Polyurethane resin composition and elastic pavement material

The polyurethane resin composition, with alicyclic polyisocyanate and balanced diethyltoluene/polyoxyalkylene amines, addresses pot life and moldability issues, resulting in high-productivity elastic paving materials with excellent uneven surfaces.

JP2024161983APending Publication Date: 2024-11-21MITSUI CHEMICALS INC

Patent Information

Application Number
JP2023077096
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing two-component curing urea waterproofing materials using polyurethane resin compositions suffer from insufficient pot life and require improved irregularity moldability for forming uneven shapes in elastic paving materials.

Method used

A polyurethane resin composition containing a polyisocyanate component with an isocyanate group-terminated prepolymer, primarily composed of alicyclic polyisocyanate, and an active hydrogen group-containing component with a specific ratio of diethyltoluene polyamine and polyoxyalkylene polyamine, optimized to enhance pot life and hilling properties.

Benefits of technology

The composition achieves an extended pot life and superior uneven surface formation, enabling high productivity and excellent hilling properties in elastic paving materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161983000002
    Figure 2024161983000002
  • Figure 2024161983000001
    Figure 2024161983000001
Patent Text Reader

Abstract

To provide a polyurethane resin composition with superior pot life and superior surface irregularity, and an elastic pavement material prepared from the polyurethane resin composition.SOLUTION: A polyurethane resin composition contains a polyisocyanate component and an active hydrogen group-containing component. The polyisocyanate component contains an isocyanate group-terminated prepolymer. The active hydrogen group-containing component contains diethyl toluene polyamine, and polyoxy alkylene polyamine. The content of amino groups derived from the diethyl toluene polyamine is more than 6 mol relative to 1 mol of amino groups derived from the polyoxy alkylene polyamine.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyurethane resin composition and an elastic paving material. [Background technology]

[0002] At present, flooring materials and paving materials containing a cured product (resin cured product) of a polyurethane resin composition are known. As a polyurethane resin composition, for example, a two-component curing type polyurethane resin composition is known. The two-component curing type resin composition includes a base agent and a curing agent. The base agent and the curing agent are mixed at the time of use to generate a cured product. The cured product is used as a flooring material and / or a paving material.

[0003] More specifically, a two-component curing urea waterproofing material has been proposed as a cured product (resin cured product) of a polyurethane resin composition. This two-component curing urea waterproofing material is obtained, for example, by reacting the following A-liquid and B-liquid. The A-liquid contains a urethane prepolymer. The B-liquid contains an active hydrogen group-containing compound. The A-liquid contains a urethane prepolymer obtained by reacting carbodiimide-modified 4,4'-diphenylmethane diisocyanate with polypropylene glycol. The B-liquid contains 100 parts by mass of polyoxyalkylene polyamine having an average molecular weight of 2000, 17.1 parts by mass of polyoxyalkylene polyamine having an average molecular weight of 5000, and 25.7 parts by mass of diethyltoluenediamine (see, for example, Patent Document 1 (Examples)). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-166201 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the above-mentioned two-component curing type urea waterproofing material, the mixture of the A component and the B component may not have a sufficient pot life.

[0006] Furthermore, when a cured product of the polyurethane resin composition is used as an elastic paving material, the elastic paving material may be required to have an uneven surface, i.e., the polyurethane resin composition is required to have excellent hill-standing properties (unevenness formability).

[0007] The present invention relates to a polyurethane resin composition having an excellent pot life and excellent hill standing property, and an elastic paving material obtained from the polyurethane resin composition. [Means for solving the problem]

[0008] The present invention [1] comprises a polyurethane resin composition comprising a polyisocyanate component and an active hydrogen group-containing component, the polyisocyanate component comprising an isocyanate group-terminated prepolymer, the active hydrogen group-containing component comprising diethyltoluenepolyamine and polyoxyalkylenepolyamine, and the content of amino groups derived from diethyltoluenepolyamine exceeds 6 moles per mole of amino groups derived from polyoxyalkylenepolyamine.

[0009] The present invention [2] comprises the polyurethane resin composition according to the above [1], in which the content ratio of amino groups derived from diethyltoluenepolyamine is 9 mol or more and 40 mol or less per 1 mol of amino groups derived from polyoxyalkylenepolyamine.

[0010] The present invention [3] comprises the polyurethane resin composition according to the above [1] or [2], in which the isocyanate-terminated prepolymer contains a reaction product of a raw material polyisocyanate and a raw material polyol, and the raw material polyisocyanate contains an alicyclic polyisocyanate.

[0011] The present invention [4] includes an elastic paving material containing a cured product of the polyurethane resin composition according to any one of the above [1] to [3]. Effect of the Invention

[0012] In the polyurethane resin composition of the present invention, the active hydrogen group-containing component contains diethyltoluene polyamine and polyoxyalkylene polyamine. The content ratio of diethyltoluene polyamine and polyoxyalkylene polyamine is adjusted. Therefore, the polyurethane resin composition has an excellent pot life and excellent peaking property.

[0013] The elastic paving material of the present invention contains a cured product of the above polyurethane resin composition, and therefore the elastic paving material of the present invention can be produced with good productivity due to its excellent pot life, and has an excellent uneven shape due to its excellent hill-standing property. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a photograph showing the cured product of Comparative Example 1 (peak shape x), the cured product of Example 2 (peak shape ◯), and the cured product of Example 1 (peak shape Δ). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] 1. Polyurethane resin composition The polyurethane resin composition contains a polyisocyanate component and an active hydrogen group-containing component. As described in detail below, the polyurethane resin composition produces a cured product (resin cured product) by a reaction between the polyisocyanate component and the active hydrogen group-containing component.

