Production method of dispersion

The twin-screw kneader method with defined kneading zones and resistance parts addresses the challenge of achieving both high dispersibility and productivity in dispersion processes, ensuring efficient and uniform dispersion of liquids or powders in a medium.

JP2024162574APending Publication Date: 2024-11-21SUMIKA COLOR CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023078210
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for dispersing liquids or powders in a dispersion medium face challenges in achieving both high productivity and dispersibility, leading to issues such as uneven dispersion, agglomeration, and reduced productivity when scaling up.

Method used

A method utilizing a twin-screw kneader with specific kneading zones and resistance parts that generate pressures of 0.1 MPa or more, combined with conditions where the viscosity of the dispersion medium is 200 poise or less and the liquid's viscosity is 10 times that of the medium, ensuring effective dispersibility and productivity.

Benefits of technology

The method achieves excellent dispersibility and productivity, reducing agglomeration and maintaining high-quality dispersion even with high-viscosity powders or liquids, while avoiding inefficiencies and temperature-related issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162574000003
    Figure 2024162574000003
  • Figure 2024162574000004
    Figure 2024162574000004
  • Figure 2024162574000005
    Figure 2024162574000005
Patent Text Reader

Abstract

To provide method for producing a dispersion including a dispersing medium and a liquid or powder dispersed in the dispersing medium with excellent productivity and dispersibility.SOLUTION: A method for producing a dispersion including a dispersing medium and a liquid or powder dispersed in the dispersing medium, comprising a kneading process for kneading the dispersing medium and the liquid or powder in a kneading zone of a twin-shaft kneader having a kneading zone and in which material flows from upstream to downstream, the kneading zone being, for example (A) a one-row flight and a resistance section that generates a pressure of 0.1 MPa or higher at the downstream end of the one-row flight, and the kneading process is performed under such conditions that the viscosity of the dispersing medium is 200 poise or less and the viscosity of the liquid is 10 times or more than the viscosity of the dispersing medium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a dispersion. [Background technology]

[0002] Dispersions containing a dispersion medium and a liquid or powder dispersed in the dispersion medium are used for various applications. Accordingly, various methods for dispersing a liquid or powder in a dispersion medium have been investigated.

[0003] For example, when dispersing other components in a low-viscosity medium, mixers such as Disper, Homomixer, or Planetary Mixer; homogenizers such as M-Technique's "Clearmix" or PRIMIX's "Filmix"; or paint conditioners (Red Devil), ball mills, sand mills (Shinmaru Enterprises' "Dynomill", etc.), attritors, pearl mills (Eirich's "DCP Mill", etc.), or media-type dispersers such as Coball mills, are often used. Batch mixers can mix efficiently in small quantities, but if you want to scale up while maintaining dispersibility, you need to extend the processing time, which tends to reduce productivity.

[0004] An example of a technique for dispersing solids in a low viscosity medium is a process for obtaining a paste for battery electrode materials.

[0005] Patent Document 1 proposes a method of kneading an electrode material at a solid content concentration of 82 to 84 wt% in a kneader having a pressure mechanism using a Banbury-type kneading blade. Since a Banbury-type kneading blade generally has a large clearance between the kneading tank and the blade, when the solid content concentration is low or the viscosity of the entire system is low, an appropriate shear stress cannot be obtained, and good dispersion may not be obtained.

[0006] Patent Document 2 proposes a method in which first, only the solid content is mixed in a planetary mixer, a smaller amount of solvent than that used in the end is added, wet kneading is performed using a twin-screw kneading extruder in a state where the solid content concentration is high, a solvent is further added, and the active material is dispersed again using a planetary mixer. In this method, it is assumed that the paint has high compaction during kneading, and it is considered difficult to obtain a uniformly dispersed paint using a device with low shear force such as a planetary mixer. In addition, since paint cannot be produced by a continuous process, it is considered to be inferior in productivity. Furthermore, since the kneaded paste is not uniformly dispersed, many coarse aggregated particles remain in the paint, and such aggregated particles exist as protrusions in the coating film formed later, and there is a concern that this may cause production problems such as the detachment of aggregated particles in a non-aqueous secondary battery, damage to the separator, and short circuits. In addition, if the paint is filtered through a filter before coating of the coating film, its permeability is significantly reduced and productivity is reduced.

