Flame-retardant floor sheet
The flame-retardant floor sheet, made of vinyl chloride resin with balanced plasticizer, antimony trioxide, and inorganic filler, addresses adhesion issues on uneven subfloors, ensuring flexibility and concealment, thus improving workability and appearance.
Patent Information
- Application Number
- JP2023077320
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
AI Technical Summary
Floor sheets with low flexibility do not adhere well to uneven subfloors, peel off over time, and rise at steps due to initial adhesive force, leading to poor adhesion and partial peeling.
A flame-retardant floor sheet composed of vinyl chloride resin with specific ratios of plasticizer, antimony trioxide, and inorganic filler, along with a backing layer, to enhance flexibility, adhesion, and concealment, while maintaining flame retardancy.
The floor sheet improves followability to the subfloor, enhances workability, and provides a beautiful finish by hiding the subfloor's hue and pattern, with improved strength and flexibility.
Smart Images

Figure 2024162103000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame-retardant floor sheet to be laid on the underfloor surface of buildings, vehicles, etc. Such floor sheets are preferably used, for example, for open corridors and verandas in buildings, and for passenger compartment floors in trains and buses. [Background technology]
[0002] For example, Patent Document 1 (JP 2013-067163 A) discloses a vehicle floor sheet comprising a floor sheet body made of flame-retardant rubber formed into a long sheet, and an adhesive layer made of an acrylic adhesive laminated to a thickness of 50 μm or more and less than 500 μm on the back side of the floor sheet body. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-067163 A Summary of the Invention [Problem to be solved by the invention]
[0004] When laying a floor sheet, adhesive is applied to the floor base, the floor sheet is placed on top of it, and the floor sheet is pressed against the floor base. At this time, floor sheets with low flexibility may not adhere well in some places due to unevenness of the floor base, and may peel off over time or due to stress caused by people walking. Also, if there is a step on the floor base, the floor sheet may rise up against the initial adhesive force, resulting in poor adhesion, and the floor sheet may also peel off in parts.
[0005] Therefore, the object of the present invention is to provide a floor sheet that has appropriate flexibility while retaining flame retardancy and is easy to install when laying the floor sheet on a floor substrate, that is, a floor sheet that can achieve both flame retardancy and flexibility. [Means for solving the problem]
[0006] In order to solve the above problems, the flame-retardant floor sheet of the present invention is: A flame-retardant floor sheet whose main resin component is polyvinyl chloride resin, containing 40 parts by mass to 75 parts by mass of a plasticizer and 1 part by mass to 8 parts by mass of antimony trioxide relative to 100 parts by mass of vinyl chloride resin; It is characterized by:
[0007] The flame-retardant floor sheet of the present invention having such a structure can improve the flame retardancy and flexibility of the floor sheet, thereby improving the conformability to the floor base when the floor sheet is laid on the floor base, and improving the workability.
[0008] In the flame-retardant floor sheet of the present invention, Further containing 10 parts by mass to 160 parts by mass of an inorganic filler relative to 100 parts by mass of the vinyl chloride resin; is preferred.
[0009] According to the flame-retardant floor sheet of the present invention having such a configuration, the floor sheet has a concealing property, so that when the floor sheet is laid on the floor base, it can be finished with a beautiful appearance by concealing the hue and pattern of the floor base or the hue and pattern of the adhesive layer for attaching the floor sheet to the floor base. Also, when a backing layer is laminated on the floor sheet to form a laminate, the hue and pattern of the backing layer can be concealed.
[0010] In the flame-retardant floor sheet of the present invention, The underside of the flame-retardant floor sheet according to claim 1 or 2, A backing layer containing 250 parts by mass or less of an inorganic filler and 50 parts by mass to 70 parts by mass of a plasticizer relative to 100 parts by mass of vinyl chloride resin is laminated; is preferred.
