Hardmask composition, hardmask layer, and method of forming patterns
A hard mask composition with specific polymer structural units addresses the etching resistance and solubility issues of spin-coated layers, enhancing etching resistance and gap fill characteristics for semiconductor manufacturing.
Patent Information
- Application Number
- JP2024075131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-20
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hard mask layers formed using spin coating methods have reduced etching resistance, and increasing the carbon content in the polymer composition to improve this resistance leads to decreased solubility in solvents, posing a challenge in achieving effective pattern formation in semiconductor manufacturing.
A hard mask composition containing a polymer with structural units represented by specific chemical formulas, including large aromatic hydrocarbon groups and tertiary or quaternary carbons, is used, which enhances etching resistance while maintaining solubility, and is applied through a spin coating method.
The composition ensures excellent etching resistance and gap fill characteristics, with improved solubility and planarization, enabling effective pattern transfer in semiconductor manufacturing.
Smart Images

Figure 2024161904000049 
Figure 2024161904000001 
Figure 2024161904000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hardmask composition, a hardmask layer including a cured product of the hardmask composition, and a pattern forming method using the hardmask composition. [Background technology]
[0002] Recently, the semiconductor industry has been evolving from patterns of hundreds of nanometers to ultrafine technology with patterns of several to tens of nanometers. Effective lithographic techniques are essential to realize such ultrafine technology.
[0003] A typical lithographic technique includes the steps of forming a material layer on a semiconductor substrate, coating a photoresist layer thereon, exposing and developing to form a photoresist pattern, and then etching the material layer using the photoresist pattern as a mask.
[0004] In recent years, as the size of a pattern to be formed decreases, it is difficult to form a fine pattern having a good profile using only the above-mentioned typical lithographic techniques. As a means for solving this problem, a technology has been developed in which an auxiliary layer, called a hard mask layer, is formed between a material layer to be etched and a photoresist layer to form a fine pattern. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Korean Patent Publication No. 10-2022-0092160 Summary of the Invention [Problem to be solved by the invention]
[0006] It is an object of the present invention to provide a hardmask composition that can be effectively applied to a hardmask layer.
[0007] Another object of the present invention is to provide a hard mask layer comprising a cured product of the above hard mask composition.
[0008] It is still another object of the present invention to provide a pattern forming method using the above hard mask composition. [Means for solving the problem]
[0009] The hard mask composition according to one embodiment of the present invention includes a polymer having a structural unit represented by the following formula 1, and a solvent:
[0010] [ka]
[0011] In the above chemical formula 1, Ar 1 teeth, (i) a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, (ii) a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or (iii) a group in which two or more of the above-mentioned substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms, two or more of the above-mentioned substituted or unsubstituted aromatic heterocyclic groups having 3 to 30 carbon atoms, or a combination thereof are linked by a single bond or a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, and R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R3 and R 4 is not a hydrogen atom at the same time, X is a group represented by the following chemical formula 2: * indicates the connection point:
[0012] [ka]
[0013] In the above chemical formula 2, Ar 2 and Ar 3 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, M 1 and M. 2 are each independently -O-, -S-, -S(=O)-, -SO2-, or -NR a - (where R a is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms), or a combination thereof; Z is at least one selected from the group consisting of moieties listed in Group 1 below, n1 is an integer from 1 to 30; n2 is 0 or 1, * indicates a connection point.
[0014] [ka]
[0015] In the above Group 1, * indicates a connection point.
[0016] Ar in the above formula 1 1 can be at least one selected from the group consisting of substituted or unsubstituted moieties listed in Group 2 below:
[0017] [ka]
[0018] In Group 2 above, Each Y is independently -O-, -S-, or -NR b - (where R b is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; R x and R y are each independently a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 10 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.
[0019] Ar in the above formula 1 1 may be substituted with at least one of a hydroxy group, a halogen atom, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms, or a combination thereof.
[0020] R in the above Chemical Formula 1 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 is preferably not simultaneously a hydrogen atom.
[0021] R in the above Chemical Formula 1 1 and R 3 are preferably the same group, and R 2 and R 4 are preferably the same group.
[0022] Ar in the above formula 1 1 is at least one selected from the group consisting of substituted or unsubstituted moieties listed in Group 2-1 below, R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 16 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 is preferably not also a hydrogen atom:
[0023] [ka]
[0024] In the above group 2-1, Each Y is independently -O-, -S-, or -NR b - (where R b is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; R x and R y are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.
[0025] Ar in the above formula 2 2 and Ar 3is preferably each independently at least one selected from the group consisting of substituted or unsubstituted moieties listed in Group 3 below.
[0026] [ka]
[0027] Ar in the above formula 2 2 and Ar 3 are preferably each independently a substituted or unsubstituted phenylene group, a substituted or unsubstituted naphthalenylene group, a substituted or unsubstituted phenanthrenylene group, a substituted or unsubstituted anthracenylene group, or a substituted or unsubstituted pyrenylene group.
[0028] Ar in the above formula 2 2 and Ar 3 each independently represents a substituted or unsubstituted phenylene group, a substituted or unsubstituted naphthalenylene group, or a substituted or unsubstituted pyrenylene group; M 1 and M. 2 is -O-; Z is at least one selected from the group consisting of moieties listed in Group 1-1 below; and n1 is preferably an integer of 1 to 5.
[0029] [ka]
[0030] In the above Group 1-1, * indicates a connection point.
[0031] In the above chemical formula 2, n1 and n2 are preferably 1.
[0032] In the above chemical formula 2, n1 is an integer of 1 to 5, and n2 is preferably 0.
