Latent heat storage particles and method for producing the same
The polyurethane polyurea resin-coated latent heat storage particles with a stable core-shell structure address leakage issues and high-temperature material integration, offering durable and efficiently producible heat storage solutions.
Patent Information
- Application Number
- JP2023077015
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-09
AI Technical Summary
Existing latent heat storage particles face issues such as material leakage due to expansion and contraction during phase transitions, especially with high-temperature materials, and they are difficult to manufacture in a simple and effective process.
The development of latent heat storage particles with a polyurethane polyurea resin shell and a core containing a latent heat storage material, ensuring a heating loss of 2% by weight or less, and using a manufacturing process involving the dispersion of a polyisocyanate, polyol, and polyamine to form a stable core-shell structure.
The solution provides stable latent heat storage particles that prevent material leakage during long-term use and can incorporate high-temperature materials, while being manufacturable in a relatively simple process.
Smart Images

Figure 2024161940000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to latent heat storage particles and a method for producing the same, and to a material containing the latent heat storage particles. [Background technology]
[0002] Core-shell type latent heat storage particles, which contain latent heat storage materials in resin capsules that utilize the latent heat (heat of transition) associated with changes in the physical state of a substance (phase transition; solidification and melting), are known. These particles are used for temperature control, such as in structural materials for buildings and structures, and for air conditioning in buildings, houses, and underground shopping malls.
[0003] For example, Patent Documents 1 and 2 disclose latent heat storage particles having a shell portion made of any one of polyurethane polyurea, polyurethane, and polyurea. Moreover, Patent Document 3 discloses heat storage particles that use a vinyl monomer for the shell portion and n-paraffin for the core portion.
[0004] Furthermore, Patent Document 4 discloses heat storage particles using melamine resin for the shell and n-paraffin for the core. However, when melamine resin is used for the shell, there is a problem that aldehyde, which is a causative substance of sick house syndrome, is generated.
[0005] In the core-shell type latent heat storage particles in which the latent heat storage material is sealed in a resin capsule, heat is transferred in and out as the latent heat storage material contained in the core part solidifies / melts, but the solidification / melting is accompanied by contraction / expansion of the core part, which leads to the shell part being loaded. Therefore, if the core part contracts / expands for a long period of time, the shell part cannot withstand the load and is destroyed, resulting in leakage of the latent heat storage material. In particular, latent heat storage materials with high phase transition (solidification / melting) temperatures generally have a large volume change due to contraction / expansion associated with solidification / melting, so the shell part tends to be destroyed more, and the problem of leakage of the latent heat storage material becomes more pronounced.
[0006] On the other hand, with the recent increase in CPU performance, there is an increasing need to prevent overheating in electronic devices and to prevent low-temperature burns in devices that come into contact with the human body, and there are hopes for the commercialization of latent heat storage particles with a melting point of 30°C or higher, as measured by JIS-K7121, that can be embedded in devices.
[0007] For example, Patent Document 5 discloses latent heat storage particles that do not generate aldehyde, improve the problem of leakage of the latent heat storage material, and have excellent durability. However, when a latent heat storage material with a phase transition temperature exceeding 30° C. is used, there is a problem that it cannot be granulated into latent heat storage particles. For example, Patent Document 6 discloses a heat storage microcapsule made of a polyurethane or polyurea film and a specific fatty acid ester. However, when the microcapsule is repeatedly expanded and contracted by melting and solidifying during long-term use, the fatty acid ester leaks due to deterioration of the film material.
[0008] Furthermore, for example, Patent Document 7 discloses a method for producing latent heat storage particles by producing porous hollow particles, impregnating the particles with a latent heat storage material through the pores, and then coating the particles with polyamide to close the pores, and the latent heat storage particles thus obtained. However, this production method requires multiple steps and complicated production processes, and is therefore not suitable for practical use. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2009-91473 A. [Patent Document 2] JP 2009-148676 A. [Patent Document 3] Patent No. 5651272. [Patent Document 4] Patent No. 4808476. [Patent Document 5] JP 2017-137437 A. [Patent Document 6] Patent No. 6899307. [Patent Document 7] JP 2016-34622 A. Summary of the Invention [Problem to be solved by the invention]
[0010] However, latent heat storage particles that solve the above problems have not yet been developed and commercialized. Therefore, an object of the present invention is to solve the above problems. That is, an object of the present invention is to provide latent heat storage particles from which the latent heat storage material does not leak even after long-term storage and / or long-term use. Furthermore, in addition to or in addition to the above-mentioned object, the present invention has an object to provide latent heat storage particles that can be granulated even when using a latent heat storage material having a melting point of 30°C or higher as measured according to JIS-K7121.
[0011] Furthermore, in addition to or in addition to the above object, an object of the present invention is to provide latent heat storage particles that can be produced in a relatively simple process, and a method for producing the same. Furthermore, in addition to or in addition to the above object, an object of the present invention is to provide a material having the above latent heat storage particles.
[0012] In order to solve the above problems, the present inventors have discovered the following invention. <1> A latent heat storage particle having a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material, the heat loss being 2% by weight or less after heating at 110°C for 6 hours.
[0013] <2> the above <1> In the above, the latent heat storage particles have a melting point of 30°C or more and 60°C or less, preferably 35 to 55°C, and more preferably 35 to 50°C, as measured according to JIS-K7121. <3> the above <1> or <2> In the above, the latent heat storage material has a water / octanol partition coefficient LogP of 8 or more and 10 or less, and is preferably at least one selected from fatty acid esters (A) having a water / octanol partition coefficient LogP of 8.0 or more and 10.0 or less, and n-paraffins (B) having a water / octanol partition coefficient LogP of 9.2 or more and 10.0 or less.
