Method for producing cyclic oligosaccharide-modified organopolysiloxane

The described method addresses the challenges of producing high molecular weight, soluble cyclic oligosaccharide-modified organopolysiloxanes by hydrosilylation and solvent washing, resulting in transparent, non-sticky, and flexible films for film-forming agents and coatings.

JP2024162026AActive Publication Date: 2024-11-21SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023077172
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

Existing methods for producing cyclic oligosaccharide-modified organopolysiloxanes face challenges in achieving high molecular weight solubility, poor compatibility with organopolysiloxanes, and residual unreacted cyclic oligosaccharides leading to stickiness and limited applications in film-forming agents and coating materials.

Method used

A method involving hydrosilylation of a composition containing high molecular weight organohydrogenpolysiloxane, cyclic oligosaccharide derivatives, and a hydrosilylation catalyst, followed by washing with organic solvents having a dielectric constant of 23 or more to remove unreacted cyclic oligosaccharides, resulting in a transparent, non-sticky, and flexible film-forming agent.

Benefits of technology

The method enables the production of high molecular weight, transparent, and flexible cyclic oligosaccharide-modified organopolysiloxanes suitable for film-forming agents and coating materials by effectively removing unreacted cyclic oligosaccharides, enhancing compatibility and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162026000001
    Figure 2024162026000001
  • Figure 2024162026000002
    Figure 2024162026000002
  • Figure 2024162026000003
    Figure 2024162026000003
Patent Text Reader

Abstract

To provide an efficient method for producing a non-cross-linked cyclic oligosaccharide-modified organopolysiloxane soluble in solvents despite its high molecular weight, by removing unreacted cyclic oligosaccharides.SOLUTION: A method for producing a cyclic oligosaccharide-modified organopolysiloxane comprises the following steps: [Step 1] obtaining an oligosaccharide-modified organopolysiloxane by hydrosilylation of a composition containing (A) to (D) in the following, namely, (A) an organohydrogen polysiloxane having one or more hydrosilyl groups per molecule having a kinematic viscosity of 50 mm2 / s or more at 25°C and a number average molecular weight of 8,000 or more, (B) a cyclic oligosaccharide derivative having an unsaturated group represented by the specified general formula (1), (C) a hydrosilylation catalyst, and (D) an organic solvent; [Step 2] cleaning and filtering the cyclic oligosaccharide-modified organopolysiloxane obtained in the Step 1 with a cleaning organic solvent having a relative permittivity of 23 or more at 25°C or a mixture of such solvents; and [Step 3] removing the organic solvents used in the Steps 1 and 2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a cyclic oligosaccharide-modified organopolysiloxane. [Background technology]

[0002] Organopolysiloxanes can have a variety of functions by modifying the terminals or side chains with various chemical structures. On the other hand, cyclic oligosaccharides are known to have voids in their molecular structure that interact with various compounds. Taking advantage of this characteristic, they are used in industrial fields such as food and cosmetics, and their introduction into various polymeric materials is being considered to develop functional materials. In fact, the introduction of cyclic oligosaccharides into organopolysiloxanes has been considered, and a gel material crosslinked with a cyclic oligosaccharide derivative has been disclosed (Patent Document 1).

[0003] However, because the above-mentioned cyclic oligosaccharide-modified organopolysiloxane is a crosslinked product, it is poorly soluble in solvents although it swells in them, and so there are limitations to its application as a film-forming agent or coating material.

[0004] Patent Document 2 and Non-Patent Document 1 disclose methods for producing non-crosslinked cyclic oligosaccharide-modified organopolysiloxanes using derivatives in which only one hydroxyl group of a cyclic oligosaccharide is modified with a reactive functional group.

[0005] However, since the compatibility between cyclic oligosaccharides and organopolysiloxanes is generally poor, addition to high molecular weight organopolysiloxanes has not been fully investigated. In fact, the number average molecular weight of the organopolysiloxanes used in Patent Document 2 and Non-Patent Document 1 is relatively low, about 1,000 to 7,500.

[0006] In addition, when considering application to a film-forming agent or a coating material, the presence of unreacted cyclic oligosaccharide derivatives can cause problems such as stickiness of the film surface. Examples of unreacted cyclic oligosaccharide derivatives include cyclic oligosaccharide derivatives that do not have a reactive functional group contained in the raw material and cyclic oligosaccharide derivatives that have an unreacted reactive functional group.

