Cured product and printed wiring board
A photosensitive resin composition with controlled inorganic filler content and water absorption rates addresses warpage and resolution issues in printed wiring boards, ensuring reliable electronic component mounting.
Patent Information
- Application Number
- JP2024144090
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
AI Technical Summary
Printed wiring boards warp when exposed to humidity changes during electronic component mounting due to high water absorption and low resolution caused by excessive inorganic filler content in photosensitive resin compositions.
A photosensitive resin composition with an inorganic filler content of 85% by mass or less, an elastic modulus of 4 to 12 GPa, and controlled water absorption rates (A≦0.3% and B-A≦0.3%) is used to form a cured product that maintains high resolution and suppresses substrate warpage.
The solution effectively reduces substrate warpage and maintains high resolution, ensuring reliable electronic component mounting by controlling the composition and curing conditions of the photosensitive resin.
Smart Images

Figure 2024161097000001 
Figure 2024161097000002 
Figure 2024161097000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cured product, and more specifically to a cured product of a photosensitive resin composition that can be suitably used as an insulating layer such as a solder resist, and a printed wiring board using the cured product. [Background technology]
[0002] In general, in a printed wiring board used in electronic devices, a solder resist layer is formed in an area other than a connection hole on a substrate on which a circuit pattern is formed, in order to prevent solder from adhering to unnecessary parts of the printed wiring board in a process such as solder reflow when mounting electronic components on the printed wiring board. The solder resist layer is mainly formed by applying a photosensitive resin composition to a substrate, drying it, exposing it to light, developing it to form a pattern, and then curing the patterned resin by heating or irradiating it with light, which is called a photo solder resist. It has also been proposed to form a solder resist layer using a photosensitive dry film without using the above-mentioned liquid photosensitive resin composition.
[0003] These photosensitive resin compositions and photosensitive dry films contain an alkali-soluble photosensitive resin component to enable exposure and development, and, if necessary, contain other photopolymerizable monomers and thermosetting components such as epoxy in consideration of heat resistance, substrate adhesion, etc. In addition, inorganic fillers are sometimes blended into the photosensitive resin composition to reduce the linear expansion coefficient and suppress peeling of the solder resist layer and warping of the substrate (Patent Document 1, etc.).
[0004] On the other hand, as the amount of inorganic filler increases, a cured product with a low linear expansion coefficient is obtained, but the resolution during exposure tends to decrease. Therefore, in order to obtain a photosensitive resin composition that contains inorganic filler but has high resolution, a specific photopolymerization initiator is used or a sensitizer is used in combination (Patent Document 2, etc.). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-72834 A [Patent Document 2] International Publication No. 2015-16362 Brochure Summary of the Invention
[0006] The printed wiring board manufactured as described above is placed in a low humidity environment by pouch packaging or the like, and is used by being taken out of the pouch packaging at the stage of mounting electronic components. If a certain amount of time passes between the time when the substrate is taken out of the pouch packaging and the time when electronic components are mounted on the substrate, the substrate may warp, resulting in mounting defects. On the other hand, when the photosensitive resin composition containing a large amount of inorganic filler as described above is used, the substrate is less likely to warp when electronic components are mounted, but the resolution tends to decrease.
[0007] Therefore, an object of the present invention is to provide a cured product of a photosensitive resin composition which has high resolution and can suppress warping of a substrate when electronic components are mounted thereon.
[0008] The present inventors have conducted research into the above-mentioned problems and have found that by making a photosensitive resin composition in which the content of inorganic filler in the composition is a certain value or less and the water absorption rate of the cured product cured under specified curing conditions is a certain value or less, it is possible to reduce warpage even when the composition is used as a printed wiring board while maintaining excellent resolution. The present invention is based on this finding. That is, the gist of the present invention is as follows.
[0009] [1] A cured product of a photosensitive resin composition comprising at least an alkali-soluble resin, a photopolymerization initiator, and an inorganic filler, The inorganic filler is contained in an amount of 85% by mass or less based on the entire photosensitive resin composition, The elastic modulus of the cured product is 4 to 12 GPa; The cured product is The water absorption rate of the cured product after being left for 60 minutes in an environment of 25°C and 10% relative humidity is A (%), When the water absorption rate of the cured product after being left for 60 minutes in an environment of 25°C and 60% relative humidity is B (%), A≦0.3%, and BA≦0.3 The cured product is characterized by satisfying the above. [2] The cured product according to [1], wherein the inorganic filler is contained in an amount of 45 to 65 mass% based on the total mass of the photosensitive resin composition. [3] The cured product according to [1], wherein the inorganic filler is surface-treated with a silane coupling agent. [4] The cured product according to [1], wherein the photosensitive resin composition further contains a sensitizer in an amount of 0.01 to 10 mass % based on the total amount of the photosensitive resin composition. [5] The cured product according to [4], wherein the sensitizer is an anthraquinone-based sensitizer having an ester bond. [6] A printed wiring board comprising: a substrate; and a coating formed on the substrate, the coating being made of the cured product according to any one of [1] to [5].
