Base material for forming resin film and release film
Patent Information
- Application Number
- JP2023077984
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
【0015】 本発明の一態様によれば、高耐熱性と、樹脂膜形成により得られる樹脂膜を剥離できる剥離性を有する樹脂膜形成用基材を提供することができる。
Smart Images

Figure 2024162461000005 
Figure 2024162461000001 
Figure 2024162461000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate for resin film formation and a release film. [Background technology]
[0002] To produce a thermoplastic polyimide film, it is necessary to heat the precursor polyamic acid or a mixture of an acid dianhydride and a diamine that constitutes an imide group to 300°C or higher to imidize it. Since the glass transition temperature of thermoplastic polyimides is generally 300°C or lower, they cannot be treated as a single-layer film at the imidization temperature, and a substrate as a support is required. The substrate used for forming a resin film at such high temperatures needs high heat resistance that can withstand high temperatures and releasability that allows the resin film obtained by resin film formation to be peeled off, but there is a problem that there is no practical substrate.
[0003] As a substrate having high heat resistance and releasability, Patent Document 1 discloses a heat-resistant release sheet having a resin layer having heat resistance and releasability on one or both sides of an expanded graphite sheet, which is used as a carrier sheet in producing a thermoplastic prepreg sheet from a heat-resistant resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-127267 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above-mentioned conventional techniques are not sufficient in terms of both high heat resistance and releasability that allows the resin film obtained by forming the resin film to be peeled off.
[0006] An object of one aspect of the present invention is to provide a substrate for resin film formation having high heat resistance and releasability that allows a resin film obtained by forming a resin film to be peeled off. [Means for solving the problem]
[0007] An embodiment of the present invention includes the following configuration.
[0008] [1] A substrate for forming a resin film, the substrate having a surface for forming a resin film which is a surface of a graphite layer, the ratio (I(D) / I(G)) of a D band intensity I(D) to a G band intensity I(G) in a Raman spectrum of the graphite layer being 0 or more and 0.030 or less, and the thickness of the graphite layer being 5 μm or more.
[0009] [2] The substrate for resin film formation according to [1], wherein the half-value width of the peak corresponding to the 002 plane in X-ray diffraction of the graphite layer is 0.30° or less.
[0010] [3] The density of the graphite layer is 0.10 g / cm 3 More than 2.25g / cm 3 The substrate for resin film formation according to [1] or [2] below.
[0011] [4] The substrate for resin film formation according to any one of [1] to [3], wherein the graphite layer has a thickness of 300 μm or less.
[0012] [5] The substrate for resin film formation according to any one of [1] to [4], which is a graphite sheet.
[0013] [6] A release film, wherein the release surface is a graphite layer, and the ratio (I(D) / I(G)) of D band intensity I(D) to G band intensity I(G) in a Raman spectrum of the graphite layer is 0 or more and 0.030 or less, and the graphite layer has a thickness of 5 μm or more.
[0014] [7] The release film according to [6], wherein the graphite layer has a half-value width of a peak corresponding to a 002 plane in X-ray diffraction of 0.30° or less. Effect of the Invention
[0015] According to one aspect of the present invention, it is possible to provide a substrate for resin film formation having high heat resistance and releasability that allows a resin film obtained by forming a resin film to be peeled off. [Brief description of the drawings]
[0016] [Figure 1] 1 is a photograph showing the state of a polyimide film peeled off from a substrate for resin film formation in an evaluation of the peelability of the polyimide films formed in Example 4 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".
[0018] [1. Base material for resin film formation] As a result of investigations conducted by the present inventors to solve the above problems, they found that a substrate for resin film formation in which the resin film formation surface is the surface of a graphite layer having a predetermined Raman spectrum D band intensity / G band intensity ratio can be suitably used as a substrate for resin film formation having high heat resistance and releasability for peeling off a resin film, even without laminating a heat-resistant and releasable resin layer on one or both sides of an expanded graphite sheet as in the heat-resistant release sheet described in Patent Document 1.
[0019] That is, the substrate for resin film formation according to one embodiment of the present invention is a substrate for resin film formation in which the resin film formation surface is the surface of a graphite layer, and the ratio (I(D) / I(G)) of the D band intensity I(D) to the G band intensity I(G) in the Raman spectrum of the graphite layer is 0 or more and 0.030 or less, and the thickness of the graphite layer is 5 μm or more.
