Capacitor, electronic device including the same, and method of manufacturing the capacitor
The introduction of an intermediate layer with a tailored crystal structure and cation composition in capacitors addresses the challenge of high leakage current, improving capacitor performance by enhancing the Schottky barrier height and maintaining capacitance.
Patent Information
- Application Number
- JP2024135672
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-07-23
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-07-22
AI Technical Summary
Existing capacitors face challenges in maintaining high capacitance while reducing leakage current, particularly due to the limitations of structural improvements and the use of ternary oxide dielectrics with small band gaps, leading to significant leakage currents between electrodes and dielectrics.
Incorporation of an intermediate layer with a specific crystal structure and composition between the thin film electrode layers and dielectric layer, comprising anionized and neutral layers with specific cations, to enhance the Schottky barrier height and reduce leakage current.
The intermediate layer effectively increases the Schottky barrier height, thereby reducing leakage current and maintaining or enhancing capacitor capacitance, while ensuring structural stability.
Smart Images

Figure 2024161500000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a capacitor, an electronic device including the same, and a method for manufacturing the same. [Background technology]
[0002] 2. Description of the Related Art Semiconductor devices such as memories and transistors are used in a variety of home and industrial devices. As the performance of home and industrial devices increases, the integration and miniaturization of semiconductor devices is progressing.
[0003] As semiconductor devices become more highly integrated and miniaturized, the size of the semiconductor devices is reduced. For example, as the size of a capacitor is reduced, the capacitance of the capacitor is reduced and leakage current is increased. To solve these problems, various methods have been proposed.
[0004] For example, the capacitance of a capacitor can be maintained by changing the structure of the capacitor by increasing the electrode area of the capacitor or reducing the dielectric thickness, or by improving the capacitor manufacturing process.
[0005] However, there is a limit to how much the capacitance of a capacitor can be maintained by structural improvements such as increasing the electrode area of the capacitor or reducing the dielectric thickness, or by improvements in the manufacturing process.
[0006] Ternary oxide dielectric materials can be used for high capacitance. A representative ternary oxide dielectric is a ternary oxide containing divalent cations and tetravalent cations, and has a perovskite crystal structure with a composition ratio of divalent cations, tetravalent cations, and oxygen of 1:1:3. The ternary oxide dielectric is, for example, SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , SrZrO 3 , PbTiO 3The ternary oxide dielectric is not limited to these, and ternary oxides containing other cations are also used as dielectrics. However, the band gap of the ternary oxide dielectric is small, 3 eV to 4 eV, so that the leakage current between the electrode and the dielectric is large.
[0007] Therefore, it is important to suppress leakage current between the electrodes and the dielectric.
[0008] As a method for improving the leakage current characteristics between the electrode and the dielectric, a method for adjusting the Schottky barrier can be considered.
[0009] The Schottky barrier is the difference between the work function (Φ) of the electrode and the electron affinity (χ) of the dielectric film of the dielectric, and when the electrode and the dielectric are in contact with each other, their Fermi levels become the same, and as a result, an energy barrier called a Schottky barrier is formed at the interface between the electrode and the dielectric, which suppresses the transfer of charges and improves leakage current. When the dielectric is an n-type semiconductor, the Schottky barrier height (SBH) becomes higher as the work function of the electrode is higher than the electron affinity of the dielectric.
[0010] In order to realize a high Schottky barrier height (SBH) between the dielectric and the electrode, the following conditions must be satisfied: the crystal structure and lattice constant of the dielectric and the electrode are similar, the stability of the interface between the dielectric and the electrode is high, and the work function of the electrode is higher than the electron affinity of the dielectric. It is not easy to realize a capacitor with a high Schottky barrier height between the dielectric and the electrode.
[0011] Therefore, a new capacitor is needed that has an increased Schottky barrier height between the dielectric and the electrodes compared to conventional capacitors, thereby suppressing leakage current. Summary of the Invention [Problem to be solved by the invention]
[0012] An object of the present invention is to provide a capacitor in which leakage current is suppressed by including an intermediate layer having a new structure.
[0013] Another object of the present invention is to provide an electronic device including the dielectric material.
[0014] Another object of the present invention is to provide a method for manufacturing the capacitor. [Means for solving the problem]
[0015] According to one aspect, a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and An interlayer is disposed between the first thin-film electrode layer and the dielectric layer, or between the second thin-film electrode layer and the dielectric layer, The intermediate layer has a crystal structure of the same type as one or more of the electrode layer and the dielectric layer in contact with the intermediate layer, and has a composition different from each other; the intermediate layer comprises a first anionized layer, a second anionized layer, or a first neutral layer; the first anionization layer comprises monovalent cations, divalent cations, or trivalent cations having an atomic weight of 20 or more; the second anionization layer comprises monovalent cations; A capacitor is provided, wherein the first neutral layer includes a plurality of trivalent cations.
[0016] The first anionization layer is [B1O 2 ] a- It is expressed as B1 is a monovalent cation, a divalent cation, or a trivalent cation having an atomic weight of 20 or more; The a may be 1, 2 or 3.
[0017] B1 can be Li, Na, K, Rb, Cs, Mg, Be, Ba, Ca, Ga or In.
[0018] The first anionization layer is [GaO 2 ] - , [InO 2 ] - , [BeO 2 ] 2- , [MgO 2 ] 2- , [BaO 2 ] 2- , [CaO 2 ] 2- , [LiO 2 ] 3- , [NaO 2 ] 3- , [KO 2 ] 3- or [RbO 2 ] 3- It may be expressed as:
[0019] the intermediate layer comprises the first anionization layer; further comprising a second neutral layer; The second neutral layer may be represented by [A1O], where A1 is a divalent cation.
[0020] The A1 can be Sr, Ca, Ba, Mg or Be.
[0021] The second neutral layer may be represented by [SrO], [CaO], [BaO], [MgO] or [BeO].
[0022] the intermediate layer comprises a first anionizable layer and a second neutral layer; the first anionization layer and the second neutral layer are stacked on top of each other; The first anionization layer and the second neutral layer may comprise different metals.
[0023] The intermediate layer may contain a metal oxide having a perovskite crystal structure represented by the following Chemical Formula 1: [Chemical formula 1] [A1B1O x ] In the above Chemical Formula 1, A1 is a divalent cation, B1 is a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 20 or more; 2.5 <x≦3.0である。
[0024] The intermediate layer is [SrGaO x ], [CaGaO x ], [BaGaO x ], [PbGaO x ], [SrInO x ], [CaInO x ], [BaInO x ], [PbInO x ], [SrBeO x ], [CaBeO x ], [BaBeO x ], [PbBeO x ], [SrMgO x ], [CaMgO x ], [BaMgO x ], [PbMgO x ], [SrBaO x ], [CaBaO x ], [PBBaO x ], [SrCaO x ], [BaCaO x ], [PbCaO x ], [SrLiO x ], [CaLiO x ], [BaLiO x ], [PbLiO x ], [SrNaO x ], [CaNaO x], [BaNaO x ], [PbNaO x ] [SrKO x ], [CaKO x ], [BaKO x ], [PbKO x ], [SrRbO x ], [CaRbO x ], [BaRbO x ] or [PbRbO x
[0023] 2.5 <x≦3.0であってもよい。
[0025] The second anionization layer is [A2O] - wherein A2 may be a monovalent cation.
[0026] The A2 may be Li, Na, K, Rb or Cs.
[0027] The second anionization layer is [LiO] - , [NaO] - , [KO] - or [RbO] - It may be expressed as:
[0028] the intermediate layer comprises the second anionizable layer; Further comprising a third neutral layer; The third neutral layer is [BO 2 ], and B2 may be a tetravalent cation.
[0029] The B2 may be Ti, Hf or Zr.
[0030] The third neutral layer is [TiO 2 ], [ZrO 2 ] or [HfO 2 ] may also be expressed as:
[0031] The intermediate layer may include a metal oxide having a perovskite crystal structure represented by the following Chemical Formula 2: [Chemical formula 2] [A2B2O x ] In the above Chemical Formula 1, A2 is a monovalent cation, B2 is a tetravalent cation, 2.5≦x≦3.0.
[0032] The intermediate layer is [LiTiO x ], [NaTiO x ], [KTiO x ], [RbTiO x ], [LiZrO x ], [NaZrO x ], [KZrO x ], [RbZrO x ], [LiHfO x ], [NaHfO x ], [KHfO x ] or [RbHfO x
[0023] 2.5 <x≦3.0でありうる。
[0033] The first neutral layer may include a metal oxide having a perovskite crystal structure represented by the following Chemical Formula 3: [Chemical formula 3] [A3B3O 3 ] In the above Chemical Formula 3, A3 is a trivalent cation, B3 is a trivalent cation.
[0034] The intermediate layer is [ScAlO 3 ], [YAlO 3 ], [LaAlO 3 ], [CeAlO 3 ], [PrAlO 3 ], [NdAlO 3 ], [SmAlO 3], [DyAlO 3 ], [ScGaO 3 ], [YGaO 3 ], [LaGaO 3 ], [CeGaO 3 ], [PrGaO 3 ], [NdGaO 3 ], [SmGaO 3 ], [DyGaO 3 ], [ScInO 3 ], [YInO 3 ], [LaInO 3 ], [CeInO 3 ], [PrInO 3 ], [NdInO 3 ], [SmInO 3 ] or [DyInO 3 The metal oxide may be selected from the group consisting of:
[0035] The first neutral layer is [A3O] + A first cationized layer represented by [B3O 2 ] - and a third anionization layer represented by The A3 may be a trivalent cation, the B3 may be a trivalent cation, and A3 and B3 may be different metals.
[0036] A3 is Sc, Y, La, Ce, Pr, Nd, Sm or Dy; The B3 can be Al, Ga or In.
[0037] The intermediate layer is [ScO] + , [YO] + , [LaO] + [CeO] + , [PrO] + , [NdO] + , [SmO] + Or [DyO] + A first cationized layer represented by [AlO 2 ]- , [GaO 2 ] - or [InO 2 ] - and a third anionization layer represented by:
[0038] the intermediate layer comprises 1 unit cell to 3 unit cells, and the thickness of the intermediate layer is 1 Å to 15 Å; a Schottky barrier height (SBH) between the first thin-film electrode layer or the second thin-film electrode layer and the dielectric layer is 1.5 eV or more; The intermediate layer may be formed by epitaxial growth.
[0039] The dielectric layer may include a dielectric material having a perovskite crystal structure represented by the following Chemical Formula 4: [Chemical formula 4] A4B4O 3 In the above Chemical Formula 4, A4 is a monovalent, divalent or trivalent cation; B4 is a trivalent cation, a tetravalent cation, or a pentavalent cation.
[0040] The dielectric layer is SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , CaHfO 3 , BaHfO 3 , SrZrO 3 , CaZrO 3 , BaZrO 3 , PbTiO 3 , NaNbO 3 , NaTaO 3 , RbTaO 3 , RbNbO 3 , RbTaO 3 or EuTiO 3 The dielectric may include a dielectric material selected from the group consisting of:
[0041] The thickness of the dielectric layer is 10 nm to 100 nm, The first thin-film electrode layer and the second thin-film electrode layer each have a thickness of 10 nm to 1,000 nm; At least one of the first thin-film electrode layer and the second thin-film electrode layer may have a perovskite crystal structure.
[0042] According to another aspect, There is provided an electronic device including a capacitor in accordance with the foregoing.
[0043] The electronic device may be a semiconductor device.
