Laminate, method for producing the same, and molded product
A laminate structure with a paper base, adhesive resin, and thermoplastic resin layers addresses adhesion and drying challenges in PHBH-paper integration, enhancing manufacturing efficiency and product quality.
Patent Information
- Application Number
- JP2023078194
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for integrating poly(3-hydroxybutyrate) (PHBH) with paper to form laminates face challenges in achieving sufficient mechanical strength and adhesion, leading to issues like peeling during the manufacturing of cup molded bodies, while also suffering from poor drying properties and quality issues due to prolonged drying times.
A laminate structure comprising a paper base layer, an adhesive resin layer with a specific basis weight and thickness, and a thermoplastic resin layer containing poly(3-hydroxyalkanoate) resin, with a balanced blend of adhesive components, is used to enhance adhesion and drying properties.
The laminate achieves high adhesive strength between the paper base layer and resin layer, improving production efficiency and quality by ensuring good drying properties and reducing manufacturing defects.
Smart Images

Figure 2024162566000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate in which a resin layer is laminated on at least one side of a paper base layer, a method for producing the same, and a molded article. [Background technology]
[0002] In recent years, environmental issues caused by discarded plastics have been attracting attention. In particular, marine pollution caused by discarded plastics is serious, and there are hopes for the widespread use of biodegradable plastics that decompose in the natural environment.
[0003] There are various types of biodegradable plastics known, among which poly(3-hydroxyalkanoate) copolymers (hereinafter sometimes referred to as "P3HA") are thermoplastic polyesters that are produced and accumulated as energy storage substances within the cells of many microbial species, and are materials that can biodegrade not only in soil but also in seawater. For this reason, they have attracted attention as a material that can solve the above problems.
[0004] In particular, the copolymer of 3-hydroxybutyrate (hereinafter sometimes referred to as "3HB") and 3-hydroxyhexanoate (hereinafter sometimes referred to as "3HH") (hereinafter sometimes referred to as "PHBH"), which is a poly(3-hydroxyalkanoate) copolymer, is a thermoplastic polyester that is produced and accumulated as an energy storage substance within the cells of many microbial species, and is a material that can biodegrade not only in soil but also in seawater. Therefore, it has attracted attention as a material that can solve the above problems.
[0005] In particular, PHBH / paper composites, in which PHBH is integrated with a base layer such as paper, have attracted considerable social interest because they can be used in food contact containers and other products that have a low environmental impact.
[0006] Methods for integrating PHBH and paper include extrusion lamination and aqueous slurry coating, but the extrusion lamination method is preferred because the resin layer does not have sufficient mechanical strength when coated. However, PHBH generally has a high melt viscosity and does not penetrate into paper well, so it is not easy to bond the melt-extruded PHBH and paper with sufficient strength. As a result, the laminate layer peels off from the paper during the manufacturing process of cup molded products such as beverage cups, causing problems such as leakage when the contents are filled.
[0007] Patent Document 1 does not disclose PHBH, but it describes a method of applying a polycaprolactone dispersion or emulsion to paper at a rate of 10 g / m for the purpose of improving the penetration of the biodegradable resin into the paper and improving the laminate strength. 2 This method involves applying the coating at a coating weight (dry weight of the layer) of 1000g, drying it, and then laminating 3-hydroxybutyric acid / 3-hydroxyvaleric acid copolymer (PHBV) by extrusion lamination. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 6-293113 Summary of the Invention [Problem to be solved by the invention]
[0009] According to the method of Patent Document 1, the adhesion between the paper and the resin layer tends to be improved, but the dispersion or emulsion of polycaprolactone is added at a concentration of 10 g / m 2 Since the coating is performed at such a large basis weight and then dried, the drying process takes a long time and productivity is low. In addition, there are problems such as deterioration of the paper base layer due to the drying process and warping of the laminate due to the paper being too dry.
[0010] The adhesive layer has a weight of 10g / m to facilitate drying. 2Although there are methods for reducing the amount of the resin layer, such methods pose a problem of insufficient adhesion between the paper base layer and the resin layer.
[0011] In view of the above-mentioned current situation, the present invention aims to provide a laminate comprising, in this order, a paper base layer, an adhesive resin layer, and a resin layer containing a thermoplastic resin that contains an adhesive component and has a poly(3-hydroxybutyrate)-based resin as a main component, which laminate has good drying properties when the adhesive resin layer is formed and has high adhesive strength between the paper base layer and the resin layer. [Means for solving the problem]
[0012] As a result of intensive research into solving the above-mentioned problems, the inventors have discovered that in a laminate comprising, in this order, a base material layer, an adhesive resin layer, and a resin layer containing a thermoplastic resin whose main component is a poly(3-hydroxyalkanoate)-based resin, the above-mentioned problems can be solved by making the basis weight of the adhesive resin layer sufficiently small while also blending a specific adhesive resin component in a specific range into the poly(3-hydroxyalkanoate)-based resin layer, and setting the thickness of the resin layer within a specific range, thereby completing the present invention.
[0013] That is, the present invention provides a laminate comprising a paper base layer (A) and a first adhesive resin layer (B) and a thermoplastic resin layer (C) mainly composed of a poly(3-hydroxyalkanoate)-based resin laminated in this order on at least one surface of the paper base layer (A), The weight of the first adhesive resin layer (B) is 0.1 g / m 2 More than 3.0g / m 2 is less than The average thickness of the thermoplastic resin layer (C) is 20 μm or more and less than 100 μm, The thermoplastic resin layer (C) relates to a laminate containing 0.1 parts by weight or more and less than 10 parts by weight of a second adhesive resin (D) based on 100 parts by weight of a poly(3-hydroxyalkanoate)-based resin.
[0014] The present invention also relates to a method for producing a laminate, the method comprising the steps of: forming a first adhesive resin layer (B) on at least one surface of a base layer (A); The present invention also relates to a method for producing a laminate, which includes a step of forming a thermoplastic resin layer (C) mainly composed of a poly(3-hydroxyalkanoate) resin on the surface of a first adhesive resin layer (B) by extrusion lamination or thermal lamination.