[0007] In the technology disclosed in Patent Document 3, when preparing an electrode, a positive electrode active material, a conductive material, a binder, a solvent, and the like are mixed to prepare an electrode paste. At this time, the conductive material is put into a twin-screw kneader at once. In the method of putting the conductive material into the twin-screw kneader at once, the dispersion degree of the conductive material in the electrode paste tends to be approximately the same, and it may be difficult to prepare an electrode paste including a conductive material with a different dispersion degree. For this reason, it tends to be difficult to form a good conductive network between the positive electrode active materials, and the internal resistance in the positive electrode cannot be sufficiently reduced, which may lead to a deterioration in battery performance.

[0008] Patent Document 4 discloses a twin-shaft kneader for producing a positive electrode composite paste, which produces a positive electrode composite paste by kneading a positive electrode active material, which is a positive electrode material, acetylene black, a binder, and a solvent. This twin-shaft kneader for producing a positive electrode composite paste includes two parallel shafts, a cylindrical barrel extending in an axial direction in which the shafts extend, a shear paddle section having a shear paddle disposed inside the barrel and rotating around the shaft as a rotation axis, and a resistance paddle section having a resistance paddle disposed inside the barrel and rotating together with the shear paddle section around the shaft as a rotation axis. The barrel has an inlet located at one end in the axial direction for feeding the positive electrode material into the barrel, and an outlet located at the other end in the axial direction for discharging the positive electrode composite paste formed by kneading the positive electrode material to the outside of the barrel. A plurality of resistance paddle sections are arranged in line in the axial direction from the inlet side toward the outlet side on each shaft. In addition, the shear paddle portion is disposed adjacent to each of the resistance paddle portions in the axial direction on each of the shafts. In this twin-screw kneader for producing a positive electrode composite paste, all of the resistance paddles have the same dimensions, and the clearance between the inner peripheral surface of the barrel and the outer peripheral surface of the resistance paddle is constant throughout the twin-screw kneader for producing a positive electrode composite paste. However, in this method, the length of the acetylene black (the length of the secondary particles in which the primary particles are linearly connected) may vary greatly in the positive electrode composite paste within the same lot produced by the twin-screw kneader for producing a positive electrode composite paste.

[0009] Patent Document 5 describes a method of dispersing pigment powder in a medium by melt-kneading the pigment powder using a batch-type kneader such as a kneader or roll, or a single-screw or twin-screw extruder. On the other hand, the batch-type kneader tends to cause unevenness in the quality of each product lot and to cause poor production efficiency. In addition, there is a concern that the dispersion of pigment coarse particles may be insufficient using a single-screw or twin-screw extruder. In order to disperse hard coarse particles present in the pigment using these single-screw or twin-screw extruders, it is considered necessary to perform the kneading operation two or more times. In this case, there is a concern that there may be a loss in efficiency, and sometimes a negative effect such as a change in the viscosity of the composition due to a temperature rise of the composition caused by kneading may occur. In addition, it is difficult to turn all of the large secondary aggregate particles present in the pigment powder into fine particles of several μm or less even if the kneading operation is performed several times, and a very small amount of coarse particles tends to remain, and there is a concern that the gloss and smoothness of the product may be impaired due to the small amount of coarse particles, thereby reducing the commercial value.

[0010] Patent Documents 6 and 7 describe a method of melt-kneading using a continuous kneading extruder having a mechanism for kneading between a rotating disk and a fixed disk. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Japanese Patent Application Publication No. 04-253157 [Patent Document 2] JP 2000-353516 A [Patent Document 3] JP 2005-222772 A [Patent Document 4] JP 2015-109175 A [Patent Document 5] JP 2000-167826 A [Patent Document 6] Special Publication No. 55-41139 [Patent Document 7] Special Publication No. 54-24743 Summary of the Invention [Problem to be solved by the invention]

[0012] However, the conventional methods described above are not sufficient in terms of both productivity and dispersibility. Therefore, an object of the present invention is to provide a method for producing a dispersion containing a dispersion medium and a liquid or powder dispersed in the dispersion medium, which method is excellent in productivity and dispersibility. [Means for solving the problem]