[0007] The manufacturing example of Patent Document 2 discloses a purification method in which a cyclic oligosaccharide-modified organopolysiloxane is dissolved in isododecane and the poorly soluble unreacted cyclic oligosaccharide derivative is removed by extraction with ethyl acetate. However, when the number average molecular weight of the organopolysiloxane is 8,000 or more, it is difficult to increase the purity of the cyclic oligosaccharide-modified organopolysiloxane by this method.

[0008] Non-Patent Document 1 discloses a purification method for removing unreacted cyclic oligosaccharide derivatives by silica gel column chromatography. However, this method is not efficient enough for industrial scale application. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Special Publication No. 2022-503533 [Patent Document 2] International Publication No. 2021 / 172468 [Non-patent literature]

[0010] [Non-Patent Document 1] Ahlem Noomen et al., Emulsions of β-cyclodextrins grafted to silicone for the transport of antifungal drugs,Materials Science and Engineering C,2008,28,p.705-715 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an efficient method for removing unreacted cyclic oligosaccharides when producing a non-crosslinked cyclic oligosaccharide-modified organopolysiloxane that is soluble in a solvent while having a high molecular weight. [Means for solving the problem]

[0012] In order to achieve the above object, the present invention provides the following method for producing a cyclic oligosaccharide-modified organopolysiloxane.

[0013] That is, the present invention provides a method for producing an oligosaccharide-modified organopolysiloxane by hydrosilylation of a composition comprising the following components (A) to (D): (A) The kinetic viscosity at 25°C is 50mm 2 / s or more and a number average molecular weight of 8,000 or more, and has one or more hydrosilyl groups per molecule. (B) A cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula (1): (C) Hydrosilylation catalyst (D) Organic Solvent [Step 2] A step of washing and filtering the cyclic oligosaccharide-modified organopolysiloxane obtained in step 1 with a washing organic solvent having a relative dielectric constant of 23 or more at 25°C or a mixture thereof. [Step 3] A step of removing the organic solvent used in steps 1 and 2 The present invention provides a method for producing a cyclic oligosaccharide-modified organopolysiloxane, comprising the steps of: [ka] (In the formula, A is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkylene group having 1 to 4 carbon atoms, R 3are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1.

[0014] According to the production method of the present invention, after adding a high molecular weight organopolysiloxane and a cyclic oligosaccharide by a hydrosilylation reaction, the unreacted cyclic oligosaccharide can be efficiently removed by washing with a cleaning organic solvent having a relative dielectric constant of 23 or more at 25° C. By removing the unreacted cyclic oligosaccharide, a transparent, non-sticky, flexible and tough film can be obtained, which is useful as a film-forming agent or coating material.

[0015] In this case, in the step 1, it is preferable to further carry out an addition reaction by hydrosilylation of an α-olefin having 2 to 16 carbon atoms after the hydrosilylation reaction of the (A) and (B). Such cyclic oligosaccharide-modified organopolysiloxanes have increased compatibility with cyclic oligosaccharides.

[0016] In addition, in the general formula (1), R 1 is a methyl group, R 3 is preferably an acetyl group.

[0017] It is even more preferable that the method is a method for producing a cyclic oligosaccharide-modified organopolysiloxane in which x is 1 in the general formula (1). In this way, the effects of the present invention can be more reliably achieved.

[0018] The method for producing the cyclic oligosaccharide-modified organopolysiloxane is preferably one having a glass transition temperature of 50 to 100° C. as measured by dynamic viscoelasticity measurement.

[0019] This method makes it possible to obtain a cyclic oligosaccharide-modified organopolysiloxane that has sufficient mechanical properties and the ability to form a flexible film at room temperature.

[0020] It is further preferred that the method for producing the cyclic oligosaccharide-modified organopolysiloxane is such that the organic solvent for washing in the step 2 is at least one selected from methanol, ethanol, and acetonitrile. Washing with such a solvent can more reliably and efficiently remove unreacted cyclic oligosaccharides. Effect of the Invention

[0021] According to the production method of the present invention, after adding a high molecular weight organopolysiloxane and a cyclic oligosaccharide by a hydrosilylation reaction, the unreacted cyclic oligosaccharide can be efficiently removed by washing with a washing organic solvent having a relative dielectric constant of 23 or more at 25° C. By removing the unreacted cyclic oligosaccharide, a coating can be obtained that is transparent, non-sticky, flexible and tough, despite its high molecular weight, and is useful as a coating agent or coating material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below, but the present invention is not limited thereto.