[0044] According to yet another aspect, providing a first thin-film electrode layer or a second thin-film electrode layer; disposing an intermediate layer on one surface of the first thin-film electrode layer or the second thin-film electrode layer by epitaxial growth; disposing a dielectric layer on the intermediate layer; and depositing another thin film electrode layer on the dielectric layer to provide a capacitor. the capacitor comprises: a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed between the first thin-film electrode layer and a dielectric layer and / or between the second thin-film electrode layer and the dielectric layer; the intermediate layer has the same crystal structure as at least one of the electrode layer and the dielectric layer in contact with the intermediate layer, and has a different composition from the electrode layer and the dielectric layer; the intermediate layer comprises a first anionizable layer, a second anionizable layer, or a first neutral layer; the first anionization layer comprises monovalent cations, divalent cations, or trivalent cations having an atomic weight of 20 or more; the second anionization layer comprises monovalent cations; the first neutral layer comprises a plurality of trivalent cations; A method for manufacturing a capacitor is provided, in which the dielectric layer comprises a ternary oxide with a perovskite crystal structure. Effect of the Invention
[0045] According to one aspect, the leakage current of the capacitor is reduced by including an intermediate layer having a novel structure. [Brief description of the drawings]
[0046] [Figure 1A] 1 is a schematic diagram of a capacitor including an intermediate layer according to an embodiment; [Figure 1B] 1 is an enlarged schematic diagram illustrating a structure of an intermediate layer portion of a capacitor including an intermediate layer according to an embodiment; [Figure 2A] 1 is a schematic diagram of a capacitor including an intermediate layer according to an embodiment; [Figure 2B] 1 is an enlarged schematic diagram illustrating a structure of an intermediate layer portion of a capacitor including an intermediate layer according to an embodiment; [Figure 3A] 1 is a schematic diagram of a capacitor including an intermediate layer according to an embodiment; [Figure 3B] 1 is an enlarged schematic diagram illustrating a structure of an intermediate layer portion of a capacitor including an intermediate layer according to an embodiment; [Figure 4A] 1 is an enlarged schematic diagram illustrating a structure of an intermediate layer portion of a capacitor including an intermediate layer according to an embodiment; [Figure 4B] 1 is an enlarged schematic diagram illustrating a structure of an intermediate layer portion of a capacitor including an intermediate layer according to an embodiment; [Figure 5A] 1 is a schematic diagram of a capacitor according to an embodiment; [Figure 5B] 1 is a schematic diagram of a capacitor according to an embodiment; [Figure 5C] 1 is a schematic diagram of a capacitor according to an embodiment; [Figure 5D] 1 is a schematic diagram of a capacitor according to an embodiment; [Figure 6]1 is a cross-sectional view showing a structure of a metal-insulator-metal (MIM) capacitor according to an embodiment. [Figure 7] 1 is a diagram showing a structure of a trench capacitor type dynamic random access memory (DRAM) according to an embodiment. [Figure 8] 1 is a cross-sectional view illustrating a memory device having a layered structure including a dielectric layer according to an embodiment; [Figure 9] 1 is a layout diagram illustrating a semiconductor device according to an embodiment; [Figure 10] 1 is a conceptual diagram illustrating a device architecture that can be applied to an electronic device according to an embodiment; [Figure 11] 1 is a conceptual diagram illustrating a device architecture that can be applied to an electronic device according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0047] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail. However, they do not limit the present inventive concept to specific embodiments, and should be understood to include all modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.
[0048] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the following, terms such as "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the context.
[0049] In the drawings, thicknesses are exaggerated or reduced to clearly depict the various layers and regions. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, or plate, is described as being "on" or "above" another part, this includes not only when it is directly on top of the other part, but also when there is another part between them. Throughout the specification, terms such as "first" and "second" may be used to describe various components, but the components are not limited by such terms. Such terms are used only to distinguish one component from another. In this specification and the drawings, components having substantially the same function and configuration are referred to by the same reference numerals to avoid redundant description.
[0050] Hereinafter, a capacitor according to example embodiments, an electronic device including the same, and a method for manufacturing the capacitor will be described in further detail.
[0051] A capacitor according to an embodiment includes a first thin-film electrode layer, a second thin-film electrode layer, a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer, and an interlayer disposed between the first thin-film electrode layer and the dielectric layer and / or between the second thin-film electrode layer and the dielectric layer, the interlayer having the same type of crystal structure as at least one of the electrode layer and the dielectric layer in contact with the interlayer, and having a different composition from the electrode layer and / or the dielectric layer, the interlayer including a first anionized layer, a second anionized layer, or a first neutral layer, the first anionized layer including a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 20 or more, the second anionized layer including a monovalent cation, and the first neutral layer including a plurality of trivalent cations. For example, the first anionized layer includes a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 40 or more.
[0052] The intermediate layer includes a first anionization layer, a second anionization layer, or a first neutral layer, so that the intermediate layer induces a screening charge on the adjacent thin-film electrode layer. Such screening electrons induce an additional electrostatic potential difference between the thin-film electrode layer and the dielectric layer. Thus, the Schottky barrier height (SBH) between the thin-film electrode layer and the dielectric layer is further increased, and as a result, the leakage current of the capacitor including the intermediate layer is reduced. For example, since the first anionization layer and the second anionization layer have a negative charge, a screening charge having a positive charge is induced on the adjacent thin-film electrode layer. For example, the first neutral layer is neutral as a whole, but includes a third positive charge layer and a first negative charge layer in the first neutral layer, so that a screening charge is induced on the adjacent thin-film electrode layer. As a result, the leakage current of the capacitor including such an intermediate layer is reduced.
[0053] Referring to FIGS. 1A and 1B, the capacitor includes a first thin film electrode layer; a second thin film electrode layer; a dielectric layer disposed between the first thin film electrode layer and the second thin film electrode layer; and an intermediate layer disposed in one or more of the spaces between the first thin film electrode layer and the dielectric layer and between the second thin film electrode layer and the dielectric layer, the intermediate layer including a first anionized layer. The first thin film electrode layer, the second thin film electrode layer, the dielectric layer, and the intermediate layer can have, for example, a perovskite type crystal structure. The perovskite type crystal structure can have a composition of ABO 3 or a similar ABO x (0 < x ≦ 3) composition. In the above composition having a perovskite structure, A can be disposed at a cuboctahedral site coordinated with 12 oxygen atoms, and B can be disposed at an octahedral site coordinated with 6 oxygen atoms. The dielectric layer includes, for example, a ternary oxide (ABO 3 ) having a perovskite crystal structure composed of a divalent A cation and a tetravalent B cation. The ternary oxide included in the dielectric layer is, for example, SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , SrZrO 3 , PbTiO 3 , etc. The oxides included in the dielectric layer are not limited thereto, and perovskite ternary oxides containing other cations are also possible.
[0054] The first anionized layer can be represented by, for example, [B1O 2 a- . B1 is, for example, a monovalent cation, a divalent cation, or a trivalent cation having an atomic weight of 20 or more or an atomic weight of 40 or more, and a is 1, 2, or 3. By including such a first anionized layer in the capacitor, the leakage current of the capacitor can be more effectively suppressed. B1 included in the first anionized layer can be disposed, for example, at an octahedral site coordinated with 6 oxygen atoms in the perovskite structure.
[0055] B1 is, for example, an alkali metal element that forms a monovalent cation, and may include Li, Na, K, Rb, or Cs. B1 is, for example, an alkaline earth metal element that forms a divalent cation, and may include Mg, Be, Ba, or Ca. B1 is, for example, an element that forms a trivalent cation, and may include Ga or In as a metal element belonging to group 13 of the periodic table. By including such an element in B1, an increased Schottky barrier height (SBH) can be effectively induced.
[0056] When B1 is an element that forms a trivalent cation with an atomic weight of less than 20 or less than 40, the ionic size (ionic radii) of the intermediate layer may be significantly different from the corresponding metal cation contained in the electrode or dielectric, and the structural stability of the intermediate layer may be reduced. Therefore, the structural stability of a capacitor having an intermediate layer containing a trivalent cation with an atomic weight of less than 20 or less than 40 may be reduced.
[0057] The first anionization layer may be, for example, [GaO 2 ] - , [InO 2 ] - , [BeO 2 ] 2- , [MgO 2 ] 2- , [BaO 2 ] 2- , [CaO 2 ] 2- , [LiO 2 ] 3- , [NaO 2 ] 3- , [KO 2 ] 3- or [RbO 2 ] 3-The intermediate layer may be expressed as follows. By including such a first anionization layer in the intermediate layer, the leakage current of the capacitor including the intermediate layer may be more effectively suppressed. The first anionization layer may be confirmed, for example, by using high-angle annular dark-field-scanning transmission electron microscopy (HAADF-STEM).
[0058] The intermediate layer may further include a second neutral layer in addition to the first anionizable layer, i.e., the intermediate layer may include a first anionizable layer and a second neutral layer.
[0059] The second neutral layer can be represented, for example, by [A1O]. A1 is, for example, a divalent cation. A1 is a cation to which 12 oxygen atoms are coordinated in the dielectric material constituting the capacitor. For example, SrTiO 3 ,SrHfO 3 ,SrZrO 3 In the case of a dielectric, the second neutral layer is [SrO] and CaTiO 3 In the case of dielectrics, the second neutral layer is [CaO] and BaTiO 3 In the case of dielectrics, the second neutral layer is [BaO] and PbTiO 3 In the case of a dielectric, the second neutral layer can be [PbO]. The composition of the second neutral layer depends on the A-site material of the dielectric material used.
[0060] The intermediate layer further includes a second neutral layer, which can improve the structural stability of the first anionization layer. In addition, the structural similarity between the intermediate layer and the thin-film electrode layer and the dielectric layer is increased, which can improve the overall structural stability of the intermediate layer. As a result, the structural stability of the capacitor can be improved. The second neutral layer can be confirmed, for example, by using HAADF-STEM.
[0061] The intermediate layer may, for example, include a first anionization layer and a second neutral layer, and the first anionization layer and the second neutral layer may be stacked on each other. The first anionization layer and the second neutral layer may be stacked in sequence along the
[0001] direction on the (001) surface of a substrate, for example, a thin-film electrode layer or a dielectric layer. The order in which the first anionization layer and the second neutral layer are stacked may be changed or selected depending on the surface structure of the substrate, for example, a thin-film electrode layer or a dielectric layer.
[0062] The first anionization layer and the second neutral layer contained in the intermediate layer each contain a different metal. By the first anionization layer and the second neutral layer each containing a different metal, the intermediate layer can have, for example, a perovskite crystal structure.
[0063] The intermediate layer can be composed of one compound by including a first anionization layer and a second neutral layer. The compound forming the intermediate layer is unstable in a bulk state, but can maintain stability when it has a thickness of several nm.
[0064] The intermediate layer may contain, for example, a metal oxide having a perovskite crystal structure represented by the following chemical formula 1: [Chemical formula 1] [A1B1O x ] In chemical formula 1, A1 is a divalent cation, B1 is a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 20 or more; 2.5 <x≦3.0である。 B1 is, for example, a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 40 or greater.
[0065] Although the metal oxide represented by Chemical Formula 1 is unstable in a bulk state, stability can be maintained in an intermediate layer having a thickness of several nm.