[0014] <4> the above <1> ~ <3> In any one of the above, the polyurethane polyurea resin preferably has a structure derived from an alicyclic diisocyanate. <5> the above <1> ~ <4> In any of the above, the latent heat storage particles have a volume average particle size of 1 to 500 μm, preferably 5 to 300 μm, more preferably 10 to 250 μm, and most preferably 20 to 200 μm.
[0015] <6> the above <1> ~ <5> In any of the above, the shell part may essentially consist of a polyurethane polyurea resin. In this specification, "essentially consist of a polyurethane polyurea resin" means that, out of 100 parts by weight of the material constituting the shell part, the "polyurethane polyurea resin" is 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight. <7> the above <1> ~ <6> In any one of the above, the shell portion is preferably made of polyurethane polyurea resin alone.
[0016] <8> the above <1> ~ <7> In any of the above, the core part is preferably essentially made of a latent heat storage material. Here, in the present specification, "essentially made of a latent heat storage material" means that the amount and type of the latent heat storage material and the amount and type of materials other than the latent heat storage material are not limited as long as the melting point of the latent heat storage particles measured by JIS-K7121 is 30°C or more and 60°C or less. Note that "essentially made of a latent heat storage material" means that out of 100 parts by weight of the material constituting the core part, the "latent heat storage material" is 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight. <9> the above <1> ~ <8> In any one of the above, the core portion is preferably made of only the latent heat storage material.
[0017] <10> the above <1> ~ <9> In any of the above, the latent heat storage particles preferably consist essentially of a shell part and a core part. In this specification, "consist essentially of a shell part and a core part" means that, although the particles may have parts other than the "shell part" and the "core part", the parts other than the "shell part" and the "core part" are 5 parts by weight or less, preferably 3 parts by weight or less, more preferably 1 part by weight or less, and most preferably 0 part by weight, per 100 parts by weight of the latent heat storage particles. <11> the above <1> ~ <10> In any one of the above, the latent heat storage particles preferably consist of only the shell portion and the core portion.
[0018] <12> the above <1> ~ <11> A material having latent heat storage particles according to any one of claims 1 to 5. Examples of the material include, but are not limited to, a resin sheet, a rubber sheet, synthetic paper, a medium (water, a heat medium), a thermoplastic resin, a thermosetting resin, and rubber. <13> the above <1> ~ <12> 2. A method for producing the latent heat storage particles according to any one of the preceding claims.
[0019] <14> A step of dispersing a raw material composition having a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine and the polyol; By having A method for producing latent heat storage particles, which has a shell portion having a polyurethane polyurea resin and a core portion having the latent heat storage material, and which produces latent heat storage particles having a heat loss of 2% by weight or less after heating at 110°C for 6 hours. Effect of the Invention
[0020] The present invention makes it possible to solve the above problems. According to the present invention, it is possible to provide latent heat storage particles from which the latent heat storage material does not leak even after long-term storage and / or long-term use. Furthermore, in addition to or in addition to the above effects, the present invention can provide latent heat storage particles that can be granulated even when using a latent heat storage material having a melting point of 30°C or higher as measured according to JIS-K7121.
[0021] Furthermore, in addition to or in addition to the above-mentioned effects, the present invention can provide latent heat storage particles that can be produced in a relatively simple process, and a method for producing the same. Furthermore, according to the present invention, in addition to or in addition to the above-mentioned effects, a material having the above-mentioned latent heat storage particles can be provided. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a latent heat storage particle of the present invention. [Diagram 2] 1 shows a cross-sectional view of an example of a material having latent heat storage particles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The invention described in this application (hereinafter sometimes abbreviated as "the present invention") will be described below. The present application provides a latent heat storage particle having a shell portion having a polyurethane polyurea resin and a core portion having a latent heat storage material, the latent heat storage particle having a heat loss of 2% by weight or less, preferably 1.5% by weight or less, more preferably 1.0% by weight or less, and most preferably 0.5% by weight or less. The present application also provides a method for producing the latent heat storage particles. Furthermore, the present application provides a material having the above-mentioned latent heat storage particles.
[0024] <Latent heat storage particles> The latent heat storage particles of the present invention have a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material. 1 shows a cross-sectional view of an example of a latent heat storage particle of the present invention. The latent heat storage particle 10 has a core portion 12 having a latent heat storage material and a shell portion 14 having a polyurethane polyurea resin that covers the core portion 12.
[0025] The latent heat storage particles of the present invention have a heat loss of 2% or less by weight, preferably 1.5% or less by weight, more preferably 1.0% or less by weight, and most preferably 0.5% or less by weight. The heat loss can be determined by measuring the weight of the latent heat storage particles before heating, heating the latent heat storage particles at 110°C for 6 hours, and then measuring the weight of the latent heat storage particles again, and calculating the weight loss, which is the difference between the two. When the heat loss is within the above range, it is possible to provide latent heat storage particles having desired properties, for example latent heat storage particles that do not leak the latent heat storage material even after long-term storage and / or long-term use. Furthermore, by having the loss on heating be within the above range, it is possible to provide latent heat storage particles having the desired characteristics, for example latent heat storage particles that can be granulated even when a latent heat storage material having a phase transition temperature exceeding 30°C is used.
[0026] The latent heat storage particles of the present invention have a melting point of 30°C or more and 60°C or less, preferably 35 to 55°C, and more preferably 35 to 50°C, as measured according to JIS-K7121.