[0011] According to the flame-retardant floor sheet of the present invention having such a configuration, in addition to the flame retardancy and flexibility of the floor sheet, the strength of the floor sheet laminate can be improved. Effect of the Invention
[0012] According to the present invention, the flame retardancy and flexibility of the floor sheet can be improved, so that the floor sheet can be improved in conformity with the base when laid on the base floor, thereby improving workability. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view showing an outline of a flame-retardant floor sheet 1 according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a flame retardant test of the flame retardant floor sheet 1. [Diagram 3] FIG. 2 is a schematic diagram of a sagging test of the flame-retardant floor sheet 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Below, a representative embodiment of the flame-retardant floor sheet according to the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to those shown in the drawings, and each drawing is intended to conceptually explain the present invention, so that the ratio of size, length, and quantity may be exaggerated or simplified as necessary for easy understanding. Furthermore, in the following description, the same or equivalent parts are given the same reference numerals, and duplicated descriptions may be omitted.
[0015] The flame-retardant floor sheet 1 includes a floor sheet body 3 formed in a long shape (see FIG. 1). The floor sheet body 3 is mainly made of vinyl chloride resin. Since vinyl chloride resin is excellent in flame retardancy and durability, is inexpensive and light in weight, it can be suitably used as the main resin component of the floor sheet body 3. In FIG. 1, the fiber sheet 7 described later is drawn to have a certain thickness, but this is a schematic representation of the laminated structure including the fiber sheet 7 and the backing layer 5. The composition components such as resin permeate the thin fiber sheet 7 with many voids during thermocompression molding, so that the fiber sheet 7 becomes almost indistinguishable in reality.
[0016] As the vinyl chloride resin, a polyvinyl chloride resin having an average degree of polymerization of 300 to 10,000 can be used. The reason for this is that if the average degree of polymerization of the vinyl chloride resin is less than 300, it may be difficult to maintain a predetermined shape or the surface tack may be excessively high. On the other hand, if the average degree of polymerization of the vinyl chloride resin is more than 10,000, it may be difficult to uniformly mix and disperse the blended components or to prepare a flame-retardant sheet with a predetermined uniform thickness. Therefore, it is more preferable to set the average degree of polymerization of the vinyl chloride resin to a value within the range of 500 to 5,000, and even more preferable to set it to a value within the range of 800 to 2,000. The average degree of polymerization of the vinyl chloride resin can be calculated from the molecular weight of the monomer and the average molecular weight converted into a standard styrene particle using a GPC device or a GC-MS device.
[0017] The floor sheet body 3 further contains a plasticizer and antimony trioxide. The plasticizer is used to impart flexibility and cushioning properties to the floor sheet main body 3. As the plasticizer, a phthalate ester plasticizer is suitable, and examples thereof include, but are not limited to, dioctyl phthalate (DOP), diisononyl phthalate (DINP), dinonyl phthalate (DNP), bisisodecyl phthalate (DIDP), diundecyl phthalate (DUP), and bis-normal-octyl phthalate (DNOP).
[0018] From the standpoint of appropriate flexibility, the floor sheet main body 3 preferably contains 40 parts by mass or more of plasticizer per 100 parts by mass of vinyl chloride resin, and more preferably contains 45 parts by mass or more of plasticizer per 100 parts by mass of vinyl chloride resin. On the other hand, an increase in the amount of plasticizer leads to a decrease in flame retardancy. Therefore, in the floor sheet main body 3, from the viewpoint of ensuring appropriate flame retardancy, it is preferable that the amount of plasticizer is 75 parts by mass or less per 100 parts by mass of vinyl chloride resin.
[0019] Antimony trioxide (Sb2O3) is used as a flame retardant. In other words, PVC resin is difficult to burn, but the plasticizer is flammable, so antimony trioxide is added as a flame retardant. Antimony trioxide can be used in the form of pellets that are hot-pressed and mixed with polyvinyl chloride resin. This is because by solidifying powdered antimony trioxide with resin, it is possible to eliminate dust and improve work efficiency, which helps improve the work environment. In addition, it is exempt from the restrictions on specific chemical substances and from the designation of hazardous substances, making it easier to store, transport, and handle. In the test examples described later, the blending amount of pellets as a flame retardant and the blending amount of antimony trioxide corresponding thereto are respectively shown.