[0033] The structural unit represented by the above chemical formula 1 is preferably at least one type selected from the group consisting of structural units represented by the following chemical formulas 1-1 to 1-4:
[0034] [ka]
[0035] In the above Chemical Formula 1-1 to Chemical Formula 1-4, R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 is not a hydrogen atom at the same time, Z 1 is at least one selected from the group consisting of the moieties listed in Group 1 below, R c and R d each independently represents a hydroxy group, a halogen atom, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms, or a combination thereof; nc and nd are each independently an integer from 0 to 6; * indicates the connection point:
[0036] [ka]
[0037] In the above Group 1, * indicates a connection point.
[0038] The structural unit represented by the above chemical formula 1 is preferably at least one type selected from the group consisting of structural units represented by the following chemical formulas 1-5 to 1-13.
[0039] [ka]
[0040] [ka]
[0041] In the above chemical formulas 1-5 to 1-13, * represents a linking point.
[0042] The weight average molecular weight of the polymer may be from 1,000 g / mol to 200,000 g / mol.
[0043] The polymer may be included in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition.
[0044] The solvent is preferably at least one selected from the group consisting of propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate.
[0045] According to another embodiment of the present invention, there is provided a hardmask layer comprising a cured product of the hardmask composition described above.
[0046] According to yet another embodiment of the present invention, there is provided a patterning method including the steps of: providing a material layer on a substrate; applying the above-described hard mask composition on the material layer; heat-treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; and etching the exposed portion of the material layer.
[0047] The step of forming the hard mask layer preferably includes a step of performing a heat treatment at 100°C to 1,000°C. Effect of the Invention
[0048] In accordance with the present invention, a hardmask composition is provided that can be effectively applied to a hardmask layer. [Brief description of the drawings]
[0049] [Figure 1] This is a calculation formula for evaluating the planarization characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0050] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0051] Unless otherwise defined in this specification, "substituted" means that a hydrogen atom in a compound is replaced with a halogen atom (F, Br, Cl, or I), a hydroxy group, an alkoxy group, a nitro group, a cyano group, an amino group, an azido group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxy group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid group or a salt thereof, a vinyl group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkyl ... It means that the group is substituted with a substituent selected from an alkynyl group having 6 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an arylaryl group having 9 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, a heterocycloalkyl group having 3 to 30 carbon atoms, and combinations thereof.
[0052] In addition, two adjacent substituents of a substituted halogen atom (F, Br, Cl, or I), a hydroxy group, a nitro group, a cyano group, an amino group, an azide group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxy group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, an alkynyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, or a heterocyclic group having 2 to 30 carbon atoms may be condensed to form a ring.
[0053] Unless otherwise defined in this specification, "aromatic hydrocarbon" refers to a group having one or more aromatic hydrocarbon moieties, and includes not only non-fused aromatic hydrocarbons, fused aromatic hydrocarbons, but also forms in which aromatic hydrocarbon moieties are linked by single bonds, forms in which aromatic hydrocarbon moieties are directly or indirectly fused to a non-aromatic fused ring, or combinations thereof.
[0054] More specifically, the substituted or unsubstituted aromatic hydrocarbon group may be, but is not limited to, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthryl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted perylenyl group, a substituted or unsubstituted indenyl group, a combination thereof, or a condensed form of a combination thereof.
[0055] Unless otherwise defined in this specification, "hetero" means containing one or more heteroatoms selected from the group consisting of N (nitrogen atom), O (oxygen atom), S (sulfur atom), Se (selenium atom), and P (phosphorus atom).
[0056] Unless otherwise defined herein, an "aromatic heterocycle" refers to an aromatic hydrocarbon ring containing at least one heteroatom selected from the group consisting of N, O, S, Se, and P.
[0057] As used herein, a polymer may include both an oligomer and a polymer. In addition, as used herein, a "structural unit" refers to a repeating unit contained in an oligomer or a polymer. Furthermore, as used herein, * in a chemical formula refers to a connection point with another atom.
[0058] Unless otherwise specified in this specification, the "weight average molecular weight" is a value measured by dissolving a powder sample in tetrahydrofuran (THF) and then using a 1200 series Agilent Technologies gel permeation chromatography (GPC) (the column used was an LF-804 manufactured by Resonac Corporation, and the standard sample was polystyrene manufactured by Resonac Corporation).
[0059] In the semiconductor industry, there is a constant demand to reduce the size of chips, and to meet this demand, the line width of the resist patterned by lithography technology must be several tens of nanometers. Therefore, the height that can withstand the line width of the resist pattern is limited, and the resist may not have sufficient resistance in the etching step. To compensate for this, an auxiliary layer called a hardmask layer may be used between the material layer to be etched and the photoresist layer. This hardmask layer serves as an intermediate film that transfers the fine pattern of the photoresist to the material layer through selective etching. Therefore, the hardmask layer is required to have etching resistance so that it can withstand the etching process required for pattern transfer.
[0060] Existing hard mask layers have been formed by chemical or physical vapor deposition, but this requires large equipment and high process costs, resulting in poor economic efficiency. Recently, a technology for forming a hard mask layer by a spin coating method has been developed. The spin coating method is easier to process than conventional methods, and a hard mask layer manufactured by this method has better gap filling and planarization properties. However, the etching resistance required for a hard mask layer formed by the spin coating method is somewhat reduced. Therefore, there is a need for a hard mask composition that can be applied to the spin coating method, and for the hard mask layer formed by this method to have the same etching resistance as a hard mask layer formed by a chemical or physical vapor deposition method.
[0061] Therefore, in order to improve the etching resistance of the hard mask layer, research has been actively conducted to increase the carbon content of the polymer contained in the hard mask composition. However, the higher the carbon content of the polymer contained in the hard mask composition, the lower the solubility of the polymer in the solvent. Therefore, it is required to increase the carbon content of the polymer contained in the hard mask composition to improve the etching resistance of the hard mask layer formed therefrom, while preventing the solubility of the polymer in the solvent from decreasing.