[0016] (1) Polyisocyanate component The polyisocyanate component is a component containing two or more isocyanate groups in the molecule. The polyisocyanate component contains an isocyanate group-terminated prepolymer.

[0017] The isocyanate-terminated prepolymer is a urethane prepolymer having at least two isocyanate groups at the molecular end. The isocyanate-terminated prepolymer contains, for example, a reaction product of a raw polyisocyanate and a raw polyol. Preferably, the isocyanate-terminated prepolymer is a reaction product of a raw polyisocyanate and a raw polyol.

[0018] Examples of raw material polyisocyanates include aliphatic polyisocyanates, aromatic polyisocyanates, and araliphatic polyisocyanates.

[0019] Examples of the aliphatic polyisocyanate include linear aliphatic polyisocyanates and alicyclic polyisocyanates.

[0020] Examples of the chain aliphatic polyisocyanate include chain aliphatic polyisocyanate monomers and chain aliphatic polyisocyanate derivatives. Examples of the chain aliphatic polyisocyanate monomers include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate (PDI) and hexamethylene diisocyanate (HDI). Examples of the chain aliphatic polyisocyanate derivatives include modified products obtained by modifying chain aliphatic polyisocyanate monomers by known methods. Examples of the modified products include uretdione modified products, isocyanurate modified products, allophanate modified products, polyol modified products, biuret modified products, urea modified products, oxadiazinetrione modified products and carbodiimide modified products. These can be used alone or in combination of two or more types.

[0021] Examples of the alicyclic polyisocyanate include alicyclic polyisocyanate monomers and alicyclic polyisocyanate derivatives. Examples of the alicyclic polyisocyanate monomers include alicyclic diisocyanates. Examples of the alicyclic diisocyanates include isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), methylene bis(cyclohexyl isocyanate) (H 12 MDI), and bis(isocyanatomethyl)cyclohexane (H 6 XDI). Examples of the alicyclic polyisocyanate derivatives include the above-mentioned modified products of the alicyclic polyisocyanate monomers. These can be used alone or in combination of two or more kinds.

[0022] Examples of aromatic polyisocyanates include aromatic polyisocyanate monomers and aromatic polyisocyanate derivatives. Examples of aromatic polyisocyanate monomers include aromatic diisocyanates. Examples of aromatic diisocyanates include diphenylmethane diisocyanate (MDI), tolylene diisocyanate (TDI), toluidine diisocyanate (TODI), paraphenylene diisocyanate, and naphthalene diisocyanate (NDI). Examples of aromatic polyisocyanate derivatives include the above-mentioned modified products of aromatic polyisocyanate monomers. In addition, examples of aromatic polyisocyanate derivatives include polymethylene polyphenylene polyisocyanates. These can be used alone or in combination of two or more.

[0023] Examples of the araliphatic polyisocyanate include araliphatic polyisocyanate monomers and araliphatic polyisocyanate derivatives. Examples of the araliphatic polyisocyanate monomers include araliphatic diisocyanates. Examples of the araliphatic diisocyanates include xylylene diisocyanate (XDI) and tetramethyl xylylene diisocyanate (TMXDI). Examples of the araliphatic polyisocyanate derivatives include the above-mentioned modified products of the araliphatic polyisocyanate monomers. These can be used alone or in combination of two or more kinds.

[0024] The raw material polyisocyanate can be used alone or in combination of two or more kinds. From the viewpoint of improving mechanical properties, the raw material polyisocyanate is preferably an alicyclic polyisocyanate or an aromatic polyisocyanate, and from the viewpoint of improving pot life, more preferably an alicyclic polyisocyanate, even more preferably an alicyclic polyisocyanate monomer, more preferably an alicyclic diisocyanate, and particularly preferably isophorone diisocyanate (IPDI).

[0025] The average number of isocyanate groups in the raw material polyisocyanate is, for example, not less than 2. In addition, the average number of isocyanate groups in the raw material polyisocyanate is, for example, not more than 4, preferably not more than 3, more preferably not more than 2.5, and further preferably not more than 2.2.

[0026] Examples of the raw material polyol include high molecular weight polyols and low molecular weight polyols.

[0027] The high molecular weight polyol has two or more hydroxyl groups in the molecule and is a relatively high molecular weight organic compound. The number average molecular weight of the high molecular weight polyol is, for example, more than 400, for example, 20,000 or less. The number average molecular weight can be calculated by a known method from the hydroxyl group equivalent and the average number of hydroxyl groups. The number average molecular weight can be measured as a polystyrene-equivalent molecular weight by gel permeation chromatography (hereinafter the same).

[0028] Examples of high molecular weight polyols include polyether polyols, polyester polyols, polycarbonate polyols, polyurethane polyols, epoxy polyols, vegetable oil polyols, polyolefin polyols, acrylic polyols, and vinyl monomer modified polyols.These high molecular weight polyols can be used alone or in combination of two or more kinds.Preferably, the high molecular weight polyols include polyether polyols.

[0029] Examples of polyether polyols include polyoxyalkylene (C2-3) polyols and polytetramethylene ether polyols. Examples of polyoxyalkylene (C2-3) polyols include polyoxyethylene polyols, polyoxypropylene polyols, polyoxytriethylene polyols, and polyoxyethylene-polyoxypropylene polyols (random or block copolymers). Examples of polytetramethylene ether polyols include crystalline polytetramethylene ether glycols and amorphous polytetramethylene ether glycols. These can be used alone or in combination of two or more kinds. Examples of polyether polyols include preferably polyoxyalkylene (C2-3) polyols, more preferably polyoxypropylene polyols.