[0015] The present invention further relates to a molded article comprising the laminate. Effect of the Invention
[0016] According to the present invention, it is possible to provide a laminate including, in this order, a base layer, an adhesive resin layer, and a thermoplastic resin layer mainly composed of a poly(3-hydroxyalkanoate)-based resin, which has good drying properties when forming an adhesive layer and has high adhesive strength between the base layer and the resin layer. Use of the laminate can improve the production efficiency and quality of molded articles. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a schematic diagram showing a laminate structure of the laminate according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0019] [Laminate] A laminate according to one embodiment of the present invention has a first adhesive resin layer (B) and a thermoplastic resin layer (C) mainly composed of a poly(3-hydroxyalkanoate)-based resin (hereinafter sometimes referred to as "P3HA") on at least one side of a base layer (A), and the thermoplastic resin layer (C) further contains a second adhesive resin (D). As shown in Fig. 1, in the laminate 1, the base layer (A) indicated by reference numeral 2, the first adhesive resin layer (B) indicated by reference numeral 3, and the thermoplastic resin layer (C) indicated by reference numeral 4 are laminated in this order.
[0020] The first adhesive resin layer (B) may be laminated directly on the base layer (A), or another layer may be further included between the first adhesive resin layer (B) and the base layer (A) as long as the adhesion is not impaired.
[0021] The thermoplastic resin layer (C) may be the outermost layer exposed on the surface of the laminate, or another layer may be laminated on the thermoplastic resin layer (C) for the purpose of imparting water resistance or gloss, etc.
[0022] The first adhesive resin layer (B) and the thermoplastic resin layer (C) may be formed on only one side of the base layer (A), or the first adhesive resin layer (B) and the thermoplastic resin layer (C) may be formed on each of both sides of the base layer (A).
[0023] When the first adhesive resin layer (B) and the thermoplastic resin layer (C) are formed on only one side of the base layer (A), no other layer is formed on the other side, and the base layer (A) may be the outermost layer exposed on the surface of the laminate, or another layer may be laminated thereon for the purpose of imparting water resistance, gloss, or adhesion, etc.
[0024] When the substrate layer (A) has a first adhesive resin layer (B) and a thermoplastic resin layer (C) on each side, the materials constituting the first adhesive resin layer (B) on the front side and the first adhesive resin layer (B) on the back side, as well as the basis weight and thickness, may be the same or different. The same applies to the thermoplastic resin layer (C) on the front side and the thermoplastic resin layer (C) on the back side. In this application, the basis weight (g / m 2 ) refers to the dry weight (solids content) of the layer.
[0025] [Base material layer (A)] The material constituting the substrate layer (A) is not particularly limited, but is preferably biodegradable. Examples include paper (mainly composed of cellulose), cellophane, cellulose ester, polyvinyl alcohol, polyamino acid, polyglycolic acid, pullulan, or a material in which inorganic substances such as aluminum and silica are vapor-deposited on these substrates. Among these, paper is preferred because it is excellent in heat resistance and inexpensive.
[0026] The type of paper is not particularly limited and can be appropriately selected depending on the application of the laminate, and examples include cup base paper, kraft paper, fine paper, coated paper, tissue paper, glassine paper, paperboard, etc. If necessary, a water-resistant agent, a water-repellent agent, an inorganic substance, etc. may be added to the paper, and the paper may be subjected to a surface treatment such as an oxygen barrier layer coating or a water vapor barrier coating.
[0027] The substrate layer (A) may be subjected to a surface treatment such as corona treatment, ozone treatment, plasma treatment, frame treatment, anchor coat treatment, oxygen barrier layer coating, water vapor barrier coating, etc. These surface treatments may be performed alone or in combination.
[0028] [First adhesive resin layer (B)] The first adhesive resin layer (B) is a layer mainly composed of a resin. The main resin contained in the first adhesive resin layer (B) is not particularly limited, but resins generally used in the coated paper field or resin film field can be suitably used. Resins having high affinity with substrates such as paper and P3HA are preferred, and examples of such resins include acrylic resins, methacrylic resins, vinyl chloride resins, styrene-acrylic resins, styrene-butadiene resins, styrene-isoprene resins, polycarbonate resins, urea resins, melamine resins, epoxy resins, phenolic resins, urethane resins, diallyl phthalate resins, and imine resins. These resins can be used alone or in a mixture of two or more resins in any ratio.
[0029] In particular, since they have excellent affinity with P3HA, it is preferable that the first adhesive resin layer (B) contains at least any one of an ester-based or acrylic-based resin, or a styrene-acrylic-based resin.
[0030] The main resin contained in the first adhesive resin layer (B) may be water-soluble or may be soluble in an organic solvent. When using a water-insoluble resin, other additives may be added to improve dispersibility in water and coatability. When coating an aqueous emulsion, an aqueous slurry, or a water-soluble resin, the solid content concentration of the resin is not particularly limited, but is preferably 30% by weight or more, more preferably 40% by weight or more, and even more preferably 50% by weight or more in order to reduce the amount of heat required for drying. In addition, from the viewpoint of avoiding sedimentation of the dispersed resin and achieving good coatability, the solid content concentration is preferably 60% or less.
[0031] The first adhesive resin layer (B) may contain only the main resin as a resin component, or may contain a tackifier resin (E) in addition to the main resin. By using a tackifier resin, the first adhesive resin layer (B) It is possible to reduce the Tg of the entire resin contained in the laminate, and the adhesive strength of the laminate can be further improved.
[0032] The tackifier resin (E) is not particularly limited, and generally used resins can be used. It may be either solid or liquid at room temperature. Specifically, rosin-based resins, terpene-based resins, ethylene-based resins, vinyl acetate-based resins, alkylphenol-formaldehyde-based resins, alkylphenol-acetylene-based resins, coumarone-indene-based resins, styrene-based resins, and xylene-formaldehyde-based resins can be preferably used. These may be used alone or in combination of two or more. In particular, rosin-based resins are preferred.
