Graft polymer, and method for producing graft polymer

A graft polymer with a defined structural unit and production method ensures enhanced temperature responsiveness, addressing the limitations of conventional polymers by providing effective temperature transitions at low concentrations.

JP2024161709AInactive Publication Date: 2024-11-20OSAKA UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023076648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional temperature-responsive polymers lack sufficient properties for various applications, necessitating the development of new polymers with enhanced temperature responsiveness, especially at low concentrations.

Method used

A graft polymer with a specific structural unit (A) representing 1 to 100% of the main chain, combined with optional structural unit (B), and produced through a method involving group transfer polymerization and reaction with vinyl ether group-containing compounds, achieving a molecular weight ratio of 1.0 to 2.0 and exhibiting LCST or UCST type temperature responsiveness.

Benefits of technology

The graft polymer demonstrates good temperature responsiveness even at extremely low concentrations, with sharp transitions and efficient production methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161709000005
    Figure 2024161709000005
  • Figure 2024161709000006
    Figure 2024161709000006
  • Figure 2024161709000007
    Figure 2024161709000007
Patent Text Reader

Abstract

To provide a novel temperature-responsive polymer.SOLUTION: A graft polymer has structural units (A) represented by general formula (1). The number of the structural units (A) in the main chain of the graft polymer is 1-100% relative to the total number of structural units constituting the main chain of the graft polymer (where R1 is a hydrogen atom or a methyl group, R2 is a divalent organic group, R3 is a hydrogen atom or a methyl group, and R4 is a monovalent organic group).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a graft polymer and a method for producing the graft polymer. [Background technology]

[0002] As heterogeneous polymerizable monomers having both radically polymerizable groups and ionically polymerizable groups in the molecule, vinyl ether group-containing (meth)acrylic acid esters are known. Polymers obtained by polymerizing such heterogeneous polymerizable monomers are highly versatile and useful industrially, and are widely used in various applications.

[0003] For example, vinyl ether pendant polymers obtained by polymerizing the (meth)acryloyl group of vinyl ether group-containing (meth)acrylic acid esters have vinyl ether groups in the side chains, and examples are known in which these are used as reaction sites. Compared to other functional groups at reaction sites, vinyl ether groups have the advantages of being less corrosive to metals, having high storage stability, and being less irritating and toxic.

[0004] Meanwhile, in recent years, stimuli-responsive polymeric materials that change their properties or morphology in response to physical stimuli such as temperature changes or chemical stimuli such as pH changes have been attracting attention. For example, a temperature-responsive polymer is a polymer that becomes insoluble or soluble above (or below) a specific temperature. As such temperature-responsive polymers, polyamide-based and polyether-based graft polymers such as copolymers of polyvinyl ether and N-isopropylacrylamide are known (for example, Non-Patent Document 1, etc.). [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Journal of Polymer Science Part A: Polymer Chemistry,2013,51,786-792 Summary of the Invention [Problem to be solved by the invention]

[0006] However, depending on the application, conventional temperature-responsive polymers may not have sufficient other properties required for the application, and therefore, there has been a demand for the development of new temperature-responsive polymers that can be used for various applications. In view of the above-mentioned current situation, an object of the present invention is to provide a new temperature-responsive polymer. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors have conducted extensive research into graft polymers using vinyl ether group pendant polymers and have succeeded in producing a new graft polymer that exhibits good temperature response even at extremely low concentrations, thereby completing the present invention.

[0008] That is, the present invention provides the following aspects. [1] A graft polymer having a structural unit (A) represented by the following general formula (1), wherein the number of the structural unit (A) in the main chain of the graft polymer is 1 to 100% based on the total number of structural units constituting the main chain of the graft polymer:

[0009] [ka]

[0010] (In the formula, R 1 R represents a hydrogen atom or a methyl group. 2 R represents a divalent organic group. 3 R represents a hydrogen atom or a methyl group. 4 represents a monovalent organic group. * represents a bonding position with adjacent structural units constituting the main chain of the graft polymer. a represents the number of structural units constituting the polymer chain of the side chain of the graft polymer, and is an integer of 1 or more. [2] The graft polymer according to the above item [1], further comprising a structural unit (B) other than the structural unit (A). [3] The graft polymer according to the above [1] or [2], having a number average molecular weight of 2,000 to 1,000,000. [4] The graft polymer according to any one of the above [1] to [3], wherein the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 1.0 to 2.0. [5] A step (1) of group transfer polymerizing a monomer component containing a vinyl ether group-containing (meth)acrylic acid ester compound, and adding R 5 -COOH(R 5 represents a hydrocarbon group having 1 to 12 carbon atoms.) and a step (3) of reacting the reaction polymer obtained in the step (2) with a vinyl ether group-containing compound to obtain a graft polymer. Effect of the Invention

[0011] The graft polymer of the present invention has good temperature responsiveness. Moreover, according to the method for producing a graft polymer of the present invention, a graft polymer having good temperature responsiveness can be efficiently produced even at an extremely low concentration. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing 1H-NMR spectra of the polymer (X1) and the reaction polymer (Y1) of Example 1. [Diagram 2] FIG. 1 is a diagram showing the 1H-NMR spectrum of the graft polymer obtained in Example 1. [Diagram 3] 1 is a graph showing the change in transmittance versus temperature for an aqueous solution (concentration: 0.1 wt %) of the graft polymer of Example 1. [Figure 4] 1 is a graph showing the change in transmittance versus temperature for aqueous solutions of the graft polymer of Example 1 (concentrations of 0.1 wt %, 0.01 wt %, 0.001 wt %, and 0.0001 wt %). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention. In this specification, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", and "(meth)acrylate" means "acrylate and / or methacrylate". In addition, a numerical range "(minimum value) to (maximum value)" means "(minimum value) or more and (maximum value) or less". For example, "5 to 10" means "5 or more and 10 or less".