[0030] The number average molecular weight of the high molecular weight polyol is, for example, more than 400, preferably 500 or more, more preferably 1000 or more, and even more preferably 1500 or more. The number average molecular weight of the high molecular weight polyol is, for example, 20000 or less, preferably 15000 or less, more preferably 10000 or less, and even more preferably 5000 or less.

[0031] The average number of hydroxyl groups in the high molecular weight polyol is, for example, 2 or more, preferably more than 2, and more preferably 2.1 or more. The average number of hydroxyl groups in the high molecular weight polyol is, for example, 4 or less, preferably 3 or less, more preferably less than 3, and even more preferably 2.9 or less.

[0032] Particularly preferred examples of the high molecular weight polyol include a polyether polyol having an average number of hydroxyl groups of 2 and a polyether polyol having an average number of hydroxyl groups of 3. The ratio of these to be used in combination is appropriately adjusted depending on the purpose and application.

[0033] The low-molecular-weight polyol is an organic compound having two or more hydroxyl groups in the molecule and a relatively low molecular weight. The molecular weight of the low-molecular-weight polyol is, for example, 40 or more, for example, 400 or less.

[0034] Examples of low molecular weight polyols include dihydric alcohols, trihydric alcohols, and tetrahydric or higher alcohols. Examples of dihydric alcohols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of trihydric alcohols include glycerin and trimethylolpropane. Examples of tetrahydric or higher alcohols include pentaerythritol and diglycerin. These can be used alone or in combination of two or more.

[0035] The raw material polyols can be used alone or in combination of two or more kinds. As the raw material polyol, preferably, a high molecular weight polyol is used alone.

[0036] The average number of hydroxyl groups in the raw material polyol is, for example, 2 or more, preferably more than 2, and more preferably 2.2 or more. The average number of hydroxyl groups in the raw material polyol is, for example, 4 or less, preferably 3 or less, more preferably less than 3, and even more preferably 2.8 or less.

[0037] A known method is used for preparing the isocyanate-terminated prepolymer. For example, a raw material polyisocyanate and a raw material polyol are subjected to a urethane reaction at a predetermined equivalent ratio. For example, the equivalent ratio (NCO / OH) of the isocyanate group of the raw material polyisocyanate to the hydroxyl group of the raw material polyol exceeds 1, preferably 1.5 or more, and is, for example, 50 or less. The reaction conditions of the raw material polyisocyanate and the raw material polyol are appropriately set. As a result, an isocyanate-terminated prepolymer is obtained as a reaction product of the raw material polyisocyanate and the raw material polyol. If necessary, the isocyanate-terminated prepolymer is purified by a known purification method. Examples of the purification method include an extraction method and a distillation method.

[0038] The polyisocyanate component may contain other polyisocyanate compounds as necessary. The other polyisocyanate compounds are polyisocyanate compounds other than isocyanate-terminated prepolymers. Examples of the other polyisocyanate compounds include known polyisocyanate monomers and known polyisocyanate derivatives.

[0039] The content ratio of the other polyisocyanate compound is appropriately set according to the purpose and application. More specifically, the content ratio of the other polyisocyanate compound is, for example, 50 mass% or less, preferably 30 mass% or less, more preferably 10 mass% or less, and particularly preferably 0 mass% based on the total amount of the polyisocyanate component.

[0040] That is, the content of the isocyanate-terminated prepolymer is, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or less, and particularly preferably 100% by mass, based on the total amount of the polyisocyanate component. In other words, the polyisocyanate component is preferably composed of an isocyanate-terminated prepolymer.

[0041] The isocyanate group content of the polyisocyanate component is, for example, 1.0 mass% or more, preferably 3.0 mass% or more. The isocyanate group content of the polyisocyanate component is, for example, 20 mass% or less, preferably 10 mass% or less, more preferably 5.0 mass% or less. The isocyanate group content is measured by the isocyanate group content test described in JIS K 7301 (1995).

[0042] (2) Active hydrogen group-containing components The active hydrogen group-containing component is a component that contains one or more active hydrogen groups (hydroxyl groups and / or amino groups) in the molecule. The active hydrogen group-containing component contains diethyltoluenepolyamine and polyoxyalkylenepolyamine.

[0043] Diethyltoluene polyamine is diethyltoluene having two or more amino groups. The amino groups include primary amino groups and / or secondary amino groups, and preferably primary amino groups (hereinafter the same). More specifically, diethyltoluene polyamines include, for example, diethyltoluene diamine and diethyltoluene triamine. These can be used alone or in combination of two or more. Diethyltoluene diamine is preferably used. Diethyltoluene diamines include, for example, 2,4-diethyltoluene diamine and 2,6-diethyltoluene diamine. These can be used alone or in combination of two or more. Diethyltoluene polyamines are available as commercial products. Commercial products include, for example, Ethacure 100 (a mixture of 2,4-diethyltoluene diamine and 2,6-diethyltoluene diamine, manufactured by Albemarle).