[0062] The hard mask composition according to one embodiment of the present invention includes a compound containing a large-sized aromatic hydrocarbon group, thereby increasing the carbon content in the composition. Therefore, the hard mask layer formed from the composition can ensure excellent etching resistance. In addition, the compound includes a tertiary carbon or a quaternary carbon, which provides the advantage of increasing the carbon content in the composition and hardly decreasing the solubility in a solvent.
[0063] Specifically, a hard mask composition according to an embodiment of the present invention includes a polymer having a structural unit represented by the following formula 1, and a solvent:
[0064] [ka]
[0065] In the above chemical formula 1, Ar 1 teeth, (i) a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, (ii) a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or (iii) a group in which two or more of the above-mentioned substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms, two or more of the above-mentioned substituted or unsubstituted aromatic heterocyclic groups having 3 to 30 carbon atoms, or a combination thereof are linked by a single bond or a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, and R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 is not a hydrogen atom at the same time, X is a group represented by the following chemical formula 2: * indicates the connection point:
[0066] [ka]
[0067] In the above chemical formula 2, Ar 2 and Ar 3 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, M 1 and M. 2 are each independently -O-, -S-, -S(=O)-, -SO2-, or -NRa - (where R a is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms), or a combination thereof; Z is at least one selected from the group consisting of moieties listed in Group 1 below, n1 is an integer from 1 to 30; n2 is 0 or 1, * indicates a connection point.
[0068] [ka]
[0069] In the above Group 1, * indicates a connection point.
[0070] As described above, the structural unit represented by the above formula 1 contains a large aromatic hydrocarbon group, which can increase the carbon content in the polymer, and therefore the hard mask layer formed from the above composition can ensure excellent etching resistance.
[0071] In addition, R in the above chemical formula 1 1 and R 2 At least one of R is not a hydrogen atom but the above-mentioned substituent, 3 and R 4 At least one of the above is not a hydrogen atom but the above-mentioned substituent, and further, the structural unit represented by the above-mentioned chemical formula 1 contains a tertiary carbon or a quaternary carbon, whereby the solubility of the above-mentioned polymer in a solvent can be improved and an oxidation reaction during curing of a composition containing the above-mentioned polymer can be suppressed, and the gap filling properties and planarization properties of a hard mask layer formed therefrom can be improved.
[0072] In addition, since the structural unit has X represented by the above chemical formula 2, a flexible structure is present in the structural unit of the polymer, which can improve the solubility of the polymer in a solvent and can also improve the gap-filling properties and planarization properties of a hard mask layer formed from a composition containing the polymer.
[0073] In one embodiment of the present invention, Ar in the above formula 1 1 may be at least one selected from the group consisting of substituted or unsubstituted moieties listed in Group 2 below, for example, at least one selected from the group consisting of substituted or unsubstituted moieties listed in Group 2-1 below, but is not limited thereto.
[0074] [ka]
[0075] [ka]
[0076] In Group 2 and Group 2-1 above, Each Y is independently -O-, -S-, or -NR b - (where R b is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; Rx and Ry are each independently a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 10 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; for example, Rx and Ry can each independently be a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, but are not limited to these.
[0077] In one embodiment of the present invention, Ar in the above formula 1 1 may be substituted with at least one of a hydroxy group, a halogen atom, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms, or a combination thereof. Also, for example, it may be substituted with a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms. In addition, for example, it may be substituted with a hydroxy group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted heteroalkyl group having 1 to 10 carbon atoms. In addition, it may be substituted with, for example, a hydroxy group or a substituted or unsubstituted alkoxy group having 1 to 3 carbon atoms, but is not limited to these.
[0078] In one embodiment of the present invention, R 1 ~R 4 may each independently be a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a combination thereof. 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 16 carbon atoms, or a combination thereof, in which R 1 and R 2 At the same time, it is not a hydrogen atom, but R 3 and R 4is not a hydrogen atom at the same time.
[0079] R in the above Chemical Formula 1 1 and R 3 are the same or different groups, and R 2 and R 4 are the same or different groups.
[0080] In one embodiment of the present invention, Ar in the above formula 2 2 and Ar 3 are each independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, and may be, for example, at least one selected from the group consisting of the substituted or unsubstituted moieties listed in Group 3 below. 2 and Ar 3 may each independently be, for example, a substituted or unsubstituted phenylene group, a substituted or unsubstituted naphthalenylene group, a substituted or unsubstituted anthracenylene group, a substituted or unsubstituted phenanthrenylene group, or a substituted or unsubstituted pyrenylene group. Also, for example, a substituted or unsubstituted phenylene group, a substituted or unsubstituted naphthalenylene group, or a substituted or unsubstituted pyrenylene group, but is not limited thereto.
[0081] [ka]
[0082] In one embodiment of the present invention, M in the above formula 2 1 and M. 2 are each independently -O-, -S-, -S(=O)-, -SO2-, or a combination thereof, for example, but not limited to, -O-.
[0083] In one embodiment of the present invention, Z in the above chemical formula 2 is at least one selected from the group consisting of moieties listed in Group 1-1 below, for example, at least one selected from the group consisting of moieties listed in Group 1-2 below, but is not limited thereto.
[0084] [ka]
[0085] In one embodiment of the present invention, n1 in the above chemical formula 2 is one of integers from 1 to 20, for example, one of integers from 1 to 10, for example, one of integers from 1 to 5, for example, one of integers from 1 to 3, but is not limited thereto.
[0086] In one embodiment of the present invention, n1 in the above chemical formula 2 may be an integer of 1 to 10, or an integer of 1 to 5, and n2 may be 0; n1 in the above chemical formula 2 may be 1 and n2 may be 1, but is not limited thereto.
[0087] In one embodiment of the present invention, the structural unit represented by Chemical Formula 1 above may be at least one selected from the group consisting of structural units represented by Chemical Formulas 1-1 to 1-4 below.
