Film, Anti-fogging film, hard coating film, method for producing film, bilayer film and method for producing bilayer film
A polymer bonding silsesquioxane and oligoethylene glycol enhances film water resistance and mechanical strength, addressing issues of peeling and cracking in antifogging films, while maintaining antifogging properties and durability.
Patent Information
- Application Number
- JP2024073883
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-20
AI Technical Summary
Existing antifogging films using hydrophilic polymers, such as polyvinyl alcohol, suffer from decreased transparency and mechanical strength due to scratches or abrasion, and exhibit poor water resistance, leading to peeling and cracking.
A polymer is developed by bonding silsesquioxane with a carboxyl group and oligoethylene glycol through an ester bond, which is then applied to a substrate, optionally with a primer film, to enhance water resistance, hardness, and antifogging properties.
The resulting film exhibits improved water resistance, mechanical strength, and antifogging properties, maintaining transparency and durability even when exposed to water, with hardness suitable for protective coatings.
Smart Images

Figure 2024161896000001 
Figure 2024161896000002 
Figure 2024161896000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a film, an anti-fogging film, a hard coat film, a method for producing a film, a bilayer film, and a method for producing a bilayer film. [Background technology]
[0002] Fogging refers to a state in which numerous fine water droplets on the surface of glass, mirrors, etc. cause light to be diffusely reflected, preventing the normal passage or reflection of light. Anti-fogging technology to prevent fogging is widely used in automobile window glass, show windows, eyeglasses, goggles, helmets, food packaging, medical equipment, etc. Anti-fogging technology mainly involves a method of making the substrate surface hydrophobic or water-repellent with a hydrophobic polymer, etc., so that water droplets themselves do not easily adhere to the substrate, and a method of making the substrate surface hydrophilic to form a thin, continuous water film.
[0003] Coating the substrate surface with a hydrophobic polymer has the disadvantage of insufficient adhesion to inorganic substrates such as glass. For this reason, the mainstream of anti-fogging film materials is coating the substrate surface with a hydrophilic polymer. However, most hydrophilic polymers, such as polyvinyl alcohol (PVA), are soft and their transparency and anti-fogging properties gradually decrease due to scratches, abrasion, etc.
[0004] In order to compensate for the drawbacks of hydrophilic polymers, anti-fogging films using hydrophilic polymers containing silsesquioxane in the main chain, such as polyhedral oligosilsesquioxane, have also been proposed (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2021-183668 A Summary of the Invention [Problem to be solved by the invention]
[0006] The film of Patent Document 1 exhibits excellent hard coat properties and anti-fogging properties, but becomes brittle when immersed in water, and peels off from the object or cracks occur, leaving room for improvement in the water resistance of the film.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a film capable of improving water resistance, an anti-fogging film, a hard coat film, a method for manufacturing a film, a bilayer film, and a method for manufacturing a bilayer film. [Means for solving the problem]
[0008] The membrane according to the first aspect of the present invention comprises: The polymer includes a silsesquioxane having a carboxyl group and an oligoethylene glycol bonded by ester bonding. It is characterized by:
[0009] Also, the silsesquioxane is a polyhedral oligosilsesquioxane, The polyhedral oligosilsesquioxane and the oligoethylene glycol may be mixed in a ratio of carboxyl group:hydroxyl group of 5:1 to 1:1.
[0010] The silsesquioxane is a polysilsesquioxane having a dicarboxylic acid group, The polysilsesquioxane and the oligoethylene glycol may be mixed in a ratio of carboxyl group:hydroxyl group of 20:1 to 5:1.
[0011] The oligoethylene glycol may have 3 to 6 repeating units of the oxyethylene group.