[0044] Polyoxyalkylene polyamine is a polyether polyamine having two or more amino groups at the molecular end. More specifically, examples of polyoxyalkylene polyamine include polyoxyethylene polyamine, polyoxypropylene polyamine, polyoxytetramethylene polyamine, and polyoxyethylene polyoxypropylene polyamine. These can be used alone or in combination of two or more. Preferably, polyoxypropylene polyamine is used. Examples of polyoxypropylene polyamine include polyoxypropylene diamine, polyoxypropylene triamine, and polyoxypropylene tetraamine. These can be used alone or in combination of two or more. Preferably, polyoxypropylene diamine is used. Polyoxyalkylene polyamine is available as a commercially available product. Commercially available products include, for example, the Jeffamine series (manufactured by Huntsman), more specifically, Jeffamine D-230, Jeffamine D-400, Jeffamine D-2000, Jeffamine T-403, and Jeffamine T-3000 (product names, all manufactured by Huntsman).

[0045] The number average molecular weight of the polyoxyalkylene polyamine is, from the viewpoint of mechanical properties (especially, elongation), for example, 200 or more, preferably 500 or more, more preferably 1000 or more, and even more preferably 1500 or more. In addition, the number average molecular weight of the polyoxyalkylene polyamine is, from the viewpoint of mechanical properties (especially, hardness and strength), for example, 20000 or less, preferably 15000 or less, more preferably 10000 or less, and even more preferably 5000 or less.

[0046] The average number of amino groups in the polyoxyalkylene polyamine is, from the viewpoint of mechanical properties (especially hardness and strength), for example, 2 or more. Also, the average number of amino groups in the polyoxyalkylene polyamine is, from the viewpoint of mechanical properties (especially elongation), for example, 4 or less, preferably 3 or less, more preferably 2.5 or less.

[0047] The content ratio of diethyltoluenepolyamine and polyoxyalkylenepolyamine is adjusted as the molar ratio of amino groups.

[0048] More specifically, from the viewpoints of pot life, mechanical properties and hill-standing property, the content ratio of amino groups derived from diethyltoluenepolyamine exceeds 6 moles per mole of amino groups derived from polyoxyalkylenepolyamine, and is preferably 7 moles or more, more preferably 9 moles or more, even more preferably 10 moles or more, and particularly preferably 15 moles or more.

[0049] In addition, from the viewpoints of pot life, mechanical properties, and hill-standing property, the content ratio of amino groups derived from diethyltoluenepolyamine is, for example, 80 mol or less, preferably 60 mol or less, more preferably 40 mol or less, even more preferably 30 mol or less, and particularly preferably 25 mol or less, per 1 mol of amino groups derived from polyoxyalkylenepolyamine.

[0050] The content ratio of diethyltoluenepolyamine to polyoxyalkylenepolyamine on a mass basis is appropriately set depending on the molecular weight of the polyoxyalkylenepolyamine.

[0051] The active hydrogen group-containing component can contain other active hydrogen compounds as necessary.The other active hydrogen compounds are active hydrogen compounds other than diethyltoluene polyamine and polyoxyalkylene polyamine.The other active hydrogen compounds include, for example, known polyamines (other than diethyltoluene polyamine and polyoxyalkylene polyamine) and the above-mentioned low molecular weight polyols.

[0052] The content ratio of other active hydrogen compounds is appropriately set according to the purpose and use. More specifically, the content ratio of other active hydrogen compounds is, for example, 50 mass% or less, preferably 30 mass% or less, more preferably 10 mass% or less, particularly preferably 0 mass% based on the total amount of active hydrogen group-containing components.

[0053] That is, the total content of diethyltoluenepolyamine and polyoxyalkylenepolyamine is, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or less, and particularly preferably 100% by mass, based on the total amount of the active hydrogen group-containing component. In other words, the active hydrogen group-containing component is preferably composed of diethyltoluenepolyamine and polyoxyalkylenepolyamine.

[0054] (3) Other ingredients The polyurethane resin composition may contain other components. The other components are components other than the polyisocyanate component and the active hydrogen group-containing component. Examples of the other components include additives.

[0055] Examples of additives include solvents, fillers, plasticizers, pigments, defoamers, catalysts, antiblocking agents, dispersants, antisettling agents, heat stabilizers, light stabilizers, antioxidants, release agents, dyes, lubricants, and hydrolysis inhibitors. These can be used alone or in combination of two or more. Preferred additives include solvents, fillers, and plasticizers.

[0056] Examples of the solvent include ketones, nitriles, alkyl esters, aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, ethers, glycol ether esters, halogenated aliphatic hydrocarbons, and polar aprotons. These can be used alone or in combination of two or more. Examples of the solvent include alkyl esters. Examples of the alkyl esters include methyl acetate, ethyl acetate, butyl acetate, and isobutyl acetate, and preferably butyl acetate.

[0057] Examples of the filler include inorganic fillers and organic fillers. Examples of the inorganic filler include granular fillers, fibrous fillers, and balloon-shaped fillers. Examples of the granular filler include calcium carbonate, aluminum oxide, hydrated basic magnesium carbonate, kaolinite, halloysite, allophane, pyrophyllite, talc, sericite, illite, mica, montmorillonite, paidelite, amesite, chamosite, calcined clay, asbestos, mica, bentonite, calcium silicate, zeolite, pumice powder, slate powder, diatomaceous earth, silica sand, silica stone powder, gibbsite, boehmite, barium sulfate, calcium sulfate, metal powder, wet silica, and dry silica. Examples of the fibrous filler include glass fiber and carbon fiber. Examples of the balloon-shaped filler include glass balloons, shirasu balloons, silica balloons, and ceramic balloons. Examples of organic fillers include wood flour, pulp powder, cotton chips, rubber powder, thermoplastic resin powder, and thermosetting resin powder. These can be used alone or in combination of two or more. Preferably, inorganic fillers are used, more preferably granular fillers are used, and even more preferably calcium carbonate is used.