[0088] [ka]
[0089] In the above chemical formulas 1-1 to 1-4, R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R3 and R 4 is not a hydrogen atom at the same time, Z 1 is at least one selected from the group consisting of the moieties listed in Group 1 above, R c and R d each independently represents a hydroxy group, a halogen atom, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms, or a combination thereof; Each of nc and nd is independently an integer of 0 to 6.
[0090] In one embodiment of the present invention, the structural unit represented by Chemical Formula 1 above may be at least one selected from the group consisting of structural units represented by Chemical Formulas 1-5 to 1-13 below.
[0091] [ka]
[0092] [ka]
[0093] The above polymers can be synthesized by appropriately referring to conventionally known synthesis methods. More specifically, those skilled in the art can easily synthesize the polymers by referring to the synthesis methods described in the Examples.
[0094] The polymer may have a weight average molecular weight of 1,000 g / mol to 200,000 g / mol. The polymer may have a weight average molecular weight of, for example, 1,000 g / mol to 150,000 g / mol, for example, 1,000 g / mol to 100,000 g / mol, for example, 1,200 g / mol to 50,000 g / mol, for example, 1,200 g / mol to 10,000 g / mol, but is not limited thereto. By having a weight average molecular weight in the above range, the carbon content and solubility in a solvent of the hard mask composition containing the polymer can be adjusted and optimized.
[0095] The polymer may be contained in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition. The amount may be, but is not limited to, 0.2% by mass to 30% by mass, for example, 0.5% by mass to 30% by mass, for example, 1% by mass to 30% by mass, for example, 1.5% by mass to 25% by mass, for example, 2% by mass to 20% by mass. By containing the polymer in the above content range, the thickness, surface roughness, flattening properties, etc. of the hard mask can be easily adjusted.
[0096] The hard mask composition according to one embodiment of the present invention includes a solvent. Examples of the solvent include, but are not limited to, at least one selected from the group consisting of propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate. The solvent is not particularly limited as long as it has sufficient solubility and / or dispersibility in the polymer.
[0097] The hard mask composition may further include additives such as a surfactant, a crosslinking agent, a thermal acid generator, and a plasticizer.
[0098] Examples of the surfactant that can be used include, but are not limited to, fluoroalkyl compounds, alkylbenzenesulfonates, alkylpyridinium salts, polyethylene glycols, and quaternary ammonium salts.
[0099] Examples of the type of crosslinking agent include melamine-based, substituted urea-based, and polymers thereof. A crosslinking agent having at least two crosslink-forming substituents is preferable, and for example, a compound such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, or butoxymethylated thiourea can be used.
[0100] In addition, a crosslinking agent having high heat resistance can be used as the crosslinking agent. As the crosslinking agent having high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (e.g., a benzene ring or a naphthalene ring) in the molecule can be used.
[0101] Examples of the thermal acid generator that can be used include, but are not limited to, acidic compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, and naphthalenecarboxylic acid, and / or 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, and other organic sulfonic acid alkyl esters.
[0102] According to another embodiment of the present invention, there is provided a hardmask layer comprising a cured product of the hardmask composition described above.
[0103] A method for forming a pattern using the above-described hard mask composition will now be described.
[0104] A patterning method according to one embodiment of the present invention includes the steps of providing a material layer on a substrate, applying a hard mask composition comprising the above-mentioned polymer and a solvent onto the material layer, heat-treating the hard mask composition to form a hard mask layer, forming a photoresist layer on the hard mask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.
[0105] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer is the material to be ultimately patterned, and may be, for example, a metal layer such as aluminum or copper, a semiconductor layer such as silicon, or an insulating layer such as silicon oxide or silicon nitride. The material layer may be formed, for example, by chemical vapor deposition.
[0106] The hard mask composition is as described above in detail, and may be prepared in the form of a solution and applied by spin coating. In this case, the thickness of the hard mask composition is not particularly limited, but may be, for example, 50 to 200,000 Å.
[0107] The step of heat treating the hard mask composition may be performed, for example, at 100° C. to 1,000° C. for 10 seconds to 1 hour. For example, the step of heat treating the hard mask composition may include a plurality of heat treatment steps, for example, a first heat treatment step and a second heat treatment step.
[0108] In one embodiment of the present invention, the step of heat treating the hard mask composition may include one heat treatment step performed for 10 seconds to 1 hour at 100° C. to 1000° C. As an example, the heat treatment step may be performed in an air or nitrogen atmosphere, or in an atmosphere having an oxygen concentration of 1% by mass or less.
[0109] In one embodiment of the present invention, the step of heat treating the hard mask composition includes a first heat treatment step performed at a temperature of, for example, 100°C to 1,000°C, for example, 100°C to 800°C, for example, 100°C to 500°C, for example, 150°C to 400°C, for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes.
[0110] Also, it may include a second heat treatment step successively performed at a temperature of, for example, 100° C. to 1,000° C., for example, 300° C. to 1,000° C., for example, 500° C. to 1,000° C., for example, 500° C. to 600° C., for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes. As an example, the first heat treatment step and the second heat treatment step may be performed in an air atmosphere or a nitrogen atmosphere, or may be performed in an atmosphere having an oxygen concentration of 1% by mass or less.
[0111] By performing at least one of the steps of heat treating the hard mask composition at a high temperature of 200° C. or higher, the hard mask composition can exhibit high etching resistance that can withstand etching gases and chemical solutions to which the hard mask composition is exposed in subsequent steps, including an etching step.
[0112] In one embodiment of the present invention, the step of forming a hard mask layer may include a UV / Vis (ultraviolet / visible) curing step and / or a near IR (near infrared) curing step.
[0113] In one embodiment of the present invention, the step of forming the hard mask layer may include at least one of a first heat treatment step, a second heat treatment step, a UV / Vis curing step, and a near IR curing step, or may include two or more steps consecutively.