[0020] In this specification, the term "graphite layer" refers to a layer made of graphite, in other words, a layer basically made of a stack of graphene layers made of a plurality of 6-membered carbon rings. The term "graphite sheet" refers to a sheet made of only a single "graphite layer" or two or more layers of "graphite layers" and does not include layers containing other materials.
[0021] In a substrate for resin film formation according to one embodiment of the present invention, the resin film formation surface is a graphite layer surface, and the ratio (I(D) / I(G)) of the D band intensity I(D) to the G band intensity I(G) in the Raman spectrum of the graphite layer is 0 or more and 0.030 or less.
[0022] In the Raman spectrum of graphite, when the graphite structure is disordered and / or defective, the peak top appears at 1580 cm -1 In addition to the G band, which is an absorption peak due to graphite crystals observed near 1300 cm -1 ~1400cm -1In general, the smaller the ratio of the D band intensity I(D) to the G band intensity I(G), the smaller the disorder in the graphite structure.
[0023] In the substrate for resin film formation according to one embodiment of the present invention, it is preferable that the ratio (I(D) / I(G)) of the D band intensity I(D) to the G band intensity I(G) of the graphite layer is within the above range, since this improves the releasability of the resin film obtained by resin film formation. The I(D) / I(G) ratio is more preferably 0 to 0.020, and even more preferably 0 to 0.010.
[0024] In this specification, I(D) / I(G) in the Raman spectrum is a value determined by the method described in the Examples.
[0025] The thickness of the graphite layer is preferably 5 μm or more, since the thickness of the graphite layer is preferably 5 μm or more, and more preferably 10 μm or more, and even more preferably 25 μm or more, since the strength required for the substrate for resin film formation can be obtained.
[0026] The upper limit of the thickness of the graphite layer is, for example, 300 μm or less, but is not limited thereto. If the thickness of the graphite layer is 300 μm or less, both the unrolled graphite layer and the rolled graphite layer have flexibility to be rolled, which is preferable.
[0027] In this specification, the thickness of the graphite layer is a value determined by the method described in the Examples section.
[0028] The substrate for resin film formation according to one embodiment of the present invention may be a substrate for resin film formation in which the surface for resin film formation is a surface of a graphite layer having a thickness of 5 μm or more and having the above-mentioned I(D) / I(G). Thus, the substrate for resin film formation may be a substrate for resin film formation made of a graphite layer having the above-mentioned I(D) / I(G), or a substrate for resin film formation having a multilayer structure in which one or more other layers are laminated on the surface of the graphite layer opposite to the surface for resin film formation.
[0029] In the substrate for resin film formation according to one embodiment of the present invention, the half-width of the peak corresponding to the 002 plane in the X-ray diffraction of the graphite layer is preferably 0.30° or less, more preferably 0.20° or less, and even more preferably 0.15° or less. If the half-width of the peak corresponding to the 002 plane in the X-ray diffraction of the graphite layer is within the above range, it is preferable because the peelability of the resin film obtained by resin film formation is improved. Since the half-width of the peak corresponding to the 002 plane in the X-ray diffraction of the graphite layer is preferably as small as possible, the lower limit is not particularly limited, but is usually 0.05° or more.
[0030] Here, the half-width of the peak is defined as the distance between two points at half the intensity of the maximum peak. The half-width of the peak corresponding to the 002 plane in the X-ray diffraction of the graphite layer is an index of the crystallinity of the graphite layer, and the smaller the half-width, the higher the crystallinity.
[0031] In this specification, the half-value width of the peak corresponding to the 002 plane in X-ray diffraction of the graphite layer is a value determined by the method described in the Examples section.
[0032] In the substrate for resin film formation according to one embodiment of the present invention, the density of the graphite layer is preferably 0.10 g / cm from the viewpoint of reducing the peel strength. 3 More than 2.25g / cm 3 The density of the graphite layer is preferably 0.15 g / cm or less. 3More preferably, it is 0.20 g / cm 3 The density of the graphite layer is more preferably 2.20 g / cm. 3 More preferably, it is 2.15 g / cm or less. 3 The following is the result.
[0033] Examples of the graphite layer include layers made of natural graphite, synthetic graphite, and graphite obtained by carbonizing and graphitizing a polymer film. Among them, the graphite layer is more preferably made of graphite obtained by carbonizing and graphitizing a polymer film, from the viewpoint of facilitating the production of a graphite layer having a desired I(D) / I(G) range. Examples of the polymer film include films made of polyimide, polyamide, polyoxadiazole, polybenzothiazole, polybenzobisthiazole, polybenzoxazole, polybenzobisoxazole, polyparaphenylenevinylene, polybenzimidazole, polybenzobisimidazole, polythiazole, and the like, and films obtained by laminating two or more layers of one or more of these films. Among them, the polymer film is more preferably a film made of polyimide, and a multilayer film of two or more layers made of a film made of polyimide may be used. This is because films made from polyimide are more likely to develop a graphene layer structure through carbonization and graphitization than polymer films made from other organic materials.
