Millable silicone rubber compound and millable silicone rubber composition

The addition of a 3-glycidyloxypropylsilanol oligomer to silicone rubber compounds addresses plasticity and reversion issues, enhancing initial plasticity and long-term stability, resulting in high-quality cured products with low hardness and improved mechanical properties.

JP2024162627APending Publication Date: 2024-11-21SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023078333
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing millable silicone rubber compounds face issues with decreased plasticity and increased plasticity reversion, leading to defective products and poor processability, especially when using conventional surface treatment agents, and high-temperature heat treatment methods are inefficient and costly.

Method used

Incorporating a specific 3-glycidyloxypropylsilanol oligomer into a millable silicone rubber compound containing organopolysiloxane raw rubber and reinforcing silica, which enhances plasticity and reduces plasticity reversion, along with a curing agent for improved properties.

Benefits of technology

The solution results in a millable silicone rubber compound with high initial plasticity and reduced plasticity reversion, ensuring stable performance over time and producing cured products with low hardness and improved mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162627000017
    Figure 2024162627000017
  • Figure 2024162627000001
    Figure 2024162627000001
  • Figure 2024162627000002
    Figure 2024162627000002
Patent Text Reader

Abstract

To provide a millable silicone rubber compound that yields a cured product with low hardness, even though the millable silicone rubber compound exhibits high plasticity and low plastic rebound, as well as a millable silicone rubber composition.SOLUTION: A millable silicone rubber compound is provided that contains (A) organopolysiloxane raw rubber having two or more alkenyl groups bound to silicon atoms in one molecule, with an average degree of polymerization of 3000-100000, (B) reinforcing silica with a predetermined specific surface area, and 3-glycidyloxypropyl silanol oligomer represented by the formula (1) (where R1 is a monovalent hydrocarbon group, R2 is a monovalent hydrocarbon group optionally substituted with a glycidyloxy group, R3 is a monovalent aliphatic hydrocarbon group, a, b, c and d are numbers fulfilling a≥0.5, b≥0, c≥0, d≥0, and a+b+c+d=1, and x and y are numbers fulfilling x≥1.0 and y≤0.5). A millable silicone rubber composition is also provided that contains the silicone rubber compound combined with (D) a curing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a millable type silicone rubber compound and a millable type silicone rubber composition. [Background technology]

[0002] When manufacturing millable silicone rubber compounds or silicone rubber compositions, it is necessary to knead the organopolysiloxane raw rubber with a reinforcing filler. At that time, a surface treatment agent for the reinforcing filler, called a dispersant (wetter), is used. Usually, an organosilane or siloxane having a silanol group is used as the surface treatment agent. However, when a large amount of surface treatment agent is used, the plasticity of the silicone rubber composition decreases, and depending on the molding method, the molded product may deform under its own weight, resulting in a defective product. In addition, there is a drawback that the surface of the silicone rubber composition may feel sticky, resulting in poor processability. Conversely, when the amount of surface treatment agent added is insufficient, the plasticity increases, but there is a problem that crepe hardening (plastic reversion) becomes large.

[0003] In order to solve the above problems, a method of increasing the plasticity by adding a resin or a polycyclic aromatic compound has been adopted, but the problem of plastic reversion has not been solved. In addition, there is a method of suppressing plastic reversion by heating the silicone rubber compound at a high temperature of 200°C or more for a long time, but this is not economical in terms of energy costs, etc. Patent Document 1 reports that the plasticity is increased by condensing silanols by adding a catalyst for condensation reaction of a specific organometallic compound to the silicone rubber compound and performing heat treatment. Although this method is certainly effective in increasing the plasticity of the silicone rubber compound, it is insufficient in terms of stability over time, and when it is made into a composition, the compression set of the cured product may be significantly deteriorated. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-109014 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above circumstances, and has an object to provide a millable-type silicone rubber compound and a millable-type silicone rubber composition which have high plasticity and little plastic reversion, even in a millable-type silicone rubber compound which gives a cured product with low hardness. [Means for solving the problem]

[0006] As a result of extensive research into achieving the above-mentioned object, the inventors discovered that by blending a specific 3-glycidyloxypropylsilanol oligomer with a millable type silicone rubber compound containing organopolysiloxane raw rubber (base polymer) and reinforcing silica, the plasticity of the silicone rubber compound is increased and plastic reversion is reduced, which led to the creation of the present invention.