[0014] 1. Graft polymer The graft polymer of the present invention is characterized in that it has a structural unit (A) represented by the above general formula (1), and the number of the structural unit (A) in the main chain of the graft polymer is 1 to 100% based on the total number of structural units constituting the main chain of the graft polymer.

[0015] The graft polymer of the present invention has excellent temperature responsiveness. Temperature responsiveness refers to a stimulus-responsive characteristic that changes physical properties such as solubility in water at a certain temperature. Examples of temperature responsiveness include lower critical solution temperature (LCST) type and upper critical solution temperature (UCST) type. LCST type temperature responsive polymers exhibit reversible phase separation behavior in which the polymer aggregates and becomes cloudy when heated to a certain temperature or higher, and dissolves again when cooled below that temperature. On the other hand, UCST type temperature responsive polymers exhibit reversible phase separation behavior in which the polymer aggregates and becomes cloudy when cooled to a certain temperature or lower, and dissolves again when heated above that temperature. The reason why the graft polymer of the present invention shows such temperature responsiveness is believed to be that it has a structure having both hydrophilic and hydrophobic structures of the polyvinyl ether chain in the above general formula (1). The graft polymer of the present invention can be a LCST type or UCST type polymer depending on the structural unit represented by the above general formula (1) and other structural units, and among them, the LCST type is preferred.

[0016] <Structural unit (A)> The graft polymer of the present invention has a structural unit (A) represented by the above general formula (1). In this specification, the term "structural unit" refers to a structure formed by a polymerization reaction of a monomer, in which a carbon-carbon double bond contained in the monomer structure is cleaved to form -CC-. In the above general formula (1), R 1 R represents a hydrogen atom or a methyl group. 1 is preferably a methyl group.

[0017] R 2 represents a divalent organic group. The divalent organic group preferably has 1 to 16 carbon atoms, more preferably 3 to 14 carbon atoms, and further preferably 5 to 12 carbon atoms.

[0018] Examples of the divalent organic group include a divalent hydrocarbon group which may have a substituent, -O-, -CO-, -COO-, -NH-, -S-, -SO-, -SO2-, or a group consisting of a combination thereof.

[0019] The divalent hydrocarbon group may be linear or cyclic, and may be saturated or unsaturated. The divalent hydrocarbon group preferably has 1 to 10 carbon atoms, and more preferably has 2 to 6 carbon atoms.

[0020] The divalent hydrocarbon group includes a divalent aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Examples of the divalent aliphatic hydrocarbon group include alkylene groups such as a methylene group, an ethylene group, a propylene group, an isopropylene group, a butylene group, an isobutylene group, a t-butylene group, and a pentylene group, and alkenylene groups such as a vinylene group and a propenylene group.

[0021] Examples of the divalent alicyclic hydrocarbon group include cycloalkylene groups such as cyclopropylene, cyclobutylene, cyclohexylene, and bicyclohexylene groups.

[0022] Examples of the divalent aromatic hydrocarbon group include arylene groups such as a phenylene group and a naphthylene group, aralkyl groups such as a benzyl group, and a biphenylene group.

[0023] Examples of the substituent that the divalent hydrocarbon group may have include a fluorine atom and an alkoxy group.

[0024] Among these, the divalent organic group is preferably a divalent hydrocarbon group which may have a substituent, -O-, -COO-, or a group consisting of a combination thereof, and -COO-(R 2a -O) n -R 2b -(R 2a and R 2b are the same or different and each represents a divalent aliphatic hydrocarbon group which may have a substituent. n is an integer of 0 to 2.) or -R 2c -(R 2c represents a divalent aromatic hydrocarbon group having 6 to 12 carbon atoms which may have a substituent.) is more preferable. R 2a and R 2b The divalent aliphatic hydrocarbon group represented by the following formula (I) is preferably an aliphatic hydrocarbon group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 2 carbon atoms. R 2c The divalent aromatic hydrocarbon group represented by the following formula (I) is preferably a phenylene group, a biphenylene group, or a naphthylene group, and more preferably a phenylene group.

[0025] R 3 represents a hydrogen atom or a methyl group.

[0026] R 4 R represents a monovalent organic group. 4 The monovalent organic group represented by the following formula (I) preferably has 2 to 12 carbon atoms, more preferably 2 to 10 carbon atoms, and further preferably 2 to 8 carbon atoms.

[0027] R 4 Examples of the monovalent organic group represented by the formula (I) include a monovalent hydrocarbon group which may have a substituent, or a group consisting of a combination of a monovalent hydrocarbon group which may have a substituent and a divalent hydrocarbon group, -O-, -CO-, -COO-, -NH-, -S-, -SO-, or -SO2-.

[0028] R 4 The optionally substituted hydrocarbon group represented by the formula (I) is a monovalent hydrocarbon group which may be substituted. The monovalent hydrocarbon group may be one obtained by adding one hydrogen atom to the divalent hydrocarbon group described above to make it monovalent. Examples of groups consisting of the above combinations include groups consisting of a combination of -O-, -CO-, -COO-, -NH-, -S-, -SO-, or -SO2- with a monovalent hydrocarbon group, or a combination of a monovalent hydrocarbon group and a divalent hydrocarbon group.

[0029] R 4 Examples of the substituent that the hydrocarbon group represented by the formula (I) may have include a fluorine atom, an alkoxy group, and a hydroxyl group.

