Friction material

A friction material using a phenolic resin composition and thermosetting resin as binders addresses manufacturing inefficiencies and performance issues by enhancing curing speed and heat resistance, resulting in a faster and more durable product.

JP2024162484AInactive Publication Date: 2024-11-21AKEBONO BRAKE IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023078023
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing friction materials face challenges in manufacturing efficiency, particularly in thermoforming time, and exhibit reduced performance due to the use of phenolic resins that require hardening post-gelation, and the addition of solid rubber at room temperature affects heat resistance.

Method used

A friction material using a phenolic resin composition comprising novolac type phenolic resin, epoxy resin, and solid resol type phenolic resin, along with a thermosetting resin as binders, to enhance curing speed and heat resistance, thereby shortening thermoforming time and improving wear characteristics.

Benefits of technology

The proposed solution allows for faster manufacturing with improved wear resistance and heat resistance, achieving a friction material with excellent moldability and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162484000001
    Figure 2024162484000001
Patent Text Reader

Abstract

To provide a friction material that shortens thermoforming time and exhibits superior wear properties.SOLUTION: A friction material contains a friction modifier, a binder and a fiber substrate. The binder includes a phenolic resin composition containing a novolac phenolic resin, an epoxy resin, and a solid resol type phenol resin, and a thermosetting resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a friction material, and more particularly to a friction material used for brake pads, brake linings, clutch facings, etc. for industrial machines, railway cars, freight cars, passenger cars, etc. [Background technology]

[0002] Friction materials are used in brakes such as disk brakes and drum brakes, or clutches, and perform braking by friction with a mating material such as a disk rotor.

[0003] Friction materials are made up of raw materials such as a fibrous base material that acts as a reinforcement, a friction modifier that imparts friction and adjusts the friction performance, and a binder that binds these components together.

[0004] Various resin materials can be used as the binder. For example, Patent Document 1 describes a friction material containing 5 to 25 volume % of phenolic resin powder with an average particle size of 10 μm or less as the binder. Patent Document 2 describes a brake friction material containing 6.0 to 6.6 mass % of unmodified phenolic resin and 1 to 2 mass % of unvulcanized nitrile rubber powder as the binder.

[0005] On the other hand, from the viewpoint of manufacturing efficiency, it is desired to shorten the thermoforming time.For example, Patent Document 3 describes a method for manufacturing a friction material, which includes (a) a step of mixing raw materials including a fibrous material, a friction modifier, and a binder to obtain a raw material mixture, (b) a step of adding a solid rubber at room temperature to a part of the raw material mixture to cover the raw material mixture, (c) a step of further adding and mixing the remaining part of the raw material mixture to obtain a friction material composition, and (d) a step of pressure molding the friction material composition at 0 to 100°C, and the pressure molding is performed in a few seconds to a few tens of seconds. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2002-097286 A [Patent Document 2] JP 2008-057693 A [Patent Document 3] JP 2011-075107 A Summary of the Invention [Problem to be solved by the invention]

[0007] Friction materials are generally produced by mixing raw materials such as a fiber base material, a friction modifier, and a binder, thermoforming the mixture into a predetermined shape, and then heat treating and processing the mixture. The phenolic resins described in Patent Documents 1 and 2 require the resin to gel before curing during thermoforming, and therefore require time for thermoforming, leaving room for improvement.

[0008] In addition, in the manufacturing method described in Patent Document 3, pressure molding is performed in a few seconds to a few tens of seconds, but since it is necessary to add rubber that is solid at room temperature to part of the raw material mixture, there is a concern that the heat resistance may decrease.

[0009] An object of the present invention is to provide a friction material which can be thermoformed in a short time and has good wear characteristics. [Means for solving the problem]

[0010] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by using a specific phenolic resin composition and a thermosetting resin together as a binder.

[0011] That is, the present invention relates to the following friction material. A friction material comprising a friction modifier, a binder and a fibrous base material, The friction material contains, as the binder, a phenolic resin composition containing a novolac-type phenolic resin, an epoxy resin, and a solid resol-type phenolic resin, and a thermosetting resin. Effect of the Invention

[0012] According to the present invention, it is possible to provide a friction material which can shorten the thermoforming time and has excellent wear characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The friction material of the present invention will be described in detail below.

[0014] The friction material of the present invention is a friction material comprising a friction modifier, a binder and a fibrous base material, and the binder comprises a phenolic resin composition containing a novolac-type phenolic resin, an epoxy resin, and a solid resol-type phenolic resin, and a thermosetting resin.