[0023] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, they discovered that unreacted cyclic oligosaccharides can be efficiently removed by washing with methanol, ethanol, acetonitrile, or a mixture thereof after addition of a high molecular weight organopolysiloxane and a cyclic oligosaccharide by a hydrosilylation reaction, and thus completed the present invention.

[0024] That is, the present invention provides, in [Step 1], a composition comprising the following (A) to (D) by hydrosilylation to produce an oligosaccharide-modified organopolysiloxane having a kinetic viscosity of 50 mm at 25°C: 2 / s or more and a number average molecular weight of 8,000 or more, and has one or more hydrosilyl groups per molecule. (B) A cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula (1): (C) Hydrosilylation catalyst (D) Organic Solvent [Step 2] A step of washing and filtering the cyclic oligosaccharide-modified organopolysiloxane obtained in step 1 with a washing organic solvent having a relative dielectric constant of 23 or more at 25°C or a mixture thereof. [Step 3] A step of removing the organic solvent used in steps 1 and 2 The present invention relates to a method for producing a cyclic oligosaccharide-modified organopolysiloxane, the method comprising the steps of: [ka] (In the formula, A is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkylene group having 1 to 4 carbon atoms, R 3 are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1.

[0025] [Process 1] Step 1 in the production method of the present invention is a step of obtaining an oligosaccharide-modified organopolysiloxane by hydrosilylation of a composition containing the following (A) to (D): (A) The kinetic viscosity at 25°C is 50mm 2 / s or more and a number average molecular weight of 8,000 or more, and has one or more hydrosilyl groups per molecule. (B) Cyclic oligosaccharide derivative having an unsaturated group represented by the above general formula (1) (C) Hydrosilylation catalyst (D) Organic Solvent Each component of the composition will now be described in detail.

[0026] [(A) Organohydrogenpolysiloxane] In the above (A), the kinetic viscosity at 25°C is 50mm 2 / s or more, and from the viewpoint of ease of handling, 50 to 25,000 mm 2 / s is preferably 50 to 10,000 mm 2 In the present invention, the kinematic viscosity is a value at 25° C. measured using a Cannon-Fenske viscometer described in JIS Z8803:2011.

[0027] The number of hydrosilyl groups contained in one molecule of the organohydrogenpolysiloxane is 1 or more, and from the viewpoint of the physical properties of the resulting film, it is preferably 1 to 40, and more preferably 1 to 20. Furthermore, the number average molecular weight is 8,000 or more, and from the viewpoint of ease of handling, it is preferably 8,000 to 50,000, and more preferably 8,000 to 35,000. In the present invention, the number average molecular weight is a value obtained by GPC (gel permeation chromatography) analysis using polystyrene as a standard substance under the following conditions.

[0028] [Measurement conditions] Developing solvent: toluene Flow rate: 0.6mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-H TSKgel SuperH5000(6.0mmI.D.×15cm×1) TSKgel SuperH4000(6.0mmI.D.×15cm×1) TSKgel SuperH3000(6.0mmI.D.×15cm×1) TSKgel SuperH2000(6.0mmI.D.×15cm×1) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 50 μL (toluene solution with a concentration of 0.3% by mass)

[0029] [(B) Cyclic oligosaccharide derivatives] The cyclic oligosaccharide derivative (B) used in the present invention is represented by the above general formula (1). In the above formula (1) of (B), A is an alkenyl group having 2 to 12 carbon atoms, preferably an alkenyl group having 2 to 4 carbon atoms from the viewpoint of procurement of synthetic raw materials, and more preferably a vinyl group. 1 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. From the viewpoint of procurement of synthetic raw materials, a methyl group or an ethyl group is preferable, and a methyl group is more preferable. 2 R is an alkylene group having 1 to 4 carbon atoms, and from the viewpoint of procurement of synthetic raw materials, an alkylene group having 2 to 3 carbon atoms is preferable, and a propylene group is more preferable. 3 are independently selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, with an acyl group having 1 to 4 carbon atoms being preferred from the viewpoint of reaction conditions, and an acetyl group being more preferred. a is an integer from 0 to 8, and from the viewpoint of procurement of synthesis raw materials, is preferably 0 to 2, and more preferably 0. b is an integer from 5 to 7. x is 0 or 1, and x is preferably 1 in order to provide excellent compatibility with the component (A). The amount of the (B) component is preferably such that the amount of the alkenyl group in the (B) component is 0.01 to 5 moles per mole of the hydrosilyl group in the (A) component. It is more preferably 0.5 to 3 moles, and even more preferably 0.8 to 1.2 moles. If it is within this range, the reaction proceeds smoothly, which is preferable.