[0033] The weight average molecular weight (Mw) of the tackifier resin (E) can be appropriately selected, but from the viewpoint of improving adhesive strength, it is preferably 100 or more and less than 5,000, more preferably 200 or more and less than 3,000, even more preferably 300 to 2,000, and particularly preferably 400 to 1,000.
[0034] In the laminate according to this embodiment, the basis weight of the first adhesive resin layer (B) is 0.1 g / m 2 More than 3.0g / m 2 The weight is adjusted to a range of less than 0.1g / m 2 If it is less than 3.0 g / m, the adhesion to the thermoplastic resin layer (C) may decrease. 2 If the drying temperature exceeds this value, a large amount of heat is required during drying, which places a large load on the equipment, and, for example, insufficient drying may cause problems such as blocking during winding of the raw material.
[0035] The weight per unit area is 0.5 g / m 2 More than 2.5g / m 2 It is preferable that the content is 0.8 g / m or less. 2 More than 2.0g / m 2 Less than 1.0 g / m is more preferable. 2 More than 1.5g / m 2 The following is even more preferred:
[0036] [Thermoplastic resin layer (C)] The thermoplastic resin layer (C) contains a poly(3-hydroxyalkanoate) resin as a main component. The main component here means the component that has the largest weight ratio among the resin components forming the thermoplastic resin layer (C). The thermoplastic resin layer (C) may be the outermost layer in the laminate according to this embodiment, and in that case, the thermoplastic resin layer can be used for heat sealing (described later).
[0037] The poly(3-hydroxyalkanoate) resin is a biodegradable aliphatic polyester (preferably a polyester not containing an aromatic ring) and is a copolymer having at least one or more types of 3-hydroxyalkanoate units. The 3-hydroxyalkanoate units are preferably represented by the following general formula (1). [-CHR-CH2-CO-O-] (1) In the general formula (1), R is C p H 2p+1 where p is an integer of 1 to 15. Examples of R include linear or branched alkyl groups such as methyl, ethyl, propyl, methylpropyl, butyl, isobutyl, t-butyl, pentyl, and hexyl. p is preferably 1 to 10, and more preferably 1 to 8.
[0038] The poly(3-hydroxyalkanoate) resin preferably contains 3-hydroxyalkanoate units (particularly units represented by general formula (1)) in an amount of 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more of the total structural units (monomer units). The poly(3-hydroxyalkanoate) resin may contain only two or more kinds of 3-hydroxyalkanoate units as the structural units of the resin, or may contain other units (e.g., 4-hydroxyalkanoate units, etc.) in addition to one or more kinds of 3-hydroxyalkanoate units.
[0039] The poly(3-hydroxyalkanoate) resin is preferably a poly(3-hydroxybutyrate) resin containing 3-hydroxybutyrate (hereinafter sometimes referred to as 3HB) units and other hydroxyalkanoate units.
[0040] The other hydroxyalkanoate units may be 3-hydroxyalkanoate units other than 3HB units, or may be hydroxyalkanoate units other than 3-hydroxyalkanoate units (e.g., 4-hydroxyalkanoate units).The other hydroxyalkanoate units may include only one type, or may include two or more types.
[0041] Specific examples of poly(3-hydroxyalkanoate) resins include poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (abbreviation: PHBV), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: PHBH), poly(3-hydroxy butyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), etc. In particular, from the viewpoint of productivity and mechanical properties of the resin composition, PHBH or P3HB4HB is preferred, and PHBH is particularly preferred.
[0042] By changing the composition ratio of the repeating units, the melting point and degree of crystallinity of PHBH can be altered, and as a result, physical properties such as Young's modulus and heat resistance can be easily adjusted. It is also possible to give PHBH physical properties between those of polypropylene and polyethylene, making it a particularly useful plastic industrially.
[0043] A specific method for producing PHBH is described in, for example, International Publication No. 2010 / 013483. Commercially available PHBH products include Kaneka Biodegradable Polymer Green Planet (registered trademark) manufactured by Kaneka Corporation.
[0044] The average content ratio of each constituent monomer in PHBH is preferably 3HB / 3HH=97-80 / 3-20 (mol% / mol%), and more preferably 3HB / 3HH=94-82 / 6-18 (mol% / mol%). When the average content ratio of 3HH in PHBH is 3 mol% or more, good adhesiveness can be obtained in the heat sealing described below. In addition, when the average content ratio of 3HH is 20 mol% or less, the crystallization rate of PHBH is not too slow, and production is relatively easy.
[0045] The average content ratio of each constituent monomer in PHBH means the molar ratio of 3HB and 3HH contained in PHBH. When PHBH is a mixture of at least two types of PHBH with different content ratios of the constituent monomers, or when PHBH is a mixture containing at least one type of PHBH and PHB, it means the molar ratio of each constituent monomer contained in the entire mixture. The average content ratio of the constituent monomers can be determined by a method known to those skilled in the art, for example, the method described in paragraph
[0047] of International Publication WO 2013 / 147139, or by NMR measurement.
[0046] As described above, the thermoplastic resin layer (C) may contain, as PHBH, at least two types of PHBH having different content ratios of constituent monomers, or may further contain PHB (a homopolymer of 3-hydroxybutyrate) in addition to at least one type of PHBH.
[0047] When at least two types of PHBH are included, it is preferable that the PHBH include a highly crystalline, high melting point PHBH having a 3HH content of less than 6 mol % and a low crystalline, low melting point PHBH having a 3HH content of 15 mol % or more.
[0048] The thermoplastic resin layer (C) is preferably a resin layer containing PHBH as a main component. Specifically, the content of PHBH in the thermoplastic resin layer (C) is preferably 50 to 100% by weight, more preferably 70 to 100% by weight, and further preferably 80 to 100% by weight. The lower limit may be 90% by weight or more, or 95% by weight or more.