[0015] <Friction adjustment material> Friction modifiers are used to impart desired friction characteristics, such as wear resistance, heat resistance, and fade resistance, to the friction material. Examples of friction modifiers include inorganic fillers, organic fillers, abrasives, solid lubricants, and metal powders.

[0016] Examples of inorganic fillers include titanates such as potassium titanate, lithium titanate, lithium potassium titanate, sodium titanate, calcium titanate, magnesium titanate, and magnesium potassium titanate, as well as inorganic materials such as barium sulfate, calcium carbonate, calcium hydroxide, vermiculite, and mica. These may be used alone or in combination of two or more.

[0017] The inorganic filler is preferably used in an amount of 30 to 80 mass %, more preferably 40 to 70 mass %, based on the entire friction material.

[0018] Examples of organic fillers include various rubber powders (raw rubber powder, tire powder, etc.), rubber dust, resin dust, cashew dust, tire tread, melamine dust, etc. These may be used alone or in combination of two or more.

[0019] The organic filler is preferably used in an amount of 1 to 15 mass %, more preferably 1 to 10 mass %, based on the entire friction material.

[0020] Examples of the abrasive include zirconium oxide, alumina, silica, magnesium oxide, zirconia, zirconium silicate, chromium oxide, iron oxide trioxide (Fe3O4), chromite, etc. These may be used alone or in combination of two or more.

[0021] The abrasive is preferably used in an amount of 1 to 20 mass %, more preferably 3 to 15 mass %, based on the total mass of the friction material.

[0022] Examples of solid lubricants include graphite, coke, antimony trisulfide, molybdenum disulfide, tin sulfide, polytetrafluoroethylene (PTFE), etc. These may be used alone or in combination of two or more.

[0023] The solid lubricant is preferably used in an amount of 1 to 25 mass %, more preferably 3 to 20 mass %, of the entire friction material.

[0024] Examples of metal powders include powders of aluminum, tin, zinc, etc. These may be used alone or in combination of two or more.

[0025] The metal powder is preferably used in an amount of 1 to 10 mass %, more preferably 1 to 5 mass %, based on the entire friction material.

[0026] The total content of friction modifiers in the friction material may be appropriately adjusted depending on the desired friction characteristics. The total amount of friction modifiers is preferably 60 to 90 mass % and more preferably 65 to 85 mass % of the total friction material.

[0027] <Fiber base material> The fiber base material is used for reinforcing the friction material. Examples of the fibrous substrate include organic fibers, inorganic fibers, metal fibers, etc. The fibrous substrates may be used alone or in combination of two or more kinds.

[0028] Examples of organic fibers include aromatic polyamide (aramid) fibers and flame-resistant acrylic fibers.

[0029] Examples of inorganic fibers include biosoluble inorganic fibers, ceramic fibers, glass fibers, carbon fibers, rock wool, etc. Examples of biosoluble inorganic fibers include biosoluble ceramic fibers such as SiO2-CaO-MgO fibers, SiO2-CaO-MgO-Al2O3 fibers, and SiO2-MgO-SrO fibers, and biosoluble rock wool.

[0030] The metal fibers include, for example, steel fibers. It is preferable not to use copper fibers or bronze fibers that contain copper.

[0031] From the viewpoint of ensuring the strength of the friction material, the content of the fibrous base material in the friction material is preferably 3 to 30 mass % of the total amount of the fibrous base material, and more preferably 5 to 20 mass %.

[0032] <Binding material> The binder is used to bind the fibrous base material and the friction modifier contained in the friction material together. The friction material according to the embodiment of the present invention contains a phenolic resin composition (hereinafter also referred to as a "specific phenolic resin composition") containing a novolac-type phenolic resin, an epoxy resin, and a solid resol-type phenolic resin, and a thermosetting resin as a binder. The specific phenolic resin composition has the advantage of being fast curing and capable of shortening the thermoforming time, but the heat resistance of the friction material is insufficient. By using the specific phenolic resin composition in combination with a thermosetting resin, the thermoforming time can be shortened and a friction material having good wear characteristics can be obtained. This is thought to be because the use of a thermosetting resin with excellent heat resistance in combination allows the friction material to be manufactured without impairing the moldability.

[0033] The novolac-type phenolic resin used in the specific phenolic resin composition is usually obtained by reacting phenols and aldehydes in the presence of an acid catalyst such as hydrochloric acid or sulfuric acid at a reaction molar ratio (F / P) of phenols (P) to aldehydes (F) of 0.5 to 0.9.