[0027] The latent heat storage particles of the present invention may have an outermost layer outside the shell portion in addition to the shell portion and the core portion. The outermost layer is preferably a layer that imparts functions such as heat resistance, solvent resistance, and water resistance to the latent heat storage particles, and examples of materials for the layer include, but are not limited to, thermoplastic resins, cured products of curable resins, and inorganic compounds.
[0028] The latent heat storage particles of the present invention are preferably essentially composed of a shell part and a core part, and preferably the latent heat storage particles of the present invention are composed only of a shell part and a core part. Note that "essentially composed of a shell part and a core part" means that the particles may have parts other than the "shell part" and the "core part", but that the parts other than the "shell part" and the "core part" are 5 parts by weight or less, preferably 3 parts by weight or less, more preferably 1 part by weight or less, and most preferably 0 part by weight, per 100 parts by weight of the latent heat storage particles.
[0029] The latent heat storage particles of the present invention have a volume average particle size of 1 to 500 μm, preferably 5 to 300 μm, more preferably 10 to 250 μm, and most preferably 20 to 200 μm. The term "volume average particle size" refers to the volume-based median size measured using a laser diffraction particle size distribution measuring device. If the volume average particle diameter of the latent heat storage particles is equal to or greater than the lower limit of the above range, the amount of latent heat storage of the latent heat storage particles is sufficiently large. In addition, even if heating and cooling are repeated, the latent heat storage material in the core portion is unlikely to seep out. In addition, the mechanical strength of the shell portion is increased, and the shell portion is unlikely to be damaged by compression or the like. If the volume average particle diameter of the latent heat storage particles is equal to or less than the upper limit of the above range, when the latent heat storage particles and other materials (building materials, media, etc.) are used as a material, such as a heat storage material, the latent heat storage particles become inconspicuous, and the appearance of the material, such as the heat storage material, becomes good. The volume average particle size of the latent heat storage particles can be made smaller by increasing the content of the dispersant in the dispersion medium in the method for producing latent heat storage particles described below, and can be made larger by decreasing the content of the dispersant.
[0030] Examples of the shape of the latent heat storage particles include a perfect sphere, a partially distorted sphere, a potbelly shape, a cylinder, a cone shape, a rectangular parallelepiped shape, and the like, but are not limited to these. The amount of the latent heat storage material in the latent heat storage particles is, in terms of the mechanical strength of the shell portion and the latent heat storage amount of the core portion, 30 to 99.9 parts by weight, preferably 50 to 99 parts by weight, more preferably 60 to 99 parts by weight, and most preferably 70 to 90 parts by weight, out of 100 parts by weight of the latent heat storage particles.
[0031] <Shell part> The shell of the latent heat storage particles of the present invention comprises a polyurethane polyurea resin. Here, "polyurethane polyurea" refers to a polymer compound having a urethane bond (-NHC(O)O-) and a urea bond (-NHC(O)NH-). It is preferable that there are a plurality of urethane bonds and a plurality of urea bonds. The shell portion of the latent heat storage particle of the present invention may contain a material other than the polyurethane polyurea resin, so long as the above-mentioned problems such as leakage of the latent heat storage material do not occur. Examples of materials other than the polyurethane polyurea resin include, but are not limited to, resins other than polyurethane polyurea, rubber, fillers, function-imparting agents, and inevitable impurities. The polyurethane polyurea resin should be at least 50 parts by weight, preferably at least 70 parts by weight, more preferably at least 90 parts by weight, and most preferably 100 parts by weight, out of 100 parts by weight of the material constituting the shell portion. The content of other components is 50 parts by weight or less, preferably 30 parts by weight or less, more preferably 10 parts by weight or less, and most preferably 0 part by weight, per 100 parts by weight of the polyurethane polyurea.
[0032] The shell of the latent heat storage particles of the present invention should essentially consist of a polyurethane polyurea resin, and preferably consist only of a polyurethane polyurea resin. Here, "consisting essentially of a polyurethane polyurea resin" means that out of 100 parts by weight of the material constituting the shell portion, the "polyurethane polyurea resin" is 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight.
[0033] The thickness of the shell of the latent heat storage particles of the present invention depends on the particle size of the resulting latent heat storage particles, the material of the shell used, particularly the polyurethane polyurea resin used, etc., but from the standpoint of mechanical strength and / or prevention of volatilization of the latent heat storage material, it is preferably 0.03 to 40 μm, preferably 0.1 to 25 μm, more preferably 0.2 to 20 μm, and most preferably 0.5 to 15 μm.
[0034] It is preferable that the polyurethane polyurea resin has both a urethane bond derived from the reaction of a polyisocyanate with a polyol and a urea bond derived from the reaction of a polyisocyanate with a polyamine, since this further increases the mechanical strength of the shell portion. That is, the polyurethane polyurea resin is derived from polyisocyanate, polyol, and polyamine, and it is preferable to use them in the method for producing latent heat storage particles of the present invention described later. Note that the origin of these materials is not limited, and they may be derived from, for example, fossil fuels or biomass.
[0035] <<Polyisocyanate>> Examples of polyisocyanates include bifunctional isocyanates having two isocyanate groups, and polyfunctional isocyanates having three or more isocyanate groups.