[0034] The film made from a polyimide is more preferably a film made from an aromatic polyimide, and among these, an aromatic polyimide prepared from an acid dianhydride (particularly an aromatic acid dianhydride) and a diamine (particularly an aromatic diamine) described below via a polyamic acid is particularly preferred as a polymer raw material for producing the graphite layer used in one embodiment of the present invention.
[0035] Examples of the acid dianhydride that can be used in the synthesis of the aromatic polyimide include pyromellitic anhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, etc. These may be used alone or in combination of two or more.
[0036] Examples of diamines that can be used in the synthesis of the aromatic polyimide include 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 1,4-diaminobenzene, 1,3-diaminobenzene, 1,2-diaminobenzene, etc. These may be used alone or in combination of two or more kinds.
[0037] The polyamic acid can be prepared from the acid dianhydride and diamine by a known method, which is prepared by dissolving at least one aromatic acid dianhydride and at least one diamine in an organic solvent and stirring the resulting solution under controlled temperature conditions until the polymerization of the acid dianhydride and diamine is completed. These polyamic acid solutions are usually obtained at a concentration of 5 to 35 wt%, preferably 10 to 30 wt%.
[0038] The polymer film can be produced by a known method from the raw material or a synthetic raw material thereof. For example, the polyimide can be produced by a thermal curing method in which a precursor polyamic acid is imidized by heating, or a chemical curing method in which a dehydrating agent (dehydration ring-closing agent) such as an acid anhydride such as acetic anhydride and / or a catalyst such as a tertiary amine such as picoline, quinoline, isoquinoline, pyridine, etc. is used as an imidization accelerator, and any of these methods may be used. The film made from the polyimide can be produced by casting an organic solvent solution of the polyamic acid, which is the polyimide precursor, on a support such as an endless belt or a stainless steel drum, and drying and imidizing it.
[0039] The graphite obtained by carbonizing and graphitizing a polymer film can be produced by a method including a carbonization step of carbonizing the polymer film, and a graphitization step of graphitizing the film carbonized in the carbonization step. The polymer film may be carbonized and graphitized as a single film, or as a stack of multiple films. The carbonization step and the graphitization step may be performed continuously or discontinuously. The carbonization step and the graphitization step may be performed in one step without being separated. In the carbonization step, the polymer film, which is the starting material, is preheated under reduced pressure or in an inert gas to carbonize it. This carbonization step is usually performed at a temperature of about 1000°C. The graphitization step following the carbonization step is performed under reduced pressure or in an inert gas. As the inert gas, argon, helium, etc. can be preferably used. The heat treatment temperature for graphitization is preferably 2400° C. or higher, more preferably 2600° C. or higher, even more preferably 2800° C. or higher, and particularly preferably 2900° C. or higher. There is no particular upper limit to the maximum temperature, but it is preferably 3300° C. or lower, and more preferably 3200° C. or lower.
[0040] The graphite layer may be a graphite layer formed by rolling a graphite layer obtained by carbonizing and graphitizing a polymer film. Rolling the graphite layer is preferable because it can impart flexibility to the graphite layer. On the other hand, the graphite layer may be an unrolled graphite layer. If the graphite layer is an unrolled graphite layer, it is preferable because there is a tendency for the graphite layer to have improved releasability, which allows a resin film obtained by forming a resin film on the graphite layer to be peeled off.
[0041] The method for rolling the graphite layer is not particularly limited, and examples thereof include a method for rolling using a metal roll, etc. The rolling step may be carried out in a state in which the produced graphite sheet has been cooled to room temperature, or may be carried out continuously with the graphitization step.
[0042] In the case where the substrate for resin film formation according to one embodiment of the present invention includes another layer in addition to the graphite layer, the other layer may be laminated on the graphite layer. The method for laminating the other layer on the graphite layer is not particularly limited, and for example, a conventionally known method such as a method of laminating the other layer on the graphite layer and then applying pressure while heating, or a method of laminating by pressure without heating can be used.
