Electrolyte and lithium-ion secondary battery
A compound-stabilized electrolytic solution addresses the instability of lithium-ion battery electrolytes at high voltages, ensuring stable performance and capacity retention in nickel-manganese-cobalt ternary systems.
Patent Information
- Application Number
- JP2023076482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-20
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electrolytes for lithium-ion secondary batteries are unstable at high voltages above 3.7V, particularly in next-generation batteries using nickel-manganese-cobalt ternary mixed systems, leading to decomposition and performance degradation.
An electrolytic solution containing a specific compound, a solvent, and a lithium salt, which includes substituents such as BIAN-thiophene, is used to stabilize the electrolyte at high voltages.
The electrolytic solution maintains stability and suppresses electrode degradation and discharge capacity loss, enabling stable operation of lithium-ion secondary batteries at high voltages (4.5V to 5.0V).
Smart Images

Figure 2024161655000008 
Figure 2024161655000009 
Figure 2024161655000010
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte solution and a lithium ion secondary battery. [Background technology]
[0002] High-power, high-capacity secondary batteries are widely used in portable devices such as electric vehicles, mobile phones, personal computers, and PDAs (Personal Digital Assistants), or as backup power sources.
[0003] As such a secondary battery, Patent Document 1 discloses a lithium secondary battery including a non-aqueous electrolyte solution containing a carbonate ester. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-6786 Summary of the Invention [Problem to be solved by the invention]
[0005] Nickel-manganese-cobalt ternary mixed metal oxide materials are being researched as electrolytes for lithium-ion secondary batteries that provide high voltage and high energy density. The LiCoO2 system currently used as the positive electrode material for commercial lithium-ion secondary batteries outputs a voltage of about 3.7 V, which is below the decomposition voltage of ethylene carbonate, a general-purpose electrolyte, and does not pose a major problem. However, it is thought that in the high-voltage system (4.5 V to 5.0 V) for next-generation batteries that utilizes the ternary mixed system, it will be difficult to use the electrolyte stably without some kind of ingenuity.
[0006] The present invention has been made to solve the above-mentioned problems, and has an object to provide an electrolyte and a lithium ion secondary battery that can be used stably even at high voltages. [Means for solving the problem]
[0007] In order to achieve the object of the present invention, one embodiment of the electrolyte according to the present invention is The composition is characterized by comprising a compound represented by formula (1), a solvent, and a lithium salt. [ka] R 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 31 , R 32 , R 33 , R 41 , R 42 and R 43 each independently represents a substituent.
[0008] In order to achieve the object of the present invention, one aspect of the lithium ion secondary battery according to the present invention is The electrolytic solution is contained. Effect of the Invention
[0009] According to the present invention, it is possible to provide an electrolyte solution and a lithium ion secondary battery that can be stably used even at high voltages. [Brief description of the drawings]
[0010] [Figure 1] FIG. 13 is a diagram showing the results of a long-term cycle test of the cathode half-cells according to the examples and the comparative examples. [Diagram 2] (A) is a scanning electron microscope (SEM) image of the LiNi1 / 3Mn1 / 3Co1 / 3O2 electrode before the cycle test, (B) is a SEM image of the LiNi1 / 3Mn1 / 3Co1 / 3O2 electrode after 100 cycles of the comparative example, and (C) is a SEM image of the LiNi1 / 3Mn1 / 3Co1 / 3O2 electrode after 100 cycles of the example. [Diagram 3]FIG. 2A is a diagram showing a rate test of the cathode half-cells according to the examples and the comparative example, and FIG. 2B is a diagram showing a cycle test of the cathode half-cells according to the examples and the comparative example. [Figure 4] FIG. 2A is a diagram showing the reductive decomposition of the electrolyte solutions of the Examples and Comparative Examples, and FIG. 2B is a diagram showing the oxidative decomposition of the electrolyte solutions of the Examples and Comparative Examples. [Diagram 5] FIG. 1 is a diagram showing a charge / discharge test of an example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an electrolyte solution and a lithium ion secondary battery according to an embodiment of the present invention will be described.