[0036] Bifunctional isocyanates include tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, lysine diisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), methylcyclohexane-2,4 (or 2,6)-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane (hydrogenated XDI), isophorone diisocyanate, trimethylhexamethylene diisocyanate, dimer acid diisocyanate, dianisidine diisocyanate, Phenyl diisocyanate, halogenated phenyl diisocyanate, methylene diisocyanate, ethylene diisocyanate, butylene diisocyanate, propylene diisocyanate, octadecylene diisocyanate, 1,5-naphthalene diisocyanate, polymethylene polyphenylene diisocyanate, naphthalene diisocyanate, tolylene diisocyanate polymer, diphenylmethane diisocyanate polymer, hexamethylene diisocyanate polymer, 3-phenyl-2-ethylene diisocyanate , cumene-2,4-diisocyanate, 4-methoxy-1,3-phenylene diisocyanate, 4-ethoxy-1,3-phenylene diisocyanate, 2,4'-diisocyanate diphenyl ether, 5,6-dimethyl-1,3-phenylene diisocyanate, 4,4'-diisocyanate diphenyl ether, benzidine diisocyanate, 9,10-anthracene diisocyanate, 4,4'-diisocyanate benzyl, 3,3'-dimethyl-4,4'-diisocyanate diphenyl methane, 2,6-dimethyl Examples of the isocyanate include, but are not limited to, 4,4'-diisocyanate diphenyl ethyl, 3,3'-dimethoxy-4,4'-diisocyanate diphenyl, 1,4-anthracene diisocyanate, phenylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,10-decamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 4,4'-methylene-bis(cyclohexyl isocyanate), and norbornane diisocyanate.
[0037] Examples of polyfunctional isocyanates include triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, 2,4,4'-triisocyanate diphenyl ether, 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, and trimers of bifunctional isocyanates (biuret, isocyanurate, adduct).
[0038] In the present invention, the polyisocyanate is preferably an alicyclic diisocyanate. If the polyisocyanate is an alicyclic diisocyanate, the formation of the shell and core during polymerization proceeds uniformly due to compatibility with the latent heat storage material, and latent heat storage particles that are dense and have sufficient strength and excellent durability can be obtained. Examples of alicyclic diisocyanates include, but are not limited to, 1,3-bis(isocyanatomethyl)cyclohexane (hydrogenated XDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), isophorone diisocyanate, and norbornane diisocyanate. The polyisocyanate may be used alone or in combination of two or more kinds.
[0039] <<Polyol>> A polyol is a compound that contains two or more hydroxyl groups (OH groups). Examples of polyols include polyester polyols, polyether polyols, polycarbonate polyols, polybutadiene polyols, hydrogenated polybutadiene polyols, acrylic polyols, polycaprolactone polyols, and aliphatic polyhydric alcohols having 1 to 20 carbon atoms, but are not limited to these.
[0040] Moreover, as the polyol, an aliphatic polyhydric alcohol having 1 to 20 carbon atoms is preferable, since the latent heat storage material is less likely to exude and latent heat storage particles having high mechanical strength are easily obtained. Examples of the aliphatic polyhydric alcohol having 1 to 20 carbon atoms include, but are not limited to, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,3-propanediol, trimethylolpropane, trimethylolethane, glycerin, pentaerythritol, and sorbitol. The polyols may be used alone or in combination of two or more kinds.
[0041] <<Polyamine>> A polyamine is a compound that contains two or more amino groups (NH2 groups). Examples of polyamines include aliphatic polyamines such as ethylenediamine, tetramethylenediamine, octamethylenediamine, decamethylenediamine, piperazine, diethylenetriamine, triethylenetetraamine, dihexamethylenetriamine, and 1,4-diaminocyclohexane; and aromatic polyamines such as paraphenylenediamine, metaphenylenediamine, paraxylylenediamine, metaxylylenediamine, 4,4'-diaminobiphenyl, and 4,4'-diaminodiphenylmethane, but are not limited to these.
[0042] The preferred proportions of the polyisocyanate-derived structural units, polyol-derived structural units, and polyamine-derived structural units in the polyurethane polyurea are the same as the preferred charging proportions of the polyisocyanate, polyol, and polyamine in the method for producing latent heat storage particles described below.
[0043] <Core> The core portion contains a latent heat storage material. The core portion may contain other components as necessary within the range not impairing the effects of the present invention. Examples of other components include, but are not limited to, resins, rubbers, fillers, functional agents, and inevitable impurities. Fillers can include, but are not limited to, metals, metal compounds, carbon materials (carbon black, carbon nanotubes, expanded graphite, carbon fibers), glass, minerals, and the like.
[0044] Examples of the function-imparting agent include, but are not limited to, antioxidants, antistatic agents, weather resistance agents, ultraviolet absorbers, antiblocking agents, crystal nucleating agents, flame retardants, vulcanizing agents, vulcanization assistants, antibacterial and antifungal agents, dispersants, coloration inhibitors, foaming agents, rust inhibitors, heavy metal deactivators, melting point adjusters (freezing point depressants), and hydrolysis inhibitors. The amount of other components is preferably 3 parts by weight or less, more preferably 2 parts by weight or less, more preferably 1 part by weight or less, and most preferably 0 part by weight, based on 100 parts by weight of the latent heat storage material.
[0045] The core may consist essentially of latent heat storage material, preferably consisting solely of latent heat storage material. In this specification, "consisting essentially of a latent heat storage material" means that the melting point of the latent heat storage particles measured according to JIS-K7121 is 30°C or more and 60°C or less, and the amount and type of the latent heat storage material and the amount and type of materials other than the latent heat storage material are not limited. "Consisting essentially of a latent heat storage material" means that out of 100 parts by weight of the material constituting the core, the "latent heat storage material" is 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight.