[0020] From the viewpoint of ensuring appropriate flame retardancy, it is preferable for the floor sheet main body 3 to contain 1 to 8 parts by mass of antimony trioxide per 100 parts by mass of vinyl chloride resin, and it is even more preferable for the floor sheet main body 3 to contain 1.2 to 7.2 parts by mass of antimony trioxide per 100 parts by mass of vinyl chloride resin.
[0021] It is preferable that the floor sheet main body 3 further contains an inorganic filler. The inorganic filler is used to improve the strength of the floor sheet main body 3 and to reduce thermal expansion and contraction, or as a bulking material. Examples of inorganic fillers include, but are not limited to, calcium carbonate, talc, clay, mica, zeolite, and silica.
[0022] The floor sheet main body 3 may contain more than 0 to 160 parts by mass of inorganic filler per 100 parts by mass of vinyl chloride resin, but from the viewpoint of ensuring appropriate concealment and flame retardancy, it preferably contains 20 to 150 parts by mass of inorganic filler per 100 parts by mass of vinyl chloride resin.
[0023] The preferred range of particle size of the inorganic filler is 0.8 to 10 μm. If the average particle size of the inorganic filler is 0.8 μm or more, secondary aggregation of the inorganic filler is suppressed, and dispersibility in the resin is good, and if it is 10 μm or less, there is no hole due to drawdown during extrusion, and moldability is excellent. Note that the "average particle size" here refers to the particle size of 50% by mass in the particle size distribution measured by a particle size distribution meter.
[0024] The floor sheet main body 3 may further contain a stabilizer. Examples of the stabilizer that can be used include, but are not limited to, liquid or powder stabilizers such as barium-zinc (Ba-Zn) composite stabilizers, lead-based, epoxy-based stabilizers such as bisphenol A glycidyl ether, and calcium-zinc composite stabilizers. The stabilizer preferably contains an epoxy-based stabilizer and a barium-zinc composite stabilizer in terms of compatibility with polyvinyl chloride resin, moldability, and low toxicity.
[0025] In addition, the floor sheet main body 3 may contain various additives, such as pigments, colorants, ultraviolet absorbing agents, and infrared reflective agents, as long as such additives are not contrary to the gist of the present invention.
[0026] The flame-retardant floor sheet 1 may further have a backing layer 5 on its lower surface side. That is, the backing layer 5 is added to the floor sheet body 3, and may be called a backing layer or a backer layer.
[0027] The backing layer 5 contains an inorganic filler and a plasticizer. The inorganic filler and the plasticizer may be the same as those contained in the floor sheet main body 3, but are not limited thereto.
[0028] The backing layer 5 preferably contains more than 0 parts by mass and not more than 250 parts by mass of inorganic filler per 100 parts by mass of vinyl chloride resin, and from the viewpoint of ensuring appropriate flexibility, it is even more preferable for the backing layer 5 to contain 50 parts by mass to 250 parts by mass of inorganic filler per 100 parts by mass of vinyl chloride resin. In addition, the backing layer 5 preferably contains 50 parts by mass to 70 parts by mass of plasticizer per 100 parts by mass of vinyl chloride resin, and from the viewpoint of achieving both flame retardancy and flexibility, it is even more preferable that the backing layer 5 contains 52 parts by mass to 67 parts by mass of plasticizer per 100 parts by mass of vinyl chloride resin.
[0029] In addition, in the flame-retardant floor sheet 1, a fiber sheet 7 may be interposed as an intermediate layer between the floor sheet main body 3 and the backing layer 5. A nonwoven or woven fabric of glass fiber or resin fiber can be used as the fiber sheet 7. By using the fiber sheet 7, the tear strength of the flame-retardant floor sheet 1 is improved, and expansion and contraction of the sheet caused by environmental temperature and direct sunlight can be suppressed.
[0030] Next, a manufacturing method of the flame-retardant floor sheet 1 will be described. The flame-retardant floor sheet 1 can be made into a sheet by hot-pressing and kneading the above-mentioned materials by extrusion molding or calendar molding, but in this embodiment, the following method is preferably used.
