Polymer

A polymer synthesized via Friedel-Crafts polyhydroxyalkylation reaction addresses the limitations of existing polymers by providing low dielectric loss tangent and broad solvent solubility, suitable for high-frequency electronic devices.

JP2024161918APending Publication Date: 2024-11-20AKITA UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024076120
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-05-08
Publication Date
2024-11-20

AI Technical Summary

Technical Problem

Existing polymers used in high-frequency electronic devices have limited solvent solubility and require toxic solvents, and as communication frequencies increase, materials with better low dielectric properties are needed.

Method used

A polymer synthesized through the Friedel-Crafts polyhydroxyalkylation reaction, represented by chemical formula (1), which has low polarity and excellent solvent solubility, particularly in amide solvents, is developed, utilizing a divalent organic group with an aromatic ring and a weight average molecular weight of 1,000 to 250,000.

Benefits of technology

The polymer exhibits excellent low dielectric loss tangent properties, improved solvent solubility, and enhanced handling characteristics, making it suitable for electronic materials, especially in high-frequency applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161918000001
    Figure 2024161918000001
  • Figure 2024161918000002
    Figure 2024161918000002
  • Figure 2024161918000003
    Figure 2024161918000003
Patent Text Reader

Abstract

To provide techniques relating to polymers for novel electronic materials soluble in various solvents such as amide solvents, with outstanding low dielectric properties.SOLUTION: A polymer according to one embodiment is represented by the following formula (1). The polymer is used as an electronic material. In formula (1), X is a divalent organic group with an aromatic ring.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polymers. [Background technology]

[0002] With the spread of high-capacity, high-speed communications such as the fifth generation communication system (5G) and millimeter wave radar for automotive ADAS (advanced driving systems), signals from communication devices are becoming increasingly high frequency. For wiring board materials used in electronic devices operated at such high frequencies, low dielectric properties are required in order to suppress transmission loss. For this reason, polyphenylene ether, which has excellent low dielectric properties, is used, for example, as described in Patent Document 1. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-198780 A [Non-patent literature]

[0004] [Non-Patent Document 1] ACS Omega,2021,6,4921-4931. Summary of the Invention [Problem to be solved by the invention]

[0005] However, polyphenylene ether is soluble in only limited solvents, and highly toxic solvents such as toluene are used even in Patent Document 1. This causes problems such as difficulty in handling the resin varnish and controlling exposure to the solvent. Furthermore, as communication signals become increasingly higher in frequency, there is a demand for materials with even better low dielectric properties. The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a new resin material for electronic materials which has excellent low dielectric properties and is soluble in various solvents such as amide-based solvents. [Means for solving the problem]

[0006] A low dielectric tangent is important to reduce transmission loss in the high frequency band. The inventors have noticed that since the dielectric tangent is significantly affected by molecular polarization, a low polarity polymer is required to achieve a low dielectric tangent. As a result of intensive research, they have newly discovered that the Friedel-Crafts polyhydroxyalkylation reaction shown in, for example, Non-Patent Document 1, is a reaction in which a polar aldehyde or ketone reacts with a nucleophile to synthesize a polymer without a polar group, and that the polymer obtained by this reaction has excellent low dielectric tangent characteristics. They have also discovered that these polymers have excellent solvent solubility. That is, the present inventors have discovered that polymers obtained by the Friedel-Crafts polyhydroxyalkylation reaction have excellent properties such as low dielectric tangent and solvent solubility, and can provide resin materials that are particularly suitable for electronic material applications, and have thus completed the present invention. An embodiment of the present invention is a polymer, which is represented by the following chemical formula (1) and is used as an electronic material. [ka] In the above chemical formula (1), X is a divalent organic group having an aromatic ring. The polymer of the above embodiment may have a weight average molecular weight of 1,000 to 250,000. Another aspect of the present invention is a resin composition for electronic materials, which contains the polymer represented by the above chemical formula (1). Effect of the Invention

[0007] According to the present invention, it is possible to provide a technology relating to a new polymer for use as an electronic material, which has excellent low dielectric properties and is soluble in various solvents such as amide-based solvents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expression "a to b" in the explanation of a numerical range means that the range is from a to b, unless otherwise specified.

[0009] (polymer) The polymer according to the embodiment is represented by the following chemical formula (1). [ka] In the above chemical formula (1), X is a divalent organic group having an aromatic ring. The divalent organic group having an aromatic ring is not particularly limited, but examples thereof include organic groups of the following formulae (2-1) to (2-8). [ka] In the polymer represented by chemical formula (1), the carbonyl group, which is a polar group of the raw material 2,2,2-trifluoroacetophenone described later, disappears by dehydration condensation. This reduces the polarity of the polymer, and preferably results in low polarity and excellent low dielectric tangent characteristics.

