Production method of formamide, catalyst for synthesizing formamide, catalyst-containing liquid for synthesizing formamide
A copper-supported zinc oxide catalyst with ethylene glycol facilitates efficient, low-cost production of formamide from carbon dioxide, hydrogen, and ammonia, addressing inefficiencies and cost issues in existing methods.
Patent Information
- Application Number
- JP2023076950
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-20
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing formamide are inefficient, require toxic materials, involve complex processes, or are costly due to the use of expensive catalysts, making them unsuitable for mass production.
A method using a solid catalyst with copper supported on zinc oxide, combined with ethylene glycol, to react carbon dioxide, hydrogen, and ammonia at low pressures and temperatures, facilitating a heterogeneous reaction suitable for large-scale synthesis.
The method enables simple, low-cost production of formamide suitable for mass production, avoiding the need for costly separation steps and expensive catalysts, and can be performed under mild conditions.
Smart Images

Figure 2024161848000003 
Figure 2024161848000001 
Figure 2024161848000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing formamide by using a catalyst to produce formamide from carbon dioxide. More specifically, the present invention relates to a method for selectively producing formamide by reacting carbon dioxide, hydrogen, and ammonia in the presence of a solid catalyst containing copper metal and diols in the presence of the coexistence of the catalyst and a catalyst-containing liquid for synthesizing formamide that contains the catalyst. [Background technology]
[0002] Formamide (N,N-dihydroformamide) is a functional chemical used as an intermediate raw material for pharmaceuticals, agrochemicals, and various organic chemicals, as a solvent, etc., and has a structure in which a nitrogen atom is directly connected to a carbonyl structure and two hydrogen atoms are substituted on the nitrogen. Examples of formamide production include industrially known production methods such as a method of reacting methyl formate with ammonia, and a method of performing an exchange reaction between hydroxyisobutyric acid amide and methyl formate as a by-product of methyl methacrylate, as well as a production method using carbon monoxide as a raw material, ammonia, and an alkali catalyst (Patent Document 1). Another method is a direct synthesis technique of formamide using carbon dioxide as a starting material. One known example of this synthesis of formamide is a two-step method of producing formamide by reacting carbon dioxide with an ammonia borane complex and ammonium hydroxide (Non-Patent Document 1).
[0003] Also known is a method for producing formamide from carbon dioxide, hydrogen and ammonia using a homogeneous catalyst of various transition metals in combination with a phosphine in the presence of various alcohols (Patent Document 2).
[0004] On the other hand, as a method for producing formamide from carbon dioxide, hydrogen, and ammonia using a solid catalyst, which is a heterogeneous catalyst, a production method using a supported catalyst containing gold is known (Patent Document 3).
[0005] In addition, although it is not formamide, a method for producing N,N-dimethylformamide under high pressure of 6 MPa or more using dimethylammonium dimethylcarbamate as a raw material and a copper solid catalyst is known (Non-Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2002-534492 [Patent Document 2] Japanese Patent Publication No. 52-87112 [Patent Document 3] Special Publication No. 2014-523448 [Non-patent literature]
[0007] [Non-Patent Document 1] Bo Zhang et al., Eur. J. Org. Chem. 2018, 14, pp.1739-1743. [Non-Patent Document 2] Jinli Liu et al., Chem. Commun. 2010, 46, pp.5770-5772. Summary of the Invention [Problem to be solved by the invention]
[0008] The above-mentioned reaction using methyl formate is energy inefficient because the target product is synthesized in two steps via a formate ester. Moreover, the method described in Patent Document 1 is undesirable from the viewpoint of safety because it uses highly toxic carbon monoxide. The method described in Non-Patent Document 1 requires a step for producing the ammonia borane complex used as the nitrogen source, and the process is complicated. In addition, a step for separating the co-product containing borane from formamide after the reaction is also required, and the processing of the co-product is costly. The method described in Patent Document 2 uses a homogeneous catalytic reaction, so it cannot be developed into a continuous synthesis, and a step for separating the catalyst from the product is required. Therefore, these methods are not applicable to mass production processes of chemical products. On the other hand, the method described in Patent Document 3 uses a heterogeneous catalytic reaction, but requires expensive gold as a catalyst, which increases production costs and also makes it unsuitable for mass production. The method described in Non-Patent Document 2 produces formamide using an inexpensive solid copper catalyst, but the reaction is carried out under high pressure, and a process is required to produce ammonium carbamate, which is used as a raw material, and ammonia, which has a lower reactivity, is not used as a raw material.