[0049] The thermoplastic resin layer (C) may contain only PHBH or only PHBH and PHB as a resin component, or may further contain a resin other than PHBH and PHB in addition to these. The resin other than PHBH and PHB is preferably a biodegradable resin, specifically, poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHB3HV), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (PHB4HB), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) (PHB3HO), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate) (PHB3HOD ... Examples of the resins include poly(3-hydroxyalkanoates) such as poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (PHB3HV3HH), polycaprolactone, polybutylene succinate adipate, polybutylene succinate, and polylactic acid, and aliphatic aromatic polyester resins such as polybutylene adipate terephthalate and polybutylene azelate terephthalate. These resins other than PHBH and PHB may be used alone or in combination of two or more.
[0050] The thermoplastic resin layer (C) contains 0.1 to 10 parts by weight of a second adhesive resin (D) described below, relative to 100 parts by weight of the resin. If the second adhesive resin (D) is 0.1 part by weight or less, the adhesion to the paper substrate is not excellent, and if it is 10 parts by weight or more, the melt tension decreases excessively when the thermoplastic resin is melt-processed, deteriorating the processability, and as a result, dimensional stability such as width and thickness may be lost.
[0051] The thermoplastic resin layer (C) may contain additives that are usually added to resin materials, as long as they do not impair the effects of the invention. Examples of such additives include inorganic fillers, colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather resistance improvers, UV absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, and sliding property improvers. These additives may be used alone or in combination of two or more. However, the additives are optional components, and the thermoplastic resin layer (C) may not contain these additives. As the additives, it is preferable to use lubricants and / or inorganic fillers from the viewpoint of improving the peelability from the pressure bonding surface of a cooling roll or the like during lamination of the thermoplastic resin layer (C).
[0052] Examples of the lubricant include saturated or unsaturated fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, oleic acid amide, and erucic acid amide; alkylene fatty acid amides such as methylene bisstearic acid amide and methylene bisstearic acid amide; and aliphatic amide compounds; and pentaerythritol.
[0053] The amount of the lubricant in the thermoplastic resin layer (C) is preferably 0.1 to 2 parts by weight, more preferably 0.2 to 1 part by weight, based on 100 parts by weight of the total amount of the resin components contained in the thermoplastic resin (C) layer. By making the amount 0.1 part by weight or more, it is possible to obtain an effect of improving the releasability by adding the lubricant. If the amount is 2 parts by weight or less, the problem of the lubricant bleeding out during compression and adhering to the compression surface of the cooling roll or the like can be suppressed, and long-term continuous processing can be performed.
[0054] Examples of the inorganic filler include talc, calcium carbonate, mica, silica, clay, kaolin, titanium oxide, alumina, zeolite, etc. The average particle size of these inorganic fillers is preferably 0.5 μm or more.
[0055] The amount of inorganic filler in the thermoplastic resin layer (C) is preferably 0.5 to 5 parts by weight, more preferably 1 to 3 parts by weight, based on 100 parts by weight of the total amount of the resin components contained in the thermoplastic resin layer. By making the amount 0.5 parts by weight or more, it is possible to obtain an effect of improving the peelability by adding the inorganic filler. When the amount is 5 parts by weight or less, it is possible to suppress the occurrence of cracks in the thermoplastic resin layer (C).
[0056] In the laminate according to this embodiment, the thickness of the thermoplastic resin layer (C) is set in the range of 20 μm or more and 100 μm or less. If the thickness is less than 5 μm, the resin is cooled too quickly during lamination of the thermoplastic resin layer (C), and the adhesion to the base layer on which the first adhesive resin layer (B) is formed may decrease. In addition, cracks are likely to occur in the thermoplastic resin layer when the laminate is processed into a molded product. The lower limit of the thickness is preferably 25 μm or more, more preferably 30 μm or more.
[0057] Furthermore, if the thickness of the thermoplastic resin layer (C) exceeds 100 μm, the resin temperature may vary greatly during the formation of the thermoplastic resin layer (C), resulting in uneven thickness and poor appearance due to melt fracture. In addition, the laminate may become too hard, resulting in molding defects. The upper limit of the thickness is preferably 80 μm or less, more preferably 60 μm or less.
[0058] [Second adhesive resin (D)] The main resin contained in the second adhesive resin (D) is not particularly limited, but resins generally used in the coated paper field or resin film field can be suitably used. Resins having high affinity with substrates such as paper and P3HA are preferred, and examples of such resins include acrylic resins, methacrylic resins, vinyl chloride resins, styrene-acrylic resins, styrene-butadiene resins, styrene-isoprene resins, polycarbonate resins, urea resins, melamine resins, epoxy resins, phenolic resins, urethane resins, diallyl phthalate resins, and imine resins. These resins can be used alone or in a mixture of two or more resins in any ratio.
[0059] In particular, since they have excellent affinity with P3HA, it is preferable that the second adhesive resin (D) contains at least any one of an ester-based or acrylic-based resin, or a styrene-acrylic-based resin.
[0060] [Method for producing laminate] An example of a method for producing the laminate according to this embodiment will be described below.
[0061] The laminate according to this embodiment can be produced by forming a first adhesive resin layer (B) on at least one side of a base layer (A) (first step), and then forming a thermoplastic resin layer (C) on the surface of the first adhesive resin layer (B) thus formed (second step).
[0062] In the first step of forming the first adhesive resin layer (B) on at least one side of the base layer (A), it is preferable to apply a solution or an aqueous dispersion such as an aqueous slurry containing the components constituting the first adhesive resin layer (B) to one or both sides of the base layer (A), and heat and dry to form a film.
