Transfer sheet
The transfer sheet design with a crosslinked acrylic polyol and dual crosslinking agents enhances scratch resistance and foil tearability, addressing the issues of thickness-related damage and poor cutting performance in existing protective layers.
Patent Information
- Application Number
- JP2023076981
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing protective layers in transfer sheets are either too thin for adequate scratch resistance or too thick, leading to damage during separation from the adhesive, resulting in poor foil cutting performance.
A transfer sheet design with a protective layer that includes a crosslinked product formed by crosslinking an acrylic polyol with a first crosslinking agent at 30°C to 70°C and a second crosslinking agent at 80°C to 160°C, along with an adhesion reinforcing layer, to enhance scratch resistance and foil tearability.
The solution provides a protective layer with improved scratch resistance and foil tearability, ensuring neat edges during separation without damage.
Smart Images

Figure 2024161926000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a transfer sheet for transferring and forming a protective layer on the surface of a recorded material. [Background technology]
[0002] In recent years, transfer sheets have been developed that transfer a transparent protective layer onto the surface of a recorded material to impart abrasion resistance to the recorded surface.
[0003] For example, Patent Document 1 discloses a thermal transfer sheet in which a protective layer and a surface layer are laminated on a substrate. The surface layer functions as an adhesive layer, and by adhering this to the surface of a recorded matter (also called a transferee) and peeling the protective layer and the surface layer from the substrate, a recorded matter whose surface is covered with the protective layer can be produced. The protective layer is formed of a polymer containing a polymerization component such as (meth)acrylic acid or carboxyalkyl (meth)acrylate, and by making the thickness of the protective layer 10 μm or less, the foil tearability when peeled off from the substrate is ensured. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-167567 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the protective layer in Patent Document 1 was thin and had insufficient abrasion resistance. Although the abrasion resistance can be improved by making the protective layer thicker, if the protective layer is too thick, when the recording material covered with the protective layer is separated from the bonded material between the transfer sheet and the receiving material, the protective layer cannot be neatly cut along the edge of the receiving material, and the foil cutting properties may be deteriorated. [Means for solving the problem]
[0006] In order to solve the above problems, a transfer sheet having the following structure is used.
[0007] A transfer sheet in which a protective layer and an adhesive layer are laminated on a substrate, the adhesive layer is heated in contact with a substrate to adhere to the substrate, and the substrate is then peeled off to transfer the protective layer to the substrate, and an adhesion strengthening layer is provided between the protective layer and the adhesive layer, and the protective layer contains a crosslinked product obtained by crosslinking an acrylic polyol with a first crosslinking agent that reacts with hydroxyl groups of the acrylic polyol at a temperature of 30°C or higher and 70°C or lower, and a second crosslinking agent that reacts with carboxyl groups of the acrylic polyol at a temperature of 80°C or higher and 160°C or lower. Effect of the Invention
[0008] According to the present invention, a transfer sheet having a protective layer excellent in abrasion resistance and foil tearability can be provided. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view of the transfer sheet of the present invention. [Diagram 2] FIG. 11 is a top view of a recorded matter in which tailing has occurred, as viewed from the transferred object side. [Diagram 3] FIG. 2 is an explanatory diagram for explaining the function of a second crosslinking agent. [Figure 4] FIG. 4 is a comparative diagram showing the change in the adhesion strengthening layer before and after heating. [Diagram 5] 1A to 1C are explanatory diagrams for explaining a method for producing a recorded matter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0011] [Transfer sheet] 1, the transfer sheet 10 of the present invention is formed by laminating a protective layer 40, an adhesion strengthening layer 30, and an adhesive layer 20 on a substrate 50. The transfer sheet 10 of the present invention can be adhered to a substrate 80 by heating the adhesive layer 20 in contact with the recording surface of the substrate 80, and then the substrate 50 can be peeled off to produce a recorded matter 100 in which the protective layer 40 has been transferred to the substrate 80.
[0012] [Base material] The substrate 50 used in the present invention serves to suppress curling of the transfer sheet 10 and improve transportability, and at the same time, can be peeled off after transfer.
[0013] The material constituting the substrate 50 may be appropriately selected depending on the application of the transfer sheet 10. However, since the transfer sheet 10 and the transferee 80 are heated when they are bonded (hereinafter also simply referred to as "adhesion"), it is preferable to use a resin film in consideration of heat resistance, dimensional stability, ease of processing, etc. Regarding the thickness of the substrate, it is preferable to set it to 12 μm or more and 50 μm or less, taking into consideration that a protective layer and an adhesion strengthening layer are coated and laminated, and that the substrate is heated when bonded. By setting the thickness to 12 μm or more, the effect of curling during coating can be reduced, and by setting the thickness to 50 μm or less, the thermal conductivity to the adhesive layer can be increased.
