Method for manufacturing toner binder

By esterifying an amorphous vinyl resin with a monohydric alcohol, the toner binder achieves a balance between low-temperature fixability and heat-resistant storage stability, enhancing long-term stability and document offset resistance.

JP2024161893APending Publication Date: 2024-11-20SANYO CHEM IND LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024071092
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-04-25
Publication Date
2024-11-20

AI Technical Summary

Technical Problem

Existing toner binders face a trade-off between low-temperature fixability and heat-resistant storage stability, with insufficient long-term stability and document offset properties, necessitating a solution that balances these properties.

Method used

The production of a toner binder involves esterifying an amorphous vinyl resin with a monohydric alcohol having 18 to 30 carbon atoms, reducing the amount of unreacted monomer and incorporating alkyl groups uniformly into the side chains, thereby improving long-term stability and document offset resistance.

Benefits of technology

The resulting toner binder achieves excellent low-temperature fixability, heat-resistant storage stability under high temperature and humidity, long-term stability, and charging stability, with improved document offset resistance after continuous printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161893000001
    Figure 2024161893000001
  • Figure 2024161893000002
    Figure 2024161893000002
  • Figure 2024161893000003
    Figure 2024161893000003
Patent Text Reader

Abstract

To provide a toner binder which is excellent in a low-temperature fixability, a heat-resistance storage property under a high-temperature and high-humidity environment, a long-term stability, and a document-resistant offset property and a charge stability after continuous printing.SOLUTION: A method for manufacturing a toner binder includes the step of esterification-reacting an amorphous vinyl resin (A) including a monomer with a carboxy group as a constituent monomer and a monovalent alcohol (B) with 18-30 carbons with each other, and preferably includes the step of reducing the pressure of the inside of the reaction system when the esterification reaction of (A) and (B) happens and / or after the esterification reaction of (A) and (B) happens.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a toner binder. [Background technology]

[0002] In recent years, along with the promotion of miniaturization, speedup, and high image quality of electrophotographic devices, from the viewpoint of energy saving, such as reducing energy consumption in the fixing process, there is a strong demand for improving the low-temperature fixability of toners. However, in general, when low-temperature fixability is improved, heat-resistant storage stability is reduced, and when heat-resistant storage stability is improved, low-temperature fixability is reduced. Therefore, there is a trade-off between low-temperature fixability and heat-resistant storage stability, and there is a demand for the development of a toner binder that can achieve both low-temperature fixability and heat-resistant storage stability. For example, in order to achieve both low-temperature fixability and heat-resistant storage stability, a toner composition containing a toner binder has been proposed that uses a combination of an amorphous resin and a crystalline resin in the binder resin, and that can improve low-temperature fixability while maintaining heat-resistant storage stability due to the melting properties of the crystalline resin (see Patent Documents 1 and 2). However, in the manufacturing method of the toner binder using the above-mentioned crystalline resin, the crystalline monomer or the synthetic raw material of the crystalline monomer remains in the toner binder at a certain concentration range, so that the long-term stability and the document offset property after continuous printing are not sufficient, and improvements in these respects are desired. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-77930 A [Patent Document 2] JP 2019-211763 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a toner binder which is excellent in low-temperature fixing property, heat-resistant storage stability under high temperature and high humidity conditions, long-term stability, document offset resistance after continuous printing, and charging stability.

[0005] The present inventors conducted extensive research to solve these problems and arrived at the present invention. That is, the present invention provides a method for producing a toner binder, comprising a step of esterifying an amorphous vinyl resin (A) containing a monomer having a carboxy group as a constituent monomer with a monohydric alcohol (B) having 18 to 30 carbon atoms. Effect of the Invention

[0006] The present invention makes it possible to provide a toner binder that is excellent in low-temperature fixing property, heat-resistant storage stability under high temperature and high humidity conditions, long-term stability, document offset resistance after continuous printing, and charging stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention will be described in detail below.

[0008] The method for producing a toner binder of the present invention includes a step of esterifying an amorphous vinyl resin (A) containing a monomer having a carboxy group as a constituent monomer with a monohydric alcohol (B) having 18 to 30 carbon atoms. The method for producing the toner binder of the present invention will be described below in detail.

[0009] In the toner binder manufacturing method of the present invention, by including a step of esterifying an amorphous vinyl resin (A) with a monohydric alcohol (B) having 18 to 30 carbon atoms, a toner binder is obtained in which an alkyl group having 18 to 30 carbon atoms is bonded to the side chain of the amorphous vinyl resin (A). The toner binder can reduce the amount of unreacted monomer remaining and incorporate the alkyl group having 18 to 30 carbon atoms relatively uniformly into the side chain compared to the case of using a crystalline vinyl resin containing a monomer having an alkyl group having 18 to 30 carbon atoms as a constituent monomer, and therefore the performance (particularly long-term stability and document offset property after continuous printing) of the toner using the toner binder obtained by this manufacturing method can be improved. In the present invention, "crystalline" means that in differential scanning calorimetry (also called DSC measurement), the DSC curve has an endothermic peak top temperature (Tm). In addition, in the present invention, "amorphous" means that when the transition temperature of a sample is measured using a differential scanning calorimeter, there is no endothermic peak top temperature. The method for measuring the peak top temperature (Tm) of the endothermic peak is described below. The measurement is performed using a differential scanning calorimeter (e.g., DSC Q20, manufactured by TA Instruments, Inc.). The sample is first heated from 30°C to 180°C at 10°C / min, then cooled from 180°C to 0°C at 10°C / min, and then heated a second time from 0°C to 180°C at 10°C / min. The top temperature of the endothermic peak during the second heating process is taken as the peak top temperature (Tm) of the endothermic peak.

[0010] [Amorphous vinyl resin (A)] The amorphous vinyl resin (A) is a polymer containing a monomer having a carboxy group as a constituent monomer, and is an amorphous vinyl resin.

[0011] Examples of the monomer having a carboxy group include unsaturated monocarboxylic acids and unsaturated dicarboxylic acids having 3 to 20 carbon atoms and anhydrides thereof. Specific examples of the vinyl monomer include carboxyl group-containing vinyl monomers such as acrylic acid, methacrylic acid, maleic acid (anhydride), maleic acid monoalkyl esters, fumaric acid, fumaric acid monoalkyl esters, crotonic acid, itaconic acid, itaconic acid monoalkyl esters, itaconic acid glycol monoether, citraconic acid, citraconic acid monoalkyl esters, and cinnamic acid.

[0012] Among the monomers having a carboxy group, from the viewpoint of low-temperature fixing property and charging stability, preferred are acrylic acid, methacrylic acid, maleic acid (anhydride), maleic acid monoalkyl esters, fumaric acid and fumaric acid monoalkyl esters, more preferred are acrylic acid, methacrylic acid, maleic acid (anhydride) and maleic acid monoalkyl esters, and even more preferred are acrylic acid and methacrylic acid.