[0066] The intermediate layer is made of [SrGaO x ], [CaGaO x ], [BaGaOx ], [PbGaO x ], [SrInO x ], [CaInO x ], [BaInO x ], [PbInO x ], [SrBeO x ], [CaBeO x ], [BaBeO x ], [PbBeO x ], [SrMgO x ], [CaMgO x ], [BaMgO x ], [PbMgO x ], [SrBaO x ], [CaBaO x ], [PbBaO x ], [SrCaO x ], [BaCaO x ], [PbCaO x ], [SrLiO x ], [CaLiO x ], [BaLiO x ], [PbLiO x ], [SrNaO x ], [CaNaO x ], [BaNaO x ], [PbNaO x ], [SrKO x ], [CaKO x ], [BaKO x ], [PbKO x ], [SrRbO x ], [CaRbO x ], [BaRbO x ] or [PbRbO x In such metal oxides, 2.5 <x≦3.0でもある。
[0067] 2A and 2B, the capacitor includes a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed at least one of between the first thin-film electrode layer and the dielectric layer and between the second thin-film electrode layer and the dielectric layer, the intermediate layer including a second anionization layer. The first thin-film electrode layer, the second thin-film electrode layer, the dielectric layer, and the intermediate layer may have, for example, a perovskite-type crystal structure. The dielectric layer may be, for example, a ternary oxide (ABO) having a perovskite crystal structure composed of divalent A cations and tetravalent B cations. 3 The ternary oxide contained in the dielectric layer is, for example, SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , SrZrO 3 , PbTiO 3 The oxide contained in the dielectric layer is not limited to these, and perovskite ternary oxides containing other cations are also possible.
[0068] The second anionization layer may be, for example, [AO] - A2 may be, for example, a monovalent cation. The capacitor may include such a second anionization layer, so that the leakage current of the capacitor may be more effectively suppressed. The A2 included in the second anionization layer may be, for example, arranged in a cuboctahedral site in which 12 oxygen atoms are coordinated in the perovskite structure.
[0069] A2 is, for example, an alkali metal element that forms a monovalent cation, and includes Li, Na, K, Rb, or Cs. A2 having such an element can effectively induce an increased Schottky barrier height (SBH).
[0070] The second anionization layer may be, for example, [LiO] - , [NaO] - , [KO] - or [RbO] -The intermediate layer may be represented by the formula: By including such a second anionization layer in the intermediate layer, the leakage current of the capacitor including the intermediate layer may be more effectively suppressed. The second anionization layer may be confirmed, for example, by using HAADF-STEM.
[0071] The intermediate layer may further include a third neutral layer in addition to the second anionizable layer, i.e., the intermediate layer may include a second anionizable layer and a third neutral layer.
[0072] The third neutral layer may be, for example, [BO 2 B2 is a cation to which six oxygen atoms are coordinated in the dielectric layer material, and B2 is, for example, a tetravalent cation. For example, SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , SrZrO 3 , PbTiO 3 In such dielectric materials, B2 can be, for example, Ti, Hf or Zr. The third neutral layer can be, for example, [TiO 2 ], [ZrO 2 ] or [HfO2].
[0073] The intermediate layer further includes a third neutral layer, which can improve the structural stability of the second anionization layer. In addition, the intermediate layer has an increased structural similarity with the thin-film electrode layer and the dielectric layer, which can improve the overall structural stability of the intermediate layer. As a result, the structural stability of the capacitor can be improved. The third neutral layer can be confirmed, for example, by using HAADF-STEM.
[0074] The intermediate layer may, for example, include a second anionization layer and a third neutral layer, and the second anionization layer and the third neutral layer may be stacked one on top of the other. The second anionization layer and the third neutral layer may be stacked in sequence along the
[0001] direction on the (001) surface of a substrate, for example, a thin-film electrode layer or a dielectric layer. The order in which the second anionization layer and the third neutral layer are stacked may be changed or selected depending on the surface structure of the substrate, for example, a thin-film electrode layer or a dielectric layer.
[0075] The second anionization layer and the third neutral layer contained in the intermediate layer each contain a different metal. By the second anionization layer and the third neutral layer each containing a different metal, the intermediate layer can have, for example, a perovskite crystal structure.
[0076] The intermediate layer can be composed of one compound by including a second anionization layer and a third neutral layer. The compound forming the intermediate layer is unstable in a bulk state, but can maintain stability when it has a thickness of several nm.
[0077] The intermediate layer may contain, for example, a metal oxide having a perovskite crystal structure represented by the following chemical formula 2: [Chemical formula 2] [A2B2O x ] In chemical formula 2, A2 is a monovalent cation, B2 is a tetravalent cation, 2.5 <x≦3.0である。
[0078] Although the metal oxide represented by Chemical Formula 2 is unstable in a bulk state, stability can be maintained in an intermediate layer having a thickness of several nm.
[0079] The intermediate layer may be, for example, [LiTiO x ], [NaTiO x ], [KTiO x ], [RbTiO x ], [LiZrO x ], [NaZrO x ], [KZrOx ], [RbZrO x ], [LiHfO x ], [NaHfO x ], [KHfO x ] or [RbHfO x In such metal oxides, 2.5 <x≦3.0でもある。
[0080] 3A and 3B, the capacitor includes a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed at least one of between the first thin-film electrode layer and the dielectric layer and between the second thin-film electrode layer and the dielectric layer, the intermediate layer including a first neutral layer. The first thin-film electrode layer, the second thin-film electrode layer, the dielectric layer, and the intermediate layer may have, for example, a perovskite-type crystal structure. The dielectric layer may be, for example, a ternary oxide (ABO) having a perovskite crystal structure composed of divalent A cations and tetravalent B cations. 3 The ternary oxide contained in the dielectric layer is, for example, SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , SrZrO 3 , PbTiO 3 The oxide contained in the dielectric layer is not limited to these, and perovskite ternary oxides containing other cations are also possible.
[0081] The intermediate layer is also a first neutral layer. The first neutral layer is, for example, represented by the following chemical formula 3 and contains a metal oxide having a perovskite crystal structure: [Chemical formula 3] [A3B3O 3 ] In chemical formula 3, A3 is a trivalent cation, B3 is a trivalent cation.
[0082] A3 and B3 are, for example, different metals.
[0083] The first neutral layer may be, for example, [ScAlO 3 ], [YAlO 3 ], [LaAlO 3 ], [CeAlO 3 ], [PrAlO 3 ], [NdAlO 3 ], [SmAlO 3 ], [DyAlO 3 ], [ScGaO 3 ], [YGaO 3 ], [LaGaO 3 ], [CeGaO 3 ], [PrGaO 3 ], [NdGaO 3 ], [SmGaO 3 ], [DyGaO 3 ], [ScInO 3 ], [YInO 3 ], [LaInO 3 ], [CeInO 3 ], [PrInO 3 ], [NdInO 3 ], [SmInO 3 ] or [DyInO 3 The present invention also includes a metal oxide selected from the group consisting of:
[0084] The compound forming the first neutral layer may also be unstable in the bulk state, but may remain stable when it has a thickness of a few nm.
[0085] The first neutral layer also includes a first cationized layer and a third anionized layer. The first neutral layer includes the first cationized layer and the third anionized layer, which may make the first neutral layer structurally stable. In addition, the structural similarity between the intermediate layer including the first neutral layer and the thin-film electrode layer and the dielectric layer is increased, which may improve the overall structural stability of the intermediate layer. As a result, the structural stability of the capacitor may be improved. The third neutral layer may be confirmed, for example, using HAADF-STEM.
[0086] The first cationic layer is [AO]+ A3 may be represented by the formula: A3 is also a trivalent cation. A3 contained in the first cationized layer may be arranged, for example, in a cuboctahedral site in a perovskite structure where 12 oxygen atoms are coordinated. A3 is, for example, a metal element belonging to Group 3 of the periodic table that forms a trivalent cation, and may include Sc, Y, La, Ce, Pr, Nd, Sm, or Dy. The first cationized layer may be, for example, [ScO] + , [YO] + , [LaO] + [CeO] + , [PrO] + , [NdO] + , [SmO] + Or [DyO] + It can be expressed as:
[0087] The third anionization layer is [BO 2 ] - B3 can also be a trivalent cation. A3 and B3 are, for example, different metals. B3 contained in the third anionization layer can be, for example, arranged in an octahedral site in the perovskite structure where six oxygen atoms are coordinated. B3 can be, for example, a metal element belonging to Group 13 of the periodic table that forms a trivalent cation, and can also include Al, Ga, or In. The third anionization layer can be, for example, [AlO 2 ] - , [GaO 2 ] - or [InO 2 ] - It can be expressed as:
[0088] The first neutral layer includes a first positive ionization layer and a third negative ionization layer, which can effectively induce an increased Schottky barrier height (SBH).
[0089] By including such a first neutral layer in the intermediate layer, the leakage current of the capacitor including the intermediate layer can be more effectively suppressed. The first positive ionization layer and the third negative ionization layer can be confirmed, for example, by using HAADF-STEM.
[0090] 4A and 4B, the capacitor includes a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed between the first thin-film electrode layer and the dielectric layer and / or between the second thin-film electrode layer and the dielectric layer. The intermediate layer may include, for example, one to three unit cells, or one or two unit cells. The first thin-film electrode layer, the second thin-film electrode layer, the dielectric layer, and the intermediate layer may have, for example, a perovskite crystal structure. By having one to three unit cells, the intermediate layer may have an increased Schottky barrier height (SBH) while maintaining the structural stability of the intermediate layer.
[0091] The thickness of the intermediate layer is, for example, 1 Å to 15 Å, 2 Å to 12 Å, or even 2 Å to 10 Å. By having the intermediate layer have a thickness in such a range, the intermediate layer can have an increased Schottky barrier height (SBH) while maintaining the structural stability of the intermediate layer.
[0092] In a capacitor including the intermediate layer, the Schottky barrier height (SBH) between the first thin-film electrode layer or the second thin-film electrode layer and the dielectric layer is 1.5 eV or more, or 1.8 eV or more.
[0093] For example, in a capacitor including the intermediate layer, the Schottky barrier height (SBH) between the first thin-film electrode layer or the second thin-film electrode layer and the dielectric layer is 1.5 eV to 2.5 eV, or 1.8 eV to 2.1 eV.
[0094] The intermediate layer may be formed, for example, by epitaxial growth, and therefore may have a similar or identical crystal structure and lattice constant to the thin-film electrode layer and / or the dielectric layer, which may enhance interface stability.
[0095] 1A to 4B, the capacitor includes a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed between the first thin-film electrode layer and the dielectric layer and between the second thin-film electrode layer and the dielectric layer. The dielectric material contained in the dielectric layer is not particularly limited, and any dielectric material used as a dielectric material in the art is possible. The dielectric constant of the dielectric material at room temperature (25° C.) from 1 kHz to 1 MHz is, for example, 50 or more, 100 or more, 250 or more, or 500 or more. The dielectric constant of the dielectric material at room temperature (25° C.) from 1 kHz to 1 MHz is, for example, 100,000 or less, 50,000 or less, 10,000 or less, 5,000 or less, 1,000 or less, or 500 or less. The dielectric constant of the dielectric material at room temperature (25° C.) from 1 kHz to 1 MHz is also from 100 to 100,000, or from 100 to 10,000, or from 100 to 1000, or from 100 to 500.
[0096] The dielectric layer may include a dielectric material having a perovskite crystal structure, for example, represented by the following chemical formula 4: [Chemical formula 4] A4B4O 3 In chemical formula 4, A4 is a monovalent, divalent or trivalent cation; B4 is a trivalent cation, a tetravalent cation, or a pentavalent cation.