[0009] An object of the present invention is to provide a method for producing formamide which is simple, low-cost, and suitable for mass production, as well as a catalyst and a catalyst-containing liquid for use in said method. [Means for solving the problem]
[0010] As a result of intensive research into solving the above-mentioned problems, the inventors have found that formamide can be obtained inexpensively and simply by using a solid catalyst in which zinc oxide, which has reducing performance while stabilizing the electronic state, is incorporated with copper as a site that acts with the raw material to promote the reduction reaction, reacting carbon dioxide, hydrogen and ammonia with each other, and further adding an optimal diol-based additive on the solid catalyst so that the carbon dioxide can easily come into contact with the solid catalyst, and carrying out the reaction, thereby completing the present invention.
[0011] Specifically, the present invention relates to the following method for producing formamide, a catalyst for synthesizing formamide, and a liquid containing a catalyst for synthesizing formamide. (1) A method for producing formamide using carbon dioxide, hydrogen and ammonia as raw materials, comprising reacting the carbon dioxide, hydrogen and ammonia in the presence of a solid catalyst comprising zinc oxide supported with copper metal and ethylene glycol. (2) The method for producing formamide according to (1) above, wherein the solid catalyst used is one in which the copper metal is contained in an amount of 10 to 40% by mass of the entire solid catalyst. (3) The method for producing formamide according to (1) or (2) above, wherein the reaction is carried out under a pressure of 1 MPa or less. (4) The method for producing formamide according to (1) or (2), wherein the reaction is carried out at a temperature of 100 to 160°C. (5) A catalyst for producing formamide using carbon dioxide, hydrogen and ammonia as raw materials, which is a solid catalyst in which copper metal is supported on zinc oxide. (6) The catalyst for formamide synthesis according to (5) above, wherein the catalyst is a solid catalyst in which the copper metal is contained in an amount of 10 to 40% by mass of the entire solid catalyst. (7) A catalyst-containing liquid for use in the synthesis of formamide, comprising the catalyst for use in the synthesis of formamide according to (5) or (6) above and ethylene glycol. In this specification, when a numerical range is indicated, it is used to mean that the numerical range includes the numerical range before and after the range as the lower and upper limits. In addition, in this specification, formamide means N,N-dihydroformamide, and is clearly distinguished from other formamides in which a group other than hydrogen is substituted on the nitrogen. Effect of the Invention
[0012] According to the present invention, it is possible to provide a method for producing formamide that is simple, low-cost, and suitable for a mass production process, and also to provide a catalyst and a catalyst-containing liquid for use in the method. [Brief description of the drawings]
[0013] [Figure 1]1 shows XRD spectra of the prepared 10% copper oxide-supported zinc oxide (before and after calcination at 500° C.). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiments of the present invention will be described in detail. Furthermore, % concentration indicates % by mass. This embodiment is a method for producing formamide using carbon dioxide, hydrogen and ammonia as raw materials, and a solid catalyst (Cu / ZnO) is made to act on these raw materials, which is made of zinc oxide that has a reducing ability while stabilizing the electronic state, and copper is mixed at a certain ratio as a site that acts on the raw materials and promotes a reduction reaction, and ethylene glycol is made to act on these raw materials to obtain formamide. In this method, the solid catalyst, ethylene glycol, and raw materials such as carbon dioxide, hydrogen and ammonia are introduced into a reactor, and heated, and formamide is easily obtained by dehydration. The solid catalyst used in the reaction is copper metal supported on zinc oxide, and inexpensive metals such as zinc and copper are used as the metal components that constitute the catalyst. Since a solid catalyst is used, a separation process after the reaction is not required, and formamide can be produced by a heterogeneous reaction that is suitable for mass synthesis such as flow synthesis. Furthermore, unlike transition metal complex catalysts which cannot be reused, the solid catalyst used in this embodiment can be reused by, for example, drying overnight at 100°C, calcining at 500°C for 2 hours in the presence of air, and then subjecting the solid catalyst to hydrogen reduction treatment at 500°C for 2 hours.