[0030] [(C) Hydrosilylation catalyst] The hydrosilylation catalyst (C) used in the present invention is intended to promote the hydrosilylation reaction between the hydrosilyl groups in the component (A) and the alkenyl groups in the component (B). The hydrosilylation catalyst (C) is preferably a platinum catalyst or a rhodium catalyst. Specifically, catalysts such as chloroplatinic acid, alcohol-modified chloroplatinic acid, and chloroplatinic acid-vinylsiloxane complexes are preferably used. The amount of catalyst used can be a catalytic amount, but the amount of platinum or rhodium is preferably 100 ppm or less, and particularly preferably 50 ppm or less, based on the total amount of components (A) to (D). Within this range, the appearance of the cyclic oligosaccharide-modified organopolysiloxane is not colored, which is preferable.

[0031] [(D) Organic solvent] The organic solvent (D) used in the present invention serves to uniformly dissolve the components (A) to (C) and promote the reaction, as well as to reduce the viscosity of the composition and increase the stirring efficiency. Examples of the organic solvent (D) include aliphatic alcohols such as methanol, ethanol, 2-propanol, and butanol; aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic hydrocarbons such as n-pentane, n-hexane, and cyclohexane; and halogenated hydrocarbons such as dichloromethane, chloroform, and carbon tetrachloride. The component (D) is preferably compatible with the components (A) and (B), and among these, toluene is preferred from the viewpoint of compatibility with the raw materials. The blend amount of the component (D) is preferably from 10 to 90 mass %, and more preferably from 30 to 70 mass %, based on the combined blend amounts of the components (A) to (D).

[0032] The hydrosilylation reaction conditions are not particularly limited, but it is preferable to carry out the reaction at 70 to 110° C. for 1 to 10 hours. After completing step 1, before proceeding to the next step, step 2, the organic solvent of component (D) may be removed before proceeding to step 2. The internal pressure during removal of component (D) may be normal pressure or reduced pressure. The temperature is not particularly limited, but is preferably 20°C to 100°C.

[0033] The method for producing the cyclic oligosaccharide-modified organopolysiloxane of the present invention can further include a step of adding an α-olefin having 2 to 16 carbon atoms after the above hydrosilylation reaction. From the viewpoint of compatibility with the cyclic oligosaccharide-modified organopolysiloxane obtained above, the α-olefin having 2 to 16 carbon atoms is preferably an alkyl group having 5 to 12 carbon atoms, more preferably an alkyl group having 6 to 8 carbon atoms, and even more preferably an octyl group. It is preferable that the amount of alkenyl groups in the cyclic oligosaccharide derivative (B) is 0.02 to 1.2 moles and the amount of alkenyl groups in the α-olefin is 0.02 to 1.98 moles per mole of hydrosilyl groups in the organohydrogenpolysiloxane (A). However, it is preferable that the total amount of the components (B) and the α-olefin is in the range of 0.8 to 2.0 moles per mole of hydrosilyl groups in the organohydrogenpolysiloxane (A).

[0034] [Process 2] Step 2 in the production method of the present invention is a step of washing and filtering the cyclic oligosaccharide-modified organopolysiloxane obtained in step 1 with a washing organic solvent having a relative dielectric constant of 23 or more at 25° C. or a mixture thereof. The dielectric constant of an organic solvent is known as an index of the polarity of the solvent. By using an organic solvent for washing having a dielectric constant of 23 or more at 25°C, only the unreacted component (B) can be dissolved, and the target cyclic oligosaccharide-modified organopolysiloxane can be recovered by filtration. The dielectric constant of the organic solvent for washing is characterized by being 23 or more, preferably 23 to 50, and more preferably 23 to 40. In the present invention, the values ​​described in the revised 5th edition of the Basic Handbook of Chemistry (edited by the Chemical Society of Japan, published in 2004) are cited as the dielectric constant at 25°C. Examples of organic solvents for cleaning with a dielectric constant of 23 or more at 25°C include methanol (32.66), ethanol (24.55), ethylene glycol (37.7), propylene glycol (32.0), N,N-dimethylformamide (36.71), N,N-dimethylacetamide (37.78), and acetonitrile (35.94) (the values ​​in parentheses indicate the dielectric constant). Among these, methanol, ethanol, and acetonitrile are preferably used. These organic solvents may be used alone or in combination of two or more. When a mixture is used, the weighted average dielectric constant of the mixture is regarded as the dielectric constant of the mixture. The temperature during dissolution is not particularly limited as long as it is equal to or lower than the boiling point of the solvent, but is preferably 20° C. to 70° C. In addition, since high transparency is required when used as a film-forming agent, the amount of the remaining component (B) in the obtained cyclic oligosaccharide-modified organopolysiloxane is preferably 10% or less, more preferably 5% or less, and even more preferably 1% or less. It has become clear from the present invention that the remaining component (B) leads to stickiness of the film and a decrease in mechanical properties.