[0030] Among them, R 4 The monovalent organic group represented by the formula: -R 4a , or -(R 4b -O) p -R 4c , -(R 4d -O) q -CO-R 4e (In the formula, R 4a ~R 4eand are the same or different and each represents a hydrocarbon group which may have a substituent. p and q are the same or different and each represents an integer of 1 to 30.) is preferred.

[0031] R 4a , R 4b , R 4c , R 4d and R 4e The hydrocarbon group represented by the formula (I) may be linear or cyclic, and may be saturated or unsaturated.

[0032] R 4a , R 4b , R 4c , R 4d and R 4e The hydrocarbon group represented by the following formula (1) preferably has 1 to 10 carbon atoms, and more preferably has 1 to 6 carbon atoms.

[0033] Among them, R 4a , R 4b , R 4c , or R 4d are preferably the same or different and are aliphatic hydrocarbon groups. R 4e is preferably an unsaturated aliphatic hydrocarbon group, and more preferably an alkenyl group such as a vinyl group or an n-propenyl group.

[0034] Each of p and q is preferably an integer of 1-9.

[0035] In the structural unit (A) represented by the above general formula (1), -CH2-CR 1 - is a portion that constitutes the main chain of the graft polymer. The number of structural units (A) in the graft polymer is not particularly limited, but is preferably 3 to 1,000, and more preferably 5 to 500. The graft polymer may have a repeating structure of two or more consecutive structural units (A), and the graft polymer may have only one or more consecutive repeating structures of the general formula (1). When there are multiple repeating structures, a structural unit (B) other than the structural unit (A) described below is present between the multiple repeating structures. When a plurality of repeating structures are present, the number of repeats in the plurality of repeating structures may be the same or different.

[0036] The above graft polymer may have only one type of structural unit (A), or may have two or more types.

[0037] <Structural unit (B)> The above graft polymer may further have a structural unit (B) other than the above structural unit (A) in the main chain. Examples of the other structural unit (B) include structural units derived from other polymerizable monomers that can provide structural units other than the structural unit (A). The other polymerizable monomers can be appropriately selected depending on the purpose and application of the polymer to be produced.

[0038] Specific examples of the other polymerizable monomers include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, adamantyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-(acetoacetate)(meth)acrylate, 2-methylpropanediol ... (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxy(meth)acrylate, 4-hydroxymethylcyclohexylmethyl (meth)acrylate, and the like; trifluoroethyl (meth)acrylate, (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxy(meth)acrylate, 4-hydroxymethylcyclohexylmethyl (meth)acrylate, and the like; Examples of the polymerizable monomer include halogen-containing (meth)acrylic esters such as octafluoropentyl acrylate, heptadodecafluorodecyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; nitrogen-containing polymerizable monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, and N,N'-dimethylaminoethyl (meth)acrylate; polyfunctional polymerizable monomers such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and pentaerythritol tri(meth)acrylate; aromatic vinyl monomers such as styrene, and diene monomers such as butadiene. The other polymerizable monomers may be used alone or in combination of two or more.

[0039] The above graft polymer may have only one type of structural unit (B), or may have two or more types.

[0040] When the above-mentioned graft polymer has the above-mentioned structural unit (A) and structural unit (B) in the main chain, it may be an alternating copolymer of the structural unit (A) and the structural unit (B), or it may be a block copolymer or a random copolymer. In addition, when the graft polymer has a plurality of different structural units all represented by the general formula (1) above, or further has a structural unit (B), the graft polymer may be an alternating copolymer, a block copolymer, or a random copolymer.

[0041] In the above graft polymer, the number of structural units (A) in the main chain of the graft polymer is 1 to 100% based on the total number of structural units constituting the main chain of the graft polymer. The number of structural units (A) in the main chain of the graft polymer is preferably 10 to 100%, more preferably 20 to 100%, and even more preferably 20 to 80%, based on the total number of structural units constituting the main chain of the graft polymer, in order to improve the temperature responsiveness of the graft polymer.

[0042] The number of structural units (B) in the main chain of the graft polymer may be appropriately designed depending on the purpose and use of the polymer, but is preferably 0 to 99% of the total number of structural units constituting the main chain of the graft polymer. Within the above range, the graft polymer can exhibit temperature responsiveness. In terms of suppressing gelation, the number of structural units (B) in the main chain of the graft polymer is more preferably 0 to 90%, even more preferably 0 to 80%, and even more preferably 20 to 80% of the total number of structural units constituting the main chain of the graft polymer.

[0043] In the structural unit (A) represented by the above general formula (1), a represents the number of structural units (a) constituting the polymer chain bonded to the side chain, represented by the following formula (1-1). When a is 2 or more, the structural unit (A) has a repeating structure in which two or more structural units (a) are consecutive. In the polymer chain of the side chain of the graft polymer, there may be only one repeating structure in which two or more structural units (a) are consecutive, or there may be more than one. When there are more than one repeating structures, another structural unit other than the structural unit (a) is present between the multiple repeating structures. When there are two or more repeating structures, the number of repeating structures of the structural unit (a) may be the same or different.

[0044] [ka] (In the formula, R 3 and R 4 are the same as in equation (1).

[0045] The total number of unit structures (a) of the side chains represented by the formula (1-1) in the polymer chains of the side chains of the graft polymer is preferably 5 to 1,000, more preferably 10 to 500.

[0046] The number of structural units (a) represented by the above formula (1-1) in the polymer chain of the side chain of the graft polymer is preferably 10 to 100%, more preferably 20 to 100%, based on the total number of structural units in the polymer chain of the side chain of the graft polymer.