[0013] The amorphous vinyl resin (A) may be used in combination with other monomers as required, for example, a monomer (c) other than the monomer having a carboxy group. The monomer (c) may be used alone or in combination of two or more kinds. Examples of the monomer (c) include vinyl hydrocarbons (c1), hydroxyl group-containing vinyl monomers (c2), nitrogen-containing vinyl monomers (c3), epoxy group-containing vinyl monomers (c4), halogen element-containing vinyl monomers (c5), and other ester monomers (c6).

[0014] Examples of the vinyl hydrocarbon (c1) include linear aliphatic vinyl hydrocarbons, alicyclic vinyl hydrocarbons, and aromatic vinyl hydrocarbons. Examples of the chain aliphatic vinyl hydrocarbon include alkenes and alkadienes. Specific examples of alkenes include ethylene, propylene, butene, isobutylene, pentene, heptene, diisobutylene, octene, dodecene, octadecene, and α-olefins other than those mentioned above. Specific examples of alkadienes include butadiene, isoprene, 1,4-pentadiene, 1,5-hexadiene, and 1,7-octadiene. Alicyclic vinyl hydrocarbons include mono- or di-cycloalkenes, and specific examples thereof include cyclohexene, (di)cyclopentadiene, vinylcyclohexene, ethylidenebicycloheptene, and terpenes (pinene, limonene, indene, etc.). Examples of aromatic vinyl hydrocarbons include styrene and its hydrocarbyl (alkyl, cycloalkyl, aralkyl and / or alkenyl) substituted derivatives, and specific examples thereof include α-methylstyrene, vinyltoluene, 2,4-dimethylstyrene, ethylstyrene, isopropylstyrene, butylstyrene, phenylstyrene, cyclohexylstyrene, benzylstyrene, crotylbenzene, divinylbenzene, divinyltoluene, divinylxylene, trivinylbenzene, and vinylnaphthalene.

[0015] Examples of the hydroxyl group-containing vinyl monomer (c2) include hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate (e.g., 2-hydroxyethyl acrylate), hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)allyl alcohol, crotyl alcohol, isocrotyl alcohol, 1-buten-3-ol, 2-buten-1-ol, 2-butene-1,4-diol, propargyl alcohol, 2-hydroxyethyl propenyl ether, and sucrose allyl ether.

[0016] Examples of the nitrogen-containing vinyl monomer (c3) include an amino group-containing vinyl monomer, an amide group-containing vinyl monomer, a quaternary ammonium cation group-containing vinyl monomer, and a nitro group-containing vinyl monomer. Examples of the amino group-containing vinyl monomer include aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, t-butylaminoethyl methacrylate, N-aminoethyl (meth)acrylamide, (meth)allylamine, morpholinoethyl (meth)acrylate, 4-vinylpyridine, 2-vinylpyridine, crotylamine, N,N-dimethylaminostyrene, methyl α-acetaminoacrylate, vinylimidazole, N-vinylpyrrole, N-vinylthiopyrrolidone, N-arylphenylenediamine, aminocarbazole, aminothiazole, aminoindole, aminopyrrole, aminoimidazole, aminomercaptothiazole, and salts thereof. Examples of the amide group-containing vinyl monomer include (meth)acrylamide, N-methyl(meth)acrylamide, N-butylacrylamide, diacetone acrylamide, N-methylol(meth)acrylamide, N,N'-methylene-bis(meth)acrylamide, N,N-dimethylacrylamide, methacrylformamide, N-methyl-N-vinylacetamide, N-vinyl-2-pyrrolidone, N-vinylpiperidone, and N-vinylcaprolactam. Examples of the vinyl monomer containing a quaternary ammonium cation group include quaternized products of tertiary amine group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and diallylamine (which are quaternized using a quaternizing agent such as methyl chloride, dimethyl sulfate, benzyl chloride, or dimethyl carbonate). Nitro group-containing vinyl monomers include nitrostyrene.

[0017] Examples of the cyclic ether group-containing vinyl monomer (c4) include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and p-vinylphenylpropylene oxide.

[0018] Examples of the halogen-containing vinyl monomer (c5) include vinyl chloride, vinyl bromide, vinylidene chloride, allyl chloride, chlorostyrene, bromostyrene, dichlorostyrene, chloromethylstyrene, tetrafluorostyrene, and chloroprene.

[0019] Examples of other ester monomers (c6) include alkyl (meth)acrylates having an alkyl group with a carbon number of 1 to 40 [methyl (meth)acrylate (methyl (meth)acrylate), butyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate (stearyl (meth)acrylate), nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, montanyl (meth)acrylate, triacontyl (meth)acrylate, dotriacontyl (meth)acrylate, and the like], alkylene ether (meth)acrylates having a carbon number of 5 to 30 [methoxy-triethylene glycol (meth)acrylate, ethoxy-diethylene glycol (meth)acrylate, methoxy-polyethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, etc.], polyfunctional (meth)acrylates [poly(meth)acrylates of polyhydric alcohols such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and polyethylene glycol di(meth)acrylate, etc.], aliphatic vinyl esters having 4 to 15 carbon atoms and aromatic vinyl esters having 9 to 15 carbon atoms [vinyl acetate, vinyl butyrate, vinyl propionate, vinyl butyrate, and methyl-4-vinyl benzoate, etc.].

[0020] Among these monomers (c), from the viewpoints of long-term stability and charging stability, preferred are vinyl hydrocarbons (c1) and nitrogen-containing vinyl monomers (c3), and more preferred are aromatic vinyl hydrocarbons and amide group-containing vinyl monomers.

[0021] From the viewpoints of low-temperature fixing property, heat-resistant storage stability under high temperature and high humidity, long-term stability, and document offset resistance after continuous printing, the amorphous vinyl resin (A) preferably contains 4 to 50% by weight, more preferably 4 to 30% by weight, of a monomer having a carboxyl group as a constituent monomer based on the weight of all constituent monomers of the amorphous vinyl resin (A). When the weight ratio of the monomer having a carboxyl group is 4% by weight or more, the low-temperature fixing property and heat-resistant storage stability under high temperature and high humidity are improved. On the other hand, when the weight ratio of the monomer having a carboxyl group is 50% by weight or less, the long-term stability and document offset resistance after continuous printing are improved.

[0022] When the amorphous vinyl resin (A) contains other monomers as constituent monomers, the content thereof is preferably 50 to 96% by weight, more preferably 70 to 96% by weight, based on the weight of all constituent monomers of the amorphous vinyl resin (A).