[0013] The present invention relates to the following: [1] A method for producing a dispersion comprising a dispersion medium and a liquid or powder dispersed in the dispersion medium, comprising the steps of: A twin-shaft mixer having a kneading zone, in which materials flow from upstream to downstream, is provided with a kneading step of kneading the dispersion medium and the liquid or the powder in the kneading zone, The kneading zone is (A) Has a single flight and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the single flight, (B) Has two flights and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the two flights, (C) having a single flight and a resistance portion that generates a pressure of 0.01 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight; or (D) a two-row flight and a resistance portion that generates a pressure of 0.01 MPa or more at a downstream end of the two-row flight and at a position 1D upstream from the downstream end of the two-row flight, The method for producing a dispersion, wherein the kneading step is carried out under conditions such that the viscosity of the dispersion medium is 200 poise or less, and the viscosity of the liquid is 10 times or more the viscosity of the dispersion medium. [2] The kneading zone (a) Has a single flight having a length of 2D or more and a resistance portion that generates a pressure of 0.5 MPa or more at the downstream end of the single flight, (b) Has two flights with a length of 2D or more and a resistance portion that generates a pressure of 0.5 MPa or more at the downstream end of the two flights, (c) having a single flight having a length of 2D or more and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight; or (d) A method for producing a dispersion as described in [1], having two flights having a length of 2D or more and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the two flights and at a position 1D upstream from the downstream end of the two flights. [3] The method for producing a dispersion according to [1] or [2], wherein the lead length of the single flight or the double flight is 0.7D or more. [4] The method for producing a dispersion according to any one of [1] to [3], wherein the twin-screw kneader has a plurality of the kneading zones. [5] The method for producing a dispersion according to any one of [1] to [3], wherein a part of the dispersion medium and the liquid or the powder are supplied to a twin-screw kneader upstream of the kneading zone, and the remaining dispersion medium is supplied to the kneading zone. [6] The method for producing a dispersion according to any one of [1] to [5], wherein the content of the dispersion medium relative to the total mass of the dispersion is 20 mass % or more and 90 mass % or less. Effect of the Invention

[0014] According to the present invention, there is provided a method for producing a dispersion containing a dispersion medium and a liquid or powder dispersed in the dispersion medium, the method being excellent in productivity and dispersibility. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic diagram showing an example of a twin-screw kneader according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram illustrating the clearance between a single flight and a cylinder. [Diagram 3] FIG. 1 is a diagram explaining the clearance between a double flight and a cylinder. [Figure 4]FIG. 1 is a diagram showing pressure in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, several embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.

[0017] The method for producing a dispersion according to the present embodiment is a method for producing a dispersion containing a dispersion medium and a liquid or powder dispersed in the dispersion medium, and includes a kneading step of kneading the dispersion medium and the liquid or powder in the kneading zone of a twin-screw kneader in which materials flow from upstream to downstream, and the kneading zone has either (A) a single flight and a resistance part that generates a pressure of 0.1 MPa or more at the downstream end of the single flight, or (B) a double flight and a resistance part that generates a pressure of 0.1 MPa or more at the downstream end of the double flight. (C) a single flight and a resistance part that generates a pressure of 0.01 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight, or (D) a double flight and a resistance part that generates a pressure of 0.01 MPa or more at the downstream end of the double flight and at a position 1D upstream from the downstream end of the double flight, and the kneading step is performed under conditions where the viscosity of the dispersion medium is 200 poise or less and the viscosity of the liquid is 10 times or more the viscosity of the dispersion medium. According to this method, it is possible to achieve both excellent dispersibility and productivity. Furthermore, according to this method, even when a powder or a high-viscosity liquid is dispersed in a low-viscosity dispersion medium, it is possible to reduce the generation of agglomerates while maintaining excellent productivity.

[0018] Single- and double-row flights are generally used as conveying segments, and the kneading zone of a twin-screw kneader generally uses a combination of screw segments generally used as kneading segments, such as a forward kneading disk (KD), a reverse kneading disk, a neutral kneading disk, a rotor, etc. In contrast, the method according to the present embodiment uses single- and double-row flights in the kneading zone. This method can achieve dispersion and mixing of powder or liquid (e.g., high-viscosity liquid material) with excellent productivity.

[0019] D usually refers to the approximate value of the cylinder diameter. In other words, "a position 1D upstream from the downstream end of a single flight" means a position approximately "1 x D" upstream from the "downstream end of a single flight." In addition, the description "2D" below indicates a length "approximately twice D," and the description "3D" indicates a length "approximately three times D." The same applies to other similar descriptions such as "4D."

[0020] In this specification, 1D is defined as the range of -7.0% to +7.0% of the cylinder diameter. In other words, when the cylinder diameter is defined as D', 1D means "0.93×D' to 1.07×D'". Similarly, "2D" means "0.93×2×D' to 1.07×2×D'", and "3D" means "0.93×3×D' to 1.07×3×D'".