[0097] The dielectric layer is, for example, SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , CaHfO 3 , BaHfO 3 , SrZrO 3 , CaZrO 3 , BaZrO 3 , PbTiO 3 , NaNbO 3 , NaTaO 3 , RbTaO 3 , RbNbO 3, RbTaO 3 or EuTiO 3 The dielectric material may also include a dielectric material selected from the group consisting of:
[0098] The thickness of the dielectric layer included in the capacitor is greater than 10 nm and / or less than 100 nm, for example, between 10 nm and 100 nm. If the thickness of the dielectric layer is excessively increased, the capacitance per unit volume of the capacitor decreases. If the thickness of the dielectric layer is excessively thin, the ratio of the dielectric constant reduction region at the interface increases, so that the capacitance per unit volume of the capacitor decreases.
[0099] The thickness of the first thin-film electrode layer and / or the second thin-film electrode layer included in the capacitor is, for example, 10 nm to 1,000 nm, or 10 nm to 100 nm, respectively. If the thickness of the thin-film electrode layer is excessively increased, the capacitance per unit volume of the capacitor decreases. Also, if the thickness of the thin-film electrode layer is excessively thin and the thickness of the dielectric layer is excessively thin, the ratio of the dielectric constant reduction region at the interface increases, so that the capacitance per unit volume of the capacitor decreases.
[0100] At least one of the first thin-film electrode layer and the second thin-film electrode layer included in the capacitor may have a perovskite crystal structure. When the thin-film electrode layer has a perovskite crystal structure, the interface stability with the dielectric layer may be improved.
[0101] The capacitor includes the intermediate layer, so that the capacitance of the capacitor is increased and the leakage current is reduced. The type of the capacitor is not particularly limited. The capacitor may be, for example, a capacitor element included in a memory cell, a multilayer capacitor used in a multilayer ceramic capacitor, or the like.
[0102] 5A shows one structure of a capacitor 20 including the aforementioned intermediate layer (not shown). The structure includes an insulating substrate 100 and a pair of electrodes, a first thin-film electrode 11, a dielectric layer 12, and a second thin-film electrode 13. The first thin-film electrode 11 and the second thin-film electrode 13 act as a lower thin-film electrode and an upper thin-film electrode, respectively. The first thin-film electrode 11 and the second thin-film electrode 13 are not electrically connected, and a dielectric layer 12 is disposed between the first thin-film electrode 11 and the second thin-film electrode 13, and an intermediate layer (not shown) is disposed between the first thin-film electrode 11 and the dielectric layer 12 and / or between the second thin-film electrode 13 and the dielectric layer 12.
[0103] 5B-5D are examples of other structures of capacitor 20 that include the intermediate layer (not shown) discussed above.
[0104] 5B, a dielectric layer 12 is disposed so as to cover the first thin-film electrode 11 on the insulating substrate 100, and a second electrode 13 is disposed so as to cover the dielectric layer 12. An intermediate layer (not shown) is disposed between the first thin-film electrode 11 and the dielectric layer 12 and / or between the second thin-film electrode 13 and the dielectric layer 12.
[0105] 5C, a first thin-film electrode 11 and a second thin-film electrode 13 are disposed on an insulating substrate 100, with a dielectric layer 12 disposed therebetween. An intermediate layer (not shown) is disposed between the first thin-film electrode 11 and the dielectric layer 12 and / or between the second thin-film electrode 13 and the dielectric layer 12.
[0106] 5D, a dielectric layer 12 is disposed so as to cover a part of a first thin-film electrode 11 on an insulating substrate 100, and a second electrode 13 is disposed so as to cover another part of the dielectric layer 12. An intermediate layer (not shown) is disposed between the first thin-film electrode 11 and the dielectric layer 12 and / or between the second thin-film electrode 13 and the dielectric layer 12.
[0107] FIG. 6 shows a structure of a metal-insulator-metal (MIM) capacitor according to another embodiment.
[0108] 6, an interlayer insulating film 203 is stacked on a semiconductor substrate 201, and a contact plug 205 is formed thereon to fill a contact hole exposing the semiconductor substrate 201. A mold insulating film 213 is formed on the substrate having the contact plug 205, and the mold insulating film 213 has a structure in which a lower mold insulating film 207, an etch stop film 209, and an upper mold insulating film 211 are stacked in this order on the substrate having the contact plug 205. The etch stop film 209 is not limited to the position shown in FIG. 6, but may also be directly formed on the upper surface of the contact plug 205 and the interlayer insulating film 203. Alternatively, the mold insulating film 213 may be formed as a double layered mold insulating film of the lower mold insulating film 207 and the upper mold insulating film 211, or as a single mold insulating film. The lower mold insulating film 207 and the upper mold insulating film 211 may have an etching selectivity with respect to the etch stop film 209. For example, when the lower mold insulating layer 207 and the upper mold insulating layer 211 are formed of silicon oxide, the etch stop layer 209 may be formed of silicon nitride. The mold insulating layer 213 is patterned to form a storage node hole 215 exposing the upper surface of the contact plug 205 and the upper surface of the interlayer insulating layer 203 adjacent thereto.
[0109] A bottom electrode film 217', i.e., a conductive film for a bottom electrode, is formed on the entire surface of the semiconductor substrate having the storage node hole 215. The conductive film for the bottom electrode 217' is formed of a conductive film that has excellent step coverage, is less deformed during a subsequent process of forming a dielectric film, and has oxidation resistant properties. For example, the conductive film for the bottom electrode 217' is formed of strontium ruthenium oxide (SrRuO 3 ), iridium ruthenium oxide (IrRuO 3 ), strontium iridium oxide (SrIrO 3 ), calcium ruthenium oxide (CaRuO 3), calcium nickel oxide (CaNiO 3 ), barium ruthenium oxide (BaRuO 3 ), barium strontium ruthenium oxide ((Ba,Sr)RuO 3 ) may also be formed by at least one metal oxide film selected from the group consisting of:
[0110] A buffer insulating film 219 is formed on the lower electrode film 217', and an isolated lower electrode film 217' and a buffer insulating film pattern (not shown) are formed in the storage node hole 215. The buffer insulating film pattern (not shown) is selectively removed to expose the inner wall of the lower electrode film 217'. A dielectric film 224 in which a lower dielectric film 219 and an upper dielectric film 223 are sequentially stacked is formed on the entire surface of the semiconductor substrate 201 having the lower electrode film 217'. The lower dielectric film 219 and the upper dielectric film 223 may also include a dielectric material. For example, the upper dielectric film 223 may be formed of a high dielectric film having a higher dielectric constant than the lower dielectric film 219. The lower dielectric film 219 may also be formed of a dielectric film having a larger energy band gap than the upper dielectric film 223.
[0111] For example, the lower dielectric film 219 or the upper dielectric film 223 may be made of strontium titanium oxide (SrTiO 3 ), lithium niobium oxide (LiNbO 3 ,) Potassium niobium oxide (KNbO 3 ), potassium tantalum oxide (KTaO 3 ), barium titanium oxide (BaTiO 3 ), sodium niobium oxide (NaNbO 3 ), sodium tantalum oxide (NaTaO 3 ), calcium zirconium oxide (CaZrO 3 ), barium zirconium oxide (BaZrO 3 ), strontium zirconium oxide (SrZrO 3 ) may also be formed by a metal oxide film selected from the group consisting of
[0112] Alternatively, although not shown in the drawings, the lower dielectric film 219 and the upper dielectric film 223 may form one dielectric film, and such a dielectric film may be formed of the above-mentioned metal oxide film.
[0113] An upper electrode 225 is formed on the upper dielectric film 223, and the upper electrode 225 is also formed of a metal film having a higher work function than the lower electrode 217'.
[0114] The upper electrode 225 is also formed of at least one layer of a noble metal film selected from the group consisting of a Ru film, a Pt film, and an Ir film.
[0115] For example, the upper dielectric film 223 is Ta 2 O 5 Membrane, TiO 2 Films, doped TiO 2 The lower dielectric film 219 is also formed of at least one film selected from the group consisting of a HfO 2 Membrane, ZrO 2 Membrane, Al 2 O 3 Membrane and La 2 O 3 It is also formed by at least one film selected from the group consisting of films.
[0116] For example, the upper dielectric film 223 and the lower dielectric film 219 may be made of strontium titanium oxide (SrTiO 3 ) membranes.
[0117] The intermediate dielectric film 221 is interposed between the lower dielectric film 219 and the upper dielectric film 223. The lower dielectric film 219 and the upper dielectric film 223 may be formed of a crystalline dielectric film or an amorphous dielectric film, and the intermediate dielectric film 221 may be formed of a crystalline dielectric film or an amorphous dielectric film. That is, the lower dielectric film 219 may be formed of HfO having a crystalline structure or an amorphous structure. 2 Membrane, ZrO 2 Membrane, Al 2 O 3 Membrane and La 2 O 3The intermediate dielectric film 221 is also formed of at least one film selected from the group consisting of strontium titanium oxide (SrTiO 3 ) membranes.
[0118] For example, the intermediate dielectric film 221 may be HfO 2 having a crystalline or amorphous structure. 2 Membrane, ZrO 2 Membrane, Al 2 O 3 Membrane, La 2 O 3 Membrane, Ta 2 O 5 The intermediate dielectric film 221 may also be formed of at least one film selected from the group consisting of a strontium-titanium oxide (SrTiO 3 The upper dielectric film 223 may also be formed of a Ta film having a crystalline structure or an amorphous structure. 2 O 5 The intermediate dielectric film 221 may be formed of at least one film selected from the group consisting of a crystalline or amorphous dielectric film, a TiO film, a doped TiO film, and an STO film. In this way, the intermediate dielectric film 221 may be formed of a dielectric film having a crystalline structure or an amorphous structure, thereby improving the breakdown voltage characteristic of the dielectric film 224. For example, when the lower dielectric film 219 and the upper dielectric film 223 are formed of a crystalline dielectric film, the breakdown voltage of the lower dielectric film 219 and the upper dielectric film 223 is improved, but the leakage current characteristic thereof is reduced. Therefore, by forming the intermediate dielectric film 221, which is a dielectric film having an amorphous structure, between the lower dielectric film 219 and the upper dielectric film 223, a capacitor having excellent electrical characteristics such as leakage current characteristic and breakdown voltage characteristic can be provided.
[0119] An intermediate layer (not shown) is formed between the front surface of the semiconductor substrate 201 having the lower electrode film 217' and a dielectric film 224 in which a lower dielectric film 219, an intermediate dielectric film 221 and an upper dielectric film 223 are stacked in order.
[0120] The MIM capacitor further includes an intermediate layer (not shown) to further improve leakage current characteristics.
[0121] The MIM capacitor shown in FIG. 6 has, for example, a concave or cylindrical structure.
[0122] According to another embodiment, an electronic device includes the above-described capacitor. By including a capacitor having an intermediate layer, the electronic device has reduced leakage current and provides excellent device characteristics.
[0123] The electronic device is, for example, a semiconductor device. The electronic device is, for example, a memory device. The memory device is, for example, a dynamic random access memory (DRAM), a flash memory, etc.
[0124] FIG. 7 illustrates the structure of a trench capacitor type dynamic random access memory (DRAM).
[0125] 7, an isolation region is formed on a p-type semiconductor substrate 320 using a field oxide film 321, and a gate electrode 323 and source / drain impurity regions 322, 322' are formed in the isolation region. A high temperature oxide (HTO) film is formed as an interlayer insulating film 324, and a portion where no trench is formed is capped using a trench buffer layer, and then a portion of the source region 322 is opened to form a contact portion (not shown).