[0010] According to the present invention, by containing an inorganic filler in a ratio not exceeding a predetermined amount and forming a cured product having a predetermined water absorption characteristic, it is possible to realize a cured product of a photosensitive resin composition that has high resolution even while containing an inorganic filler and can suppress warping of a board when electronic components are mounted on it. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Cured product] The present invention relates to a cured product of a photosensitive resin composition comprising at least an alkali-soluble resin, a photopolymerization initiator, and an inorganic filler, the cured product having an elastic modulus of 4 to 12 GPa, and when the water absorption rate of the cured product after being left for 60 minutes in an environment of 25°C and a relative humidity of 10% is A (%) and the water absorption rate of the cured product after being left for 60 minutes in an environment of 25°C and a relative humidity of 10% is B (%), A≦0.3, and BA≦0.3 The present invention provides a cured product that satisfies the above requirements. By containing an inorganic filler in a proportion of 85 mass% or less based on the entire photosensitive resin composition and adjusting the composition of the photosensitive resin composition and curing conditions so that the water absorption rate of the cured product falls within the above-mentioned specified range, it is possible to achieve high resolution and suppress warping of the board when mounting electronic components. The reason for this is unclear, but is thought to be as follows.
[0012] The water absorption rate of the cured product when the photosensitive resin composition is cured depends on the components constituting the photosensitive resin composition, but it is considered that not only the water absorption rate of the components but also the interaction of the components constituting the cured product, such as the degree of crosslinking, is related. In the present invention, the cured product has an elastic modulus in the range of 4 to 12 GPa, and the lower the water absorption rate of the cured product, the more the warping of the printed wiring board is suppressed. In addition, by using a photosensitive resin composition that has a lower water absorption rate when the cured product is formed, the warping of the substrate that occurs when the photosensitive resin composition is applied to the substrate or a dry coating film (dry film) of the photosensitive resin composition is laminated to the substrate is also reduced. As a result, it is considered that the decrease in resolution due to the influence of the warping of the substrate is suppressed. In other words, it is considered that both the warping of the substrate before curing of the photosensitive resin composition and the warping of the substrate after curing can be simultaneously reduced by adjusting the composition of the photosensitive resin composition and the curing conditions so that the elastic modulus of the cured product is in a predetermined range and the water absorption rate is equal to or less than a certain value.
[0013] From the viewpoints of resolution and suppression of warpage of the substrate, the elastic modulus of the cured product of the present invention is preferably in the range of 6 to 12 GPa, more preferably in the range of 7 to 9 GPa. In the present invention, the elastic modulus of the cured product means a value calculated from a stress-strain curve measured in accordance with JIS K 7127, and specifically, a tensile test is performed on the cured product using a tensile tester at an environment of 25°C and a tensile speed of 1 mm / min, and the elastic modulus is the slope of a straight line calculated from the obtained stress-strain curve between stresses of 2 N and 7 N.
[0014] From the viewpoints of resolution and suppression of warpage of the substrate, the cured product of the present invention preferably has an A value of 0.25% or less, and more preferably 0.2% or less. In other words, the cured product preferably has a low water absorption rate in a dry state (relative humidity 10%). The BA value is preferably 0.25% or less, and more preferably 0.2%. In the present invention, the water absorption rate of the cured product can be specifically measured as follows.
[0015] First, the photosensitive resin composition is applied to the entire surface of a copper-clad laminate (MCL-E-770G, manufactured by Showa Denko K.K., copper thickness 18 μm) having a thickness of 200 μm and a size of 100×100 mm as a support, so that the film thickness after curing is 20 μm, to form a dry coating film, which is then exposed to light and then heated to cure the coating film, and the cured coating film is peeled off from the support to obtain a cured product. The peeled off cured product is placed on a weighing dish, and the mass of the cured product after leaving it in an environment of 100° C. for 1 hour (absolutely dry state) is measured as W 0 The amount of the sample placed in the weighing dish may be about 10 to 50 mg. Next, the cured product is left for 60 minutes in an environment of 25°C and 10% relative humidity, and then the mass of the cured product is measured (the mass at this time is W 10 (Assuming that.) The cured product was then left for 60 minutes in an environment of 25°C and 60% relative humidity, after which the mass of the cured product was measured (the mass at this time was W 60 (Assuming that.) The water absorption rates A and B of the cured material are defined as follows: Water absorption rate A(%)=(W 10 -W 0 ) / W 0 ×100 Water absorption rate B(%)=(W 60 -W 0 ) / W 0 ×100
[0016] The above-mentioned measurement is a procedure for measuring the water absorption rate of a cured product formed from a photosensitive resin composition, and it goes without saying that the measurement can be performed in the same way when a coating of the cured product is provided in advance on a support such as a copper-clad laminate. For example, when a coating of the cured product is provided in advance on a support, the surface of the coating of the cured product is peeled or scraped off and used as a sample, and the water absorption rate of the cured product is measured as described above. 0、 W 10、 W 60 By measuring the respective values of water absorption rate A and water absorption rate B, it is possible to measure the water absorption rate A and water absorption rate B.
[0017] The elastic modulus and water absorption rate of the cured product can be controlled by appropriately adjusting the components of the photosensitive resin composition, the blending ratio of each component, the curing conditions, etc. Each component constituting the photosensitive resin composition according to the present invention will be described below.