[0014] Examples of the resin film include films made of polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene terephthalate / isophthalate copolymer; polyolefin-based resins such as polyethylene, polypropylene, and polymethylpentene; polyfluoroethylene-based resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, and ethylene-tetrafluoroethylene copolymer; polyamide-based resins such as nylon 6 and nylon 6,6; vinyl polymer resins such as polyvinyl chloride, vinyl chloride / vinyl acetate copolymer, ethylene / vinyl acetate copolymer, ethylene / vinyl alcohol copolymer, polyvinyl alcohol, and vinylon; cellulose-based resins such as cellulose triacetate and cellophane; acrylic-based resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; and other synthetic resins such as polystyrene, polycarbonate, polyarylate, and polyimide. Among them, films made of crystalline resins having a melting point (Tm) of 100° C. or more, such as polyester resins, polyolefin resins, and polyamide resins, are preferable because they are relatively inexpensive and easily available, and have excellent heat resistance and dimensional stability. These may be used alone, or two or more types may be combined or laminated.
[0015] In addition, fillers such as silica, alumina, graphite, etc. may be added to the resin film in order to increase the thermal conductivity during adhesion, and an auxiliary layer for improving slipperiness may be provided on the back surface of the film (the surface on which protective layer 40 is not provided) in order to improve transportability.
[0016] [Release layer] The transfer sheet 10 of the present invention may have a release layer (not shown) between the substrate 50 and the protective layer 40 in order to improve the releasability of the substrate after transfer. The release layer is released together with the substrate when the substrate 50 is peeled off from the bonded material of the transfer sheet 10 and the transferee 80, and can be formed on the substrate using a known release agent. Examples of the release agent include silicone waxes such as silicone waxes, silicone-based release agents such as silicone resins, fluorine-based release agents such as fluorine resins, polyethylene resins, etc., and each of these may be used alone or in combination of two or more kinds. In addition, additives such as adhesion imparting agents and antistatic agents may be added to the release layer in the present invention.
[0017] [Protective layer] The transfer sheet 10 of the present invention is provided with a protective layer 40 that can protect the recorded matter 100 produced using the transfer sheet 10 of the present invention from various environmental changes, chemicals, friction, etc. In addition, since the recorded matter 100 produced using the transfer sheet 10 of the present invention is observed through the protective layer 40, the protective layer 40 is transparent, and the transparency is preferably 50% or more in total light transmittance based on JIS K7375, and more preferably 90% or more in total light transmittance based on JIS K7375.
[0018] The material for the protective layer 40 is preferably a thermoplastic acrylic resin, and examples of such materials that can be used include polymethacrylate, styrene-acrylic copolymer, polyethylene acrylic resin, acrylic ester resin, and copolymer of acrylic ester and vinyl compound. Among these, copolymers of acrylic ester and vinyl compound are preferred, and acrylic polyol having multiple hydroxyl groups in the molecule is particularly preferred because it can be crosslinked under mild conditions using the first crosslinking agent (isocyanate compound) described below.
[0019] In addition, it is preferable that the acrylic polyol having a hydroxyl group in the molecule has a carboxyl group in the molecule, which allows the crosslinked product crosslinked with the first crosslinking agent to be further crosslinked with the second crosslinking agent described below, thereby improving the scratch resistance and foil cutting properties of the protective layer at the same time.
[0020] Here, the term "foil tearability" refers to the ease with which the protective layer 40, the adhesive strengthening layer 30, and the adhesive layer 20 are peeled off along the edge of the transferee 80 in the process of separating the recorded matter 100 from the bonded matter in which the transfer sheet 10 and the transferee 80 are bonded. If the foil tearability is poor, burrs 70 and tailing 71 are generated on the cut surface from the protective layer 40 to the adhesive layer 20, as shown in FIG. 2. The tailing is a phenomenon that occurs downstream when the recorded matter 100 is separated from one end, and refers to the laminate from the protective layer 40 to the adhesive layer 20 being cut off and protruding significantly from the edge of the transferee 80.
[0021] The total amount of hydroxyl groups and carboxyl groups in the acrylic polyol used in the protective layer 40 may be 0.1 mmol or more per 1 g of the acrylic polyol. The molar ratio of the hydroxyl groups to the carboxyl groups may be selected in the range of 1:0.1 to 1:1.5, taking into consideration the solubility in the solvent and the viscosity during coating.
[0022] Furthermore, the acrylic polyol used in the protective layer 40 preferably has a ratio of weight average molecular weight (Mw) to the total content of functional groups (-OH, -COOH) (total amount of hydroxyl value (mgKOH / g) and acid value (mgKOH / g)) in the range of 1,000:1 to 2,500:1. By making the ratio of weight average molecular weight to the total amount of functional groups 1,000 or more, the distance between the crosslinks between molecules becomes appropriate, and the abrasion resistance required for the protective layer is obtained. In addition, by making the ratio of weight average molecular weight to the total amount of functional groups 2,500 or less, it is possible to prevent cracks from occurring in the protective layer when the transfer sheet 10 is wound into a roll.