[0063] The method of applying the solution or aqueous dispersion to the substrate is not particularly limited, and any known method capable of forming a resin layer on the substrate can be appropriately used.Specifically, the spraying method, the scattering method, the slit coater method, the air knife coater method, the roll coater method, the bar coater method, the comma coater method, the blade coater method, the screen printing method, the gravure printing method, etc. can be used.Before applying the solution or aqueous dispersion, the substrate may be subjected to a surface treatment such as the above-mentioned corona treatment.
[0064] The drying treatment after coating can be carried out using a known heating method, such as hot air heating, infrared heating, microwave heating, roll heating, hot plate heating, etc., which can be used alone or in combination of two or more kinds.
[0065] Next, a second step is performed to form a thermoplastic resin layer (C) on the surface of the formed first adhesive resin layer (B). The method for forming the thermoplastic resin layer (C) may be a method of applying a solution or aqueous dispersion containing components constituting the thermoplastic resin layer (C) to the surface of the first adhesive resin layer (B), heating, drying and forming a film. However, from the viewpoint of adhesion with the first adhesive resin layer (B), productivity, or quality for suppressing thermal deterioration, it is preferable to form the thermoplastic resin layer (C) on the surface of the first adhesive resin layer (B) by extrusion lamination or thermal lamination.
[0066] The extrusion lamination method may be a general extrusion lamination method. Specifically, a molten resin material is extruded from a T-shaped die into a film shape, and is pressed onto the surface of the first adhesive resin layer (B) while being cooled using a cooling roll, and immediately thereafter, the resin material is peeled off from the cooling roll to form a thermoplastic resin layer (C) and produce a laminate.
[0067] When the thermoplastic resin layer (C) is formed by the extrusion lamination method, the temperature of the resin immediately after being melt-extruded from the tip of the T-shaped die is preferably equal to or higher than the melting point of the poly(3-hydroxyalkanoate) resin contained as the main component in the thermoplastic resin layer (C) and lower than 165° C. The melting point here refers to the peak temperature in the melting (endothermic) curve obtained when the temperature is increased at a rate of 10° C. / min in differential scanning calorimetry (DSC method).
[0068] The thermal lamination method may be a general thermal lamination method. Specifically, a molten resin material is extruded, for example, from a T-shaped die, and cooled using a cooling roll to form a film containing the resin material. The resulting film is then pressed onto the surface of the first adhesive resin layer (B) using a heat roll or the like to produce a molded product.
[0069] When forming the thermoplastic resin layer (C) by the thermal lamination method, it is preferable that when forming the film constituting the thermoplastic resin layer (C), the resin temperature immediately after being melt-extruded from the tip of the T-shaped die is equal to or higher than the melting point of the poly(3-hydroxyalkanoate) resin contained as the main component in the thermoplastic resin layer (C) and lower than 165°C.
[0070] For the purpose of improving the adhesion between the thermoplastic resin layer (C) and the base layer (A) on which the first adhesive resin layer (B) is formed, the surface of the first adhesive resin layer (B) may be subjected to corona treatment, frame treatment, ozone treatment, etc.
[0071] From the viewpoint of adhesion and processability (balance between melting and crystallization), the first and second steps are preferably carried out successively.
[0072] [Molded body] The molded article according to one aspect of the present embodiment includes the laminate described above and has a desired size and shape. The molded article is formed from a laminate including a thermoplastic resin layer (C), and is therefore advantageous in various applications.
[0073] The molded article is not particularly limited as long as it contains the laminate, and examples thereof include paper, film, sheet, tube, plate, rod, container (e.g., bottle container), bag, part, etc. From the viewpoint of measures against marine pollution, the molded article is preferably a bag or a bottle container.
[0074] The molded article may be the laminate itself, or may be a product obtained by subjecting the laminate to secondary processing.
[0075] Since the laminate is subjected to secondary processing, the molded article can be suitably used as various packaging container materials such as shopping bags, various bags, food and confectionery packaging materials, cups, trays, cartons, etc. (in other words, in various fields such as food, cosmetics, electronics, medicine, and pharmaceuticals.) Since the molded article includes a thermoplastic resin layer (C) having high adhesion to a substrate and good heat resistance, it can be more suitably used as a container for holding liquids, particularly as a container for holding hot contents such as cups for food and drink such as instant noodles, instant soup, and coffee, trays for prepared foods, lunch boxes, and microwave foods.
[0076] The secondary processing can be carried out in the same manner as conventional resin-laminated paper or coated paper, i.e., using various bag-making machines, filling and packaging machines, etc. Processing can also be carried out using devices such as paper cup forming machines, punching machines, and box making machines. In these processing machines, known techniques can be used for bonding the laminate, such as heat sealing, impulse sealing, ultrasonic sealing, high-frequency sealing, hot air sealing, and frame sealing.
[0077] The heat seal temperature of the laminate varies depending on the adhesion method, but for example, when a heat-sealing tester having a seal bar is used, the resin temperature is usually set to 180°C or less, preferably 170°C or less, and more preferably 160°C or less. Within the above range, melting of the resin near the sealed portion can be avoided, and an appropriate resin layer thickness and seal strength can be ensured. In addition, the lower limit of the resin temperature when a heat-sealing tester having a seal bar is used is usually 100°C or more, preferably 110°C or more, and more preferably 120°C or more. Within the above range, appropriate adhesion at the sealed portion can be ensured.
[0078] The heat seal pressure of the laminate varies depending on the adhesion method, but for example, when a heat seal tester having a seal bar is used, it is usually 0.1 MPa or more, preferably 0.5 MPa or more. Within the above range, appropriate adhesion at the sealed portion can be ensured. Furthermore, the upper limit of the heat seal pressure when a heat seal tester having a seal bar is used is usually 1.0 MPa or less, preferably 0.75 MPa or less. Within the above range, thinning of the film thickness at the sealed end can be avoided, and the seal strength can be ensured.
[0079] In order to improve the physical properties of the molded article, the molded article can be composited with another molded article made of a material different from the molded article (e.g., fiber, thread, rope, woven fabric, knitted fabric, nonwoven fabric, paper, film, sheet, tube, plate, rod, container, bag, part, foam, etc.). These materials are also preferably biodegradable.