[0007] That is, the present invention provides the following millable type silicone rubber compound and silicone rubber composition. In the present invention, a mixture containing the following components (A) to (C) before blending with a curing agent is referred to as the silicone rubber compound, and this compound blended with a curing agent is referred to as the silicone rubber composition. 1. (A) Organopolysiloxane gum having two or more alkenyl groups bonded to silicon atoms in each molecule and an average degree of polymerization of 3,000 to 100,000: 100 parts by mass, (B) Specific surface area by BET adsorption method is 50 to 450 m 2 / g reinforcing silica: 5 to 50 parts by mass, (C) 3-glycidyloxypropylsilanol oligomer represented by the following formula (1): 0.1 to 15 parts by mass [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and R 2 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a glycidyloxy group, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, a, b, c, and d are numbers that satisfy a ≧ 0.5, b ≧ 0, c ≧ 0, d ≧ 0, and a + b + c + d = 1, and x and y are numbers that satisfy x ≧ 1.0, y ≦ 0.5. A millable type silicone rubber compound comprising: 2. The millable type silicone rubber compound according to 1, wherein the weight average molecular weight of component (C) is 500 to 10,000. 3. The millable type silicone rubber compound according to 1, wherein in the above formula (1), b, c, and d are numbers satisfying b=0, 0≦c≦0.5, and 0≦d≦0.2. 4. 100 parts by mass of the millable type silicone rubber compound according to any one of 1 to 3, (D) Hardener: effective hardening amount A millable type silicone rubber composition comprising: 5. The component (D) is an addition reaction type curing agent (D1), and the component (D1) is (a) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in the organohydrogenpolysiloxane (a) to alkenyl groups bonded to silicon atoms in the component (A) (hydrosilyl groups / alkenyl groups) is 0.5 to 10; and (b) Hydrosilylation catalyst: 1 ppm to 1% by mass calculated as the mass of platinum group metal relative to the mass of component (A). 5. The millable type silicone rubber composition according to 4, which comprises 6. The millable type silicone rubber composition according to 4, wherein the component (D) is an organic peroxide curing agent (D2), and the millable type silicone rubber composition contains 0.1 to 8 parts by mass of the component (D2) per 100 parts by mass of the millable type silicone compound. Effect of the Invention

[0008] According to the present invention, it is possible to provide millable-type silicone rubber compounds and millable-type silicone rubber compositions that have high plasticity and little plastic reversion, even in millable-type silicone rubber compounds that give cured products with low hardness. [Brief description of the drawings]

[0009] [Figure 1] 1 is a 1H-NMR spectrum chart of the 3-glycidyloxypropylsilanol oligomer (C) used in the present invention synthesized in Synthesis Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will now be described in more detail. (1) Silicone rubber compound The millable type silicone rubber compound of the present invention contains the following components (A) to (C): (A) Organopolysiloxane raw rubber having two or more alkenyl groups bonded to silicon atoms in each molecule and an average degree of polymerization of 3,000 to 100,000. (B) Specific surface area by BET adsorption method is 50 to 450 m 2 / g of reinforcing silica (C) 3-glycidyloxypropylsilanol oligomer represented by the following formula (1): [ka]

[0011] -(A) Component- In the present invention, component (A) is an organopolysiloxane raw rubber having two or more silicon-bonded alkenyl groups per molecule. Here, raw rubber refers to a state in which there is no self-flowing property at 25°C.

[0012] The alkenyl group preferably has 2 to 8 carbon atoms, and more preferably has 2 to 6 carbon atoms. Specific examples thereof include vinyl, allyl, butenyl, pentenyl, hexenyl, and cyclohexenyl groups. Of these, the vinyl group is preferred.