[0018] <Alkali-soluble resin> The alkali-soluble resin may be any resin that is alkali-soluble, and known and commonly used resins are used. The alkali-soluble resin may be used alone or in combination of two or more. Examples include water-soluble resins such as carboxyl group-containing resins and phenolic hydroxyl group-containing resins. Among them, carboxyl group-containing resins and phenolic hydroxyl group-containing resins are preferred because of their excellent developability, and carboxyl group-containing resins are more preferred. The alkali-soluble resin can be made alkaline developable by containing a carboxyl group. In addition, from the viewpoint of photosensitivity, it is preferable to have an ethylenically unsaturated double bond in the molecule in addition to the carboxyl group, but only a carboxyl group-containing resin that does not have an ethylenically unsaturated double bond may be used. When the carboxyl group-containing resin does not have an ethylenically unsaturated double bond, it is necessary to use a photopolymerizable monomer in combination to make the composition photocurable. As the ethylenically unsaturated double bond, those derived from acrylic acid or methacrylic acid or derivatives thereof are preferred.
[0019] Specific examples of carboxyl group-containing resins include the following compounds (which may be either oligomers or polymers): In this specification, (meth)acrylate is a general term for acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.
[0020] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0021] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0022] (3) Carboxylic acid-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.
[0023] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).
[0024] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).
[0025] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.
[0026] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0027] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0028] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.
[0029] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0030] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0031] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).
[0032] These carboxyl group-containing resins are not limited to those listed above, and may be used alone or in combination of two or more kinds.
[0033] The acid value of the carboxyl group-containing resin is preferably 40 to 150 mgKOH / g. By making the acid value of the carboxyl group-containing resin 40 mgKOH / g or more, alkaline development becomes good. Also, by making the acid value 150 mgKOH / g or less, it becomes easy to draw a good resist pattern. More preferably, it is 50 to 130 mgKOH / g.
[0034] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000. By making the weight average molecular weight 2,000 or more, it is possible to improve tack-free performance and resolution. Furthermore, by making the weight average molecular weight 150,000 or less, it is possible to improve developability and storage stability. It is more preferably 5,000 to 15,000. The weight average molecular weight can be measured by gel permeation chromatography (GPC).
[0035] The amount of the carboxyl group-containing resin in the photosensitive resin composition is preferably 10 to 50% by mass, calculated as solid content. By making it 10% by mass or more, the coating strength can be improved. Also, by making it 50% by mass or less, the viscosity becomes appropriate and the printability is improved. More preferably, it is 10 to 30% by mass.
[0036] <Photopolymerization initiator> The photosensitive resin composition according to the present invention contains a photopolymerization initiator for photopolymerization. As the photopolymerization initiator, known ones can be used, for example, α-aminoacetophenone-based photopolymerization initiators such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and N,N-dimethylaminoacetophenone; 1-hydroxy-cyclohexylphenylketone; Hydroxyacetophenone photoinitiators such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, and 2-hydroxy-2-methyl-1-phenylpropan-1-one; bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethyl Phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylphenylphosphine oxide, acylphosphine oxide photopolymerization initiators such as methylbenzoyl)-phenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphine acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenylphosphine acid isopropyl ester, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide;Benzoin-based photopolymerization initiators such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ether-based photopolymerization initiators; benzophenone-based photopolymerization initiators such as benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone; acetophenone, 2,2-dimethoxy-2-phenylacetophenone acetophenone-based photopolymerization initiators such as 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone; thioxanthone-based photopolymerization initiators such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chlorothioxanthone, and chlorothioxanthone; Anthraquinone-based photopolymerization initiators such as chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketal-based photopolymerization initiators such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoic acid ester-based photopolymerization initiators such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenyl)anthraquinone ... oxime ester photoinitiators such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium;These photopolymerization initiators may be used alone or in combination of two or more.
[0037] Commercially available α-aminoacetophenone-based photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins. Commercially available acylphosphine oxide photopolymerization initiators include Omnirad 819 manufactured by IGM Resins. Commercially available titanocene photopolymerization initiators include JMT-784 manufactured by Yueyang Kimoutain Sci-Tech Co., Ltd. and GR-FMT manufactured by Hubei Kimoutain Sci-Tech Co., Ltd.
[0038] In addition, a photopolymerization initiator having two oxime ester groups in the molecule can also be suitably used, and specific examples thereof include oxime ester compounds having a carbazole structure represented by the following general formula (I).
[0039] [ka]
[0040] In the above formula, X represents a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), a naphthyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), and Y and Z each represent a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, Ar represents an alkylene having 1 to 10 carbon atoms, vinylene, phenylene, biphenylene, pyridylene, naphthylene, thiophene, anthrylene, thienylene, furylene, 2,5-pyrrole-diyl, 4,4'-stilbene-diyl, or 4,2'-styrene-diyl, and n is an integer of 0 or 1.
[0041] In particular, in the above formula, X 1 , Y 1 are each a methyl group or an ethyl group, Z is methyl or phenyl, n is 0, and Ar is phenylene, naphthylene, thiophene, or thienylene.
[0042] The amount of the photopolymerization initiator in the photosensitive resin composition is preferably 1 to 50 parts by mass, and more preferably 1 to 20 parts by mass, calculated as solid content, relative to 100 parts by mass of the carboxyl group-containing resin, which can improve the curing property in deep portions.
[0043] <Sensitizer> The photosensitive resin composition of the present invention preferably contains a sensitizer in combination with the above-mentioned photopolymerization initiator. By using a sensitizer in combination, the water absorption rate of the cured product can be reduced without increasing the amount of inorganic filler to be described later, and a cured product with high resolution and hardness can be obtained.