[0043] [2. Release film] The substrate for resin film formation according to one embodiment of the present invention has high heat resistance and releasability that allows the resin film obtained by resin film formation to be peeled off, and therefore can be used as a release film that can be easily peeled off from a resin layer formed thereon at high temperatures.
[0044] That is, in a release film according to one embodiment of the present invention, the release surface is a graphite layer, the ratio (I(D) / I(G)) of the D band intensity I(D) to the G band intensity I(G) in a Raman spectrum of the graphite layer is 0 or more and 0.030 or less, and the thickness of the graphite layer is 5 μm or more.
[0045] The graphite layer preferably has an X-ray diffraction peak half-width corresponding to the 002 plane of 0.30° or less.
[0046] The configuration, characteristics, production method, etc. of the release film according to one embodiment of the present invention are the same as those described for the substrate for resin film formation, and therefore a description thereof will be omitted here.
[0047] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0048] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these.
[0049] [Evaluation method] The thickness, density, ratio of D band intensity to G band intensity in Raman spectrum, and half-width of the peak corresponding to 002 plane in X-ray diffraction of the graphite sheet used as the substrate for resin film formation in the examples and comparative examples were measured by the following method. Also, the peel strength of the resin film formed on the substrate for resin film formation in the examples and comparative examples was evaluated by the following method.
[0050] (Thickness and density) A substrate for resin film formation cut into a 5 cm square was used as a measurement sample, and the thicknesses of four points located at the four corners of the measurement sample and one point in the center (the intersection of two diagonals) were measured using a micrometer (manufactured by Mitutoyo Corporation, OMV-25MX, measurement surface diameter φ6.3 mm). The average value of the thickness measurements obtained at a total of five points was taken as the thickness of the substrate for resin film formation.
[0051] The mass of the measurement sample was measured. The measured mass value was divided by the volume of the measurement sample calculated using the measured thickness to obtain the density of the substrate for resin film formation.
[0052] (Ratio of D band intensity to G band intensity in Raman spectrum) For the Raman measurements, a Raman microscope, Raman-11, manufactured by Nanophoton Corporation, was used. Measurements were performed using a laser beam with a wavelength of 532 nm, and the G band (1580 cm) derived from graphite crystals was detected. -1 around 1350 cm ), and the D band (1350 cm ) due to the disordered structure. -1 Based on the fitted peaks, the intensity ratio between the G band and the D band (I(D) / I(G)) and the half-width of the G band were calculated.
[0053] For the measurements, five points were randomly selected from three fields of view in the microscope images of one location near the center and two locations near the edges of a graphite sheet cut into a 5 cm square, and measurements were taken at least one point from each field of view, for a total of five points, and the average value of the five points was calculated.
[0054] (Half-width of the peak corresponding to the 002 plane in X-ray diffraction) The half-width of the peak corresponding to the 002 plane in X-ray diffraction was measured using a SmartLab manufactured by Rigaku Corporation. Specifically, the measurement was performed by the focusing method using characteristic X-rays CuKα=1.5418Å at a scan speed of 5° / min, and the half-width of the 002 peak at 2θ=26° was evaluated. A graphite sheet cut into 3 cm squares was used as the measurement sample, and the four corners of the measurement sample were fixed to a sample holder for measurement.
[0055] (Removability of resin film) In the examples and comparative examples, the substrate for resin film formation on which the resin film was formed was cut into a rectangle of 1 inch wide x 5 cm long to be used as a measurement sample. The substrate for resin film formation side of the measurement sample was attached to a stainless steel plate with double-sided tape, and the stainless steel plate was fixed horizontally. Using a 5N force gauge (Imada Co., Ltd., ZTA-5N), the resin film was pulled in the 90° direction at a speed of 300 mm / min to measure the force applied when peeling in the length direction at a width of 1 inch. A graph showing the change in force over time was created, and the average value of the force at the point where the force was stable horizontally was used as the measured value of the peel strength. The measurement was performed twice, and the average value of the two measured values was used as the peel strength.
[0056] The peelability was evaluated according to the following criteria. A: The peel strength is less than 0.5 N / inch, and the resin film can be peeled off over a length of 4 cm without breaking. B: The resin film can be peeled off over 4 cm without breaking, but the peel strength is 0.5 N / inch or more. C: Cannot be peeled off.