[0046] The latent heat storage material preferably has a water / octanol partition coefficient LogP of 8 or more and 10 or less, and is preferably at least one selected from fatty acid ester (A) having a water / octanol partition coefficient LogP of 8.0 or more and 10.0 or less, and / or n-paraffin (B) having a water / octanol partition coefficient LogP of 9.2 or more and 10.0 or less. When the LogP of fatty acid ester (A) and n-paraffin (B) is within the specified value range, the following three advantages are obtained. (1) Due to the compatibility, the formation of the shell and core portions during polymerization proceeds uniformly, resulting in latent heat storage particles that are dense, have sufficient strength, and are highly durable. (2) Since the melting point of the latent heat storage material as measured by JIS-K7121 is higher than 30°C, it is in a solid state at room temperature. Even after becoming latent heat storage particles, it is not easily volatilized and has excellent long-term storage properties. (3) Since the melting point of the latent heat storage material measured by JIS-K7121 is lower than 60°C, it is in a liquid state at the polymerization temperature of 65°C, making it possible to polymerize latent heat storage particles with a good core-shell structure.
[0047] The water / octanol partition coefficient (LogP value) can be measured by the flask shaking method described in JIS Z-7260-107 (2000). The water / octanol partition coefficient (LogP value) can also be estimated by computational chemistry methods or empirical methods instead of actual measurements.
[0048] As a method for calculating LogP, Crippen's fragmentation method (J. Chem. Inf. Comput. Sci., 27, p. 21 (1987)), Viswanadhan's fragmentation method (J. Chem. Inf. Comput. Sci., 29, p. 163 (1989)), Broto's fragmentation method (Eur. J. Med. Chem. Chim. Theor., 19, p.71 (1984)), CLogP method (references Leo, A., Jow, PYC, Silipo, C., Hansch, C., J. Med. Chem., 18, 865 (1975)), etc. are preferably used, but Crippen's fragmentation method and CLogP method are more preferable. When using the CLogP method, calculations can be performed using free software available on the Molinspiration Cheminformatics website.
[0049] As described above, the core of the latent heat storage particle of the present invention uses a latent heat storage material from the viewpoints of a large heat storage amount, precise temperature control, ease of particle production, etc. The latent heat storage material is preferably selected depending on the application of the latent heat storage particle. The latent heat storage material is a fatty acid ester (A) having a water / octanol partition coefficient LogP of 8.0 or more and 10.0 or less, and an n-paraffin (B) having a water / octanol partition coefficient LogP of 9.2 or more and 10.0 or less. The fatty acid ester (A) and the n-paraffin (B) may be used alone or in combination.
[0050] Examples of fatty acid ester (A) having a water / octanol partition coefficient LogP of 8.0 or more and 10.0 or less (melting point measured by JIS-K7121 of 30° C. or more and 60° C. or less) include methyl stearate, methyl arachidate, methyl behenate, methyl lignocerate, myristyl myristate, cetyl myristate, cetyl palmitate, etc. As fatty acid ester (A), methyl stearate, myristyl myristate, cetyl myristate, and cetyl palmitate are preferred, and methyl stearate, myristyl myristate, and cetyl myristate are more preferred. In particular, methyl stearate, myristyl myristate, and cetyl myristate are preferred because they are available as inexpensive, high-purity industrial products, are compatible with alicyclic isocyanates, and the formation of the shell portion (wall film) of the core-shell structure proceeds uniformly during polymerization, resulting in latent heat storage particles with sufficient strength. The fatty acid ester (A) may be used alone or in combination of two or more kinds.
[0051] Examples of n-paraffins (B) having a water / octanol partition coefficient LogP of 9.2 or more and 10.0 or less (melting points measured according to JIS-K7121 of 30° C. or more and 60° C. or less) include eicosane, docosane, tetracosane, hexacosane, etc. As n-paraffins (B), eicosane and docosane are preferred. In particular, eicosane and docosane are preferred because they are available as inexpensive, high-purity industrial products. The n-paraffin (B) may be used alone or in combination of two or more kinds.
[0052] In the present invention, the entire amount of the core is preferably the fatty acid ester (A) and / or the n-paraffin (B), but latent heat storage materials other than these may be used in combination. When a latent heat storage material other than the fatty acid ester (A) and n-paraffin (B) is used in combination, the total weight proportion of the fatty acid ester (A) and / or n-paraffin (B) is preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight.
[0053] Examples of latent heat storage materials other than fatty acid esters (A) and n-paraffins (B) include "fatty acid esters other than fatty acid esters (A)", "n-paraffins other than n-paraffins (B)", "petroleum waxes (paraffin wax, microcrystalline wax)", "fatty acids", "fatty ethers", "fatty ketones", and "fatty alcohols".
[0054] As fatty acid esters other than the fatty acid ester (A), the following can be used. For example, fatty acid esters having a water / octanol partition coefficient LogP of less than 8.0 (melting point measured by JIS-K7121 of less than 30°C) include, but are not limited to, methyl palmitate, methyl myristate, methyl laurate, and lauryl laurate. Furthermore, for example, fatty acid esters having a water / octanol partition coefficient LogP of more than 10.0 (melting point measured according to JIS-K7121 of more than 30° C.) include, but are not limited to, stearyl stearate.
[0055] As n-paraffins other than the n-paraffin (B), the following can be used. For example, n-paraffins having a water / octanol partition coefficient LogP of less than 9.2 (melting point measured by JIS-K7121 of less than 30° C.) include, but are not limited to, nonadecane, octadecane, heptadecane, hexadecane, pentadecane, and tetradecane. Furthermore, for example, n-paraffins having a water / octanol partition coefficient LogP of more than 10.0 (melting point measured by JIS-K7121 of more than 60° C.) include, but are not limited to, octacosane, nonacosane, and triacontane.