[0035] [Process 3] Step 3 in the production method of the present invention is a step of removing the organic solvent used in steps 1 and 2. In step 3, the internal pressure during removal of the organic solvent may be normal pressure or reduced pressure. The temperature is not particularly limited, but is preferably 20°C to 100°C.

[0036] The glass transition temperature of the cyclic oligosaccharide-modified organopolysiloxane obtained by the method of the present invention is preferably 50 to 100° C., and from the viewpoint of the properties of the film formed, is more preferably 60 to 95° C., and even more preferably 65 to 90° C. If it is within the above range, a flexible film is formed while having sufficient mechanical properties at room temperature. The glass transition temperature in the present invention is a value determined by dynamic viscoelasticity measurement under the conditions shown in the examples described later.

[0037] [Film-forming agent] The cyclic oligosaccharide-modified organopolysiloxane obtained by the method of the present invention can be used as a film-forming agent because it is highly transparent, flexible, non-sticky, and forms a tough film.

[0038] As the film-forming agent, the above-mentioned cyclic oligosaccharide-modified organopolysiloxane can be used alone, but from the viewpoints of film-forming properties and workability, it is preferable to use it after diluting it with an organic solvent.

[0039] The organic solvent is selected from volatile siloxanes, saturated aliphatic hydrocarbons, saturated alicyclic hydrocarbons, aromatic hydrocarbons, chlorinated hydrocarbons, chlorofluorohydrocarbons, alcohols, etc. Particularly preferred are volatile organosiloxanes and light liquid isoparaffins having a boiling point of 100 to 270°C at normal pressure (1013hPa). Examples of volatile siloxanes include cyclic siloxanes such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, trimethyltriethylcyclotrisiloxane, hexaethyltricyclosiloxane, diethyltetramethylcyclotrisiloxane, dimethyltetraethylcyclotrisiloxane, diethylhexamethylcyclotetrasiloxane, and tetraethyltetramethylcyclotetrasiloxane; linear siloxanes such as hexamethyldisiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, dodecamethylpentasiloxane, hexaethyldisiloxane, and octaethyltrisiloxane; and branched siloxanes such as methyltris(trimethylsiloxy)silane and phenyltris(trimethylsiloxy)silane. Moreover, the light liquid isoparaffin is exemplified by those containing isoparaffin having 8 to 16 carbon atoms as a main component.

[0040] When an organic solvent is used, the amount of the cyclic oligosaccharide-modified organopolysiloxane is preferably 0.1 to 80%, and more preferably 0.5 to 20%.

[0041] As the coating method, a known method can be adopted depending on the type of substrate to be coated.

[0042] Applications of the cyclic oligosaccharide-modified organopolysiloxane film-forming agent obtained by the method of the present invention include damage protection agents, water repellents, and stripping agents for cosmetics, paints, paper, plastic sheets, and rubber articles, damage protection agents, water repellents, waterproofing agents, texture improving agents, filling agents for fabrics, water repellents, waterproofing agents, and stripping agents for concrete, mortar, and wood, and it can be used for the purpose of imparting cosmetic durability, slipperiness, water repellency, etc. EXAMPLES

[0043] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.

[0044] [Measurement method] Various measurements were carried out by the following methods.

[0045] <Glass transition temperature> The glass transition temperature is obtained by creating a film 0.25 mm thick and analyzing the dynamic viscoelasticity data measured using a Hitachi High-Tech Science "DMA7100" in tensile mode at a frequency of 1 Hz in the range of 25 to 120°C at a heating rate of 5°C / min. The temperature at which tan δ (loss tangent), expressed as E'' (loss modulus) / E' (storage modulus), is maximized is identified, and this temperature is taken as the glass transition temperature.