[0010] The weight average molecular weight (Mw) of the polymer represented by the above chemical formula (1) is, for example, 1,000 to 500,000, preferably 1,000 to 250,000, and more preferably 100,000 to 250,000. The weight average molecular weight (Mw) is measured by gel permeation chromatography (GPC) using polystyrene as the conversion standard.

[0011] The polymer according to the embodiment has an Mw of 1,000 to 250,000, and is therefore particularly suitable for electronic material applications because it has excellent solubility in general organic solvents such as amide solvents, chloroform, and tetrahydrofuran, and excellent handling properties in varnishes after dissolution. In addition, the polymer according to the embodiment has excellent dielectric properties, heat resistance, and strength. The molecular weight dispersity (Mw / Mn) of the polymer according to the embodiment is preferably 1.2 to 4.0.

[0012] The polymer of the present embodiment has excellent dielectric properties, heat resistance, and strength, and can therefore be suitably used as an electronic material for electronic components.

[0013] Examples of electronic components include LSIs (large-scale integrated circuits) used in personal computers, smartphones, and next-generation mobile communication systems such as 5G. The polymer of the present embodiment is preferably used to form an insulating film in the LSI, more preferably used to form a permanent coating, and even more preferably used to form a solder resist, an interlayer insulating layer, a coverlay, and an encapsulant.

[0014] (Polymer manufacturing method) The method for producing a polymer according to the embodiment includes a reaction step of reacting 2,2,2-trifluoroacetophenone (hereinafter referred to as TFAP) with an aromatic compound in a liquid containing a superacid, an organic solvent, TFAP, and an aromatic compound.

[0015] The following is a generalized reaction scheme showing the Friedel-Crafts polycondensation reaction that proceeds in the above reaction process. [ka] As shown in the above reaction formula, the polymer obtained by the reaction process of the present embodiment contains a structural unit represented by the following chemical formula (1): In the following chemical formula (1), X is a divalent organic group having an aromatic ring. [ka]

[0016] As shown in the above reaction formula, the Friedel-Crafts polycondensation reaction proceeds in the presence of a super strong acid. This reaction causes the carbonyl group, which is a polar group contained in TFAP, to disappear through dehydration condensation. This reduces the polarity of the polymer represented by chemical formula (1), and preferably produces a low-polarity polymer.

[0017] Each compound used in the above-mentioned reaction steps will now be described.

[0018] <Aromatic compounds> Examples of the aromatic compound include a bridged tricyclic compound, a bridged bicyclic compound, a monocyclic compound, and a condensed polycyclic compound.

[0019] Examples of the bridged tricyclic compound include p-terphenyl and m-terphenyl.

[0020] Examples of bridged bicyclic compounds include biphenyl, diphenyl ether, dibenzofuran, and 2,2'-dimethoxybiphenyl.

[0021] An example of a monocyclic compound is benzene.

[0022] Examples of the condensed polycyclic compounds include naphthalene, phenanthrene, and anthracene.

[0023] <Super strong acid> A super strong acid refers to an acid that is more acidic than 100% sulfuric acid. Examples of the super strong acid include trifluoromethanesulfonic acid (CF3SO3H) and fluorosulfonic acid (FSO3H). In this embodiment, the Friedel-Crafts polycondensation reaction proceeds in a mixed solution of a super strong acid and an organic solvent described below. In a liquid containing a super strong acid, an organic solvent, 2,2,2-trifluoroacetophenone (hereinafter referred to as TFAP), and an aromatic compound, the molar ratio of the super strong acid to TFAP (moles of super strong acid / moles of TFAP) is preferably 2.0 to 5.0. This makes it possible to obtain a polymer exhibiting sufficient strength.

[0024] <Organic solvent> The organic solvent is not particularly limited as long as it is compatible with the super strong acid and does not inhibit the above-mentioned Friedel-Crafts polycondensation reaction. Such organic solvents include one or more selected from the group consisting of dichloromethane, chloroform, 1,2-dichloroethane, nitromethane, and trifluoroacetic acid. Among these, it is preferable to use a halogenated hydrocarbon such as dichloromethane as the organic solvent from the viewpoints of compatibility with the super strong acid, resistance or stability to the super strong acid, and suitability as a reaction field.

[0025] According to the above-described method for producing a polymer, the reaction between TFAP and an aromatic compound is carried out in a mixed solution of a super strong acid and an organic solvent, thereby reducing the amount of the super strong acid used, and thus reducing the production cost of the polymer compared to the case where the reaction is carried out in a solution consisting of only a super strong acid. In addition, the degree of polymerization of the resulting polymer can be suppressed compared to when the reaction is carried out in a solution consisting of only a super strong acid, and this leads to a polymer with improved solubility in organic solvents and reduced polarity. The polymer obtained by the above-described method for producing a polymer has the following characteristics: excellent dielectric properties, high strength, and excellent heat resistance.