[0012] The anti-fogging film according to the second aspect of the present invention comprises: The polymer includes a silsesquioxane having a carboxyl group and an oligoethylene glycol bonded by ester bonding. It is characterized by:
[0013] The hard coat film according to the third aspect of the present invention comprises: The polymer includes a silsesquioxane having a carboxyl group and an oligoethylene glycol bonded by ester bonding. It is characterized by:
[0014] A method for producing a membrane according to a fourth aspect of the present invention comprises the steps of: a bonding step of carrying out an ester bond reaction between a carboxyl group of the silsesquioxane and a hydroxyl group of the oligoethylene glycol; A heating step of heating the polymer obtained in the bonding step. It is characterized by:
[0015] The bilayer membrane according to the fifth aspect of the present invention comprises: a primer film containing a polymer obtained by condensing an alkoxysilane having an epoxy group and a tetraalkoxysilane; A membrane containing a polymer in which a silsesquioxane having a carboxyl group and an oligoethylene glycol are ester-bonded, It is characterized by:
[0016] A method for producing a bilayer membrane according to a sixth aspect of the present invention comprises the steps of: A step of applying a polymer solution obtained by polymerizing an alkoxysilane having an epoxy group and a tetraalkoxysilane onto a substrate and heating the polymer solution to form a primer film; A step of applying a polymer solution in which silsesquioxane having a carboxyl group and oligoethylene glycol are polymerized onto the primer film and heating the solution to form a film. It is characterized by: Effect of the Invention
[0017] According to the present invention, it is possible to provide a film capable of improving water resistance, an anti-fogging film, a hard coat film, a method for producing a film, a bilayer film, and a method for producing a bilayer film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] (film) The membrane according to the present embodiment contains a polymer in which silsesquioxane having a carboxyl group and oligoethylene glycol are bonded via ester bonds.
[0019] Silsesquioxane is a type of RSiO obtained by hydrolysis / condensation reaction of trifunctional organosilane compounds such as organotrialkoxysilane and organotrichlorosilane. 1.5 (R is an organic group or H) in a repeating structure. Various structures such as random, cage (polyhedral), ladder, and rod structures are known for silsesquioxane, and any of these structures may be used. Cage-type oligo SQ has a three-dimensional ring-closed structure formed by siloxane bonds. Cage-type oligo SQ has a polyhedral skeleton structure with silicon atoms at the vertices and siloxane bonds on the edges. Cage-type oligo SQ is also called polyhedral oligo SQ, and is abbreviated as POSS (polyhedral oligomeric silsesquioxane).
[0020] The silsesquioxane according to the present embodiment has a carboxyl group as an organic group in a side chain. The carboxyl group may be in a form in which it exists as a partial substituent of the organic group, for example, indirectly bonded via an alkylene chain, or may exist as a substituent having two or more carboxyl groups, such as a dicarboxylic acid group.
[0021] When the silsesquioxane according to the present embodiment is a POSS, there are no particular limitations as long as it has a polyhedral skeleton structure, and examples thereof include a T6 structure in which the number of silicon atoms arranged at the vertices of the polyhedron is 6, a T7 structure in which the number is 7, a T8 structure in which the number is 8, a T9 structure in which the number is 10, 10 Structure and 12 T 12 The number of silicon atoms may be the same or different.
[0022] The oligoethylene glycol imparts water-insoluble properties to the film. The number of repeating units of the oxyethylene group of the oligoethylene glycol is not limited, and may be, for example, 1 to 6, 2 to 6, 3 to 6, 4 to 6, 3 to 5, 5 to 6, or 4 to 5.
[0023] When the silsesquioxane is POSS, the blending ratio of POSS to oligoethylene glycol is not limited, but may be, for example, 5:1 to 1:1, or 2:1 to 1:1, for the carboxyl group of POSS:hydroxyl group of oligoethylene glycol.
[0024] Furthermore, when the silsesquioxane is a polysilsesquioxane having a dicarboxylic acid group, the blending ratio of the polysilsesquioxane to the oligoethylene glycol is not limited, and may be, for example, 20:1 to 5:1, or 20:1 to 10:1, in terms of the ratio of the carboxyl group of the polysilsesquioxane to the hydroxyl group of the oligoethylene glycol.
[0025] (Membrane manufacturing method) A method for producing the membrane will be described. The method for producing the membrane includes a bonding step and a heating step. In the bonding step, a reaction is carried out to bond a carboxyl group of the silsesquioxane with a hydroxyl group of the oligoethylene glycol.
[0026] In the bonding step, the silsesquioxane and the oligoethylene glycol are mixed, dissolved, and reacted in a solvent capable of dissolving the silsesquioxane and the oligoethylene glycol. An esterification reaction occurs between the carboxyl group of the silsesquioxane and the hydroxyl group of the oligoethylene glycol, and the silsesquioxane and the oligoethylene glycol are bonded by an ester bond. Examples of the solvent include known solvents such as N,N-dimethylformamide.