[0114] In one embodiment of the present invention, the method may further include forming a silicon-containing thin film layer on the hard mask layer. The silicon-containing thin film layer may be formed of a material such as SiCN, SiOC, SiON, SiOCN, SiC, SiO, and / or SiN.
[0115] In one embodiment of the present invention, before the step of forming the photoresist layer, a bottom anti-reflective coating (BARC) may be further formed on the silicon-containing thin film layer or the hard mask layer.
[0116] In one embodiment of the present invention, the step of exposing the photoresist layer can be performed using, for example, an ArF excimer laser, a KrF excimer laser, or EUV (extreme ultraviolet), etc. After the exposure, a heat treatment process can be performed at a temperature of 100°C to 700°C.
[0117] In one embodiment of the present invention, the step of etching the exposed portions of the material layer can be performed by dry etching using an etching gas, which can be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3, and mixtures thereof.
[0118] The etched material layer can be formed in a variety of patterns, which can be diverse, such as metal patterns, semiconductor patterns, insulating patterns, etc., and can be applied as various patterns within a semiconductor integrated circuit device, for example. EXAMPLES
[0119] The above-mentioned embodiments of the present invention will be described in more detail with reference to the following examples. However, the following examples are merely for illustrative purposes and are not intended to limit the scope of the present invention.
[0120] [Polymer synthesis] (Synthesis Example 1) (1st step) A solution was prepared by adding 70.08 g of 4,4'-oxybis(benzoyl chloride) and 350.00 g of tetrahydrofuran to a flask. 79.92 g of methylmagnesium bromide was gradually added to this solution in an ice bath, and the solution was stirred until all of the 4,4'-oxybis(benzoyl chloride) had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product A-1.
[0121] (2nd process) A solution was prepared by adding 37.54 g of the intermediate product A-1 and 360.00 g of N,N-dimethylformamide to a flask. 9.44 g of sodium hydride was gradually added to this solution at room temperature, and then 93.03 g of methyl iodide was added and stirred until all of the intermediate product A-1 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product A-2.
[0122] (3rd step) 69.80 g of the intermediate product A-2, 48.45 g of 1-hydroxypyrene, 1.74 g of sulfuric acid, and 80.00 g of propylene glycol monomethyl ether acetate were added to a flask, and the mixture was reacted for 8 hours with stirring at 100° C. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, n-hexane was added, and the generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula A (Mw: 3,082 g / mol).
[0123] [ka]
[0124] (Synthesis Example 2) Into a flask, 48.84 g of the intermediate product A-2 obtained in Synthesis Example 1 above, 48.82 g of 9,9-bis(6-hydroxy-2-naphthyl)fluorene, 1.22 g of sulfuric acid, and 80.00 g of propylene glycol monomethyl ether acetate were added, and the mixture was reacted for 7 hours at 100° C. with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, n-hexane was added, and the generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula B (Mw: 3,020 g / mol).
[0125] [ka]
[0126] (Synthesis Example 3) (1st step) A solution was prepared by adding 71.20 g of 4,4'-oxybis(benzaldehyde) and 350.00 g of tetrahydrofuran to a flask. 78.80 g of methylmagnesium bromide was gradually added to this solution in an ice bath, and the solution was stirred until all of the 4,4'-oxybis(benzaldehyde) had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product C-1.
[0127] (2nd process) A solution was prepared by adding 37.26 g of the intermediate product C-1 and 350.00 g of N,N-dimethylformaldehyde to a flask. 10.38 g of sodium hydride was gradually added to this solution at room temperature, and then 102.36 g of methyl iodide was added and stirred until all of the intermediate product C-1 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product C-2.
[0128] (3rd step) The intermediate product C-2 (67.06 g), 1-hydroxypyrene (51.11 g), sulfuric acid (1.84 g), and propylene glycol monomethyl ether acetate (80.00 g) were added to a flask, and the mixture was reacted for 8 hours with stirring at 100° C. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, n-hexane was added, and the generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula C (Mw: 2,920 g / mol).
[0129] [ka]
[0130] (Synthesis Example 4) 46.14 g of the intermediate product C-2 obtained in Synthesis Example 3 above, 72.59 g of 9,9-bis(6-hydroxy-2-naphthyl)fluorene, 1.26 g of sulfuric acid, and 80.00 g of propylene glycol monomethyl ether acetate were added to a flask, and the mixture was reacted for 9 hours at 100° C. with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, n-hexane was added, and the generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula D (Mw: 3,020 g / mol).
[0131] [ka]
[0132] (Synthesis Example 5) (1st step) A solution was prepared by adding 73.29 g of 4,4'-oxybis(benzaldehyde) and 350.00 g of tetrahydrofuran to a flask. 96.71 g of phenylmagnesium chloride was gradually added to this solution in an ice bath, and the solution was stirred until all of the 4,4'-oxybis(benzaldehyde) had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product E-1.
[0133] (2nd process) A solution was prepared by adding 49.28 g of the intermediate product E-1 and 350.00 g of N,N-dimethylformamide to a flask. 9.28 g of sodium hydride was gradually added to this solution at room temperature, and then 91.44 g of methyl iodide was added and stirred until all of the intermediate product E-1 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product E-2.
[0134] (3rd step) The intermediate product E-2 (56.69 g), 9,9-bis(6-hydroxy-2-naphthyl)fluorene (62.22 g), sulfuric acid (1.08 g), and propylene glycol monomethyl ether acetate (80.00 g) were added to a flask, and the mixture was reacted for 8 hours at 100° C. with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, and n-hexane was added to generate a solid, which was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula E (Mw: 3,120 g / mol).