[0047] As described above, the structural unit (a) represented by the above formula (1-1) is, among others, 3 represents a hydrogen atom or a methyl group, R 4 But -R 4a , or -(R 4b -O) p -R 4c (In the formula, R 4a , R 4b , and R 4care the same or different and represent a hydrocarbon group which may have a substituent. p represents an integer of 1 to 30. A structural unit (a') representing the following is preferred. The number of such structural units (a') is preferably 10 to 100%, more preferably 20 to 100%, and even more preferably 50 to 100%, based on the total number of structural units in the polymer chain of the side chain of the graft polymer.

[0048] The polymer chain of the side chain of the graft polymer may further have a structural unit (b) other than the structural unit (a). Examples of the monomer that gives the structural unit (b) include the polymerizable monomer that gives the structural unit (B) described above, such as aromatic vinyl monomers such as styrene. These may be used alone or in combination of two or more.

[0049] When the polymer chain of the side chain of the above graft polymer has the structural unit (a) and the structural unit (b), the polymer may be an alternating copolymer of the structural unit (a) and the structural unit (b), a block copolymer, or a random copolymer. In addition, when the graft polymer has a plurality of different structural units (a) all represented by the above general formula (1-1), or further has a structural unit (b), the graft polymer may be an alternating copolymer, a block copolymer, or a random copolymer.

[0050] By appropriately selecting the structural unit (b) of the above graft polymer, it is possible to obtain a temperature-responsive polymer of LCST type or UCST type, and further a crosslinkable polymer.

[0051] The number of structural units (b) in the polymer chain of the side chain of the graft polymer is preferably 0 to 90%, more preferably 0 to 80%, based on the total number of structural units in the polymer chain of the side chain of the graft polymer.

[0052] The number average molecular weight (Mn) of the graft polymer is preferably 2000 to 1000000. When the weight average molecular weight is within the above range, handling is easy.

[0053] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the graft polymer is preferably 1.0 to 2.0. When the ratio (Mw / Mn) is within the above range, the molecular weight distribution of the graft polymer becomes small, and the polymer is likely to exhibit sharp temperature responsiveness. The ratio (Mw / Mn) is more preferably 1.0 to 1.8, and even more preferably 1.0 to 1.5, in that the polymer can exhibit sharper temperature responsiveness.

[0054] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the graft polymer can be determined by gel permeation chromatography (GPC) as described in the Examples below, and the ratio (Mw / Mn) can be determined by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn).

[0055] The graft polymer exhibits LCST or UCST type temperature responsiveness. The lower critical solution temperature and the upper critical solution temperature can be measured by preparing an aqueous solution of the graft polymer and measuring the transmittance of the aqueous solution at a specific wavelength using an ultraviolet-visible spectrometer equipped with a temperature controller.

[0056] 2. Method for producing graft polymer The method for producing the graft polymer of the present invention is not particularly limited as long as it is a method that can obtain a graft polymer having the above-mentioned structural unit (A), but examples thereof include a method of polymerizing a monomer component containing a vinyl ether group-containing monomer, reacting a carboxylic acid compound with the vinyl ether group of the obtained polymer, and reacting the obtained reactant with a monomer component containing a vinyl ether group-containing compound to obtain a graft polymer, and a method of reacting a carboxylic acid compound with a vinyl ether group-containing monomer, polymerizing a monomer component containing the obtained reactant, and reacting the obtained polymer with a monomer component containing a vinyl ether group-containing compound to obtain a graft polymer, etc. Among them, a production method including a step (1) of polymerizing a monomer component containing a vinyl ether group-containing monomer, a step (2) of reacting a carboxylic acid compound with the polymer obtained in the above polymerization step (1), and a step of reacting a monomer component containing a vinyl ether group-containing compound with the reacted polymer obtained in the above reaction step (2) to obtain a graft polymer is preferred in that gelation is suppressed and a graft polymer with less by-products is easily obtained.

[0057] Process (1) A preferred method for producing a graft polymer of the present invention includes a step of polymerizing a monomer component containing a vinyl ether group-containing monomer. In step (1), the monomer component is polymerized without reacting the vinyl ether group to obtain a polymer (X) having a vinyl ether group in a side chain.

[0058] The vinyl ether group-containing monomer may be a compound having a vinyl ether group and a polymerizable double bond. The polymerizable double bond is a polymerizable carbon-carbon double bond, and may be, for example, a (meth)acryloyl group, a vinyl group, an allyl group, or a methallyl group. Among them, a vinyl group or a (meth)acryloyl group is preferred, and a (meth)acryloyl group is more preferred.

[0059] Specific examples of the vinyl ether group-containing monomer include vinyl ether group-containing (meth)acrylic acid ester compounds such as 2-(2-vinyloxyethoxy)ethyl acrylate and 2-(2-vinyloxyethoxy)ethyl methacrylate; and vinyl ether group-containing styrene compounds such as 4-vinyloxystyrene, (2-vinyloxyethoxy)styrene, and (2-(2-vinyloxyethoxy)ethyl)styrene.

[0060] The monomer component may further contain other monomers that provide the structural unit (B) described above. The amount of each monomer contained in the monomer component may be appropriately adjusted depending on the structure of the target polymer, but the proportion of other monomers that provide the structural unit (B) in 100% by mass of the monomer component is preferably 0 to 99% by mass. More preferably, it is 0 to 50% by mass, and even more preferably, it is 0 to 30% by mass.

[0061] The method for polymerizing the monomer components is not particularly limited as long as a polymer having a vinyl ether group on the side chain can be obtained, and any known polymerization method such as radical polymerization, coordination polymerization, anionic polymerization, etc. can be used. Among these, group transfer polymerization is preferred in that it is more efficient in that a polymer having a vinyl ether group on the side chain can be obtained by reacting only the polymerizable double bonds without reacting the vinyl ether groups.