[0013] The component (A) is characterized by having two or more alkenyl groups in one molecule, preferably 2 to 50, and more preferably 2 to 20 alkenyl groups. In this case, it is preferable that 0.01 to 20 mol %, particularly 0.02 to 10 mol %, of all siloxane units in the organopolysiloxane are siloxane units having an alkenyl group. The alkenyl group may be bonded to a silicon atom at the molecular chain terminal, or to a silicon atom in the middle of the molecular chain (non-terminal of the molecular chain), or both, but it is preferable that the alkenyl group is bonded to a silicon atom at at least the molecular chain terminal. In addition, it is preferable that 80 mol % or more, preferably 90 mol % or more, more preferably 95 mol % or more, of all siloxane units in the organopolysiloxane, and even more preferably all siloxane units except for siloxane units having alkenyl groups, are dialkylsiloxy groups, and more preferably dimethylsiloxy groups.

[0014] Substituents other than alkenyl groups bonded to silicon atoms are not particularly limited, and examples thereof include monovalent hydrocarbon groups having 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms. The monovalent hydrocarbon group may be linear, branched, or cyclic, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, hexyl, and octyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; aryl groups such as phenyl and tolyl groups; and aralkyl groups such as benzyl and 2-phenylethyl groups. Furthermore, halogen-substituted monovalent hydrocarbon groups such as fluoroalkyl groups in which some of the hydrogen atoms of these monovalent hydrocarbon groups have been substituted with halogen atoms may also be used. Of these, a methyl group and a phenyl group are preferred, and a methyl group is more preferred.

[0015] The molecular structure of the organopolysiloxane, component (A), is preferably linear or partially branched.Specifically, the repeating structure of the diorganosiloxane unit constituting the main chain of the organopolysiloxane is preferably one consisting of repeating dimethylsiloxane units alone, or one in which diorganosiloxane units such as diphenylsiloxane units, methylphenylsiloxane units, or methylvinylsiloxane units are introduced as part of the repeating structure.

[0016] In addition, both molecular chain terminals are preferably capped with a group selected from the group consisting of trimethylsiloxy groups, dimethylphenylsiloxy groups, vinyldimethylsiloxy groups, divinylmethylsiloxy groups, trivinylsiloxy groups, methylphenylvinylsiloxy groups, etc., and are particularly preferably capped with vinyldimethylsiloxy groups. Specific examples of the organopolysiloxane of component (A) include dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylpolysiloxanes capped at both molecular chain terminals with methylphenylvinylsiloxy groups, dimethylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, etc. Among these, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups are preferred.

[0017] Such organopolysiloxanes can be obtained, for example, by (co)hydrolytic condensation of one or more organohalogenosilanes, or by ring-opening polymerization of a cyclic polysiloxane (such as a siloxane trimer or tetramer) using an alkaline or acidic catalyst.

[0018] The average degree of polymerization of the organopolysiloxane is 3,000 to 100,000, preferably 3,500 to 50,000, more preferably 4,000 to 30,000, still more preferably 4,500 to 20,000, and particularly preferably 4,500 to 10,000. If the average degree of polymerization is too low, the dispersion of the silica of component (B) may result in agglomerates, and the agglomerates may make dispersion difficult. The average degree of polymerization is calculated from the weight average molecular weight obtained by gel permeation chromatography (GPC) analysis measured under the conditions shown below, using polystyrene of known molecular weight as a standard substance. [Measurement conditions] Equipment: Tosoh Corporation HLC-8320GPC Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-H TSKgel SuperHM-N(6.0mmI.D.×15cm×1) TSKgel SuperH2500(6.0mmI.D.×15cm×1) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 50 μL (2.0% by mass in THF solution)

[0019] The component (A) may be a single type, or a mixture of two or more types differing in molecular weight (degree of polymerization) or molecular structure.

[0020] -(B) Component- Component (B) is reinforcing silica. Component (B) reinforcing silica is a filler that is added to obtain a silicone rubber composition with excellent mechanical strength. For this purpose, the specific surface area of ​​the reinforcing silica measured by the BET adsorption method is set to be 50 to 450 m. 2 / g, and preferably 100 to 450 m 2 / g, more preferably 100 to 300m2 / g. The specific surface area is 50m 2 If it is less than 1 / g, the mechanical strength of the cured product will be reduced.

[0021] Examples of such reinforcing silica include fumed silica and precipitated silica, and those whose surfaces have been hydrophobized with chlorosilane, hexamethyldisilazane, etc. are also preferably used. Among these, fumed silica, which has excellent dynamic fatigue properties, is preferred. Regarding the hydrophobization treatment, the reinforcing silica may be mixed while being treated with the hydrophobizing agent when mixed, or commercially available reinforcing silica fine powder that has been hydrophobized may be used. The component (B) may be used alone or in combination of two or more kinds.