[0012] The lithium ion secondary battery according to the embodiment includes a positive electrode, a negative electrode, an electrolyte, and a separator.
[0013] (positive electrode) The positive electrode preferably includes a current collector and a positive electrode active material layer formed on the current collector. An example of the current collector is an aluminum substrate. The positive electrode active material layer preferably includes a positive electrode active material and a binder. The positive electrode active material layer may include a conductive assistant. The positive electrode active material is preferably a compound capable of reversibly inserting and extracting lithium ions.
[0014] As the positive electrode active material, from the viewpoint of the structural stability of the positive electrode active material, Layered oxide; LiNi x Co y Ma 1-x-y O2 (wherein Ma represents one or more selected from the group consisting of Mn and Al, 0≦x≦1, 0≦y≦1, and x+y≦1), Spinel-type oxide; LiMn 2-x Mb x O4 (wherein Mb represents one or more selected from the group consisting of transition metals, and 0.2≦x≦0.7), Li-excess layered oxide: a composite oxide of an oxide represented by Li2McO3 (wherein Mc each independently represents one or more selected from the group consisting of transition metals) and an oxide represented by LiMdO2 (wherein Md each independently represents one or more selected from the group consisting of transition metals), wherein zLi2McO3-(1-z)LiMdO2 (wherein Mc each independently represents one or more selected from the group consisting of transition metals, and Md each independently represents one or more selected from the group consisting of transition metals, and 0.05≦z≦0.95), Olivine-type oxide; LiMe 1-x Fe x PO4, wherein Me represents one or more selected from the group consisting of Mn and Co, and 0≦x≦1; An oxide; Li2MfPO4F (wherein Mf represents one or more selected from the group consisting of transition metals); It is preferable that the material is a mixture of one or more selected from the group consisting of: The positive electrode active material is LiNi x Co y Ma 1-x-y It is preferable that the compound contains O2 (wherein Ma represents one or more selected from the group consisting of Mn and Al, 0≦x≦1, 0≦y≦1, and x+y≦1).
[0015] The binder serves to facilitate adhesion of the positive electrode active material to one another or to the current collector, and examples of the binder include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, polyvinylidene fluoride, polytetrafluoroethylene, polyimide, and polyimide amide.
[0016] (Negative electrode) The negative electrode preferably includes a current collector and a negative electrode active material layer formed on the current collector. Examples of the current collector include copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations of two or more of these. Examples of the negative electrode active material include a material capable of reversibly inserting / desorbing lithium ions, metallic lithium, an alloy of metallic lithium, a material capable of doping and dedoping lithium, and a transition metal oxide.
[0017] Examples of the material capable of reversibly inserting / desorbing lithium ions include crystalline carbon, amorphous carbon, and combinations of these. Examples of crystalline carbon include amorphous graphite, plate-like graphite, flaky graphite, spherical graphite, and fibrous graphite. Examples of amorphous carbon include soft carbon, hard carbon, mesophase pitch carbide, and calcined coke. As the alloy of metallic lithium, for example, an alloy of lithium and a metal such as Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, or Sn can be used. Examples of the material capable of doping and dedoping lithium include Si, SiO x (0 < x < 2), Si-C composite, Si-Q alloy (Q is an alkali metal, alkaline earth metal, group 13 to 16 element, transition metal, rare earth element, or a combination thereof and is not Si), Sn, SnO2, Sn-C composite, Sn-R (R is an alkali metal, alkaline earth metal, group 13 to 16 element, transition metal, rare earth element, or a combination thereof and is not Sn).
[0018] The negative electrode active material layer may contain a binder. Examples of the binder include those exemplified for the binder contained in the positive electrode active material layer described above.
[0019] (Electrolyte) The electrolyte contains a compound, a solvent, and a lithium salt.
[0020] The compound is represented by formula (1): 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 31 , R 32 , R 33 , R 41 , R 42 and R 43 each independently represents a substituent.