[0126] A trench is formed on the sidewall of the interlayer insulating film 324, and a sidewall oxide film 325 is formed on the entire sidewall of the trench. The sidewall oxide film 325 compensates for damage to the silicon substrate during etching for forming the trench, and also acts as a dielectric film between the silicon substrate and a storage electrode to be formed later. The source region 322 formed on the sidewall of the trench has a structure in which the entire sidewall of the source region 322 is exposed except for the gate side source region 322.
[0127] A PN junction 332 is formed on the sidewall of the source region 322 by impurity injection, the source region 322 is formed on the left side of the gate electrode, and the drain region 322' is formed on the right side of the gate electrode. A trench is formed in the source region 322, and the gate side of the trench directly contacts the source region 322 on the sidewall, and impurities are further injected into the source region 322 to form the PN junction 332.
[0128] A polysilicon layer is formed as a storage electrode 326 on a part of the interlayer insulating film 324, the exposed source region 322, and the surface of the sidewall oxide film 325 in the trench. The storage electrode 326 is formed so as to contact not only the source region 322 on the gate electrode 323 side, but also the entire source region 322 abutting the periphery of the upper sidewall of the trench. The source region 322 formed around the upper sidewall of the trench is expanded by the implanted impurities, and is more clearly in contact with the storage electrode 326. An insulating film 327 is formed along the upper surface of the storage electrode 326 as a dielectric of the capacitor, and a polysilicon layer is formed on the insulating film 327 as a plate electrode 328, thereby completing a trench capacitor type DRAM.
[0129] In such a trench capacitor type DRAM, the aforementioned intermediate layer (not shown) is further disposed between the storage electrode 326 and the dielectric insulating film 327 .
[0130] A method for manufacturing a capacitor according to another embodiment includes the steps of providing a first thin film electrode layer or a second thin film electrode layer, disposing an intermediate layer by epitaxial growth on one surface of the first thin film electrode layer or the second thin film electrode layer, disposing a dielectric layer on the intermediate layer, and disposing another thin film electrode layer on the dielectric layer to provide a capacitor, the capacitor including the first thin film electrode layer; the second thin film electrode layer; a dielectric layer disposed between the first thin film electrode layer and the second thin film electrode layer; and a dielectric layer disposed between the first thin film electrode layer and the dielectric layer, and The capacitor further includes an intermediate layer disposed between the second thin-film electrode layer and the dielectric layer, the intermediate layer having the same crystal structure as one or more of the electrode layer and the dielectric layer in contact with the intermediate layer, but having a different composition from them, the intermediate layer includes a first anionization layer, a second anionization layer, or a first neutral layer, the first anionization layer includes a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 20 or more, the second anionization layer includes a monovalent cation, and the first neutral layer includes a plurality of trivalent cations. For example, the first anionization layer may include a monovalent cation, a divalent cation, or a trivalent cation with an atomic weight of 40 or more. The capacitor manufactured by the above-mentioned manufacturing method may have a reduced leakage current by including an intermediate layer.
[0131] 5A to 5D, first, a first thin film electrode 11 or a second thin film electrode 13 is provided.
[0132] The first thin-film electrode 11 and / or the second thin-film electrode 13 are each made of, for example, strontium ruthenium oxide (SrRuO 3 ), iridium ruthenium oxide (IrRuO 3 ), strontium iridium oxide (SrIrO 3 ), calcium ruthenium oxide (CaRuO 3 ), calcium nickel oxide (CaNiO 3 ), barium ruthenium oxide (BaRuO 3 ), barium strontium ruthenium oxide ((Ba,Sr)RuO 3 ), iridium (Ir), iridium-ruthenium alloy (IrRu), iridium oxide (IrO2 ), titanium aluminum nitride (TiAlN), titanium oxide (TiO 2 ), ruthenium (Ru), platinum (Pt), zirconium oxide (ZrO 2 ), tin oxide (SnO 2 Any electrode material known in the art may be used, including, but not limited to, tin oxide (ITO), indium tin oxide (ITO), etc. They may be used alone or mixed with each other.
[0133] At least one of the first thin-film electrode 11 and the second thin-film electrode 13 is an oxide having a perovskite structure. For example, at least one of the first thin-film electrode 11 and / or the second thin-film electrode 13 is an oxide having a perovskite structure such as strontium ruthenium oxide (SrRuO 3 ), iridium ruthenium oxide (IrRuO 3 ), strontium iridium oxide (SrIrO 3 ), calcium ruthenium oxide (CaRuO 3 ), calcium nickel oxide (CaNiO 3 ), barium ruthenium oxide (BaRuO 3 ), barium strontium ruthenium oxide ((Ba,Sr)RuO 3 ) is also selected.
[0134] The first electrode 11 and / or the second electrode 13 are formed by depositing a metal, a metal oxide, a metal nitride, a metal oxynitride, or an alloy by an electron beam epitaxial process, a liquid phase epitaxial process, a vapor phase epitaxial process, a chemical vapor deposition process, a sputtering process, an atomic layer deposition process, a pulsed laser deposition process, etc. The first electrode 11 and the second electrode 13 have a single layer structure or a multilayer structure.
[0135] Alternatively, the first electrode 11 or the second electrode 13 is formed by coating and drying an electrode paste containing a conductive material to obtain a coating film, and then heat treating the coating film.
[0136] This coating method does not use a vacuum process or a high-temperature process, and therefore allows the first electrode 11 or the second electrode 13 to be manufactured easily.
[0137] The electrode paste includes conductive material particles, an organic component, and a solvent.
[0138] The conductive material can be any material that can be generally used as an electrode. The conductive material can be, for example, conductive metal oxides such as tin oxide, indium oxide, and indium tin oxide (ITO); metals such as platinum, gold, silver, copper, iron, tin, zinc, aluminum, indium, chromium, lithium, sodium, potassium, cesium, calcium, magnesium, palladium, molybdenum, amorphous silicon, and polysilicon, and alloys thereof; inorganic conductive materials such as copper iodide and copper sulfide; conductive polymers such as polythiophene, polypyrrole, polyaniline, polyethylenedioxythiophene, and polystyrenesulfonic acid, whose conductivity is improved by doping with a complex or iodine; and carbon materials. Such conductive materials may be used alone, but multiple materials can be used in a laminated or mixed form.
[0139] The conductive material is, for example, metal particles. By using the metal particles, the bending resistance of the capacitor is improved, and the coercive field does not increase even when the voltage is repeatedly applied. This is because the adhesion between the electrode and the dielectric layer is improved by the anchor effect caused by forming unevenness on the conductive film surface and disposing the dielectric layer on the unevenness. The metal particles are, for example, metal particles containing at least one of gold, silver, copper, platinum, lead, tin, nickel, aluminum, tungsten, molybdenum, ruthenium oxide, chromium, titanium, carbon, or indium.
[0140] The organic component and the solvent may be the same as those used for the dielectric layer.
[0141] Next, an intermediate layer (not shown) is disposed on one surface of the first thin-film electrode 11 or the second thin-film electrode 13 by epitaxial growth.
[0142] The intermediate layer may be the first anionization layer, the second anionization layer, or the first neutral layer. For more details regarding the intermediate layer, please refer to the capacitor section.
[0143] Epitaxial growth can use, for example, a molecular beam epitaxial process, a liquid phase epitaxial process, a vapor phase epitaxial process, and the like.
[0144] In the case of forming an intermediate layer (not shown) using a molecular beam epitaxy process, for example, the insulating substrate 100 on which the surface-treated first thin-film electrode 11 is formed is loaded into a reaction chamber, and the first thin-film electrode 11 is maintained at a temperature of about 400° C. to about 800° C., and the oxidant partial pressure in the chamber, for example, the oxygen partial pressure, is maintained at 10 -8 Torr or 10 -5 Torr. Metal was sublimated from the metal precursor to supply the metal constituting the intermediate layer. Next, the gaseous metal was introduced onto the surface-treated first thin-film electrode 11, and then an oxidizing agent was supplied to form an intermediate layer (not shown) on the surface-treated first thin-film electrode 11. The intermediate layer (not shown) was [GaO 2 ] - When the metal precursor comprises gallium or a first precursor compound containing gallium, the oxidizing agent is oxygen (O 2 ), ozone (O 3 ), nitrogen dioxide (NO 2 ) or nitrous oxide (N 2 O), etc. The oxidizing agent is, for example, oxygen.
[0145] Next, the dielectric layer 12 is disposed on the intermediate layer (not shown).
[0146] The dielectric layer 12 is, for example, strontium titanium oxide (SrTiO 3 ), lithium niobium oxide (LiNbO 3 ,) Potassium niobium oxide (KNbO 3 ), potassium tantalum oxide (KTaO 3), barium titanium oxide (BaTiO 3 ), calcium titanium oxide (CaTiO 3 ), lead titanium oxide (PbTiO 3 ), sodium niobium oxide (NaNbO 3 ), sodium tantalum oxide (NaTaO 3 ), calcium zirconium oxide (CaZrO 3 ), barium zirconium oxide (BaZrO 3 ), strontium zirconium oxide (SrZrO 3 ) is also selected.
[0147] The dielectric layer 12 may be an oxide having a perovskite structure. For example, the dielectric layer 12 may be strontium titanium oxide (SrTiO 3 ) as well.
[0148] The dielectric layer 12 may be formed using, for example, a chemical vapor deposition process, a metal organic chemical vapor deposition process, a molecular beam epitaxy process, a vapor phase epitaxy process, a liquid phase epitaxy process, a sol-gel process, a sputtering process, a pulsed laser deposition process, an atomic layer deposition process, or the like.
[0149] In the case of forming the dielectric layer 12 using a molecular beam epitaxy process, for example, the insulating substrate 100 on which the surface-treated first thin-film electrode 11 is formed is loaded into a reaction chamber, and the first thin-film electrode 11 is maintained at a temperature of about 400° C. to about 800° C., and the oxidant partial pressure in the chamber, for example, the oxygen partial pressure, is set to 10 -8 Torr or 10 -5 Torr. Metal is evaporated from a metal precursor to provide a vapor-phase metal that constitutes the intermediate layer. Next, the vapor-phase metal is introduced onto the surface-treated first thin-film electrode 11, and then an oxidizing agent is supplied to form an intermediate layer (not shown) on the surface-treated first thin-film electrode 11. The dielectric layer 12 is SrTiO 3In the case of the layer, the first metal precursor is strontium or a first precursor compound containing strontium, titanium or a second precursor compound containing titanium, and the oxidizing agent is oxygen (O 2 ), ozone (O 3 ), nitrogen dioxide (NO 2 ) or nitrous oxide (N 2 O), etc. The oxidizing agent is, for example, oxygen.
[0150] When the dielectric layer 12 is formed using a chemical vapor deposition process, the insulating substrate 100 on which the surface-treated first thin film electrode 11 is formed is loaded into a reaction chamber, and the reaction chamber is maintained at a temperature of about 500° C. to about 600° C. and a pressure of about 1 Torr to about 10 Torr. Next, an organometallic precursor is introduced onto the surface-treated first electrode 11, and an oxidizing agent is then supplied to form the dielectric layer 12 on the surface-treated first electrode 11. The dielectric layer 12 is SrTiO 3 In the case of the present invention, the organometallic precursor is strontium or a first precursor compound containing strontium, titanium or a second precursor compound containing titanium, and the oxidizing agent is oxygen (O 2 ), ozone (O 3 ), nitrogen dioxide (NO 2 ) or nitrous oxide (N 2 O) and others.