[0027] The reaction conditions for the binding step are appropriately set. For example, the reaction temperature is 40 to 120°C, 60 to 100°C, or 70 to 90°C. The reaction time is adjusted according to the reaction rate, and is, for example, 30 to 90 minutes. The polymer obtained in the binding step may be isolated, purified, and concentrated by a known method. For example, the polymer may be obtained through operations such as reprecipitation, decantation, filtration, washing, and concentration.
[0028] In the heating step, the polymer obtained in the binding step is heated to 100° C. or higher. The heating temperature is set according to the properties of the obtained polymer, etc. The heating temperature is, for example, 100 to 200° C. The heating time is, for example, 5 to 60 minutes, 10 to 50 minutes, or 20 to 40 minutes.
[0029] Preferably, in the heating step, the polymer is heated on the substrate on which the film is to be formed. In this case, the substrate on which the polymer solution is applied is heated. The solvent of the polymer solution is not limited as long as the polymer is dissolved therein, and examples thereof include alcohols such as methanol, ethanol, and isopropyl alcohol, dimethyl sulfoxide, N,N-dimethylformamide, or mixtures thereof. In addition, when the polymer is not isolated after the binding step, the solution obtained in the binding step may be used as the polymer solution as it is.
[0030] The substrate is not particularly limited as long as the polymer can form a film, preferably a thin film. Substrate materials include, for example, inorganic materials and organic materials. Inorganic materials include nonmetallic inorganic materials and metallic inorganic materials. Nonmetallic inorganic materials include, for example, glass and ceramic materials. Metallic inorganic materials include, for example, cast iron, steel, iron, iron alloys, aluminum, aluminum alloys, nickel, nickel alloys, and zinc die-casting. The metallic inorganic material may also be a metal plating film applied to the surface of a nonmetallic inorganic material or an organic material.
[0031] Examples of organic materials include synthetic resin materials such as polyvinyl chloride resin, polyethylene, polypropylene, polycarbonate, acrylic resin polyacetal, fluororesin, silicone resin, ethylene-vinyl acetate copolymer (EVA), acrylonitrile-butadiene rubber (NBR), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyvinyl butyral (PVB), ethylene-vinyl alcohol copolymer (EVOH), polyimide, polyphenylene sulfide (PPS), polyetherimide (PEI), polyetheretherimide (PEEI), polyetheretherketone (PEEK), melamine resin, and acrylonitrile-butadiene-styrene (ABS) resin, as well as fiber materials.
[0032] A known method can be used to apply the polymer solution to the substrate. Specifically, the polymer solution can be applied to the substrate by using a solution casting method, a dip coating method, a spin coating method, a spray coating method, a brush coating method, an impregnation method, a roll method, a wire bar method, a die coating method, a gravure printing method, an inkjet method, etc. The thickness of the film is not particularly limited, but is, for example, 1 nm to 1 mm, 10 nm to 500 μm, or 100 nm to 50 μm.
[0033] The film according to the present embodiment has transparency and antifogging properties. Antifogging properties can be evaluated by various known methods. For example, as specified in the JIS standard, there is a method of visually checking the presence or absence of fogging under specified conditions (JIS K2399, JIS S7027 / S7301 and JIS A1514). Antifogging properties can be evaluated based on the transmittance of laser light as in the EN standard (EN168). In addition, antifogging properties can be evaluated using a commercially available antifogging property evaluation device using the natural condensation method and the humidified injection method, or visual tests such as breath antifogging property test, steam antifogging property test and low temperature antifogging property test, as well as image analysis.
[0034] The film according to the present embodiment has excellent mechanical strength because it contains a polymer having silsesquioxane as a main chain. Therefore, the film has high hardness. The hardness of the film can be evaluated by a known method. The hardness can be evaluated by an indentation test method or a dynamic test method. The hardness is indicated by Rockwell hardness, Vickers hardness, Brinell hardness, Shore hardness, Knoop hardness, etc. based on the test method. An example of a hardness that can be easily evaluated is pencil hardness. The pencil hardness can be evaluated by a known tester such as a pencil scratch tester. The hardness of the film according to the present embodiment is 2H or more or 3H or more, preferably 5H or more or 5H, in terms of pencil hardness.