[0058] Examples of the plasticizer include phthalate ester plasticizers, adipate ester plasticizers, aliphatic dibasic acid ester plasticizers, glycol ester plasticizers, phosphate ester plasticizers, and epoxy plasticizers. These can be used alone or in combination of two or more. Examples of the plasticizer include phthalate ester plasticizers and adipate ester plasticizers. Examples of the phthalate ester plasticizers include dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diheptyl phthalate, di-n-octyl phthalate, diisooctyl phthalate, di-2-ethylhexyl phthalate, dinonyl phthalate, diisodecyl phthalate, ditridecyl phthalate, dibutyl pentyl phthalate, and dicyclohexyl phthalate. Examples of the adipate plasticizer include dimethyl adipate, diethyl adipate, dibutyl adipate, diheptyl adipate, diisononyl adipate, di-n-octyl adipate, diisooctyl adipate, di-2-ethylhexyl adipate, dinonyl adipate, diisononyl adipate, diisodecyl adipate, ditridecyl adipate, dibutyl pentyl adipate, and dicyclohexyl adipate. These can be used alone or in combination of two or more. Preferably, phthalate plasticizers are used, and more preferably, diisononyl phthalate (DINP).

[0059] The amount and timing of the additives are appropriately set according to the purpose and application. For example, in a two-liquid resin composition described later, the additives may be contained in the A liquid described later, or in the B liquid described later. Preferably, the additives are contained in both the A liquid described later and the B liquid described later.

[0060] (4) Method for producing polyurethane resin composition The polyurethane resin composition may be, for example, a two-component type resin composition or a one-component type resin composition. The polyurethane resin composition is preferably a two-component type resin composition.

[0061] When the polyurethane resin composition is a two-component resin composition, the polyurethane resin composition is produced, for example, by separately preparing a liquid A containing a polyisocyanate component and a liquid B containing an active hydrogen group-containing component.

[0062] Liquid A contains, for example, the above-mentioned polyisocyanate component as an essential component. Liquid A also contains, for example, the above-mentioned additives as optional components, and preferably contains the above-mentioned solvent. Particularly preferably, Liquid A consists of a polyisocyanate component and a solvent. In such a case, Liquid A is prepared, for example, by mixing the polyisocyanate component and the solvent by a known method. The content ratio of each component in Liquid A is appropriately set according to the purpose and application.

[0063] For example, the content of the polyisocyanate component is, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, based on the total amount of the polyisocyanate component and the solvent. Also, the content of the polyisocyanate component is, for example, 99.9% by mass or less, preferably 99% by mass or less, more preferably 98% by mass or less, based on the total amount of the polyisocyanate component and the solvent.

[0064] The content of the solvent is, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more, based on the total amount of the polyisocyanate component and the solvent. The content of the solvent is, for example, 50% by mass or less, preferably 30% by mass or less, more preferably 10% by mass or less, based on the total amount of the polyisocyanate component and the solvent.

[0065] The content of the solvent is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, more preferably 2 parts by mass or more, relative to 100 parts by mass of the polyisocyanate component. The content of the solvent is, for example, 50 parts by mass or less, preferably 30 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the polyisocyanate component.

[0066] Liquid B contains, for example, the active hydrogen group-containing component as an essential component. Liquid B also contains, for example, the additives as optional components, and preferably contains the inorganic filler, the plasticizer, and the solvent. Particularly preferably, Liquid B consists of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent. In such a case, Liquid B is prepared, for example, by mixing the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent by a known method. The content ratio of each component in Liquid B is appropriately set according to the purpose and application.

[0067] For example, the content of the active hydrogen group-containing component is, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more, based on the total amount of the active hydrogen group-containing component, inorganic filler, plasticizer and solvent. Also, the content of the active hydrogen group-containing component is, for example, 50% by mass or less, preferably 30% by mass or less, more preferably 10% by mass or less, based on the total amount of the active hydrogen group-containing component, inorganic filler, plasticizer and solvent.

[0068] The content of the inorganic filler is, for example, 40% by mass or more, preferably 50% by mass or more, more preferably 60% by mass or more, based on the total amount of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent. The content of the inorganic filler is, for example, 90% by mass or less, preferably 80% by mass or less, more preferably 70% by mass or less, based on the total amount of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent.

[0069] The content of the plasticizer is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 10% by mass or more, based on the total amount of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent. The content of the plasticizer is, for example, 60% by mass or less, preferably 40% by mass or less, more preferably 20% by mass or less, based on the total amount of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent.

[0070] The content of the solvent is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 10% by mass or more, based on the total amount of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent. The content of the solvent is, for example, 60% by mass or less, preferably 40% by mass or less, more preferably 20% by mass or less, based on the total amount of the active hydrogen group-containing component, the inorganic filler, the plasticizer, and the solvent.

[0071] The content of the inorganic filler is, for example, 500 parts by mass or more, preferably 900 parts by mass or more, more preferably 1000 parts by mass or more, relative to 100 parts by mass of the active hydrogen group-containing component. The content of the inorganic filler is, for example, 4000 parts by mass or less, preferably 2000 parts by mass or less, more preferably 1500 parts by mass or less, relative to 100 parts by mass of the active hydrogen group-containing component.

