Surface light source
A polycarbonate resin composition with a thioether compound enhances light guiding and thermal stability, addressing issues of yellowing and humidity resistance, suitable for LED lighting and other industrial applications.
Patent Information
- Application Number
- JP2024135605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polycarbonate resin compositions used in light guides for LED lighting suffer from insufficient light guiding properties, thermal stability, and resistance to yellowing and deterioration in humid environments, limiting their application in edge-light type light sources.
A polycarbonate resin composition blended with a specific proportion of a thioether compound, along with optional phenolic antioxidants and mold release agents, to enhance light guiding properties and resistance to yellowing and humidity.
The composition exhibits excellent light guiding properties, minimal yellowing, and improved thermal stability, enabling its use in various industrial applications including LED lighting, OA equipment, electrical and electronic equipment, and automobiles.
Smart Images

Figure 2024161494000001 
Figure 2024161494000002 
Figure 2024161494000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface light source using a molded article made of a polycarbonate resin composition having light-guiding properties. More specifically, the present invention relates to a surface light source using a molded article made of a polycarbonate resin composition having excellent light-guiding properties, little yellowing during molding, little deterioration in a humid and hot environment, and suitable for use as an optical element such as a light-guiding plate, or a cover for a display panel or lighting. [Background technology]
[0002] Light sources using LEDs as a light source have been attracting attention as the next generation of light sources from the viewpoint of power saving and long life. Since the development of blue light emitting diodes in the 1990s, the practicality of white light illumination using LEDs has increased, and commercial products have rapidly appeared, mainly for local lighting. In addition, LED light sources for surface light sources such as displays have the advantage that the color purity of the light emitted by RGB three-color LEDs is higher than the colors (red, green, and blue) obtained by passing the white light emitted by cold cathode fluorescent lamps through a color filter, and the color reproduction range can be greatly expanded, so LED light sources are being increasingly used. On the other hand, since LEDs are point light sources, when attempting to illuminate a wide area, many LEDs must be installed on the back of the light source (backlight method), and each LED appears as a point light source, which is a disadvantage that it is prone to unevenness. Recently, in order to eliminate this unevenness and to reduce costs, further power saving, and even thinner products, so-called edge light type light sources in which LEDs are placed on the edge of the light source are increasing. In edge light type light sources, a light guide that transmits light over a long distance is used to achieve uniform surface emission. However, the light source body in the edge light system has a problem that the light becomes darker as it gets farther away from the light source. Therefore, the material for the molded body having light guiding properties is required to have a property of less attenuation of light from the light source, that is, light guiding properties, and polymethyl methacrylate (hereinafter sometimes referred to as "PMMA") has been used as the most suitable material among transparent resins. However, PMMA does not necessarily have sufficient impact resistance and thermal stability, and there is a problem that the environment in which it can be used is limited for the above-mentioned applications. Also, with the shift to LED light sources, light guiding bodies have begun to be required to have heat resistance in addition to the above properties. Therefore, technology to improve the light guiding properties of polycarbonate resin, which has excellent heat resistance and impact resistance, has begun to attract attention.
[0003] As an example of improving the light guide of polycarbonate, Patent Document 1 reports an aromatic polycarbonate resin composition for light guide plates, which is made by blending a specific phosphorus-based stabilizer and a release agent with a polycarbonate resin having a viscosity average molecular weight of 13,000 to 15,000. However, there is a problem with strength, and the phosphorus-based stabilizer reduces the moist heat resistance, so that the applications are limited. Patent Documents 2 and 3 report aromatic polycarbonate resin compositions for light guide plates, which are blended with a small amount of a specific siloxane compound. However, silicone-based compounds may generate low molecular weight silicone gas under high temperature conditions. Patent Document 4 reports a light guide plate in which a light scattering layer is provided on the front or back of a plate-shaped molded body molded using a resin composition made of polycarbonate and an acrylic resin. Patent Document 5 reports an aromatic polycarbonate resin composition made of an aromatic polycarbonate resin and another thermoplastic resin whose refractive index difference with the aromatic polycarbonate resin is 0.001 or more. However, since an acrylic resin is added because it is inherently incompatible with polycarbonate resin, the amount of the acrylic resin that can be added is limited, and there are cases in which the light-guiding properties are not fully exhibited. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-204737 A [Patent Document 2] JP 2004-250557 A [Patent Document 3] JP 2015-157901 A [Patent Document 4] Japanese Patent Application Publication No. 10-73725 [Patent Document 5] JP 2002-60609 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a surface light source using a molded article made of a polycarbonate resin composition which has excellent light conductivity and is less susceptible to yellowing during molding and deterioration in a moist and hot environment. [Means for solving the problem]
[0006] As a result of extensive research aimed at achieving the above-mentioned object, the inventors discovered that the above-mentioned object could be achieved by a surface light source using a molded product made of a polycarbonate resin composition in which a thioether-based compound is blended in a specific ratio with a polycarbonate resin, and thus arrived at the present invention.
[0007] That is, according to the present invention, the following configurations (1) to (9) are provided. (1) A surface light source using a molded article made of a polycarbonate resin composition having light guiding properties, which consists of only 100 parts by weight of (A) a polycarbonate resin (component A) obtained by reacting 2,2-bis(4-hydroxyphenyl)propane with a carbonate precursor, (B) 0.005 to 0.2 parts by weight of a thioether-based compound (component B) represented by the following formula [1] or [2], 0 to 1 part by weight of a phosphorus-based antioxidant, 0 to 1 part by weight of a phenol-based antioxidant, and 0 to 1 part by weight of a release agent, said molded article being a surface light source having a thickness of 2 mm and an average spectral light transmittance of 85.0% or more in a wavelength range of 340 nm to 420 nm. (R 1 -S-CH2-CH2-C(O)O-CH2)4-C [1] [In formula (1), R 1 may be the same or different and are linear or branched alkyl groups having 4 to 20 carbon atoms.] (R 2 -OC(O)-CH2-CH2-)2-S 〔2〕 [In formula (2), R 2 may be the same or different and are linear or branched alkyl groups having 6 to 22 carbon atoms.] (2) The surface light source according to the above (1), wherein the thioether compound is at least one thioether compound selected from the group consisting of dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate and pentaerythritol tetrakis(3-laurylthiopropionate). (3) A surface light source according to the preceding paragraph (1) or (2), in which the b* value of a molded product having a thickness of 2 mm is 0.4 or less. (4) A surface light source according to the preceding paragraph (1) or (2), in which the haze value of a molded product having a thickness of 2 mm is 0.1 or less. (5) A surface light source according to the preceding paragraph (1) or (2), in which the ΔHaze value of a molded product with a thickness of 2 mm before and after moist heat treatment (at 120°C for 24 hours) is 1.0 or less. (6) The surface light source according to the above item (1) or (2), wherein the molded product is a molded plate obtained by molding a polycarbonate resin composition into a plate shape. (7) The surface light source according to the above item (6), in which a light source is provided on at least one side of a molded plate and a reflector is provided on one side of the molded plate. (8) A surface light source according to the above item (7), wherein the light source of the surface light source is a fluorescent lamp, a cold cathode fluorescent tube, an LED, a laser diode or an organic electroluminescence (EL). (9) The surface light source according to (1) or (2) above, which is a display part for a mobile phone, a mobile terminal, a camera, a watch, a notebook computer, a display, lighting, a signal, an automobile lamp, or a home appliance or optical device. Effect of the Invention
[0008] The surface light source body using a molded article made of the polycarbonate resin composition of the present invention is a surface light source body using a molded article made of a polycarbonate resin composition comprising a polycarbonate resin and a thioether compound, and exhibits excellent light conductivity, hue, and heat and humidity resistance. Since the surface light source body using a molded article made of the polycarbonate resin composition of the present invention has the above effects, it is extremely useful for various industrial applications such as the lighting field including LED lighting, the OA equipment field, the electric and electronic equipment field, and the automotive field, and the industrial effect it exhibits is extremely large. Specifically, examples include surface light source bodies for mobile phones, mobile terminals, cameras, watches, notebook computers, displays, lighting, signals, automotive lamps, and display components of home appliances and optical devices.