[0023] The Tg (glass transition temperature) of the acrylic polyol used in the protective layer 40 is preferably 40° C. or more and 80° C. or less. If the Tg is within this range, two or more acrylic polyols having different Tgs may be used in combination. By using an acrylic polyol having a Tg of 40° C. or more, the scratch resistance is improved, and by using an acrylic polyol having a Tg of 80° C. or less, peeling of the protective layer 40 from the substrate 50 can be suppressed when the transfer sheet 10 is wound into a roll.
[0024] Nano-sized inorganic particles such as silica and alumina may be added to the protective layer 40 as long as the transparency is not impaired. This can further improve the foil-cutting properties of the protective layer 40.
[0025] The protective layer 40 is formed by mixing the above-mentioned acrylic polyol, the first and second crosslinking agents described below, and an arbitrary solvent to prepare a coating liquid, and coating the coating liquid on the substrate 50. The drying temperature during coating is preferably higher than the reaction temperature between the hydroxyl group of the acrylic polyol and the first crosslinking agent, and lower than the reaction temperature between the carboxyl group of the acrylic polyol and the second crosslinking agent, and is preferably set in the range of 40 to 70°C. This allows the protective layer 40 to be formed without reacting with the second crosslinking agent. In the present invention, in order to obtain good foil cutting properties, it is important to suppress the reaction between the carboxyl group of the acrylic polyol and the second crosslinking agent as much as possible until the transfer sheet 10 is adhered to the transferee 80.
[0026] The thickness of the protective layer 40 is not particularly limited, but is preferably 8 μm or more and 30 μm or less. By making the thickness of the protective layer 40 8 μm or more, scratch resistance can be ensured, and by making the thickness of the protective layer 40 30 μm or less, foil cutting ability can be ensured.
[0027] [First crosslinker] The protective layer 40 in the present invention contains a crosslinked product in which the main component, acrylic polyol, is crosslinked by the first crosslinking agent. This improves the scratch resistance of the protective layer 40. Although a small amount of the crosslinked product of the acrylic polyol by the first crosslinking agent may be generated when the protective layer 40 is formed on the substrate 50, most of the crosslinked product is generated by newly performing a heat treatment on the formed protective layer 40. On the other hand, since it is necessary to take care not to react with the second crosslinking agent when performing the heat treatment, it is preferable to set the temperature of the heat treatment in the range of 40°C to 70°C, which is lower than the temperature at which the carboxy group of the acrylic polyol reacts with the second crosslinking agent. In addition, the time of the heat treatment is not particularly limited, and it is sufficient to adjust it so that the acrylic polyol and the first crosslinking agent are crosslinked by 50% or more.
[0028] As the first crosslinking agent, a known isocyanate-based compound having a functional group (e.g., -NCO) that reacts with the hydroxyl group of the acrylic polyol can be used, but it is preferable to use a compound that reacts under relatively mild conditions, for example, a compound that reacts with the hydroxyl group of the acrylic polyol at 30° C. to 70° C. Furthermore, it is more preferable to use a compound that reacts with 50% or more of the hydroxyl group of the acrylic polyol when heated at 30° C. to 70° C. for 5 to 100 hours.
[0029] Isocyanate compounds include bifunctional polyisocyanates such as diisocyanates and trifunctional polyisocyanates, which will be described later. Trifunctional polyisocyanates are preferred because they can provide a high degree of crosslinking with a small amount. Trifunctional polyisocyanates include biuret and adduct polyisocyanates in which a functional group (-NCO) is bonded to the end of an alkyl chain branched into three, and isocyanurate polyisocyanates in which a functional group (-NCO) is bonded to three alkyl chains added to an isocyanurate ring. However, isocyanurate polyisocyanates are preferred because they are structurally more stable. Furthermore, aromatic TDI (toluene diisocyanate) and aliphatic HDI (hexamethylene diisocyanate) are available as isocyanurate isocyanates. HDI is more weather resistant than TDI (it is less likely to yellow due to ultraviolet rays), so it can be used preferably.
[0030] The amount of the first crosslinking agent added is preferably adjusted so that the molar ratio of the hydroxyl groups (-OH) of the acrylic polyol to the functional groups (-NCO) of the first crosslinking agent is 1:0.75 to 1:1.0. By controlling the content within this range, a protective layer 40 with excellent abrasion resistance can be formed. The content of the hydroxyl groups (-OH) of the acrylic polyol and the functional groups (-NCO) of the first crosslinking agent can be calculated by the following formula. Amount of hydroxyl groups (mmol) = amount of acrylic polyol used (g) × hydroxyl value of acrylic polyol (mgKOH / g) / formula amount of KOH (56.1g / mol) Equation 1 NCO amount (mmol) = amount of first crosslinker used (g) × NCO content (%) / formula amount of NCO (42.0 g / mol) × 1000 Equation 2
[0031] [Second crosslinker] The protective layer 40 in the present invention contains a crosslinked product of acrylic polyol crosslinked with a first crosslinking agent, and a second crosslinking agent that crosslinks unreacted acrylic polyol that has not been crosslinked with the first crosslinking agent, thereby further improving the abrasion resistance of the protective layer 40 and at the same time improving the foil cutting property.