[0057] [Substrate for resin film formation] The substrates for resin film formation used in the examples and comparative examples are as follows. 25GS: GRAPHINITY (registered trademark) manufactured by Kaneka Corporation (thickness: 25μm) 32GS: A 62μm thick Apical polyimide film (same composition as Apical AH) after graphitization and rolling process 40GS: GRAPHINITY (registered trademark) manufactured by Kaneka Corporation (thickness: 40 μm) 70GS: GRAPHINITY (registered trademark) manufactured by Kaneka Corporation (thickness: 70 μm) Unrolled GS1: A 62μm thick Apical polyimide film (same composition as Apical AH) after the graphitization process Unrolled GS2: 75μm thick apical polyimide film after graphitization process of NPI Expanded graphite sheet: PERMA-FOIL (registered trademark) manufactured by Toyo Tanso Co., Ltd. (thickness: 0.2 mm) Polyimide film: UBE Corporation, Upilex (registered trademark) 75S (thickness: 75 μm) Aluminum foil: A1N30H-H18 (thickness: 30 μm) Glass plate: AS ONE Corporation, ASLAB (registered trademark) slide glass 1-9647-11 (thickness: 1.0 to 1.2 mm) Table 1 shows the thickness and density of the graphite sheet used as the substrate for forming a resin film in the examples and comparative examples.
[0058] [Table 1]
[0059] In addition, the ratio of the D band intensity to the G band intensity in the Raman spectrum of the graphite sheets used as the substrate for forming a resin film in the examples and comparative examples, and the half-value width of the peak corresponding to the 002 plane in the X-ray diffraction are shown in Table 2 below.
[0060] [Table 2]
[0061] [Example 1] 25GS was used as a substrate for resin film formation, and a resin film of polyimide resin was formed on the substrate for resin film formation.
[0062] (Preparation of polyimide varnish) Phthalic anhydride (PA) (0.0024 mol, 0.36 g), methanol (0.09 mol, 2.88 g), and N-methyl-2-pyrrolidone (NMP) (17.22 g) were added to 4,4'-oxydiphthalic anhydride (ODPA) (0.0288 mol, 8.93 g), and the mixture was stirred at 40°C for 3 hours, after which 3,4'-oxydianiline (3,4'-ODA) (0.03 mol, 6.01 g) was added and the mixture was stirred overnight to obtain a polyimide varnish.
[0063] (Formation of polyimide resin film) The four corners of the substrate for resin film formation cut into 10 cm squares were fixed with polyimide tape to a roll-shaped aluminum foil with a circumference of 30 cm or more and a thickness of 0.030 mm. Then, polyimide varnish was applied to the substrate for resin film formation using a comma coater with a gap adjusted so that the polyimide resin film after imidization was about 25 μm. The substrate for resin film formation coated with polyimide varnish was removed from the aluminum foil and placed on a wire mesh, the four corners were fixed to the wire mesh, and dried in an oven at 100 ° C. for 60 minutes. Then, the substrate for resin film formation coated with the dried polyimide varnish was moved from a low temperature to a high temperature oven in a state fixed to the wire mesh in an oven set at 170 ° C., 250 ° C., and 300 ° C., respectively, and heated for 5 minutes, 1 minute, and 3 minutes, respectively, to advance imidization. After cooling, the peelability between the polyimide resin film and the substrate for resin film formation was evaluated. The results are shown in Table 3.
[0064] [Examples 2 to 6, Comparative Examples 1 to 4] Except for using the substrate for resin film formation shown in Table 3, the same operation as in Example 1 was performed to form a polyimide resin film on the substrate for resin film formation, and the peelability between the polyimide resin film and the substrate for resin film formation was evaluated. In Comparative Example 4 using glass, the same operation as in Example 1 was performed to form a polyimide resin film on the substrate for resin film formation, except that a slide glass was used as it was instead of the substrate for resin film formation cut into 10 cm squares. The results are shown in Table 3.
[0065] [Table 3]
[0066] [Example 7] 25GS was used as a substrate for resin film formation, and a resin film made of phenol resin was formed on the substrate for resin film formation.
[0067] (Formation of phenolic resin film) The four corners of the resin film forming substrate cut into 10 cm squares were fixed to a roll-shaped aluminum foil with a circumference of 30 cm or more and a thickness of 0.030 mm with polyimide tape. Then, a phenolic resin solution (Phenolite (registered trademark) 5010, manufactured by DIC Corporation) was applied to the resin film forming substrate using a comma coater with a gap adjustment so that the resin film of the phenolic resin after curing was about 25 μm. The resin film forming substrate coated with the phenolic resin solution was removed from the aluminum foil, placed on a wire mesh, and the four corners were fixed to the wire mesh and dried in an oven at 70 ° C. for 60 minutes. Then, the resin film forming substrate coated with the dried phenolic resin solution was moved from a low temperature to a high temperature oven in a state fixed to the wire mesh in an oven set at 100 ° C., 130 ° C., 150 ° C., and 180 ° C., respectively, and heated for 30 minutes each to proceed with the curing of the phenolic resin. After cooling, the peelability between the phenol resin film and the substrate for resin film formation was evaluated. The results are shown in Table 4.