[0080] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] A laminate comprising a paper base layer (A) and a first adhesive resin layer (B) and a thermoplastic resin layer (C) mainly composed of a poly(3-hydroxyalkanoate) resin, laminated in this order on at least one surface of the paper base layer (A); The weight of the first adhesive resin layer (B) is 0.1 g / m 2 More than 3.0g / m 2 is less than The average thickness of the thermoplastic resin layer (C) is 20 μm or more and less than 100 μm, The thermoplastic resin layer (C) comprises 0.1 parts by weight or more and less than 10 parts by weight of a second adhesive resin (D) based on 100 parts by weight of a poly(3-hydroxyalkanoate)-based resin. [Item 2] Item 2. The laminate according to item 1, wherein the first adhesive resin layer (B) contains at least one resin selected from the group consisting of ester-based resins, acrylic or methacrylic resins, vinyl chloride-based resins, styrene-acrylic resins, styrene-butadiene-based resins, styrene-isoprene-based resins, polycarbonate-based resins, urea resins, melamine-based resins, epoxy-based resins, phenol-based resins, urethane-based resins, diallyl phthalate-based resins, and imine-based resins. [Item 3] 3. The laminate according to item 1 or 2, wherein the second adhesive resin (D) contains at least one resin selected from the group consisting of ester-based resins, acrylic or methacrylic resins, vinyl chloride-based resins, styrene-acrylic resins, styrene-butadiene-based resins, styrene-isoprene-based resins, polycarbonate-based resins, urea resins, melamine-based resins, epoxy-based resins, phenol-based resins, urethane-based resins, diallyl phthalate-based resins, and imine-based resins. [Item 4] The laminate according to any one of items 1 to 3, wherein the first adhesive resin layer (B) contains at least one tackifying resin (E) selected from the group consisting of rosin-based resins, terpene-based resins, ethylene-based resins, vinyl acetate-based resins, alkylphenol-formaldehyde-based resins, alkylphenol-acetylene-based resins, coumarone-indene-based resins, styrene-based resins, and xylene-formaldehyde-based resins. [Item 5] 5. The laminate according to item 4, wherein the tackifying resin (E) has a weight average molecular weight (Mw) of 100 or more and less than 5,000. [Item 6] 6. The laminate according to any one of items 1 to 5, wherein the poly(3-hydroxyalkanoate)-based resin is a poly(3-hydroxybutyrate)-based resin. [Item 7] 7. The laminate according to any one of items 1 to 6, wherein the poly(3-hydroxyalkanoate)-based resin is poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). [Item 8] A method for producing a laminate according to any one of items 1 to 7, forming the first adhesive resin layer (B) on at least one surface of the base layer (A); A method for producing a laminate, comprising the step of forming the thermoplastic resin layer (C) on a surface of the first adhesive resin layer (B) by extrusion lamination or thermal lamination. [Item 9] 9. The method for producing a laminate according to item 8, wherein, when the thermoplastic resin layer (C) is formed by the extrusion lamination method, the temperature of the resin immediately after being melt-extruded from the tip of a T-shaped die is equal to or higher than the melting point of a poly(3-hydroxyalkanoate)-based resin contained as a main component in the thermoplastic resin layer (C) and lower than 165°C. [Item 10] Item 9. The method for producing a laminate according to item 8, wherein in the thermal lamination method, a film constituting the thermoplastic resin layer (C) is used, and the film is a film formed at a resin temperature immediately after melt extrusion from the tip of a T-shaped die of not less than the melting point of a poly(3-hydroxyalkanoate)-based resin contained as a main component in the thermoplastic resin layer (C) and not more than 165°C. [Item 11] A molded article comprising the laminate according to any one of items 1 to 10. EXAMPLES
[0081] The present invention will be specifically described below with reference to examples, but the technical scope of the present invention is not limited to these examples.
[0082] [Production Example] (Method of preparing coating liquid) Coating solution 1: Styrene / methyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid (all manufactured by Tokyo Chemical Industry Co., Ltd.) were polymerized to a molar ratio of 10 / 81 / 3 / 6, and then diluted with a water / isopropanol mixture to a solid content of 5%, to obtain coating solution 1 made of an acrylic-type styrene resin.
[0083] Coating solution 2: Methyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid (all manufactured by Tokyo Chemical Industry Co., Ltd.) were polymerized to a molar ratio of 91 / 3 / 6, and then diluted with a water / isopropanol mixture to a solid content of 5% to obtain coating solution 2.
[0084] Coating liquid 3: After polymerization to a molar ratio of styrene / methyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid (all manufactured by Tokyo Chemical Industry Co., Ltd.) = 10 / 81 / 3 / 6, the coating liquid was obtained by diluting with a water / isopropanol mixture to a solid content concentration of 5%. Then, a solution in which rosin ester (RE-650 manufactured by Arakawa Chemical Industries Co., Ltd., weight average molecular weight 600) was dissolved in a toluene / isopropanol mixture was mixed so that the rosin ester was 5 wt% of the total amount of styrene-acrylic resin and rosin ester, and coating liquid 3 was obtained.
[0085] Coating liquid 4: After polymerization to a molar ratio of styrene / methyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid (all manufactured by Tokyo Chemical Industry Co., Ltd.) = 10 / 81 / 3 / 6, the coating liquid was obtained by diluting with a water / isopropanol mixture to a solid concentration of 15%. Then, a solution in which rosin ester (RE-650 manufactured by Arakawa Chemical Industries Co., Ltd., weight average molecular weight 600) was dissolved in a toluene / isopropanol mixture was mixed so that the rosin ester was 5 wt% of the total amount of styrene-acrylic resin and rosin ester, and coating liquid 4 was obtained.