[0021] [ka]
[0022] The type of the substituent is not particularly limited, and examples thereof include a hydrogen atom, a halogen atom, an alkyl group (including a cycloalkyl group), an alkenyl group (including a cycloalkenyl group and a bicycloalkenyl group), an alkynyl group, an aromatic group (for example, an aromatic hydrocarbon group, an aromatic heterocyclic group), a cyano group, a hydroxyl group, a nitro group, a carboxyl group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic oxy group, an acyloxy group, a carbamoyloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an amino group (including an anilino group), an acylamino group, an aminocarbonylamino group, an alkoxy group, an aryloxycarbonyl ... Examples of such groups include dicarbonylamino groups, aryloxycarbonylamino groups, sulfamoylamino groups, alkyl and arylsulfonylamino groups, mercapto groups, alkylthio groups, arylthio groups, heterocyclic thio groups, sulfamoyl groups, sulfo groups, alkyl and arylsulfinyl groups, alkyl and arylsulfonyl groups, acyl groups, aryloxycarbonyl groups, alkoxycarbonyl groups, carbamoyl groups, aryl and heterocyclic azo groups, imido groups, phosphino groups, phosphinyl groups, phosphinyloxy groups, phosphinylamino groups, silyl groups, and combinations thereof.
[0023] Among the above-mentioned substituents, the substituents include an isocyanate group (N=C=O), a silyloxy group (Si-O), and a phosphonate group (P(OR)), which capture the HF generated by the decomposition of LiPF6. 51 )2R 52 ) is preferred. 51 , R 52 is an organic group. In addition, a substituent containing boron, sulfur, phosphorus, or fluorine is preferable for forming a coating that protects the electrode from corrosion by HF. In addition, the content of the compound in the electrolyte is not particularly limited, but the content of the compound in the electrolyte is preferably more than 0 mg / ml, more preferably 0.5 mg / ml or more. This allows the effect of the compound to be obtained. In addition, the content of the compound in the electrolyte is preferably 6.0 mg / ml or less, more preferably 3.0 mg / ml or less, and even more preferably 1.5 mg / ml or less. This allows the decrease in charge / discharge capacity to be suppressed.
[0024] The method for synthesizing the compound is not particularly limited. For example, the compound can be synthesized by dissolving acenaphthenequinone and 2 equimolar amounts of methyl 2-aminothiophene in acetonitrile in the presence of an acid catalyst and stirring overnight under reflux in a nitrogen atmosphere.
[0025] The type of the solvent is not particularly limited, and examples of the solvent include non-aqueous solvents, such as carbonate-based solvents, ester-based solvents, ether-based solvents, ketone-based solvents, alcohol-based solvents, and aprotic solvents.
[0026] Examples of carbonate solvents include cyclic carbonate solvents and chain carbonate solvents, such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, and butylene carbonate.
[0027] Examples of ester-based solvents include methyl acetate, ethyl acetate, n-propyl acetate, 1,1-dimethylethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, and caprolactone.
[0028] Examples of ether solvents include dibutyl ether, tetraglyme, triglyme, dibutyl ether, Glyme, dimethoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran Examples include:
[0029] An example of the ketone solvent is cyclohexanone.
[0030] Examples of alcohol-based solvents include ethyl alcohol and isopropyl alcohol.
[0031] Aprotic solvents include nitriles, amides such as dimethylformamide, 1, These include dioxolanes, such as 3-dioxolane, and sulfolanes.
[0032] The solvent preferably contains ethylene carbonate and diethyl carbonate. The content of the solvent in the electrolytic solution is not particularly limited, but is preferably 50 to 99 mass % and more preferably 85 to 98 mass % based on the total mass of the electrolytic solution in terms of superior effect.
[0033] The type of lithium salt is not particularly limited, and may be LiPF6, LiBF4, LiClO4, LiAsF6, LiC(CF3SO2)3, Li2SiF6, LiiOSO2C k F2 k+1 (k is an integer from 1 to 8), LiN(SO2C k F 2k+1 )2 [k is an integer from 1 to 8], LiPF n (C k F 2k+1 ) 6-n[n is an integer of 1 to 5, and k is an integer of 1 to 8], LiPF4(C2O2), and LiPF2(C2O2)2.
