the laminate 310, or the laminate 320 described above, and the embodiment of the double-sided board may refer to the embodiment of the laminate 210 described above. The laminates 410, 420, 430, 440, 450, and 460 are pressed together to form the multilayer board ML4. In the multilayer board ML4, the number of laminates may be arbitrarily adjusted according to design needs, and the number may be, but is not limited to, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, or 21.
[0034] The present disclosure provides a method for producing a laminate, comprising the steps of: preparing a liquid crystal polymer film with a liquid crystal polymer having a melting point of 345°C or higher; in some embodiments, the melting point is between 345°C and 400°C, such as 345, 350, 355, 360, 365, 370, 375, 385, 390, 395, or 400°C; the liquid crystal polymer is polymerized by a reactant including a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers, or a combination thereof; the first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or a combination thereof, the second monomers are aromatic hydroxycarboxylic acids, the third monomers are aromatic diols, aliphatic diols, or a combination thereof, and the fourth monomers are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or a combination thereof; forming at least one metal layer attached to a surface of the liquid crystal polymer film.
[0035] For example, the first monomer is [ka] HOOC(CH2) n A1 is a halogen group or an alkyl group, for example, a fluoro group, a chloro group, a bromo group, or an iodo group, and an alkyl group is for example, a methyl group, an ethyl group, an n-propyl group, or an isopropyl group. For example, the second monomer is [ka] or combinations thereof. A2 is a halogen group or an alkyl group, the halogen group being, for example, a fluoro group, a chloro group, a bromo group, or an iodo group, and the alkyl group being, for example, a methyl group, an ethyl group, an n-propyl group, or an isopropyl group. For example, the third monomer is [ka] HO(CH2) n OH (n is an integer from 2 to 12) or a combination thereof. A3 and A4 are independently a halogen group or an alkyl group, and A5 is H, a halogen group or an alkyl group, the halogen group being, for example, a fluoro group, a chloro group, a bromo group or an iodo group, and the alkyl group being, for example, a methyl group, an ethyl group, an n-propyl group or an isopropyl group. For example, the fourth monomer is [ka] or combinations thereof, including, but not limited to,
[0036] In some embodiments, the liquid crystal polymer having a melting point of 345° C. or higher is polymerized with an aromatic diol and an aromatic dicarboxylic acid.
[0037] In some embodiments, the liquid crystal polymer having a melting point of 345° C. or higher is polymerized with an aromatic diol and an aromatic hydroxycarboxylic acid.
[0038] In some embodiments, the liquid crystal polymer is a first type of thermotropic liquid crystal polymer. In some embodiments, the first type of thermotropic liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units. Each of the first monomer units is [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] It is.
[0039] In some embodiments, the liquid crystal polymer having a melting point of 345° C. or more is polymerized with an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid. For example, the liquid crystal polymer is polymerized with 4-hydroxybenzoic acid (HBA), 6-hydroxy-2-naphthalene carboxylic acid (HNA), terephthalic acid (TPA), and hydroquinone (HQ), and the following first monomer unit, second monomer unit, third monomer unit, and fourth monomer unit can be obtained by HBA, HNA, TPA, and HQ, respectively. In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. Each first monomer unit is [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] and each fourth monomer unit is [ka] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol% to 74 mol%, the second monomer units are 14 mol% to 16 mol%, the third monomer units are 5 mol% to 13 mol%, and the fourth monomer units are 5 mol% to 13 mol%. In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol% to 74 mol%, the second monomer units are 16 mol% to 18 mol%, the third monomer units are 9 mol% to 12 mol%, and the fourth monomer units are 9 mol% to 12 mol%. The molar percentages of the first monomer units, the second monomer units, the third monomer units, and the fourth monomer units may be any positive integer within the above numerical ranges.