[0035] Furthermore, since the film according to the present embodiment is water-insoluble, it exhibits good water resistance, and even when immersed in water, it is possible to suppress defects such as dissolution, cracking, and peeling from the substrate. In addition, since it has both hardness and anti-fogging properties, it can be used as an anti-fogging film that is scratch-resistant and has excellent durability. In addition, the film is also useful as a hard coat film that protects the substrate from external factors.
[0036] (double layer membrane) Although the film is formed depending on the physical properties of the substrate, there is a risk that the film will not maintain water resistance and peel off from the substrate. In such a case, it is preferable to form a two-layer film by forming a primer film on the substrate and forming the above-mentioned film on the primer film. Examples of the above-mentioned substrate include resins such as acrylic resin, epoxy resin, polycarbonate resin, and polyethylene terephthalate resin.
[0037] The primer film is a film containing a polymer obtained by condensation polymerization of an alkoxysilane having an epoxy group (hereinafter, referred to as an epoxy group-containing alkoxysilane) and a tetraalkoxysilane. Examples of the epoxy group-containing alkoxysilane include glycidyloxypropyltrimethoxysilane and glycidyloxypropyltriethoxysilane. Examples of the tetraalkoxysilane include tetramethoxysilane and tetraethoxysilane.
[0038] The bonding state between the primer film and the substrate is presumed to be an ester bond between the epoxy group of the primer film and the carboxyl group of the substrate, and the bonding state between the primer film and the substrate is presumed to be a hydrogen bond between the hydroxyl group generated by ring-opening of the epoxy group of the primer film and the carbonyl group of the substrate.
[0039] The compounding ratio of epoxy group-containing alkoxysilane to tetraalkoxysilane is preferably 10:1 to 1:2 by molar ratio, more preferably 9:1 to 1.5:1, further preferably 9:1 to 31, and most preferably 3:1. If the compounding ratio of epoxy group-containing alkoxysilane is too high, the formation of a polymer network is impaired. On the other hand, if the compounding ratio of tetraalkoxysilane is too high, cracks are likely to occur in the obtained primer film.
[0040] (Method of manufacturing bilayer membrane) The two-layer film includes the steps of depositing a primer film on a substrate and depositing the above-mentioned film on the primer film.
[0041] In the step of forming the primer film, the epoxy group-containing alkoxysilane and the tetraalkoxysilane are mixed and dissolved in a solvent capable of dissolving the epoxy group-containing alkoxysilane and the tetraalkoxysilane. A hydrochloric acid solution or the like is added to the mixture to cause a sol-gel reaction, thereby obtaining a polymer solution in which the epoxy group-containing alkoxysilane and the tetraalkoxysilane are polycondensed. Examples of the solvent include known solvents such as N,N-dimethylformamide. The reaction temperature may be room temperature, and the reaction time is adjusted according to the reaction rate, for example, 30 to 90 minutes.
[0042] The prepared polymer solution is applied onto a substrate, and a heat treatment is then performed to form a primer film on the substrate. The heat treatment is preferably performed by preheating (e.g., at 30 to 50°C for 5 to 7 hours) followed by high-temperature heat treatment (e.g., at 90 to 110°C for 1 to 3 hours).
[0043] The polymer solution can be applied to the substrate by a known method. Specifically, the polymer solution can be applied to the substrate by using a solution casting method, a dip coating method, a spin coating method, a spray coating method, a brush coating method, an impregnation method, a roll method, a wire bar method, a die coating method, a gravure printing method, an inkjet method, etc. The thickness of the film is not particularly limited, but is, for example, 1 nm to 1 mm, 10 nm to 500 μm, or 100 nm to 50 μm.
[0044] A two-layer film can be manufactured by forming the above-mentioned film on the formed primer film. The film formation on the primer film is the same as the above-mentioned film manufacturing method, so the description is omitted. It is preferable to form the film by subjecting the primer film to hydrophilic treatment such as oxygen plasma irradiation.
[0045] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples. EXAMPLES
[0046] (Experimental Example 1) <Synthesis of POSS with a carboxyl group in the side chain (POSS-C)> According to a known method (T. Kozuma and Y. Kaneko, J. Polym. Sci. Part A: Polym. Chem., 2019, 57, 2511), POSS-C was synthesized as shown in the following reaction scheme.