[0032] The second crosslinking agent is a compound capable of reacting with the carboxy group of the acrylic polyol, and the temperature at which it reacts with the carboxy group is preferably higher than the temperature at which the first crosslinking agent reacts with the hydroxyl group of the acrylic polyol (30°C or higher and 70°C or lower). Specifically, it is preferable that it reacts with the carboxy group of the acrylic polyol at 80°C or higher and 160°C or lower, and more preferable that it reacts with the carboxy group of the acrylic polyol by 1.0% or more when heated at 80°C or higher and 160°C or lower for 1 minute. By adding the second crosslinking agent to the protective layer 40, the reaction between the acrylic polyol and the second crosslinking agent can be caused in the process of adhering the transfer sheet 10 and the transferee 80 (i.e., the process in which the protective layer 40 is heated to 80°C or higher). In addition, by creating a region with a high degree of crosslinking partially in the protective layer 40 (for example, the region (b) shown in FIG. 3), the abrasion resistance and foil cutting property of the protective layer 40 can be improved. Furthermore, by using as the second crosslinking agent a crosslinking agent that reacts with the carboxyl group of the acrylic polyol at 160°C or below, deformation of the transfer object 80, which has low heat resistance (for example, a PVC card), can be suppressed when the transfer sheet 10 and the transfer object 80 are adhered to each other.
[0033] Examples of compounds that react with the carboxy group of the acrylic polyol include monomers such as diamines, diols, diisocyanates, and dioxazolines, and polymers such as oxazoline group-containing polymers and polycarbodiimide resins. Among these, oxazoline group-containing polymers are preferred because they react with the carboxy group of the acrylic polyol at temperatures in the range of 80° C. to 160° C. The molecular weight is not particularly limited, but is preferably 5×10 in consideration of the foil cutting properties. 4 It is preferable to select the following:
[0034] The amount of the second crosslinking agent added is preferably adjusted so that the molar ratio of the carboxy group (-COOH) of the acrylic polyol to the functional group (oxazoline group) of the second crosslinking agent is 1:0.75 to 1:1.25. By controlling the content within this range, a protective layer 40 with excellent abrasion resistance can be formed. The content of the carboxy group of the acrylic polyol and the functional group of the second crosslinking agent can be calculated by the following formula. Amount of carboxyl group (mmol) = amount of acrylic polyol used (g) × hydroxyl value of acrylic polyol (mgKOH / g) / formula amount of KOH (56.1g / mol) Equation 3 Amount of oxazoline group (mmol) = Amount of second crosslinker used (g) × Solid content concentration (%) × Oxazoline equivalent (mmol / g) Equation 4
[0035] The reason why the abrasion resistance and foil cutting properties of the protective layer 40 can be improved simultaneously by adding the second crosslinking agent to the protective layer 40 is presumed to be as follows.
[0036] The transfer sheet 10 is adhered to the transferee 80 by overlapping the transfer sheet 10 on the transferee 80 and heating and pressing it with a heat roller 90 and a pressure roller 91, as shown in FIG. 4(b). At that time, the protective layer 40 is heated by the heat roller 90, and when the protective layer 40 reaches 80°C or higher, the crosslinked product of the acrylic polyol crosslinked with the first crosslinking agent in the protective layer or the carboxyl group of the unreacted acrylic polyol not crosslinked with the first crosslinking agent reacts with the functional group (oxazoline group) of the second crosslinking agent. In particular, the nip pressure is higher in the region (b) of FIG. 3 than in the region (a), and the amount of heat transferred to the protective layer is large, so the reaction is more likely to proceed and the degree of crosslinking is higher. It is considered that this improves the wear resistance of the protective layer 40 in the region (b).
[0037] On the other hand, in the region without the transfer object 80, such as region (a) in FIG. 3, the nip pressure is lower than in region (b), so the amount of heat transferred from the heat roller 90 to the protective layer 40 is lower. Therefore, in region (a), the reaction between the carboxyl group of the acrylic polyol and the second crosslinking agent does not proceed, and the degree of crosslinking of the acrylic polyol by the second crosslinking agent is low. In other words, region (b) and its vicinity are harder and more brittle than region (a). In addition, since the pressure applied during lamination is different between region (a) and region (b), small cracks are more likely to occur at the boundary between the two regions of the protective layer 40, and it is believed that the foil cutting property is improved by the fact that the pressure applied during lamination is different between region (a) and region (b), and that the small cracks are more likely to occur at the boundary between the two regions of the protective layer 40, and that the cuts are more likely to occur from these cracks.
[0038] [Adhesion reinforcement layer] The transfer sheet 10 of the present invention includes an adhesion strengthening layer 30 between the protective layer 40 and the adhesive layer 20 in order to improve the adhesive strength between the protective layer 40 and the adhesive layer 20. There is no limit to the thickness of the adhesion strengthening layer 30, but if it is too thin, the adhesive strength cannot be ensured, and if it is too thick, the foil cutting property becomes poor, so it is preferable to adjust the thickness within the range of 0.01 μm to 1 μm.