[0021] In this specification, the viscosity of the dispersion medium or liquid in the kneading step refers to a value measured by a flow tester CFT-500D or a B-type (Brookfield) viscometer.

[0022] A specific example of the method according to this embodiment will now be described.

[0023] Fig. 1 is a schematic diagram showing an example of a twin-screw kneader according to this embodiment. This twin-screw kneader includes a cylinder (not shown), a screw 2 disposed in the cylinder, and a die (not shown) provided at the downstream end of the cylinder. The twin-screw kneader may be configured to include screws that rotate and mesh with each other. An example of the twin-screw kneader is a unidirectional intermeshing type twin-screw kneading extruder.

[0024] The twin-screw kneader includes, in order from the upstream in the material flow direction, a supply zone 20, a first kneading zone 21, a conveying zone 22, a second kneading zone 23, and a conveying zone 24. The supply zone 20 and the conveying zone 22 are provided with a first supply port 1a and a second supply port 1b, respectively, and the conveying zone 24 is provided with a vent port 5. That is, the twin-screw kneader includes, in order from the upstream in the material flow direction, a first supply port 1a, a first kneading zone 21, a second supply port 1b, and a second kneading zone 23. The kneading step according to the method for producing a dispersion of this embodiment is carried out in the second kneading zone 23. The first supply port 1a and the second supply port 1b are connected to a liquid feed pump such as a plunger pump, a diaphragm pump, a tube pump, or a twin-screw pump; a gravimetric feeder; or a hopper (not shown). These can be appropriately selected depending on the type of material to be fed. When a liquid material is supplied from the supply port, it is preferable that a liquid pump is connected to the supply port, and when a solid material is supplied from the supply port, it is preferable that a gravimetric feeder is connected to the supply port, which allows the material to be supplied quantitatively.

[0025] The second kneading zone 23 has a mixing / dispersing section 23a on the upstream side and a resistance section 23b on the downstream side as viewed from the direction of material flow. The resistance section is a region configured as a screw segment in which the pressure is highest at the upstream end of the resistance section 23b and decreases toward the downstream side, and the mixing / dispersing section 23a has a pressure decreasing from the downstream end (the upstream end of the resistance section 23b) toward the upstream side. It is considered that the second kneading zone 23 has the resistance section 23b, which makes it easier for the mixture of the dispersion medium and the liquid or powder dispersed in the dispersion medium to fill the gap between the flight and the cylinder, improving dispersibility.

[0026] The mixed dispersion section 23a is composed of one or two flights. The length of the one or two flights constituting the mixed dispersion section 23a may be, for example, 1D or more, 2D or more, or 3D or more, from the viewpoint of dispersibility. The lead length of the one or two flights may be, for example, 0.7D or more. This lead length may be, for example, 1.0D or more, or 1.5D or more.

[0027] Lead length is the distance traveled axially along the helical winding of a flight as it makes one revolution around the axis.

[0028] The clearance between the flights (one or two flights) constituting the mixing / dispersing portion 23a and the cylinder is preferably 1.50% or less of the cylinder diameter, and more preferably 1.00% or less.

[0029] Fig. 2 is a diagram for explaining the clearance between a single flight and a cylinder, in which a indicates the clearance, b indicates the cylinder, c indicates the flight width, and dx indicates the cylinder diameter.

[0030] When a single flight is used, the flight width is preferably 20% or more of the lead length of the flight, and more preferably about 30%. By widening the flight width, it tends to be easier to obtain the effect of dispersion and mixing in the gap between the screw and the flight.

[0031] Fig. 3 is a diagram for explaining the clearance between the double flight and the cylinder, in which a indicates the clearance, b indicates the cylinder, and dx indicates the cylinder diameter.

[0032] The resistance portion 23b is a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the single-flight or double-flight; or a resistance portion that generates a pressure of 0.01 MPa or more at the downstream end of the single-flight or double-flight and at a position 1D upstream from the downstream end of the single-flight or double-flight. The resistance portion 23b may be a resistance portion that generates a pressure of 0.5 MPa or more, 1.0 MPa or more, or 2.0 MPa or more at the downstream end of the single-flight or double-flight. The resistance portion 23b may be a resistance portion that generates a pressure of 0.1 MPa or more, 0.2 MPa or more, or 0.3 MPa or more at the downstream end of the single-flight or double-flight and at a position 1D upstream from the downstream end of the single-flight or double-flight.