[0023] The amorphous vinyl resin (A) can be produced by polymerizing a monomer composition by a known method (e.g., radical polymerization, anionic polymerization, cationic polymerization, living radical polymerization, living anionic polymerization, living cationic polymerization, etc.). In the case of radical polymerization, for example, the resin can be synthesized by a solution polymerization method (e.g., JP-A-5-117330) in which the monomer is reacted with a radical reaction initiator (d) in a solvent (e.g., toluene). The radical reaction initiator may be a known radical reaction initiator (d). The radical reaction initiator (d) is not particularly limited, and examples thereof include inorganic peroxides (d1), organic peroxides (d2), and azo compounds (d3). These radical reaction initiators may also be used in combination.

[0024] The inorganic peroxide (d1) is not particularly limited, but examples thereof include hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate.

[0025] The organic peroxide (d2) is not particularly limited, and examples thereof include benzoyl peroxide, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, α,α-bis(t-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di-t-butylperoxyhexyne-3, acetyl peroxide, isobutyryl peroxide, octanyl peroxide, decanolyl peroxide, Examples of peroxyalkylene oxides include lauroyl peroxide, 3,3,5-trimethylhexanoyl peroxide, m-toluyl peroxide, t-butyl peroxyisobutyrate, t-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxy-3,5,5-trimethylhexanoate, t-butyl peroxylaurate, t-butyl peroxybenzoate, t-butyl peroxyisopropyl monocarbonate, and t-butyl peroxyacetate.

[0026] The azo compound (d3) is not particularly limited, but examples thereof include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, 2,2'-azobis(2-methylbutyronitrile), and azobisisobutyronitrile.

[0027] The weight average molecular weight of the amorphous vinyl resin (A) in the present invention, as measured by gel permeation chromatography (GPC), is preferably from 2,000 to 200,000, more preferably from 5,000 to 100,000, even more preferably from 10,000 to 70,000, and particularly preferably from 20,000 to 50,000, from the viewpoints of low-temperature fixability and document offset resistance after continuous printing.

[0028] In the present invention, the number average molecular weight (hereinafter sometimes abbreviated as Mn) and weight average molecular weight (hereinafter sometimes abbreviated as Mw) of the crystalline vinyl resin (A) can be measured using GPC under the following conditions. Equipment (example): HLC-8120 [Tosoh Corporation] Column (example): 2 TSK GEL GMH6 [Tosoh Corporation] Measurement temperature: 40℃ Sample solution: 0.25% by weight in THF Mobile phase: Tetrahydrofuran (no polymerization inhibitor) Solution injection volume: 100μL Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weights: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation] For measuring the molecular weight, a sample is dissolved in tetrahydrofuran (hereinafter abbreviated as THF) to a concentration of 0.25% by weight, and the insoluble matter is filtered off using a glass filter to obtain a sample solution. Incidentally, for the toner binder described later, Mn and Mw can be determined in the same manner as above.

[0029] The glass transition temperature (Tg) of the amorphous vinyl resin (A) in the present invention is preferably 30 to 130° C., more preferably 40 to 125° C., and further preferably 50 to 120° C., from the viewpoints of low-temperature fixability and heat-resistant storage stability under high-temperature and high-humidity conditions. The glass transition temperature can be measured, for example, by the method specified in ASTM D3418-82 (DSC method) using DSC Q20 manufactured by TA Instruments Co., Ltd.

[0030] The acid value of the amorphous vinyl resin (A) in the present invention is preferably 20 to 400 mgKOH / g, more preferably 70 to 390 mgKOH / g, from the viewpoint of reactivity and charge stability. The acid value of the amorphous vinyl resin (A) can be adjusted by the acid value of the monomer and the content of the monomer having an acid value. The acid value of (A) can be measured, for example, by a method such as JIS K 0070.

[0031] [Monohydric alcohols with carbon numbers of 18 to 30 (B)] The monohydric alcohol (B) having 18 to 30 carbon atoms is not particularly limited as long as it has 18 to 30 carbon atoms and one hydroxyl group. The alcohol may be any of primary, secondary and tertiary alcohols, but from the viewpoint of reactivity, primary alcohols are preferred. The monohydric alcohol (B) having 18 to 30 carbon atoms may be used alone or in combination of two or more kinds.

[0032] Examples of the monohydric alcohol (B) having 18 to 30 carbon atoms include alcohols having a straight-chain alkyl group and alcohols having a branched alkyl group. Examples of alcohols having a straight-chain alkyl group include 1-octadecanol (stearyl alcohol), 1-nonadecanol, 1-icosanol, 1-heneicosanol, 1-docosanol (behenyl alcohol), 1-tetracosanol, and 1-triacontanol. An example of the alcohol having a branched alkyl group is 2-decyl-1-tetradecanol.

[0033] Among these monohydric alcohols (B) having 18 to 30 carbon atoms, preferred are monohydric alcohols having a linear alkyl group, more preferred are monohydric alcohols having 18 to 24 carbon atoms, and even more preferred is 1-docosanol (behenyl alcohol). If the carbon number of the monohydric alcohol is less than 18, the heat resistance storage stability under high temperature and high humidity conditions may be poor, whereas if it exceeds 30, the low temperature fixability may be poor.

[0034] [Esterification reaction] The esterification reaction in the production method of the present invention is not particularly limited as long as it is a reaction in which a carboxy group portion of an amorphous vinyl resin (A) containing a monomer having a carboxy group as a constituent monomer and a hydroxy group portion of a monohydric alcohol (B) having 18 to 30 carbon atoms are condensed. For example, a method in which a monomer composition (A0) containing a monomer having a carboxy group, which is a constituent monomer of the amorphous vinyl resin (A), is mixed in advance with a monohydric alcohol (B) having 18 to 30 carbon atoms, and an esterification reaction is carried out while obtaining an amorphous vinyl resin (A) in the presence of the monohydric alcohol (B) having 18 to 30 carbon atoms, or a method in which a monomer composition (A0) containing a monomer having a carboxy group is polymerized to obtain an amorphous vinyl resin (A), and then the amorphous vinyl resin (A) is mixed with a monohydric alcohol (B) having 18 to 30 carbon atoms for esterification, can be mentioned.

[0035] The esterification reaction can be carried out in a sealed vessel at a temperature of preferably 120 to 280° C., more preferably 130 to 230° C., and even more preferably 140 to 180° C. From the viewpoint of ensuring that the esterification reaction is carried out, the reaction time is preferably 30 minutes or more, more preferably 2 to 40 hours. From the viewpoint of reactivity (dehydration), it is preferable to have a step of reducing the pressure in the reaction system during and / or after the esterification reaction, and the degree of reduced pressure is preferably 20 kPa or less, more preferably 15 kPa or less, even more preferably 10 kPa or less, and particularly preferably 5 kPa or less. From the viewpoints of low-temperature fixability and heat-resistant storage stability under high temperature and high humidity, the reaction rate of the esterification reaction is preferably 90% or more, more preferably 95%, and particularly preferably 97% or more. The reaction rate of the esterification reaction can be determined by measuring the content of the monohydric alcohol (B) having 18 to 30 carbon atoms before and after the reaction.