[0015] The zinc oxide used in this embodiment has a hexagonal wurtzite crystal structure, and preferably has a specific surface area of 10 square meters or more. Any copper compound may be used as the supported copper as long as it has a shape that allows it to be supported, but copper is supported at 0.1-60% of the total mass of the solid catalyst, and more preferably, 10-40% of the total mass is supported from the viewpoint of activity. The amount of the copper is selected from the range of 1-200 mg, more preferably 50-100 mg, per about 0.1 mmol of ammonia (0.08-0.12 mmol).
[0016] The raw material carbon dioxide used in the production method of this embodiment can be used in a solid, liquid, or gaseous state. It is preferable to use a gaseous form because it is easy to obtain and handle. In the case of a gaseous form, a gas mixture containing carbon dioxide (for example, a mixed gas with water vapor) that is widely used industrially can also be used. Hydrogen and carbon dioxide may contain nitrogen or a rare gas, or may contain other inert gases.
[0017] The hydrogenation of carbon dioxide is carried out in the liquid phase at a temperature preferably in the range of 20-160°C and a total pressure in the range of 0.1-1 MPa (absolute pressure), where the total pressure is preferably at least 0.5 MPa (absolute pressure), and the higher the pressure, the higher the reactivity. From the viewpoint of the balance with the equipment cost, the total pressure is particularly preferably 1 MPa (absolute pressure). The reaction temperature is preferably 100-160°C, and particularly preferably 120-140°C, because the generated formamide is easily decomposed by heat. The reaction can be carried out under such mild conditions of low pressure and low temperature.
[0018] The partial pressure of carbon dioxide in the reactor is preferably 0.25-0.75 MPa, more preferably 0.50-0.75 MPa from the viewpoint of reactivity. The partial pressure of hydrogen is preferably 0.25-0.75 MPa, more preferably 0.50-0.75 MPa from the viewpoint of reactivity.
[0019] The molar ratio of carbon dioxide to hydrogen in the reactor feed is preferably 0.3-3, more preferably 0.5-1. In this reaction, carbon dioxide and hydrogen react to produce formic acid, and then ammonia addition and dehydration occur to produce formamide. Here, carbon dioxide and hydrogen are theoretically thought to react at a ratio of 1:1, and the molar ratio of carbon dioxide to hydrogen may be set to a ratio with a certain margin around that ratio, or the molar ratio may be set to 1.
[0020] The molar ratio of carbon dioxide to ammonia in the reactor feed is preferably 1-100, more preferably 10-30. Since ammonia easily reacts with carbon dioxide to inhibit the reaction process of producing ammonium carbamate, it is advisable to use a larger amount of carbon dioxide as the raw material.
[0021] The ammonia used may be diluted with nitrogen or a rare gas before being introduced into the reactor. In this case, the dilution ratio is preferably such that the ammonia content relative to the total gas is in the range of 1 to 10% by volume.
[0022] The ammonia used may be dissolved in an organic solvent, and the ammonia content in the entire solution is preferably in the range of 0.01 to 2 mol / L, more preferably in the range of 0.5 to 1 mol / L.
[0023] In the production method of this embodiment, an organic solvent can also be used. In that case, all common organic solvents can be used, and more preferably, nitriles such as acetonitrile and propionitrile, which are aprotic polar solvents, can be used. These can be used alone or in combination of two or more. The amount used is selected from the range of 0.1-1000 times, preferably 1-100 times, by mass relative to the substrate (ammonia). It is not necessary to use an organic solvent, and it is preferable not to use one since the reaction proceeds more efficiently.