[0151] A heat treatment process may be performed on the dielectric layer 12 to further crystallize the material that constitutes the dielectric layer 12. For example, the dielectric layer 12 may be formed by adding oxygen (O 2 ) gas, nitrogen (N 2 ) gas, argon (Ar) gas, ammonia (NH 4 The substrate is then heat-treated by rapid thermal processing (RTP) in an atmosphere of a fluorine-containing gas, a fluorine-containing gas, or a mixture thereof, at a temperature of about 500° C. to about 650° C. for about 30 seconds to about 3 minutes.
[0152] Alternatively, the dielectric layer 12 may be formed by coating a dielectric paste containing the above-mentioned dielectric material, drying the resulting coating film, and then heat treating the resulting coating film.
[0153] This coating method does not use a vacuum process or a high-temperature process, so that the dielectric layer 12 can be easily manufactured.
[0154] The dielectric paste includes the above-mentioned dielectric, an organic component, and a solvent. The dielectric paste includes dielectric particles. The organic component fills the gaps between the dielectric particles to prevent short circuits in the capacitor and improve the production yield of the capacitor.
[0155] The organic component is, for example, a monomer, an oligomer or a polymer, a photopolymerization initiator, a plasticizer, a leveling agent, a surfactant, a silane coupling agent, an antifoaming agent, a pigment, a dispersant, etc. From the viewpoint of improving the bending resistance of the capacitor, for example, the organic component is an oligomer or a polymer. The oligomer or the polymer is, for example, a thermoplastic resin, a thermosetting resin, etc. For example, an acrylic resin, an epoxy resin, a novolac, a phenolic resin, a polyimide precursor resin, a polyimide resin, a polysiloxane resin, a fluorine-based resin, a polyvinyl acetal resin, etc.
[0156] The solvent may be any solvent that disperses the dielectric particles and dissolves the organic components. For example, ketone-based solvents such as methyl ethyl ketone, acetone, diethyl ketone, methyl isobutyl ketone, methyl isopropyl ketone, cyclopentanone, and cyclohexanone; alcohol-based solvents such as methanol, ethanol, isopropanol, isobutyl alcohol, benzyl alcohol, methoxymethylbutanol, ethylene glycol, diethylene glycol, and glycerin; ether-based solvents such as diethyl ether, diisopropyl ether, 1,2-dimethoxyethane, 1,4-dioxane, tetrahydrofuran, tetrahydropyran, anisole, diethylene glycol dimethyl ether (diglyme), and diethylene glycol ethyl ether (carbitol); cellosolve-based solvents such as methyl cellosolve, ethyl cellosolve, and phenyl cellosolve; and aliphatic hydrocarbons such as hexane, pentane, heptane, and cyclohexane. aromatic hydrocarbon solvents such as toluene, xylene, and benzene; aromatic heterocyclic compound solvents such as pyridine, pyrazine, furan, pyrrole, thiophene, and N-methylpyrrolidone; amide solvents such as N,N-dimethylformamide and N,N-dimethylacetamide; halogen compound solvents such as trichloroethylene, dichloromethane, chloroform, 1,2-dichloroethane, and chlorobenzene; ester solvents such as ethyl acetate, methyl acetate, ethyl formate, ethyl lactate, dimethyl carbonate, diethyl carbonate, propylene carbonate, and γ-butyrolactone; sulfur compound solvents such as dimethyl sulfoxide and sulfolane; nitrile solvents such as acetonitrile, propionitrile, and acrylonitrile; and organic acid solvents such as formic acid, acetic acid, trichloroacetic acid, and trifluoroacetic acid, or mixed solvents containing them.
[0157] Examples of the coating method include spin coating, blade coating, slit die coating, screen printing, bar coater, mold method, gravure printing, flexographic printing, offset printing, dip printing, inkjet method, dispenser method, etc. Among these coating methods, from the viewpoints of pattern processability and film removal property, for example, screen printing, gravure printing, flexographic printing, offset printing, inkjet method, and dispenser method are used.
[0158] The method for removing the solvent from the coating film includes, for example, heat drying using an oven, a hot plate, infrared rays, or vacuum drying, and is carried out at a temperature in the range of, for example, 50° C. to 140° C. for one minute to several hours.
[0159] Next, the coating film is cured to improve the dielectric properties. The curing temperature is selected depending on the type of dielectric compound, the solvent used, and the type of substrate. For example, when the organic component in the dielectric paste is an acrylic resin, the curing temperature is in the range of 50°C to 300°C from the viewpoint of heat resistance. Also, when the insulating substrate is polyethylene terephthalate, the curing temperature is preferably in the range of 50°C to 150°C from the viewpoint of preventing a decrease in processing precision due to thermal expansion of the substrate. Examples of the curing method include heat curing or vacuum curing using an oven, an inert oven, a hot plate, or infrared rays, curing using a xenon flash lamp, and photocuring using UV light.
[0160] In order to improve the flatness of the dielectric layer, a flattening layer can be formed on the coating film obtained by coating and drying a dielectric paste. The material of the flattening layer is, for example, a known resin such as polyimide resin, polysiloxane resin, acrylic resin, or epoxy resin. The thickness of the flattening layer is, for example, thinner than that of the dielectric layer in terms of dielectric properties.
[0161] The dielectric layer may be patterned or unpatterned. It may be patterned from the viewpoint of preventing misreading by reducing crosstalk between dielectric elements. For example, in terms of microfabrication, photolithography is used as the patterning method, in which the organic component includes a photosensitive organic component. By using the photolithography, high integration of the dielectric elements is possible.
[0162] Another thin film electrode layer is then deposited over dielectric layer 12 to provide capacitor 20.
[0163] The method for disposing the other thin-film electrode layers is the same as the method for disposing the first thin-film electrode 11 or the second thin-film electrode 13.
[0164] First, when the first thin-film electrode 11 is arranged, the second thin-film electrode 13 is arranged on the dielectric layer 12, and when the second thin-film electrode 13 is arranged, the first thin-film electrode 11 is arranged on the dielectric layer 12.
[0165] The second thin-film electrode 13 or the first thin-film electrode 11 is disposed on the dielectric layer 12, thereby preparing the capacitor 20.
[0166] 8 illustrates a memory device 1200 including a layer structure according to an example embodiment. The memory device 1200 may be, for example, a non-volatile ferroelectric memory device (e.g., FRAM (ferroelectric random access memory)).
[0167] 8, the memory device 1200 may include a substrate 1210, a first doping region 1220 and a second doping region 1230 formed in the substrate 1210, a gate stack 1240, a conductive plug 1260, a data storage element 1270, and an interlayer insulating film 1250. The substrate 1210 may include a semiconductor substrate. The first doping region 1220 and the second doping region 1230 are separated from each other. The first doping region 1220 and the second doping region 1230 may be formed by doping a predetermined region of the substrate 1210 with P-type conductive impurities or N-type conductive impurities. For example, when the substrate 1210 is a P-type semiconductor substrate, the first doping region 1220 and the second doping region 1230 may be regions doped with N-type conductive impurities. One of the first doping region 1220 and the second doping region 1230 is a source region, and the other is a drain region.
[0168] A gate stack 1240 is formed on the substrate 1210 between the first doping region 1220 and the second doping region 1230. The gate stack 1240 also includes a gate insulating layer and a gate electrode, which are stacked in sequence. The gate stack 1240, the first doping region 1220, and the second doping region 1230 may form a transistor.
[0169] The interlayer insulating film 1250 is formed to cover the transistor. The upper surface of the interlayer insulating film 1250 is also flat. As an example, the interlayer insulating film 1250 may include, but is not limited to, a silicon oxide film. A via hole H1 is formed in the interlayer insulating film 1250 to expose the second doping region 1230. The via hole H1 may be located on the second doping region 1230. The conductive plug 1260 is also included in the via hole H1. For example, the via hole H1 may be completely filled with the conductive plug 1260. One surface (e.g., a bottom surface) of the conductive plug 1260 is in direct contact with the second doping region 1230.
[0170] A capacitor 20, which is a data storage element, may be provided on the interlayer insulating film 1250 to cover the via hole H1 and the conductive plug 1260. The capacitor 20 may be in direct contact with the conductive plug 1260. The data storage element may also include a lower electrode 11, a dielectric layer 12, and an upper electrode 13. The capacitor 20 including the lower electrode 11, the dielectric layer 12, and the upper electrode 13, which are sequentially stacked, may also be the capacitor 20, the first thin film electrode 11, the dielectric layer 12, and the second thin film electrode 13 of FIGS. 5A to 5D, respectively. In an example embodiment, the gate insulating film may also include the dielectric layer 12.
[0171] However, memory device 1200 is not so limited. For example, in some embodiments, capacitor 20 may be directly coupled to a transistor and / or capacitor 20 and transistor may share a doped region (e.g., second doped region 1230).
[0172] 9, a semiconductor device D10 may have a structure in which a plurality of capacitors 20 and a plurality of field effect transistors are repeatedly arranged.
[0173] 9, the semiconductor device D10 includes a field effect transistor including a gate stack 1240 and a substrate 1210 having a source, a drain, and a channel; a contact structure 1230 arranged on the substrate 1210 without overlapping with the gate stack 1240; and a capacitor 20 arranged on the contact structure 1230. The semiconductor device D10 further includes a bit line structure 930 that electrically connects the field effect transistors to each other. Although FIG. 9 illustrates the semiconductor device D10 in which the contact structures 1230 and the capacitors 20 are repeatedly arranged in the X and Y directions, this is a non-limiting example. For example, the contact structures 1230 are also arranged in the X and Y directions, and the capacitors 20 are also arranged in a hexagonal shape such as a honeycomb structure.
[0174] 10 and 11 are conceptual diagrams that generally illustrate electronic device architectures that can be applied to electronic devices according to embodiments of the present invention.
[0175] Referring to FIG. 10, the electronic device architecture 3000 also includes a memory unit 3010, an arithmetic logic unit (ALU) 3020, and a control unit 3030. The memory unit 3010, the ALU 3020, and the control unit 3030 may be electrically coupled to each other. For example, the electronic device architecture 3000 may be embodied by a single chip including the memory unit 3010, the ALU 3020, and / or the control unit 3030. For example, the memory unit 3010, the ALU 3020, and the control unit 3030 may be coupled to each other via metal lines on the chip and communicate directly. The memory unit 3010, the ALU 3020, and / or the control unit 3030 may be monolithically integrated on a single substrate to form a single chip. The input / output device 2000 is also coupled to the electronic device architecture (chip) 3000. The control unit 3030 may be a processing circuit such as hardware including logic circuits; a hardware / software combination such as a processor executing software; or a combination thereof. For example, the processing circuit may more specifically include a central processing unit (CPU), an arithmetic logic unit (ALU), a digital signal processor, a microcomputer, a field programmable gate array (FPGA), a programmable logic unit, a microprocessor, an application specific integrated circuit (ASIC), etc. Similarly, although the electronic device architecture 3000 is illustrated as including an ALU 3020, the electronic device architecture 3000 is not limited thereto and may include additional and / or alternative processing circuits. The memory unit 3010 may include a main memory and a cache memory. The electronic device architecture (chip) 3000 may be an on-chip memory processing device. The memory unit 3010, the ALU 3020, and / or the control unit 3030 may each independently include the layer structure described above.