[0086] Coating liquid 5: After polymerization to a molar ratio of styrene / methyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid (all manufactured by Tokyo Chemical Industry Co., Ltd.) = 10 / 81 / 3 / 6, the coating liquid was obtained by diluting with a water / isopropanol mixture to a solid content concentration of 5%. Then, a solution in which rosin ester (RE-2160 manufactured by Arakawa Chemical Industries Co., Ltd., weight average molecular weight 2160) was dissolved in a toluene / isopropanol mixture was mixed so that the rosin ester was 5 wt% of the total amount of styrene-acrylic resin and rosin ester, and coating liquid 5 was obtained.
[0087] (PHBH Powder) The PHBH powder used was manufactured in accordance with the method described in International Publication No. 2019-142845. The specific formulation is as follows.
[0088] PHBH powder: PHBH powder with a weight-average molecular weight of 590,000 and a ratio of 3HH to the total of 3HB and 3HH in PHBH of 15 mol%. (PHBH pellet manufacturing method) PHBH pellet 1: The PHBH powder (100 parts by weight) was dry-blended with behenamide (0.5 parts by weight), pentaerythritol (1.0 part by weight), and acrylic-styrene resin (5.0 parts by weight) obtained by drying the coating liquid 1, and the mixture was melt-kneaded and extruded into strands using a twin-screw extruder at a set temperature of 150°C and a screw rotation speed of 100 rpm, and then passed through hot water at 40°C to solidify and cut into pellets. The weight-average molecular weight was 550,000, and the melting point was 150°C. PHBH pellet 2: The PHBH powder (100 parts by weight) was dry-blended with behenamide (0.5 parts by weight), pentaerythritol (1.0 part by weight), and acrylic-styrene resin (1.5 parts by weight) obtained by drying the coating liquid 1, and the mixture was melt-kneaded and extruded into strands using a twin-screw extruder at a set temperature of 150°C and a screw rotation speed of 100 rpm, and then passed through hot water at 40°C to solidify and cut into pellets. The weight-average molecular weight was 550,000, and the melting point was 150°C. PHBH pellet 3: The PHBH powder (100 parts by weight) was dry-blended with behenamide (0.5 parts by weight), pentaerythritol (1.0 part by weight), and acrylic-styrene resin (9.0 parts by weight) obtained by drying the coating liquid 1, and the mixture was melt-kneaded and extruded into strands using a twin-screw extruder at a set temperature of 150°C and a screw rotation speed of 100 rpm, and then passed through hot water at 40°C to solidify and cut into pellets. The weight-average molecular weight was 550,000, and the melting point was 150°C. PHBH pellet 4: The PHBH powder (100 parts by weight) was dry-blended with behenamide (0.5 parts by weight) and pentaerythritol (1.0 parts by weight), and the mixture was melt-kneaded and extruded into strands at a set temperature of 150°C and a screw speed of 100 rpm using a twin-screw extruder, solidified by passing through hot water at 40°C, and cut into pellets. The weight-average molecular weight was 550,000, and the melting point was 150°C.
[0089] [Evaluation method] The evaluations in the examples and comparative examples were carried out by the following methods.
[0090] (Evaluation of Laminate Strength) The laminate strength test was conducted on the day after extrusion lamination. Specifically, a thin cross cut was made on the surface of the thermoplastic resin layer (C) of the obtained laminate with a cutter blade, and a Nichiban No. CT-17 tape was firmly attached to the cut part, and then lightly peeled off by hand to create a starting point. Then, a piece was cut out to a width of 15 mm, and the peeled laminate layer and paper were held with a jig so that they were at an angle of 180°, and a peel strength test was conducted. The tensile speed was 200 mm / min. The peel tester used was a Shimadzu Autograph EZ-LX (manufactured by Shimadzu Corporation).
[0091] <Evaluation> ◎: 4.0N / 15mm or more ○: 3.0N / 15mm or more, less than 4.0N / 15mm △: 2.0N / 15mm or more, less than 3.0N / 15mm ×: Less than 2.0N / 15mm If the above evaluation result is .circle., ◯, or Δ, it can be said that the laminate strength is sufficient.
[0092] (Evaluation of drying properties) Basis weight 210g / m 2A4-sized base paper (paper substrate layer (A)) was coated under the conditions described in the Examples and Comparative Examples to form a first adhesive resin layer (B), which was then heated in a hot air oven at 100°C for 30 seconds and then removed, and the surface condition of the first adhesive resin layer (B) was observed.
[0093] <Evaluation> ○: The surface is not wet and the coating is sufficiently formed. △: The surface is slightly wet, but the coating is sufficiently formed. ×: Puddles are formed on the surface and the coating film is not sufficiently formed. If the above evaluation result is ◯ or Δ, drying and coating film formation in a typical papermaking process are possible.
[0094] (Measurement of basis weight of first adhesive resin layer (B)) The papers with the first adhesive resin layer (B) obtained in the Examples and Comparative Examples were thoroughly dried for 10 minutes in a hot air oven heated to 100°C, and then aged for one week under conditions of 25°C and 60% humidity. They were then cut into 10cm x 10cm pieces and weighed. The weight value was subtracted from the weight of the base paper and multiplied by 100 to obtain the basis weight of the first adhesive resin layer (B). <Production of laminates by extrusion lamination method> Example 1 Basis weight 210g / m 2 Coating solution 1 was coated onto an A4-sized base paper (paper substrate layer (A)) using a bar coater No. 10, and immediately thereafter, the paper substrate was placed in a hot air oven heated to 100°C for 30 seconds to dry, forming a first adhesive resin layer (B) on the paper substrate. The basis weight and drying property of the obtained first adhesive resin layer (B) were evaluated, and the results are shown in Table 1.
[0095] Next, the PHBH pellet 1 was put into a single-screw extruder equipped with a T-type die, extruded from the T-type die under conditions such that the resin temperature immediately after extrusion was 163° C., and taken up with a cooling roll set at 60° C. to form a film having a thickness of 30 μm. The paper base material with the first adhesive resin layer (B) obtained above and the PHBH film were sandwiched so that the heating roll was in contact with the paper side and the cooling roll was in contact with the PHBH film side, and the conditions were adjusted so that the surface temperature of the PHBH film was 163° C., to obtain a laminate including the paper base material, the first adhesive resin layer (B), and the thermoplastic resin layer (C) in this order.