Embodiments for Carrying Out the Invention
[0009] Hereinafter, the details of the present invention will be described. <Component A: Polycarbonate Resin> The polycarbonate resin used as Component A of the present invention is usually obtained by reacting a dihydroxy compound and a carbonate precursor by an interfacial polycondensation method or a melt transesterification method. In addition, it can also be obtained by polymerizing a carbonate prepolymer by a solid-phase transesterification method or by polymerizing a cyclic carbonate compound by a ring-opening polymerization method. The dihydroxy component used here may be any of those usually used as the dihydroxy component of polycarbonate resins, and may be bisphenols or aliphatic diols.
[0010] Examples of bisphenols include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxy-3,3'-biphenyl)propane, 2,2-bis(4-hydroxy- 3-isopropylphenyl)propane, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl) 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-sulfonyldiphenol, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 2,2'-dimethyl -4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfide, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,Examples of the bisphenol compound include 4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, 4,8-bis(4-hydroxyphenyl)tricyclo[5.2.1.02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, and a bisphenol compound having a siloxane structure represented by the following general formula [3].
[0011] [ka]
[0012] [In the formula, R 3 and R 4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; R 5 , R 6 , R 7 , R 8 , R 9 and R 10 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, p and q are each an integer of 1 to 4, e is a natural number, f is 0 or a natural number, and e+f is a natural number less than 100. X is a divalent aliphatic group having 2 to 8 carbon atoms.]
[0013] Examples of aliphatic diols include 2,2-bis-(4-hydroxycyclohexyl)-propane, 1,14-tetradecanediol, octaethylene glycol, 1,16-hexadecanediol, 4,4'-bis(2-hydroxyethoxy)biphenyl, bis{(2-hydroxyethoxy)phenyl}methane, 1,1-bis{(2-hydroxyethoxy)phenyl}ethane, 1,1-bis{(2-hydroxyethoxy)phenyl}-1-phenylethane, 2,2-bis{(2-hydroxyethoxy)phenyl}propane, 2,2-bis{(2-hydroxyethoxy)phenyl}propane, 2,2-bis{4-(2-hydroxyethoxy)-3-methylphenyl}propane, 1,1-bis(2-hydroxyethoxy)phenyl}-3,3,5-trimethylcyclohexane, 2,2-bis{4-(2-hydroxyethoxy)-3,3'-biphenyl}propane, 2,2-bis{(2-hydroxyethoxy)-3-isopropylphenyl}propane, 2,2-bis{3-t-butyl-4-(2-hydroxyethoxy)phenyl}propane, 2,2-bis{(2-hydroxyethoxy)phenyl}butane, 2,2-bis{(2-hydroxyethoxy)phenyl}-4-methylpentane, 2 ,2-Bis{(2-hydroxyethoxy)phenyl}octane, 1,1-bis{(2-hydroxyethoxy)phenyl}decane, 2,2-bis{3-bromo-4-(2-hydroxyethoxy)phenyl}propane, 2,2-bis{3,5-dimethyl-4-(2-hydroxyethoxy)phenyl}propane, 2,2-bis{3-cyclohexyl-4-(2-hydroxyethoxy)phenyl}propane, 1,1-bis{3-cyclohexyl-4-(2-hydroxyethoxy)phenyl}cyclohexane, bis{(2-hydroxyethoxy)phenyl}diphenyl Methane, 9,9-bis{(2-hydroxyethoxy)phenyl}fluorene, 9,9-bis{4-(2-hydroxyethoxy)-3-methylphenyl}fluorene, 1,1-bis{(2-hydroxyethoxy)phenyl}cyclohexane, 1,1-bis{(2-hydroxyethoxy)phenyl}cyclopentane, 4,4'-bis(2-hydroxyethoxy)diphenyl ether, 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether, 1,3-bis[2-{(2-hydroxyethoxy)phenyl}propyl]benzene, 1,Examples of the 4-bis[2-{(2-hydroxyethoxy)phenyl}propyl]benzene include 1,4-bis{(2-hydroxyethoxy)phenyl}cyclohexane, 1,3-bis{(2-hydroxyethoxy)phenyl}cyclohexane, 4,8-bis{(2-hydroxyethoxy)phenyl}tricyclo[5.2.1.02,6]decane, 1,3-bis{(2-hydroxyethoxy)phenyl}-5,7-dimethyladamantane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, 1,4:3,6-dianhydro-D-sorbitol (isosorbide), 1,4:3,6-dianhydro-D-mannitol (isomannide), and 1,4:3,6-dianhydro-L-iditol (isoidide).
[0014] Among these, aromatic bisphenols are preferred, and in particular, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 9,9 ... Preferred are 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 4,4'-sulfonyldiphenol, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, a bisphenol compound represented by the above general formula [3]. Among them, 2,2-bis(4-hydroxyphenyl)propane, which has excellent strength and good durability, is the most suitable. These may be used alone or in combination of two or more kinds.
[0015] The polycarbonate resin used as component A of the present invention may be a branched polycarbonate resin by using a branching agent in combination with the above dihydroxy compound. Examples of the trifunctional or higher polyfunctional aromatic compounds used in such branched polycarbonate resins include phloroglucin, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2,2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 26-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 4-{4-[1,1-bis(4- Examples of the trisphenols include trisphenols such as 1,4-dimethylbenzylphenol, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among these, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.