[0044] As the sensitizer, a conventionally known one can be used, and examples thereof include benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. Among these, thioxanthone compounds and anthraquinone compounds can be preferably used from the viewpoint of deep section curing.
[0045] Among the above-mentioned sensitizers, compounds having functional groups such as ester groups and amino groups are considered to react with the above-mentioned alkali-soluble resins and photopolymerizable monomers described below, and a crosslinked structure is partially formed in the cured product obtained by curing the photosensitive resin composition. As a result, the water absorption rate of the cured product can be further reduced. Examples of sensitizers having such functional groups include anthraquinone-based sensitizers represented by the following formula.
[0046] [ka]
[0047] The anthraquinone sensitizer may be a commercially available product, for example, Anthracure UVS-581 (manufactured by Kawasaki Chemical Industries, Ltd.).
[0048] The amount of the sensitizer is preferably 0.01 to 10% by mass, and more preferably 0.01 to 3% by mass, based on the total amount of the photosensitive resin composition, which can reduce the water absorption of the cured product while maintaining excellent resolution.
[0049] <Inorganic filler> The photosensitive resin composition according to the present invention contains an inorganic filler. By incorporating an inorganic filler, the water absorption rate of the cured product can be reduced, and the cured product can be given necessary strength and reduced in thermal expansion coefficient. As the inorganic filler, known ones can be used, and in particular, silica, talc, mica, aluminum oxide, calcium oxide, magnesium oxide, zinc oxide, calcium carbonate, magnesium carbonate, fly ash, dewatered sludge, kaolin, clay, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, aluminum silicate, magnesium silicate, calcium silicate, wollastonite, potassium titanate, magnesium sulfate, calcium sulfate, magnesium phosphate, sepiolite, zonolite, boron nitride, aluminum borate, silica balloon, glass flake, glass balloon, iron slag, copper, iron, iron oxide, sendust, alnico magnet, magnetic powder such as various ferrites, cement, glass powder, Neuburg diatomaceous earth, diatomaceous earth, antimony trioxide, magnesium oxysulfate, aluminum hydrate, hydrated gypsum, alum, barium sulfate, etc. can be mentioned. These inorganic fillers can be used alone or in combination of two or more. Among the above, silica is preferable.
[0050] From the viewpoint of dispersibility, the inorganic filler preferably has an average particle size (D50) of 0.1 to 100 μm, more preferably 0.1 to 50 μm. The average particle size means a particle size at 50% cumulative volume obtained by using a laser diffraction scattering particle size distribution measurement method. The average particle size of the filler means a value measured as described above for the filler before preparing (preliminary mixing, kneading) the photosensitive resin composition.
[0051] The amount of inorganic filler in the photosensitive resin composition must be 85% by mass or less based on the total amount of the photosensitive resin composition from the viewpoint of achieving both the elastic modulus, water absorption rate, and resolution of the cured product. If the amount exceeds 85% by mass, the water absorption rate of the cured product is reduced and warping is suppressed, but the resolution becomes insufficient. The amount of inorganic filler is preferably 45 to 85% by mass, and more preferably 45 to 65% by mass.
[0052] The above-mentioned filler may be surface-treated to enhance dispersibility in the photosensitive resin composition. By using a surface-treated inorganic filler, the water absorption rate of the cured product can be further reduced, and as a result, the warping of the printed wiring board can be reduced. The surface treatment method is not particularly limited, and a publicly known and commonly used method may be used, but it is preferable to treat the surface of the inorganic filler with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.
[0053] Examples of the curable reactive group include photocurable reactive groups and thermosetting reactive groups. Examples of the photocurable reactive group include ethylenically unsaturated groups such as vinyl groups, styryl groups, methacryl groups, and acrylic groups. Among these, at least one of vinyl groups and (meth)acrylic groups is preferred. Examples of the thermocurable reactive group include hydroxyl groups, carboxyl groups, isocyanate groups, amino groups, imino groups, epoxy groups, oxetanyl groups, mercapto groups, methoxymethyl groups, methoxyethyl groups, ethoxymethyl groups, ethoxyethyl groups, and oxazoline groups. Among these, at least one of amino groups and epoxy groups is preferred. The surface-treated inorganic filler may have a photocurable reactive group in addition to the thermocurable reactive group.
[0054] As the coupling agent, silane-based, titanate-based, aluminate-based, zircoaluminate-based, and other coupling agents can be used. Among them, silane-based coupling agents are preferred. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane, which can be used alone or in combination. It is preferable that these silane-based coupling agents are immobilized on the surface of the filler in advance by adsorption or reaction. Here, the amount of the coupling agent to be treated with respect to 100 parts by mass of the spherical silica is preferably 0.5 to 10 parts by mass.