[0046] < 1 H-NMR> The measurements were performed using an AVANCE-III 400 MHz (manufactured by BRUKER) and deuterated chloroform as the measurement solvent.

[0047] [Synthesis Example 1: Synthesis of cyclic oligosaccharide derivatives with unsaturated bonds] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 50.0 g of mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin (C6-Ts-β-CD) and 500.0 g of allylamine were charged. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 53°C for 7 hours, cooled to room temperature, and stirred overnight. The mixture was concentrated using an evaporator, 1,000 mL of acetonitrile was added to the resulting solid, and the precipitate was collected by filtration. 1,000 mL of distilled water was added to the resulting precipitate to dissolve it, and the solution was dropped into 1,000 mL of acetonitrile, and the precipitate was collected by filtration. The precipitate was washed with acetone and then dried in a vacuum dryer at 40°C to obtain vinyl-modified compound A (white solid, 42.7 g).

[0048] [ka]

[0049] [Synthesis Example 2: Synthesis of cyclic oligosaccharide derivatives with unsaturated bonds] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 30.0 g of the vinyl-modified compound A, 110.0 g of acetic anhydride, and 170.0 g of pyridine were charged. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 60°C for 7 hours, cooled to room temperature, and stirred overnight. 170 mL of toluene was added to the solution in the flask, washed twice with 170 mL of 1 mM hydrochloric acid and once with 170 mL of saturated saline, and the solution obtained by liquid separation was concentrated with an evaporator. The collected solid was then dissolved in 50 mL of acetone, and the solution was dropped into 500 mL of distilled water, and the precipitate was collected by filtration. The precipitate was dried in a vacuum dryer at 40°C to obtain vinyl-modified compound B (white solid, 31.8 g).

[0050] [ka]

[0051] [Synthesis Example 3: Synthesis of cyclic oligosaccharide derivatives with unsaturated bonds] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 48.0 g of mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin (C6-Ts-β-CD), 300.0 g of 1-vinyl, 3-(3-aminopropyl)tetramethyldisiloxane, and 60.0 g of N,N-dimethylformamide were charged. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 75°C for 7 hours, cooled to room temperature, and stirred overnight. The solution in the flask was dropped into 1,200 mL of acetonitrile, and the precipitate was collected by filtration. 60.0 g of N,N-dimethylformamide was added to the obtained precipitate to dissolve it, and the solution was dropped into 1,200 mL of toluene, and the precipitate was collected by filtration. The precipitate was washed with acetone and then dried in a vacuum dryer at 40°C to obtain vinyl-modified compound C (white solid, 42.5 g).

[0052] [ka]

[0053] [Synthesis Example 4: Synthesis of cyclic oligosaccharide derivatives having unsaturated bonds] A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel was charged with 42.0 g of the vinyl-modified compound C, 134.4 g of acetic anhydride, and 210.0 g of pyridine. After replacing the atmosphere in the flask with nitrogen, the mixture was stirred at 60°C for 7 hours, cooled to room temperature, and stirred overnight. 210 mL of toluene was added to the solution in the flask, washed twice with 210 mL of 1 mM hydrochloric acid and once with 210 mL of saturated saline, and the solution obtained by liquid separation was concentrated with an evaporator. The collected solid was then dissolved in 150 mL of toluene, and the solution was dropped into 300 mL of hexane, and the precipitate was collected by filtration. The precipitate was dried in a vacuum dryer at 40°C to obtain a vinyl-modified compound D (white solid, 50.1 g).

[0054] [ka]

[0055] [Example 1] Into a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 100.0 g of a polyorganohydrogensiloxane represented by the following formula (2) (kinetic viscosity: 3,340 mm 2 The flask was charged with 24.9 g of the vinyl-modified compound B (vinyl group amount: 0.012 mol) (1.0 g / s, number average molecular weight: 31,100, hydrosilyl group amount: 0.040 mol), 24.9 g of the vinyl-modified compound B (vinyl group amount: 0.012 mol), and 200.0 g of toluene. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.3 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask and stirred at 90°C for 4 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 6.4 g (0.057 mol) of 1-octene and 0.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. 250 g of methanol was added to the obtained solid, and the process of washing the solid at 50 ° C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane E (light brown solid, 119.7 g).