[0040] Next, a thermal shock test is performed on the laminate including the liquid crystal polymer film and the copper wiring. Please refer to FIG. 5, which is a schematic diagram of performing a thermal shock test according to various embodiments of the present disclosure. The laminate 510 includes a liquid crystal polymer film 512 and a metal layer 514 attached to the lower surface S10 of the liquid crystal polymer film 512. The laminate 520 includes a liquid crystal polymer film 522, a metal layer 524, and a metal layer 526, and the metal layer 526 and the metal layer 524 are attached to the upper surface S11 and the lower surface S12 of the liquid crystal polymer film 522, respectively. The laminate 510 is a single-sided flexible printed circuit board, and the laminate 520 is a double-sided flexible printed circuit board. The laminate 510 and the laminate 520 are overlapped, and the metal layer 524 is in contact with the upper surface S9 of the liquid crystal polymer film 512. The laminate 510 and the laminate 520 are thermocompressed by the cushion pad 532 of the hot electrode 530, and the thickness of the cushion pad 532 is 25 um. The liquid crystal polymer films 512 and 522 are made of the same material, and each contains a liquid crystal polymer polymerized by HBA, HNA, TPA, and HQ, so that the liquid crystal polymer contains the above-mentioned first monomer unit, second monomer unit, third monomer unit, and fourth monomer unit. The liquid crystal polymer films 512 and 522 are 50 um thick, and the metal layers 514, 524, and 526 are copper wiring, and the copper wiring has a thickness of 12 um, a line width of 1 mm, and a line distance of 1 mm. The thermocompression temperature may be 250°C to 320°C, the thermocompression pressure is 10 N, the thermocompression time is 20 seconds, and the thermocompression number is 10. Please refer to FIG. 6, which is a schematic bottom view of a laminate according to various embodiments of the present disclosure. The laminate 510 shown in Fig. 5 is a local cross-sectional view of the laminate 510 in Fig. 6. The wiring patterns of the metal layers 524 and 526 may be designed with reference to the wiring pattern of the metal layer 514. See Table 1 below for the test results of thermal shock on different liquid crystal polymer films. [Table 1]
[0041] As can be seen from Table 1, the melting points of the liquid crystal polymer films of Examples 1 to 4 are greater than 345°C. A liquid crystal polymer film having a melting point of 350°C can withstand a thermocompression temperature of 275°C, and more specifically, the copper wiring of this liquid crystal polymer laminate does not collapse into the liquid crystal polymer film at 275°C. A liquid crystal polymer film having a melting point of 355°C can withstand a thermocompression temperature of 285°C, and more specifically, the copper wiring of this liquid crystal polymer laminate does not collapse into the liquid crystal polymer film at 285°C. On the contrary, in Comparative Example 1 and Comparative Example 2, the melting points of the liquid crystal polymer films are less than 345°C, so the copper wiring collapses completely into the liquid crystal polymer film.
[0042] The present disclosure provides another method for manufacturing a laminate, which includes the following operations: A first liquid crystal polymer film is prepared from a liquid crystal polymer having a melting point of less than 345°C. The liquid crystal polymer is polymerized by a reactant including a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers, or a combination thereof. The first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or a combination thereof, the second monomers are aromatic hydroxycarboxylic acids, the third monomers are aromatic diols, aliphatic diols, or a combination thereof, and the fourth monomers are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or a combination thereof. For the embodiments of the first monomers, the second monomers, the third monomers, and the fourth monomers, please refer to the above-mentioned embodiments, and the description thereof will be omitted here. By adjusting the ratio of the monomers used to synthesize the liquid crystal polymer, the melting point of the liquid crystal polymer can be less than, equal to, or greater than 345°C. The first melting point of the first liquid crystal polymer film is T m and T m The first liquid crystal polymer film is heated by a heating process to form a second liquid crystal polymer film having a second melting point of 345° C. or more. The heating temperature of the heating process is T m -40℃~T mAt least one metal layer is formed on the surface of the second liquid crystal polymer film. The laminate of any one of the above-mentioned embodiments can be manufactured by this method, and the laminate can be a single-sided plate or a double-sided plate.
[0043] In some embodiments, the heating temperature is, for example, T m -40, T m -35, T m -30, T m -25, T m -20, T m -15, T m -10, T m -5 or T m ℃. During heating, the polymer in the liquid crystal polymer film is rearranged, which increases the molecular weight of the polymer, makes the polymer arrangement more orderly, and increases the melting point of the liquid crystal polymer film. By increasing the melting point, the liquid crystal polymer film can have good heat resistance, and when a multi-layer liquid crystal polymer laminate is pressed to form a multi-layer plate, the quality of the pressing can be good, and the metal wiring is less likely to fall into the liquid crystal polymer film. In some embodiments, the heating rate of the heating process is 0.1 ℃ / min to 30 ℃ / min. The heating rate is, for example, 0.1, 0.5, 1, 5, 10, 15, 20, 25, or 30 ℃ / min. In some embodiments, the heating time of the heating process is 10 minutes to 900 minutes. The heating time is, for example, 10, 20, 40, 60, 80, 100, 200, 300, 400, 500, 600, 700, 800, or 900 minutes. In some embodiments, the heating process is carried out in an inert environment, for example, the inert gas in the inert environment is argon gas, nitrogen gas, or a combination thereof.