[0016] These polycarbonate resins are produced by a reaction means known per se for producing ordinary aromatic polycarbonate resins, for example, a method of reacting an aromatic dihydroxy component with a carbonate precursor such as phosgene or a carbonic acid diester. The basic means for the production method will be briefly described below.
[0017] In the reaction using, for example, phosgene as the carbonate precursor, the reaction is usually carried out in the presence of an acid binder and a solvent. As the acid binder, for example, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide or an amine compound such as pyridine is used. As the solvent, for example, a halogenated hydrocarbon such as methylene chloride or chlorobenzene is used. In addition, a catalyst such as a tertiary amine or a quaternary ammonium salt can be used to promote the reaction. In this case, the reaction temperature is usually 0 to 40°C, and the reaction time is several minutes to 5 hours. The transesterification reaction using a carbonic acid diester as the carbonate precursor is carried out by a method in which a predetermined ratio of aromatic dihydroxy components is stirred with the carbonic acid diester while heating in an inert gas atmosphere, and the generated alcohol or phenol is distilled off. The reaction temperature varies depending on the boiling point of the generated alcohol or phenol, but is usually in the range of 120 to 300°C. The reaction is completed by reducing the pressure from the beginning and distilling off the generated alcohol or phenol. In addition, a catalyst usually used in the transesterification reaction can be used to promote the reaction. Examples of the carbonic acid diester used in the transesterification reaction include diphenyl carbonate, dinaphthyl carbonate, bis(diphenyl) carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, etc. Among these, diphenyl carbonate is particularly preferred.
[0018] In the present invention, a terminal terminator is used in the polymerization reaction. The terminal terminator is used to adjust the molecular weight, and the obtained polycarbonate resin has excellent thermal stability compared to those not having the terminals blocked, since the terminals are blocked. As such terminal terminators, monofunctional phenols represented by the following general formulas [4] to [6] can be mentioned.
[0019] [ka]
[0020] [In formula [4], A is a hydrogen atom, an alkyl group having 1 to 9 carbon atoms, an alkylphenyl group (the alkyl portion has 1 to 9 carbon atoms), a phenyl group, or a phenylalkyl group (the alkyl portion has 1 to 9 carbon atoms), and r is an integer of 1 to 5, preferably 1 to 3].
[0021] [ka]
[0022] [ka]
[0023] [In the formulas [5] and [6], Y is -RO-, -R-CO-O- or -RO-CO-, where R represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 5 carbon atoms, and n represents an integer of 10 to 50.]
[0024] Specific examples of the monofunctional phenols represented by the above general formula [4] include phenol, isopropylphenol, p-tert-butylphenol, p-cresol, p-cumylphenol, 2-phenylphenol, 4-phenylphenol, and isooctylphenol.
[0025] The monofunctional phenols represented by the above general formula [5] or [6] are phenols having a long-chain alkyl group or an aliphatic ester group as a substituent. When these are used to block the ends of a polycarbonate resin, they not only function as an end terminator or molecular weight regulator, but also improve the melt fluidity of the resin, facilitating molding and processing, and have the effect of lowering the water absorption of the resin, and are therefore preferably used.
[0026] As the substituted phenols of the above general formula [5], those in which n is 10 to 30, particularly 10 to 26, are preferred. Specific examples thereof include decylphenol, dodecylphenol, tetradecylphenol, hexadecylphenol, octadecylphenol, eicosylphenol, docosylphenol, and triacontylphenol.
[0027] As the substituted phenol of the above general formula [6], a compound in which Y is -R-COO- and R is a single bond is suitable, and n is preferably 10 to 30, particularly preferably 10 to 26. Specific examples thereof include decyl hydroxybenzoate, dodecyl hydroxybenzoate, tetradecyl hydroxybenzoate, hexadecyl hydroxybenzoate, eicosyl hydroxybenzoate, docosyl hydroxybenzoate, and tricontyl hydroxybenzoate.
[0028] Among these monofunctional phenols, the monofunctional phenols represented by the above general formula [4] are preferred, more preferably alkyl- or phenylalkyl-substituted phenols, and particularly preferably p-tert-butylphenol, p-cumylphenol or 2-phenylphenol.
[0029] It is desirable that the terminal terminator of these monofunctional phenols is introduced into the terminals in an amount of at least 5 mol %, and preferably at least 10 mol %, based on the total terminals of the obtained polycarbonate resin. The terminal terminator may be used alone or in combination of two or more kinds.
[0030] The polycarbonate resin used as component A of the present invention may be a polyester carbonate copolymerized with an aromatic dicarboxylic acid such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid or a derivative thereof, as long as it does not impair the spirit of the present invention.
[0031] The viscosity average molecular weight of the polycarbonate resin used as Component A of the present invention is preferably in the range of 11,500 to 50,000, more preferably 12,500 to 40,000, even more preferably 13,500 to 35,000, and most preferably 15,000 to 30,000. When the molecular weight exceeds 50,000, the melt viscosity may become too high and the moldability may be poor. When the molecular weight is less than 11,500, problems may occur in mechanical strength. The viscosity average molecular weight referred to in the present invention is first obtained by using an Ostwald viscometer from a solution prepared by dissolving 0.7 g of polycarbonate resin in 100 ml of methylene chloride at 20°C to obtain the specific viscosity calculated by the following formula, and then inserting the obtained specific viscosity into the following formula to obtain the viscosity average molecular weight Mv. Specific viscosity (η SP ) = (t - t0) / t0 [t0 is the dropping time of methylene chloride, t is the dropping time of the sample solution] η SP / c = [η] + 0.45×[η] 2 c (where [η] is the intrinsic viscosity) [η] = 1.23×10 -4 Mv 0.83 c = 0.7
[0032] The total Cl (chlorine) content in the resin of the polycarbonate resin used as Component A of the present invention is preferably 0 to 500 ppm, more preferably 0 to 350 ppm. When the total Cl content in the polycarbonate resin is within the above range, it is excellent in hue and thermal stability and is preferable.
[0033] <Component B: Thioether compound> The thioether compound used as Component B of the present invention improves the thermal stability during the production or molding process of the polycarbonate resin and improves the mechanical properties, hue, and molding stability. The thioether compound used in the present invention is preferably at least one thioether compound selected from the group consisting of the compounds represented by the following formula [1] and the following formula [2]. (R 1 -S-CH2-CH2-C(O)O-CH2)4-C 〔1〕 [In the formula, R1 may be the same or different and are linear or branched alkyl groups having 4 to 20 carbon atoms.] (R 2 -OC(O)-CH2-CH2-)2-S 〔2〕 [In the formula, R 2 may be the same or different and are linear or branched alkyl groups having 6 to 22 carbon atoms.]