[0034] The phenols are not particularly limited, and examples thereof include phenol, orthocresol, meta-cresol, para-cresol, xylenol, para-tertiary butylphenol, para-octylphenol, para-phenylphenol, bisphenol A, bisphenol F, and resorcinol. Usually, phenol and cresol are often used. Similarly, the aldehydes are not particularly limited, and examples thereof include aldehydes such as formaldehyde, acetaldehyde, butylaldehyde, and acrolein, or mixtures thereof. Although substances that are sources of these aldehydes or solutions of these aldehydes can be used, formaldehyde is usually used. The form of the novolac-type phenolic resin thus obtained is not particularly limited, and any form such as liquid, solid, or powder can be used.

[0035] The amount of the novolac phenolic resin in the specific phenolic resin composition is not particularly limited, but is preferably 50 to 95 mass % and more preferably 60 to 90 mass % based on the total composition. If the amount of the novolac phenolic resin is equal to or less than the upper limit, the composition is sufficiently cured, and if it is equal to or more than the lower limit, the resin is not cured too quickly and the fluidity during molding is not reduced, so that the mechanical strength of the friction material is good.

[0036] The epoxy resin used in the specific phenolic resin composition is not particularly limited, but may be any resin having at least two epoxy groups in one molecule and being solid or liquid at room temperature, such as bisphenol A type, bisphenol S type, phenol novolac type, cresol novolac type, biphenyl type, naphthalene type, aromatic amine type, etc. These may be used alone or in combination.

[0037] The amount of the epoxy resin in the specific phenolic resin composition is not particularly limited, but is preferably 1 to 50 mass % and more preferably 5 to 40 mass % based on the total amount of the composition. If the amount of the epoxy resin is within this range, the resin component is sufficiently cured, and sufficient mechanical strength as a friction material is obtained.

[0038] The solid resol-type phenolic resin used in the specific phenolic resin composition is usually prepared by reacting phenols and aldehydes in the presence of an alkaline catalyst such as an alkali metal hydroxide, a tertiary amine, an alkaline earth metal oxide or hydroxide, or an alkaline substance, such that the reaction molar ratio (F / P) of the aldehydes (F) to the phenols (P) is preferably 0.7 to 3.0, and more preferably 0.9 to 1.8.

[0039] The phenols used here are not particularly limited, but examples thereof include phenols such as phenol, orthocresol, meta-cresol, para-cresol, xylenol, para-tertiary butylphenol, para-octylphenol, para-phenylphenol, bisphenol A, bisphenol F, and resorcin, and phenol and cresol are usually used. Similarly, the aldehydes are not particularly limited, but examples thereof include aldehydes such as formaldehyde, acetaldehyde, butylaldehyde, and acrolein, or mixtures thereof. Substances that are sources of these aldehydes, or solutions of these aldehydes can also be used, but formaldehyde is usually used. The resol-type phenolic resin obtained in this manner is used in the form of a solid.

[0040] The amount of the solid resol type phenolic resin in the specific phenolic resin composition is not particularly limited, but is preferably 1 to 50 mass % and more preferably 5 to 40 mass % based on the total composition. When the amount of the solid resol type phenolic resin is equal to or more than the lower limit, the composition is cured sufficiently, and when the amount is equal to or less than the upper limit, the resin is not cured too quickly and the flowability during molding is not easily reduced, so that the mechanical strength of the cured product is not easily reduced.

[0041] In the present invention, the specific phenolic resin composition can be produced by melt-kneading raw materials including a novolac phenolic resin, an epoxy resin, a curing catalyst, and a solid resol phenolic resin. Here, it is preferable to melt-knead at least the novolac phenolic resin and the epoxy resin and / or the curing agent using a pressurized kneading device. Furthermore, it is more preferable to mix the novolac phenolic resin, the epoxy resin, the curing catalyst, and the solid resol phenolic resin uniformly in a state where the phenolic resin and the epoxy resin do not substantially cure when the novolac phenolic resin, the epoxy resin, the curing catalyst, and the solid resol phenolic resin are melted and flowing. The temperature during mixing is appropriately a temperature at which the phenolic resin and the epoxy resin melt but do not start curing. In addition, by using a pressurized kneading device, it is possible to uniformly disperse the phenolic resin, the epoxy resin, and the curing catalyst.

[0042] As the specific phenolic resin composition, for example, the phenolic resin composition described in JP-A-2008-222851 can be used.