[0056] [ka]

[0057] [Example 2] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 128.3 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.052 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 256.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours.1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 8.2 g (0.073 mol) of 1-octene and 0.9 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. 300 g of methanol was added to the obtained solid, and the process of washing the solid at 50 ° C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane F (light brown solid, 148.3 g).

[0058] [ka]

[0059] [Example 3] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 128.3 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.052 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 256.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 8.2 g (0.073 mol) of 1-octene and 0.9 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. 300 g of ethanol was added to the obtained solid, and the process of washing the solid at 50 ° C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane G (light brown solid, 147.8 g).

[0060] [ka]

[0061] [Example 4] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 128.3 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.052 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 256.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 8.2 g (0.073 mol) of 1-octene and 0.9 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. 300 g of acetonitrile was added to the obtained solid, and the process of washing the solid at 50 ° C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane H (light brown solid, 148.0 g).

[0062] [ka]

[0063] [Example 5] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 77.0 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.031 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 154.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.1 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 3.5 g (0.031 mol) of 1-octene and 0.6 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. 240 g of methanol was added to the obtained solid, and the process of washing the solid at 50 ° C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane I (light brown solid, 113.3 g).

[0064] [ka]

[0065] [Example 6] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 35.0 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.014 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 70.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 0.6 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. The reaction solution was then cooled to room temperature, and the toluene was removed under reduced pressure using an evaporator. 140 g of methanol was added to the resulting solid, and the process of washing the solid at 50°C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40°C to obtain cyclic oligosaccharide-modified organopolysiloxane J (light brown solid, 64.3 g).

[0066] [ka]

[0067] [Comparative Example 1] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 128.3 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.052 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 256.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 8.2 g (0.073 mol) of 1-octene and 0.9 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. Finally, the mixture was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane K (light brown solid, 159.7 g).

[0068] [ka]

[0069] [Comparative Example 2] Into a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 6.9 g of a polyorganohydrogensiloxane represented by the following formula (3) (kinetic viscosity: 17 mm 2 The flask was charged with 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), 100.0 g of toluene, and 100.0 g of toluene. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 0.6 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 8.2 g (0.073 mol) of 1-octene and 0.3 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. 100 g of methanol was added to the obtained solid, and the process of washing the solid at 50 ° C was repeated three times. Finally, the solid was dried in a vacuum dryer at 40 ° C to obtain cyclic oligosaccharide-modified organopolysiloxane L (light brown solid, 44.6 g).

[0070] [ka]

[0071] [Comparative Example 3] In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, 128.3 g of polyorganohydrogensiloxane represented by the following formula (2) (hydrosilyl group amount: 0.052 mol), 45.0 g of the vinyl-modified compound D (vinyl group amount: 0.016 mol), and 256.0 g of toluene were charged. After replacing the atmosphere in the flask with nitrogen, the temperature was raised to 90°C, and 1.7 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) was added to the flask, and the mixture was stirred at 90°C for 2 hours. 1 The progress of the reaction was confirmed by the disappearance of the vinyl group peak (5.6-6.1 ppm) by H-NMR. Then, 8.2 g (0.073 mol) of 1-octene and 0.9 g of a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (platinum concentration 0.5 wt%) were added to the flask and stirred at 90 ° C for 4 hours. Then, the reaction solution was cooled to room temperature, and toluene was distilled off under reduced pressure using an evaporator. When 300 g of acetone (relative dielectric constant 20.7) was added to the obtained solid and heated to 50 ° C, the product also dissolved, so the evaluation was discontinued without proceeding to the subsequent process. Films were prepared from the compounds obtained in the above Examples and Comparative Examples by the following methods, and various evaluations were carried out.

[0072] [Film Creation] The various cyclic oligosaccharide-modified organopolysiloxanes obtained in the above synthesis examples, examples, and comparative examples were dissolved in toluene to prepare a 30% solution. The above solution was poured onto a Teflon (registered trademark) coated plate with a pattern of 5 cm length x 5 cm width x 0.25 mm thickness, and left overnight at 25°C, and then dried in a dryer at 80°C for 1 hour to produce a film. The appearance of the obtained film was visually observed, and the presence or absence of stickiness was examined by touching with the hand. In addition, dynamic viscoelasticity was measured to identify the glass transition temperature.