[0176] Referring to FIG. 11, the cache memory 1510, the ALU 1520, and the control unit 1530 constitute the CPU 1500, and the cache memory 1510 also includes SRAM (static random access memory). The main memory 1600 and the auxiliary storage device 1700 are provided separately from the CPU 1500. The main memory 1600 also includes DRAM (dynamic random access memory) having the layer structure as described above. The input / output device 2500 can also be connected to the CPU 1500.
[0177] In some cases, the electronic device architecture is also embodied in a form in which a single-chip unit computer device and a unit memory device are adjacent to each other without sub-units.
[0178] The present invention will be described in more detail through the following examples and comparative examples. However, these examples are for illustrative purposes only, and the scope of the present invention is not limited thereto.
[0179] (Manufacture of Dielectric) Example 1: [GaO 2 ] - First anionization layer: 1 unit cell SrRuO with a thickness of 100 Å 3 On the (001) plane of the first thin film electrode, using a molecular beam epitaxial process, in the
[0001] direction, [GaO2] - The first anionized layer and the [SrO] second neutral layer were sequentially grown to form an intermediate layer.
[0180] The intermediate layer is represented as SrGaO as a compound x (2.5 < x ≤ 3.0). The thickness of the intermediate layer including one unit cell was 4.0 Å. The molecular beam epitaxial process was carried out at an oxygen partial pressure of 5×10 -8 to 8×10 -8 Torr, and the temperature of the first thin film electrode was 700°C.
[0181] SrGaO x On the intermediate layer, SrTiO 3 The dielectric layer was grown to a thickness of 100 Å.
[0182] SrTiO 3 On the dielectric layer, a 200 Å thick SrRuO 3 A second thin-film electrode was then disposed to complete the capacitor.
[0183] Example 2: [InO 2 ] - First anionization layer: 1 unit cell [GaO 2 ] - Instead of the anionization layer, [InO 2 ] - A capacitor was manufactured in the same manner as in Example 1, except that the anionization layer was formed.
[0184] Example 3: [BeO 2 ] 2- First anionization layer: 1 unit cell [GaO 2 ] - Instead of the anionized layer, [BeO 2 ] 2- A capacitor was manufactured in the same manner as in Example 1, except that the anionization layer was formed.
[0185] Example 4: [MgO 2 ] 2- First anionization layer: 1 unit cell [GaO 2 ] - Instead of the anionized layer, [MgO 2 ] 2- A capacitor was manufactured in the same manner as in Example 1, except that the anionization layer was formed.
[0186] Example 5: [LiO 2 ] 3- First anionization layer: 1 unit cell [GaO 2 - Instead of the anionized layer, a capacitor was manufactured in the same manner as in Example 1, except that an [LiO 2 3- anionized layer was formed.
[0187] Example 6: [LiO] - Second anionization layer: 1 unit cell On the (001) plane of the first thin film electrode with a thickness of 100 Å, using a molecular beam epitaxial process, in the
[0001] direction, [LiO] 3 a second anionized layer and [TiO - a third neutral layer were sequentially grown to form an intermediate layer. 2 The intermediate layer is represented as a compound by LiTiO
[0188] (2.5 < x ≤ 3.0). The thickness of the intermediate layer containing 1 unit cell was 4.0 Å. The molecular beam epitaxial process was carried out at an oxygen partial pressure of 5×10 x to 8×10 -8 Torr, and the temperature of the first thin film electrode was 700°C. -8 On the LiTiO
[0189] intermediate layer, a SrTiO x dielectric layer was grown to a thickness of 100 Å in the same manner. 3 On the SrTiO
[0190] dielectric layer, a second thin film electrode with a thickness of 100 Å of SrRuO 3 was disposed in the same manner to manufacture a capacitor. 3
[0191] Example 7: [NaO] Second anionization layer: 1 unit cell - [LiO] - Instead of the anionized layer, a capacitor was manufactured in the same manner as in Example 6, except that a [NaO - anionized layer was formed.
[0192] Example 8: [KO] - Second anionization layer: 1 unit cell [LiO] - Instead of the anionized layer, [KO] - A capacitor was manufactured in the same manner as in Example 6, except that an anionization layer was formed.
[0193] Example 9: [RbO] - Second anionization layer: 1 unit cell [LiO] - Instead of the anionized layer, [RbO] - A capacitor was manufactured in the same manner as in Example 6, except that an anionization layer was formed.
[0194] Example 10: [ScO] + The first positive ionization layer and [GaO 2 ] - Third anionization layer: 1 unit cell 100 Å thick SrRuO 3 On the (001) surface of the first thin-film electrode, a molecular beam epitaxy process was used to grow [ScO] + The first positive ionization layer and [GaO 2 ] - A third anionization layer was then grown in sequence to form the intermediate layer.
[0195] The intermediate layer is a perovskite compound, ScGaO 3 The thickness of the intermediate layer containing one unit cell was 4.0 Å. The molecular beam epitaxial process was performed at 5×10 -8 Or 8 x 10 -8 The treatment was performed at an oxygen partial pressure of 10 Torr and the temperature of the first thin film electrode was 700°C.
[0196] ScGaO 3 On the intermediate layer, SrTiO 3 The dielectric layer was grown to a thickness of 100 Å.
[0197] SrTiO 3On the dielectric layer, a 100 Å thick SrRuO 3 A second thin-film electrode was then disposed to complete the capacitor.
[0198] Example 11: [LaO] + The first cation layer and [AlO 2 ] - Third anionization layer: 1 unit cell 100 Å thick SrRuO 3 On the (001) surface of the first thin-film electrode, [LaO] was grown in the
[0001] direction using a molecular beam epitaxial process. + The first cation layer and [AlO 2 ] - Anionized layers were grown in sequence to form the intermediate layer.
[0199] The intermediate layer is a perovskite compound, LaAlO 3 The thickness of the intermediate layer containing one unit cell was 4.0 Å. The molecular beam epitaxial process was performed at 5×10 -8 Or 8 x 10 -8 The treatment was carried out at an oxygen partial pressure of 10 Torr and the electrode temperature was 700°C.
[0200] LaAlO 3 On the intermediate layer, SrTiO 3 The dielectric layer was grown to a thickness of 100 Å. SrTiO 3 On the dielectric layer, a 100 Å thick SrRuO 3 A second thin-film electrode was then disposed to complete the capacitor.
[0201] Example 12: [GaO 2 ] - First anionization layer: 2 unit cells SrGaO x A capacitor was manufactured in the same manner as in Example 1, except that the thickness of the intermediate layer was changed to two unit cells.
[0202] Comparative example 1: [LaO] + First cation layer: 1 unit cell SrRuO with a thickness of 100 Å 3 On the (001) plane of the first thin-film electrode, using the molecular beam epitaxial process, in the
[0001] direction, [LaO] + The first cationic layer and [TiO 2 The third neutral layer were sequentially grown to form an intermediate layer.
[0203] The intermediate layer is a compound and is represented by LaTiO x (2.5 < x ≤ 3.0). The thickness of the intermediate layer containing 1 unit cell was 4.0 Å. The molecular beam epitaxial process was carried out at an oxygen partial pressure of 5×10 -8 to 8×10 -8 Torr, and the temperature of the first thin-film electrode was 700 °C.
[0204] LaTiO x On the intermediate layer, in the same manner, SrTiO 3 The dielectric layer was grown to a thickness of 100 Å.
[0205] SrTiO 3 On the dielectric layer, in the same manner, SrRuO with a thickness of 100 Å 3 The second thin-film electrode was arranged to manufacture a capacitor.
[0206] Comparative Example 2: [YO] + First cation layer: 1 unit cell [LaO] + Instead of the cationic layer, a capacitor was manufactured in the same manner as Comparative Example 1, except that [YO] + the cationic layer was formed.
[0207] Comparative Example 3: [YO] + First cation layer: 2 unit cells A capacitor was manufactured in the same manner as Comparative Example 2, except that the thickness of the intermediate layer was increased to 2 unit cells.
[0208] Comparative Example 4: Intermediate layer free: 1 unit cell A capacitor was manufactured in the same manner as in Example 1, except that the step of providing the intermediate layer was omitted.
[0209] Evaluation example 1: Schottky barrier height (SBH) calculation: first anionization layer SrRuO 3 (electrode) / SrTiO 3 In contrast to the (dielectric) laminate, SrRuO 3 / SrTiO 3 The amount of change (ΔV) in the Schottky barrier height (SBH) of the laminate in which the first anionization layer was disposed as an intermediate layer between the first anionization layer and the second anionization layer was calculated, and some of the results are shown in Table 1 below.
[0210] Referring to FIG. 1A and FIG. 1B, SrRuO 3 / SrTiO 3 A first anionization layer is disposed between the first and second anionization layers as an intermediate layer. The metal cations contained in the intermediate layer are located at octahedral sites in the perovskite structure where six oxygen atoms are coordinated. 3 In this case, it corresponds to B.
[0211] The dielectric constants and band gaps were calculated in the density functional theory (DFT) framework using the Vienna Ab initio Simulation Package (VASP).
[0212] The Schottky barrier height of the laminate in which the intermediate layer is disposed is expressed by the following formula 1. The Goldschmidt tolerance factor (t) is a parameter indicating the stability of the cubic perovskite structure. The closer to 1, the higher the structural stability of the cubic perovskite, and is expressed by the following formula 2.
[0213] [Formula 1] SBH=Φ-χ+ΔV
[0214] In Equation 1, Φ is the work function of the electrode, χ is the electron affinity of the dielectric, and ΔV is the amount of change in SBH.
[0215]
number
[0216] In formula 2, r A is the ionic radius of the A ion, and r B is the ionic radius of the B ion, and r O is the ionic radius of oxygen and t is the Goldschmidt tolerance factor.
[0217] [Table 1]
[0218] As can be seen from Table 1, it was confirmed that the Schottky barrier height of the stack including the intermediate layer having a cubic perovskite structure with a stable tolerance factor in the range of 0.9 to 1.10 was increased by disposing the first anionization layer as an intermediate layer between the electrode and the dielectric layer.
[0219] Such an increase in Schottky barrier height is believed to be due to the first anionization layer inducing shielding charges of opposite polarity on the corresponding electrode side, thereby inducing an additional electrostatic potential difference between the electrode and the dielectric layer.
[0220] Therefore, it has been confirmed that the first anionization layer disposed as an intermediate layer between the electrode and the dielectric layer is suitable as a leakage current blocking layer for a capacitor.
[0221] Evaluation example 2: Schottky barrier height (SBH) calculation: second negative ionization layer SrRuO 3 (electrode) / SrTiO 3 In contrast to the (dielectric) laminate, SrRuO 3 / SrTiO 3 The amount of change (ΔV) in the Schottky barrier height (SBH) of the laminate in which a second anionization layer was disposed as an intermediate layer between the first and second anionization layers was calculated, and some of the results are shown in Table 2 below.
[0222] Referring to FIG. 2A and FIG. 2B, SrRuO 3 / SrTiO 3 A second anionization layer is disposed between the first and second anionization layers as an intermediate layer. The metal cations contained in the intermediate layer are located at cuboctahedral sites in the perovskite structure where 12 oxygen atoms are coordinated. 3 In this case, it corresponds to A. The dielectric constant and band gap were calculated on the basis of density functional theory (DFT) using the Vienna Ab initio Simulation Package (VASP).
[0223] The Schottky barrier height of the laminate in which the intermediate layer is disposed is expressed by the following formula 1. The tolerance factor (t: Goldschmidt tolerance factor) is a parameter indicating the stability of the cubic perovskite structure. The closer to 1, the higher the structural stability of the cubic perovskite, and is expressed by the following formula 2.