[0036] In this case, an esterification catalyst can be used as necessary. Examples of the esterification catalyst include tin-containing catalysts (e.g., dibutyltin oxide, etc.), antimony trioxide, titanium-containing catalysts [e.g., titanium alkoxide, potassium oxalate titanate, titanium terephthalate, titanium alkoxide terephthalate, catalysts described in JP-A-2006-243715 (titanium diisopropoxybistriethanolaminate, titanium dihydroxybistriethanolaminate, titanium monohydroxytriethanolaminate, titanyl bistriethanolaminate, and intramolecular polycondensates thereof, etc.), and catalysts described in JP-A-2007-11307 (titanium tributoxyterephthalate, titanium triisopropoxyterephthalate, titanium diisopropoxyditerephthalate, etc.)], zirconium-containing catalysts (e.g., zirconyl acetate, etc.), and zinc acetate. Among the esterification catalysts, titanium-containing catalysts are preferred from the viewpoint of reaction efficiency, and titanium alkoxides are more preferred.

[0037] The content of the esterification catalyst is preferably 0.1 to 10% by weight, more preferably 0.2 to 5% by weight, based on the weight of the amorphous vinyl resin (A) from the viewpoint of reaction efficiency.

[0038] The weight ratio of the amorphous vinyl resin (A) to the monohydric alcohol (B) having 18 to 30 carbon atoms before the esterification reaction [(A):(B)] is preferably 30:70 to 70:30 from the viewpoints of low-temperature fixability, heat-resistant storage stability under high-temperature and high-humidity conditions, long-term stability, and charging stability. The proportion of the monomer having a carboxy group that is esterified with the monohydric alcohol (B) having 18 to 30 carbon atoms is preferably 60% to 95% based on the number of moles of the monomer having a carboxy group, from the viewpoint of reactivity (the content of the crystalline monomer or the crystalline monomer synthesis raw material). The weight ratio of the monomer having a carboxy group, which is a component of the amorphous vinyl resin (A), to the monohydric alcohol (B) having 18 to 30 carbon atoms [(monomer having a carboxy group):(B)] before the ester exchange reaction is preferably 5:95 to 95:5, and more preferably 20:80 to 80:20, from the viewpoints of low-temperature fixability, heat-resistant storage stability under high-temperature and high-humidity conditions, long-term stability, and charging stability.

[0039] [Toner binder] The toner binder obtained by the present invention is a toner binder containing a resin obtained by an esterification reaction between an amorphous vinyl resin (A) and a monohydric alcohol (B) having 18 to 30 carbon atoms. The toner binder obtained by the present invention may contain other resins known as resins for toner binders (such as the polymers described in JP-A-06-194876). The other resins may be one type of resin or a mixture of two or more types of resins.

[0040] The toner binder obtained by the present invention preferably has at least one endothermic peak top temperature (Tm) in the range of 45 to 100° C. When Tm is in this range, the toner binder has a good balance between low-temperature fixability and heat-resistant storage stability under high-temperature and high-humidity conditions. Tm is more preferably 50 to 90° C. The endothermic peak top temperature (Tm) of the toner binder can be adjusted by the type and composition ratio of the monomer constituting the crystalline vinyl resin (for example, by adjusting the carbon number of the monohydric alcohol (B) having 18 to 30 carbon atoms that reacts with the monomer having a carboxy group and by adjusting the weight ratio of the alcohol (B) constituting the crystalline vinyl resin), the weight average molecular weight, etc. For example, the endothermic peak top temperature of the toner binder can be increased by increasing the carbon number of the alcohol (B) or increasing the weight ratio of the alcohol (B). However, the peak top temperature (Tm) of the endothermic peak is measured using a differential scanning calorimeter (e.g., DSC Q20, manufactured by TA Instruments, Inc.) and is the peak top temperature of the endothermic peak during the second heating process when the toner binder is heated for the first time from 20°C to 150°C at a rate of 10°C / min, then cooled to 0°C at a rate of 10°C / min, and then heated for the second time from 0°C to 150°C at a rate of 10°C / min.

[0041] The weight average molecular weight (Mw) of the toner binder obtained by the present invention is preferably 5,000 to 200,000, more preferably 10,000 to 200,000, still more preferably 20,000 to 200,000, and particularly preferably 30,000 to 150,000, from the viewpoint of achieving both hot offset resistance of the toner and document offset resistance after continuous printing. The weight average molecular weight of the toner binder can be measured by the same method and conditions as those for the crystalline vinyl resin (A).

[0042] The acid value of the toner binder obtained by the present invention is preferably from 0 to 40 mgKOH / g, more preferably from 0 to 30 mgKOH / g, from the viewpoint of the charge stability of the toner. The acid value of the toner binder can be measured by the same method and conditions as those for the amorphous vinyl resin (A).

[0043] The content of unreacted monohydric alcohol (B) having 18 to 30 carbon atoms in the toner binder is preferably 5% by weight or less, more preferably 4% by weight or less, and even more preferably 3% by weight or less, from the viewpoints of low-temperature fixability and heat-resistant storage stability under high-temperature and high-humidity conditions.

[0044] [toner] The toner binder obtained by the production method of the present invention can be used as a material for toner. When producing a toner using the toner binder obtained by the production method of the present invention, one or more known additives selected from a colorant, a release agent, a charge control agent, a fluidizing agent, etc. can be used as necessary in addition to the toner binder.

[0045] As the colorant, all of the dyes and pigments used as toner colorants can be used. For example, carbon black, iron black, Sudan Black SM, Fast Yellow G, Benzidine Yellow, Pigment Yellow, India Fast Orange, Irgasin Red, Paranitroaniline Red, Toluidine Red, Carmine FB, Pigment Orange R, Lake Red 2G, Rhodamine FB, Rhodamine B Lake, Methyl Violet B Lake, Phthalocyanine Blue, Pigment Blue, Brilliant Green, Phthalocyanine Green, Oil Yellow GG, Kayaset YG, Orazol Brown B, and Oil Pink OP can be mentioned, and the colorant may be a single one or a mixture of two or more kinds. In addition, if necessary, magnetic powder (powder of ferromagnetic metals such as iron, cobalt, nickel, etc., or compounds such as magnetite, hematite, and ferrite) can be contained to function as a colorant.

[0046] For the release agent, the flow softening point (T 1 / 2

[0033] is preferably 50 to 170°C, and examples thereof include aliphatic hydrocarbon waxes such as polyolefin wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax, and oxides thereof, carnauba wax, montan wax, and deacidified waxes thereof, ester wax, fatty acid amides, fatty acids, higher alcohols, fatty acid metal salts, and mixtures thereof.