[0056] The petroleum wax is preferably one having 20 or more carbon atoms. Petroleum waxes can include, but are not limited to, paraffin wax, microcrystalline wax, and the like. Paraffin wax is a saturated hydrocarbon that is solid at room temperature and is produced by separating and refining the distillate from vacuum distillation using petroleum or natural gas as a raw material.
[0057] Paraffin wax having 20 to 40 carbon atoms is preferred. Commercially available paraffin wax products include HNP-9, HNP-51, FNP-0090, and FT115 manufactured by Nippon Seiro Co., Ltd., but are not limited to these. Microcrystalline wax is a saturated hydrocarbon that is solid at room temperature and is produced by separating and refining vacuum distillation residue oil or heavy distillate oil using petroleum as a raw material. As the microcrystalline wax, those having 30 to 60 carbon atoms are preferred.
[0058] The fatty acid is preferably a fatty acid having 8 to 30 carbon atoms. The fatty acid may be any of linear saturated fatty acid, linear unsaturated fatty acid, branched saturated fatty acid and branched unsaturated fatty acid, with linear saturated fatty acid being preferred because of its large latent heat. Examples of straight-chain saturated fatty acids include, but are not limited to, octanoic acid, nonanoic acid, decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), eicosanoic acid, docosanoic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, and triacontanoic acid. Examples of fatty acid metal salts include, but are not limited to, lithium 12-hydroxystearate, aluminum 2-ethylhexanoate, and the like.
[0059] As the aliphatic ether, a fatty acid ether having 14 to 60 carbon atoms is preferred. Examples of the aliphatic ether include heptyl ether, octyl ether, tetradecyl ether, and hexadecyl ether, and the ether having one oxygen atom and a symmetrical structure is preferred. Aliphatic ketones can include, but are not limited to, 2-octanone, 3-octanone, 2-nonanone, 3-nonanone, cycloheptanone, and the like. The aliphatic alcohol is preferably an aliphatic alcohol having 8 to 60 carbon atoms. As the aliphatic alcohol, a primary alcohol is preferred. Aliphatic alcohols can include, but are not limited to, 2-dodecanol, 1-tetradecanol, 7-tetradecanol, 1-octadecanol, 1-eicosanol, 1,10-decanediol, and the like. The origin of the latent heat storage material is not limited, and any of those derived from fossil fuels and biomass, including fatty acid esters (A) and n-paraffins (B), may be used.
[0060] <Method of manufacturing latent heat storage particles> The present application also provides a method for producing the above-mentioned latent heat storage particles. The production method is, for example, A step of dispersing a raw material composition having a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine and the polyol; has.
[0061] As a result, as described above, latent heat storage particles can be obtained which have a shell portion having a polyurethane polyurea resin and a core portion having the latent heat storage material, and which have a heat loss, which is the weight loss after heating at 110°C for 6 hours, of 2% by weight or less. The terms "polyisocyanate," "polyol," "latent heat storage material," "polyamine," "polyurethane polyurea resin," "shell portion," "core portion," and "latent heat storage particles" have the same definitions as those described above.
[0062] The step of dispersing a raw material composition having a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension depends on the polyisocyanate used, the latent heat storage material used, the dispersion medium used, etc., and as the conditions, conventionally known conditions depending on the polyisocyanate used, etc. can be used, but are not limited thereto. It is preferable to stir the dispersoid and the dispersion medium during dispersion. In this step, components other than the latent heat storage material contained in the core portion may be added.
[0063] The dispersion medium contains water and may contain a dispersant other than water. Examples of dispersants include, but are not limited to, cellulose-based water-soluble resins (methyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, etc.), polyvinyl alcohol, polyacrylates, polyethylene glycol, polyvinylpyrrolidone, polyacrylamide, tertiary phosphates, colloidal silica, and the like. The dispersing agent may be used alone or in combination of two or more kinds. The content of the dispersant is 0.001 to 5 parts by weight, preferably 0.1 to 4.9 parts by weight, more preferably 0.5 to 4.8 parts by weight, and most preferably 1.0 to 4.7 parts by weight, relative to 100 parts by weight of water.
[0064] The dispersion medium may contain a surfactant. Examples of the surfactant include, but are not limited to, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. The surfactants may be used alone or in combination of two or more kinds.
[0065] The raw material composition preferably contains a urethanization catalyst. Examples of the urethanization catalyst include, but are not limited to, metal catalysts such as dibutyltin laurate, and amine catalysts such as triethylamine.
[0066] Next, the production method of the present invention carries out a step of adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine, and the polyol. This step depends on the suspension used, specifically the polyisocyanate, latent heat storage material, and dispersion medium used, and also on the polyol and polyamine used. During and after the addition of the polyol and polyamine, the suspension should be stirred.
[0067] The amounts of polyisocyanate, polyol and polyamine depend on the polyisocyanate, polyol, latent heat storage material, dispersion medium, polyamine and the like used. For example, the amount of polyisocyanate is 5 to 99.5 parts by weight, preferably 45 to 98.0 parts by weight, more preferably 55 to 96.5 parts by weight, and most preferably 65 to 95.0 parts by weight, based on 100 parts by weight in total of polyisocyanate, polyol, and polyamine. For example, the amount of polyol is preferably 1 to 80 parts by weight, 2 to 50 parts by weight, more preferably 3 to 30 parts by weight, and most preferably 5 to 20 parts by weight, out of 100 parts by weight in total of polyisocyanate, polyol, and polyamine. Furthermore, for example, the amount of polyamine is 0.5 to 15 parts by weight, preferably 1.5 to 14 parts by weight, more preferably 2.0 to 12 parts by weight, and most preferably 3.0 to 10 parts by weight, based on 100 parts by weight in total of polyisocyanate, polyol, and polyamine.