[0224] [Formula 1] SBH=Φ-χ+ΔV
[0225] In Equation 1, Φ is the work function of the electrode, χ is the electron affinity of the dielectric, and ΔV is the amount of change in SBH.
[0226]
number
[0227] In formula 2, r A is the ionic radius of the A ion, and r B is the ionic radius of the B ion, and r O is the ionic radius of oxygen and t is the Goldschmidt tolerance factor.
[0228] [Table 2]
[0229] As can be seen from Table 2, by disposing the second anionization layer between the electrode and the dielectric layer as an intermediate layer to which monovalent cations are applied, it was confirmed that the Schottky barrier height of the stack was almost increased and the cubic perovskite structure was stabilized with a tolerance factor close to 1.
[0230] Therefore, it has been confirmed that the second anionizable layer disposed as an intermediate layer between the electrode and the dielectric layer is suitable as a leakage current blocking layer for the capacitor.
[0231] In contrast, when a cationic layer was disposed as an intermediate layer between the electrode and the dielectric layer, the Schottky barrier height of the stack was rather reduced.
[0232] Evaluation example 3: Schottky barrier height (SBH) calculation: first neutral layer SrRuO 3 (electrode) / SrTiO 3 In contrast to the (dielectric) laminate, SrRuO 3 / SrTiO 3 The amount of change (ΔV) in the Schottky barrier height (SBH) of the stack in which the first neutral layer was disposed as an intermediate layer between the first and second neutral layers was calculated, and some of the results are shown in Table 3 below.
[0233] Referring to FIG. 3A and FIG. 3B, SrRuO 3 / SrTiO 3 A first neutral layer is disposed between the first and second layers as an intermediate layer. 3 It is a perovskite compound having the following composition.
[0234] The dielectric constants and band gaps were calculated on the basis of density functional theory (DFT) using the Vienna Ab initio Simulation Package (VASP).
[0235] The Schottky barrier height of the stack including the intermediate layer is expressed by the following formula 1. [Formula 1] SBH=Φ-χ+ΔV
[0236] In Equation 1, Φ is the work function of the electrode, χ is the electron affinity of the dielectric, and ΔV is the amount of change in SBH.
[0237] [Table 3]
[0238] As can be seen from Table 3, the Schottky barrier height of the stack was increased by providing the first neutral layer as an intermediate layer between the electrode and the dielectric layer.
[0239] Therefore, it was confirmed that the first neutral layer disposed as an intermediate layer between the electrode and the dielectric layer is suitable as a leakage current blocking layer for a capacitor.
[0240] Evaluation example 4: Schottky barrier height (SBH) calculation: thickness change SrRuO 3 (electrode) / SrTiO 3 In contrast to the (dielectric) laminate, SrRuO 3 / SrTiO 3 In a laminate in which a first anionization layer or a cationization layer is disposed as an intermediate layer between the first anionization layer and the second anionization layer, the change in Schottky barrier height (SBH) (ΔV) due to the thickness of the intermediate layer was calculated, and some of the results are shown in Table 4 below. 3 / SrTiO 3 A first anionization layer is disposed between the first and second anionization layers as an intermediate layer, the intermediate layer having a thickness of 1 unit cell and 2 unit cells.
[0241] The dielectric constants and band gaps were calculated on the basis of density functional theory (DFT) using the Vienna Ab initio Simulation Package (VASP).
[0242] The Schottky barrier height of the laminate including the intermediate layer is expressed by the following formula 1.
[0243] [Formula 1] SBH=Φ-χ+ΔV
[0244] In Equation 1, Φ is the work function of the electrode, χ is the electron affinity of the dielectric, and ΔV is the amount of change in SBH.
[0245] [Table 4]
[0246] As can be seen from Table 4, in the stack in which the first anionization layer was disposed as the intermediate layer, the Schottky barrier height of the stack increased as the thickness of the intermediate layer increased.
[0247] Therefore, it was confirmed that by increasing the thickness of the first anionization layer disposed in the intermediate layer disposed between the electrode and the dielectric layer, the intermediate layer is suitable as a leakage current blocking layer for the capacitor.
[0248] In contrast, in a stack in which a cationization layer was disposed as an intermediate layer, the Schottky barrier height of the stack decreased as the thickness of the intermediate layer increased.
[0249] Evaluation example 5: Leakage current measurement The leakage current of the capacitors produced in Example 1, Example 12, Comparative Example 1 and Comparative Example 4 was measured.
[0250] The leakage current is the current density when a voltage of 1 V is applied to the capacitor. The measurement results are shown in Table 5 below.
[0251] [Table 5]
[0252] As can be seen from Table 5, the capacitors of the examples including an intermediate layer had reduced leakage current compared to the capacitor of Comparative Example 4 that did not include an intermediate layer and the capacitor of Comparative Example 1 that included only a cationic intermediate layer.
[0253] Therefore, it was confirmed that the capacitor including the intermediate layer is suitable for manufacturing a capacitor including a dielectric layer having a high dielectric constant. [Explanation of symbols]
[0254] 11 First electrode, first thin film electrode 12 Dielectric layer 13 Second electrode, second thin film electrode 20 Capacitor 100 Insulating substrate 201 Semiconductor substrate 203 Interlayer insulating film 205 Contact plug 207 Lower mold insulating film 209 Etching stop film 211 Upper mold insulating film 213 Mold insulating film 215 Storage Node Hall 217' Lower electrode film, conductive film for lower electrode 219 Buffer insulating film, lower dielectric film 221 Intermediate Dielectric Film 223 Upper dielectric film 224 Dielectric Film 225 Upper electrode 320 p-type semiconductor substrate 321 Field oxide film 322 Source Region 322' Drain region 323 Gate electrode 324 Interlayer insulating film 325 Sidewall oxide film 326 Storage Electrode 327 Insulating Film 328 Plate Electrode 332 PN junction 930 Bit Line Structure 1200 Memory Device 1210 Board 1220 First doping region 1230 Second doping region 1240 Gate Stack 1250 Interlayer insulating film 1500 CPU 1510 Cache Memory 1520 ALU 1530 Control Unit 1600 Main memory 1700 Auxiliary Storage Device 2000 I / O devices 2500 I / O device 3000 Electronic Device Architecture 3010 Memory Unit 3020 ALU 3030 Control Unit
Claims
1. a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed between the first thin-film electrode layer and a dielectric layer and / or between the second thin-film electrode layer and the dielectric layer; the intermediate layer has a crystal structure of the same form as one or more of the electrode layer and the dielectric layer in contact with the intermediate layer, and has a composition different from each other; the intermediate layer comprises a first neutral layer; the first neutral layer comprises a plurality of trivalent cations; A capacitor, wherein a Schottky barrier height (SBH) between the first thin-film electrode layer or the second thin-film electrode layer and the dielectric layer is 1.5 eV or more.
2. 2. The capacitor of claim 1, wherein the first neutral layer comprises a metal oxide having a perovskite crystal structure represented by the following chemical formula 3: [Chemical formula 3] <h2 style=";text-align:left;direction:ltr">[A3B3O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ] In the above Chemical Formula 3, A3 is a trivalent cation, B3 is a trivalent cation.
3. The intermediate layer is [ScAlO] 3 ][YLLO 3 ][LaAlO] 3 ][CeeAllO 3 ][PrrAllO 3 ][N$AlO 3 ][SmAlO 3 ][D]AlO 3 ]、 [ScGaO 3 ]、[YG 3 ]、[LaGaO 3 ]、[CeGaO 3 ]、[PrGaO 3 ]、[NdGaO 3 ]、[SmGaO 3 ]、[DyGaO 3 ]、 [ScInO 3 ], [YInO 3 ], [LaInO 3 ], [CeInO 3 ], [PrInO 3 ], [NdInO 3 ], [SmInO 3 ] or [DyInO 3 2. The capacitor of claim 1, comprising a metal oxide selected from the group consisting of:
4. The first neutral layer is [A3O] + A first cationization layer represented by [B3O 2 ] - and a third anionization layer represented by 2. The capacitor of claim 1, wherein A3 is a trivalent cation and B3 is a trivalent cation, and A3 and B3 are different metals.
5. A3 is Sc, Y, La, Ce, Pr, Nd, Sm or Dy; The capacitor of claim 4 , wherein B3 is Al, Ga or In.
6. The intermediate layer is [ScO] + , [YO] + [LaO] + [CeO] + , [PrO] + [NdO] + [SmO] + Or [DyO] + A first cationization layer represented by [AlO 2 ] - , [GaO 2 ] - or [InO 2 ] - and a third anionization layer represented by:
7. the intermediate layer comprises 1 unit cell to 3 unit cells, and the thickness of the intermediate layer is 1 Å to 15 Å; The capacitor of claim 1 , wherein the intermediate layer is formed by epitaxial growth.
8. 2. The capacitor of claim 1, wherein the dielectric layer comprises a dielectric material having a perovskite crystal structure represented by the following chemical formula 4: [Chemical formula 4] A4B4O 3 In the above Chemical Formula 4, A4 is a monovalent, divalent or trivalent cation; B4 is a trivalent cation, a tetravalent cation, or a pentavalent cation.
9. The dielectric layer is SrTiO 3 , CaTiO 3 , BaTiO 3 , SrHfO 3 , CaHfO 3 , BaHfO 3 , SrZrO 3 , CaZrO 3 , BaZrO 3 , PbTiO 3 , NaNbO 3 , NaTaO 3 , RbTaO 3 , RbNbO 3 , RbTaO 3 or EuTiO 3 10. The capacitor of claim 1, comprising a dielectric selected from the group consisting of:
10. The thickness of the dielectric layer is 10 nm to 100 nm, The first thin-film electrode layer and the second thin-film electrode layer each have a thickness of 10 nm to 1,000 nm; The capacitor of claim 1 , wherein at least one of the first thin-film electrode layer and the second thin-film electrode layer has a perovskite crystal structure.
11. 11. An electronic device comprising a capacitor according to any one of claims 1 to 10.
12. The electronic device of claim 11 , wherein the electronic device is a semiconductor device.
13. providing a first thin-film electrode layer or a second thin-film electrode layer; disposing an intermediate layer on one surface of the first thin-film electrode layer or the second thin-film electrode layer by epitaxial growth; disposing a dielectric layer on the intermediate layer; and depositing another thin film electrode layer on the dielectric layer to provide a capacitor. the capacitor comprises: a first thin-film electrode layer; a second thin-film electrode layer; a dielectric layer disposed between the first thin-film electrode layer and the second thin-film electrode layer; and an intermediate layer disposed between the first thin-film electrode layer and a dielectric layer and / or between the second thin-film electrode layer and the dielectric layer; the intermediate layer has a crystal structure of the same form as one or more of the electrode layer and the dielectric layer in contact with the intermediate layer, and has a composition different from each other; the intermediate layer comprises a first neutral layer; the first neutral layer comprises a plurality of trivalent cations; the dielectric layer comprises a ternary oxide having a perovskite crystal structure; A method for manufacturing a capacitor, wherein a Schottky barrier height (SBH) between the first thin-film electrode layer or the second thin-film electrode layer and the dielectric layer is 1.5 eV or more.
Citation Information
Patent Citations
Thin film capacitor and semiconductor memory
JP1996139292A
Dielectric laminating thin film and electronic parts using the same
JP2003045987A
Method for evaluating characteristics of electronic component
JP2012032160A
MIM capacitor and method for fabricating the same
KR1020080084434A
Ferroelectric type semiconductor device having a barium titanate type dielectric film and method for manufacturing the same
US5739563A