[0034] In the thioether compound represented by the formula [1], R 1 is an alkyl group having 4 to 20 carbon atoms, preferably an alkyl group having 10 to 18 carbon atoms. Specific examples include pentaerythritol tetrakis(3-laurylthiopropionate), pentaerythritol tetrakis(3-myristylthiopropionate), pentaerythritol tetrakis(3-stearylthiopropionate), and the like, of which pentaerythritol tetrakis(3-laurylthiopropionate) and pentaerythritol tetrakis(3-myristylthiopropionate) are preferred, and pentaerythritol tetrakis(3-laurylthiopropionate) is particularly preferred.
[0035] In addition, in the thioether compound represented by the formula [2], R 2 is an alkyl group having 6 to 22 carbon atoms, preferably an alkyl group having 10 to 18 carbon atoms. Specific examples include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, etc., of which dilauryl-3,3'-thiodipropionate and dimyristyl-3,3'-thiodipropionate are preferred, and dimyristyl-3,3'-thiodipropionate is particularly preferred.
[0036] The content of the thioether compound is in the range of 0.005 to 0.2 parts by weight, preferably 0.01 to 0.15 parts by weight, and most preferably 0.02 to 0.1 parts by weight, relative to 100 parts by weight of the polycarbonate resin. If it is less than 0.005 parts by weight, excellent light guiding properties cannot be obtained, and the effect of suppressing discoloration during molding is insufficient, which is not preferable. Also, even if the amount exceeds 0.2 parts by weight, no further improvement in the effect is observed, and heat resistance is rather reduced, which is not preferable. Thioether compounds are commercially available as Sumilizer TP-D (trade name) from Sumitomo Chemical Co., Ltd. and Irganox PS802FL (trade name) from BASF, and can be easily used.
[0037] <Other ingredients> Other resins and fillers may be blended into the polycarbonate resin composition of the present invention as long as the transparency, light-guiding properties, etc. are not impaired. However, since many other resins and fillers impair transparency, the type and amount of the other resins and fillers should be selected while taking this into consideration. In consideration of the above points, additives that are used to improve the thermal stability, designability, etc. of the polycarbonate resin composition of the present invention are advantageously used. These additives will be specifically described below.
[0038] (I) Heat stabilizer The polycarbonate resin composition of the present invention may contain various known heat stabilizers, such as phosphorus-based antioxidants and phenol-based antioxidants. Specific examples of such phosphorus-based antioxidants include phosphorous acid (phosphite), phosphonite, phosphinite, phosphine, phosphoric acid (phosphate), phosphonate, phosphinate, and phosphine oxide, and among these, phosphites, phosphonites, phosphines, phosphonates, and phosphates are preferably used. Specific examples of the phosphite compound include trimethyl phosphite, triethyl phosphite, tripropyl phosphite, triisopropyl phosphite, tributyl phosphite, triphenyl phosphite, tris(nonylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, tris(diethylphenyl)phosphite, tris(di-isopropylphenyl)phosphite, phenyl) phosphite, tris(di-n-butylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, tris(2,6-di-tert-butylphenyl) phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl) pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, bis(nonylphenyl) pentaerythritol diphosphite, dicyclohexyl pentaerythritol diphosphite, etc. Furthermore, as other phosphite compounds, those having a cyclic structure that reacts with dihydric phenols can also be used.For example, 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2,4-di-tert-butylphenyl)phosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite, 2,2'-methylenebis(4-methyl-6-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite, 2,2'-ethylidenebis(4-methyl-6-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite, and the like can be mentioned.
[0039] Examples of the phosphonite compounds include tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenylphosphonite, bis Examples of the phosphonite include (2,4-di-tert-butylphenyl)-3-phenyl-phenylphosphonite, bis(2,6-di-n-butylphenyl)-3-phenyl-phenylphosphonite, bis(2,6-di-tert-butylphenyl)-4-phenyl-phenylphosphonite, and bis(2,6-di-tert-butylphenyl)-3-phenyl-phenylphosphonite. Tetrakis(di-tert-butylphenyl)-biphenylene diphosphonite and bis(di-tert-butylphenyl)-phenyl-phenylphosphonite are preferred, and tetrakis(2,4-di-tert-butylphenyl)-biphenylene diphosphonite and bis(2,4-di-tert-butylphenyl)-phenyl-phenylphosphonite are more preferred. Such phosphonite compounds can be used in combination with the phosphite compounds having an aryl group substituted with two or more alkyl groups, and are therefore preferred.
[0040] Examples of the phosphine compound include triethylphosphine, tripropylphosphine, tributylphosphine, trioctylphosphine, triamylphosphine, dimethylphenylphosphine, dibutylphenylphosphine, diphenylmethylphosphine, diphenyloctylphosphine, triphenylphosphine, tri-p-tolylphosphine, trinaphthylphosphine, and diphenylbenzylphosphine. A particularly preferred phosphine compound is triphenylphosphine.
[0041] Examples of the phosphonate compound include dimethyl benzenephosphonate, diethyl benzenephosphonate, and dipropyl benzenephosphonate. Examples of the phosphate compound include tributyl phosphate, trimethyl phosphate, tricresyl phosphate, triphenyl phosphate, trichlorophenyl phosphate, triethyl phosphate, diphenyl cresyl phosphate, diphenyl monoorthoxenyl phosphate, tributoxyethyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, and the like, and preferably triphenyl phosphate and trimethyl phosphate.
[0042] Specific examples of phenol-based antioxidants include vitamin E, n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenylacrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-tert-butyl-4-hydroxybenzylphosphonate diethyl ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenyl)propionate, phenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-dimethylene-bis(6-α-methyl-benzyl-p-cresol) 2,2'-ethylidene-bis(4,6-di-tert-butylphenol), 2,2'-butylidene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol) , triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, bis[2-tert-butyl-4-methyl 6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl]terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethylethyl}-2,4,8,10 -Tetraoxaspiro[5,5]undecane, 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl)sulfide, 4,4'-di-thiobis(2,6-di-tert-butylphenol), 4,4'-tri-thiobis(2,6-di-tert-butylphenol), 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylenebis-(3,5-di-tert-butyl-4-hydroxyhydrocinnamide), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4- hydroxyphenyl) isocyanurate, tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl) isocyanurate, 1,3,5-tris-2[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane, etc. can be mentioned, and can be preferably used.
[0043] Among these, n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, and tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane are preferred, and n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate is more preferred.
[0044] The phosphorus-based antioxidants and phenol-based antioxidants listed above can be used alone or in combination of two or more kinds. The content of these phosphorus-based antioxidants or phenol-based antioxidants is preferably 0.0001 to 1 part by weight per 100 parts by weight of component A. More preferably, it is 0.0005 to 0.5 parts by weight, and even more preferably, it is 0.001 to 0.2 parts by weight.