[0039] The material used for the adhesion strengthening layer 30 is not particularly limited, but since the adhesion strengthening layer 30 is placed on the image after transfer, it is preferable to select a material having transparency. Specific examples include vinyl compounds such as vinyl acetate, polyvinyl acetal, vinyl chloride-vinyl acetate copolymer, ethylene vinyl acetate, and vinyl chloride. Among them, vinyl chloride-vinyl acetate copolymer is preferable because it has excellent adhesive strength with the protective layer 40.
[0040] The transfer sheet 10 of the present invention can be manufactured by forming a protective layer 40 and an adhesion strengthening layer 30 in this order on a substrate 50 to manufacture a laminate, subjecting the obtained laminate to a heat treatment, and then forming an adhesive layer 20 on the adhesion strengthening layer 30 of the laminate. The heat treatment itself is carried out for the purpose of reacting the acrylic polyol in the protective layer 40 with the first crosslinking agent, and at this time, the adhesion strengthening layer 30 is heated, so that the adhesiveness between the protective layer 40 after crosslinking (i.e., the protective layer containing the crosslinked product generated by the acrylic polyol and the first crosslinking agent) and the adhesion strengthening layer 30 can be improved. The apparatus for forming the protective layer 40, the adhesion strengthening layer 30, and the adhesive layer 20 is not particularly limited, and a known coater can be used.
[0041] The detailed reason why the adhesiveness between the protective layer 40 and the adhesive strengthening layer 30 after crosslinking can be improved by heating the adhesive strengthening layer 30 is unclear. However, when the adhesive strengthening layer 30 is formed on the protective layer 40 that has been crosslinked in advance (the protective layer including the crosslinked product produced by the acrylic polyol and the first crosslinking agent), the adhesiveness between the protective layer 40 and the adhesive strengthening layer 30 is significantly reduced. In addition, when the heated vinyl-based compound is analyzed as described below, a thermally denatured substance can be confirmed, and it is presumed that the thermally denatured substance is highly likely to be involved in the adhesiveness between the protective layer 40 and the adhesive strengthening layer 30.
[0042] The fact that the adhesion strengthening layer 30 contains a thermally altered product of a vinyl-based compound can be confirmed by measuring the adhesion strengthening layer 30 before and after heating with infrared spectroscopy (IR). For example, when the vinyl chloride-vinyl acetate copolymer used in the adhesion strengthening layer 30 is heated alone, the results shown in FIG. 4 are obtained. The dotted line is the absorption curve of the adhesion strengthening layer 30 before heating, and the solid line is the absorption curve of the adhesion strengthening layer 30 after heating, with the reference being 1230 cm -1 When the peak due to the CO stretching is fitted, the waveform changes before and after heating. -1 Based on the peak at 1700 cm before heating -1 Peak (X, C=O stretching) at 1700 cm after heating -1 The relative intensity of the peak (Y) of the crosslinked product changes, and this change confirms that the heat-denatured product is contained in the adhesion-reinforcing layer 30 after heating. When a vinyl chloride-vinyl acetate copolymer is used for the adhesion-reinforcing layer 30, if the relative intensity of the peak (Y) to the peak (X) is 110% or more, the adhesive strength between the protective layer 40 containing the crosslinked product and the adhesive layer 20 becomes good, which is preferable.
[0043] In addition, infrared spectroscopy data (Figure 4) shows that the 1700 cm -1 The change in peak intensity is due to the C=O stretching vibration at 1710 cm -1 From 1700cm -1 It appears to be caused by a shift to the α-direction. In other words, the thermally denatured vinyl compound is a mutation of a part of the carbonyl group in the vinyl compound, and it is considered that the properties of the adhesive strengthening layer 30 itself change when this is generated in the adhesive strengthening layer 30, and as a result, the adhesiveness between the cross-linked protective layer 40 and the adhesive strengthening layer 30 is improved. The thermally denatured vinyl compound in the adhesive strengthening layer 30 can also be directly confirmed by cutting the cross section of the transfer sheet 10 obliquely and measuring the cut surface using a microscopic infrared spectrophotometer.
[0044] [Adhesive layer] The transfer sheet 10 of the present invention has an adhesive layer 20 on an adhesive strengthening layer 30 so as to be adhered to a transfer-receiving body 80. If the thickness of the adhesive layer 20 is too thin, the adhesiveness cannot be ensured, whereas if it is too thick, the foil cutting property is affected, so it is preferable to adjust the thickness within the range of 0.1 μm to 3 μm.
[0045] The material used for the adhesive layer 20 is not particularly limited and any known material can be used, but since the adhesive layer 20 is placed on the image after transfer, it is preferable to select a material having transparency. In addition, in order to prevent the adhesive layer 20 from sticking to the substrate 50 when the manufactured transfer sheet 10 is wound into a roll, it is preferable to use a material for the adhesive layer 20 whose Tg is equal to or higher than room temperature and equal to or lower than the thermal transfer temperature.