[0043] The friction material according to the embodiment of the present invention contains a thermosetting resin as a binder. A thermosetting resin is a resin that has the property of going from a liquid state to a solid state when heat is applied. By including the specific phenolic resin composition and a thermosetting resin as a binder, the curing speed is increased by the specific phenolic resin composition, so that the time required for thermoforming the friction material can be shortened, and the heat resistance of the thermosetting resin improves the wear resistance of the friction material. Examples of the thermosetting resin include straight phenolic resin, various modified phenolic resins with elastomers, etc., melamine resin, epoxy resin, polyimide resin, etc. Examples of the elastomer-modified phenolic resin include various modified phenolic resins such as acrylic rubber-modified phenolic resin, silicone rubber-modified phenolic resin, and NBR rubber-modified phenolic resin. These thermosetting resins can be used alone or in combination of two or more.

[0044] The mass ratio of the specific phenol resin composition to the thermosetting resin is preferably 3:1 to 1:1, and more preferably 2:1 to 1:1. When the mass ratio is equal to or more than the lower limit, the resin is cured sufficiently quickly, and when the mass ratio is equal to or less than the upper limit, the resin is cured sufficiently, and as a result, a friction material having excellent wear resistance can be obtained even when produced in a short thermoforming time.

[0045] The content of the specific phenolic resin composition in the friction material is preferably 1 to 10 mass %, more preferably 3 to 8 mass %. When the content of the specific phenolic resin composition is equal to or more than the above lower limit, the resin hardening speed is sufficient, and when the content is equal to or less than the above upper limit, the moldability is good, and as a result, a friction material with excellent wear resistance can be obtained even when thermoformed in a short time.

[0046] The content of the thermosetting resin in the friction material is preferably 1 to 7 mass %, more preferably 2 to 6 mass %. When the content of the thermosetting resin is equal to or more than the lower limit, sufficient heat resistance is obtained, and when the content is equal to or less than the upper limit, stable friction characteristics can be obtained. As a result, a friction material with excellent wear resistance can be obtained even when produced in a short thermoforming time.

[0047] When the thermosetting resin is a straight phenol resin, the total content of the phenol resin and the specific phenol resin composition is preferably 1 to 15 mass % in the friction material.

[0048] The binder may contain other resins in addition to the specific phenol resin composition and thermosetting resin described above.

[0049] In order to ensure sufficient mechanical strength and wear resistance, the content of the binder in the friction material is preferably 1 to 20 mass %, and more preferably 3 to 15 mass %.

[0050] The friction material according to the embodiment of the present invention may contain other materials as required in addition to the fiber base material, the friction modifier, and the binder.

[0051] However, from the viewpoint of reducing the environmental load, the friction material according to the embodiment of the present invention does not contain a copper component. "Does not contain a copper component" means that the copper component is substantially not contained, and does not exclude that the copper component is inevitably contained. More specifically, it means that the copper content as an element is 0.5 mass% or less.

[0052] The friction material according to the embodiment of the present invention contains a phenolic resin composition containing a novolac-type phenolic resin, an epoxy resin, and a solid resol-type phenolic resin as a binder, and a thermosetting resin, thereby achieving both a shortened thermoforming time and excellent wear characteristics.

[0053] The friction material of the present invention can be produced by a known production process. For example, the friction material can be produced through processes such as preforming, thermoforming, heating, and polishing of the friction material composition. A method for manufacturing a brake pad having a friction material generally includes the following steps. (a) A process in which a steel plate (pressure plate) is formed into a desired shape using a sheet metal press. (b) A process of degreasing, chemically treating and priming the pressure plate, and applying an adhesive thereto. (c) A process of blending powdered raw materials such as a fiber base material, a friction modifier, and a binder, and mixing the resulting friction material composition to be sufficiently homogenized, and molding the resulting mixture at room temperature under a predetermined pressure to produce a preform. (d) A thermoforming process in which the preform and the pressure plate coated with adhesive are bonded together by applying a predetermined temperature and pressure (forming temperature: 130 to 180°C, forming pressure: 30 to 80 MPa, forming time: 1 to 10 minutes). (e) After-curing (150-300°C, 1-5 hours) and final finishing such as polishing, surface baking, and painting. Through these steps, the friction material according to the embodiment of the present invention can be manufactured. In particular, with regard to the molding time in step (d), conventional friction materials preferably require 4 minutes or more, and more preferably 5 minutes or more, whereas the friction material according to the present embodiment can produce a friction material with excellent moldability and wear resistance even in a molding time of 3 minutes or less.