[0072] The content of the plasticizer is, for example, 100 parts by mass or more, preferably 200 parts by mass or more, more preferably 250 parts by mass or more, relative to 100 parts by mass of the active hydrogen group-containing component. The content of the plasticizer is, for example, 1000 parts by mass or less, preferably 500 parts by mass or less, more preferably 300 parts by mass or less, relative to 100 parts by mass of the active hydrogen group-containing component.

[0073] The content of the solvent is, for example, 50 parts by mass or more, preferably 100 parts by mass or more, more preferably 150 parts by mass or more, relative to 100 parts by mass of the active hydrogen group-containing component. The content of the solvent is, for example, 500 parts by mass or less, preferably 300 parts by mass or less, more preferably 200 parts by mass or less, relative to 100 parts by mass of the active hydrogen group-containing component.

[0074] (5) Cured resin product The polyurethane resin composition is cured by the reaction between the polyisocyanate component and the active hydrogen group-containing component. More specifically, when the polyurethane resin composition is a two-liquid type resin composition, liquid A and liquid B are mixed when the polyurethane resin composition is used. This causes a urethane reaction between the polyisocyanate component and the active hydrogen group-containing component, and the polyurethane resin composition is cured.

[0075] The mixing ratio of liquid A and liquid B is set, for example, according to the molar ratio of the isocyanate group in the polyisocyanate component in liquid A to the active hydrogen group (preferably amino group) in the active hydrogen group-containing component in liquid B.

[0076] More specifically, the equivalent ratio (isocyanate group / active hydrogen group) of the isocyanate group of the polyisocyanate component in the A liquid to the active hydrogen group of the active hydrogen group-containing component in the B liquid is, for example, 0.5 or more, preferably 0.7 or more, more preferably 0.9 or more, even more preferably 1.0 or more, even more preferably more than 1.0, and particularly preferably 1.1 or more. In addition, the equivalent ratio (isocyanate group / active hydrogen group) of the isocyanate group of the polyisocyanate component in the A liquid to the active hydrogen group of the active hydrogen group-containing component in the B liquid is, for example, 5.0 or less, preferably 3.0 or less, more preferably 2.0 or less.

[0077] The mixture of liquid A and liquid B is degassed if necessary. Then, the mixture is poured into a predetermined mold as required, and undergoes a hardening reaction (urethane hardening).

[0078] The curing conditions are not particularly limited. For example, the curing temperature is, for example, 0° C. or higher, preferably 5° C. or higher. The curing temperature is, for example, 80° C. or lower, preferably 40° C. or lower. The curing time is, for example, 10 hours or longer, preferably 24 hours or longer. The curing time is, for example, 20 days or shorter, preferably 10 days or shorter.

[0079] This gives a cured product of the polyurethane resin composition (resin cured product). The cured product of the polyurethane resin composition is aged, if necessary.

[0080] The aging conditions are not particularly limited. For example, the aging temperature is, for example, 0° C. or higher, preferably 5° C. or higher. The aging temperature is, for example, 40° C. or lower, preferably 30° C. or lower. The aging time is, for example, 1 hour or longer, preferably 2 hours or longer. The aging time is, for example, 5 days or shorter, preferably 3 days or shorter.

[0081] (6) Effects In the polyurethane resin composition, the active hydrogen group-containing component contains diethyltoluene polyamine and polyoxyalkylene polyamine. The content ratio of diethyltoluene polyamine and polyoxyalkylene polyamine is adjusted to a predetermined range. Therefore, the polyurethane resin composition has an excellent pot life and excellent peaking property.

[0082] That is, the two-component curing urea waterproofing material described in Patent Document 1 does not have a sufficient pot life. More specifically, in the B component, the content ratio of the amino group derived from diethyltoluenediamine ([25.7 parts by mass x number of functional groups 2 / molecular weight 178] = 0.29 molar parts) is about 2.6 times the content ratio of the amino group derived from polyoxyalkylene polyamine ([100 parts by mass x number of functional groups 2 / molecular weight 2000] + [17.1 parts by mass x number of functional groups 3 / molecular weight 5000] = 0.11 molar parts). Therefore, in the two-component curing urea waterproofing material described in Patent Document 1, there is a problem that the pot life of the mixture of the A component and the B component is not sufficient.

[0083] On the other hand, in the above polyurethane resin composition, the active hydrogen group-containing component contains diethyltoluene polyamine and polyoxyalkylene polyamine. The content ratio of diethyltoluene polyamine and polyoxyalkylene polyamine is adjusted as described above. Therefore, the above polyurethane resin composition has an excellent pot life. Furthermore, the above polyurethane resin composition has an excellent hill-standing property.

[0084] In particular, in the above polyurethane resin composition, if the raw material polyisocyanate of the isocyanate group-terminated prepolymer contains an alicyclic polyisocyanate, a particularly excellent pot life can be obtained compared to when the raw material polyisocyanate is an aromatic polyisocyanate.

[0085] On the other hand, when the raw material polyisocyanate of the isocyanate group-terminated prepolymer contains an alicyclic polyisocyanate, the peaking property may be reduced compared to when the raw material polyisocyanate is an aromatic polyisocyanate.

[0086] However, in the above polyurethane resin composition, the content ratio of diethyltoluenepolyamine and polyoxyalkylenepolyamine is adjusted as described above, so that excellent peaking properties can be obtained even when the raw material polyisocyanate of the isocyanate-terminated prepolymer contains an alicyclic polyisocyanate.

[0087] Therefore, the polyurethane resin composition is suitable for use in various industrial fields requiring pot life and hill-standing property, more specifically, in the field of elastic paving materials.