[0026] (Resin composition for electronic materials) The electronic material resin composition according to the embodiment contains the polymer represented by the above chemical formula (1). The electronic material composition also contains at least one other component.

[0027] Examples of other components include organic solvents, inorganic fillers such as silica, peroxides, crosslinking curing agents, polymerization initiators, resin and polymer components such as maleimide resins, styrene-based elastomers, and polyphenylene ether, as well as additives such as sensitizers, adhesion aids, surfactants, leveling agents, plasticizers, adhesion agents, colorants, fibers, silane coupling agents, flame retardants, cellulose nanofibers, dispersants, thermosetting catalysts, thickeners, defoamers, antioxidants, rust inhibitors, and adhesion imparting agents. By including these components, it is possible to impart various properties to the electronic material composition, and the composition can be preferably used for electronic material applications.

[0028] In particular, the polymer represented by the above chemical formula (1) has excellent solubility in general organic solvents, and can be used as a resin composition for electronic materials containing an organic solvent. The resin composition for electronic materials containing an organic solvent can be easily handled as a varnish, and even when other components other than the organic solvent are added, the resin composition for electronic materials can be easily adjusted. In addition, since it has excellent dielectric properties, it can be particularly preferably used for electronic material applications.

[0029] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES

[0030] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0031] Example 1 A mixed solvent was prepared by mixing 2.7 mL (30 mmol) of trifluoromethanesulfonic acid (CF3SO3H) and 7.5 mL of dichloromethane. 1.045 g (6.0 mmol) of TFAP (molar ratio of CF3SO3H to TFAP: 5.0) and 1.152 g (5.0 mmol) of p-terphenyl were added to this mixed solvent and stirred at 25°C for 30 minutes. After stirring, the mixture was added to methanol to precipitate a solid reactant. The resulting precipitate was removed by suction filtration and then vacuum dried overnight at room temperature. The resulting solid was dissolved in chloroform and then added to methanol to precipitate a solid reactant. The resulting precipitate was removed by suction filtration and then vacuum dried overnight at 50°C to obtain a polymer represented by the following chemical formula. [ka] The polymer of Example 1 had a polystyrene-equivalent weight average molecular weight (Mw) of 100,400 as measured by GPC, and Mw / Mn of 1.5.

[0032] Example 2 A polymer of Example 2 represented by the following chemical formula was obtained using the same molar ratio and procedure as in Example 1, except that m-terphenyl was used instead of p-terphenyl and the reaction time in the mixed solvent was 2 hours. [ka] With respect to the polymer of Example 2, the weight average molecular weight (Mw) in terms of polystyrene measured by GPC was 103,700, and the Mw / Mn was 1.8.

[0033] Example 3 A polymer of Example 3 represented by the following chemical formula was obtained using the same molar ratio and procedure as in Example 1, except that dibenzofuran was used instead of p-terphenyl and the reaction time in the mixed solvent was 1 hour. [ka] The polymer of Example 3 had a weight average molecular weight (Mw) of 245,200 and Mw / Mn of 3.4, calculated based on polystyrene standards by GPC.

[0034] Example 4 A polymer of Example 4 represented by the following chemical formula was obtained using the same molar ratio and procedure as in Example 1, except that biphenyl was used instead of p-terphenyl and the reaction time in the mixed solvent was 24 hours. [ka] The polymer of Example 4 had a weight average molecular weight (Mw) of 169,100 and Mw / Mn of 2.6, calculated based on polystyrene standards by GPC.

[0035] Example 5 A mixed solvent was prepared by mixing 1.1 mL (12 mmol) of trifluoromethanesulfonic acid (CF3SO3H) and 7.5 mL of dichloromethane. 1.045 g (6.0 mmol) of TFAP (molar ratio of CF3SO3H to TFAP: 2.0) and 0.851 g (5.0 mmol) of diphenyl ether were added to this mixed solvent and stirred at 25°C for 2 hours. After stirring, the mixture was added to methanol to precipitate a solid reaction product. The resulting precipitate was removed by suction filtration and then vacuum dried overnight at room temperature. The resulting solid was dissolved in chloroform and then added to methanol to precipitate a solid reaction product. The resulting precipitate was removed by suction filtration and then vacuum dried overnight at 50°C to obtain a polymer represented by the following chemical formula. [ka] The polymer of Example 5 had a weight average molecular weight (Mw) of 100,400 and Mw / Mn of 1.5, calculated based on polystyrene standards by GPC.