[0047] Flow softening point [T 1 / 2 The measurement method of is described below. Using a constant test force extrusion capillary rheometer flow tester {e.g., Shimadzu Corporation, CFT-500D}, 1 g of the test sample is heated at a temperature increase rate of 6°C / min. At this time, a load of 1.96 MPa is applied by the plunger, and the sample is extruded from a nozzle with a diameter of 1 mm and a length of 1 mm. A graph of "plunger drop (flow value)" vs. "temperature" is drawn, and the temperature corresponding to half the maximum value of the plunger drop is taken as the flow softening point [T1 / 2 〕

[0048] Examples of polyolefin waxes include (co)polymers of olefins (e.g., ethylene, propylene, 1-butene, isobutylene, 1-hexene, 1-dodecene, 1-octadecene, and mixtures thereof) [including those obtained by (co)polymerization and those obtained by further thermal degradation thereof] (e.g., low molecular weight polypropylene, low molecular weight polyethylene, low molecular weight polypropylene-polyethylene copolymer), oxides of olefin (co)polymers with oxygen and / or ozone, maleic acid modified products of olefin (co)polymers [e.g., maleic acid and its derivatives (maleic anhydride, monomethyl maleate, monobutyl maleate, dimethyl maleate, etc.) modified products], copolymers of olefins and unsaturated carboxylic acids [(meth)acrylic acid, itaconic acid, maleic anhydride, etc.] and / or unsaturated carboxylic acid alkyl esters [(meth)acrylic acid alkyl (alkyl having 1 to 18 carbon atoms) esters and maleic acid alkyl (alkyl having 1 to 18 carbon atoms) esters, etc.], and the like.

[0049] Examples of microcrystalline waxes include Hi-Mic-2095, Hi-Mic-1090, Hi-Mic-1080, Hi-Mic-1070, Hi-Mic-2065, Hi-Mic-1045, and Hi-Mic-2045 manufactured by Nippon Seiro Co., Ltd.

[0050] Examples of paraffin waxes include Paraffin WAX-155, Paraffin WAX-150, Paraffin WAX-145, Paraffin WAX-140, Paraffin WAX-135, HNP-3, HNP-5, HNP-9, HNP-10, HNP-11, HNP-12, and HNP-51, manufactured by Nippon Seiro Co., Ltd.

[0051] Examples of Fischer-Tropsch wax include Sasolwax C80 manufactured by Sasol and FT-0070 manufactured by Nippon Seiro Co., Ltd.

[0052] An example of carnauba wax is Refined Carnauba Wax Special No. 1 manufactured by Kato Yoko Co., Ltd.

[0053] Examples of the ester wax include fatty acid ester waxes (for example, Nissan Electol WEP-2, WEP-3, WEP-4, WEP-5, and WEP-8 manufactured by NOF Corporation).

[0054] The higher alcohols include aliphatic alcohols having 30 to 50 carbon atoms, such as triacontanol. The fatty acids include fatty acids having 30 to 50 carbon atoms, such as triacontancarboxylic acid.

[0055] Examples of fatty acid amides include Diamid Y and Diamid 200 manufactured by Mitsubishi Chemical Corporation.

[0056] The charge control agent may be either a positively charged charge control agent or a negatively charged charge control agent, and examples of the charge control agent include nigrosine dyes, triphenylmethane dyes containing a tertiary amine as a side chain, quaternary ammonium salts, polyamine resins, imidazole derivatives, polymers containing a quaternary ammonium base, metal-containing azo dyes, copper phthalocyanine dyes, metal salicylic acid salts, boron complexes of benzilic acid, sulfonic acid group-containing polymers, fluorine-containing polymers, and halogen-substituted aromatic ring-containing polymers.

[0057] Examples of the fluidizing agent include silica, titania, alumina, calcium carbonate, fatty acid metal salt, silicone resin particles, and fluororesin particles, and two or more of them may be used in combination. From the viewpoint of the chargeability of the toner, silica is preferred. From the viewpoint of the transferability of the toner, the silica is preferably hydrophobic silica. From the viewpoint of the transferability of the toner, the silica is preferably hydrophobic silica.

[0058] The content of the toner binder in the toner is preferably 30 to 97% by weight, more preferably 40 to 95% by weight, and further preferably 45 to 92% by weight, based on the weight of the toner. The content of the colorant is preferably 0.05 to 60% by weight, more preferably 0.1 to 55% by weight, and further preferably 0.5 to 50% by weight, based on the weight of the toner. The content of the release agent is preferably 0 to 30% by weight, more preferably 0.5 to 20% by weight, and further preferably 1 to 10% by weight, based on the weight of the toner. The content of the charge control agent is preferably 0 to 20% by weight, more preferably 0.1 to 10% by weight, and further preferably 0.5 to 7.5% by weight, based on the weight of the toner. The content of the fluidizing agent is preferably 0 to 10% by weight, more preferably 0 to 5% by weight, and further preferably 0.1 to 4% by weight, based on the weight of the toner. The total content of the additives is preferably 3 to 70% by weight, more preferably 4 to 58% by weight, and further preferably 5 to 50% by weight, based on the toner weight.

[0059] The toner containing the toner binder obtained by the present invention may be obtained by any of known methods such as a kneading and pulverizing method, an emulsion phase inversion method, an emulsion polymerization method, a suspension polymerization method, a solution suspension method, and an emulsion aggregation method. For example, when a toner is obtained by a kneading and pulverizing method, the components constituting the toner except for the fluidizing agent are dry-blended using a Henschel mixer, a Nauta mixer, a Banbury mixer, or the like, and then melt-kneaded using a continuous mixing device such as a twin-screw kneader, an extruder, a continuous kneader, or a three-roll mill, and then coarsely pulverized using a mill or the like, and finally micronized using an air flow type micropulverizer, or the like, and further adjusted in particle size distribution using a classifier such as an elbow jet to form toner particles [preferably particles having a volume average particle size (D50) of 5 to 20 μm], and then the fluidizing agent can be mixed therein to produce the toner.

[0060] The volume average particle size (D50) of the toner particles (toner) can be measured using a Coulter counter [for example, trade name: Multisizer III (manufactured by Beckman Coulter, Inc.)]. Specifically, 0.1 to 5 mL of a surfactant (alkylbenzene sulfonate) is added as a dispersant to 100 to 150 mL of an electrolyte solution, ISOTON-II (manufactured by Beckman Coulter). 2 to 20 mg of a measurement sample is then added, and the electrolyte solution in which the sample is suspended is dispersed for approximately 1 to 3 minutes using an ultrasonic disperser. The volume and number of toner particles are measured using a 50 μm aperture with the measurement device, and the volume distribution and number distribution are calculated. From the distribution obtained, the volume average particle size (D50) (μm), number average particle size (μm), and particle size distribution (volume average particle size / number average particle size) of the toner particles are obtained.