[0044] In some embodiments, the liquid crystal polymer having a melting point of less than 345° C. is polymerized with an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid. In some embodiments, the liquid crystal polymer having a melting point of less than 345° C. is polymerized with an aromatic diol and an aromatic dicarboxylic acid. In some embodiments, the liquid crystal polymer having a melting point of less than 345° C. is polymerized with an aromatic diol and an aromatic hydroxycarboxylic acid.
[0045] In some embodiments, the reactants include different first and second aromatic hydroxycarboxylic acids. In some embodiments, the liquid crystal polymer film includes a second type of thermotropic liquid crystal polymer. In some embodiments, the second type of thermotropic liquid crystal polymer is polymerized with p-hydroxybenzoic acid (HBA) and 6-hydroxy-2-naphthoic acid (HNA). The following first and second monomer units can be obtained by HBA and HNA, respectively. In some embodiments, the liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units. Each first monomer unit is [ka] and each second monomer unit is [ka] and the first monomer units are 70 mol % to 85 mol % and the second monomer units are 15 mol % to 30 mol %. The molar percentages of the first monomer units and the second monomer units may be any positive integer within the above numerical ranges.
[0046] In some embodiments, the liquid crystal polymer having a melting point of less than 345° C. is polymerized with an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aromatic hydroxylamine. In some embodiments, the liquid crystal polymer is polymerized with 6-hydroxy-2-naphthoic acid (HNA), terephthalic acid (TPA), and p-aminophenol (AP). The second monomer unit, the third monomer unit, and the fourth monomer unit in the following liquid crystal polymer can be obtained by HNA, TPA, and AP, respectively. In some embodiments, the liquid crystal polymer includes a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. Each second monomer unit is [ka] and each third monomer unit is [ka] and each fourth monomer unit is [ka] and the second monomer units are 55 mol % to 65 mol %, the third monomer units are 15 mol % to 25 mol %, and the fourth monomer units are 15 mol % to 25 mol %. The molar percentages of the second monomer units, the third monomer units, and the fourth monomer units may be any positive integer within the above numerical ranges.
[0047] In some embodiments, the liquid crystal polymer having a melting point of less than 345° C. is polymerized with an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid. In some embodiments, the liquid crystal polymer is polymerized with p-hydroxybenzoic acid (HBA), 6-hydroxy-2-naphthoic acid (HNA), terephthalic acid (TPA), and 4,4′-biphenol (BP). The first monomer unit, the second monomer unit, the third monomer unit, and the fifth monomer unit in the following liquid crystal polymer can be obtained by HBA, HNA, TPA, and BP, respectively. In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fifth monomer units. Each first monomer unit is [ka] and each second monomer unit is [ka] and each third monomer unit is [ka] and each fifth monomer unit is [ka] It is.
[0048] For the melting points and molar percentages of the monomer units of the liquid crystal polymer films 1 to 4, see Table 2 below. [Table 2]
[0049] In some embodiments, the liquid crystal polymer is polymerized with an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aliphatic diol. [ka] It contains the monomer unit:
[0050] Next, a thermal shock test was performed in the arrangement shown in FIG. 5, and the test results are shown in Table 3 below. During the test, the liquid crystal polymer film 1 or the liquid crystal polymer film 3 in Table 2 above was selected as the liquid crystal polymer film of Comparative Example 3 and Examples 5 to 7, and the melting point of the liquid crystal polymer film was adjusted by a heating process to obtain the melting point after heating in Table 3. After copper wiring was formed on the liquid crystal polymer film, a thermal shock test was performed. After copper wiring was formed on the liquid crystal polymer film, the liquid crystal polymer film 2 in Table 2 above was selected as the liquid crystal polymer film of Comparative Example 4 and Examples 8 to 9, and the melting point of the liquid crystal polymer film was adjusted by a heating process to obtain the melting point after heating in Table 3. After copper wiring was formed on the liquid crystal polymer film, a thermal shock test was performed. [Table 3]
[0051] As can be seen from Table 3, the liquid crystal polymer films having melting points of 345°C, 350°C and 355°C after heating can withstand the thermocompression temperatures of 260°C, 275°C and 285°C, respectively, and in particular, the copper wiring of these liquid crystal polymer laminates does not collapse into the liquid crystal polymer film at the above thermocompression temperatures. On the contrary, in Comparative Example 3 and Comparative Example 4, since the melting points of the liquid crystal polymer films are lower than 345°C, the copper wiring collapses completely into the liquid crystal polymer film.