[0033] The resistance portion 23b may be, for example, a screw element such as a reverse flight, a seal ring, a neutral kneading disk, a reverse kneading disk, a notched segment (a flight or ring with a notch), or a combination of these. The resistance portion 23b may be formed, for example, by adjusting the combination and length of the screw elements so that the conveying force toward the downstream side is lower than the discharge amount under the operating conditions of the twin-screw kneader. Among them, a reverse flight with one or two threads can efficiently form a resistance portion. When the resistance portion is constituted by a flight, it is preferable that the clearance between the flight and the cylinder is 1% or less. The flight may be, for example, a flight with two or more revolutions, and is preferably a flight with four revolutions.

[0034] Hereinafter, a method for producing a dispersion containing a dispersion medium and a liquid or powder dispersed in the dispersion medium using the above-mentioned twin-screw kneader will be described.

[0035] First, a dispersion medium is supplied from the first supply port 1a to the supply zone 20. The dispersion medium supplied from the first supply port 1a to the supply zone 20 is transported to the first kneading zone .

[0036] The dispersion medium is not particularly limited as long as it is a material that can have a viscosity of 200 poise or less. The dispersion medium may be, for example, a liquid or a solid at room temperature. The dispersion medium may be appropriately selected from the properties required for the purpose of use, such as heat resistance, chemical resistance, and moldability.

[0037] Examples of dispersion media that are liquid at room temperature include water, epoxy resins such as bisphenol A type, bisphenol F type, and novolac type, ethylene α-olefin co-oligomers, and mixtures thereof. These may be used alone or in combination of two or more.

[0038] The dispersion medium may contain a dispersant as necessary. The dispersant is not particularly limited, and anionic, cationic, amphoteric, or nonionic surfactants can be used.

[0039] Examples of dispersion media that are solid at room temperature include olefin waxes such as low molecular weight polyethylene and low molecular weight polypropylene, natural waxes such as low molecular weight polyester, beeswax, carnauba wax, montan wax, paraffin wax, and microcrystalline wax, synthetic waxes such as amide wax, and mixtures thereof. These may be used alone or in combination of two or more.

[0040] In the first kneading zone 21, the viscosity of the dispersion medium supplied from the first supply port 1a is adjusted as necessary. The dispersion medium leaving the first kneading zone 21 is transported to the conveying zone 22, where it joins with the liquid or powder.

[0041] The liquid or powder is supplied from the supply port 1b to the transport zone 22, where it meets with the dispersion medium.

[0042] The liquid is a material whose viscosity can be increased to 10 times or more that of the dispersion medium during the kneading process. The liquid or powder can be appropriately selected based on the required properties such as heat resistance, chemical resistance, moldability, etc. depending on the purpose of use.

[0043] Examples of the liquid include epoxy resins such as bisphenol A type, bisphenol F type, and novolac type, ethylene α-olefin co-oligomers, and mixtures thereof. These may be used alone or in combination of two or more.

[0044] Examples of the powder include inorganic pigments, organic pigments, inorganic fillers, and mixtures thereof. These may be used alone or in combination of two or more.

[0045] Examples of inorganic pigments include titanium oxide (CI Pigment W-6, W-7), iron oxide (CI Pigment R-101, Y-42, BL-11, etc.), barium sulfate (CI Pigment W-21, W-22, etc.), zinc oxide (CI Pigment W-4, etc.), calcium carbonate (CI Pigment W-18), silica (CI Pigment W-27), aluminum (CI Pigment W-24), pearl pigments (CI Pigment W-20, etc.), brass, and mica.