[0088] 2. Elastic paving material The elastic paving material contains a cured product of the above polyurethane resin composition. That is, the cured product of the above polyurethane resin composition is preferably used as the elastic paving material.

[0089] When the cured product of the above polyurethane resin composition is used as an elastic pavement material, for example, the above polyurethane resin composition is applied to any desired location by a known application method.

[0090] In this method, the polyurethane resin composition is preferably applied so as to form an uneven shape on the surface of the cured product. Examples of the application method include roller embossing and spray embossing.

[0091] In the roller embossing method, for example, first, a base is prepared at a given location to form a base. Next, a primer is uniformly applied to the base. The coating method is not particularly limited, and a known method can be adopted. Next, the surface (flat surface) of the polyurethane resin composition is treated with an embossing roller. This forms an uneven shape on the surface of the polyurethane resin composition. Thereafter, the polyurethane resin composition is cured by the above method. This allows a cured product of the polyurethane resin composition to be formed on the base. If necessary, the surface (uneven surface) of the cured product of the polyurethane resin composition is treated with a top coat.

[0092] The cured product of such a polyurethane resin composition has an uneven surface, and therefore can be used as an elastic paving material having an uneven surface.

[0093] In the spray embossing method, similarly to the above, first, the surface of an arbitrary location is adjusted to form a base. Next, a primer is applied to the base. Next, a polyurethane resin composition is applied onto the primer by a spray method. In this way, the polyurethane resin composition is applied and an uneven shape is formed. Thereafter, the polyurethane resin composition is cured by the above method. In this way, a cured product of the polyurethane resin composition can be formed on the base. If necessary, the surface (uneven surface) of the cured product of the polyurethane resin composition is topcoat-treated.

[0094] The cured product of such a polyurethane resin composition also has an uneven surface, and therefore can be used as an elastic paving material having an uneven surface.

[0095] The elastic paving material contains a cured product of the polyurethane resin composition, and therefore the elastic paving material has an excellent pot life, which allows it to be produced with good productivity, and also has an excellent uneven shape, which results from its excellent hill-standing properties. EXAMPLES

[0096] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, specific numerical values ​​such as blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values ​​(numerical values ​​defined as "less than or equal to" or "less than") or lower limit values ​​(numerical values ​​defined as "more than or equal to" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the above "Form for carrying out the invention".

[0097] <Polyisocyanate component> Manufacturing Example 1 172.7 parts by mass of isophorone diisocyanate (manufactured by Evonik Japan), 619.9 parts by mass of polyether polyol (manufactured by Mitsui Chemicals SKC Polyurethanes, product name Actocol Diol 2000, number average molecular weight 2000, average number of hydroxyl groups 2), and 207.4 parts by mass of polyether polyol (manufactured by Mitsui Chemicals SKC Polyurethanes, product name Actocol Triol 3000, number average molecular weight 3000, average number of hydroxyl groups 3) were heated and mixed at 95°C for 4 hours under a nitrogen atmosphere. As a result, an IPDI-based prepolymer was obtained as an isocyanate group-terminated prepolymer. The isocyanate group content of the IPDI-based prepolymer (based on JIS K 7301 (1995)) was 3.05% by mass.

[0098] Manufacturing Example 2 191.9 parts by mass of 4,4'-diphenylmethane diisocyanate (manufactured by Tosoh), 605.5 parts by mass of polyether polyol (manufactured by Mitsui Chemicals SKC Polyurethanes, product name Actocol Diol 2000, number average molecular weight 2000, average number of hydroxyl groups 2), and 202.6 parts by mass of polyether polyol (manufactured by Mitsui Chemicals SKC Polyurethanes, product name Actocol Triol 3000, number average molecular weight 3000, average number of hydroxyl groups 3) were mixed under nitrogen atmosphere at 95°C for 4 hours. As a result, an MDI-based prepolymer was obtained as an isocyanate group-terminated prepolymer. The isocyanate group content of the MDI-based prepolymer (based on JIS K 7301 (1995)) was 3.05% by mass.

[0099] <Components containing active hydrogen groups> Preparation example 1 As diethyltoluenepolyamine, Ethacure 100 (manufactured by Mitsui Chemicals, amino group number 2) was prepared.

[0100] Preparation example 2 As the polyoxyalkylene polyamine, Jeffamine D-2000 (a polyoxypropylene diamine, manufactured by Huntsman, with a number average molecular weight of 2000 and an average number of amino groups of 2) was prepared.

[0101] Preparation example 3 As the polyoxyalkylene polyamine, Jeffamine D-230 (a polyoxypropylene diamine, manufactured by Huntsman, with a number average molecular weight of 230 and an average number of amino groups of 2) was prepared.

[0102] Preparation example 4 As the polyoxyalkylene polyamine, Jeffamine T-403 (a polyoxypropylene triamine, manufactured by Huntsman, number average molecular weight 440, average number of amino groups 3) was prepared.

[0103] <Polyurethane resin composition> Examples 1 to 6 and Comparative Examples 1 to 2 According to the recipe shown in Table 1, a polyisocyanate component and a solvent were mixed to prepare liquid A.

[0104] In addition, according to the formulation shown in Table 1, diethyltoluenepolyamine and polyoxypropylenepolyamine were mixed with an inorganic filler (product name Sealets 200, calcium carbonate, manufactured by Maruo Calcium Co., Ltd.), a plasticizer (diisononyl phthalate, DINP), and a solvent (butyl acetate) to prepare an active hydrogen group-containing component (liquid B).