[0096] The laminate strength of the obtained laminate was evaluated, and the results are shown in Table 1.
[0097] (Examples 2 to 12, Comparative Examples 2 to 4) A laminate was prepared in the same manner as in Example 1, except that the coating liquid, basis weight in the first adhesive resin layer (B), PHBH pellets in the thermoplastic resin layer (C), the surface temperature of the PHBH film, or the thickness were changed as shown in Table 1, and the same evaluations were performed as in Example 1. The results are summarized in Table 1.
[0098] Comparative Example 1 PHBH pellet 1 was placed on the surface of the paper base layer (A) in a single-screw extruder equipped with a T-die, and directly extruded from the T-die under conditions such that the resin temperature immediately after extrusion was 163°C. The PHBH pellet was then taken up with a cooling roll set at 60°C, and a thermoplastic resin layer (C) having a thickness of 30 μm was laminated on the surface of the paper base layer (A). Thus, a laminate was obtained that did not include a first adhesive resin layer (B) but included the paper base layer (A) and the thermoplastic resin layer (C).
[0099] The laminate strength of the obtained laminate was evaluated, and the results are shown in Table 1.
[0100] [Table 1] <Result> From Table 1, it can be seen that in each example, the base material layer (A) and the thermoplastic resin layer (C) are bonded with sufficient strength via the first adhesive resin layer (B), and the drying properties after coating of the first adhesive resin layer (B) are also good.
[0101] On the other hand, the adhesiveness is insufficient in Comparative Examples 1 to 3, and the drying property is poor in Comparative Example 4, which shows that neither the adhesiveness nor the drying property is compatible in each Comparative Example. [Explanation of symbols]
[0102] 1. Laminate 2 Paper base layer (A) 3 First adhesive resin layer (B) 4 Thermoplastic resin layer (C) mainly composed of poly(3-hydroxyalkanoate) resin
Claims
1. A laminate comprising a paper base layer (A) and a first adhesive resin layer (B) and a thermoplastic resin layer (C) mainly composed of a poly(3-hydroxyalkanoate) resin laminated in this order on at least one surface of the paper base layer (A); The weight of the first adhesive resin layer (B) is 0.1 g / m 2 3.0g / m or more 2 is less than The average thickness of the thermoplastic resin layer (C) is 20 μm or more and less than 100 μm, The thermoplastic resin layer (C) contains 0.1 parts by weight or more and less than 10 parts by weight of a second adhesive resin (D) based on 100 parts by weight of a poly(3-hydroxyalkanoate)-based resin.
2. The laminate according to claim 1, wherein the first adhesive resin layer (B) contains at least one resin selected from the group consisting of ester-based resins, acrylic or methacrylic resins, vinyl chloride-based resins, styrene-acrylic resins, styrene-butadiene-based resins, styrene-isoprene-based resins, polycarbonate-based resins, urea resins, melamine-based resins, epoxy-based resins, phenol-based resins, urethane-based resins, diallyl phthalate-based resins, and imine-based resins.
3. The laminate according to claim 1 or 2, wherein the second adhesive resin (D) contains at least one resin selected from the group consisting of ester-based resins, acrylic or methacrylic resins, vinyl chloride-based resins, styrene-acrylic resins, styrene-butadiene-based resins, styrene-isoprene-based resins, polycarbonate-based resins, urea resins, melamine-based resins, epoxy-based resins, phenol-based resins, urethane-based resins, diallyl phthalate-based resins, and imine-based resins.
4. 3. The laminate according to claim 1 or 2, wherein the first adhesive resin layer (B) contains at least one tackifying resin (E) selected from the group consisting of rosin-based resins, terpene-based resins, ethylene-based resins, vinyl acetate-based resins, alkylphenol-formaldehyde-based resins, alkylphenol-acetylene-based resins, coumarone-indene-based resins, styrene-based resins, and xylene-formaldehyde-based resins.
5. The laminate according to claim 4 , wherein the tackifier resin (E) has a weight average molecular weight (Mw) of 100 or more and less than 5,000.
6. 3. The laminate according to claim 1, wherein the poly(3-hydroxyalkanoate)-based resin is a poly(3-hydroxybutyrate)-based resin.
7. 3. The laminate according to claim 1, wherein the poly(3-hydroxyalkanoate)-based resin is poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
8. A method for producing the laminate according to claim 1 or 2, comprising the steps of: A step of forming the first adhesive resin layer (B) on at least one surface of the base layer (A); A method for producing a laminate, comprising the step of forming the thermoplastic resin layer (C) on a surface of the first adhesive resin layer (B) by extrusion lamination or thermal lamination.
9. 9. The method for producing a laminate according to claim 8, wherein, when the thermoplastic resin layer (C) is formed by the extrusion lamination method, the temperature of the resin immediately after being melt-extruded from the tip of a T-shaped die is equal to or higher than the melting point of a poly(3-hydroxyalkanoate)-based resin contained as a main component in the thermoplastic resin layer (C) and lower than 165°C.
10. 9. The method for producing a laminate according to claim 8, wherein in the thermal lamination, a film constituting the thermoplastic resin layer (C) is used, and the film is a film formed at a resin temperature immediately after melt extrusion from the tip of a T-shaped die that is equal to or higher than the melting point of a poly(3-hydroxyalkanoate)-based resin contained as a main component in the thermoplastic resin layer (C) and lower than 165°C.
11. A molded article comprising the laminate according to claim 1 or 2.
Citation Information
Patent Citations
Production of laminate
JP1994293113A
Cited By
High-bio-based biodegradable paper-plastic composite film and preparation method thereof
CN120003135A
Laminate and method for producing same