[0031] That is, a rod-shaped body extruded by extrusion molding of a resin mixture of the various materials, or a sheet-shaped body produced by calendar molding or extrusion molding, is cut with a cutter or the like into small lumps, pellets, or flakes. These small lumps are spread on a belt conveyor to form a layer, which is then introduced into a heating furnace to heat and melt, and further pressed with rolls to form the floor sheet body 3 into a flame-retardant floor sheet 1.
[0032] To manufacture the flame-retardant floor sheet 1 in which the backing layer 5 is laminated to the floor sheet main body 3, first, small resin globules for the backing layer 5 are spread on the belt conveyor, and then the fiber sheet 7 for the intermediate layer is placed on top of them. Then, small resin globules for the floor sheet main body 3 are spread on top of the fiber sheet 7. This is followed by the same process as described above to form the flame-retardant floor sheet 1 in which the backing layer 5 is laminated to the floor sheet main body 3.
[0033] Next, a method for laying the flame-retardant floor sheet 1 on a floor subfloor will be described. The adhesive is applied to the floor substrate in a comb pattern using a comb trowel. As the adhesive, for example, a one-liquid curing urethane adhesive can be suitably used. The flame-retardant floor sheet 1 is laid on the floor base coated with an adhesive, and then the flame-retardant floor sheet 1 is pressed against the floor base using a roller or the like, thereby adhering and laying the flame-retardant floor sheet 1.
[0034] Test Example Various tests were carried out on "1. Floor sheet body 3", "2. Backing layer 5", and "3. Sheet composed of floor sheet body 3, fiber sheet 7 and backing layer 5". The test methods and results are shown below.
[0035] 1. Testing of floor sheet body 3 Floor sheet bodies 3 were prepared with different blend amounts of flame retardant (antimony trioxide), plasticizer, and inorganic filler, and tests were conducted on (1) flame retardancy, (2) flexibility, and (3) base concealment ability. The results are shown in Tables 1 to 3 below. In Tables 1 to 3, Test Nos. 1 to 6 used specimens T that differed in the amount of flame retardant (antimony trioxide), Test Nos. 7 to 10 used specimens T that differed in the amount of plasticizer, and Test Nos. 11 to 14 used specimens T that differed in the amount of inorganic filler. Polyvinyl chloride resin (average polymerization degree 1000) was used as the main resin component of the floor sheet body 3. In addition, antimony trioxide master batch MK80-D manufactured by Nihon Seiko Co., Ltd. was used as the flame retardant (this master batch contains 80 mass% antimony trioxide, 20 mass% vinyl chloride resin, and 12 mass% phthalate ester plasticizer, but these are included in the vinyl chloride resin and plasticizer columns in the composition blends in Tables 1 to 3). Calcium carbonate with an average particle size of 2.7 μm was used as the inorganic filler.
[0036] (1) Flame retardancy test Flame retardancy tests are in accordance with Taiwan Vehicle Safety Inspection Standard 19-1, Vehicle Interior Material Flame Retardancy Requirements - Section 6.5, and vertical burning rate tests.
[0037] Specifically, the evaluation will be performed under the following procedures and conditions. That is, as shown in FIG. 2, a sheet-like test specimen T having a size of 120×10 mm is suspended from an arm 72 of a testing device 71, and an alcohol lamp 76 is placed at the lower end of the test specimen T. A flame 77 with a height L1 of about 40 mm is emitted from an alcohol lamp 76, and the lower end of the test specimen T is inserted L2 of about 20 mm into the flame 77. The test specimen T is held in this state for 12 seconds. After 12 seconds have elapsed, the lamp 76 is removed from the test specimen T. Then, the time until the flame 77 from the test specimen T goes out (afterflame time) is measured. This was tested on three test specimens T (N=3). If the afterflame time was within 5 seconds for each, the test specimen T was judged to meet the standard, and otherwise was judged to be out of standard. The results of the flame retardancy test are shown in the following Tables 1 to 3 (the tables show the specimen with the longest after-flame time among the three test specimens).