[0047] [ka]
[0048] 2-Methacryloyloxyethyl phosphorylcholine (MPC) was added to 2-cyanoethyltriethoxysilane, and the mixture was stirred at room temperature for 15 hours after adding an aqueous sodium hydroxide solution of 2 mol / L. Then, the solvent was distilled off by heating under open system conditions at a set temperature of 50 °C, and the mixture was heated in an oven at a set temperature of 100 °C for 2 hours. It was neutralized with a 1 mol / L aqueous hydrochloric acid solution, and the solvent was evaporated by heating under open system conditions. The product was quickly washed with water and freeze-dried to obtain PolySQ-COOH.
[0049] An aqueous trifluoromethanesulfonic acid solution was added to the synthesized PolySQ-COOH and stirred. The solvent was distilled off by heating under open system conditions at a set temperature of 50 °C, and the mixture was heated in an oven at a set temperature of 100 °C for 2 hours. The crude product was dissolved in acetone, reprecipitated with an acetone / chloroform (1 / 9) mixed solvent, and stirred at room temperature for 15 hours. It was suction filtered, washed with acetonitrile, and dried under reduced pressure to obtain POSS-C.
[0050] <Preparation of a film using POSS-C and oligoethylene glycol (POSS-C / OEG film)> POSS-C (0.1 mmol unit) and oligoethylene glycol were mixed in 0.3 mL of N,N-dimethylformamide (DMF), and 7 μL of concentrated hydrochloric acid was added. Then, a polymer solution was prepared by heating and stirring in a sealed system at 80 °C for 1 hour. The prepared polymer solution was applied to a hydrophilically treated glass plate. The solvent was distilled off by heating under open system conditions at a set temperature of 50 °C for 1 hour, and a POSS-C / OEG film was prepared on the glass substrate by heating at a set temperature of 150 °C for 30 minutes.
[0051] Also, a polymer solution was prepared in the same manner as above except that concentrated hydrochloric acid was not added, and a POSS-C / OEG film was prepared in the same manner as above using this polymer solution without added concentrated hydrochloric acid.
[0052] Regarding the blending of POSS-C and oligoethylene glycol, the carboxyl group of POSS-C: the hydroxyl group of oligoethylene glycol was made to be 5:1, 2:1, and 1:1, and films were formed respectively.
[0053] In addition, oligoethylene glycols with 1, 2, 3, 4, 5, and 6 repeating units of oxyethylene groups (EG, 2EG, 3EG, 4EG, 5EG, and 6EG, respectively) were used to form films, respectively.
[0054] <Evaluation of POSS-C / OEG Films> The prepared POSS-C / OEG films were evaluated for anti-fogging properties, hardness, and water resistance.
[0055] The anti-fogging property was evaluated by placing the film 2 cm above the water surface of warm water at about 40 °C, exposing it to water vapor, and measuring the time until it fogged.
[0056] Hardness was measured using a pencil scratch tester (manufactured by TP Giken Co., Ltd., 750 g) in accordance with JIS K5600-5-4. The tip of the pencil (uni, manufactured by Mitsubishi Pencil Co., Ltd.) was sharpened flat, and the pencil was attached to the tester so that the angle of the pencil with respect to the cast film was 45 degrees. The pencil was moved 7 mm at a speed of 0.5 - 1 mm / s. The pencil hardness, which is the hardness of the hardest pencil that did not cause a scratch mark, was evaluated as the hardness.
[0057] The water resistance was evaluated by immersing the coated glass in water at room temperature for 1 hour, visually inspecting the appearance of the film after taking it out, and designating it as "OK" if the transparency and shape were maintained, and as "NG" if defects such as dissolution, cracking, and peeling were observed.
[0058] The results of the POSS-C / OEG films formed using polymer solutions without added concentrated hydrochloric acid with carboxyl group:hydroxyl group = 5:1, 2:1, and 1:1 are shown in Tables 1 - 3, respectively.
[0059]
Table 1
[0060]
Table 2
[0061] [Table 3]
[0062] When the ratio of carboxyl group to hydroxyl group was 5:1, 5EG and 6EG had good water resistance. When the ratio of carboxyl group to hydroxyl group was 2:1, 4EG to 6EG showed good water resistance. When the ratio of carboxyl group to hydroxyl group was 1:1, 4EG to 6EG showed good water resistance.