[0105] As a result, a polyurethane resin composition comprising liquid A and liquid B (two-component curing polyurethane resin) was obtained.

[0106] Next, liquid A and liquid B were mixed to obtain a mixture according to the recipe shown in Table 1. Liquid A and liquid B were mixed in such a ratio that the equivalent ratio (isocyanate group / amino group) of the isocyanate group of the polyisocyanate component in liquid A to the amino group of the active hydrogen group-containing component in liquid B was 1.14.

[0107] The mixture was degassed, poured into a mold according to the evaluation method described below, and cured for 7 days at 23°C and 55% relative humidity to obtain a cured product. The cured product was then demolded and aged for 2 days at 23°C and 55% relative humidity.

[0108] <Evaluation> (1) Pot life Liquid A was weighed out into a stirring vessel according to the recipe in Table 1. Next, liquid B was added to the stirring vessel according to the recipe in Table 1, and liquids A and B were mixed by stirring at room temperature for 3 minutes. Then, the viscosity of the mixture of liquids A and B was measured.

[0109] More specifically, 100 g of the mixture was placed in a 100 mL container, and the viscosity of the mixture was measured using a B-8M type rotational viscometer in a thermostatic water bath at 25° C. A No. 4 rotor was used. The rotation speed was 6 rpm. The viscosity was measured every minute.

[0110] After mixing liquids A and B, the time it took for the viscosity of the mixture (at 25°C) to reach 100,000 mPa·s was measured as the pot life (working time). The results are shown in the table.

[0111] (2) Mechanical properties Liquid A was weighed out into a stirring vessel according to the recipe in Table 1. Next, liquid B was added to the stirring vessel according to the recipe in Table 1, and liquids A and B were mixed by stirring at room temperature for 3 minutes. The mixture of liquids A and B was then degassed and cured to obtain a sheet made of a cured product.

[0112] More specifically, in accordance with the method described in JIS A6021 (2011) "Urethane rubber-based waterproof coating material for roofs," the mixture was poured into a mold coated with Teflon (registered trademark) to produce a sheet approximately 2 mm thick.

[0113] To prepare the sheets, the mixture was cured for 7 days at 23°C and 50% relative humidity, then removed from the mold and left to cure for 2 days at 23°C and 50% relative humidity with the reverse side facing up.

[0114] The Shore A hardness (HsA) of the obtained sheet was measured according to JIS K6253 (2012). In addition, the tensile strength (TS), elongation at break (EL) and tear strength (TR) were measured according to JIS A6021 (2011). The results are shown in the table.

[0115] (3) Mountain-dwelling Liquid A was weighed out into a stirring vessel according to the recipe in Table 1. Next, liquid B was added to the stirring vessel according to the recipe in Table 1, and liquids A and B were mixed by stirring at room temperature for 3 minutes. Then, the hill-like property of the mixture of liquids A and B was evaluated.

[0116] More specifically, 100 g of the mixture was placed in a 100 mL container and the temperature was adjusted in a thermostatic water bath at 25° C. Next, 80 g of the mixture was evenly coated on a polypropylene plate of A4 size (210 mm×297 mm). After that, a hand roller (embossing roller) was made to reciprocate once on the coated mixture to give an uneven shape to the surface of the mixture.

[0117] The mixture was then cured for 7 days at 23° C. and 50% relative humidity, and then aged for 2 days at 23° C. and 50% relative humidity, to obtain a cured product.

[0118] The surface irregularities of the cured product were visually evaluated. The results are shown in the table. The evaluation criteria are as follows.

[0119] ○: The uneven shape had a large difference in height and a sharp peak. Δ: The unevenness was moderate in height, and the apex was slightly pointed. ×: The height difference of the uneven shape was small and the apex was not sharp.

[0120] FIG. 1 is a photograph showing the cured product of Comparative Example 1 (peak shape x), the cured product of Example 2 (peak shape ◯), and the cured product of Example 1 (peak shape Δ).

[0121] [Table 1]

Claims

1. Contains a polyisocyanate component and an active hydrogen group-containing component, The polyisocyanate component contains an isocyanate group-terminated prepolymer, The active hydrogen group-containing component is Contains diethyltoluene polyamine and polyoxyalkylene polyamine, A polyurethane resin composition, comprising: a diethyltoluenepolyamine-derived amino group content exceeding 6 moles per mole of the polyoxyalkylenepolyamine-derived amino group;

2. 2. The polyurethane resin composition according to claim 1, wherein the content of the amino groups derived from diethyltoluenepolyamine is from 9 mol to 40 mol per 1 mol of the amino groups derived from polyoxyalkylenepolyamine.

3. The isocyanate-terminated prepolymer contains a reaction product of a raw material polyisocyanate and a raw material polyol, The polyurethane resin composition according to claim 1 , wherein the raw material polyisocyanate contains an alicyclic polyisocyanate.

4. An elastic paving material comprising a cured product of the polyurethane resin composition according to claim 1.

Citation Information

Patent Citations

  • Sprayable and castable polyurea elastomer

    JP1991131620A

  • Atomizable and flowable polyurea elastomer

    JP1991185020A

  • Reaction injection molded polyurea elastomer and manufacture thereof

    JP1992213315A

  • Production of polyoxyalkylenepolyamine and production of polyurethaneurea resin using the same

    JP1999060719A

  • Methods and compositions for attenuating noise, vibration and harshness in substrates

    JP2002518160A

Cited By

  • Elastic packaging material having heat-insulating performance and method for manufacturing the same

    KR102980291B1