[0055] The surface-treated inorganic filler may be contained in the resin layer in a surface-treated state, and the inorganic filler and the silane coupling agent may be separately blended into the photosensitive resin composition to surface-treat the inorganic filler in the composition, but it is preferable to blend the inorganic filler that has been surface-treated in advance. By blending the inorganic filler that has been surface-treated in advance, it is possible to suppress the occurrence of cracks and the like due to the silane coupling agent that was not consumed in the surface treatment that may remain when blended separately. When the surface is treated in advance, it is preferable to blend a pre-dispersion in which the inorganic filler is pre-dispersed in an alkali-soluble resin or solvent, etc., and the surface-treated inorganic filler is pre-dispersed in a solvent and the pre-dispersion is blended into the composition, or it is more preferable to pre-disperse the surface-untreated inorganic filler in a solvent and then sufficiently surface-treat it, and then blend the pre-dispersion into the composition.
[0056] <Photopolymerizable monomer> The photosensitive resin composition of the present invention may contain a photopolymerizable monomer. The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Polyhydric alcohols such as polyhydric alcohols or their alkylene oxide adducts or ε-caprolactone adducts; phenols such as phenoxy acrylate and bisphenol A diacrylate or their alkylene oxide adducts; glycidyl ether acrylates such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and acrylates obtained by directly acrylate or urethane acrylate of polyols such as polyether polyols, polycarbonate diols, hydroxyl group-terminated polybutadiene, and polyester polyols, as well as melamine acrylates and at least one of the methacrylates corresponding to the acrylates, can be appropriately selected and used. Such photopolymerizable monomers can also be used as reactive diluents.
[0057] The photopolymerizable monomer may be used alone or in combination of two or more. The amount of the photopolymerizable monomer is preferably 0.5 to 30 parts by mass in terms of solid content per 100 parts by mass of the carboxyl group-containing resin. When the amount is 0.5 parts by mass or more, the photocurability is good, and pattern formation is easy in alkaline development after irradiation with active energy rays. When the amount is 30 parts by mass or less, halation is unlikely to occur and good resolution can be obtained.
[0058] <Thermosetting component> The photosensitive resin composition of the present invention may contain a thermosetting component. Examples of the thermosetting component include known and commonly used components such as isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy compounds, oxetane compounds, and episulfide resins. Among these, the preferred thermosetting component is an epoxy resin.
[0059] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, and the like. These may be used alone or in combination of two or more.
[0060] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation; YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd.; EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation; and RE-306 manufactured by Nippon Kayaku Co., Ltd.
[0061] The equivalent weight of the epoxy group of the epoxy resin in the photosensitive resin composition is preferably 0.5 to 2.5 in terms of solid content relative to the equivalent weight of the carboxyl group of the carboxyl group-containing resin (1). By making it 0.5 equivalent weight or more, it is possible to prevent the carboxyl group from remaining in the cured product, and to obtain good heat resistance, alkali resistance, electrical insulation, etc. Also, by making the blending amount 2.5 equivalent weight or less, it is possible to prevent the low molecular weight cyclic (thio)ether group from remaining in the dried coating film, and to ensure good strength of the cured product, etc.
[0062] <Thermosetting catalyst> The photosensitive resin composition of the present invention may contain a heat curing catalyst for promoting the curing of the above-mentioned heat curing component. Examples of the heat curing catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Other commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (trade name of dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and salts thereof) manufactured by San-Apro Co., Ltd.
[0063] The compounds are not limited to the above, and may be used alone or in combination of two or more as long as they are heat curing catalysts for epoxy resins or oxetane compounds, or catalysts that promote the reaction of at least one of epoxy groups and oxetanyl groups with carboxyl groups. In addition, S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct may also be used, and preferably, these compounds that also function as adhesion promoters are used in combination with the heat curing catalyst.
[0064] The thermosetting catalyst may be used alone or in combination of two or more. From the viewpoint of the storage stability of the resin composition and the heat resistance of the cured coating, the amount of the thermosetting catalyst is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, calculated as solid content, per 100 parts by mass of the carboxyl group-containing resin.
[0065] <Other ingredients> In addition to the above-mentioned components, the photosensitive resin composition according to the present invention may contain, if necessary, components such as colorants, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based defoamers and leveling agents, and flame retardants such as phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be known in the field of electronic materials.
[0066] The photosensitive resin composition of the present invention may contain an organic solvent from the viewpoints of ease of preparation and coatability. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents can be used alone or in combination of two or more.
[0067] The amount of the organic solvent in the photosensitive resin composition can be appropriately changed depending on the materials constituting the photosensitive resin composition, and can be, for example, 30 to 300 parts by mass in terms of solid content per 100 parts by mass of the (A) carboxyl group-containing resin.
[0068] The photosensitive resin composition of the present invention may be used in the form of a dry film or in the form of a liquid. When used in the form of a liquid, the composition may be one-component or two or more-component.
[0069] <Dry film> The above-mentioned photosensitive resin composition can be in the form of a dry film having a first film and a resin layer made of the photosensitive resin composition formed on the first film. The cured product of the present invention is obtained by curing the above-mentioned photosensitive resin composition or the resin layer of the above-mentioned dry film.
[0070] The first film in the dry film according to the present invention refers to a film that is at least adhered to the resin layer when the dry film is laminated by heating or the like so that the resin layer side made of the photosensitive resin composition formed on the dry film is in contact with a base material such as a substrate to be integrally molded. The first film may be peeled off from the resin layer in a step after lamination. In particular, in the present invention, it is preferable to peel off from the resin layer in a step after exposure.