[0063] Tables 4 to 6 show the results of the POSS-C / OEG films formed using a polymer solution containing concentrated hydrochloric acid at a carboxyl group:hydroxyl group ratio of 5:1, 2:1, and 1:1.
[0064] [Table 4]
[0065] [Table 5]
[0066] [Table 6]
[0067] When the ratio of carboxyl groups to hydroxyl groups was 5:1, only 6EG had good water resistance.When the ratio of carboxyl groups to hydroxyl groups was 2:1, only 6EG showed good water resistance.When the ratio of carboxyl groups to hydroxyl groups was 1:1, 5EG showed good water resistance.
[0068] (Experimental Example 2) <Synthesis of polysilsesquioxane (PSQ-2C) with two carboxyl groups in the side chain> According to a known method (J. Liu and Y. Kaneko, Bull. Chem. Soc. Jpn., 2018, 91, 1120), PSQ-2C was synthesized as shown in the following reaction scheme.
[0069] [Chem.]
[0070] To 3-triethoxysilylpropyl succinic anhydride (TESPSA) (10 mmol, 3.2732 g), 0.5 mol / L hydrochloric acid aqueous solution was added in an amount of 3 equivalents (30 mmol, 60 mL) relative to TESPSA, and the mixture was stirred at room temperature for 2 hours. The obtained sol solution was heated on a hot plate set at a temperature of 50 °C in an open system to distill off the solvent, and then heated in an oven set at a temperature of 100 °C for 2 hours. The obtained crude product was added to methanol (10 mL) and dissolved by heating on a hot plate set at a temperature of 60 °C. The obtained solution was poured into 300 mL of ethyl acetate for reprecipitation, and the insoluble part was recovered by decantation. The recovered insoluble part was washed with ethyl acetate and dried under reduced pressure to obtain PSQ-2C.
[0071] [Preparation of a membrane using PSQ-2C and oligoethylene glycol (PSQ-2C / OEG membrane)] PSQ-2C (0.1 mmol unit) and oligoethylene glycol were mixed in 0.3 mL of DMF, and 7 μL of concentrated hydrochloric acid was added. Then, the mixture was heated and stirred at 80 °C for 1 hour in a sealed system to prepare a polymer solution.
[0072] The polymer solution was applied to a hydrophilized glass plate. After heating in an open system at a set temperature of 50 °C for 2 hours to distill off the solvent, it was heated and dried at a set temperature of 150 °C for 30 minutes. Then, it was immersed in purified water for 1 hour and dried at room temperature to prepare a PSQ-2C / OEG membrane on the glass plate.
[0073] Regarding the blending of PSQ-2C and oligoethylene glycol, the carboxyl group of PSQ-2C: the hydroxyl group of oligoethylene glycol was made to be 20:1, 10:1, and 5:1, and films were formed respectively.
[0074] In addition, oligoethylene glycols with 1, 2, 3, 4, 5, or 6 repeating units of oxyethylene groups (EG, 2EG, 3EG, 4EG, 5EG, and 6EG, respectively) were used.
[0075] <Evaluation of PSQ-2C / OEG Film> For the fabricated PSQ-2C / OEG film, antifogging property, hardness, and water resistance were evaluated by the same evaluation method as the above-described POSS-C / OEG film.
[0076] The evaluation results of PSQ-2C / OEG films formed with carboxyl group:hydroxyl group = 20:1, 10:1, and 5:1 are shown in Tables 7 to 9, respectively.
[0077] [Table 7]
[0078] [Table 8]
[0079] [Table 9]
[0080] When carboxyl group:hydroxyl group = 20:1, water resistance was good in 3EG to 6EG. Also, when carboxyl group:hydroxyl group = 10:1, good water resistance was shown in 3EG to 6EG. Further, when carboxyl group:hydroxyl group = 5:1, good water resistance was shown in 2EG to 4EG.
[0081] (Experimental Example 3) An acrylic resin plate was used as the substrate, and a two-layer film was fabricated on the acrylic resin plate for evaluation.
[0082] <Synthesis of GOPTS / TOMS Polymer> 3-Glycidyloxypropyltrimethoxysilane (GOPTMS, 3.75 mmol) and tetramethoxysilane (TMOS, 1.25 mmol) were dissolved in DMF, and an aqueous solution of hydrochloric acid (1.0 mol / L, 0.5 mL) was added. The mixture was stirred at room temperature for 15 minutes to prepare a GOPTS / TOMS polymer solution.