[0052] In summary, the present disclosure provides a laminate and a method for manufacturing the same, and a multilayer board. The laminate includes a liquid crystal polymer film and at least one metal layer attached to the surface of the liquid crystal polymer film. Since the laminate of the present disclosure has good heat resistance, when a multilayer board is formed by thermocompression bonding of multiple laminates, it is possible to avoid the metal wiring from falling into the liquid crystal polymer film, thereby avoiding problems such as impedance error of the circuit due to deformation of the wiring, increased transmission loss, and increased crosstalk between wiring. Therefore, the multilayer board can have good quality after thermocompression bonding.
[0053] Although the present disclosure has been described in considerable detail with reference to certain embodiments, other embodiments are possible, and therefore, the spirit and scope of the appended claims should not be limited to the description of the embodiments contained herein.
[0054] It will be apparent to those skilled in the art that various modifications and variations can be made to the structure of the present disclosure without departing from the scope or spirit of the disclosure. In view of the foregoing, it is intended that the present disclosure cover modifications and variations of the present disclosure that fall within the scope of the appended claims. [Explanation of symbols]
[0055] 110, 120, 210, 220, 310, 320, 410, 420, 430, 440, 450, 460, 510, 520 Laminates 212, 222, 312, 322, 512, 522 Liquid crystal polymer film 214, 216, 224, 314, 324, 514, 524, 526 metal layer 530 Thermal Electrode 532 Cushion Pad ML1, ML2, ML3, ML4, ML5 multilayer board S1, S3, S5, S7, S9, S11 Top S2, S4, S6, S8, S10, S12 Bottom side
Claims
1. a liquid crystal polymer film comprising a liquid crystal polymer having a melting point of 345° C. or more, polymerized by a reactant comprising a plurality of first monomers which are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, a plurality of second monomers which are aromatic hydroxycarboxylic acids, a plurality of third monomers which are aromatic diols, aliphatic diols or a combination thereof, a plurality of fourth monomers which are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids or a combination thereof, or a combination thereof; at least one metal layer attached to a surface of the liquid crystal polymer film; A laminate comprising:
2. 2. The laminate according to claim 1, wherein the liquid crystal polymer is formed by polymerization of the aromatic diol, the aromatic dicarboxylic acid, and the aromatic hydroxycarboxylic acid.
3. 2. The laminate according to claim 1, wherein the liquid crystal polymer is formed by polymerization of the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid, and the aromatic hydroxyamine.
4. 2. The laminate according to claim 1, wherein the liquid crystal polymer is formed by polymerization of the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid, and the aliphatic diol.
5. The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units, each of the first monomer units being 【Chemistry 1】 and each second monomer unit is 【Chemistry 2】 and each third monomer unit is 【Chemistry 3】 and each fourth monomer unit is 【Chemistry 4】 2. The laminate according to claim 1 .
6. 6. The laminate according to claim 5, wherein in the liquid crystal polymer, the plurality of first monomer units are 60 mol% to 74 mol%, the plurality of second monomer units are 14 mol% to 16 mol%, the plurality of third monomer units are 5 mol% to 13 mol%, and the plurality of fourth monomer units are 5 mol% to 13 mol%.
7. 6. The laminate according to claim 5, wherein in the liquid crystal polymer, the plurality of first monomer units are 60 mol% to 74 mol%, the plurality of second monomer units are 16 mol% to 18 mol%, the plurality of third monomer units are 9 mol% to 12 mol%, and the plurality of fourth monomer units are 9 mol% to 12 mol%.
8. The liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units, each of the first monomer units being 【Chemistry 5】 and each second monomer unit is 【Chemistry 6】 2. The laminate according to claim 1, wherein the first monomer units are present in an amount of 70 mol % to 85 mol % and the second monomer units are present in an amount of 15 mol % to 30 mol %.