[0045] In addition, since the amount of phosphorus-based antioxidants, particularly phosphite-based antioxidants, that is added in large amounts reduces the moist heat resistance of the polycarbonate resin, the amount of the antioxidants added is preferably less than 0.02 parts by weight, more preferably 0.015 parts by weight or less, even more preferably 0.01 parts by weight or less, particularly preferably 0.005 parts by weight or less, and most preferably 0.001 parts by weight or less.Furthermore, it is preferable that the antioxidants are not added substantially at all.
[0046] (II) Release agent The polycarbonate resin composition of the present invention may contain a release agent as necessary. Such a release agent may be one known per se. Examples of such a release agent include saturated fatty acid esters, unsaturated fatty acid esters, polyolefin waxes (polyethylene wax or 1-alkene polymers may be mentioned. These may also be modified with a functional group-containing compound such as an acid modification), silicone compounds, fluorine compounds, paraffin wax, and beeswax. Among these, saturated fatty acid esters, linear or cyclic polydimethylsiloxane oils, polymethylphenyl silicone oils, and fluorine oils are preferred. Particularly preferred release agents include saturated fatty acid esters, such as monoglycerides such as stearic acid monoglyceride, polyglycerin fatty acid esters such as decaglycerin deca stearate and decaglycerin tetrastearate, lower fatty acid esters such as stearic acid stearate, higher fatty acid esters such as sebacate behenate, and erythritol esters such as pentaerythritol tetrastearate. The content of such a release agent is preferably 0.01 to 1 part by weight per 100 parts by weight of component A.
[0047] (III) Ultraviolet absorbers The polycarbonate resin composition of the present invention can be blended with an ultraviolet absorbing agent as required. Examples of such ultraviolet absorbing agents include benzophenone-based ultraviolet absorbing agents such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodiumsulfoxybenzophenone, and bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane.
[0048] Examples of the ultraviolet absorber include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-3'-dodecyl-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-bis(α,α'-dimethylbenzyl)phenylbenzotriazole, 2-[2'-hydroxy-3'- Benzotriazole-based ultraviolet absorbers typified by (3”,4”,5”,6”-tetraphthalimidomethyl)-5’-methylphenyl]benzotriazole, 2-(2’-hydroxy-3’-tert-butyl-5’-methylphenyl)-5-chlorobenzotriazole, 2-(2’-hydroxy-3’,5’-di-tert-butylphenyl)-5-chlorobenzotriazole, 2,2’methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], and methyl-3-[3-tert-butyl-5-(2H-benzotriazol-2-yl)-4-hydroxyphenylpropionate-polyethylene glycol condensate can be mentioned.
[0049] Further examples of the ultraviolet absorber include hydroxyphenyltriazine compounds such as 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxy-phenol and 2-(4,6-bis-(2,4-dimethylphenyl-1,3,5-triazin-2-yl)-5-hexyloxy-phenol, and malonate compounds such as 2-(1-arylalkylidene)malonate esters such as Hostavin PR-25 manufactured by Clariant Japan and Hostavin B-CAP manufactured by Clariant Japan. The content of the ultraviolet absorber is preferably 0.01 to 5 parts by weight, and more preferably 0.02 to 1 part by weight, per 100 parts by weight of the A component.
[0050] (IV) Light stabilizers The polycarbonate resin composition of the present invention may contain a light stabilizer as required. Examples of such light stabilizers include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2n-butylmalonate, condensation product of 1,2,3,4-butanecarboxylic acid, 2,2,6,6-tetramethyl-4-piperidinol, and tridecyl alcohol, and condensation product of 1,2,3,4-butanedicarboxylic acid and 1,2,2,6,6-tetramethyl-4-piperidinol. Condensation product of pentamethyl-4-piperidinol and tridecyl alcohol, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, poly{[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethylpiperidyl)imino]hexamethylene[(2,2,6,6-tetramethylpiperidyl)imino]hexamethylene Poly{[6-morpholino-s-triazine-2,4-diyl][(2,2,6,6-tetramethylpiperidyl)imino]hexamethylene[(2,2,6,6-tetramethylpiperidyl)imino]}, Condensation product of 1,2,3,4-butanetetracarboxylic acid, 2,2,6,6-tetramethyl-4-piperidinol and β,β,β',β'-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5]undecane)diethanol, N,N'-bis(3-aminopropyl)ethylenediamine and 2,4- Examples of the hindered amine include a condensation product of bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-chloro-1,3,5-triazine, a condensation product of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β',β'-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5]undecane)diethanol, and polymethylpropyl 3-oxy-[4-(2,2,6,6-tetramethyl)piperidinyl]siloxane.The content of the light stabilizer is preferably from 0.01 to 5 parts by weight, and more preferably from 0.02 to 1 part by weight, per 100 parts by weight of the A component.
[0051] (V) Bluing agent The polycarbonate resin composition of the present invention can be blended with a bluing agent to counteract the yellowish color caused by the ultraviolet absorbing agent, etc. As the bluing agent, any agent normally used for polycarbonate resins can be used without any problem. In general, anthraquinone dyes are easily available and are preferred. Specific examples of the bluing agent include Solvent Violet 13 (CA.No (Color Index No) 60725; trademarks: Bayer's Macrolex Violet B, Mitsubishi Chemical's DiaResin Blue G, and Sumitomo Chemical's Sumiplast Violet B), Solvent Violet 31 (CA.No 68210; trademark: Mitsubishi Chemical's DiaResin Violet D), Solvent Violet 33 (CA.No 60725; trademark: Mitsubishi Chemical's DiaResin Blue J), Solvent Blue 94 (CA.No 61500; trademark: Mitsubishi Chemical's DiaResin Blue N), Solvent Violet 36 (CA.No 68210; trademark: Bayer's Macrolex Violet 3R), and Solvent Blue 97 (trademark: Examples of the bluing agent include "Macrolex Blue RR" manufactured by Bayer and Solvent Blue 45 [CA. No. 61110; trade name "Terazol Blue RLS" manufactured by Sandoz], and in particular, Macrolex Blue RR, Macrolex Violet B and Terazol Blue RLS are preferred. The content of the bluing agent is preferably 0.000005 to 0.001 part by weight, more preferably 0.00001 to 0.0001 part by weight, per 100 parts by weight of component A.