[0083] <Preparation of primer film (GOPTS / TOMS film)> The GOPTS / TOMS polymer solution was applied to an acrylic resin substrate that had been hydrophilized by oxygen plasma exposure, and the solvent was removed by drying at room temperature for one day. The substrate was then heated at 40°C for six hours, and then at 100°C for two hours to produce a GOPTS / TOMS film.
[0084] <Synthesis of POSS with a carboxyl group in the side chain (POSS-C)> POSS-C (0.4 mmol unit) and OEG were mixed in DMF (0.3 mL), and 7 μL of concentrated hydrochloric acid was added. After that, the mixture was heated and stirred at 80°C in a closed system for 1 hour to prepare a POSS-C / OEG polymer solution. The blending ratio of POSS-C and OEG was 5:1 (carboxyl group:hydroxyl group), and OEG was tetraethylene glycol.
[0085] <Preparation of bilayer membrane> The prepared POSS-C / OEG polymer solution was applied onto the GOPTS / TOMS film that had been hydrophilized by oxygen plasma irradiation. The solvent was removed by heating for 2 hours at 50°C in an open system. The film was then heated for 2 hours at 100°C, and then heated for 1 hour at 150°C to produce a POSS-C / OEG film on the GOPTS / TOMS film.
[0086] <Evaluation of bilayer membrane> The prepared bilayer film was evaluated for anti-fogging property, hardness, and water resistance by the same evaluation methods as in Experimental Example 1. The evaluation results of the bilayer film are shown in Table 10.
[0087] [Table 10]
[0088] The two-layer film thus prepared showed no peeling from the acrylic resin plate, good water resistance, and good hardness and anti-fogging properties. [Industrial Applicability]
[0089] The present invention is suitable for imparting anti-fogging properties to window panes of automobiles, show windows, eyeglasses, goggles, helmets, food packaging, medical instruments, and the like.
Claims
1. The polymer includes a silsesquioxane having a carboxyl group and an oligoethylene glycol bonded by ester bonding. A membrane characterized in that
2. the silsesquioxane is a polyhedral oligosilsesquioxane; The polyhedral oligosilsesquioxane and the oligoethylene glycol are mixed in a ratio of carboxyl group:hydroxyl group of 5:1 to 1:
1. The membrane of claim 1 .
3. The silsesquioxane is a polysilsesquioxane having a dicarboxylic acid group, The polysilsesquioxane and the oligoethylene glycol are mixed in a ratio of carboxyl group:hydroxyl group of 20:1 to 5:
1. The membrane of claim 1 .
4. The number of repeating units of the oxyethylene group of the oligoethylene glycol is 3 to 6. A membrane according to any one of claims 1 to 3.
5. The polymer includes a silsesquioxane having a carboxyl group and an oligoethylene glycol bonded by ester bonding. The anti-fogging film is characterized by the above.
6. The polymer includes a silsesquioxane having a carboxyl group and an oligoethylene glycol bonded by ester bonding. The hard coat film is characterized by the above-mentioned.
7. a bonding step of carrying out an ester bond reaction between a carboxyl group of the silsesquioxane and a hydroxyl group of the oligoethylene glycol; A heating step of heating the polymer obtained in the bonding step. A method for producing a membrane comprising the steps of:
8. a primer film containing a polymer obtained by condensing an alkoxysilane having an epoxy group and a tetraalkoxysilane; A membrane containing a polymer in which a silsesquioxane having a carboxyl group and an oligoethylene glycol are ester-bonded, A bilayer membrane characterized by:
9. A step of applying a polymer solution obtained by polymerizing an alkoxysilane having an epoxy group and a tetraalkoxysilane onto a substrate and heating the polymer solution to form a primer film; A step of applying a polymer solution in which silsesquioxane having a carboxyl group and oligoethylene glycol are polymerized onto the primer film and heating the solution to form a film. A method for producing a bilayer membrane comprising the steps of:
Citation Information
Patent Citations
Film, antifogging film, hard coat film, and production method of film
JP2021183668A
Cited By
Self-healing film, self-healing anti-fogging film, self-healing hard coat film, and method for manufacturing a self-healing film
JP2026176430A