[0054] Based on the above, the present specification discloses the following friction material. [1] A friction material comprising a friction modifier, a binder and a fibrous base material, The friction material contains, as the binder, a phenolic resin composition containing a novolac-type phenolic resin, an epoxy resin, and a solid resol-type phenolic resin, and a thermosetting resin. [2] The friction material according to [1], wherein a mass ratio of the phenolic resin composition to the thermosetting resin is 3:1 to 1:1. [3] The friction material according to [1] or [2], wherein the content of the phenol resin composition is 1 to 10 mass %. [4] The friction material according to any one of [1] to [3], wherein the content of the thermosetting resin is 1 to 7 mass %. EXAMPLES

[0055] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0056] <Manufacture of friction materials> (Examples 1-2, Comparative Examples 1-2) The ingredients shown in Table 1 were put into a mixer and mixed at room temperature for 4 minutes to obtain a friction material composition. The obtained friction material composition was then subjected to the following steps of (i) preforming, (ii) thermoforming, and (iii) heat treatment to produce brake pads equipped with the friction material. (i) Preforming The mixture was placed in a mold of a preforming press and molded at room temperature at 20 MPa for 10 seconds to prepare a preforming body. (ii) Thermoforming This preform was placed in a thermoforming mold, and a metal plate (pressure plate) to which an adhesive had been applied was placed on top of it, followed by heat and pressure molding at 150° C. and 50 MPa for 2 minutes. (iii) Heat treatment This hot-pressed compact was heat-treated at 250° C. for 3 hours, and then the surface was polished. Next, the surface of this hot-pressed molded body was given a finish coating to obtain a friction material.

[0057] As the phenolic resin composition, a phenolic resin composition manufactured by Sumitomo Bakelite Co., Ltd. (a phenolic resin composition containing a total of 65 mass % of novolac type phenolic resin and solid resol type phenolic resin, and 35 mass % of epoxy resin) was used. As the thermosetting resin, straight phenolic resin was used.

[0058] The obtained friction materials were evaluated for moldability and wear resistance according to the following methods and criteria.

[0059] <Moldability evaluation> The obtained friction materials were inspected by hammering and visually checked for the presence or absence of cracks and blisters, and the yield was calculated. The evaluation criteria are as follows: ○: 100% yield (no cracks or blisters) ×: Yield is less than 100%

[0060] <Wear resistance evaluation> Test pieces (20mm x 30mm) were cut out from the obtained friction material, and a wear resistance evaluation test was carried out under the following conditions using a 1 / 7 scale tester to measure the amount of pad wear. Note that a cast iron rotor (FC200) was used as the mating material. (1) Adjustment: initial speed 50km / h, hydraulic pressure 2.0MPa, rotor temperature at start of braking 100℃, number of braking cycles 200 (2) 300°C wear: initial speed 50km / h, hydraulic pressure 2.0MPa, braking start rotor temperature 300°C, braking count 200 times The amount of pad wear was calculated based on 1,000 braking cycles. The evaluation criteria are as follows: ◎: Less than 0.20g ○: 0.20g or more and less than 0.40g ×: 0.40g or more

[0061] The results of each test are shown in Table 1.

[0062] [Table 1]

[0063] From the above results, it can be seen that the friction materials of Example 1 and Example 2, which contain a phenolic resin composition and a thermosetting resin as a binder, have a yield of 100% and a pad wear amount of 0.40 g or less, and are therefore excellent in both moldability and wear resistance. The friction material of Comparative Example 1, which contained only a phenolic resin composition as a binder, had a low yield and poor moldability, while the friction material of Comparative Example 2, which contained only a thermosetting resin as a binder, had a large pad wear amount and poor wear resistance.

Claims

1. A friction material comprising a friction modifier, a binder and a fibrous base material, The friction material contains, as the binder, a phenolic resin composition containing a novolac-type phenolic resin, an epoxy resin, and a solid resol-type phenolic resin, and a thermosetting resin.

2. 2. The friction material according to claim 1, wherein a mass ratio of the phenolic resin composition to the thermosetting resin is from 3:1 to 1:

1.

3. 3. The friction material according to claim 1, wherein the content of the phenolic resin composition is 1 to 10 mass %.

4. 3. The friction material according to claim 1, wherein the content of the thermosetting resin is 1 to 7 mass %.

Citation Information

Patent Citations

  • Friction material

    JP2002097286A

  • Brake friction material

    JP2008057693A

  • Method for manufacturing friction material

    JP2011075107A