[0052] (VI) Fluorescent whitening agents In the polycarbonate resin composition of the present invention, the fluorescent brightener is not particularly limited as long as it is used to improve the color tone of the resin or the like to white or bluish white, and examples thereof include stilbene-based, benzimidazole-based, benzoxazole-based, naphthalimide-based, rhodamine-based, coumarin-based, and oxazine-based compounds. Specific examples thereof include CI Fluorescent Brightener 219:1, Eastman Chemical Company's EASTOBRITE OB-1, and Hakkol Chemical Company's "Hakkol PSR." The fluorescent brightener absorbs ultraviolet energy of light and radiates this energy in the visible region. The content of the fluorescent brightener is preferably 0.001 to 0.1 parts by weight, more preferably 0.001 to 0.05 parts by weight, based on 100 parts by weight of the A component.
[0053] (VII) Epoxy compounds The polycarbonate resin composition of the present invention may contain an epoxy compound as required. Such an epoxy compound is added for the purpose of suppressing mold corrosion, and basically all epoxy functional groups can be used. Specific examples of preferred epoxy compounds include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, copolymers of methyl methacrylate and glycidyl methacrylate, and copolymers of styrene and glycidyl methacrylate. The amount of such an epoxy compound to be added is preferably 0.003 to 0.2 parts by weight, more preferably 0.004 to 0.15 parts by weight, and even more preferably 0.005 to 0.1 parts by weight, based on 100 parts by weight of component A.
[0054] (VIII) Organometallic salts An organic metal salt compound can be blended into the polycarbonate resin composition of the present invention. Such an organic metal salt is blended for the purpose of imparting flame retardancy, and is preferably an alkali (earth) metal salt of an organic acid having 1 to 50, preferably 1 to 40 carbon atoms, and more preferably an alkali (earth) metal salt of an organic sulfonate. The alkali (earth) metal salt of an organic sulfonate includes a metal salt of a fluorine-substituted alkylsulfonic acid such as a metal salt of a perfluoroalkylsulfonic acid having 1 to 10, preferably 2 to 8 carbon atoms and an alkali metal or an alkaline earth metal, and a metal salt of an aromatic sulfonic acid having 7 to 50, preferably 7 to 40 carbon atoms and an alkali metal or an alkaline earth metal. Examples of the alkali metal constituting the metal salt include lithium, sodium, potassium, rubidium, and cesium, and examples of the alkaline earth metal include beryllium, magnesium, calcium, strontium, and barium. An alkali metal is more preferable. Among these alkali metals, rubidium and cesium, which have a larger ionic radius, are suitable when transparency is required, but they are not widely used and are difficult to purify, which may result in a disadvantage in terms of cost. On the other hand, metals with a smaller ionic radius, such as lithium and sodium, may be disadvantageous in terms of flame retardancy. Taking these factors into consideration, the alkali metals in the alkali metal sulfonates can be used differently, but potassium sulfonates, which have an excellent balance of properties, are most suitable in all respects. Such potassium salts can also be used in combination with alkali metal sulfonates made of other alkali metals.
[0055] Specific examples of the alkali metal salt of perfluoroalkylsulfonate include potassium trifluoromethanesulfonate, potassium perfluorobutanesulfonate, potassium perfluorohexanesulfonate, potassium perfluorooctane sulfonate, sodium pentafluoroethanesulfonate, sodium perfluorobutanesulfonate, sodium perfluorooctane sulfonate, lithium trifluoromethanesulfonate, lithium perfluorobutanesulfonate, lithium perfluoroheptanesulfonate, cesium trifluoromethanesulfonate, cesium perfluorobutanesulfonate, cesium perfluorooctane sulfonate, cesium perfluorohexanesulfonate, rubidium perfluorobutanesulfonate, and rubidium perfluorohexanesulfonate, and these can be used alone or in combination of two or more. Here, the carbon number of the perfluoroalkyl group is preferably in the range of 1 to 18, more preferably in the range of 1 to 10, and even more preferably in the range of 1 to 8. Among these, potassium perfluorobutanesulfonate is particularly preferred. In the alkali (earth) metal salt of perfluoroalkylsulfonic acid made of an alkali metal, fluoride ions are usually mixed in at least a small amount. The presence of such fluoride ions can be a factor in reducing flame retardancy, so it is preferable to reduce them as much as possible. The proportion of such fluoride ions can be measured by ion chromatography. The content of fluoride ions is preferably 100 ppm or less, more preferably 40 ppm or less, and particularly preferably 10 ppm or less. It is also preferable that the content is 0.2 ppm or more for efficient production. The alkali (earth) metal salt of perfluoroalkylsulfonic acid having a reduced amount of fluoride ions can be produced by using a known production method, and by a method of reducing the amount of fluoride ions contained in the raw material when producing a fluorine-containing organic metal salt, a method of removing hydrogen fluoride and the like obtained by the reaction by gas generated during the reaction or by heating, and a method of reducing the amount of fluoride ions by using a purification method such as recrystallization and reprecipitation when producing a fluorine-containing organic metal salt.In particular, since organometallic salt flame retardants are relatively soluble in water, it is preferable to manufacture them using ion-exchanged water, particularly water that has an electrical resistance of 18 MΩ cm or more, i.e., an electrical conductivity of approximately 0.55 μS / cm or less, by dissolving and washing the material at a temperature higher than room temperature, and then cooling and recrystallizing the material. Specific examples of the aromatic sulfonic acid alkali (earth) metal salts include disodium diphenyl sulfide-4,4'-disulfonate, dipotassium diphenyl sulfide-4,4'-disulfonate, potassium 5-sulfoisophthalate, sodium 5-sulfoisophthalate, polysodium polyethylene terephthalate polysulfonate, calcium 1-methoxynaphthalene-4-sulfonate, disodium 4-dodecylphenyl ether disulfonate, polysodium poly(2,6-dimethylphenylene oxide) polysulfonate, polysodium poly(1,3-phenylene oxide) polysulfonate, polysodium poly(1,4-phenylene oxide) polysulfonate, polypotassium poly(2,6-diphenylphenylene oxide) polysulfonate, lithium poly(2-fluoro-6-butylphenylene oxide) polysulfonate, potassium sulfonate of benzenesulfonate, sodium benzenesulfonate, and benzenesulfonic acid. Examples of the sulfonate include strontium, magnesium benzenesulfonate, dipotassium p-benzenedisulfonate, dipotassium naphthalene-2,6-disulfonate, calcium biphenyl-3,3'-disulfonate, sodium diphenylsulfone-3-sulfonate, potassium diphenylsulfone-3-sulfonate, dipotassium diphenylsulfone-3,3'-disulfonate, dipotassium diphenylsulfone-3,4'-disulfonate, sodium α,α,α-trifluoroacetophenone-4-sulfonate, dipotassium benzophenone-3,3'-disulfonate, disodium thiophene-2,5-disulfonate, dipotassium thiophene-2,5-disulfonate, calcium thiophene-2,5-disulfonate, sodium benzothiophenesulfonate, potassium diphenylsulfoxide-4-sulfonate, a formalin condensate of sodium naphthalenesulfonate, and a formalin condensate of sodium anthracenesulfonate.Among these aromatic sulfonic acid alkali (earth) metal salts, potassium salts are particularly preferred. Among these aromatic sulfonic acid alkali (earth) metal salts, potassium diphenylsulfone-3-sulfonate and dipotassium diphenylsulfone-3,3'-disulfonate are particularly preferred, and mixtures thereof (wherein the weight ratio of the former to the latter is 15 / 85 to 30 / 70) are particularly preferred.