[0068] [Examples 8 and 9, Comparative Example 5] A resin film of phenolic resin was formed on the substrate for resin film formation by the same procedure as in Example 7, except that the substrate for resin film formation shown in Table 4 was used, and the peelability between the resin film of phenolic resin and the substrate for resin film formation was evaluated. The results are shown in Table 4.
[0069] [Table 4]
[0070] [summary] As shown in Table 2, the ratio of the D band intensity to the G band intensity in the Raman spectrum of 25GS, 32GS, 40GS, 70GS, unrolled GS1, and unrolled GS2 used as the resin film-forming substrate in Examples 1 to 9 was 0.030 or less. In contrast, the ratio of the D band intensity to the G band intensity in the Raman spectrum of the expanded graphite sheet used as the resin film-forming substrate in Comparative Examples 1 and 5 was 0.036.
[0071] As shown in Tables 3 and 4, in Examples 1 to 6 and 7 to 9 in which a graphite sheet having a ratio of D band intensity to G band intensity of less than 0.030 was used as a substrate for forming a resin film, the peel strength for peeling off the obtained resin layer was small, and a resin film of 4 cm or more could be peeled off without breaking, regardless of whether a polyimide or phenolic resin layer was formed on the substrate for forming a resin film. From these results, it was shown that the substrate for forming a resin film used in the examples has high heat resistance capable of withstanding a high temperature of 300°C and peelability capable of peeling off the resin film. In contrast, in Comparative Examples 1 and 5 in which an expanded graphite sheet, which is a graphite sheet having a ratio of D band intensity to G band intensity of more than 0.030, was used as a substrate for forming a resin film, neither the formed resin layer of polyimide nor the phenolic resin could be peeled off from the substrate for forming a resin film. 1, in the polyimide film 101 peeled off in the peelability evaluation of the polyimide film produced in Example 4, the resin film was peeled off without any breakage, whereas in the polyimide film 102 peeled off in the peelability evaluation of the polyimide film produced in Comparative Example 1, the resin film was broken and graphite was adhered to the resin film, so that the resin film could not be peeled off. In Comparative Examples 2 to 4, in which a substrate on which the resin film was formed was not a graphite layer, the formed resin layer could not be peeled off or required 0.5 N / inch or more for peeling. [Industrial Applicability]
[0072] According to one embodiment of the present invention, a substrate for resin film formation can be provided that has high heat resistance and releasability that allows a resin film obtained by forming a resin film to be peeled off. Therefore, it can be used for forming a resin film at a high temperature and is very useful.
Claims
1. A substrate for resin film formation, the surface on which the resin film is formed is a surface of a graphite layer, a ratio (I(D) / I(G)) of a D band intensity I(D) to a G band intensity I(G) in a Raman spectrum of the graphite layer is 0 or more and 0.030 or less; The substrate for resin film formation, wherein the graphite layer has a thickness of 5 μm or more.
2. 2. The substrate for resin film formation according to claim 1, wherein the half width of a peak corresponding to a 002 plane in an X-ray diffraction of the graphite layer is 0.30° or less.
3. The density of the graphite layer is 0.10 g / cm 3 Above, 2.25g / cm 3 The substrate for resin film formation according to claim 1, which is as follows:
4. The substrate for resin film formation according to claim 1 , wherein the graphite layer has a thickness of 300 μm or less.
5. The substrate for resin film formation according to claim 1 , which is a graphite sheet.
6. the release surface is a graphite layer, and a ratio (I(D) / I(G)) of a D band intensity I(D) to a G band intensity I(G) in a Raman spectrum of the graphite layer is 0 or more and 0.030 or less; The graphite layer has a thickness of 5 μm or more.
7. 7. The release film according to claim 6, wherein the graphite layer has an X-ray diffraction peak corresponding to a 002 plane with a half-value width of 0.30° or less.
Citation Information
Patent Citations
Heat-resistant release sheet and method for manufacturing the sheet
JP2003127267A