[0073] [Table 1] From the results in Table 1, it was found that the cyclic oligosaccharide-modified organopolysiloxane obtained by the manufacturing method of the present invention can form a transparent, non-sticky, flexible and tough coating. On the other hand, the product of Comparative Example 1, in which step 2 was omitted, was cloudy and sticky. Moreover, the product of Comparative Example 2 had a low molecular weight and lacked flexibility and toughness.

[0074] The present specification includes the following aspects. [1]: [Step 1] A step of obtaining an oligosaccharide-modified organopolysiloxane by hydrosilylation of a composition containing the following (A) to (D): (A) The kinetic viscosity at 25°C is 50mm 2 / s or more and a number average molecular weight of 8,000 or more, and has one or more hydrosilyl groups per molecule. (B) A cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula (1): (C) Hydrosilylation catalyst (D) Organic Solvent [Step 2] A step of washing and filtering the cyclic oligosaccharide-modified organopolysiloxane obtained in step 1 with a washing organic solvent having a relative dielectric constant of 23 or more at 25°C or a mixture thereof. [Step 3] A step of removing the organic solvent used in steps 1 and 2 A method for producing a cyclic oligosaccharide-modified organopolysiloxane, comprising: [ka] (In the formula, A is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkylene group having 1 to 4 carbon atoms, R 3are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1. [2]: A method for producing a cyclic oligosaccharide-modified organopolysiloxane according to [1], characterized in that in step 1, after the hydrosilylation reactions of (A) and (B), an α-olefin having 2 to 16 carbon atoms is further added by hydrosilylation. [3] In the general formula (1), R 1 is a methyl group, R 3 The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to [1] or [2], wherein is an acetyl group. [4]: The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to any one of [1] to [3], wherein, in the general formula (1), x is 1. [5]: The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to any one of [1] to [4], wherein the cyclic oligosaccharide-modified organopolysiloxane has a glass transition temperature of 50 to 100°C as measured by dynamic viscoelasticity measurement. [6]: The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to any one of [1] to [5], wherein the organic solvent for washing used in step 2 is one or more selected from methanol, ethanol, and acetonitrile.

[0075] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. [Step 1] A step of obtaining an oligosaccharide-modified organopolysiloxane by hydrosilylation of a composition containing the following (A) to (D): (A) Kinematic viscosity at 25 ° C. is 50 mm 2 / s or more and a number average molecular weight of 8,000 or more, and having one or more hydrosilyl groups per molecule. (B) A cyclic oligosaccharide derivative having an unsaturated group represented by the following general formula (1): (C) Hydrosilylation catalyst (D) Organic Solvent [Step 2] A step of washing and filtering the cyclic oligosaccharide-modified organopolysiloxane obtained in Step 1 with a washing organic solvent having a relative dielectric constant of 23 or more at 25°C or a mixture thereof. [Step 3] A step of removing the organic solvent used in Steps 1 and 2 A method for producing a cyclic oligosaccharide-modified organopolysiloxane, comprising: 【Chemical 1】 (Wherein A is an alkenyl group having 2 to 12 carbon atoms, R 1 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkylene group having 1 to 4 carbon atoms, R 3 are independently a group selected from an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, a is an integer of 0 to 8, b is an integer of 5 to 7, and x is 0 or 1.

2. The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to claim 1, characterized in that in step 1, after the hydrosilylation reaction of (A) and (B), an α-olefin having 2 to 16 carbon atoms is further added by hydrosilylation.

3. In the general formula (1), R 1 is a methyl group, R 3 The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to claim 1, wherein is an acetyl group.

4. 2. The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to claim 1, wherein x is 1 in the general formula (1).

5. 2. The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to claim 1, wherein the cyclic oligosaccharide-modified organopolysiloxane has a glass transition temperature of 50 to 100°C as measured by dynamic viscoelasticity measurement.

6. 2. The method for producing a cyclic oligosaccharide-modified organopolysiloxane according to claim 1, wherein the organic solvent used for washing in step 2 is at least one selected from the group consisting of methanol, ethanol, and acetonitrile.

Citation Information

Patent Citations

  • Cyclodextrin derivative and its preparation

    JP1995252303A

  • Organopolysiloxane modified cyclodextrin compound and its manufacturing method, as well as cosmetic material containing the same

    JP2023000461A

  • Resin material including siloxane-bond-containing polymer having host group and / or guest group

    WO2021172468A1

  • Composition containing siloxane bond-containing polymer compound that has host group and / or guest group

    WO2024232289A1

  • Cyclic oligosaccharide-modified organopolysiloxane and film-forming agent

    WO2024232321A1