[0056] Suitable examples of organic metal salts other than alkali (earth) metal sulfonates include alkali (earth) metal salts of sulfates and alkali (earth) metal salts of aromatic sulfonamides. Examples of alkali (earth) metal salts of sulfates include alkali (earth) metal salts of sulfates of monohydric and / or polyhydric alcohols, and examples of sulfates of monohydric and / or polyhydric alcohols include methyl sulfate, ethyl sulfate, lauryl sulfate, hexadecyl sulfate, sulfate of polyoxyethylene alkylphenyl ether, mono-, di-, tri-, and tetrasulfate of pentaerythritol, sulfate of lauric acid monoglyceride, sulfate of palmitic acid monoglyceride, and sulfate of stearic acid monoglyceride. Examples of the alkali (earth) metal salts of these sulfates include alkali (earth) metal salts of lauryl sulfate. Examples of the alkali (earth) metal salt of aromatic sulfonamide include saccharin, N-(p-tolylsulfonyl)-p-toluenesulfonimide, N-(N'-benzylaminocarbonyl)sulfanilimide, and alkali (earth) metal salt of N-(phenylcarboxyl)sulfanilimide. The content of the organic metal salt is preferably 0.001 to 1 part by weight, more preferably 0.005 to 0.5 parts by weight, still more preferably 0.01 to 0.3 parts by weight, and particularly preferably 0.03 to 0.15 parts by weight, relative to 100 parts by weight of component A.
[0057] (IX) Other In addition to the above, the resin composition of the present invention can be blended with known additives to impart various functions to the molded product or improve its characteristics, as long as the purpose of the present invention is not impaired. Examples of such additives include reinforcing fillers, sliding agents (e.g., PTFE particles), colorants, fluorescent dyes, inorganic phosphors (e.g., phosphors with aluminate as the mother crystal), antistatic agents, crystal nucleating agents, inorganic and organic antibacterial agents, photocatalytic antifouling agents (e.g., fine titanium oxide particles, fine zinc oxide particles), light diffusing agents, flow modifiers, radical generators, infrared absorbing agents (heat ray absorbing agents), and photochromic agents.
[0058] <Production of polycarbonate resin composition> Any method can be used to produce the polycarbonate resin composition of the present invention. For example, the A component, the B component, and any other components can be thoroughly mixed using a premixing means such as a V-type blender, a Henschel mixer, a mechanochemical device, or an extrusion mixer, and then granulated using an extrusion granulator or a briquetting machine, if necessary, and then melt-kneaded using a melt kneader, such as a vented twin-screw extruder, and pelletized using a pelletizer or other device. As an alternative method, the A component, the B component, and any other components can be independently supplied to a melt kneader, such as a vented twin-screw extruder, a method in which the A component and a part of the other components are premixed and then supplied to the melt kneader independently of the remaining components, a method in which the B component is diluted and mixed with water or an organic solvent and then supplied to the melt kneader, or such a diluted mixture is premixed with the other components and then supplied to the melt kneader. If any of the components to be blended is liquid, a so-called liquid injection device or liquid addition device can be used to supply the components to the melt kneader.
[0059] <Production of molded products> Any method can be used to manufacture a molded article made of the polycarbonate resin composition of the present invention. For example, the polycarbonate resin composition can be kneaded with an extruder, a Banbury mixer, a roll, or the like, and then molded by a conventionally known method such as injection molding, extrusion molding, or compression molding to obtain a molded article. A light source can also be provided on at least one side of the molded plate obtained by molding into a plate shape, and a reflector can be provided on one side of the molded plate to form a surface light source. As the light source for such molded plate and surface light source, a self-illuminating body such as a cold cathode tube, an LED, a laser diode, or an organic EL can be used in addition to a fluorescent lamp. The molded plate and surface light source of the molded article obtained by the present invention are used for mobile phones, mobile terminals, cameras, watches, notebook computers, displays, lighting, signals, automobile lamps, display parts of home appliances and optical devices, etc.
[0060] The present inventors currently consider the best embodiment of the present invention to be one that embodies the preferred ranges of each of the above-mentioned requirements, and representative examples thereof are described in the following examples, although the present invention is not limited to these embodiments. EXAMPLES
[0061] The present invention will be further explained below with reference to examples, but is not limited to these examples. The details of each component used and the evaluation are as follows.
[0062] (Component A) A-1: Bisphenol A type aromatic polycarbonate resin (Teijin: CM-1000, viscosity average molecular weight 15,400) A-2: Bisphenol A type aromatic polycarbonate resin (Teijin: L-1225WX, viscosity average molecular weight 19,900) (B component) B-1: Pentaerythritol tetrakis(3-laurylthiopropionate) (Sumitomo Chemical Co., Ltd.: Sumilizer TP-D) B-2: Dimyristyl-3,3'-thiodipropionate (BASF: Irganox PS802FL) (Other ingredients) (Antioxidants) C: Bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite (ADEKA: Adeka STAB PEP-36) D: Tris(2,4-di-tert-butylphenyl)phosphite (BASF: Irgafos 168) E: Hindered phenol antioxidant (BASF: Irganox 1076) (Release agent) F: Glycerin monostearate (Riken Vitamin Co., Ltd.: Rikemal S-100A)
[0063] (Evaluation method) (1) Spectral light transmittance The pellets obtained from each composition of the examples were dried in a hot air circulation dryer at 120°C for 5 hours, and molded into a molded plate with a width of 50 mm, a length of 90 mm, and a thickness of 2 mm using an injection molding machine [J85-ELIII manufactured by Japan Steel Works, Ltd.] at a molding temperature of 270°C and a mold temperature of 80°C. The spectral light transmittance of this molded plate with a thickness of 2 mm was measured at 1 nm intervals in the wavelength range of 200 nm to 800 nm using a spectrophotometer [Cary5000 manufactured by Agilent]. The average spectral light transmittance in the wavelength range of 340 nm to 420 nm was calculated from the obtained spectral light transmittance. A higher spectral light transmittance indicates less light attenuation and better light-guiding performance. A spectral light transmittance of 85.0% or more was evaluated as ◯, and a value of less than 85.0% was evaluated as ×.