[0046] Examples of organic pigments include soluble azo pigments (CI Pigment R-48:3, R-57:1, R-53:1, R-48:1, etc.), insoluble azo pigments (CI Pigment Y-12, Y-13, Y-14, Y-17, Y-55, Y-81, Y-83, Y-87, Y-124, Y-152, Y-165, O-16, R-146, etc.), naphthol AS pigments (CI Pigment R-146, etc.), condensed azo pigments (CI Pigment Y-93, Y-128, Y-166, R-144, R-166, R-214, R-262, O-31, etc.), benzimidazolone pigments (CI Pigment Y-93, Y-128, Y-166, R-144, R-166, R-214, R-262, O-31, etc.), and the like. Y-120, Y-180, R-171, V-32, O-36, etc.), Phthalocyanine (C.I.Pigment B-15:3, B-15:4, B-75, G-7, G-36, etc. C.I.P.B (Pigment Blue) 15:1, PB15:2, PB15:3, PB15:4, PB15:5, PB15:6, PB16, PG (Pigment Green) 7, PG36, C.I.P.B (Pigment Blue) 15:1, PB15:2, PB15:3, PB15:4, PB15:5, PB15:6, PB16, PG (Pigment Green) 7, PG36), Dioxazine (C.I.Pigment V-23, etc.), Quinacridone (C.I.Pigment R-122, R-202, V-19, O-48, etc.), perylenes (CIPigment R-123, R-149, V-29, etc.), perinones (CIPigment R-194, O-43, etc.), thioindigo (CIPigment B-63, R-181, etc.), anthanthrones, isoindolines (CIPigment Y-139, Y-185, R-260, O-66, etc. PO66), isoindolinones (CIPigment Y-109, Y-110, O-61, etc.), threnes (CIPigment R-168, R-177, etc.), anthraquinones (CIPigment Y-24, Y-108, R-168, B-60, etc.), quinophthalones (CIPigment Y-138, etc.), azomethine-based, diketopyrrolopyrrole-based (CI Pigment R-254, R-255, O-71, etc.), and carbon black (CI Pigment BL-6, BL-7, etc.).

[0047] Examples of inorganic fillers include metal oxides such as silica, alumina, zinc oxide, titanium oxide, iron oxide, and zirconium oxide; fluorides such as magnesium fluoride, calcium fluoride, and aluminum fluoride; metal carbonates such as calcium carbonate, magnesium carbonate, and zinc carbonate; sulfides such as iron sulfide, magnesium sulfide, and zinc sulfide; and nitrides such as magnesium nitride and carbon nitride.

[0048] The dispersion medium and the liquid or powder that have left the conveying zone 22 are subjected to the kneading step according to this embodiment in the second kneading zone 23. This makes it possible to obtain the dispersion according to this embodiment.

[0049] The above-mentioned resistance portion is formed in the second kneading zone 23. In the second kneading zone 23, the dispersion medium and the liquid or powder are kneaded under the following conditions. Mixing conditions: The viscosity of the dispersion medium is 200 poise or less. The viscosity of the liquid is at least 10 times that of the dispersion medium. The powder can be in a solid state.

[0050] The viscosity of the dispersion medium in the kneading step may be, for example, 100 poise or less, or 50 poise or less. The viscosity of the dispersion medium in the kneading step may be, for example, 0.1 poise or more, 1 poise or more, 5 poise or more, or 10 poise or more.

[0051] The viscosity of the liquid in the kneading step may be, for example, 2000 poise or less, 200 poise or less, 100 poise or less, or 50 poise or less. The viscosity of the liquid in the kneading step may be, for example, 1 poise or more, 5 poise or more, or 10 poise or more.

[0052] The viscosity of the liquid in the kneading step may be, for example, 50 times or more, or 100 times or more. The viscosity of the liquid in the kneading step may be, for example, 10,000 times or less, 5,000 times or less, or 1,000 times or less that of the dispersion medium.

[0053] The dispersion leaving the second kneading zone 23 passes through a conveying zone 24 and is discharged from the twin-screw kneader through a die.

[0054] The content of the dispersion medium relative to the total mass of the dispersion may be, for example, 20% by mass or more and 90% by mass or less, 30% by mass or more and 80% by mass or less, or 40% by mass or more and 70% by mass or less.

[0055] The content of the liquid or powder relative to the total mass of the dispersion may be, for example, 10% by mass or more and 80% by mass or less, 20% by mass or more and 70% by mass or less, or 30% by mass or more and 60% by mass or less.

[0056] The content of the liquid or powder per 100 parts by mass of the dispersion medium may be, for example, 15 parts by mass or more, 30 parts by mass or more, or 50 parts by mass or more, and may be 400 parts by mass or less, 300 parts by mass or less, or 200 parts by mass or less.

[0057] Although an example of the method for producing the resin composition according to the present embodiment has been described above, the method is not limited to this.

[0058] For example, the liquid or powder may be supplied from the first supply port 1a together with the dispersion medium. In this case, it is preferable to perform preliminary kneading in the first kneading zone 21 using a kneading disk or the like.

[0059] A part of the dispersion medium and the liquid or powder may be supplied to the twin-screw kneader upstream of the kneading zone 23 , and the remaining dispersion medium may be supplied to the kneading zone 23 .

[0060] The feed zone 20, the first kneading zone 21, the conveying zone 22, the conveying zone 24 and the vent port may be present or absent. A plurality of kneading zones 23 may be present.