[0038] (2) Flexibility test The flexibility test of the floor sheet main body 3 was carried out as follows. That is, a test piece T having dimensions of 120×10 mm in length and width and a thickness t of 0.9 to 1.1 mm is left in a room at 23° C. for 24 hours to adjust, and then the test piece T is placed on a rectangular parallelepiped test stand 81 as shown in FIG. 3. At this time, the tip of the test piece T is set to protrude L3=100 mm from the test stand 81, and the part placed on the test stand 81 is fixed with a weight 82. Then, the drooping width L4 of the test piece T is measured after 60 seconds. Here, the drooping width L4 is the distance between the outer circumferential surface of the measurement stand 81 and the tip of the test piece T, and is used as an index of the resistance of the test piece T to sagging. The sagging width amount L4 was divided by the thickness t (mm) of the test specimen T to obtain the sagging width amount X (= L4 / t) per unit thickness, which was used as an index of flexibility. If the sagging width amount X per unit thickness was 50 or less, the test specimen T was judged to meet the standard. The results of the flexibility test are shown in Tables 1 to 3 below.
[0039] (3) Concealment test The hiding power test was carried out as follows. That is, as a standard, the hue (L*, a*, b*) of only the backing layer 5 of test No. 17 was measured. In addition, the hue of test specimen T of the floor sheet main body 3 placed on this backing layer (test No. 17) was measured. The hiding power of test specimen T was evaluated by comparing these hues.
[0040] The conditions for measuring the hue are as follows: Spectrophotometer: Konica Minolta Japan Inc. spectrophotometer CM-3600A Optical system: d / 8 (diffuse illumination, 8° directional light reception) Light source: D65 light source Field of view: 10 degree field of view Measurement area: LAV φ25.4mm
[0041] Then, the color difference between the hue of the test specimen and the standard (ΔE = [(ΔE*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2 is expressed in the L*a*b* color space. If ΔE is 52 or less, the hue and pattern of the background can be hidden without showing through.
[0042] [Table 1]
[0043] From Table 1, it can be seen that the test specimens containing 1.2 parts by mass or more of antimony trioxide per 100 parts by mass of polyvinyl chloride resin all satisfy the flame retardancy, flexibility, and base hiding properties. In addition, the test specimen containing 7.2 parts by mass of antimony trioxide does not produce afterflames, so there is no need to add more expensive antimony trioxide. Therefore, it can be said that the more preferable upper limit of the amount of antimony trioxide to be added is 7.2 parts by mass.
[0044] [Table 2]
[0045] From Table 2, it can be seen that the test specimens in which the blending amount of the plasticizer was 45 parts by mass to 75 parts by mass per 100 parts by mass of the vinyl chloride resin were satisfactory in all respects of flame retardancy, flexibility, and base hiding ability. In contrast, the test specimen with 40 parts by mass of plasticizer per 100 parts by mass of vinyl chloride resin does not satisfy the flexibility requirement, and the test specimen with 80 parts by mass of plasticizer per 100 parts by mass of vinyl chloride resin does not satisfy the flame retardancy requirement.
[0046] [Table 3]
[0047] From Table 3, it can be seen that the test specimens in which the inorganic filler was blended in an amount of 20 to 150 parts by mass per 100 parts by mass of polyvinyl chloride resin were satisfactory in terms of flame retardancy, flexibility, and base concealment. In addition, the test specimens containing no inorganic filler did not satisfy the concealment properties. It can also be seen that the test specimens containing 180 parts by mass of inorganic filler did not satisfy the flame retardancy. Note that the reason why the afterflame time becomes longer when the amount of inorganic filler is increased is thought to be because the increased amount of inorganic filler reduces the proportion of antimony trioxide in the overall composition, resulting in a reduced effect of suppressing combustion.
[0048] 2. Preparation of Backing Layer 5 The backing layer 5 was prepared with different blending amounts of the plasticizer and inorganic filler. The above-mentioned polyvinyl chloride resin (average degree of polymerization 1000) and calcium carbonate (average particle size 2.7 μm) were used as the constituent materials of the test specimen of the backing layer 5. DOP was used as the phthalate ester plasticizer.
[0049] 3. Testing of a three-layer sheet consisting of a floor sheet body 3, a fiber sheet 7, and a backing layer 5 A three-layer sheet consisting of a floor sheet body 3, a fiber sheet 7, and a backing layer 5 with a different material composition was prepared, and tests were carried out on flexibility and flame retardancy. The results are shown in Tables 4 and 5 below.
[0050] Table 4 shows the results of Test Nos. 15 to 19. In these tests, the floor sheet main body 3 had the same material composition as Test No. 4, and the fiber sheet 7 was made of glass nonwoven fabric (thickness: 0.25 mm), while the backing layer 5 was made of backing layers B1 to B5, which had different compositions of inorganic filler. Note that these backing layers did not contain flame retardants such as antimony trioxide.
[0051] [Table 4]
[0052] It is apparent from Table 4 that the blending amount of the inorganic filler in the backing layer 5 is preferably 50 parts by mass or more per 100 parts by mass of the vinyl chloride resin, from the viewpoint of increased volume.
[0053] Moreover, the three-layer sheet of Test No. 19 lacked appropriate flexibility. This is believed to be due to an excessive amount of inorganic filler in the backing layer 5. In other words, it is found that the amount of inorganic filler in the backing layer 5 is preferably 250 parts by mass or less per 100 parts by mass of vinyl chloride resin.
[0054] Table 5 shows the results of Test Nos. 20 to 23. In these tests, the floor sheet main body 3 had the same material composition as Test No. 4, and the fiber sheet 7 was made of glass nonwoven fabric (thickness 0.25 mm), while the backing layer 5 was made of backing layers Nos. B6 to B9, which had different plasticizer compositions. These backing layers also did not contain flame retardants such as antimony trioxide.
[0055] [Table 5]
[0056] From Table 5, the three-layer sheet of Test No. 20 lacks appropriate flexibility. This is considered to be due to a lack of plasticizer in the backing layer 5. In other words, it is found that the amount of plasticizer in the backing layer 5 is preferably 52 parts by mass or more per 100 parts by mass of vinyl chloride resin.
[0057] The three-layer sheet of Test No. 23 does not have sufficient flame retardancy. This is believed to be due to an excess of plasticizer in the backing layer 5. In other words, it is found that the amount of plasticizer in the backing layer 5 is preferably 67 parts by mass or less per 100 parts by mass of vinyl chloride resin.
[0058] Furthermore, with regard to the floor sheet main body 3 and the backing layer 5, the suitable thickness ratio [backing layer thickness (mm)] / [floor sheet main body thickness (mm)] is generally 0.6 or more and less than 1.0, and more preferably 0.7 to 0.9, from the viewpoint of achieving both flame retardancy and flexibility.
[0059] Although typical embodiments of the present invention have been described above, the present invention is not limited to these, and various design modifications are possible. It goes without saying that such modified versions (variations) of the design are also included in the technical scope of the present invention. [Explanation of symbols]
[0060] 1. Flame-retardant floor sheet 3 Floor sheet body 5 Backing layer 5 7 Fiber Sheet
Claims
1. A flame-retardant floor sheet whose main resin component is polyvinyl chloride resin, Contains 40 to 75 parts by mass of a plasticizer and 1 to 8 parts by mass of antimony trioxide relative to 100 parts by mass of vinyl chloride resin; A flame-retardant floor sheet characterized by:
2. Further containing 10 parts by mass to 160 parts by mass of an inorganic filler relative to 100 parts by mass of the vinyl chloride resin; The flame-retardant floor sheet according to claim 1,
3. The underside of the flame-retardant floor sheet according to claim 1 or 2, A backing layer containing 250 parts by mass or less of an inorganic filler and 50 to 70 parts by mass of a plasticizer relative to 100 parts by mass of vinyl chloride resin is laminated; A flame-retardant floor sheet characterized by:
Citation Information
Patent Citations
Highly flame-resistant vinyl chloride resin composition
JP1996127688A
Backing material for polyvinyl chloride resin
JP2005187963A
Polyvinyl chloride-based floor material
JP2007085149A
Auxiliary flame retardant, and flame-retardant vinyl chloride resin composition
JP2012172068A
Fire retardant plasticized polyvinyl chloride compositions containing triphosphate plasticizer, aluminum hydroxide and antimony trioxide filler
US4246158A