[0071] To prepare a dry film, the photosensitive resin composition of the present invention is diluted with an organic solvent to adjust the viscosity to an appropriate level, and then coated onto a first film in a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and typically dried for 1 to 30 minutes at a temperature of 50 to 130° C. to obtain a film. There are no particular limitations on the coating film thickness, but it is generally appropriately selected within the range of 1 to 150 μm, preferably 10 to 60 μm, in terms of the film thickness after drying.
[0072] As the first film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the first film.
[0073] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.
[0074] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0075] After forming a resin layer of the photosensitive resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer, etc. The second film in the dry film of the present invention refers to a film that is peeled off from the resin layer before lamination when the dry film is laminated by heating or the like so that the resin layer side of the dry film is in contact with a base material such as a substrate to be integrally molded.
[0076] The second film that can be peeled off from the resin layer may be, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc., as long as the adhesive strength between the resin layer and the second film is smaller than the adhesive strength between the resin layer and the first film when the second film is peeled off.
[0077] The thickness of the second film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0078] [Printed wiring board] The printed wiring board of the present invention comprises a substrate and a cured coating film made of a cured product provided on the substrate. As described above, the cured product of the present invention can be obtained from a resin layer of a photosensitive resin composition or a dry film. As a method for producing the printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and coated on a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100 ° C. to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off to form a resin layer on the substrate.
[0079] The above-mentioned substrates include printed wiring boards and flexible printed wiring boards with circuits formed in advance using copper or the like, as well as materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high-frequency circuits using materials such as fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.
[0080] In the case of a dry film form, the lamination onto the substrate is preferably performed under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, even if the surface of the circuit substrate is uneven, the dry film adheres to the circuit substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0081] When the photosensitive resin composition of the present invention contains an organic solvent, it is preferable to apply the photosensitive resin composition to the surface of a substrate and then perform volatilization drying. The volatilization drying can be performed using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of countercurrent contact of hot air in a dryer using a heat source of an air heating method using steam, or a method of spraying the hot air from a nozzle onto the substrate).
[0082] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed portion is developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of the cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is performed to form a patterned cured product on the substrate. In addition, in the case of a dry film form, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed, as long as the characteristics are not impaired. Furthermore, a cured coating excellent in various properties such as adhesion and hardness can be formed by irradiating the cured product with active energy rays and then heat curing (e.g., 100 to 220°C), or irradiating active energy rays after heat curing, or by heat curing only to perform final finish curing (main curing).
[0083] When the cured product is prepared as described above, the elastic modulus of the cured product can be adjusted by changing the curing conditions. The elastic modulus is a physical property value that indicates the resistance of the cured product to deformation. For example, the degree of progress of the crosslinking reaction of the reactive group changes depending on the conditions of photocuring and thermal curing, and as a result, the elastic modulus of the cured product is also affected. In other words, if the degree of progress of the crosslinking reaction differs, the amount of strain of the cured product when stress is applied changes, and the value of the elastic modulus differs.
[0084] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. Furthermore, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0085] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0086] After the cured coating is formed on the substrate as described above, components such as electronic elements are mounted on the substrate by solder reflow treatment. The solder reflow treatment can be performed by a conventionally known method. In general, the solder reflow treatment is performed under treatment conditions of, for example, 245 to 260°C for 5 to 10 seconds.
[0087] The photosensitive resin composition or dry film of the present invention is preferably used for manufacturing electronic parts such as printed wiring boards, and more preferably used to form a permanent coating. In this case, the photosensitive resin composition or dry film of the present invention is used to form a cured product by the above-mentioned method or the like. When the resin layer of the photosensitive resin composition or dry film of the present invention is insulating, it is preferably used to form a solder resist, a coverlay, or an interlayer insulating layer. The photosensitive resin composition of the present invention may also be used to form a solder dam. EXAMPLES
[0088] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.
[0089] <Synthesis Example 1 (Synthesis of Carboxyl Group-Containing Resin A)> Into an autoclave equipped with a thermometer, a nitrogen introduction device, an alkylene oxide introduction device, and a stirrer, 119.4 parts by mass of a novolac cresol resin (trade name "Shounol CRG951", manufactured by Aica Kogyo Co., Ltd., OH equivalent: 119.4), 1.19 parts by mass of potassium hydroxide, and 119.4 parts by mass of toluene were introduced, and the system was replaced with nitrogen while stirring, and the temperature was raised. Next, 63.8 parts by mass of propylene oxide was gradually added dropwise, and the mixture was heated to 125-132°C and 0-4.8 kg / cm. 2 The mixture was reacted at 100° C. for 16 hours. After that, the mixture was cooled to room temperature, and 1.56 parts by mass of 89% phosphoric acid was added to the reaction solution and mixed to neutralize the potassium hydroxide, to obtain a propylene oxide reaction solution of a novolac cresol resin [solid content: 62.1%; hydroxyl value: 182.2 mg KOH / g (307.9 g / eq.)]. This propylene oxide reaction solution had an average of 1.08 moles of propylene oxide added per equivalent of phenolic hydroxyl group. 293.0 parts by mass of the resulting propylene oxide reaction solution of the novolac cresol resin, 43.2 parts by mass of acrylic acid, 11.53 parts by mass of methanesulfonic acid, 0.18 parts by mass of methyl hydroquinone, and 252.9 parts by mass of toluene were introduced into a reactor equipped with a stirrer, a thermometer, and an air blowing tube, and the mixture was reacted at 110°C for 12 hours while blowing air at a rate of 10 ml / min and stirring. 12.6 parts by mass of water produced by the reaction were distilled off as an azeotropic mixture with toluene. The mixture was then cooled to room temperature, and the resulting reaction solution was neutralized with 35.35 parts by mass of a 15% aqueous sodium hydroxide solution, and then washed with water. The mixture was then distilled off while replacing the toluene with 118.1 parts by mass of diethylene glycol monoethyl ether acetate in an evaporator, to obtain a novolac acrylate resin solution. Next, 332.5 parts by mass of the obtained novolac type acrylate resin solution and 1.22 parts by mass of triphenylphosphine were introduced into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and air was blown in at a rate of 10 ml / min. While stirring, 60.8 parts by mass of tetrahydrophthalic anhydride was gradually added, and the mixture was reacted at 95 to 101°C for 6 hours, cooled, and then removed. In this way, a solution of carboxyl group-containing resin A (solid content: 65%; acid value of solid content: 87.7 mg KOH / g) was obtained.