[0036] Example 6 The polymer of Example 6, represented by the following chemical formula, was obtained using the same molar ratio and procedure as in Example 5, except that 2,2'-dimethoxybiphenyl was used instead of diphenyl ether and the reaction time in the mixed solvent was 25 hours. [ka] The polymer of Example 6 had a weight average molecular weight (Mw) of 170,500 and Mw / Mn of 3.2, calculated based on polystyrene standards by GPC.

[0037] Comparative Example 1 In a 500mL separable flask, 19.8g (0.162mol) of 2,6-dimethylphenol and 2.42g (0.018mol) of 2-allylphenol were dissolved in 261g of toluene as raw material phenols to prepare a raw material solution. Furthermore, di-μ-hydroxo-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride (Cu / TMEDA) was adjusted to 0.18wt% and tetramethylethylenediamine (TMEDA) to 0.16wt%, and the reaction was carried out at 40℃ for 8 hours while blowing dry air into the reaction solution at a flow rate of 75mL / min, stirring at a stirring speed of 200rpm. After stopping the heating of the reaction solution and the blowing of dry air, di-μ-hydroxo-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride (Cu / TMEDA) was removed by filtration, and reprecipitated in a mixture of 1,200 mL of methanol, 4.0 mL of concentrated hydrochloric acid, and 27.0 mL of HO. The precipitate was then filtered under reduced pressure, washed with methanol, and dried at 80° C. for 24 hours to obtain the polymer (polyphenylene ether) of Comparative Example 1. Regarding the polymer of Comparative Example 1, the weight average molecular weight (Mw) in terms of polystyrene measured by GPC was 43,400, and Mw / Mn was 2.7.

[0038] <Preparation of test samples> 5 mL of chloroform was added to 0.3 g of each polymer of Examples 1 to 4 and Comparative Example 1, and the mixture was stirred to prepare a polymer solution. The obtained polymer solution was poured into a flat glass petri dish having a diameter of 7 cm, and the solvent was evaporated at room temperature, after which the film was peeled off from the petri dish. The obtained film was dried at 100° C. for 12 hours to prepare a test sample. The film thickness was approximately 50 μm.

[0039] <Dielectric property evaluation> The test sample was cut into a length of 80 mm and a width of 45 mm to be used as a test piece, and the relative dielectric constant Dk and dielectric loss tangent Df were measured by the SPDR (Split Post Dielectric Resonator) resonator method. The measuring equipment used was a vector network analyzer E5071C manufactured by Keysight Technologies, LLC, an SPDR resonator, and a calculation program manufactured by QWED. The conditions were a frequency of 10 GHz and a measurement temperature of 25°C. The obtained relative dielectric constant Dk and dielectric loss tangent Df are shown in Table 1.

[0040] <Tensile strength and tensile modulus measurement> The test samples were molded into JIS No. 8 dumbbell pieces and used as measurement specimens. The tensile strength and tensile modulus were measured using Shimadzu Corporation's "EZ-LX" measuring device. The measurement conditions were as follows: Distance between gripping tools: 30mm Test speed: 1mm / min The obtained tensile strength and tensile modulus are shown in Table 1.

[0041] <Measurement of linear expansion coefficient> The linear expansion coefficient α1 at 30-100° C. and the linear expansion coefficient α2 at 150-250° C. of the test sample were measured by the TMA method. The linear expansion coefficient α1 and the linear expansion coefficient α2 obtained are shown in Table 1. Sample width: 3mm Distance between gripping tools: 16mm Heating rate: 10℃ / min

[0042] <Glass transition temperature measurement> A test sample was cut into a length of 40 mm and a width of 10 mm, and the glass transition temperature (Tg) was measured under the following measurement conditions using a DMA device (Hitachi High-Tech Science Corporation, DMA7100). Temperature range: 25~450℃ Heating rate: 5℃ / min Frequency: 1Hz Distortion amplitude: 10μm Minimum tension: 200mN Grip distance: 20mm In the obtained temperature profile, the temperature at which the loss modulus showed a maximum was determined as the glass transition temperature (Tg).

[0043] [Table 1]

[0044] <Solubility test> The solubility was tested by adding 0.01 g of each of the polymers in Examples 1 to 6 to 1 ml of each of the solvents shown in Table 2 and stirring at room temperature for 30 minutes. In Table 2, "A" indicates that "the polymer was dissolved" and "C" indicates that "a part or all of the polymer remained undissolved."

[0045] [Table 2]

Claims

1. Represented by the following chemical formula (1): A polymer used as an electronic material. 【Chemistry 1】 In the above formula (1), X is a divalent organic group having an aromatic ring.

2. The polymer of claim 1 having a weight average molecular weight of 1,000 to 250,000.