[0046] Specifically, the adhesives include resin adhesives such as vinyl acetate, polyol, polyvinyl acetal, vinyl chloride-vinyl acetate copolymer, ethylene vinyl acetate, vinyl chloride, acrylic, polyester, polyamide, cellulose, olefin, styrene, urea, melamine, phenol, resorcinol, epoxy, polyurethane, silicone, polyamide, polybenzimidazole, polyimide, isocyanate, chloroprene rubber, nitrile rubber, styrene butadiene rubber, polysulfide, butyl rubber, silicone rubber, acrylic rubber, modified silicone rubber, urethane rubber, and silylated urethane; inorganic adhesives such as water glass adhesives and ceramic adhesives such as sodium silicate. One or more of these adhesives can be used in combination, but it is more preferable to use the same material as the adhesive layer in consideration of the adhesiveness with the adhesive layer.
[0047] Among these, materials containing vinyl chloride-vinyl acetate copolymers are preferred because they have excellent adhesive strength with the adhesion strengthening layer 30 containing a thermally denatured substance and with the transfer-receiving body 80 described below.
[0048] [Recordings] The recorded matter 100 of the present invention is formed by laminating an adhesive layer 20, an adhesion strengthening layer 30, and a protective layer 40 in this order on the recording surface side of a transfer receiving body 80.
[0049] [Transferred object] The material of the transfer object 80 is not particularly limited, and known materials can be used. For example, there are papers made of pulp or cotton, coated papers such as coated paper and art paper, films or cards made of polyester resins such as polyvinyl chloride (PVC), polyethylene terephthalate (PET), and PET-G, polycarbonate, acrylic resins, olefin resins, acrylonitrile-butadiene-styrene copolymer resins, and polyester resins. The transfer object 80 may be a composite of these materials alone or in layers. In addition, the image formed on the recording surface of the transfer object 80 may be formed by a known printing method such as letterpress printing, offset printing, gravure printing, and screen printing, or may be formed by a known recording method such as electrophotography, inkjet, and thermal transfer.
[0050] [Manufacturing method of recorded matter] The recorded matter 100 of the present invention can be manufactured by the process shown in FIG.
[0051] Specifically, the adhesive layer 20 is brought into contact with the recording surface of the transferee 80, and the transfer sheet 10 and the transferee 80 are heated and pressed by a heat roller 90 and a pressure roller 91 in a state of being stacked together to adhere to each other (see Figs. 5(a) and (b)). After that, the substrate 50 is peeled off using a peeling roller 92 to obtain a recorded matter 100 (see Figs. 5(c) and (d)). The temperature of the heat roller 90 is preferably set in the range of 80°C to 200°C so that the second crosslinking agent can react with the carboxyl group of the acrylic polyol. This allows the degree of crosslinking in the protective layer 40 to be different between the region (a) and the region (b) shown in Fig. 3. The pressure roller 91 is preferably set to a linear pressure of 5 to 10 kgf. If the linear pressure is less than 5 kgf, the transfer sheet 10 and the transferee 80 may not adhere to each other, and if the linear pressure is more than 10 kgf, the transferee 80 may be deformed. The device for heating and pressing is not particularly limited, and a known laminator may be used. EXAMPLES
[0052] Specific examples of the present invention will be described below. However, the present invention is not limited in any way by the following examples. In the following description, "parts" and "%" are based on mass unless otherwise specified.
[0053] [Preparation of Coating Solution A for Forming Protective Layer] 30.00 parts of acrylic polyol (trade name: ACRYDIC BL-616-BA, Tg: 60°C, hydroxyl value: 18 mgKOH / g, solids concentration: 45.0%, manufactured by DIC Corporation) (hydroxyl group amount: 4.33 mmol, carboxyl group amount: 0.48 mmol), 0.787 parts of a first crosslinking agent (trade name: DURANATE TPA-100, NCO amount: 23.1%, solids concentration: 100%, manufactured by Asahi Kasei Corporation) (NCO amount: 4.33 mmol), 1.782 parts of a second crosslinking agent (trade name: EPOCROS RPS-1005, oxazoline equivalent = 0.27 mmol / g, manufactured by Nippon Shokubai Co., Ltd.) (oxazoline group amount: 0.48 mmol), and 4.153 parts of MEK were mixed in a static mixer to prepare a coating solution A for forming a protective layer. In the coating liquid, the ratio of the amount of hydroxyl groups in the acrylic polyol to the amount of isocyanate in the first crosslinking agent was 1:1, and the ratio of the amount of carboxy groups in the acrylic polyol to the amount of oxazoline groups in the second crosslinking agent was 1:1.
[0054] [Preparation of Coating Solution B for Forming Protective Layer] Except for changing the amount of the first crosslinking agent to 0.590 parts (NCO amount: 3.25 mmol), the protective layer forming coating solution B was prepared in the same manner as the protective layer forming coating solution A. The content ratio of the hydroxyl group amount of the acrylic polyol and the isocyanate group amount of the first crosslinking agent in the coating solution was 1:0.75, and the content ratio of the carboxyl group amount of the acrylic polyol and the oxazoline group amount of the second crosslinking agent was 1:1.