[0062] Group transfer polymerization can be carried out by polymerizing monomer components in the presence of a polymerization initiator, such as a silane compound having a carbon-carbon double bond, and a catalyst.

[0063] Examples of the silane compound having a carbon-carbon double bond include silyl acetal compounds, vinyl silane compounds, allyl silane compounds, etc., as described in International Publication No. 2019 / 240049. Among these, silyl ketene acetal compounds are preferred.

[0064] Specific examples of the silyl ketene acetal compound include methyl(trimethylsilyl)dimethyl ketene acetal, methyl(triethylsilyl)dimethyl ketene acetal, methyl(triisopropylsilyl)dimethyl ketene acetal, methyl(tert-butyldimethylsilyl)dimethyl ketene acetal, methyl(trimethylsilyl)diethyl ketene acetal, methyl(triphenylsilyl)dimethyl ketene acetal, methyl(methyldiphenylsilyl)dimethyl ketene acetal, methyl(dimethylphenylsilyl)dimethyl ketene acetal, methyl(triethoxysilyl)dimethyl ketene acetal, ethyl(trimethylsilyl)dimethyl ketene acetal, 2-ethylhexyl(trimethylsilyl)dimethyl ketene acetal, tert-butyl(trimethylsilyl)dimethyl ketene acetal, and 1-[(1-methoxy-2-methyl-1-propenyl)oxy]-1-methylsilacyclobutane. Among these, methyl(trimethylsilyl)dimethylketene acetal is preferred because of its ready availability.

[0065] The polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used is not particularly limited as long as the desired polymer can be obtained. However, in order to obtain a polymer more efficiently, it is preferable to use an amount of the polymerization initiator of 1×10 to the monomer component used. -4 ~10 mol%, more preferably 1 × 10 -3 ~5 mol%, more preferably 1 × 10 -2 %.

[0066] Examples of the catalyst include those described in WO 2019 / 240049. Among them, a basic catalyst is preferred, and an organic phosphorus compound, an N-heterocyclic carbene, a fluorine ion-containing compound, a cyclic amine compound, or an ammonium salt compound is more preferred, and an ammonium salt compound is even more preferred.

[0067] Examples of the ammonium salt compound include tetrabutylammonium bisacetate, tetrabutylammonium acetate, tetrabutylammonium benzoate, tetrabutylammonium bisbenzoate, tetrabutylammonium metachlorobenzoate, tetrabutylammonium cyanate, tetrabutylammonium methoxide, tetrabutylammonium thiolate, tetrabutylammonium bibromide, and ammonium salt compounds in which the ammonium cation is replaced with a tetramethylammonium, triethylammonium, benzyltributylammonium, N-methyl-N-butylpiperidinium, N-methyl-N-butylpyrrolidinium cation, or a pyridinium cation.

[0068] The amount of the catalyst used is not particularly limited as long as the desired polymer can be obtained. However, in order to obtain a polymer more efficiently, it is preferable to use an amount of the catalyst of 1×10 to the monomer component used. -4 ~10 mol%, more preferably 1 × 10 -3 ~5 mol%, more preferably 1 × 10 -2 %.

[0069] The polymerization reaction may or may not involve the use of a solvent, but it is preferred to use a solvent, which is preferably an aprotic solvent.

[0070] Specific examples of the solvent include aromatic hydrocarbon solvents such as toluene, xylene, and benzene; aliphatic hydrocarbon solvents such as hexane, pentane, heptane, and cyclohexane; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; halogenated hydrocarbon solvents such as chlorobenzene, dichloromethane, chloroform, and 1,2-dichloroethane; nitrile solvents such as acetonitrile, propionitrile, and valeronitrile; ester solvents such as methyl acetate, ethyl acetate, isopropyl acetate, and butyl acetate; dimethylformamide (DMF), dimethylacetamide, Amide-based solvents such as N-methylpyrrolidone; ether-based solvents such as diethyl ether, diisopropyl ether, 1,2-dimethoxyethane (DME), 1,4-dioxane, tetrahydrofuran (THF), tetrahydropyran (THP), anisole, diethylene glycol dimethyl ether (diglyme), diethylene glycol ethyl ether (carbitol), cyclopentyl methyl ether (CPME); fluorine-based solvents such as perfluorohexane, perfluorocyclohexane, pentafluorobenzene, octafluorotoluene; DMSO, nitromethane, etc. Among them, at least one selected from the group consisting of aromatic hydrocarbon-based solvents, aliphatic hydrocarbon-based solvents, ketone-based solvents, halogenated hydrocarbon-based solvents, ether-based solvents, ester-based solvents, and nitrile-based solvents is preferred in that the polymerization reaction proceeds more smoothly, and aromatic hydrocarbon-based solvents, ether-based solvents, and ester-based solvents are more preferred. The above solvents may be used alone or in combination of two or more.

[0071] The reaction atmosphere for the polymerization may be air, but is preferably an inert gas atmosphere such as nitrogen or argon.

[0072] The reaction temperature in the above polymerization is preferably -20 to 100°C, more preferably -10 to 50°C, still more preferably 0 to 40°C, and particularly preferably 0 to 30°C, in order to narrow the molecular weight distribution, i.e., to reduce the above ratio (Mw / Mn).

[0073] The number average molecular weight (Mn) of the polymer (polymer (X)) obtained in step (1) is, in terms of allowing the next step to proceed efficiently, preferably 1000 to 500000, more preferably 2000 to 200000, and even more preferably 2000 to 100000. The weight average molecular weight can be determined by gel permeation chromatography (GPC).