[0034] The content of the lithium salt in the electrolytic solution is not particularly limited, but in terms of obtaining a superior effect, it is preferably 0.2 to 3.0 mol / L, and more preferably 0.4 to 2.0 mol / L.
[0035] The electrolyte may contain components other than the above-mentioned compound, solvent, and lithium salt.
[0036] The method for preparing the electrolyte solution is not particularly limited as long as it is a method that can mix the above-mentioned compound, solvent, and lithium salt, as well as any optional components added as necessary, and uniformly dissolve or disperse each component.
[0037] The configuration of the lithium ion secondary battery containing the above-mentioned electrolyte is not particularly limited, and may be the same as that of a known lithium ion secondary battery. Usually, the lithium ion secondary battery containing the above-mentioned electrolyte includes a negative electrode and a positive electrode, and may include a separator or an exterior body as necessary. The shape of the lithium ion secondary battery is not particularly limited, and may be, for example, a cylindrical type, a square type, a laminate type, or a coin type.
[0038] (Separator) The separator may be any material that is commonly used in conventional lithium ion secondary batteries. Examples of materials that may be used for the separator include glass fiber, polyester, Teflon (registered trademark), polyethylene, polypropylene, polytetrafluoroethylene (PTFE), and polyimide.
[0039] As described above, the electrolyte and the lithium ion secondary battery of the present embodiment can be used stably even at high voltages. Specifically, as described in the examples below, the electrolyte of the present embodiment can suppress the decrease in discharge capacity in a long-term cycle test. In addition, the electrolyte of the present embodiment can suppress the denaturation of the electrode and the decomposition of the electrolyte. In contrast, an electrolyte that does not contain the above-mentioned compound has problems such as the oxidative decomposition of the carbonate-based electrolyte and the difficulty in maintaining structural stability under high voltages using a ternary mixed metal oxide material. In addition to the problem of the electrochemical stability of the carbonate-based electrolyte itself, various transition metals contained in the ternary electrode act catalytically to promote the decomposition (LiPF6→LiF+PF5) of the lithium salt (LiPF6) contained in the ethylene carbonate solution. Furthermore, if a trace amount of moisture is present in the system, PF5 is hydrolyzed to generate hydrofluoric acid such as PF5+H2O→PF3O+2HF, and this hydrofluoric acid may further destroy the coating on the electrode and corrode the electrode. In addition, there are few additives known that can simultaneously stabilize the positive and negative electrodes, and the electrolyte of the present embodiment is considered to be effective for stabilizing the full cell. The manufacturing method and effects will be described in more detail in the examples described below. EXAMPLES
[0040] The effects of the electrolyte solution and the lithium ion secondary battery are demonstrated below by examples. These examples show one embodiment of the present disclosure, and the present disclosure is not limited thereto in any way.
[0041] First, bisiminoacenaphthenequinone (BIAN-thiophene), a compound with a thiophene structure contained in the electrolyte, was synthesized as follows. As shown in the reaction formula below, acenaphthenequinone and 2 equimolar amounts of methyl 2-aminothiophene-3-carboxylate were dissolved in acetonitrile, and stirred overnight under reflux in a nitrogen atmosphere to synthesize BIAN-thiophene. This BIAN-thiophene has a carbonyl group.
[0042] [ka]
[0043] Next, the components shown in Table 1 were mixed to prepare the electrolyte solutions of Example 1 and Comparative Example 1. 1.0M LiPF6 was used as the lithium salt, and EC (Ethylene Carbonate):DEC (Diethyl Carbonate) = 1:1 was used as the solvent. The electrolyte solution of Example 1 contains 1.0mg / ml of BIAN-thiophene synthesized as described above. The electrolyte solution of Comparative Example 1 is the same as the electrolyte solution of Example 1, except that it does not contain BIAN-thiophene.
[0044] [Table 1]
[0045] Next, the electrolyte of Example 1 and LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 A 2025-type coin cell, which is a cathode half-cell, was prepared using an O2 electrode and Li metal as a counter electrode. Similarly, the electrolyte of Comparative Example 1 and LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 A 2025-type coin cell of Comparative Example 1, which is a cathode half cell, was prepared using an O2 electrode and Li metal as a counter electrode.