[0055] [Preparation of Coating Solution C for Forming Protective Layer] Except for changing the amount of the second crosslinking agent to 0.891 parts (amount of oxazoline groups: 0.24 mmol), the protective layer forming coating solution C was prepared in the same manner as the protective layer forming coating solution A. In the coating solution, the content ratio of the hydroxyl groups of the acrylic polyol to the isocyanate groups of the first crosslinking agent was 1:1, and the content ratio of the carboxyl groups of the acrylic polyol to the oxazoline groups of the second crosslinking agent was 1:0.5.
[0056] [Preparation of Coating Solution D for Forming Protective Layer] Coating solution D for forming a protective layer was prepared in the same manner as coating solution A for forming a protective layer, except that the second crosslinking agent was not used.
[0057] [Preparation of Coating Solution E for Forming Protective Layer] A protective layer-forming coating solution E was prepared in the same manner as the protective layer-forming coating solution A, except that the first crosslinking agent was not used.
[0058] [Preparation of coating solution for forming adhesion reinforcing layer] A coating liquid for forming an adhesion-reinforcing layer was prepared by adding 1 part of MEK to 1 part of vinyl chloride-vinyl acetate copolymer (product name: Solvine C, solid content: 30%, manufactured by Showa Ink Co., Ltd.).
[0059] [Preparation of coating solution for forming adhesive layer] A coating liquid for forming an adhesive layer was prepared by adding 1 part of MEK to 1 part of vinyl chloride-vinyl acetate copolymer (product name: Solvine C, solid content: 30%, manufactured by Showa Ink Co., Ltd.).
[0060] [Production of transfer sheet A] A PET film (trade name: Tetoron G2, thickness: 25 μm, manufactured by Teijin DuPont Films) was prepared as a substrate, and the protective layer forming coating liquid A was applied thereon using a gravure coater (coating speed: 5 m / min, drying temperature: 60 ° C.) so that the thickness of the protective layer after drying was 12.5 μm. Next, the adhesive layer forming coating liquid was applied on the protective layer using a gravure coater (coating speed: 5 m / min, drying temperature: 60 ° C.) so that the thickness of the layer after drying was 1 μm, and then heat treatment was performed at 60 ° C. for 5 days to crosslink the acrylic polyol in the protective layer with the first crosslinking agent. Next, the adhesive layer forming coating liquid was applied on the adhesive layer forming layer using a gravure coater (coating speed: 5 m / min, drying temperature: 60 ° C.) so that the thickness of the adhesive layer after drying was 1 μm, and a transfer sheet A was produced.
[0061] (Confirmation of thermally altered substances in the adhesive reinforcement layer) Coating solution A for forming an adhesion strengthening layer was placed in a petri dish and dried at 60 ° C. to prepare two pseudo adhesion strengthening layers with a thickness of 1 μm after drying. Then, one of them was heated at 60 ° C. for 5 days, and this and one that was not heated were measured three times each (accumulation number during measurement: 200) with an infrared spectrophotometer (product name: IR Prestige-21, manufactured by Shimadzu Corporation), and the 1710 cm -1 The peak intensity was measured. Furthermore, the relative intensity of the heated sample to that of the unheated sample was measured to confirm the presence or absence of thermally altered substances in the adhesive reinforcement layer. The relative intensity obtained was 120%.
[0062] [Manufacturing of transfer sheets B to E] Transfer sheets B to E were produced in the same manner as for transfer sheet A, except that protective layer forming coating liquid A was changed to protective layer forming coating liquids B to E.
[0063] Example 1 The adhesive layer 20 of the transfer sheet A was brought into contact with the PVC card serving as the transferee 80, and the transfer sheet A and the transferee 80 were heated and pressed with a heat roller and a pressure roller in a state where they were stacked together, and then the base material 50 was peeled off to produce the recorded matter A. The set temperature of the heat roller was 180°C, the linear pressure of the pressure roller was 8 kgf, and the conveying speed was 30 mm / s. When only the PVC card was passed under these conditions, the surface temperature of the upper surface of the card rose to 100°C.
[0064] (Rating 1: Scratch resistance of protective layer) The abrasion resistance of the protective layer of recorded matter A was evaluated using a Taber abrasion tester (product name: Rotary Ablation Tester TS-2, manufactured by Toyo Seiki Seisakusho) under test conditions of a rotation speed of 60 rpm, a load of 500 g, and an abrasion wheel: CS-10F. The results are shown in Table 1. In the "Abrasion Resistance" column in the table, "◯" indicates that the printed surface was not abraded even when the abrasion wheel was rotated more than 2,000 times, "△" indicates that the printed surface was abraded when the abrasion wheel was rotated 1,000 to less than 2,000 times, and "×" indicates that the printed surface was abraded when the abrasion wheel was rotated less than 1,000 times.