[0061] The above-described method for producing a dispersion described above is a method for producing a dispersion containing a dispersion medium and a liquid or powder dispersed in the dispersion medium, and includes a kneading step of kneading the dispersion medium and the liquid or powder in the kneading zone of a twin-screw kneader in which materials flow from upstream to downstream, and the kneading zone has either (A) a single flight and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the single flight, or (B) a double flight and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the double flight. or (C) a single flight and a resistance portion generating a pressure of 0.01 MPa or more at the downstream end of the single flight and at a position 1 D upstream from the downstream end of the single flight, or (D) a double flight and a resistance portion generating a pressure of 0.01 MPa or more at the downstream end of the double flight and at a position 1 D upstream from the downstream end of the double flight, and the kneading step is performed under conditions where the viscosity of the dispersion medium is 200 poise or less and the viscosity of the liquid is 10 times or more the viscosity of the dispersion medium. According to this method, both excellent dispersibility and productivity can be achieved.

[0062] In this method, the kneading zone preferably has (a) a single flight having a length of 2D or more and a resistance part at the downstream end of the single flight that generates a pressure of 0.5 MPa or more, (b) a double flight having a length of 2D or more and a resistance part at the downstream end of the double flight that generates a pressure of 0.5 MPa or more, (c) a single flight having a length of 2D or more and a resistance part at the downstream end of the single flight and a position 1D upstream from the downstream end of the single flight that generates a pressure of 0.1 MPa or more, or (d) a double flight having a length of 2D or more and a resistance part at the downstream end of the double flight and a position 1D upstream from the downstream end of the double flight that generates a pressure of 0.1 MPa or more. This can further improve dispersibility and productivity.

[0063] In this method, the lead length of the single flight or double flight is preferably 0.7D or more, which can further improve dispersibility and productivity.

[0064] The twin-screw kneader may be provided with a plurality of the kneading zones, which can further improve the dispersibility and productivity.

[0065] In this method, a part of the dispersion medium and the liquid or powder may be fed to the twin-screw kneader upstream of the kneading zone, and the remaining dispersion medium may be fed to the kneading zone, which can further improve the dispersion and productivity. EXAMPLES

[0066] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0067] (material) The materials used in the examples and comparative examples are shown below.

[0068] [Dispersion medium] Low molecular weight PE resin: Mitsui Chemicals, Hiwax NL-800 (melting point (mp): 105°C, viscosity at 105°C: 181 poise, viscosity at 140°C: 35 poise)

[0069] [powder] Inorganic pigment 1: Chemours Ti-Pure R-104 Inorganic pigment 2: Ultramarine No. 2000, manufactured by Daiichi Chemical Industry Co., Ltd.

[0070] (Configuration and conditions of twin-screw kneader) The following processing machine was used as the twin-screw kneader. The following screw segments were used as the screw segments constituting the mixing / dispersing section and the resistance section.

[0071] Processing machine 1: Co-rotating twin screw extruder TEM-26SX (Shibaura Machine Co., Ltd.), cylinder bore: 26.6 mm Processing machine 2: Manual heating three-roll mill, SH-4; 3 / 4 x 11 type (manufactured by Inoue Seisakusho Co., Ltd.)

[0072] [Screw segment] (Mixing dispersion section) Single flight A: A single flight with a flight lead length b of 1D, a clearance with the cylinder of 0.66% of the cylinder diameter, and a flight width c of 30% of the cylinder diameter. Single flight B: A single flight with a flight lead length b of 1D, a clearance with the cylinder of 1.50% of the cylinder diameter, and a flight width c of 30% of the cylinder diameter. (Resistance part) Single-row inverted flight: The lead length b of the flight is 1D, the clearance with the cylinder is 0.66% of the cylinder diameter, and the flight width c is 30% of the cylinder diameter.

[0073] [Examples 1 to 4] 50% by weight of low molecular weight PE resin, 45% by weight of inorganic pigment 1, and 5% by weight of inorganic pigment 2 were mixed using a co-rotating twin screw extruder TEM-26SX to obtain a sample for evaluation. The configuration of the mixing / dispersion section and resistance section of the twin screw extruder, the discharge rate, and the screw rotation speed are shown in Table 1. Table 2 also shows the resin pressure at a position 65.0 mm upstream (corresponding to 2.40 D upstream) from the downstream end of the mixing / dispersion section (downstream end of the flight) during mixing. The temperature of the material at the extruder outlet was 105°C.