[0074] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the polymer (X) obtained in step (1) is preferably 1.0 to 2.0. When the ratio (Mw / Mn) is within the above range, a graft polymer having a narrow molecular weight distribution can be obtained, and a sharp temperature response can be exhibited. The ratio (Mw / Mn) is more preferably 1.0 to 1.8, and even more preferably 1.0 to 1.6. The weight average molecular weight can be determined by gel permeation chromatography (GPC).

[0075] Process (2) The method for producing the graft polymer next includes a step (2) of reacting the polymer obtained in the polymerization step (1) with a carboxylic acid compound. In step (2), the vinyl ether group in the side chain of the polymer obtained in step (1) (polymer (X)) is reacted with a carboxylic acid compound to carry out acetalization.

[0076] The carboxylic acid compound is preferably R 5 -COOH(R 5 represents a hydrocarbon group having 1 to 12 carbon atoms.

[0077] R 5 The hydrocarbon group represented by the formula (I) may be linear or cyclic, and may be saturated or unsaturated. Among them, linear or cyclic saturated hydrocarbon groups are preferred, and linear saturated hydrocarbon groups are more preferred, in that the cationic polymerization in step (3) can be efficiently carried out. R 5 The number of carbon atoms in the hydrocarbon group represented by the following formula is preferably 1 to 6, and more preferably 1 to 4, in terms of facilitating removal of the unreacted carboxylic acid compound after step (2).

[0078] Specific examples of the carboxylic acid compound include aliphatic carboxylic acids such as acetic acid, propionic acid, butyric acid, isobutyric acid, pivalic acid, valeric acid, caproic acid, enanthic acid, heptyl acid, octanoic acid, lauric acid, myristic acid, palmitic acid, and stearic acid; and aromatic carboxylic acids such as benzoic acid. Of these, aliphatic carboxylic acids are preferred, and acetic acid, propionic acid, butyric acid, isobutyric acid, and pivalic acid are more preferred. The above carboxylic acid compounds may be used alone or in combination of two or more.

[0079] The amount of the carboxylic acid compound used in the above reaction is preferably 1 to 1.5 equivalents, more preferably 1 to 1.2 equivalents, relative to 1 equivalent of the vinyl ether group in the polymer (X) obtained in the step (1).

[0080] The above reaction is not particularly limited, and can be carried out by a known method such as mixing the respective components and heating them. The reaction conditions are not particularly limited, but for example, the reaction temperature is preferably 10 to 120°C, more preferably 10 to 100°C, and even more preferably 10 to 70°C, in order to suppress gelation and elimination of acetal.

[0081] In the above reaction, a catalyst for accelerating the reaction may be added.

[0082] Process (3) In the above-mentioned method for producing a graft polymer, the reaction polymer (reaction polymer (Y)) obtained in step (2) is further reacted with a monomer component containing a vinyl ether group-containing compound to obtain the graft polymer of the present invention. In step (3), the acetalized portion produced in the reaction in step (2) serves as an initiation point for polymerization to proceed, forming a polymer chain of the side chain of the graft polymer.

[0083] The vinyl ether group-containing compound used in step (3) is not particularly limited as long as it is a compound containing a vinyl ether group, but examples thereof include compounds represented by the following formula (2): CH2=CR 3 -OR 4 (2) (In the formula, R 3 and R 4 is the same as the above formula (1). Examples of the compound include compounds represented by the following formula:

[0084] Specific examples of the compound represented by the above formula (2) include, for example, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, 2-ethylhexyl vinyl ether, cyclohexyl vinyl ether, hydroxyethyl vinyl ether, 2-methoxyethyl vinyl ether, 2-ethoxyethyl vinyl ether, 2-(ethoxyethoxy)ethyl vinyl ether, perfluoropropyl vinyl ether, 2-vinyloxyethyl (meth)acrylate, and 2-(2-vinyloxyethoxy)ethyl (meth)acrylate. Among these, 2-methoxyethyl vinyl ether and isobutyl vinyl ether are preferred because they are easy to obtain a graft polymer with excellent temperature responsiveness. These may be used alone or in combination of two or more. By changing the vinyl ether group-containing compound used, a temperature-responsive polymer of LSCT type or UCST type can be obtained. Furthermore, for example, by using 2-vinyloxyethyl (meth)acrylate, 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, or the like, a crosslinkable polymer having a (meth)acryloyl group in the side chain can be obtained.

[0085] The monomer component may further contain other monomers that give the structural unit (b) described above. The amount of each monomer contained in the monomer component may be appropriately adjusted depending on the structure of the target polymer, but the proportion of the compound represented by the above formula (2) in 100% by mass of the monomer component is preferably 10 to 100% by mass. More preferably, it is 30 to 100% by mass, and even more preferably, it is 50 to 100% by mass.

[0086] The reaction in step (3) is preferably living polymerization, and more preferably living cationic polymerization, since a graft polymer having a narrow molecular weight distribution is likely to be obtained. The reaction in step (3) can be carried out by polymerizing a monomer component containing a vinyl ether group-containing compound to give a reaction polymer (Y) in the presence of a catalyst.

[0087] The above catalyst is preferably a Lewis acid catalyst, and examples thereof include metal halides such as BF3, BBr3, AlF3, AlBr3, TiCl4, TiBr4, FeCl3, FeCl2, SnCl4, WCl6, MoCl5, ZrCl4, SbCl3, SbCl5, TeCl2, GaCl3, or ZnCl2; metal alkyl compounds such as Et2AlCl3, EtAlCl2, Et3Al2Cl3, (i-Bu)2AlCl, (i-Bu)AlCl2, or Bu3SnCl; and trispentafluorophenylborane. These may be used alone or in combination of two or more. Among these, a combination of a metal halide and a metal alkyl compound is preferred.