[0090] <Preparation of inorganic filler> The following two types of inorganic filler were prepared: A surface-treated inorganic filler (solid content 70%) was obtained by uniformly dispersing 70 g of spherical silica (SFP-30M manufactured by Denka Co., Ltd., average particle size: 600 nm), 28 g of PMA (propylene glycol monomethyl ether acetate) as a solvent, and 2 g of a silane coupling agent having a methacryl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.).
[0091] 70 g of spherical silica (SFP-30M manufactured by Denka Co., Ltd., average particle size: 600 nm) and 28 g of PMA (propylene glycol monomethyl ether acetate) as a solvent were uniformly dispersed to obtain a surface-untreated inorganic filler (solid content 70%).
[0092] <Preparation of Photosensitive Resin Composition> The components shown in Table 1 below were blended and mixed at room temperature using a three-roll mill to obtain the photosensitive resin compositions shown in the table (Examples 1 to 6 and Comparative Examples 1 and 2). Each value in the table indicates parts by mass.
[0093] In addition, each component *1 to *7 in Table 1 below is as follows. *1: Acylphosphine oxide photoinitiator (IGM Resins Omnirad 819) *2: Anthracure UVS-581 (manufactured by Kawasaki Chemical Industries, Ltd.) *3:KAYACURE DETX-S (Nippon Kayaku Co., Ltd.) *4: Dipentaerythritol hexaacrylate (manufactured by Sanyo Chemical Industries, Ltd.) *5: Phenol novolac epoxy resin (DIC Corporation) *6: Melamine (Nissan Chemical Co., Ltd., D50 = 0.5 μm, solid content 55%) *7: Dicyandiamide (manufactured by Mitsubishi Chemical Corporation, solid content 73%) *8: A mixture of Phthalocyanine Blue and PIGMENT Yellow 147 (content ratio 57:43, solid content 10%) The values in the table represent the amounts blended in a solution containing solids and a solvent.
[0094] <Measurement of water absorption rate of cured product> For the photosensitive resin compositions obtained as described above (Examples 1 to 6 and Comparative Examples 1 to 2), a copper-clad laminate (MCL-E-770G, manufactured by Showa Denko K.K., copper thickness 18 μm) having a thickness of 200 μm and a size of 100×100 mm was used as a support, and the photosensitive resin composition was applied to the entire surface so that the film thickness after curing would be 20 μm. The composition was then dried for 30 minutes in a hot air circulation drying oven (DF610, manufactured by Yamato Scientific Co., Ltd.) at 80° C. to form a dry coating film. Thereafter, the dry coating film was exposed to a UV conveyor oven (KUV-28351-XK-DM, manufactured by Toshiba Corporation) equipped with a metal halide lamp as a light source at a wavelength of 365 nm with an integrated exposure dose of 1000 mJ / cm. 2 (38mW cm 2 The coating was then cured by heating at a temperature of 150° C. for 60 minutes, and the cured coating was then peeled off from the support to obtain a cured product. In the photosensitive resin composition of Example 1, the cumulative exposure dose was 500 mJ / cm 2 (38mW cm 2 A cured coating film was formed in the same manner as in Example 1, except that the heating conditions were changed to 120° C. and 60 minutes, and a cured product (Example 7) was obtained.
[0095] 30 mg of the obtained cured product was placed in a weighing dish, and the mass of each cured product was measured after leaving it in an environment of 100°C for 1 hour (absolutely dry state) (the mass at this time was W 0 (Assuming that.) Next, the cured product was left for 60 minutes in an environment of 25°C and 10% relative humidity, after which the mass of each cured product was measured (the mass at this time was W 10 (Assuming that.) The cured products were then left for 60 minutes in an environment of 25°C and 60% relative humidity, after which the masses of the cured products were measured (the masses at this time were referred to as W 60 (Assuming that.) From the obtained mass, the water absorption rates A and B were calculated according to the following formula. Water absorption rate A(%)=(W 10 -W 0 ) / W 0 ×100 Water absorption rate B(%)=(W 60 -W 0 ) / W 0 ×100 The difference (BA) between the water absorption rates A and B is shown in Table 1 below.