[0074] [Comparative Example 1] 50% by weight of low molecular weight PE resin, 45% by weight of inorganic pigment 1, and 5% by weight of inorganic pigment 2 were kneaded three times using a manual heated three-roll mill SH-4; 3 / 4 × 11 type heated to 90 to 100 °C to obtain a sample for evaluation.

[0075] [Sample evaluation] The obtained samples were evaluated according to the following procedures.

[0076] [Pigment dispersion] 90% by weight of LDPE resin (Sumikathene L-705) and 10% by weight of the above sample were extruded at 1 kg / h using a Labo Plastomill 4C150 type extrusion tester (single screw) manufactured by Toyo Seiki Seisakusho Co., Ltd., equipped with a 40 μm filter at a set temperature of 180° C., and the pressure rise value after extrusion was measured under the condition of 1 kg / h. A pressure rise value of less than 1.0 MPa was evaluated as good. The smaller this value, the better the dispersibility. The results are shown in Table 2.

[0077] [Table 1]

[0078] [Table 2]

[0079] For Example 1, the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section), and the pressures at positions 2.40D upstream, 4.00D upstream, and 1.60D downstream from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section) are shown in Fig. 4. In Fig. 4, "0.00D" indicates the position of the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section), "-2.40D" indicates the position 2.40D upstream from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section), "-4.00D" indicates the position 4.00D upstream from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section), and "1.60D" indicates the position 1.60D downstream from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section). As is clear from Figure 4, in Example 1, the pressure is highest at the upstream end of the resistance section and decreases toward the downstream, and the mixing / dispersion section has a region configured with screw segments where the pressure decreases from the downstream end (upstream end of the resistance section) toward the upstream side.

[0080] It is clear that the method according to the embodiment has excellent dispersibility while maintaining productivity. [Explanation of symbols]

[0081] 1a, 1b...supply port, 5...vent port, 20...supply zone, 21...first kneading zone, 22, 24...conveying zone, 23...second kneading zone, 23b...resistance section, 23a...mixing and dispersing section.

Claims

1. A method for producing a dispersion comprising a dispersion medium and a liquid or powder dispersed in the dispersion medium, comprising the steps of: A twin-shaft mixer having a kneading zone, in which materials flow from upstream to downstream, is provided with a kneading step of kneading the dispersion medium and the liquid or the powder in the kneading zone, The kneading zone is (A) having a single flight and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the single flight; (B) having a double flight and a resistance portion that generates a pressure of 0.1 MPa or more at the downstream end of the double flight; (C) having a single flight and a resistance portion that generates a pressure of 0.01 MPa or more at a downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight; or (D) a two-row flight and a resistance portion that generates a pressure of 0.01 MPa or more at a downstream end of the two-row flight and at a position 1D upstream from the downstream end of the two-row flight, The method for producing a dispersion, wherein the kneading step is carried out under conditions such that the viscosity of the dispersion medium is 200 poise or less, and the viscosity of the liquid is 10 times or more the viscosity of the dispersion medium.

2. The kneading zone is (a) having a single flight having a length of 2D or more and a resistance portion that generates a pressure of 0.5 MPa or more at the downstream end of the single flight; (b) having a double flight having a length of 2D or more and a resistance portion that generates a pressure of 0.5 MPa or more at the downstream end of the double flight; (c) having a single flight having a length of 2D or more and a resistance portion that generates a pressure of 0.1 MPa or more at a downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight; or (d) a double flight having a length of 2D or more, and a resistance portion that generates a pressure of 0.1 MPa or more at a downstream end of the double flight and at a position 1D upstream from the downstream end of the double flight, the method for producing a dispersion described in claim 1.

3. The method for producing a dispersion according to claim 1 or 2, wherein the lead length of the single flight or the double flight is 0.7D or more.

4. The method for producing a dispersion according to claim 1 or 2, wherein the twin-screw kneader has a plurality of the kneading zones.

5. 3. The method for producing a dispersion according to claim 1, wherein a part of the dispersion medium and the liquid or the powder are supplied to a twin-screw kneader upstream of the kneading zone, and the remaining dispersion medium is supplied to the kneading zone.

6. The method for producing a dispersion according to claim 1 or 2, wherein a content of the dispersion medium relative to a total mass of the dispersion is 20% by mass or more and 90% by mass or less.

Citation Information

Patent Citations

  • Culture of shiitakeemushroom

    JP1979024743A

  • Coreless motor

    JP1980041139A

  • Manufacture of electrode plate for nickel-cadmium storage battery

    JP1992253157A

  • Manufacture of pigment resin composition