[0088] The amount of the catalyst used is preferably 0.001 to 1 equivalent, and more preferably 0.01 to 0.5, relative to 1 equivalent of the monomer component containing the vinyl ether group-containing compound used in the step (3).

[0089] In the reaction of step (3), it is preferable to add tetrahydrofuran, 2,6-di-tert-butylpyridine, or the like in order to suppress side reactions. In the above reaction, known additives other than those mentioned above may be used.

[0090] The reaction in step (3) can be carried out in a solvent. Examples of the solvent include the same as those used in step (1) above. Among them, aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ether solvents, ester solvents, and halogenated hydrocarbon solvents are preferred, and aromatic hydrocarbon solvents are more preferred. Only one type of solvent may be used, or two or more types may be used in combination.

[0091] The reaction conditions for step (3) are not particularly limited as long as the desired reaction proceeds. For example, the reaction conditions are preferably -40°C to 70°C, more preferably -20°C to 50°C, and even more preferably -20°C to 40°C.

[0092] As described above, the method for producing the graft polymer preferably includes steps (1) to (3). Among them, when a vinyl ether group-containing (meth)acrylic acid ester compound is used as the vinyl ether group-containing monomer for polymerization, the method includes a step (1) of group transfer polymerizing a monomer component containing a vinyl ether group-containing (meth)acrylic acid ester compound, a step (2) of polymerizing the monomer component containing a vinyl ether group-containing (meth)acrylic acid ester compound by group transfer polymerization, and a step (3) of polymerizing the monomer component containing a vinyl ether group-containing (meth)acrylic acid ester compound by group transfer polymerization. 5 -COOH(R 5 represents a hydrocarbon group having 1 to 12 carbon atoms.) and a step (3) of reacting the reaction polymer obtained in the step (2) with a monomer component containing a vinyl ether group-containing compound to obtain a graft polymer. Such a method for producing a graft polymer also constitutes one aspect of the present invention.

[0093] The method for producing the graft polymer may include other steps in addition to the steps described above. Examples of the other steps include a dilution step, a drying step, a concentration step, a purification step, etc. These steps can be carried out by known methods.

[0094] 3.Applications The graft polymer of the present invention has excellent temperature responsiveness, particularly LCST type temperature responsiveness. Therefore, the graft polymer of the present invention can be suitably used in applications requiring temperature responsiveness. Examples of such applications include drug delivery systems (DDS), water treatment agents, cell culture vessels, etc. Furthermore, by making the polymer have a crosslinkable functional group (e.g., a (meth)acryloyl group) in the side chain, it can be made into a material with excellent curing properties and can be used for applications such as paints, coatings, and adhesives. EXAMPLES

[0095] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0096] The polymers and the like in each example were analyzed as follows. <Molecular weight measurement> (Step 1 and Step 2) The obtained polymer solution was dissolved and diluted with tetrahydrofuran, filtered through a filter having a pore size of 0.45 μm, and then measured by gel permeation chromatography (GPC) using the following apparatus and conditions. Equipment: HLC-8020GPC (Tosoh Corporation) Elution solvent: Tetrahydrofuran Standard material: Standard polystyrene (Tosoh Corporation) Separation column: TSKgel SuperHM-M, TSKgel SuperH-RC (Tosoh Corporation) (Step 3) The obtained graft polymer solution was dissolved and diluted with chloroform, filtered through a filter having a pore size of 0.2 μm, and then measured by gel permeation chromatography (GPC) using the following apparatus and conditions. Equipment: HLC-8020GPC (Tosoh Corporation) Elution solvent: Chloroform Standard material: Standard polystyrene (Tosoh Corporation) Separation column: TSKgel GMH HR-M (Tosoh Corporation)

[0097] < 1 H-NMR measurement> (Step 1 and Step 2) Equipment: Agilent Technologies nuclear magnetic resonance spectrometer (600MHz) Measurement solvent: deuterated chloroform Sample preparation: Several mg to several tens of mg of the polymer obtained in step 1 or 2 was dissolved in a measurement solvent. (Step 3) Equipment: JEOL nuclear magnetic resonance spectrometer (500MHz) Measurement solvent: deuterated chloroform Sample preparation: Several milligrams to several tens of milligrams of the graft polymer obtained in step 3 was dissolved in the measurement solvent.

[0098] Example 1 Synthesis of polymer (X1) having vinyl ether group in the side chain (Step 1) Cyclopentyl methyl ether (CPME) (250 g), tetrabutylammonium benzoate (45.4 mg, 0.125 mmol) dissolved in 2.5 mL of cyclopentyl methyl ether, and methyl(trimethylsilyl)dimethylketene acetal (2.56 mL, 12.5 mmol) were added to a 1 L separable flask. The reaction solution was cooled to 10°C, and a mixture of 2-(2-vinyloxyethoxy)ethyl acrylate (146 g, 730 mmol) and butyl methacrylate (104 g, 730 mmol) was added dropwise over 30 minutes while stirring. After stirring for 3 hours, the mixture was quenched with a small amount of methanol to obtain a CPME solution of polymer (X1) having a vinyl ether group in the side chain. The molecular weight of the obtained polymer (X1) was Mn (number average molecular weight) = 18358, Mw (weight average molecular weight) = 23876, and Mw / Mn = 1.301. The content of structural units derived from 2-(2-vinyloxyethoxy)ethyl acrylate in the polymer (X1) was 50% based on the total number of structural units in the polymer, and the content of structural units derived from butyl methacrylate was 50% based on the total number of structural units in the polymer. In addition, the obtained polymer (X1) 1 The H-NMR spectrum is shown in Figure 1.