[0024] For example, in the method of this embodiment, a solid catalyst is introduced into a pressure-resistant reactor, a previously prepared ethylene glycol solution of ammonia is introduced, and carbon dioxide and hydrogen are introduced therein at a predetermined pressure, respectively, and a reaction is carried out at a predetermined temperature. In this case, the solid catalyst becomes a catalyst-containing liquid mixed and dispersed in ethylene glycol, and by doing so, the reaction can be promoted by dissolving carbon dioxide in ethylene glycol and increasing the contact opportunity with the solid catalyst. Then, after the reaction is completed, the obtained formamide can be separated and taken out by distillation or chromatographic separation.
[0025] The reaction time in the production method of this embodiment depends on the amount of catalyst used, the reaction temperature, etc. and cannot be generally determined, but is usually within the range of 1 to 72 hours, preferably within the range of 2 to 5 hours. As described above, according to the present embodiment, formamide can be produced from carbon dioxide, hydrogen, and ammonia under mild conditions of low pressure and low temperature of 1 MPa or less and 160° C. or less, using an inexpensive solid catalyst which can be obtained by a relatively simple operation, without using a compound which serves as a nitrogen source and which requires complicated separation after the reaction, a transition metal complex catalyst which cannot be reused, or an expensive noble metal-supported solid catalyst. EXAMPLES
[0026] The present embodiment will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0027] Example 1 (Catalyst Preparation) A beaker was charged with an aqueous solution (200 mL) of 6 g of copper nitrate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), 52 g of zinc nitrate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and a basic aqueous solution (200 mL) of 33 g of potassium carbonate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and the resulting mixture was precipitated as copper and zinc oxide. The precipitate was filtered, dried overnight in an oven at 100°C, and then calcined at 500°C for 2 hours to obtain zinc oxide supported with 10% copper oxide (20 g). The obtained catalyst was measured by powder X-ray diffraction (XRD) (Figure 1) using a MiniFlex (registered trademark) 600 manufactured by Rigaku Corporation in the 2θ range of 20 to 80°, and it was confirmed that zinc oxide supported copper in a hexagonal wurtzite crystal structure. The catalyst was compressed and crushed at room temperature at 1 ton using a mini press machine, and then sieved to select catalysts with particle sizes of 355-710 micrometers.
[0028] Example 2 A catalyst was prepared in the same manner and under the same conditions as in Example 1, except that an aqueous solution containing 22 g of copper nitrate and 32 g of zinc nitrate was used, to obtain 40% copper oxide-supported zinc oxide (15 g).
[0029] Example 3 (Synthesis of formamide) As a pretreatment of the catalyst, 10% copper oxide-supported zinc oxide (Cu / ZnO) was produced by hydrogen treatment of the 10% copper oxide-supported zinc oxide prepared in Example 1. The hydrogen treatment was carried out by blowing nitrogen gas containing 10% hydrogen by volume into a MicrotrackBell Corporation Bellcat (registered trademark) II at 500°C for 2 hours at 50 mL per minute. Next, a glass test tube (volume 7.5 mL) was placed in a sealable autoclave (Taiatsu Glass Industry Co., Ltd., TVS-N2 type portable reactor, volume 12 mL), and 100 mg of hydrogen-treated 10% copper-supported zinc oxide was introduced into the glass test tube. 0.1 mL of a solution (i.e., 0.089 millimoles of ammonia) in which ammonia was dissolved in ethylene glycol (Fujifilm Wako Pure Chemical Industries Co., Ltd.) at a concentration of 0.89 mol / L was introduced thereinto, and carbon dioxide (Iwatani Gas Corporation) was sealed in the autoclave at a partial pressure of 0.5 MPa (2.45 millimoles, the molar ratio of carbon dioxide to ammonia is 27.5) and hydrogen (Taiyo Nippon Sanso Corporation) was sealed in the autoclave at a partial pressure of 0.5 MPa (2.45 millimoles, the molar ratio of carbon dioxide to hydrogen is 1) using a pressure gauge and a valved gas line, and the mixture was heated and stirred at 120°C for 3 hours. The ammonia-containing ethylene glycol liquid with a concentration of 0.89 mol / L was prepared by blowing helium gas (manufactured by Taiyo Nippon Sanso Co., Ltd.) containing 5% ammonia by volume into ethylene glycol at a rate of 50 mL per minute overnight. After the reaction, liquid phase chromatography measurement (Shimadzu Corporation, LC-20AD) was carried out under the following conditions. The mixture was developed at 40°C with 10 mM phosphoric acid solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and a TSKgel ODS100V (manufactured by Tosoh Corporation) was used as a column. Peaks were detected at a wavelength of 200 nm with UV (manufactured by Shimadzu Corporation, SPD-20A). The yield was calculated by comparing with a calibration curve based on a standard product. The yield of formamide was 0.97%.