[0135] [ka]
[0136] (Synthesis Example 6) (1st step) A solution was prepared by adding 36.87 g of 4,4'-oxybis(benzaldehyde) and 350.00 g of tetrahydrofuran to a flask. 113.13 g of 2-naphthylmagnesium bromide was gradually added to this solution in an ice bath, and the solution was stirred until all of the 4,4'-oxybis(benzaldehyde) had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product F-1.
[0137] (2nd process) A solution was prepared by adding 57.26 g of the intermediate product F-1 and 350.00 g of N,N-dimethylformamide to a flask. 8.54 g of sodium hydride was gradually added to this solution at room temperature, and then 84.20 g of methyl iodide was added and stirred until all of the intermediate product F-1 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product F-2.
[0138] (3rd step) The intermediate product F-2 (63.23 g), 9,9-bis(6-hydroxy-2-naphthyl)fluorene (55.79 g), sulfuric acid (0.97 g), and propylene glycol monomethyl ether acetate (80.00 g) were added to a flask, and the mixture was reacted at 100° C. for 12 hours with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, and n-hexane was added to generate a solid, which was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula F (Mw: 2,890 g / mol).
[0139] [ka]
[0140] (Synthesis Example 7) (1st step) A solution was prepared by adding 70.33 g of 9,9-bis(4-hydroxyphenyl)fluorene, 50.32 g of 4-fluorobenzaldehyde, 69.35 g of potassium carbonate, and 310.00 g of N,N-dimethylformamide to a flask. The mixture was stirred at 140°C until all of the 9,9-bis(4-hydroxyphenyl)fluorene had reacted. After the reaction was completed, the mixture was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product G-1.
[0141] (2nd process) A solution was prepared by adding 66.89 g of the intermediate product G-1 and 350.00 g of tetrahydrofuran to a flask. 83.11 g of phenylmagnesium chloride was gradually added to this solution in an ice bath, and the mixture was stirred until all of the intermediate product G-1 reacted. After the reaction was completed, the mixture was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product G-2.
[0142] (3rd step) A solution was prepared by adding 71.65 g of the intermediate product G-2 and 350.00 g of N,N-dimethylformamide to a flask. 7.22 g of sodium hydride was added to this solution at room temperature and stirred at 60°C for 2 hours. After stirring, 71.13 g of methyl iodide was added at room temperature and stirred until all of the intermediate product G-2 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product G-3.
[0143] (4th step) 74.21 g of the intermediate product G-3, 45.01 g of 9,9-bis(6-hydroxy-2-naphthyl)fluorene, 0.78 g of sulfuric acid, and 80.00 g of propylene glycol monomethyl ether acetate were added to a flask, and the mixture was reacted for 29 hours with stirring at 110° C. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, n-hexane was added, and the generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula G (Mw: 2,996 g / mol).
[0144] [ka]
[0145] (Synthesis Example 8) (1st step) A solution was prepared by adding 58.98 g of 4,4'-cyclohexylidenebisphenol, 55.10 g of 4-fluorobenzaldehyde, 75.93 g of potassium carbonate, and 310.00 g of N,N-dimethylformamide to a flask. The mixture was stirred at 140°C until all of the 4,4'-cyclohexylidenebisphenol had reacted. After the reaction was completed, the mixture was neutralized with a 1% by mass aqueous hydrochloric acid solution until the pH was about 7, then washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product H-1.
[0146] (2nd process) A solution was prepared by adding 61.06 g of the intermediate product H-1 and 350.00 g of tetrahydrofuran to a flask. 88.94 g of phenylmagnesium chloride was gradually added to this solution in an ice bath, and the mixture was stirred until all of the intermediate product H-1 had reacted. After the reaction was completed, the mixture was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product H-2.
[0147] (3rd step) A solution was prepared by adding 67.10 g of the intermediate product H-2 and 350.00 g of N,N-dimethylformamide to a flask. 7.64 g of sodium hydride was gradually added to this solution at room temperature, and then 75.26 g of methyl iodide was added and stirred until all of the intermediate product H-2 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product H-3.
[0148] (4th step) 70.85 g of the intermediate product H-3, 48.31 g of 9,9-bis(6-hydroxy-2-naphthyl)fluorene, 0.84 g of sulfuric acid, and 80.00 g of propylene glycol monomethyl ether acetate were added to a flask, and the mixture was reacted for 8 hours at 100° C. with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, and n-hexane was added. The generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula H (Mw: 3,102 g / mol).
[0149] [ka]
[0150] (Synthesis Example 9) (1st step) A solution was prepared by adding 29.62 g of 1,4-dihydroxybenzene, 67.44 g of 4-fluorobenzaldehyde, 92.94 g of potassium carbonate, and 310.00 g of N,N-dimethylformamide to a flask. The mixture was stirred at 140°C until all of the 1,4-dihydroxybenzaldehyde had reacted. After the reaction was completed, the mixture was neutralized to a pH of about 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product I-1.
[0151] (2nd process) A solution was prepared by adding 47.16 g of the intermediate product I-1 and 350.00 g of tetrahydrofuran to a flask. 102.84 g of phenylmagnesium chloride was gradually added to this solution in an ice bath, and the mixture was stirred until all of the intermediate product I-1 had reacted. After the reaction was completed, the mixture was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed, concentrated under reduced pressure, and purified using a column to obtain intermediate product I-2.
[0152] (3rd step) A solution was prepared by adding 56.66 g of the intermediate product I-2 and 350.00 g of N,N-dimethylformamide to a flask. 8.60 g of sodium hydride was gradually added to this solution at room temperature, and then 84.74 g of methyl iodide was added and stirred until all of the intermediate product I-2 had reacted. After the reaction was completed, the solution was neutralized to about pH 7 using a 1% by mass aqueous hydrochloric acid solution, washed and concentrated under reduced pressure, and purified using a column to obtain intermediate product I-3.