[0064] (2) Molded plate hue The pellets obtained from each composition of the examples were dried in a hot air circulation dryer at 120° C. for 5 hours, and molded into a molded plate having a width of 50 mm, a length of 90 mm, and a thickness of 2 mm using an injection molding machine [J85-ELIII manufactured by Japan Steel Works, Ltd.] at a molding temperature of 270° C. and a mold temperature of 80° C. The hue (L*, a*, b*) of this molded plate having a thickness of 2 mm was measured using an integrating sphere spectrophotometer [CE-7000A manufactured by X-Rite] in accordance with JIS-K7105 under the conditions of a light source of D65, a viewing angle of 10 degrees, and a transmission method. The higher the b* value of the molded plate, the more likely it is to turn yellow. A b* value of 0.4 or less is marked as ◯, and a value exceeding 0.4 is marked as ×.
[0065] (3) Moisture and heat resistance The pellets obtained from each composition of the examples were dried in a hot air circulation dryer at 120°C for 5 hours, and molded into a molded plate with a width of 50 mm, length of 90 mm, and thickness of 2 mm at a molding temperature of 270°C and a mold temperature of 80°C using an injection molding machine [J85-ELIII manufactured by Japan Steel Works, Ltd.]. This molded plate was subjected to a wet heat treatment (temperature of 120°C, 24 hours) using a steam sterilizer [SN-510 manufactured by Yamato Scientific Co., Ltd.], and the haze and viscosity average molecular weight (Mv) before and after the wet heat treatment were measured. The haze of the molded plate was measured according to JIS-K7361-1, and the viscosity average molecular weight (Mv) was measured by the following method.
[0066] Viscosity average molecular weight (Mv) measurement The specific viscosity (η SP ) was measured using an Ostwald viscometer from a solution of polycarbonate resin dissolved in 100 ml of methylene chloride at 20°C, and the specific viscosity (η SP ) and the viscosity average molecular weight Mv was calculated using the following formula: Specific viscosity (η SP )=(t-t0) / t0 [t0 is the number of seconds that methylene chloride falls, and t is the number of seconds that the sample solution falls] η SP / c=[η]+0.45×[η] 2 c (where [η] is the intrinsic viscosity) [η]=1.23×10 -4 Mv 0.83 c=0.7
[0067] The higher the haze after moist heat treatment, the lower the transparency of the molded plate, and the greater the decrease in viscosity average molecular weight after moist heat treatment, the more susceptible the resin is to hydrolysis. The increase in haze before and after moist heat treatment is expressed as ΔHaze, with ΔHaze of 1.0 or less being rated as O and anything over 1.0 being rated as X. Additionally, the decrease in Mv before and after moist heat treatment is expressed as ΔMv, with ΔMv of 1,000 or less being rated as O and anything over 1,000 being rated as X.
[0068] [Examples 1 to 10 and Comparative Examples 1 to 7] Component A, component B and other components were mixed in a blender in the amounts shown in Table 1, and then melt-kneaded using a vented twin-screw extruder to obtain pellets. The vented twin-screw extruder used was a TEX30α (fully intermeshing, same-direction rotation, two-thread screw) manufactured by Japan Steel Works, Ltd. The extrusion conditions were a discharge rate of 30 kg / h, a screw rotation speed of 270 rpm, and a vent vacuum of 1 kPa, and the extrusion temperature was 260°C (when component A-1 was used) and 290°C (when component A-2 was used). The evaluation results are shown in Table 1.
[0069] [Table 1] [Industrial Applicability]
[0070] The polycarbonate resin composition of the present invention has excellent light conductivity and is less susceptible to yellowing during molding and deterioration in a moist and hot environment. Molded articles obtained from the polycarbonate resin composition are extremely useful for various industrial applications, such as in the fields of lighting including LED lighting, office automation equipment, electric and electronic equipment, and automobiles.
Claims
1. A surface light source using a molded article made of a polycarbonate resin composition having light guiding properties, the polycarbonate resin composition comprising 100 parts by weight of (A) a polycarbonate resin (component A) obtained by reacting 2,2-bis(4-hydroxyphenyl)propane with a carbonate precursor, (B) 0.005 to 0.2 parts by weight of a thioether compound (component B) represented by the following formula [1] or [2], 0 to 1 part by weight of a phosphorus-based antioxidant, 0 to 1 part by weight of a phenol-based antioxidant, and 0 to 1 part by weight of a release agent, the molded article having a thickness of 2 mm and an average spectral transmittance of 85.0% or more in a wavelength range of 340 nm to 420 nm. (R 1 -S-CH 2 -CH 2 -C(O)O-CH 2 ) 4 -C 〔1〕 [In formula (1), R 1 may be the same or different and are linear or branched alkyl groups having 4 to 20 carbon atoms. (R 2 -O-C(O)-CH 2 -CH 2 -) 2 -S 〔2〕 [In formula (2), R 2 may be the same or different and are linear or branched alkyl groups having 6 to 22 carbon atoms.
2. 2. The surface light source according to claim 1, wherein the thioether compound is at least one thioether compound selected from the group consisting of dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate and pentaerythritol tetrakis(3-laurylthiopropionate).
3. 3. The surface light source according to claim 1, wherein the b* value of a molded product having a thickness of 2 mm is 0.4 or less.
4. 3. The surface light source according to claim 1, wherein a molded product having a thickness of 2 mm has a haze value of 0.1 or less.
5. 3. The surface light source according to claim 1, wherein a .DELTA.Haze value of a molded product having a thickness of 2 mm before and after wet heat treatment (at 120.degree. C. for 24 hours) is 1.0 or less.
6. 3. The surface light source according to claim 1, wherein the molded product is a molded plate obtained by molding a polycarbonate resin composition into a plate shape.
7. 7. The surface light source according to claim 6, wherein the surface light source comprises a shaped plate having a light source disposed on at least one side thereof and a reflector disposed on one side thereof.
8. 8. The surface light source according to claim 7, wherein the light source of the surface light source is a fluorescent lamp, a cold cathode fluorescent tube, an LED, a laser diode or an organic EL.
9. 3. The surface light source according to claim 1 or 2, which is used as a display part of a mobile phone, a mobile terminal, a camera, a watch, a notebook computer, a display, a lighting device, a signal, an automobile lamp, or a home electronics or optical device.
Citation Information
Patent Citations
Molding material for optical application
JP1991079659A
Aromatic polycarbonate resin composition
JP1999106632A
Aromatic polycarbonate resin composition for lightguide plate, and lightguide plate
JP2007204737A
Polycarbonate resin composition for light guide panel and light guide panel made of polycarbonate resin composition
JP2008024911A
Polycarbonate resin composition and light guide body composed of the same
JP2018044062A