[0061] In addition, when the toner is obtained by the emulsion phase inversion method, the components constituting the toner except for the fluidizing agent are dissolved or dispersed in an organic solvent, and then emulsified by adding water or the like, followed by separation and classification to produce the toner. The volume average particle size of the toner is preferably 3 to 15 μm. The toner containing the toner binder obtained by the manufacturing method of the present invention is mixed with carrier particles such as iron powder, glass beads, nickel powder, ferrite, magnetite, and ferrite coated with resin (acrylic resin, silicone resin, etc.) as necessary, and used as a developer for an electric latent image. When carrier particles are used, the weight ratio of the toner to the carrier particles is preferably 1 / 99 to 99 / 1. Also, the toner can be rubbed against a member such as a charging blade instead of the carrier particles to form an electric latent image. The toner containing the toner binder obtained by the production method of the present invention may be in an embodiment that does not contain carrier particles.

[0062] The toner containing the toner binder obtained by the production method of the present invention is fixed to a support (paper, polyester film, etc.) by a copier, printer, etc. to form a recording material. As a method for fixing to a support, a known heat roll fixing method, flash fixing method, etc. can be used.

[0063] The toner produced by using the toner binder obtained by the production method of the present invention is used for developing electrostatic images or magnetic latent images in electrophotography, electrostatic recording, electrostatic printing, etc. More specifically, it is used for developing electrostatic images or magnetic latent images that are particularly suitable for full color. EXAMPLES

[0064] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following, "parts" refers to parts by weight unless otherwise specified.

[0065] <Production Example 1> [Production of amorphous vinyl resin (A-1)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while the autoclave was sealed under stirring, and then the pressure was released, and the temperature was raised to 170°C while the autoclave was sealed under stirring. A mixed solution of 300.0 parts of styrene, 225.0 parts of acrylic acid, 225.0 parts of N-vinyl-2-pyrrolidone, and 1.5 parts of di-t-butyl peroxide was dropped over 3 hours while controlling the temperature inside the autoclave to 170°C, and polymerization was carried out. After dropping, the dropping line was washed with 15.0 parts of xylene. After maintaining the same temperature for another 0.5 hours, the reaction rate of acrylic acid was confirmed after cooling to 130°C. Since the reaction rate of acrylic acid was less than 98%, 1.9 parts of di-t-butyl peroxide was further added and reacted until the reaction rate reached 98% or more. The solvent was removed at 170°C for 3 hours under reduced pressure of 0.5 to 2.5 kPa to obtain amorphous vinyl resin (A-1).

[0066] <Production Example 2> [Production of amorphous vinyl resin (A-2)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while the autoclave was sealed under stirring, and then the pressure was released, and the temperature was raised to 170°C while the autoclave was sealed under stirring. A mixed solution of 225.0 parts of styrene, 375.0 parts of acrylic acid, 150.0 parts of N-vinyl-2-pyrrolidone, and 1.5 parts of di-t-butyl peroxide was dropped over 3 hours while controlling the temperature inside the autoclave to 150°C, and polymerization was carried out. After dropping, the dropping line was washed with 15.0 parts of xylene. After maintaining the same temperature for 3.7 hours, the reaction rate of acrylic acid was confirmed after cooling to 130°C. Since the reaction rate of acrylic acid was less than 98%, 1.9 parts of di-t-butyl peroxide was further added and reacted until the reaction rate reached 98% or more. The solvent was removed at 170°C for 3 hours under reduced pressure of 0.5 to 2.5 kPa to obtain amorphous vinyl resin (A-2).

[0067] <Production Example 3> [Production of amorphous vinyl resin (A-3)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while the autoclave was sealed under stirring, and then the pressure was released, and the temperature was raised to 170°C while the autoclave was sealed under stirring. A mixed solution of 412.5 parts of styrene, 75.0 parts of acrylic acid, 262.5 parts of N-vinyl-2-pyrrolidone, and 1.5 parts of di-t-butyl peroxide was dropped over 3 hours while controlling the temperature inside the autoclave to 170°C, and polymerization was carried out. After dropping, the dropping line was washed with 15.0 parts of xylene. After maintaining the same temperature for another 0.5 hours, the reaction rate of acrylic acid was confirmed after cooling to 130°C. Since the reaction rate of acrylic acid was less than 98%, 1.9 parts of di-t-butyl peroxide was further added and reacted until the reaction rate was 98% or more. The solvent was removed at 170°C for 3 hours under reduced pressure of 0.5 to 2.5 kPa to obtain amorphous vinyl resin (A-3).

[0068] <Production Example 4> [Production of amorphous vinyl resin (A-4)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while the autoclave was sealed under stirring, and then the pressure was released, and the temperature was raised to 170°C while the autoclave was sealed under stirring. A mixed solution of 375.0 parts of styrene, 30.0 parts of acrylic acid, 262.5 parts of N-vinyl-2-pyrrolidone, 82.5 parts of butyl acrylate, and 1.5 parts of di-t-butyl peroxide was dropped over 3 hours while controlling the temperature inside the autoclave to 170°C, and polymerization was carried out. After dropping, the dropping line was washed with 15.0 parts of xylene. After holding at the same temperature for another 0.5 hours, the reaction rate of acrylic acid was confirmed after cooling to 130°C. Since the reaction rate of acrylic acid was less than 98%, 1.9 parts of di-t-butyl peroxide was further added and reacted until the reaction rate was 98% or more. The solvent was removed at 170° C. for 3 hours under a reduced pressure of 0.5 to 2.5 kPa to obtain an amorphous vinyl resin (A-4).

[0069] <Production Example 5> [Production of amorphous vinyl resin (A-5)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while the autoclave was sealed under stirring, and then the pressure was released, and the temperature was raised to 170°C while the autoclave was sealed under stirring. A mixed solution of 255.0 parts of styrene, 270.0 parts of methacrylic acid, 225.0 parts of N-vinyl-2-pyrrolidone, and 1.5 parts of di-t-butyl peroxide was dropped over 3 hours while controlling the temperature inside the autoclave to 170°C, and polymerization was carried out. After dropping, the dropping line was washed with 15.0 parts of xylene. After holding at the same temperature for another 0.5 hours, the reaction rate of methacrylic acid was confirmed after cooling to 130°C. Since the reaction rate of methacrylic acid was less than 98%, 1.9 parts of di-t-butyl peroxide was further added and reacted until the reaction rate was 98% or more. The solvent was removed at 170° C. for 3 hours under a reduced pressure of 0.5 to 2.5 kPa to obtain an amorphous vinyl resin (A-5).