[0153] (4th step) The intermediate product I-3 (62.76 g), 9,9-bis(6-hydroxy-2-naphthyl)fluorene (56.26 g), sulfuric acid (0.98 g), and propylene glycol monomethyl ether acetate (80.00 g) were added to a flask, and the mixture was reacted at 100° C. for 9 hours with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, and n-hexane was added. The generated solid was filtered, extracted, and dried under reduced pressure to obtain a polymer containing a structural unit represented by the following chemical formula I (Mw: 3,084 g / mol).
[0154] [ka]
[0155] (Comparative synthesis example) 75.44 g of 9,9-bis(6-hydroxy-2-naphthyl)fluorene, 46.25 g of 4,4'-bis(methoxymethyl)benzene, 1.31 g of sulfuric acid, and 80.00 g of propylene glycol monomethyl ether acetate were added to a flask, and the mixture was reacted for 10 hours at 100° C. with stirring. After the reaction was completed, the mixture was washed and concentrated under reduced pressure, and n-hexane was added. The generated solid was filtered, extracted, and dried under reduced pressure to obtain a comparative polymer containing a structural unit represented by the following chemical formula J (Mw: 3,010 g / mol).
[0156] [ka]
[0157] [Preparation of hard mask composition] (Examples 1 to 9 and Comparative Example 1) The polymers obtained in Synthesis Examples 1 to 9 and the comparative polymers obtained in Comparative Synthesis Examples were each dissolved in cyclohexanone, and then filtered through a membrane filter having a diameter of 0.1 μm to produce hard mask compositions having a compound content of 10.0 mass %.
[0158] [Evaluation 1: Gap-fill characteristics] The hard mask compositions according to Examples 1 to 9 and Comparative Example 1 were each coated on a patterned silicon wafer by spin coating, and then heat-treated at 400° C. for 60 seconds to form a hard mask layer. A field emission scanning electron microscope (FE-SEM) was used to observe the cross-sectional image of the hard mask layer pattern to check for the presence or absence of voids. The results are shown in Table 1 below.
[0159] [Table 1]
[0160] Referring to Table 1 above, it was found that no voids were formed in the hard mask layers formed from the hard mask compositions according to the Examples and Comparative Examples, and therefore there was no difference in the gap fill properties between the hard mask compositions according to the Examples and Comparative Examples.
[0161] [Evaluation 2: Flattening properties] The hard mask compositions according to Examples 1 to 9 and Comparative Example 1 were coated on a patterned silicon wafer by spin coating, and then heat-treated at 400° C. for 60 seconds to form a hard mask layer. Then, a field emission scanning electron microscope (FE-SEM) was used to observe the cross-sectional image of the pattern. The thickness of the hard mask layer shown in the cross-sectional image of the pattern was measured, and the planarization characteristics were quantified according to the calculation formula of FIG. 1. In FIG. 1, h1 means the average value of the thickness of the hard mask layer measured at three arbitrary points where no pattern was formed, and h2 means the average value of the thickness of the hard mask layer measured at three arbitrary points where a pattern was formed. When the result of the quantification of the planarization characteristics was less than 5, it was expressed as “A (very good)”, when it was 5 or more and less than 10, it was expressed as “B (good)”, and when it was 10 or more, it was expressed as “C (poor)”. The results are shown in Table 2 below.
[0162] [Table 2]
[0163] Referring to Table 2 above, it can be seen that the planarization characteristics of the hard mask layers formed from the hard mask compositions according to Examples 1 to 9 are very good, whereas the planarization characteristics of the hard mask layers according to the comparative examples are inferior to all the examples.
[0164] [Evaluation 3: Etching resistance] The hard mask compositions according to Examples 1 to 9 and Comparative Example 1 were coated on a silicon wafer by spin coating, and then heat-treated at 400°C for 60 seconds to form a hard mask layer. The hard mask layer was dry-etched for 30 seconds using a CF4 / Ar mixed gas, and the thickness of the hard mask layer before and after etching was measured using a thin film thickness measuring device manufactured by K-MAC, and the etching rate (bulk etch rate, BER) was calculated according to the following calculation formula 2. The etching resistance was evaluated by the ratio of the etching rate of the hard mask layer formed from the composition according to Examples 1 to 9 to the etching rate of the hard mask layer formed from the composition according to Comparative Example 1. Specifically, if the etching rate ratio was less than 0.95, it was expressed as "A (very good)", if it was 0.95 or more and less than 1.00, it was expressed as "B (good)", and if it was 1.00 or more, it was expressed as "C (poor)". The results are shown in Table 3 below.
[0165]
number
[0166] [Table 3]
[0167] Referring to Table 3 above, it can be seen that the etching resistance of the hard mask layer according to the embodiment is superior to the etching resistance of the hard mask layer according to the comparative example.
[0168] [Evaluation 4: Evaluation of contractility] The hard mask compositions according to Examples 1 to 9 and Comparative Example 1 were coated on a silicon wafer by spin coating, and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The thickness of the hard mask layer was measured using a thin film thickness measuring device manufactured by K-MAC. Next, the hard mask layer was re-heat-treated at 400°C for 1 minute, and the thickness of the hard mask layer was measured. The difference in thickness of the hard mask layer before and after the heat treatment was calculated, and when it was less than 90% of the value of Comparative Example 1, it was evaluated as "A (very good)", when it was 90% or more but less than 95%, it was evaluated as "B (good)", and when it was 95% or more, it was evaluated as "C (poor)". The results are shown in Table 4 below.
[0169] [Table 4]
[0170] Referring to Table 4 above, it can be seen that the hard mask layers formed from the compositions of Examples 1 to 9 had lower shrinkage rates than the hard mask layer formed from the composition of Comparative Example 1.