[0099] Synthesis of reactive polymer (Y1) (Step 2) A cyclopentyl methyl ether solution (1 g, solid content 50% by mass) of the polymer (X1) and acetic acid (0.2 mL) were placed in a test tube and stirred overnight at 60° C. Water was added to the reaction solution, and the mixture was extracted with toluene. The toluene-containing organic layer was separated and washed with water, passed through a silica gel short column, and then concentrated to obtain a reaction polymer (Y1). The molecular weight of the reaction polymer (Y1) was Mn=25470, Mw=42590, and Mw / Mn=1.672. 1 The H-NMR spectrum is shown in Figure 1. From Figure 1, it was confirmed that all the vinyl ether groups in the side chains of the polymer (X1) were acetalized.

[0100] Synthesis of graft polymer (step 3) Polymerization was carried out in a glass test tube equipped with a three-way stopcock under a dry nitrogen atmosphere. The glass test tube equipped with a three-way stopcock was baked in advance for 10 minutes under dry nitrogen using a heat gun (hot air temperature: approximately 450°C), cooled under nitrogen pressure, and then returned to normal pressure for use. All reagents were injected using a syringe. Toluene (1.69 mL), the reaction polymer (Y1) obtained in step 2 (2.2 mM toluene solution, 0.35 mL), THF (2.0 M toluene solution, 0.35 mL), and 2,6-di-tert-butylpyridine (DTBP) (0.10 M toluene solution, 0.18 mL) were injected into the baked glass test tube equipped with a three-way stopcock using a dried syringe, stirred, and then cooled to 0°C under nitrogen pressure. Et 1.5 AlCl 1.5 A solution (0.25M in toluene, 0.35mL) was added and stirred for about 20 minutes using a magnetic stirrer. It was then cooled to -20℃ under nitrogen pressure. Polymerization was initiated by adding SnCl4 solution (0.15M in heptane / toluene, 0.35mL) and 2-methoxyethyl vinyl ether (MOVE) (0.24mL) pre-cooled to -20℃ to this solution. After 48 hours, the polymerization was stopped by adding a large excess of methanol containing a small amount of aqueous ammonia. The reaction mixture was diluted with dichloromethane and then washed with dilute hydrochloric acid (about 0.6N), followed by water. It was further washed with aqueous sodium hydroxide (about 0.6N), followed by water until neutral. The product polymer was recovered from the organic layer by evaporating the volatiles under reduced pressure, followed by drying in vacuum for at least 6 hours. The molecular weight of the resulting graft polymer was Mn=111000, Mn=138000, and Mw / Mn=1.24. The obtained graft polymer 1 The H-NMR spectrum is shown in Figure 2. In Figure 2, "before fractionation" refers to the graft polymer obtained in step 3, and "after fractionation" refers to the graft polymer obtained in step 3 that was purified using preparative GPC before being subjected to the evaluation of temperature responsiveness.

[0101] The temperature response of the obtained graft polymer was evaluated by the following method. (Temperature responsiveness evaluation) An aqueous solution of the graft polymer with a concentration of 0.1 wt% was prepared, and transmittance measurements were performed twice while changing the temperature. The transmittance was measured at a wavelength of 500 nm by varying the temperature using an ultraviolet-visible spectrometer equipped with a temperature controller (JASCO-V-550 manufactured by JASCO Corporation, with heating and cooling rates of 1°C / 1 min). A graph showing the change in transmittance versus temperature for the aqueous solution of the graft polymer is shown in Figure 3. In Figure 3, (a) shows the graph for the first measurement, (b) shows the graph for the second measurement, and (c) shows the graph for the first and second measurements superimposed on each other. In the figure, the solid line shows the results when the temperature was rising, and the dotted line shows the results when the temperature was falling. As can be seen from FIG. 3, the obtained graft polymer showed a steep change in transmittance between 65° C. and 70° C. in both the first and second measurements, indicating a sharp temperature responsiveness.

[0102] In addition, a similar evaluation was performed under highly dilute conditions (graft polymer concentrations of 0.01 wt%, 0.001 wt%, and 0.0001 wt%). The results are shown in Figure 4. As shown in Figure 4, even under highly dilute conditions, temperature responsiveness was confirmed, although the behavior was broad.

Claims

1. A graft polymer having a structural unit (A) represented by the following general formula (1): The number of the structural units (A) in the main chain of the graft polymer is 1 to 100% based on the total number of structural units constituting the main chain of the graft polymer. A graft polymer characterized by: 【Chemistry 1】 (In the formula, R 1 represents a hydrogen atom or a methyl group. 2 represents a divalent organic group. 3 represents a hydrogen atom or a methyl group. 4 represents a monovalent organic group. * represents a bonding position with an adjacent structural unit constituting the main chain of the graft polymer. a represents the number of structural units constituting the polymer chain of the side chain of the graft polymer, and represents an integer of 1 or more.

2. 2. The graft polymer according to claim 1, further comprising a structural unit (B) other than the structural unit (A).

3. 2. The graft polymer according to claim 1, wherein the number average molecular weight is 2,000 to 1,000,000.

4. 2. The graft polymer according to claim 1, wherein the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 1.0 to 2.

0.

5. A step (1) of subjecting a monomer component containing a vinyl ether group-containing (meth)acrylic acid ester compound to group transfer polymerization; The polymer obtained in step (1) is added with R 5 -COOH(R 5 represents a hydrocarbon group having 1 to 12 carbon atoms; and A step (3) of reacting the reaction polymer obtained in the step (2) with a vinyl ether group-containing compound to obtain a graft polymer. A method for producing a graft polymer, comprising: