Method for producing fibrous cellulose-containing material and method for producing fibrous cellulose composite resin
By mixing carbamated cellulose fibers with resin powder additives in a dry state with specific length and moisture content, the method overcomes aggregation issues, enabling the use of low melting point resins and improving the dispersibility and reinforcing effect of fibrous cellulose composite resins.
Patent Information
- Application Number
- JP2023077702
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for producing fibrous cellulose-containing materials face challenges in using resins with low melting points as compatibilizers due to aggregation during drying, which is exacerbated by the hydrophilic nature of cellulose fibers and hydrophobic nature of resins.
The method involves mixing cellulose fibers with resin powder additives in a dry state, where the cellulose fibers are carbamated to have an average fiber length of 0.1 to 0.5 mm and a water content of 1 to 10%, preventing aggregation and allowing the use of low melting point resins by avoiding drying.
This approach enables the effective use of low melting point resins as additives, improving the dispersibility and reinforcing effect of the fibrous cellulose composite resin, enhancing its physical properties and reducing the risk of thermal degradation.
Smart Images

Figure 2024162320000001 
Figure 2024162320000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a fibrous cellulose-containing material and a method for producing a fibrous cellulose composite resin. [Background technology]
[0002] In recent years, fine fibers such as cellulose nanofibers and microfiber cellulose (microfibrillated cellulose) have been in the spotlight for use as a reinforcing material for resins. However, since fine fibers are hydrophilic while resins are hydrophobic, there is a problem with the dispersibility of the fine fibers when using the fine fibers as a reinforcing material for resins. Therefore, a technology has been proposed in which a compatibilizer made of resin powder is mixed with cellulose fibers (see, for example, Patent Document 1). This proposal involves mixing a compatibilizer with a slurry of cellulose fibers, and then drying the mixture appropriately to form a fibrous cellulose-containing material, or further kneading the mixture to form a fibrous cellulose composite resin. According to this proposal, the mixing of a compatibilizer suppresses the aggregation of cellulose fibers, and therefore this is considered to be an extremely useful technology.
[0003] However, in this proposal, the compatibilizer is mixed and then dried, and therefore, unless a resin powder with a high melting point is used, there is a possibility that the compatibilizer will not be able to maintain its powdery form during drying. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-195405 Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present invention is to provide a method for producing a fibrous cellulose-containing material, which allows the use of resins having low melting points as additives such as compatibilizers, and a method for producing a fibrous cellulose composite resin. [Means for solving the problem]
[0006] In order to be able to use resins with low melting points as additives such as compatibilizers, it is necessary to not dry the cellulose fibers and additives when mixing them, that is, to mix them in a dry state (dry mixing). However, in order to perform dry mixing, it is necessary to mix the cellulose fibers with additives such as compatibilizers in a dry state, not in a slurry state. However, if the cellulose fibers are simply not in a slurry state, the cellulose fibers will irreversibly aggregate before being mixed with additives such as compatibilizers. As a result of conducting research and development from the perspective of how to suppress this aggregation, the following method was conceived.
[0007] That is, When cellulose fibers and an additive comprising a resin powder are mixed in a dry state to prepare a fibrous cellulose-containing material, The cellulose fibers are carbamate-treated to have an average fiber length of 0.1 to 0.5 mm and a moisture content of 1 to 10%. The present invention relates to a method for producing a fibrous cellulose-containing material.
[0008] Also, A method for producing a fibrous cellulose-containing material by mixing cellulose fibers and an additive comprising a resin powder in a dry state, and then kneading the fibrous cellulose-containing material or the fibrous cellulose-containing material and a resin to produce a fibrous cellulose composite resin, comprising the steps of: The cellulose fibers are carbamate-treated to have an average fiber length of 0.1 to 0.5 mm and a moisture content of 1 to 10%. The present invention relates to a method for producing a fibrous cellulose composite resin. Effect of the Invention
[0009] According to the present invention, there is provided a method for producing a fibrous cellulose-containing material and a method for producing a fibrous cellulose composite resin, in which a resin having a low melting point can be used as an additive such as a compatibilizer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Next, an embodiment of the present invention will be described. Note that the embodiment is an example of the present invention. The scope of the present invention is not limited to the scope of the embodiment.
[0011] In the method for producing a fibrous cellulose-containing material of this embodiment, cellulose fibers are mixed in a dry state with an additive made of resin powder. The cellulose fibers are those in which some or all of the hydroxyl groups (-OH groups) are replaced with carbamate groups, that is, those that are carbamate-converted. The cellulose fibers used are those with an average fiber length of 0.1 to 0.5 mm and a moisture content of 1 to 10%. By adopting such a form, aggregation of the cellulose fibers is prevented as much as possible, and dry mixing (i.e., mixing without drying) is possible. As a result, resins with low melting points and water-soluble resins can be used as additives made of resin powder. On the other hand, in the method for producing a fibrous cellulose composite resin, the above-mentioned fibrous cellulose-containing material or the fibrous cellulose-containing material and a resin are kneaded. The following will explain in detail.
[0012] (Cellulose fiber) In this embodiment, the cellulose fibers (also referred to as "fibrous cellulose") are preferably microfiber cellulose (microfibrillated cellulose) having an average fiber diameter (width) of 0.1 to 19 μm. Microfiber cellulose with such a fiber diameter significantly improves the reinforcing effect of the resin. In addition, microfiber cellulose is easier to modify with carbamate groups (carbamation) than cellulose nanofiber, which is also a fine fiber. However, it is more preferable to carbamate the cellulose raw material before it is pulverized, and in this case, microfiber cellulose and cellulose nanofiber are equivalent.
[0013] In this embodiment, microfiber cellulose means a fiber having a larger average fiber diameter (width) than cellulose nanofiber. Specifically, the average fiber diameter is, for example, 0.1 to 19 μm, preferably 0.2 to 15 μm, and more preferably more than 0.5 to 10 μm. When the average fiber diameter of microfiber cellulose is less than 0.1 μm, it becomes the same as cellulose nanofiber, and there is a possibility that the effect of improving the strength of the resin (particularly the bending modulus) is not sufficiently obtained. In addition, the defibration time becomes longer, and a large amount of energy is required. Furthermore, the dehydration of the cellulose fiber slurry is deteriorated. When the dehydration is deteriorated, a large amount of energy is required for drying, and if a large amount of energy is applied to the drying, the microfiber cellulose may be thermally deteriorated, and the strength may be reduced. In addition, the strengthening of the drying may lead to irreversible aggregation of the cellulose fibers. On the other hand, when the average fiber diameter of microfiber cellulose exceeds 19 μm, it becomes the same as pulp, and there is a possibility that the reinforcing effect may be insufficient. In addition, it may be difficult to adjust and maintain the moisture content of the cellulose fiber.
[0014] The method for measuring the average fiber diameter of fine fibers (microfiber cellulose and cellulose nanofiber) is as follows.
[0015] First, 100 ml of an aqueous dispersion of fine fibers with a solid content concentration of 0.01 to 0.1% by mass is filtered through a Teflon (registered trademark) membrane filter, and the solvent is replaced once with 100 ml of ethanol and three times with 20 ml of t-butanol. Next, the sample is freeze-dried and osmium-coated to obtain a sample. This sample is observed using an electron microscope SEM image at a magnification of 3,000 to 30,000 times depending on the width of the fibers that constitute it. Specifically, two diagonal lines are drawn on the observed image, and three straight lines passing through the intersections of the diagonal lines are arbitrarily drawn. Furthermore, the widths of a total of 100 fibers that intersect with these three straight lines are visually measured. The median diameter of the measured values is then taken as the average fiber diameter.
[0016] Microfiber cellulose can be obtained by defibrating (refining) a cellulose raw material (hereinafter also referred to as "raw pulp"). As the raw pulp, one or more types can be selected from wood pulp made from broadleaf trees, coniferous trees, etc., non-wood pulp made from straw, bagasse, cotton, hemp, bast fiber, etc., and waste paper pulp (DIP) made from recycled waste paper, broke paper, etc. The above various raw materials may be in the form of a pulverized material (powdered material), for example, called cellulose-based powder.
[0017] However, in order to prevent impurities from being mixed in as much as possible, it is preferable to use wood pulp as the raw material pulp. As the wood pulp, for example, one or more types may be selected from chemical pulps such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP), and mechanical pulp (TMP), etc.
[0018] The hardwood kraft pulp may be bleached hardwood kraft pulp, unbleached hardwood kraft pulp, or semi-bleached hardwood kraft pulp. Similarly, the softwood kraft pulp may be bleached softwood kraft pulp, unbleached softwood kraft pulp, or semi-bleached softwood kraft pulp.
[0019] As the mechanical pulp, for example, one or more types can be selected and used from stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), ground pulp (GP), thermo-mechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), refiner mechanical pulp (RMP), bleached thermo-mechanical pulp (BTMP), etc.
[0020] As the raw material pulp, it is preferable to use pulp with a lignin content of 1% or less, and more preferably pulp with a lignin content of 0.8% or less. In this embodiment, the cellulose fiber is heat-treated so that the amount of carbamate groups introduced is 0.5 mmol / g or more, so that discoloration tends to progress. However, if the lignin content of the raw material pulp is 1% or less, discoloration caused by lignin can be reliably suppressed.
[0021] The lignin content is a value measured in accordance with the Lignin Content Test Method (JAPAN TAPPI No. 61 (2000)).
[0022] For the same reason, the kappa number of the raw pulp is preferably 2 or less, and more preferably 1 or less.
[0023] The kappa number is a value measured in accordance with the kappa number test method (JIS P 8211 (2011)).
[0024] The lignin content and the kappa number can be adjusted, for example, by selecting the raw pulp, cooking, bleaching, etc.
[0025] In this embodiment, the whiteness of the raw material pulp is preferably 50% or more, more preferably 80% or more, and particularly preferably 82% or more. If the whiteness of the raw material pulp itself is less than 50%, it will be further colored during melt-kneading with the resin, and the whiteness of the composite resin itself will be low.
[0026] The whiteness value is a value measured in accordance with JIS P 8148:2001.
[0027] The raw pulp can be pretreated by a chemical method prior to defibration. Examples of pretreatment by a chemical method include hydrolysis of polysaccharides by acid (acid treatment), hydrolysis of polysaccharides by enzymes (enzyme treatment), swelling of polysaccharides by alkali (alkali treatment), oxidation of polysaccharides by an oxidizing agent (oxidation treatment), reduction of polysaccharides by a reducing agent (reduction treatment), and the like. However, as the pretreatment by a chemical method, it is preferable to carry out an enzyme treatment, and it is more preferable to additionally carry out one or more treatments selected from an acid treatment, an alkali treatment, and an oxidation treatment. The enzyme treatment will be described in detail below.
[0028] As the enzyme used in the enzymatic treatment, it is preferable to use at least one of cellulase enzymes and hemicellulase enzymes, and more preferably to use both in combination. The use of these enzymes makes it easier to defibrate the cellulose raw material. Note that cellulase enzymes cause the decomposition of cellulose in the presence of water. Also, hemicellulase enzymes cause the decomposition of hemicellulose in the presence of water.
[0029] Examples of cellulase enzymes that can be used include enzymes produced by the genera Trichoderma (filamentous fungi), Acremonium (filamentous fungi), Aspergillus (filamentous fungi), Phanerochaete (basidiomycetes), Trametes (basidiomycetes), Humicola (filamentous fungi), Bacillus (bacteria), Schizophyllum (basidiomycetes), Streptomyces (bacteria), and Pseudomonas (bacteria). These cellulase enzymes are available as reagents or commercially available products. Examples of commercially available products include Cellulose T2 (manufactured by HPI), Meicerase (manufactured by Meiji Seika Kaisha), Novozym 188 (manufactured by Novozym), Multifect CX10L (manufactured by Genencor), and cellulase enzyme GC220 (manufactured by Genencor).
[0030] As the cellulase enzyme, either EG (endoglucanase) or CBH (cellobiohydrolase) can be used. EG and CBH can be used alone or in combination. They can also be used in combination with a hemicellulase enzyme.
[0031] Examples of hemicellulase enzymes that can be used include xylanase, which is an enzyme that breaks down xylan, mannase, which is an enzyme that breaks down mannan, and arabanase, which is an enzyme that breaks down araban. Also, pectinase, which is an enzyme that breaks down pectin, can be used.
[0032] Hemicellulose is a polysaccharide, excluding pectins, found between cellulose microfibrils in plant cell walls. Hemicellulose is diverse and differs depending on the type of wood and between the layers of the cell wall. In the secondary walls of softwoods, glucomannan is the main component, while in the secondary walls of hardwoods, 4-O-methylglucuronoxylan is the main component. Therefore, when obtaining fine fibers from softwood bleached kraft pulp (NBKP), it is preferable to use mannase. Also, when obtaining fine fibers from hardwood bleached kraft pulp (LBKP), it is preferable to use xylanase.
[0033] The amount of enzyme added to the cellulose raw material is determined by, for example, the type of enzyme, the type of wood used as the raw material (coniferous or broadleaf), the type of mechanical pulp, etc. However, the amount of enzyme added to the cellulose raw material is preferably 0.1 to 3 mass%, more preferably 0.3 to 2.5 mass%, and particularly preferably 0.5 to 2 mass%. If the amount of enzyme added is less than 0.1 mass%, the effect of adding the enzyme may not be sufficiently obtained. On the other hand, if the amount of enzyme added is more than 3 mass%, cellulose may be saccharified, and the yield of fine fibers may decrease. There is also a problem that the effect improvement corresponding to the increase in the amount added may not be observed.
[0034] When a cellulase enzyme is used as the enzyme, the pH during the enzyme treatment is preferably in the weak acidic range (pH = 3.0 to 6.9) from the viewpoint of the reactivity of the enzyme reaction, whereas when a hemicellulase enzyme is used as the enzyme, the pH during the enzyme treatment is preferably in the weak alkaline range (pH = 7.1 to 10.0).
[0035] The temperature during the enzyme treatment is preferably 30 to 70° C., more preferably 35 to 65° C., and particularly preferably 40 to 60° C., regardless of whether a cellulase enzyme or a hemicellulase enzyme is used as the enzyme. If the temperature during the enzyme treatment is 30° C. or higher, the enzyme activity is less likely to decrease, and it is possible to prevent the treatment time from being prolonged. On the other hand, if the temperature during the enzyme treatment is 70° C. or lower, it is possible to prevent the enzyme from being deactivated.
[0036] The time for the enzyme treatment depends on, for example, the type of enzyme, the temperature of the enzyme treatment, the pH during the enzyme treatment, etc. However, the time for the enzyme treatment is generally 0.5 to 24 hours.
[0037] After the enzyme treatment, it is preferable to inactivate the enzyme. Examples of methods for inactivating the enzyme include a method of adding an alkaline aqueous solution (preferably pH 10 or higher, more preferably pH 11 or higher) and a method of adding hot water at 80 to 100°C.
[0038] In addition, the enzyme treatment breaks down cellulose into oligosaccharides and monosaccharides, which turn brown and discolor when heated, like caramelized sugar. Therefore, after the enzyme treatment, it is preferable to thoroughly wash the raw pulp with water.
[0039] Next, the method of alkali treatment will be described. When the pulp is treated with alkali prior to defibration, some of the hydroxyl groups in the hemicellulose and cellulose contained in the pulp are dissociated and the molecules are anionized, weakening intra- and intermolecular hydrogen bonds and promoting the dispersion of the cellulose raw material during defibration.
[0040] Examples of the alkali used in the alkali treatment include organic alkalis such as sodium hydroxide, lithium hydroxide, potassium hydroxide, an aqueous ammonia solution, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. However, from the viewpoint of production costs, it is preferable to use sodium hydroxide.
[0041] By subjecting the microfibrous cellulose to an enzyme treatment, acid treatment, or oxidation treatment prior to defibration, the water retention of the microfibrous cellulose can be reduced, the crystallinity can be increased, and the homogeneity can be improved. In this regard, when the water retention of the microfibrous cellulose is low, it becomes easier to dehydrate, and the dewaterability of the cellulose fiber slurry is improved.
[0042] When raw pulp is treated with enzymes, acids, or oxidation, the hemicellulose and amorphous regions of cellulose contained in the pulp are decomposed. As a result, the energy required for defibration can be reduced, and the uniformity and dispersibility of the cellulose fibers can be improved. However, since pretreatment reduces the aspect ratio of microfiber cellulose, excessive pretreatment is preferably avoided when using it as a reinforcing material for resins.
[0043] The raw material pulp can be defibrated by beating the raw material pulp using, for example, a homogenizer such as a beater, a high-pressure homogenizer, or a high-pressure homogenizer, a stone mill-type friction machine such as a grinder or a grinding machine, a single-shaft kneader, a multi-shaft kneader, a kneader refiner, a jet mill, etc. However, it is preferable to use a refiner or a jet mill.
[0044] The average fiber length of the microfiber cellulose (average length of single fibers) is preferably 0.1 to 0.5 mm, more preferably 0.20 to 0.47 mm, and particularly preferably 0.30 to 0.45 mm. If the average fiber length is less than 0.1 mm, problems such as easy leakage during dehydration and easy aggregation during drying may occur. If the average fiber length is short, a three-dimensional network between the fibers may not be formed, and the flexural modulus of the composite resin may decrease, and the reinforcing effect may not be improved. On the other hand, if the average fiber length exceeds 0.5 mm, the volume change of the fibers during drying becomes large, and the fibers may aggregate due to this volume change.
[0045] The average fiber length of the microfibrous cellulose can be adjusted as desired by, for example, selecting the raw pulp, pre-treating, defibrating, and the like.
[0046] The average fiber length and the fine ratio described below are measured using a fiber analyzer "FS5" manufactured by Valmet.
[0047] The fine ratio of the microfiber cellulose is preferably 20 to 45%, more preferably 25 to 43%, and particularly preferably 30 to 41%. If the fine ratio is less than 20%, the viscosity during melt-kneading with the resin becomes too high, which may increase the torque of the kneader, reduce the amount of stable production, and deteriorate productivity. On the other hand, if the fine ratio exceeds 45%, irreversible aggregation during drying becomes strong, and the fibers may be extremely poorly dispersed during melt-kneading with the resin, which may deteriorate the physical properties of the composite resin.
[0048] The fine ratio can be adjusted by pretreatment such as enzyme treatment. However, especially when enzyme treatment is performed, the fiber itself may become tattered, and the reinforcing effect of the resin may decrease. Therefore, from this viewpoint, the amount of enzyme added is preferably 2% by mass or less, more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less. Also, not performing enzyme treatment (addition amount 0% by mass) is also an option.
[0049] Fine rate refers to the mass ratio of pulp fibers with a fiber length of 0.2 mm or less.
[0050] The aspect ratio of the microfibrous cellulose is preferably 2 to 15,000, more preferably 10 to 10,000. If the aspect ratio is less than 2, a three-dimensional network cannot be sufficiently constructed, and therefore even if the average fiber length is 0.1 mm or more, the reinforcing effect may be insufficient. On the other hand, if the aspect ratio exceeds 15,000, the entanglement of the microfibrous cellulose becomes high, and dispersion in the resin may be insufficient.
[0051] The aspect ratio is the average fiber length divided by the average fiber width. The larger the aspect ratio, the more points at which snagging occurs, and therefore the greater the reinforcing effect. However, on the other hand, the more snagging occurs, and this is thought to reduce the ductility of the resin.
[0052] The fibrillation rate of the microfiber cellulose is preferably 2.0% or less, more preferably 0.1 to 2.0%, and particularly preferably 0.2 to 1.5%. If the fibrillation rate exceeds 2.0%, the number of contacts with the surrounding fibers increases during drying, which makes the cellulose more likely to aggregate strongly, and the cellulose is extremely poorly dispersed when melt-kneaded with the resin, which may result in a decrease in the physical properties of the composite resin. On the other hand, if the fibrillation rate is less than 0.1%, the cellulose may not be caught in the resin in the composite resin, which may result in a brittle material that is easily broken when an external force is applied.
[0053] The fibrillation rate is the ratio of the projected area of small fibers to the projected area of the entire fiber, i.e., the fuzzed area / the entire fiber including fuzz. This value is measured, for example, by a fiber analyzer "FS5" manufactured by Valmet.
[0054] The crystallinity of the microfiber cellulose is preferably 50% or more, more preferably 55% or more, and particularly preferably 60% or more. If the crystallinity is less than 50%, the mixability with other fibers such as pulp and cellulose nanofibers is improved, but the strength of the fiber itself is reduced, so that the strength of the resin may not be improved. On the other hand, the crystallinity of the microfiber cellulose is preferably 95% or less, more preferably 90% or less, and particularly preferably 85% or less. If the crystallinity is more than 95%, the proportion of strong hydrogen bonds in the molecule increases, the fiber itself becomes rigid, and dispersibility becomes poor.
[0055] The crystallinity of the microfibrous cellulose can be adjusted as desired, for example, by selecting the raw pulp, pre-treating it, and refining it.
[0056] The crystallinity is a value measured in accordance with JIS K 0131 (1996).
[0057] The pulp viscosity of the microfiber cellulose is preferably 2 cps or more, more preferably 4 cps or more. If the pulp viscosity of the microfiber cellulose is less than 2 cps, it may be difficult to suppress the aggregation of the microfiber cellulose.
[0058] The pulp viscosity is a value measured in accordance with TAPPI T 230.
[0059] The freeness of the microfiber cellulose is preferably 500 ml or less, more preferably 300 ml or less, and particularly preferably 100 ml or less. If the freeness of the microfiber cellulose exceeds 500 ml, the effect of improving the strength of the resin may not be sufficiently obtained.
[0060] The freeness is a value measured in accordance with JIS P8121-2 (2012).
[0061] The zeta potential of the microfibrous cellulose is preferably -150 to 20 mV, more preferably -100 to 0 mV, and particularly preferably -80 to -10 mV. If the zeta potential is less than -150 mV, the compatibility with the resin may be significantly reduced, resulting in insufficient reinforcing effect. On the other hand, if the zeta potential is more than 20 mV, the dispersion stability may be reduced.
[0062] The water retention of the microfiber cellulose is preferably 80 to 400%, more preferably 90 to 350%, and particularly preferably 100 to 300%. If the water retention is less than 80%, the reinforcing effect may be insufficient because it is the same as the raw material pulp. On the other hand, if the water retention is more than 400%, the dewatering property tends to be poor and the cellulose tends to aggregate easily. On the other hand, if the water retention is 80 to 400%, it becomes easy to make the moisture content of the fibrous cellulose-containing material described later 10% or less, and the fibers are less likely to be damaged, which contributes to improving the strength of the composite resin. The water retention of the microfiber cellulose can be further reduced by substituting the hydroxyl group of the fiber with a carbamate group, and the dewatering property and drying property can be improved.
[0063] The water retention of the microfiber cellulose can be adjusted as desired by, for example, selecting the raw pulp, pre-treating it, defibrating it, and the like.
[0064] The water retention is a value measured in accordance with JAPAN TAPPI No. 26 (2000).
[0065] The moisture content of the microfiber cellulose is preferably 1 to 10%, more preferably 2 to 10%, and particularly preferably 3 to 10%. If the moisture content is less than 1%, the fibers may adhere to each other due to electrostatic charge, which may cause fiber aggregation. The problem of electrostatic charge of the fibers may include problems such as the cellulose fibers adhering to the vicinity of the inlet of various devices that process the cellulose fibers and the formation of bridges of the cellulose fibers. On the other hand, if the moisture content exceeds 10%, the fibers may adhere to each other due to moisture, which may cause fiber aggregation.
[0066] As a method for adjusting the moisture content of the microfibrous cellulose, for example, there is a method in which the microfibrous cellulose is dried prior to mixing with an additive made of resin powder, but this drying is limited to a range in which the moisture content of the microfibrous cellulose is 1% or more (preferably 3 to 10%). Another method is to dry the microfibrous cellulose until the moisture content of the microfibrous cellulose becomes less than 1%, and then wait for the moisture content to return to 1% or more, and mix it with an additive made of resin powder after the moisture content reaches 1% or more.
[0067] In any case, the important thing is the size of the microfiber cellulose, especially the relationship between the average fiber length and the moisture content. That is, if the fiber size is too large, the difference in moisture content between the surface and the inside will be large, and the moisture inside may seep out and cause fiber aggregation. On the other hand, if the fiber size is too small, other fibers will surround the fibers, causing a difference in moisture content and the same problems as when the fiber size is large may occur.
[0068] The preferred fiber size is as described above. If necessary, the fiber may be dehydrated prior to drying to obtain a dehydrated product. This dehydration may be performed using one or more dehydration devices selected from, for example, a belt press, a screw press, a filter press, a twin roll, a twin wire former, a valveless filter, a center disk filter, a membrane treatment, a centrifuge, and the like.
[0069] The drying of cellulose fibers can be carried out by using one or more selected from, for example, rotary kiln drying, disc drying, air flow drying, media flow drying, spray drying, drum drying, screw conveyor drying, paddle drying, uniaxial kneading drying, multiaxial kneading drying, vacuum drying, stirring drying, and the like.
[0070] The moisture content (moisture content) of cellulose fiber was calculated using the following formula by holding a sample at 105°C for 6 hours or more in a constant temperature dryer, and taking the mass after drying as the point at which no change in mass was observed. Moisture content (%) = [(mass before drying - mass after drying) ÷ mass before drying] × 100
[0071] The microfiber cellulose has a carbamate group. There is no particular limitation on how the microfiber cellulose has the carbamate group. For example, the microfiber cellulose may have the carbamate group by carbamateizing a cellulose raw material, or the microfiber cellulose (a finely divided cellulose raw material) may have the carbamate group by carbamateizing.
[0072] Incidentally, having a carbamate group means that a carbamate has been introduced into the fibrous cellulose. The carbamate group is a group represented by -O-CO-NH-, for example, a group represented by -O-CO-NH2, -O-CONHR, -O-CO-NR2, etc. In other words, the carbamate group can be represented by the following structural formula (1).
[0073] [ka]
[0074] Here, n represents an integer of 1 or more. Each R is independently at least one of a hydrogen atom, a saturated linear hydrocarbon group, a saturated branched hydrocarbon group, a saturated cyclic hydrocarbon group, an unsaturated linear hydrocarbon group, an unsaturated branched hydrocarbon group, an aromatic group, and a group derived therefrom.
[0075] Examples of the saturated linear hydrocarbon group include linear alkyl groups having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, and a propyl group.
[0076] Examples of the saturated branched hydrocarbon group include branched alkyl groups having 3 to 10 carbon atoms, such as an isopropyl group, a sec-butyl group, an isobutyl group, and a tert-butyl group.
[0077] Examples of the saturated cyclic hydrocarbon group include cycloalkyl groups such as a cyclopentyl group, a cyclohexyl group, and a norbornyl group.
[0078] Examples of the unsaturated linear hydrocarbon group include linear alkenyl groups having 2 to 10 carbon atoms, such as ethenyl, propen-1-yl, and propen-3-yl, and linear alkynyl groups having 2 to 10 carbon atoms, such as ethynyl, propyn-1-yl, and propyn-3-yl.
[0079] Examples of the unsaturated branched hydrocarbon group include branched alkenyl groups having 3 to 10 carbon atoms, such as a propen-2-yl group, a buten-2-yl group, and a buten-3-yl group, and branched alkynyl groups having 4 to 10 carbon atoms, such as a butyn-3-yl group.
[0080] Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group.
[0081] Examples of derivative groups include groups in which one or more hydrogen atoms in the above-mentioned saturated linear hydrocarbon groups, saturated branched hydrocarbon groups, saturated cyclic hydrocarbon groups, unsaturated linear hydrocarbon groups, unsaturated branched hydrocarbon groups, and aromatic groups are substituted with substituents (e.g., hydroxy groups, carboxy groups, halogen atoms, etc.).
[0082] In microfiber cellulose having a carbamate group (introduced with a carbamate group), some or all of the highly polar hydroxyl groups are substituted with carbamate groups having relatively low polarity. Therefore, microfiber cellulose having a carbamate group has low hydrophilicity and high affinity with resins having low polarity. As a result, microfiber cellulose having a carbamate group has excellent uniform dispersion with resins. In addition, a slurry of microfiber cellulose having a carbamate group has low viscosity and good handling properties.
[0083] The amount of carbamate groups introduced relative to the hydroxyl groups of the microfiber cellulose is preferably 0.5 to 2.0 mmol / g, more preferably 0.5 to 1.5 mmol / g, and particularly preferably 0.5 to 1.0 mmol / g. When the amount introduced is 0.5 mmol / g or more, the hydrogen bonds between the cellulose fibers caused by the hydroxyl groups of the cellulose fibers are weakened (agglomeration relaxation effect), and in addition, the affinity with the resin is increased (affinity improvement effect) by the introduction of carbamate groups, which are more hydrophobic than hydroxyl groups, so that the microfiber cellulose does not aggregate in the resin and reliably plays the role of reinforcing the resin. However, when the amount introduced exceeds 2.0 mmol / g, it becomes difficult to increase the moisture content of the microfiber cellulose, and it also becomes difficult to adjust the moisture content of the microfiber cellulose. In addition, when the amount introduced exceeds 2.0 mmol / g, there is a possibility that the heat resistance of the composite resin may be reduced. In this regard, when cellulose fibers are subjected to heat, hydroxyl groups are usually released, and the molecular chain may become shorter from the point where the release occurs. If some of the hydroxyl groups are modified by carbamate, etc., the release of hydroxyl groups is more likely to occur. Therefore, if the carbamate conversion rate is increased too much, the molecular chain becomes too short, the decomposition temperature decreases, and the heat resistance decreases. In addition, if the amount of carbamate groups introduced exceeds 2.0 mmol / g, the average fiber length of the pulp becomes shorter when the cellulose fibers are carbamate, and as a result, there is a problem that the average fiber length of the microfiber cellulose is easily less than 0.1 mm.
[0084] In this embodiment, the amount of carbamate groups introduced (mmol / g) refers to the amount of carbamate groups contained in 1 g of cellulose raw material having carbamate groups. The amount of carbamate groups introduced is determined by measuring the N atoms present in the carbamate-treated pulp by the Kjeldahl method and calculating the carbamate conversion rate per unit weight. Cellulose is a polymer with anhydroglucose as a structural unit, and has three hydroxyl groups per structural unit.
[0085] <Carbamate formation> Regarding the introduction of carbamate groups (carbamation) into microfiber cellulose (when carbamate is performed before defibration, it is the cellulose raw material. Hereinafter, the same is also referred to as "microfiber cellulose, etc."), there are a method of carbamate-ifying the cellulose raw material and then refining it, as described above, and a method of refining the cellulose raw material and then carbamate-ifying it. In this regard, in this specification, defibration of the cellulose raw material is explained first, and then carbamate-ification (modification) is explained. However, either defibration or carbamate-ification can be performed first. However, it is preferable to perform carbamate-ification first and then defibration. This is because the cellulose raw material before defibration has a high dehydration efficiency, and the cellulose raw material is in a state that is easily defibrated by the heating associated with carbamate-ification.
[0086] The process of carbamate-forming microfiber cellulose and the like can be mainly divided into, for example, a mixing process, a removal process, and a heat treatment. The mixing process and the removal process can be collectively called a preparation process for preparing a mixture to be subjected to a heat treatment. Carbamate-forming has an advantage that it can be chemically modified without using an organic solvent.
[0087] In the mixing process, microfiber cellulose or the like (which may be a cellulose raw material as described above, the same applies below) and urea or a urea derivative (hereinafter simply referred to as "urea, etc.") are mixed in a dispersion medium.
[0088] Examples of urea and urea derivatives that can be used include urea, thiourea, biuret, phenylurea, benzylurea, dimethylurea, diethylurea, tetramethylurea, and compounds in which the hydrogen atoms of urea are substituted with alkyl groups. These urea and urea derivatives can be used alone or in combination. However, it is preferable to use urea.
[0089] The lower limit of the mixture mass ratio of urea etc. to microfiber cellulose etc. (urea etc. / microfiber cellulose etc.) is preferably 8 / 100, more preferably 5 / 100. On the other hand, the upper limit is preferably 20 / 100, more preferably 15 / 100. By making the mixture mass ratio 5 / 100 or more, the efficiency of carbamate formation is improved. On the other hand, even if the mixture mass ratio exceeds 20 / 100, the amount of urea that does not react with microfiber cellulose increases, and the amount of ammonia gas generated by thermal decomposition of urea increases, and large-scale equipment such as a scrubber required for gas treatment is required, which increases costs and is not industrially preferable.
[0090] The dispersion medium is usually water, although other dispersion media such as alcohols, ethers, and mixtures of water with other dispersion media may also be used.
[0091] In the mixing treatment, for example, microfibrous cellulose, etc. and urea, etc. may be added to water, microfibrous cellulose, etc. may be added to an aqueous solution of urea, etc., or urea, etc. may be added to a slurry containing microfibrous cellulose, etc. In order to mix uniformly, stirring may be performed after addition. Furthermore, the dispersion containing microfibrous cellulose, etc. and urea, etc. may contain other components.
[0092] In the removal treatment, the dispersion medium is removed from the dispersion liquid containing the microfibrous cellulose etc. and urea etc. obtained in the mixing treatment. By removing the dispersion medium, the urea etc. can be reacted efficiently in the subsequent heat treatment.
[0093] The dispersion medium is preferably removed by volatilizing it by heating, which makes it possible to efficiently remove only the dispersion medium while leaving behind the components such as urea.
[0094] When the dispersion medium is water, the lower limit of the heating temperature in the removal treatment is preferably 50°C, more preferably 70°C, and particularly preferably 90°C. By setting the heating temperature at 50°C or higher, the dispersion medium can be efficiently volatilized (removed). On the other hand, the upper limit of the heating temperature is preferably 120°C, more preferably 100°C. If the heating temperature exceeds 120°C, the dispersion medium and urea may react, and the urea may independently decompose.
[0095] The heating time in the removal treatment can be appropriately adjusted depending on the solid content concentration of the dispersion liquid, etc. Specifically, it is, for example, 6 to 24 hours.
[0096] In the heat treatment following the removal treatment, a mixture of the microfiber cellulose and urea is heat-treated. In this heat treatment, some or all of the hydroxyl groups of the microfiber cellulose react with urea and are replaced with carbamate groups. More specifically, when urea is heated, it is decomposed into isocyanic acid and ammonia as shown in the following reaction formula (1). Isocyanic acid is very reactive and forms carbamate groups on the hydroxyl groups of cellulose as shown in the following reaction formula (2). NH2-CO-NH2→ HN=C=O + NH3…(1) Cell-OH + HN=C=O → Cell-O-CO-NH2…(2)
[0097] The lower limit of the heating temperature in the heat treatment is preferably 120°C, more preferably 130°C, particularly preferably the melting point of urea (about 134°C) or higher, even more preferably 140°C, and most preferably 150°C. By setting the heating temperature at 120°C or higher, carbamate formation is efficiently carried out. The upper limit of the heating temperature is preferably 200°C, more preferably 180°C, and particularly preferably 170°C. If the heating temperature exceeds 200°C, the microfiber cellulose and the like may decompose, resulting in insufficient reinforcing effect.
[0098] The lower limit of the heating time in the heat treatment is preferably 1 minute, more preferably 5 minutes, particularly preferably 30 minutes, even more preferably 1 hour, and most preferably 2 hours. By setting the heating time to 1 minute or more, the carbamate reaction can be carried out reliably. On the other hand, the upper limit of the heating time is preferably 15 hours, more preferably 10 hours. If the heating time exceeds 15 hours, it is not economical, and carbamate reaction can be sufficiently carried out in 15 hours.
[0099] However, prolonged heating time leads to deterioration of cellulose fibers. Therefore, the pH conditions in the heat treatment are important. The pH is preferably 9 or more, more preferably 9 to 13, and particularly preferably 10 to 12, which is an alkaline condition. As a second best option, the pH is 7 or less, preferably 3 to 7, and particularly preferably 4 to 7, which is an acidic or neutral condition. Under neutral conditions of pH 7 to 8, the average fiber length of the cellulose fibers is shortened, and the reinforcing effect of the resin may be inferior. On the other hand, under alkaline conditions of pH 9 or more, the reactivity of the cellulose fibers is increased, the reaction with urea, etc. is promoted, and the carbamate reaction occurs efficiently, so that the average fiber length of the cellulose fibers can be sufficiently secured. On the other hand, under acidic conditions of pH 7 or less, the reaction of decomposing urea, etc. into isocyanic acid and ammonia proceeds, the reaction with cellulose fibers is promoted, and the carbamate reaction occurs efficiently, so that the average fiber length of the cellulose fibers can be sufficiently secured. However, if possible, it is preferable to perform the heat treatment under alkaline conditions. This is because acidic conditions may cause acid hydrolysis of cellulose to proceed.
[0100] The pH can be adjusted by adding an acidic compound (eg, acetic acid, citric acid, etc.) or an alkaline compound (eg, sodium hydroxide, calcium hydroxide, etc.) to the mixture.
[0101] As a heating device in the heat treatment, for example, a hot air dryer, a papermaking machine, a dry pulp machine, etc. can be used.
[0102] The mixture after the heat treatment may be washed. This washing may be performed with water or the like. By this washing, the unreacted remaining urea and the like can be removed.
[0103] (Additives) The cellulose fiber-containing material of this embodiment contains, together with the cellulose fibers, an additive consisting of a resin powder, preferably an acid-modified resin, more preferably an organic acid-modified resin.
[0104] Examples of the acid-modified resin include acid-modified polyolefin resin, acid-modified epoxy resin, and acid-modified styrene-based elastomer resin. However, it is preferable to use an acid-modified polyolefin resin. The acid-modified polyolefin resin is a copolymer of an unsaturated carboxylic acid component and a polyolefin component.
[0105] As the polyolefin component, for example, one or more alkene polymers such as ethylene, propylene, butadiene, isoprene, etc. can be selected and used, although it is preferable to use ethylene or propylene.
[0106] As the unsaturated carboxylic acid component, for example, one or more selected from maleic anhydrides, phthalic anhydrides, itaconic anhydrides, citraconic anhydrides, citric anhydrides, etc. can be used. However, it is preferable to use maleic anhydrides. In other words, it is preferable to use maleic anhydride-modified polypropylene or maleic anhydride-modified polyethylene resin.
[0107] The average particle diameter of the additive made of resin powder is preferably 1 to 1,000 μm, more preferably 5 to 800 μm, and particularly preferably 10 to 500 μm. If the average particle diameter exceeds 1,000 μm, when mixed with dry fine cellulose fibers, the additive and the fine cellulose fibers do not mix well, and one of them is present unevenly, which causes unevenness when melted and kneaded, and since they are not mixed uniformly, they may be significantly colored due to local shear and heat generation, or the dispersibility of the fine cellulose fibers may deteriorate. On the other hand, if the average particle diameter is less than 1 μm, the additives may become lumpy, and when mixed with dry fine cellulose fibers, the additives and the fine cellulose fibers may not mix well, which may cause coloring and deterioration of dispersibility due to local shear, and since the additive is a fine powder, there is a risk of dust explosion when handled, and there is a possibility of adverse effects on the human body when inhaled.
[0108] The amount of the additive made of resin powder mixed is preferably 10 to 100 parts by mass, more preferably 20 to 80 parts by mass, and particularly preferably 40 to 60 parts by mass, relative to 100 parts by mass of the microfiber cellulose. In particular, when the additive made of resin powder is a maleic anhydride-modified polypropylene resin, the amount is preferably 20 to 80 parts by mass, more preferably 40 to 60 parts by mass. If the amount mixed is less than 10 parts by mass, the improvement in strength is not sufficient. On the other hand, if the amount mixed is more than 100 parts by mass, it becomes excessive and the strength tends to decrease.
[0109] The weight average molecular weight of the additive made of resin powder is, for example, 1,000 to 100,000, and preferably 3,000 to 50,000.
[0110] The acid value of the additive made of resin powder is preferably 0.5 mgKOH / g or more and 100 mgKOH / g or less, and more preferably 1 mgKOH / g or more and 50 mgKOH / g or less.
[0111] Furthermore, the MFR (melt flow rate) of the additive made of resin powder is preferably 2000 g / 10 min (190° C. / 2.16 kg) or less, more preferably 1500 g / 10 min or less, and particularly preferably 500 g / 10 min or less. If the MFR exceeds 2000 g / 10 min, the dispersibility of the cellulose fiber may decrease.
[0112] The acid value is measured in accordance with JIS-K2501 by titration with potassium hydroxide, while the MFR is measured in accordance with JIS-K7210 by placing a load of 2.16 kg at 190°C and measuring the weight of the sample that flows out in 10 minutes.
[0113] (Other additives) The cellulose fiber-containing material of this embodiment preferably contains a dispersant as an additive. The dispersant is preferably an aromatic compound having an amine group and / or a hydroxyl group, or an aliphatic compound having an amine group and / or a hydroxyl group.
[0114] Examples of compounds having an amine group and / or a hydroxyl group in an aromatic group include anilines, toluidines, trimethylanilines, anisidines, tyramines, histamines, tryptamines, phenols, dibutylhydroxytoluenes, bisphenol A, cresols, eugenols, gallic acids, guaiacols, picric acids, phenolphthaleins, serotonins, dopamines, adrenalines, noradrenalines, thymols, tyrosines, salicylic acids, methyl salicylates, a Examples of such alcohols include varnish alcohols, salicylic alcohols, sinapyl alcohols, diphenidols, diphenylmethanols, cinnamyl alcohols, scopolamines, tryptophols, vanillyl alcohols, 3-phenyl-1-propanols, phenethyl alcohols, phenoxyethanols, veratryl alcohols, benzyl alcohols, benzoins, mandelic acids, mandelonitriles, benzoic acids, phthalic acids, isophthalic acids, terephthalic acids, mellitic acids, and cinnamic acids.
[0115] Examples of compounds having an amine group and / or a hydroxyl group in an aliphatic group include capryl alcohols, 2-ethylhexanols, pelargonic alcohols, capric alcohols, undecyl alcohols, lauryl alcohols, tridecyl alcohols, myristyl alcohols, pentadecyl alcohols, cetanols, stearyl alcohols, elaidyl alcohols, oleyl alcohols, linoleyl alcohols, methylamines, dimethylamines, trimethylamines, ethylamines, diethylamines, and ethylenediamines. , triethanolamines, N,N-diisopropylethylamines, tetramethylethylenediamines, hexamethylenediamines, spermidines, spermines, amantadines, formic acids, acetic acids, propionic acids, butyric acids, valeric acids, caproic acids, enanthic acids, caprylic acids, pelargonic acids, capric acids, lauric acids, myristic acids, palmitic acids, margaric acids, stearic acids, oleic acids, linoleic acids, linolenic acids, arachidonic acids, eicosapentaenoic acids, docosahexaenoic acids, and sorbic acids.
[0116] The above dispersants inhibit hydrogen bonding between cellulose fibers. Therefore, the microfibrous cellulose is reliably dispersed in the resin when the microfibrous cellulose and the resin are kneaded. The above dispersants also have the role of improving the compatibility of the microfibrous cellulose and the resin. In this respect, the dispersibility of the microfibrous cellulose in the resin is improved.
[0117] It is possible to add a separate compatibilizer (chemical) when kneading the fibrous cellulose and resin, but rather than adding the chemical at this stage, mixing the fibrous cellulose with a dispersing agent (chemical) in advance to form a fibrous cellulose-containing material will allow the chemical to adhere more uniformly to the fibrous cellulose, thereby improving compatibility with the resin.
[0118] Also, for example, polypropylene has a melting point of 160°C, so the kneading of fibrous cellulose and resin is carried out at about 180°C. However, if a dispersant (liquid) is added in this state, it dries out in an instant. Therefore, there is a method in which a master batch (composite resin with a high concentration of microfiber cellulose) is produced using a resin with a low melting point, and then the concentration is reduced with a normal resin. However, resins with low melting points generally have low strength. Therefore, this method may reduce the strength of the composite resin.
[0119] The amount of the dispersant mixed is preferably 0.1 to 1,000 parts by mass, more preferably 1 to 500 parts by mass, and particularly preferably 10 to 200 parts by mass, relative to 100 parts by mass of the microfiber cellulose. If the amount of the dispersant mixed is less than 0.1 parts by mass, the improvement in resin strength may be considered insufficient. On the other hand, if the amount mixed is more than 1,000 parts by mass, the resin strength tends to decrease due to excessive use.
[0120] In this respect, the additives such as the acid-modified resin described above improve compatibility by ionic bonding between the acid group and the carbamate group of the microfibrous cellulose, thereby enhancing the reinforcing effect, and since the molecular weight is large, it is easily compatible with the resin and is thought to contribute to improving strength. On the other hand, the dispersant described above is interposed between the hydroxyl groups of the microfibrous cellulose to prevent aggregation, thereby improving dispersibility in the resin, and since the molecular weight is smaller than that of the additives such as the acid-modified resin, it can enter the narrow space between the microfibrous cellulose where the additives such as the acid-modified resin cannot enter, and plays a role of improving dispersibility and improving strength. From the above viewpoint, the molecular weight of the additives such as the acid-modified resin is preferably 2 to 2,000 times, preferably 5 to 1,000 times, the molecular weight of the dispersant.
[0121] In the above, the average particle size of a powder is a median diameter calculated from a volume-based particle size distribution measured using a particle size distribution measuring device (e.g., a laser diffraction / scattering particle size distribution measuring device manufactured by Horiba, Ltd.) while the powder is either as is or in the form of a water dispersion.
[0122] (Manufacturing method) The cellulose fibers and the additives made of resin powder are mixed in a dry state (dry mixing) to obtain a fibrous cellulose-containing material. The temperature during this dry mixing is preferably 1 to 50°C, more preferably 1 to 45°C, and particularly preferably 1 to 40°C. If the mixing temperature is less than 1°C, the moisture attached to the cellulose fibers and additives freezes, and the water cannot release static electricity, which may cause adhesion to the inner wall of the pipe due to static electricity or poor feeding to the kneader. On the other hand, if the mixing temperature exceeds 50°C, the moisture attached to the cellulose fibers and additives evaporates, and the water that releases static electricity is lost, which may cause adhesion to the inner wall of the pipe due to static electricity or poor feeding to the kneader. Incidentally, since the method of this embodiment employs dry mixing, a water-soluble dispersant can be used at this stage.
[0123] A fibrous cellulose-containing material or the fibrous cellulose-containing material and a resin are kneaded to obtain a fibrous cellulose composite resin. In this regard, the fibrous cellulose-containing material is preferably pulverized to a powder before being kneaded with the resin. This pulverization can be performed using one or more of a bead mill, a kneader, a disperser, a twist mill, a cut mill, a hammer mill, etc.
[0124] The average particle size of the powdery material is preferably 1 to 10,000 μm, more preferably 10 to 5,000 μm, and particularly preferably 100 to 2,000 μm. If the average particle size of the powdery material exceeds 10,000 μm, it may be poor in kneadability with resin. On the other hand, it is not economical to reduce the average particle size of the powdery material to less than 1 μm because a large amount of energy is required.
[0125] The average particle size of the powdery material can be controlled by controlling the degree of pulverization, as well as by classification using a classifying device such as a filter or a cyclone.
[0126] The bulk density of the mixture (powder material) is preferably 0.03 to 1.0, more preferably 0.04 to 0.9, and particularly preferably 0.05 to 0.8. A bulk density exceeding 1.0 means that the hydrogen bonds between the fibrous cellulose are stronger, and it is not easy to disperse the cellulose in the resin. On the other hand, a bulk density below 0.03 is disadvantageous in terms of transportation costs.
[0127] The bulk density is a value measured in accordance with JIS K7365.
[0128] It is preferable to compress the fibrous cellulose-containing material prior to kneading. In this regard, compression refers to a process of applying external pressure to the material (mixture), and can be performed, for example, using an apparatus that applies external pressure to a powdery or granular material to compress it and granulate it into pellets. Examples of such an apparatus include a biomass pellet manufacturing apparatus from Earth Engineering Co., Ltd., a press pelletizer from Chiyoda Machinery Co., Ltd., a wood pellet manufacturing apparatus from Apte Japan Co., Ltd., a biomass pellet manufacturing apparatus from Shinko Koki Co., Ltd., a pelletizer from Tosa Tech Co., Ltd., a briquette from WELHOUSE Co., Ltd., and a briquette machine from Nippon Steel Corporation. The fibrous cellulose-containing material is compressed into a pellet-shaped microfiber cellulose solid by being put into these devices.
[0129] The fibrous cellulose-containing material (resin reinforcing material) obtained as described above is kneaded as it is or with a resin (addition of resin) to obtain a fibrous cellulose composite resin. This kneading can be performed, for example, by mixing the pellet-shaped resin with the reinforcing material, or by melting the resin first and adding the reinforcing material to the melt.
[0130] For the kneading treatment, for example, one or more of a single-shaft or multi-shaft kneader having two or more shafts, a mixing roll, a kneader, a roll mill, a Banbury mixer, a screw press, a disperser, etc. can be selected and used. Among these, it is preferable to use a multi-shaft kneader having two or more shafts. Two or more multi-shaft kneaders having two or more shafts may be used in parallel or in series.
[0131] The kneading temperature is equal to or higher than the glass transition point of the resin, and differs depending on the type of resin, but is preferably 80 to 280°C, more preferably 90 to 260°C, and particularly preferably 100 to 240°C.
[0132] As the resin, it is preferable to use at least one of a thermoplastic resin and a thermosetting resin.
[0133] As the thermoplastic resin, for example, one or more selected from polyolefins such as polypropylene (PP) and polyethylene (PE), polyester resins such as aliphatic polyester resins and aromatic polyester resins, polyacrylic resins such as polystyrene, methacrylate and acrylate, polyamide resins, polycarbonate resins, polyacetal resins, etc. can be used.
[0134] However, it is preferable to use at least one of polyolefin and polyester resin. As the polyolefin, it is preferable to use polypropylene. As the polyester resin, examples of the aliphatic polyester resin include polylactic acid and polycaprolactone, and examples of the aromatic polyester resin include polyethylene terephthalate, but it is preferable to use a biodegradable polyester resin (also simply called "biodegradable resin").
[0135] As the biodegradable resin, for example, one or more types may be selected from hydroxycarboxylic acid-based aliphatic polyesters, caprolactone-based aliphatic polyesters, dibasic acid polyesters, and the like and used.
[0136] As the hydroxycarboxylic acid-based aliphatic polyester, one or more selected from homopolymers of hydroxycarboxylic acids such as lactic acid, malic acid, glucose acid, 3-hydroxybutyric acid, etc., and copolymers using at least one of these hydroxycarboxylic acids, etc. However, it is preferable to use polylactic acid, copolymers of lactic acid and the above hydroxycarboxylic acids other than lactic acid, polycaprolactone, and copolymers of at least one of the above hydroxycarboxylic acids and caprolactone, and it is particularly preferable to use polylactic acid.
[0137] As the lactic acid, for example, L-lactic acid, D-lactic acid, etc. can be used, and these lactic acids may be used alone or in combination of two or more kinds.
[0138] As the caprolactone-based aliphatic polyester, for example, one or more types may be selected from homopolymers of polycaprolactone and copolymers of polycaprolactone or the like with the above-mentioned hydroxycarboxylic acids and the like.
[0139] As the dibasic acid polyester, for example, one or more types may be selected from polybutylene succinate, polyethylene succinate, polybutylene adipate, and the like and used.
[0140] The biodegradable resin may be used alone or in combination of two or more kinds.
[0141] Examples of the thermosetting resin that can be used include phenol resins, urea resins, melamine resins, furan resins, unsaturated polyesters, diallyl phthalate resins, vinyl ester resins, epoxy resins, urethane resins, silicone resins, thermosetting polyimide resins, etc. These resins can be used alone or in combination of two or more.
[0142] The resin may contain an inorganic filler, preferably in a proportion that does not interfere with thermal recycling.
[0143] Examples of inorganic fillers include simple substances, oxides, hydroxides, carbonates, sulfates, silicates, and sulfites of metal elements in Groups I to VIII of the periodic table, such as Fe, Na, K, Cu, Mg, Ca, Zn, Ba, Al, Ti, and silicon, as well as various clay minerals composed of these compounds.
[0144] Specific examples include barium sulfate, calcium sulfate, magnesium sulfate, sodium sulfate, calcium sulfite, zinc oxide, silica, heavy calcium carbonate, light calcium carbonate, aluminum borate, alumina, iron oxide, calcium titanate, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, sodium hydroxide, magnesium carbonate, calcium silicate, clay wollastonite, glass beads, glass powder, silica sand, silica stone, quartz powder, diatomaceous earth, white carbon, glass fiber, etc. A plurality of these inorganic fillers may be contained. Also, it may be one contained in waste paper pulp.
[0145] The blending ratio of the resin to the fibrous cellulose is preferably 0.4 to 19, preferably 0.5 to 13, more preferably 0.6 to 9, per 1 part by mass of the fibrous cellulose. In particular, when the blending ratio of the fibrous cellulose is 10 to 50 parts by mass in 100 parts by mass of the fibrous cellulose composite resin, the strength of the resin composition, particularly the bending strength and tensile modulus, can be significantly improved.
[0146] The content ratio of the fibrous cellulose and the resin in the final resin composition is usually the same as the above-mentioned blending ratio of the fibrous cellulose and the resin.
[0147] Solubility parameters (cal / cm) of microfiber cellulose and resin 3 ) 1 / 2 The difference in SP value is the SP value of microfiber cellulose. MFC Value, resin SPPOL value, the difference in SP value = SP MFC Value − SP POL The difference in SP value is preferably 10 to 0.1, more preferably 8 to 0.5, and particularly preferably 5 to 1. If the difference in SP value exceeds 10, the microfiber cellulose may not disperse in the resin, and the reinforcing effect may not be obtained. On the other hand, if the difference in SP value is less than 0.1, the microfiber cellulose will dissolve in the resin, will not function as a filler, and the reinforcing effect will not be obtained. In this regard, the SP of the resin (solvent) POL Value and SP of microfiber cellulose (solute) MFC The smaller the difference in the values, the greater the reinforcing effect.
[0148] The solubility parameter (cal / cm 3 ) 1 / 2 The SP value is a measure of the intermolecular force acting between a solvent and a solute, and the closer the SP values of the solvent and solute are, the greater the solubility.
[0149] (Molding process) The kneaded mixture of the fibrous cellulose-containing material and the resin can be molded into a desired shape after re-kneading as necessary. The size, thickness, shape, etc. of the molded product are not particularly limited, and can be, for example, a sheet, pellet, powder, fiber, etc.
[0150] The temperature during the molding process is equal to or higher than the glass transition point of the resin, and differs depending on the type of resin, but is, for example, 90 to 260°C, and preferably 100 to 240°C.
[0151] The kneaded material can be molded by, for example, mold molding, injection molding, extrusion molding, hollow molding, foam molding, etc. The kneaded material can also be spun into fibers and mixed with the above-mentioned plant materials to form a mat or board. The mixed fibers can be simultaneously deposited by air laying, for example.
[0152] As the apparatus for molding the kneaded product, for example, one or more types may be selected from an injection molding machine, a blow molding machine, a hollow molding machine, a blow molding machine, a compression molding machine, an extrusion molding machine, a vacuum molding machine, a pressure molding machine, etc., and may be used.
[0153] The above molding can be carried out following kneading, or the kneaded mixture can be cooled once and then chipped using a crusher or the like, and the chips can be fed into a molding machine such as an extrusion molding machine or an injection molding machine. Of course, molding is not an essential requirement of the present invention.
[0154] (Other compositions) The fibrous cellulose may contain cellulose nanofibers together with microfiber cellulose. Cellulose nanofibers are fine fibers like microfiber cellulose, and play a role in complementing microfiber cellulose in improving the strength of resin. However, if possible, it is preferable to use only microfiber cellulose as fine fibers without including cellulose nanofibers. The average fiber diameter of the cellulose nanofibers (average fiber width; average diameter of a single fiber) is preferably 4 to 100 nm, more preferably 10 to 80 nm.
[0155] The fibrous cellulose may also contain pulp. Pulp plays a role in significantly improving the dewaterability of the cellulose fiber slurry. However, as with the cellulose nanofiber, it is most preferable that no pulp is added, that is, that the content is 0 mass%.
[0156] The resin composition can contain, or may contain, in addition to fine fibers and pulp, fibers derived from plant materials obtained from various plants such as kenaf, jute, Manila hemp, sisal, gampi, mitsumata, paper mulberry, banana, pineapple, coconut, corn, sugarcane, bagasse, palm, papyrus, reed, esparto, sabai grass, wheat, rice, bamboo, various coniferous trees (such as cedar and cypress), broad-leaved trees, and cotton.
[0157] For example, one or more of antistatic agents, flame retardants, antibacterial agents, colorants, radical scavengers, foaming agents, etc. may be added to the resin composition within a range that does not impair the effects of the present invention. These raw materials may be added to a dispersion of fibrous cellulose, added when kneading fibrous cellulose and resin, added to a kneaded product thereof, or added by other methods. However, from the viewpoint of production efficiency, it is preferable to add them when kneading fibrous cellulose and resin.
[0158] The resin composition may contain an ethylene-α-olefin copolymer elastomer or a styrene-butadiene block copolymer as a rubber component. Examples of α-olefins include butene, isobutene, pentene, hexene, methyl-pentene, octene, decene, and dodecene. EXAMPLES
[0159] Next, an embodiment of the present invention will be described. A sizing agent was added to the pulp slurry, and the mixture was made into paper in the wire part to a predetermined Cobb sizing degree, and then passed through the press part and the pre-dryer part to produce a paper base material with a predetermined basis weight.
[0160] Next, in the coater part, a paper substrate was coated and impregnated with a urea aqueous solution of a predetermined concentration, and then dried in the after-dryer part to obtain a urea-coated paper. The obtained urea-coated paper was reacted in a roll-to-roll reactor at a predetermined temperature and for a predetermined residence time to obtain a carbamate-modified paper.
[0161] The carbamate-modified paper was then diluted with water to a solids concentration of 5% using a disintegrator and disintegrated. The disintegrated carbamate-modified pulp water dispersion was dehydrated and washed twice. The washed carbamate-modified pulp was beaten in a refiner until the fine ratio (the proportion of fibers with a length distribution of 0.2 mm or less as measured by FS5) reached 40% or more, yielding carbamate-modified microfiber cellulose.
[0162] 1000 g of carbamate-modified microfibrous cellulose adjusted to a solid content concentration of 3.0 mass% was heated and dried using a contact dryer heated to 140°C, and then pulverized in a pulverizer to obtain a carbamate-modified fiber dried product with a moisture content of 3 to 10% and an average particle size of 1100 μm.
[0163] 30 g of dried carbamate-modified fiber was collected in a sealable bag in terms of bone dry weight, and maleic anhydride-modified polypropylene or maleic anhydride-modified polyethylene was added thereto so that the dry weight ratio of the dried carbamate-modified fiber to the maleic anhydride-modified resin was the blend ratio shown in Table 1. The bag was then shaken to mix, and carbamate-modified fiber-containing materials with moisture contents of 3 to 10% were obtained (Test Examples 2 to 4, 6 to 9).
[0164] If necessary, the carbamate-modified fiber-containing material was dried in a thermostatic dryer heated to 105° C. to obtain a carbamate-modified fiber-containing material with a moisture content of 0%. (Test Example 1)
[0165] In addition, a material containing carbamate-modified fiber was left to stand under humid conditions at room temperature to obtain a material containing carbamate-modified fiber with a moisture content of 15% (Test Example 5).
[0166] For comparison, samples were also prepared by the wet mixing method described below (Test Examples 10 to 13).
[0167] To 1000 g of carbamate-modified microfiber cellulose adjusted to a solid content concentration of 3.0 mass%, maleic anhydride-modified polypropylene or maleic anhydride-modified polyethylene was added so that the bone dry weight ratio was the blending ratio shown in Table 1, and after stirring, the mixture was heated and dried using a contact dryer heated to 140°C to obtain a carbamate-modified cellulose fiber-containing material. The moisture content of this carbamate-modified cellulose fiber-containing material (wet mix) was 3 to 10%.
[0168] When maleic anhydride polyethylene was used, the material to be dried covered and adhered to the surface of the contact dryer, preventing the heat source from being transmitted to the material to be dried, and the dryer could not be operated normally.
[0169] The carbamate-modified fiber-containing material obtained in the above manner was melt-kneaded at 160°C to 180°C and 200 rpm using a φ15 mm twin-screw extruder, and then cut into cylindrical shapes with a diameter of 2 mm and a length of 2 mm, to obtain a carbamate-modified fiber composite resin with a fiber loading ratio of 66.7%.
[0170] A carbamate-modified fiber composite resin with a fiber load ratio of 66.7% and PP pellets were dry-blended so that the fiber load ratio after mixing was 10.0%, kneaded in a twin-screw kneader at 180°C and 200 rpm, and cut into cylindrical shapes with a diameter of 2 mm and a length of 2 mm using a pelleter, to obtain a carbamate-modified fiber composite resin with a fiber load ratio of 10%.
[0171] Each carbamate-modified fiber composite resin with a fiber loading rate of 10% was injection molded at 180°C into a rectangular specimen (length 59 mm, width 9.6 mm, thickness 3.8 mm).
[0172] (Effectiveness Test 1) The test was conducted by feeding the dry powdered raw material to be kneaded at a rate of 12 g / min at a rotation speed of 75 rpm using a φ15 mm twin-screw extruder heated to 180° C. One minute after feeding, if the raw material was found to adhere to the bottom of the inner wall of the feeding port, it was marked with an X, and if the raw material was not found to adhere, it was marked with an ◯. The results are shown in Table 1.
[0173] [Table 1]
[0174] (Effectiveness test 2) 1 g of carbamate modified fiber composite resin with a fiber loading rate of 10% was pressed in a heat press at 180°C for 3 minutes to obtain a circular film-like sample for confirming aggregates. The sample for confirming aggregates was cut into a 5 x 5 cm square and the number of aggregates of 0.5 mm or more was visually counted, with 10 or less being rated as ◯, between 10 and 30 being △, and 30 or more being ×. The results are shown in Table 1.
[0175] Incidentally, the reason why the results of Test Examples 8 and 9 were △ is thought to be that MAPP is less likely to melt with heat than MAPE, and while it mixes well with cellulose fibers if it is mixed in a molten state during melt-kneading, MAPE melts the moment it enters the kneader and mixes well with cellulose fibers, while MAPP takes some time to melt after entering the kneader, so the time it spends mixing with cellulose fibers in a molten state is shorter than in the case of MAPE, resulting in poor dispersibility. However, when the fiber:dispersant ratio is high, there is a lot of dispersant between the fibers, so it can be said that it can be sufficiently dispersed even in a short time.
[0176] (Effectiveness Test 3)
[0177] A bending test was conducted using a rectangular specimen injection-molded from a carbamate-modified fiber composite resin with a fiber loading rate of 10%. Bending modulus: In the bending test based on JIS K7171, 2.0 GPa or more was rated as ◯, and less than 2.0 GPa was rated as ×. The results are shown in Table 1. [Industrial Applicability]
[0178] INDUSTRIAL APPLICABILITY The present invention can be used as a method for producing a fibrous cellulose-containing material and a method for producing a fibrous cellulose composite resin.
Claims
1. When cellulose fibers and an additive comprising a resin powder are mixed in a dry state to prepare a fibrous cellulose-containing material, The cellulose fibers are carbamate-treated to have an average fiber length of 0.1 to 0.5 mm and a moisture content of 1 to 10%. A method for producing a fibrous cellulose-containing material, comprising the steps of:
2. The amount of carbamate groups introduced into the cellulose fibers is 0.5 to 2.0 mmol / g. A method for producing the fibrous cellulose-containing material according to claim 1.
3. The temperature of the mixing is 1 to 50° C. A method for producing the fibrous cellulose-containing material according to claim 1.
4. The resin powder is an organic acid anhydride-modified polyolefin. A method for producing the fibrous cellulose-containing material according to claim 1.
5. The average particle size of the resin powder is 1 to 1,000 μm. A method for producing a fibrous cellulose-containing material according to claim 4.
6. The cellulose fibers have an average fiber diameter of 0.1 to 19 μm and a fine ratio of 20 to 45%. A method for producing the fibrous cellulose-containing material according to claim 1.
7. The fibrillation rate of the cellulose fiber is 2.0% or less. A method for producing the fibrous cellulose-containing material according to claim 1.
8. drying the cellulose fibers prior to said mixing; This drying is limited to a range in which the moisture content of the cellulose fibers is 1% or more. A method for producing the fibrous cellulose-containing material according to claim 1.
9. Prior to said mixing, said cellulose fibers are dried to a moisture content of less than 1%; Thereafter, the mixing is performed after the moisture content of the cellulose fibers has returned to 1% or more. A method for producing the fibrous cellulose-containing material according to claim 1.
10. A method for producing a fibrous cellulose-containing material by mixing cellulose fibers and an additive comprising a resin powder in a dry state, and then kneading the fibrous cellulose-containing material or the fibrous cellulose-containing material and a resin to produce a fibrous cellulose composite resin, comprising the steps of: The cellulose fibers are carbamate-treated to have an average fiber length of 0.1 to 0.5 mm and a moisture content of 1 to 10%. A method for producing a fibrous cellulose composite resin comprising the steps of:
Citation Information
Patent Citations
Fibrous cellulose-containing material, fibrous cellulose composite resin, and method for producing fibrous cellulose-containing material
JP2021195405A