[0096] <Measurement of elastic modulus of cured product> For each of the cured products obtained as described above, test pieces were prepared by cutting into a size of 10 mm x 80 mm, and a stress-strain curve was obtained using a tensile tester in accordance with JIS K 7127 under conditions of a jig distance of 40 mm, a tensile speed of 1 mm / min, and 25°C. For the obtained curve, the slope of the straight line calculated between stresses of 2 N and 7 N was taken as the elastic modulus of the cured product. The elastic modulus of each cured product was as shown in Table 1.
[0097] <Evaluation of the cured product> (1) Warping of the board A substrate having a 20 μm thick cured coating (cured product) formed on a copper-clad laminate in the same manner as described above was left for 1 hour in an environment of 25°C and relative humidity of 60%, and the amount of warping at the four corners of the substrate was measured using calipers, and the warping was evaluated according to the following evaluation criteria. ○: The average warpage at the four corners is less than 5.5 mm △: The average value of the warpage at the four corners is 5.5 mm or more and less than 7.5 mm. ×: The average value of the warpage at the four corners is 7.5 mm or more. The evaluation results are shown in Table 1 below.
[0098] (2) Resolution (undercut) In the same manner as described above, each photosensitive resin composition was applied to the entire surface of a copper-clad laminate so that the film thickness after curing would be 20 μm, and then the composition was dried for 30 minutes in a hot air circulation drying oven (DF610 manufactured by Yamato Scientific Co., Ltd.) at 80° C. to form a dry coating film, and a first film (Lumirror T60 manufactured by Toray Industries, Inc., thickness 125 μm) was laminated onto the dry coating film. The dried coating film was pattern-exposed at an optimum exposure dose through a negative mask of SRO 80 μm using an exposure device equipped with a metal halide lamp as a light source (HMW-680-GW20 manufactured by Oak Manufacturing Co., Ltd.). Here, the optimum exposure dose was determined by exposing the dried coating film obtained above through a step tablet with 21 steps of sensitivity using an exposure device equipped with a metal halide lamp, and exposing the film to 0.2 mass % Na at a liquid temperature of 30° C. 2 CO 3 The exposure dose was set to such that when development was carried out for 60 seconds using an aqueous solution at a spray pressure of 0.2 MPa, a 6-step pattern of the remaining step tablet was formed. Next, the first film was peeled off, and a solution of Na with a concentration of 0.2 mass % at a liquid temperature of 30° C. was added. 2 CO 3 The resist was developed using an aqueous solution and then washed with water. Finally, it was cured at 150°C for 60 minutes to prepare a test piece for evaluating the resolution. The resolution of the obtained test pieces was evaluated according to the following criteria. ○: The ratio of the top and bottom opening diameters is 0.85 or more △: The ratio of the top and bottom opening diameters is less than 0.85 and 0.70 or more ×: The ratio of the top and bottom opening diameters is less than 0.70 The evaluation results are shown in Table 1 below.
[0099] [Table 1]
[0100] As is clear from Table 1, the photosensitive resin compositions (Examples 1 to 7) having an inorganic filler content of 85 mass % or less, an elastic modulus of the cured product in the range of 4 to 12 GPa, a water absorption coefficient A of 0.3 mass % or less, and a water absorption coefficient difference (BA) of 0.3 mass % or less have high resolution and can suppress warping of the printed wiring board. On the other hand, a cured product made of a photosensitive resin composition containing an excessive amount of inorganic filler (Comparative Example 1) has a water absorption coefficient A of 0.3 mass% or less and a water absorption coefficient difference (BA) of 0.3 mass% or less, but an elastic modulus outside the range of 4 to 12 GPa, and although it can suppress warping of a printed wiring board, the resolution is insufficient. Also, a cured product made of a photosensitive resin composition in which only the blending amount of inorganic filler is reduced in order to maintain the resolution (Comparative Example 2) has an improved resolution, but an elastic modulus of more than 12 GPa and a water absorption coefficient difference (BA) of more than 0.3 mass%, and it is found that it is not possible to suppress warping of a board.
Claims
1. A cured product of a photosensitive resin composition comprising at least an alkali-soluble resin, a photopolymerization initiator, and an inorganic filler, The inorganic filler is contained in an amount of 85% by mass or less based on the entire photosensitive resin composition, The elastic modulus of the cured product is 4 to 12 GPa; The cured product is The water absorption rate of the cured product after being left for 60 minutes in an environment of 25° C. and 10% relative humidity is A (%), When the water absorption rate of the cured product after being left for 60 minutes in an environment of 25° C. and 60% relative humidity is B (%), A≦0.3%, and B-A≦0.3 The cured product is characterized by satisfying the above.
2. The cured product according to claim 1, wherein the inorganic filler is contained in an amount of 45 to 65% by mass based on the total mass of the photosensitive resin composition.
3. The cured product according to claim 1 , wherein the inorganic filler is surface-treated with a silane coupling agent.
4. The cured product according to claim 1, wherein the photosensitive resin composition further contains a sensitizer in an amount of 0.01 to 10% by mass based on the total amount of the photosensitive resin composition.
5. The cured product according to claim 4 , wherein the sensitizer is an anthraquinone-based sensitizer having an ester bond.
6. A printed wiring board comprising a substrate and a coating formed on the substrate, the coating being made of the cured product according to any one of claims 1 to 5.
Citation Information
Patent Citations
Resin composition for build-up process, insulating material for build-up process and build-up printed circuit