[0068] It is advisable to heat the reaction step. The heating conditions depend on the suspension used, specifically the polyisocyanate, latent heat storage material, and dispersion medium used, as well as the polyol and polyamine used, but examples of the conditions include, but are not limited to, a temperature of 50 to 70°C for 1 to 6 hours, followed by a temperature of 90 to 100°C for 1 to 3 hours. It is advisable to stir the suspension when heating.
[0069] After the reaction step, the mixture is cooled to room temperature, and the latent heat storage particles are recovered by a conventionally known solid-liquid separation method. The recovered latent heat storage particles are preferably washed and dried.
[0070] <Material Having Latent Heat Storage Particles of the Present Invention> The present application provides a material having latent heat storage particles. The latent heat storage particles of the present invention may be used as they are, or may be mixed with other materials to form a material having latent heat storage particles. Examples of materials include, but are not limited to, paper, media (water, heat transfer media), thermoplastic resins, thermosetting resins, rubber, elastomers, and thermoplastic elastomers. For example, the latent heat storage particles of the present invention may be disposed on at least one surface of a support made of a sheet-like material such as synthetic paper, plastic film, rubber sheet, metal sheet, glass, etc. This latent heat storage particle layer may further contain a binder resin (e.g., UV-curable resin such as urethane acrylate or acrylic acrylate, water-soluble resin such as polyvinyl alcohol or polyacrylamide), a thickener, a leveling agent, a binder resin curing agent (organic peroxide, photoradical generator), etc., as necessary. These may be used in combination. In particular, the latent heat storage particles of the present invention are preferably mixed with a resin and provided as a resin sheet or rubber sheet having the latent heat storage particles. The content of the latent heat storage particles in the material having the latent heat storage particles is not particularly limited. 2 shows a cross-sectional view of an example of a material having the latent heat storage particles of the present invention. For example, by mixing the latent heat storage particles 10 of the present invention with a resin 22 such as a thermoplastic resin or a thermosetting resin, applying the resulting material 20 to a substrate 24, and then drying it, a material having the latent heat storage particles of the present invention on its surface, such as a heat storage sheet, can be provided.
[0071] The latent heat storage particles and materials containing latent heat storage particles of the present invention can be used for various purposes. For example, the material can be used for, but is not limited to, electronic devices (e.g., mobile phones (particularly smartphones), wearables, personal digital assistants, personal computers (particularly portable personal computers), game consoles, remote controls, etc.); battery cases for electrically powered mobility (cars, motorcycles, drones); building materials (e.g., flooring, roofing, wall materials, etc.) suitable for temperature control in response to sudden temperature increases during the day or when heating or cooling indoors; clothing (e.g., underwear, jackets, winter clothing, gloves, etc.) suitable for temperature control in response to changes in environmental temperature or changes in body temperature during exercise or at rest; bedding; and exhaust heat utilization systems that store unnecessary exhaust heat and use it as thermal energy. The applications include the following, but are not limited to the following applications as long as the latent heat storage particles can be used to take in and release heat. Heat pumps; air conditioning applications in buildings, homes, underground shopping malls, etc.; vehicle air conditioning and canister applications; applications to prevent heating of electronic components such as IC chips and electrical and electronic equipment; constant temperature applications for clothing; cold storage applications for fresh food or organ transport containers; constant temperature applications for structural materials in buildings (homes, buildings, etc.) and structures (roads, bridges, etc.); anti-fogging applications for mirror surfaces such as convex mirrors; anti-freezing applications for road surfaces; cooling and constant temperature applications for home appliances such as refrigerators; ice packs and hand warmers for everyday items, etc. EXAMPLES
[0072] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. Example 1 A 2 L separable flask equipped with a stirrer was charged with 800 g of water, and 10 g of hydroxypropyl methylcellulose was dissolved in the water to prepare a dispersion medium. A raw material composition was prepared by mixing 210 g of cetyl myristate (LogP: 9.93, melting point 47°C, latent heat 230 J / g) and 80 g of hydrogenated XDI isocyanurate. LogP was calculated using free software based on the CLogP method and available on the Molinspiration Cheminformatics website. The temperature of the dispersion medium was raised to 50° C., and the raw material composition was added to the dispersion medium while stirring at 300 rpm to prepare a suspension for polymerization. While stirring the polymerization suspension, 5 g of ethylene glycol and 5 g of ethylenediamine were added to the liquid and stirred for 1 hour. Then, the polymerization suspension was heated to 60° C. and stirred for 2 hours, and further heated to 95° C. and stirred for 1 hour. The dispersion was cooled to room temperature, and the particles in the dispersion were collected by solid-liquid separation.
[0073] The obtained particles were thoroughly washed with water and then dried at 60°C for 20 hours to obtain heat storage particles with a volume average particle diameter of 151 μm. The volume average particle diameter was measured using a laser diffraction particle size distribution measuring device (LA-950V2, manufactured by Horiba, Ltd.) and the volume-based median diameter was used as the volume average particle diameter. The above-described particles were measured using a differential scanning calorimeter (DSC, manufactured by Rigaku Corporation, DSCvesta) in accordance with JIS K-7121. The melting point and latent heat were confirmed from the obtained DSC chart and were found to be 47° C. and 170 J / g, respectively. In addition, in order to confirm the durability in long-term use, the particles obtained above were subjected to 100 melt-solidification cycles in which they were heated from 25°C to 65°C over 30 minutes and then cooled to 25°C over a further 30 minutes.Then, a thermal shock test was performed to check the dissolution of the material contained in the core into the oil blotting paper, and no dissolution of the material into the oil blotting paper was confirmed.