[0046] Next, a long-term cycle test was carried out on the 2025-type coin cells of Example 1 and Comparative Example 1. The results of the long-term cycle test are shown in Figure 1. In 80 cycles, the discharge capacity of Comparative Example 1 decreased to about 65% from the initial discharge capacity, whereas the discharge capacity of Example 1 was maintained at about 80% of the initial discharge capacity. The coulombic efficiency of Example 1 and Comparative Example 1 were almost the same.
[0047] Next, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3The SEM (Scanning Electron Microscope) image of the O2 electrode was observed. Figure 2 (A) shows the LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 SEM image of the O2 electrode, and LiNi after 100 cycles in Comparative Example 1 (B) 1 / 3 Mn 1 / 3 Co 1 / 3 SEM image of the O2 electrode, and LiNi after 100 cycles in Example 1 (C) 1 / 3 Mn 1 / 3 Co 1 / 3 The SEM image of the LiNiO2 electrode shows that the micrometer-sized spherical particles in the bead-like form are decomposed on the electrode surface of the electrolyte of Comparative Example 1, and deposits are observed. On the other hand, the electrode surface of the electrolyte of Example 1 largely maintained the shape of the spherical particles. Therefore, the presence of BIAN-thiophen resulted in the formation of LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 It is believed that the denaturation of the O2 electrode and the decomposition of the electrolyte were suppressed.
[0048] Next, anode half-cells were prepared using the electrolytes of Example 1 and Comparative Example 1, and rate and cycle tests were carried out. As shown in FIG. 3(A), Example 1 showed a higher discharge capacity than Comparative Example 1 in the low charge / discharge rate range. On the other hand, Example 1 did not have an advantage over Comparative Example 1 in the rate test at 1C or more, so the cycle test was carried out at a rate of 0.1C. As shown in FIG. 3(B), the cycle test showed that Example 1 suppressed deterioration of battery performance after 100 cycles. The coulombic efficiency of Example 1 and Comparative Example 1 was almost the same.
[0049] Next, a stainless steel plate was used as the working electrode and Li metal was used as the counter electrode, and the electrolytes of Example 1 and Comparative Example 1 were compared at a sweep rate of 1 mV / s. -1Linear Sweep Voltammetry (LSV) measurements were performed in the scanning range of 0V to 6.0V and the scanning range of 2.5V to 0.01V. In the electrolyte of Example 1, as shown in FIG. 4(A), a reduction peak was observed on the high potential side, and as shown in FIG. 4(B), an oxidation peak was observed on the low potential side, suggesting that the compound BIAN-thiophen decomposes before the solvent. It is believed that the reduction peak was observed on the high potential side in the electrolyte of Example 1 because the compound contains BIAN. It is believed that the oxidation peak was observed on the low potential side in the electrolyte of Example 1 because the compound contains thiophen. This shows that the electrolyte can be used stably by containing the compound BIAN-thiophen in the electrolyte.
[0050] Next, the electrolyte solutions of Examples 1 to 7 and Comparative Example 1 were prepared by mixing the components at the content ratios shown in Table 2. 1.0M LiPF6 was used as the lithium salt, and EC (Ethylene Carbonate):DEC (Diethyl Carbonate) = 1:1 was used as the solvent. The electrolyte solutions of Examples 1 to 7 contain BIAN-thiophene synthesized as described above at the concentrations shown in Table 2. The electrolyte solution of Comparative Example 1 is the same as the electrolyte solutions of Examples 1 to 7, except that it does not contain BIAN-thiophene.