[0070] <Production Example 6> [Production of amorphous vinyl resin (A-6)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while stirring and sealed, and then the pressure was released, and the temperature was raised to 170°C while stirring and sealed. A mixed solution of 300.0 parts of styrene, 225.0 parts of acrylic acid, 225.0 parts of N,N-dimethylacrylamide, and 1.5 parts of di-t-butyl peroxide was dropped over 3 hours while controlling the temperature inside the autoclave to 170°C, and polymerization was carried out. After dropping, the dropping line was washed with 15.0 parts of xylene. After maintaining the same temperature for another 0.5 hours, it was cooled to 130°C and the reaction rate of acrylic acid was confirmed. Since the reaction rate of acrylic acid was less than 98%, 1.9 parts of di-t-butyl peroxide was further added and reacted until the reaction rate was 98% or more. The solvent was removed at 170°C for 3 hours under reduced pressure of 0.5 to 2.5 kPa to obtain amorphous vinyl resin (A-6).

[0071] The compositions and physical properties of the amorphous vinyl resins (A-1) to (A-6) obtained in Production Examples 1 to 6 are shown in Table 1.

[0072] [Table 1]

[0073] <Comparative Production Example 1> [Production of Crystalline Vinyl Resin (A'-1)] 235.0 parts of xylene was charged into the autoclave, and the temperature was raised to 135°C while the autoclave was sealed under stirring, and then the pressure was released, and the temperature was raised to 170°C while the autoclave was sealed under stirring. A mixed solution of 468.8 parts of docosyl acrylate, 147.8 parts of styrene, 111.0 parts of N-vinyl-2-pyrrolidone, 22.5 parts of acrylic acid, and 1.5 parts of di-t-butyl peroxide was adjusted to 50°C, and the temperature inside the autoclave was controlled to 150°C, while dropping the mixture over 3 hours to polymerize. After dropping, the dropping line was washed with 15.0 parts of xylene. After holding at the same temperature for another 3.7 hours, the mixture was cooled to 70°C, and the reaction rate of docosyl acrylate was confirmed. Since the reaction rate of docosyl acrylate was less than 98%, 1.5 parts of di-t-butyl peroxide was further added and reacted until the reaction rate reached 98% or more. The solvent was removed at 170°C for 3 hours under reduced pressure of 0.5 to 2.5 kPa to obtain a crystalline vinyl resin (A'-1). The endothermic peak top temperature (Tm) of the crystalline vinyl resin (A'-1) was 61°C, the weight average molecular weight (Mw) was 33,000, and the acid value was 21 mgKOH / g.

[0074] [Table 2]

[0075] <Example 1> [Production of toner binder (C-1)] 48.0 parts of amorphous vinyl resin (A-1), 52.0 parts of 1-docosanol, and 0.2 parts of titanium tetrabutoxide were added to a pressurized reaction vessel equipped with a stirrer, a heating / cooling device, a thermometer, an air inlet tube, a pressure reducing device, and a water reducing device, and then the temperature was raised to 150°C in a sealed state with stirring. The reaction was carried out for 3 hours while the temperature inside the reaction vessel was maintained at 150°C. Thereafter, esterification was carried out for 15 hours at 170°C under a reduced pressure of 0.5 to 2.5 kPa while distilling off the distillate, to obtain a toner binder (C-1).

[0076] <Examples 2 to 8, Comparative Example 2> [Production of Toner Binders (C-2) to (C-8), (C'-2)] Toner binders were produced in the same manner as in Example 1 using the blending amounts of the raw materials shown in Table 3, and toner binders (C-2) to (C-8) and (C'-2) according to Examples 2 to 7 were obtained.

[0077] <Comparative Example 1> [Production of Toner Binder (C'-1)] The crystalline vinyl resin (A'-1) produced in Comparative Production Example 1 was used as a toner binder (C'-1).

[0078] The compositions and physical properties of the toner binders (C-1) to (C-8) obtained in Examples 1 to 8 and the toner binders (C'-1) to (C'-2) obtained in Comparative Examples 1 and 2 are shown in Table 3. Note that, as the amount of remaining unreacted monomer, the amount of remaining monohydric alcohol (B) having 18 to 30 carbon atoms is shown for Examples 1 to 8, the amount of remaining docosyl acrylate is shown for Comparative Example 1, and the amount of remaining monohydric alcohol (B') other than (B) is shown for Comparative Example 2.

[0079] [Table 3]

[0080] <Example 9> [Production of Toner (T-1)] To 86 parts of the toner binder (C-1) of Example 1, 7 parts of a pigment carbon black [MA-100, manufactured by Mitsubishi Chemical Corporation] as a colorant, 5 parts of a release agent Fischer-Tropsch wax [FT-0070, manufactured by Nippon Seiro Co., Ltd.], and 1 part of a charge control agent [T-77, manufactured by Hodogaya Chemical Co., Ltd.] were added, and a toner was prepared by the following method. First, the mixture was premixed using a Henschel mixer [FM10B, Nippon Coke & Engineering Co., Ltd.], then mixed using a twin-screw mixer [PCM-30, Ikegai Co., Ltd.]. Then, the mixture was finely pulverized using a supersonic jet mill, Labojet [KJ-25, Kurimoto Iron Works Co., Ltd.], and classified using an elbow jet classifier [EJ-L-3(LABO) type, Matsubo Co., Ltd.] to obtain toner particles with a volume average particle size D50 of 7 μm. Next, 1 part of hydrophobic silica (Aerosil R972, manufactured by Nippon Aerosil Co., Ltd.) as a fluidizing agent was mixed with 100 parts of the toner particles in a sample mill to obtain a toner (T-1) according to Example 9.

[0081] <Examples 10 to 16> [Production of Toners (T-2) to (T-8)] Toners (T-2) to (T-8) were obtained in the same manner as in Example 9, except that the toner binder (C-1) in Example 9 was replaced with (C-2) to (C-8).

[0082] <Comparative Examples 3 and 4> [Production of Toners (T'-1) and (T'-2)] Toners (T'-1) to (T'-2) were obtained in the same manner as in Example 9, except that the toner binder (C-1) in Example 9 was replaced with (C'-1) to (C'-2).

[0083] [Evaluation method] The methods for evaluating the low-temperature fixing property, heat-resistant storage stability under high temperature and high humidity conditions, long-term stability, document offset resistance after continuous printing, and charging stability of the obtained toners (T-1) to (T-8) and (T'-1) to (T'-2) are described below, along with the criteria for evaluation.

[0084] <Low temperature fixability> Toner is applied to the paper at 1.00 mg / cm 2 The powder was applied evenly so that it would be uniform. The method for applying the powder to the paper surface at this time was to use a printer without a thermal fixing unit. The paper was passed through a soft roller at a fixing speed (circumferential speed of the heating roller) of 213 mm / sec, and at a heating roller temperature range of 80 to 180°C in 5°C increments. Next, the presence or absence of cold offset in the fixed image was visually observed, and the temperature at which cold offset occurs (MFT) was measured. The lower the temperature at which cold offset occurs, the better the low-temperature fixing ability is. Under these evaluation conditions, it is generally preferable that the MFT is 120° C. or less.