9. The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units, each of the first monomer units being 【Chemistry 7】 and each second monomer unit is 【Chemistry 8】 and each third monomer unit is 【Chemistry 9】 2. The laminate of claim 1, wherein the first monomer units are 55 mol% to 65 mol%, the second monomer units are 15 mol% to 25 mol%, and the third monomer units are 15 mol% to 25 mol%.
10. At least one single-sided board or at least one double-sided board; The laminate according to any one of claims 1 to 9, which is bonded to the at least one single-sided board or the at least one double-sided board; A multilayer board including
11. preparing a liquid crystal polymer film from a liquid crystal polymer having a melting point of 345° C. or greater, the liquid crystal polymer being polymerized by reactants including a plurality of first monomers which are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or combinations thereof, a plurality of second monomers which are aromatic hydroxycarboxylic acids, a plurality of third monomers which are aromatic diols, aliphatic diols, or combinations thereof, a plurality of fourth monomers which are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or combinations thereof, or combinations thereof; forming at least one metal layer attached to a surface of the liquid crystal polymer film; A method for producing a laminate comprising the steps of:
12. The method according to claim 11 , wherein the liquid crystal polymer is polymerized from the aromatic diol, the aromatic dicarboxylic acid, and the aromatic hydroxycarboxylic acid.
13. The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units, each of the first monomer units being 【Chemistry 10】 and each second monomer unit is 【Chemistry 11】 and each third monomer unit is 【Chemistry 12】 and each fourth monomer unit is 【Chemistry 13】 The method according to claim 11, wherein
14. 14. The method of claim 13, wherein in the liquid crystal polymer, the plurality of first monomer units is 60 mol% to 74 mol%, the plurality of second monomer units is 14 mol% to 16 mol%, the plurality of third monomer units is 5 mol% to 13 mol%, and the plurality of fourth monomer units is 5 mol% to 13 mol%.
15. 14. The method of claim 13, wherein in the liquid crystal polymer, the plurality of first monomer units is 60 mol% to 74 mol%, the plurality of second monomer units is 16 mol% to 18 mol%, the plurality of third monomer units is 9 mol% to 12 mol%, and the plurality of fourth monomer units is 9 mol% to 12 mol%.
16. 1. A liquid crystal polymer having a melting point of less than 345° C. and polymerized by a reactant comprising a plurality of first monomers which are aromatic dicarboxylic acids, aliphatic dicarboxylic acids, or combinations thereof, a plurality of second monomers which are aromatic hydroxycarboxylic acids, a plurality of third monomers which are aromatic diols, aliphatic diols, or combinations thereof, a plurality of fourth monomers which are aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, or combinations thereof, m preparing a first liquid crystal polymer film, Heating temperature is T m -40℃~T m heating the first liquid crystal polymer film by a heating process, forming at least one metal layer attached to a surface of the second liquid crystal polymer film; A method for producing a laminate comprising the steps of:
17. 17. The method according to claim 16, wherein the liquid crystal polymer is polymerized from the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid and the aromatic hydroxyamine.
18. The method according to claim 16, wherein the liquid crystal polymer is polymerized from the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid, and the aliphatic diol.
19. The liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units, each of the first monomer units being 【Chemistry 14】 and each second monomer unit is 【Chemistry 15】 17. The method of claim 16, wherein the plurality of first monomer units is between 70 mol% and 85 mol% and the plurality of second monomer units is between 15 mol% and 30 mol%.
20. The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units, each of the first monomer units being 【Chemistry 16】 and each second monomer unit is 【Chemistry 17】 and each third monomer unit is 【Chemistry 18】 17. The method of claim 16, wherein the first plurality of monomer units is 55 mol% to 65 mol%, the second plurality of monomer units is 15 mol% to 25 mol%, and the third plurality of monomer units is 15 mol% to 25 mol%.
Citation Information
Patent Citations
Liquid crystal polyester resin composition
JP2015174913A
Thermoplastic polyester resin composition, molded product, and method for producing molded product
JP2021031574A
Thermoplastic liquid crystal polymer film, laminate, and molded article, and methods for producing the same
JP2022070936A
Thermoplastic liquid crystal polymer film, laminate, and molded article, and methods for producing the same
JP2022070938A
Porous liquid crystal polymer sheet, porous liquid crystal polymer sheet with metal layer, and electronic circuit board
JP7521702B2