[0171] From the above, it was found that the hard mask layers formed from the compositions according to Examples 1 to 9 were all excellent in gap-filling properties, planarization properties, etching resistance, and shrinkage. On the other hand, it was confirmed that the hard mask layers formed from the compositions according to the comparative examples had the same gap-filling properties as the hard mask layers of the Examples, but were inferior in planarization properties, etching resistance, and shrinkage to the hard mask layers of the Examples of the present invention.
[0172] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.
Claims
1. A hard mask composition comprising a polymer having a structural unit represented by the following chemical formula 1, and a solvent: 【Chemistry 1】 In the above Chemical Formula 1, Ar 1 teeth, (i) a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, (ii) a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or (iii) a group in which two or more of the above-mentioned substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms, two or more of the above-mentioned substituted or unsubstituted aromatic heterocycles having 3 to 30 carbon atoms, or a combination thereof are linked by a single bond or a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, and R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 is not a hydrogen atom at the same time, X is a group represented by the following chemical formula 2: * is the connection point: 【Chemistry 2】 In the above Chemical Formula 2, Ar 2 and Ar 3 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, M 1 and M. 2 are each independently -O-, -S-, -S(=O)-, or -SO 2 --, --NR a - (where R a is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms), or a combination thereof; Z is at least one selected from the group consisting of moieties listed in Group 1 below, n1 is an integer from 1 to 30; n2 is 0 or 1; * is the connection point: 【Chemistry 3】 In Group 1, * indicates a connection point.
2. Ar in Formula 1 1 is at least one selected from the group consisting of substituted or unsubstituted moieties listed in Group 2 below: 【Chemistry 4】 In Group 2, Each Y is independently -O-, -S-, or -NR b - (where R b is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; Rx and Ry are each independently a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 10 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.
3. Ar in Formula 1 1 is a group substituted with at least one of a hydroxy group, a halogen atom, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms, or a combination thereof.
4. R in Formula 1 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 and are not simultaneously hydrogen atoms.
5. R in Formula 1 1 and R 3 are the same group, and R 2 and R 4 The hardmask composition of claim 1 , wherein are the same group.
6. Ar in Formula 1 1 is at least one of the substituted or unsubstituted moieties listed in Group 2-1 below, R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 16 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 and are not simultaneously hydrogen atoms. 【Chemistry 5】 In the group 2-1, Each Y is independently -O-, -S-, or -NR b - (where R b is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; Rx and Ry each independently represent a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.
7. Ar in Formula 2 2 and Ar 3 10. The hard mask composition of claim 1, wherein each independently is at least one of the substituted or unsubstituted moieties listed in Group 3 below. 【Chemistry 6】
8. Ar in Formula 2 2 and Ar 3 wherein each is independently a substituted or unsubstituted phenylene group, a substituted or unsubstituted naphthalenylene group, a substituted or unsubstituted phenanthrenylene group, a substituted or unsubstituted anthracenylene group, or a substituted or unsubstituted pyrenylene group.
9. Ar in Formula 2 2 and Ar 3 are each independently a substituted or unsubstituted phenylene group, a substituted or unsubstituted naphthalenylene group, or a substituted or unsubstituted pyrenylene group; M 1 and M. 2 is -O-; Z is at least one of the moieties listed in Group 1-1 below; and n1 is an integer from 1 to 5. 【Chemistry 7】 In the group 1-1, * indicates a connection point.
10. The hard mask composition of claim 1 , wherein n1 and n2 in Formula 2 are 1.
11. 2. The hard mask composition of claim 1, wherein n1 in Formula 2 is an integer of 1 to 5, and n2 is 0.
12. The hard mask composition according to claim 1, wherein the structural unit represented by Chemical Formula 1 is at least one of structural units represented by the following Chemical Formulas 1-1 to 1-4: 【Chemistry 8】 In the above Chemical Formula 1-1 to Chemical Formula 1-4, R 1 ~R 4 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a combination thereof, in which R 1 and R 2 is not a hydrogen atom at the same time, R 3 and R 4 is not a hydrogen atom at the same time, Z 1 is at least one selected from the group consisting of the moieties listed in Group 1 below, R c and R d each independently represents a hydroxy group, a halogen atom, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 20 carbon atoms, or a combination thereof; n c and nd are each independently an integer from 0 to 6; * is the connection point: 【Chemistry 9】 In Group 1, * indicates a connection point.
13. The hard mask composition according to claim 1, wherein the structural unit represented by Chemical Formula 1 is at least one selected from the group consisting of structural units represented by the following Chemical Formulas 1-5 to 1-13: 【Chemistry 10】 【Chemistry 11】 In the above chemical formulas 1-5 to 1-13, * represents a linking point.
14. 2. The hard mask composition of claim 1, wherein the weight average molecular weight of the polymer is from 1,000 g / mol to 200,000 g / mol.
15. The hard mask composition of claim 1 , wherein the polymer is present in an amount of 0.1% by weight to 30% by weight based on the total weight of the hard mask composition.
16. 2. The hard mask composition of claim 1, wherein the solvent is at least one selected from the group consisting of propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate.
17. A hardmask layer comprising a cured product of the hardmask composition according to any one of claims 1 to 16.
18. Providing a layer of material on a substrate; applying a hard mask composition according to any one of claims 1 to 16 onto the material layer; heat-treating the hard mask composition to form a hard mask layer; forming a photoresist layer over the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose portions of the material layer; etching the exposed portions of the layer of material; A pattern forming method comprising:
19. The method of claim 18, wherein the step of forming the hard mask layer comprises a step of performing a heat treatment at 100° C. to 1,000° C.
Citation Information
Patent Citations
Naphthalene derivative, resist underlayer film material, resist underlayer film forming method, and pattern forming method
JP2012001687A
Semiconductor substrate production method and composition
WO2022270484A1
Resist underlayer film-forming composition
WO2023048021A1
Hardmask composition, hardmask layer and method of forming patterns
KR1020220092160A