[0030] The yield was calculated according to the following formula based on the results of liquid phase chromatography. Yield (%) = (number of moles of target compound / number of moles of ammonia used) x 100 Furthermore, unless otherwise noted, in the following examples and comparative examples, the same reagents (compounds) and methods as those in Example 3 were used.
[0031] Example 4 The reaction was carried out in the same manner and under the same conditions as in Example 3, except that 40% copper-supported zinc oxide (Cu / ZnO) (Example 2) was used instead of 10% copper-supported zinc oxide (Example 1). As a result, the yield of formamide was 0.71%.
[0032] (Examples 5-9) The reaction was carried out in the same manner and under the same conditions as in Example 3, except that the reaction temperature was changed to the range of 100-160° C. As a result, the yield of formamide was 0.26-1.38%. The results are shown in Table 1.
[0033] [Table 1]
[0034] (Examples 10-13) The reaction was carried out in the same manner and under the same conditions as in Example 7 (reaction temperature 140°C), except that the amount of catalyst of 10% copper-supported zinc oxide (Cu / ZnO) was changed in the range of 10-200 mg. As a result, the yield of formamide was 0.49-1.10%. The results are shown in Table 2.
[0035] [Table 2]
[0036] Example 14 Except for changing the reaction time to 72 hours, the reaction was carried out in the same manner and under the same conditions as in Example 3. As a result, the yield of formamide was 0.87%.
[0037] Comparative Example 1 Except for not adding 10% copper-supported zinc oxide, the reaction was carried out in the same manner and under the same conditions as in Example 3. As a result, the yield of formamide was 0%.
[0038] Comparative Example 2 The reaction was carried out under the same conditions as in Example 7, except that 0.1 mL of a 0.1 mol / L solution of ammonia in ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added instead of using a solution of ammonia dissolved in ethylene glycol. As a result, the yield of formamide was 0%.
[0039] Comparative Example 3 The reaction was carried out in the same manner and under the same conditions as in Example 7, except that 0.1 mL of a 0.1 mol / L solution of 1,2-propanediol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) containing ammonia was added in advance instead of using a solution in which ammonia was dissolved in ethylene glycol. As a result, the yield of formamide was 0%.
[0040] Comparative Example 4 The reaction was carried out in the same manner and under the same conditions as in Example 7, except that 0.1 mL of a 0.1 mol / L solution of 1,3-propanediol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) containing ammonia was added in advance instead of using a solution in which ammonia was dissolved in ethylene glycol. As a result, the yield of formamide was 0%.
[0041] Comparative Example 5 The reaction was carried out in the same manner and under the same conditions as in Example 7, except that 0.1 mL of a 0.1 mol / L solution of 1,4-butanediol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) containing ammonia was added in advance instead of using a solution in which ammonia was dissolved in ethylene glycol. As a result, the yield of formamide was 0%.
[0042] Comparative Example 6 The reaction was carried out in the same manner and under the same conditions as in Example 7, except that 100 mg (2.4 times the amount of 10% copper-supported zinc oxide in terms of copper equivalent) of copper(II) acetylacetonato complex (Sigma-Aldrich) was added as a copper complex having a carbonyl-based ligand, which is a homogeneous catalyst having the same copper as the active site, instead of 10% copper-supported zinc oxide. As a result, the yield of formamide was 0%.