[0065] (Evaluation 2: Foil cutting ability) After the transfer sheet was heated and pressed onto the recipient, the non-adhesive portion was pulled at a 90° angle when peeling off the base material, and the length of the protective layer that protruded from the edge of the card remaining on the recipient side was evaluated. The results are shown in Table 1. In the "Foil tearability" column in the table, "◯" indicates that the length of the protective layer protruding from the edge of the card was less than 0.1 mm, "△" indicates that the length of the protective layer protruding from the edge of the card was 0.1 mm or more but less than 0.2 mm, and "×" indicates that the length of the protective layer protruding from the edge of the card was 0.2 mm or more.
[0066] (Examples 2 and 3) Recorded materials B and C were produced in the same manner as in Example 1, except that transfer sheet A was changed to transfer sheets B and C, and the abrasion resistance and foil cutting properties were evaluated. The obtained results are shown in Table 1.
[0067] (Comparative Examples 1 and 2) Recorded matter D and E were produced in the same manner as in Example 1, except that transfer sheet A was changed to transfer sheets D and E, and the abrasion resistance and foil cutting properties were evaluated. The obtained results are shown in Table 1.
[0068] [Table 1]
[0069] As is clear from Table 1, the transfer sheets (Examples 1 to 3) having a protective layer containing a crosslinked product of acrylic polyol and the first crosslinking agent (produced by heat treatment after forming the adhesion-reinforcing layer) and a second crosslinking agent had better foil cutting properties than the transfer sheet (Comparative Example 1) that did not contain the second crosslinking agent. In addition, the transfer sheets (Examples 1 to 3) having a protective layer containing a crosslinked product of acrylic polyol and the first crosslinking agent and a second crosslinking agent had better abrasion resistance than the transfer sheet (Comparative Example 2) that did not contain the first crosslinking agent.
[0070] The disclosure of this embodiment includes the following configurations and methods. (Configuration 1) A protective layer and an adhesive layer are laminated on the substrate, A transfer sheet capable of adhering the adhesive layer to a transferee by heating the adhesive layer in contact with the transferee, and then transferring the protective layer to the transferee by peeling off the base material, An adhesion-enhancing layer is provided between the protective layer and the adhesive layer, The protective layer is a crosslinked product obtained by crosslinking an acrylic polyol with a first crosslinking agent that reacts with a hydroxyl group of the acrylic polyol at a temperature of 30° C. or more and 70° C. or less; A second crosslinking agent that reacts with the carboxy group of the acrylic polyol at 80° C. or higher and 160° C. or lower. A transfer sheet characterized by: (Configuration 2) The transfer sheet according to configuration 1, wherein the first crosslinking agent is an isocyanate compound, and the second crosslinking agent is an oxazoline group-containing polymer. (Configuration 3) The transfer sheet according to the first or second aspect, wherein the adhesion-reinforcing layer contains a thermally denatured product of a vinyl compound. (Configuration 4) 4. The transfer sheet according to any one of configurations 1 to 3, wherein the adhesive layer is made of a material containing a vinyl compound. (Configuration 5) 5. The transfer sheet according to claim 3 or 4, wherein the vinyl compound contains a carbonyl group. (Configuration 6) 6. The transfer sheet according to any one of configurations 3 to 5, wherein the vinyl compound is a vinyl chloride-vinyl acetate copolymer. [Explanation of symbols]
[0071] 10: Transfer sheet 20: Adhesive layer 30: Adhesion reinforcement layer 40:Protective layer 50: Base material 70: Bali 71: Tail pulling 72: Direction for separating the recording material from the adhesive material between the transfer sheet and the receiving material 80: Transferee 90: Heat roller 91: Pressure roller 92: Peeling roller 100: Recordings
Claims
1. A protective layer and an adhesive layer are laminated on the substrate, A transfer sheet capable of adhering the adhesive layer to a transferee by heating the adhesive layer in contact with the transferee, and then transferring the protective layer to the transferee by peeling off the base material, An adhesion-enhancing layer is provided between the protective layer and the adhesive layer, The protective layer is a crosslinked product obtained by crosslinking an acrylic polyol with a first crosslinking agent that reacts with a hydroxyl group of the acrylic polyol at 30° C. or more and 70° C. or less; A second crosslinking agent that reacts with a carboxy group of the acrylic polyol at 80° C. or more and 160° C. or less. A transfer sheet characterized by:
2. 2. The transfer sheet according to claim 1, wherein the first crosslinking agent is an isocyanate compound, and the second crosslinking agent is an oxazoline group-containing polymer.
3. 2. The transfer sheet according to claim 1, wherein the adhesion-reinforcing layer contains a thermally modified vinyl compound.
4. 2. The transfer sheet according to claim 1, wherein the adhesive layer is made of a material containing a vinyl compound.
5. 5. The transfer sheet according to claim 3, wherein the vinyl compound contains a carbonyl group.
6. 5. The transfer sheet according to claim 3, wherein the vinyl compound is a vinyl chloride-vinyl acetate copolymer.
Citation Information
Patent Citations
Thermal transfer sheet
JP2018167567A