[0085] <Heat resistance under high temperature and humidity conditions> 1 g of toner and 0.013 g of Aerosil R8200 (manufactured by Evonik Japan Co., Ltd.) were mixed in a shaker for 1 hour, the mixture was placed in a sealed container and left to stand for 48 hours in an atmosphere of 47°C and 90% humidity. The cohesion was then measured using a powder tester, and the heat resistance storage stability under high temperature and high humidity conditions was evaluated. The lower the value in the cohesion test determined by the following method, the better the heat resistance storage stability under high temperature and high humidity conditions. Under these evaluation conditions, a value of 4% or less is preferable. Equipment: POWDER TESTER model PT-X (manufactured by Hosokawa Micron) Sieve openings: 355μm, 250μm, 150μm Vibration width: 1mm Vibration duration: 30 seconds Operation method: Set the sieves on the vibration table of the powder tester in the following order: top 355μm, middle 250μm, bottom 150μm. Place 1g of toner on the top sieve and vibrate with a vibration amplitude of 1mm for 30 seconds. Measure the weight of toner remaining on each sieve. Cohesion: Calculated from the weight of toner used for measurement and the weight of toner remaining after sieving. Cohesion degree (%)=(U / N+M / N×3 / 5+L / N×1 / 5)×100 U: weight of top row, M: weight of middle row, L: weight of bottom row, N: weight of sample (1g)

[0086] <Long-term stability> 1 g of toner was placed in an open container and left to stand for 30 days in a thermostatic dryer at 47°C. The toner after standing for 30 days and the toner that had not been placed in the 47°C dryer and was left to stand for 30 days in an environment of 25°C and 50% humidity were subjected to elemental analysis using an X-ray photoelectron spectrometer (AXIS NOVA, manufactured by Shimadzu Corporation) and the carbon atom concentration on the toner surface was compared to evaluate long-term stability. [Judgment criteria] The carbon atom concentration increase rate (%) = [carbon atom concentration (%) of toner left undisturbed for 30 days at 47°C] / [carbon atom concentration (%) of toner left undisturbed for 30 days at 25°C and humidity of 50%] × 100 (%) was calculated, and the results are shown in Table 4. In this evaluation, 10% or less is preferable.

[0087] <Document offset resistance after continuous printing> The toner was used to make 10,000 continuous copies using a commercially available monochrome copier [AR5030, manufactured by Sharp Corporation]. Using the fixed image at 120°C after the 10,000 continuous copies, the image area was stacked facing each other so that it overlapped with the non-image area and the image area, and the overlapping areas were subjected to a pressure of 80 g / cm 2 A weight was placed on the paper to ensure it was equivalent to the paper weight, and the paper was left in a high-temperature, high-humidity chamber at 50°C and 50% humidity for 24 hours. After leaving the paper, the degree of image defects on the two overlapping fixed images was visually judged, and the document offset properties (paper blocking resistance during continuous printing) were evaluated according to the following criteria. The evaluation criteria were ◯ and ◎, which are at a level suitable for practical use, and were therefore judged to be passable, while the ranks Δ and × were judged to be failable. [Evaluation Criteria] ⊚: No image transfer was observed at all in either the image or non-image areas. ◯: No white spots are observed in the image area. Slight image transfer is observed in the non-image area. Δ: White spots are observed in the image area, and image transfer is observed in the non-image area. ×: Two overlapping prints are stuck together and cannot be peeled off. If you try to peel them off forcefully, the entire surface of the paper comes off, causing significant image loss.

[0088] <Charge stability> 0.5 g of toner and 20 g of ferrite carrier (F-150, Powder Tech Co., Ltd.) were placed in a 50 mL glass bottle and conditioned at 23°C and 50% relative humidity for 8 hours or more. Next, the mixture was friction-mixed at 50 rpm for 10 minutes and 60 minutes in a Turbula shaker mixer, and the charge amount at each time was measured using a blow-off charge amount measuring device [Kyocera Chemical Co., Ltd.]. Using the obtained value, "charge amount after 60 minutes of friction / charge amount after 10 minutes of friction×100(%)" was calculated, and this was taken as the charge stability index. A larger charge stability index indicates a more excellent charge retention rate. Under these evaluation conditions, a charge stability index of 80% or more is preferable.

[0089] The above evaluation results are shown in Table 4.

[0090] [Table 4]

[0091] As is clear from the evaluation results in Table 4, all of the toners (T-1) to (T-8) containing the toner binders (C-1) to (C-8) of Examples 1 to 8 produced by the production method of the present invention achieved excellent results in all performance evaluations. On the other hand, the toners (T'-1) and (T'-2) containing the toner binders (C'-1) and (C'-2) according to Comparative Examples 1 and 2 were poor in some performance items. [Industrial Applicability]

[0092] The toner binder of the present invention can be suitably used as an electrophotographic toner used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like. Further, it is suitable for use as an additive for paints, an additive for adhesives, particles for electronic paper, and the like.

Claims

1. A method for producing a toner binder, comprising a step of subjecting (A) an amorphous vinyl resin containing a monomer having a carboxy group as a constituent monomer to an esterification reaction with (B) a monohydric alcohol having 18 to 30 carbon atoms.

2. The method for producing a toner binder according to claim 1 , further comprising a step of reducing the pressure in the reaction system during and / or after the esterification reaction.

3. 3. The method for producing a toner binder according to claim 1, wherein the amorphous vinyl resin (A) contains, as a constituent monomer, a monomer having a carboxy group in an amount of 4 to 50% by weight based on the weight of all constituent monomers of the amorphous vinyl resin (A).

4. 3. The method for producing a toner binder according to claim 1, wherein a weight ratio [(A):(B)] of the amorphous vinyl resin (A) to the monohydric alcohol having 18 to 30 carbon atoms before an esterification reaction is 30:70 to 70:

30.

5. The method for producing a toner binder according to claim 1 or 2, wherein the toner binder has at least one endothermic peak top temperature (Tm) in the range of 45 to 100° C. The endothermic peak top temperature (Tm) is measured using a differential scanning calorimeter, and is the peak top temperature of the endothermic peak during a second heating process when the toner binder is heated for the first time from 20° C. to 150° C. at a rate of 10° C. / min, then cooled to 0° C. at a rate of 10° C. / min, and then heated for the second time from 0° C. to 150° C. at a rate of 10° C. / min.

Citation Information

Patent Citations

  • Crystalline polyester for toner

    JP2005077930A

  • Toner binder

    JP2019211763A