[0051] [Table 2]
[0052] A charge / discharge test was carried out on the batteries using the electrolytes of Examples 1 to 7 and Comparative Example 1. The results are shown in FIG. 5. It was found that the effect of BIAN-thiophene can be obtained by adding a small amount of the compound. It was also found that the content of the compound in the electrolyte is preferably more than 0 mg / ml, more preferably 0.5 mg / ml or more. It was also found that adding 6.0 mg / ml or more would result in a discharge capacity lower than that of a system without the compound, so it was found that it is better to avoid adding an excessive amount. In detail, it was found that the content of the compound in the electrolyte is preferably 6.0 mg / ml or less, more preferably 3.0 mg / ml, and even more preferably 1.5 mg / ml or less.
[0053] As described above, by using the electrolyte of Example 1, in the 80th cycle of the long-term cycle test, the initial discharge capacity was maintained at about 80%, whereas in Comparative Example 1, the initial discharge capacity decreased to about 65%. This shows that the decrease in discharge capacity can be suppressed by using the electrolyte of Example 1. In addition, the LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 When the SEM image of the O2 electrode was observed, the electrode surface of the electrolyte of Example 1 generally maintained the shape of spherical particles. 1 / 3 Mn 1 / 3 Co 1 / 3 It is believed that the degeneration of the O2 electrode and the decomposition of the electrolyte were suppressed. 1 / 3 Mn 1 / 3 Co 1 / 3Nickel-manganese-cobalt ternary mixed metal oxide material containing O2 is an electrolyte for lithium ion secondary batteries that provides high voltage and high energy density, and it was found that by using the electrolyte of Example 1, it can be stably used even at high voltage. Therefore, it was found that even in a high voltage system (4.5V to 5.0V) for next-generation batteries utilizing a ternary mixed system, the electrolyte of Example 1 can be stably used. In the compound included in Example 1, BIAN-thiophen has a carbonyl group, but it is not necessary to have a carbonyl group, and it is considered that the same effect can be obtained even if it has a substituent other than a carbonyl group. In addition to or instead of a carbonyl group, boron, sulfur, phosphorus, fluorine, an isocyanate group (N=C=O), a silyloxy group (Si-O), a phosphonate group (P(OR 51 )2R 52 ) may be included. 51 , R 52 is an organic group. When it contains boron, sulfur, phosphorus, or fluorine as a substituent, it is believed to be effective in forming a coating that protects the electrode from corrosion by HF. In addition, when it contains an isocyanate group (N=C=O), a silyloxy group (Si-O), a phosphonate group (P(OR 51 )2R 52 ), it is believed that the effect of capturing HF generated by the decomposition of LiPF6 can be obtained.
[0054] The present invention allows various embodiments and modifications without departing from the broad spirit and scope of the present invention. The above-described embodiments are for the purpose of explaining the present invention and do not limit the scope of the present invention. That is, the scope of the present invention is indicated by the claims, not the embodiments. Various modifications made within the scope of the claims and the scope of the invention equivalent thereto are considered to be within the scope of the present invention.
Claims
1. A method for producing a liquid crystal display comprising: a compound represented by formula (1), a solvent, and a lithium salt; An electrolyte solution characterized by: 【Chemical 1】 R 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 31 , R 32 , R 33 , R 41 , R 42 and R 43 each independently represents a substituent.
2. The compound is contained in the electrolyte solution in an amount of more than 0 mg / ml and not more than 6.0 mg / ml.
2. The electrolyte solution according to claim 1 .
3. The substituents include boron, sulfur, phosphorus, fluorine, an isocyanate group (N=C=O), a silyloxy group (Si—O), a phosphonate group (P(OR 51 ) 2R 52 ) and R 51 , R 52 is an organic group, 3. The electrolyte solution according to claim 1 or 2.
4. The solvent includes ethylene carbonate and diethyl carbonate.
3. The electrolyte solution according to claim 1 or 2.
5. The electrolyte solution according to claim 1 or 2 is contained. A lithium-ion secondary battery characterized by:
6. As the positive electrode active material, LiNi x Co y Ma 1-x-y O 2 (wherein Ma represents one or more members selected from the group consisting of Mn and Al, and 0≦x≦1, 0≦y≦1, and x+y≦1.) 6. The lithium ion secondary battery according to claim 5.
Citation Information
Patent Citations
Nonaqueous electrolyte and nonaqueous electrolyte battery
JP1995006786A