[0074] Furthermore, in order to confirm long-term storage stability, an accelerated test was performed to measure the weight loss at 110°C for 6 hours, which was 0.1%. The heat loss was calculated from the change in weight before and after the heat treatment using the following formula (1). The heat loss was evaluated three times and the average value was used. [Weight loss from heating (%)] = 100 × {[Weight of latent heat storage particles before heat treatment (g)] - [Weight of latent heat storage particles after treatment (g)]} / [Weight of latent heat storage particles before heat treatment (g)] Formula (1)
[0075] (Examples 2 to 11, Comparative Examples 1 to 8) Latent heat storage particles were obtained in the same manner as in Example 1, except that the types or amounts of the solvent, polyisocyanate, latent heat storage material, and dispersion medium were changed as shown in Table 1. When a "solvent" was used, it was mixed with the latent heat storage material and polyisocyanate to prepare a raw material composition. The "solvent" was then evaporated from the particles in a process of heating to 95°C and stirring for 1 hour. The latent heat storage materials used in the examples and comparative examples are described below. The melting point and latent heat quantity of the latent heat storage material were measured in the same manner as the above-mentioned measurement method for the particles. Cetyl myristate (LogP: 9.93, melting point 47°C, latent heat 230 J / g) Methyl stearate (LogP: 8.32, melting point 38°C, latent heat 220 J / g) n-Docosane (LogP: 9.56, melting point 42°C, latent heat 250 J / g) Stearyl stearate (LogP: 10.29, melting point 62°C, latent heat 230 J / g) Methyl hexadecanoate (LogP: 7.37, melting point 27°C, latent heat 220 J / g) Methyl tetradecanoate (LogP: 6.36, melting point 18°C, latent heat 210 J / g) n-Heptadecane (LogP: 8.79, melting point 9, 19℃, latent heat 230J / g) n-Octacosane (LogP 10.1, melting point 64°C, latent heat 165 J / g).
[0076] The obtained particles were subjected to volume average particle size measurement, melting point measurement, thermal shock test, and heat loss measurement in the same manner as in Example 1. The results are shown in Table 2. In the "thermal shock test" in Table 2, "○" indicates that no elution of the latent heat storage material was confirmed after the thermal shock test, and "×" indicates that elution of the latent heat storage material was confirmed after the thermal shock test. It can be seen from Tables 1 and 2 that Examples 1 to 11 have the desired properties, ie, the desired heat loss value, the desired melting point, the desired thermal shock test resistance, and the desired volume average particle size.
[0077] On the other hand, in Comparative Example 1, an isocyanurate of HDI was used as the polyisocyanate, but it was found that it could not be granulated by the above method. In addition, in Comparative Example 2, stearyl stearate was used as the latent heat storage material, but it was found that it could not be granulated by the above-mentioned method. Furthermore, in Comparative Example 5, n-octacosane was used as the latent heat storage material, but it was found that it could not be granulated by the above method.
[0078] In Comparative Example 3, methyl tetradecanoate was used as the latent heat storage material and granulated, but the heat loss value (2.2%) was not the desired value, and the melting point (18° C.) was also not the desired value. In Comparative Example 4, n-heptadecane was used as the latent heat storage material to form the particles, but the loss on heating (2.5%) was not the desired value, the melting points (9°C and 19°C) were not the desired values, and the particles did not have resistance to thermal shock tests. In Comparative Examples 6 to 8, particles were formed without using polyol (Comparative Example 6), polyamine (Comparative Example 7), or neither polyol nor polyamine (Comparative Example 8), but none of them had resistance to the thermal shock test.
[0079] [Table 1] TIFF2024161940000003.tif218162
[0080] [Table 2]
Claims
1. A latent heat storage particle having a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material, the heat loss being 2% by weight or less after heating at 110° C. for 6 hours.
2. 2. The latent heat storage particles according to claim 1, wherein the melting point of the latent heat storage particles as measured in accordance with JIS-K7121 is 30° C. or higher and 60° C. or lower.
3. 2. The latent heat storage particle according to claim 1, wherein the latent heat storage material has a water / octanol partition coefficient Log P of 8 or more and 10 or less.
4. 2. The latent heat storage particle according to claim 1, wherein the polyurethane polyurea resin has a structure derived from an alicyclic diisocyanate.
5. 2. The latent heat storage particles according to claim 1, wherein the latent heat storage particles have a volume average particle size of 1 to 500 μm.
6. A material comprising the latent heat storage particles according to any one of claims 1 to 5.
7. A step of dispersing a raw material composition having a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine and the polyol; By having A method for producing latent heat storage particles, which has a shell portion having a polyurethane polyurea resin and a core portion having the latent heat storage material, and which produces latent heat storage particles having a heat loss of 2% by weight or less after heating at 110°C for 6 hours.
Citation Information
Patent Citations
Wall material for building
JP2019112929A
Heat storage particles, method for producing same, and heat storage material
WO2017135025A1
Thermal storage sheet, thermal storage member, and electronic device
WO2020110662A1
Microcapsule, heat storage composition, heat storage sheet, and method for producing microcapsule
WO2021131404A1
Method of classifying coarse substance by classifing current in horizontal direction and device for executing said method
JP1981051272A