[0043] Comparative Example 7 The reaction was carried out in the same manner and under the same conditions as in Example 7, except that 100 mg (2.2 times the amount of 10% copper-supported zinc oxide in terms of copper equivalent) of bis(1,3-propanediamine)copper(II) dichloride complex (manufactured by Tokyo Chemical Industry Co., Ltd.), a homogeneous catalyst with the same copper as the active site and an easily available copper complex having a diamino bidentate ligand, was added instead of 10% copper-supported zinc oxide. As a result, the yield of formamide was 0%.
[0044] Comparative Example 8 The reaction was carried out in the same manner and under the same conditions as in Example 7, except that, instead of 10% copper-supported zinc oxide (Example 1), 100 mg (2.0 times the amount of 10% copper-supported zinc oxide in terms of copper equivalent) of dichloro(1,10-phenanthroline)copper(II) complex (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a homogeneous catalyst with the same copper as the active site, which is an easily available and highly stable complex with an aromatic ring ligand. As a result, the yield of formamide was 0%.
[0045] The results of the above examples and comparative examples can be summarized as follows. (1) A method for producing formamide using carbon dioxide, hydrogen and ammonia as raw materials, in which formamide can be produced by using a solid catalyst in which copper is supported on zinc oxide together with ethylene glycol in a mixed system of the raw materials. (2) The amount of the solid catalyst used is preferably 10 to 200 mg, more preferably 50 to 100 mg, per 0.089 (about 0.1) millimole of ammonia. (3) The mixing ratio of copper to zinc oxide in the solid catalyst used is preferably 10-40%. (4) The temperature inside the reactor is preferably 100 to 160°C, particularly preferably 120 to 140°C. [Industrial Applicability]
[0046] Formamide is a functional chemical used as an intermediate raw material, solvent, etc. for pharmaceuticals, agricultural chemicals, and various organic chemicals. According to the present invention, formamide can be produced from carbon dioxide, hydrogen, and ammonia using an inexpensive solid catalyst that can be obtained by a relatively simple operation, without using a compound that serves as a nitrogen source that requires complicated separation after the reaction, a transition metal complex catalyst that cannot be reused, or an expensive precious metal solid catalyst. Therefore, the present invention can be mainly used for producing intermediate raw materials and solvents for pharmaceuticals, agricultural chemicals, and various organic chemicals.
Claims
1. A method for producing formamide using carbon dioxide, hydrogen and ammonia as raw materials, comprising the steps of: A method for producing formamide, comprising reacting the carbon dioxide, the hydrogen, and the ammonia in the presence of a solid catalyst in which copper metal is supported on zinc oxide, and ethylene glycol.
2. 2. The method for producing formamide according to claim 1, wherein the solid catalyst used is one in which the copper metal is contained in an amount of 10 to 40% by mass of the entire solid catalyst.
3. 3. The method for producing formamide according to claim 1, wherein the reaction is carried out under a pressure of 1 MPa or less.
4. The method for producing formamide according to claim 1 or 2, wherein the reaction is carried out at a temperature of 100 to 160°C.
5. A catalyst for producing formamide using carbon dioxide, hydrogen and ammonia as raw materials, characterized in that the catalyst is a solid catalyst in which copper metal is supported on zinc oxide.
6. 6. The catalyst for formamide synthesis according to claim 5, wherein the catalyst is a solid catalyst containing the copper metal in a proportion of 10 to 40% by mass of the entire solid catalyst.
7. A catalyst-containing liquid for use in formamide synthesis, comprising the catalyst for use in formamide synthesis according to claim 5 or 6 and ethylene glycol.
Citation Information
Patent Citations
Production of formamide
JP1977087112A
Method for making formamide using sodium diformylamide
JP2002534492A
Method for producing formamide and formic acid esters
JP2014523448A