[0022] The amount of reinforcing silica (B) blended is 5 to 50 parts by mass, and preferably 10 to 45 parts by mass, per 100 parts by mass of the organopolysiloxane (A). If the amount of component (B) blended is too small, the reinforcing effect is not obtained, whereas if the amount is too large, processability is deteriorated, mechanical strength is reduced, and dynamic fatigue durability is also deteriorated.

[0023] -(C) Component- In the present invention, 3-glycidyloxypropylsilanol oligomer represented by the following formula (1) is used as component (C). This component (C) is an essential component for interacting or reacting with hydroxyl groups present on the surface of silica, which is the aforementioned component (B), and for quickly dispersing component (B) in component (A).

[0024] [ka]

[0025] In the above formula, R 1 R is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and preferably a monovalent hydrocarbon group having 1 to 6 carbon atoms. 1The monovalent hydrocarbon group may be linear, branched, or cyclic, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and decyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; alkenyl groups such as vinyl and allyl groups; and aryl groups such as phenyl and naphthyl groups. Among these, methyl, ethyl, propyl, and phenyl groups are preferred, methyl and ethyl groups are more preferred, and methyl is even more preferred.

[0026] R 2 R are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, which may be substituted with a glycidyloxy group, and preferably a monovalent hydrocarbon group having 1 to 6 carbon atoms. 2 The monovalent hydrocarbon group may be linear, branched, or cyclic. Specific examples thereof include the above-mentioned R 1 and glycidyloxy-substituted alkyl groups such as glycidyloxypropyl and glycidyloxyoctyl groups. 2 is a monovalent hydrocarbon group substituted with a glycidyloxy group, the number of carbon atoms does not include the number of carbon atoms of the glycidyloxy group. Among these, methyl, ethyl, propyl, glycidyloxypropyl, and phenyl groups are preferred, methyl and ethyl groups are more preferred, and methyl group is even more preferred.

[0027] R 3 R is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, more preferably 1 or 2 carbon atoms, and further preferably an alkyl group having 1 or 2 carbon atoms. 3 The aliphatic hydrocarbon group may be linear, branched, or cyclic. Specific examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl groups; and alkenyl groups such as vinyl and allyl groups. Of these, methyl, ethyl, propyl, and butyl groups are preferred, with methyl and ethyl groups being more preferred, and methyl groups being even more preferred.

[0028] a, b, c, and d each represent a molar ratio of the respective siloxane units present, and are numbers that satisfy a≧0.5, b≧0, c≧0, d≧0, and a+b+c+d=1. It is preferable that a is a number that satisfies 0.5≦a≦1. If a is less than 0.5, the amount of available epoxy groups will be so small that the intended effect cannot be expected, and the resulting silanol oligomer will have a high viscosity or become gummy or solid, making it difficult to handle. The number b is preferably a number that satisfies 0≦b<0.5, and 0 is more preferable. It is preferable that c is a number that satisfies 0≦c≦0.5. The number d is preferably a number that satisfies 0≦d≦0.2, and 0 is more preferable.

[0029] x and y are the numbers of hydroxy groups or alkoxy groups bonded to 1 mole of silicon atoms in the siloxane units a to d, and are numbers that satisfy x≧1.0 and y≦0.5. It is preferable that x is a number that satisfies 1≦x≦2. The number y is preferably a number that satisfies y≦0.4, and more preferably a number that satisfies y≦0.3.

[0030] The component (C) is preferably one represented by the following formula (1a), and more preferably one represented by the following formula (1a'). [ka]

[0031] In the above formula, R 2 and R 3 is the same as above, a1, c1, and d1 are numbers that satisfy a1≧0.5, 0≦c1≦0.5, 0≦d1≦0.2, and a1+c1+d1=1, and x1 and y1 are numbers that satisfy x1≧1, y1≦0.5. As the component (C), in the above formula (1a'), R 2 is a methyl group or a 3-glycidyloxypropyl group, and R 3 More preferably, is a methyl group. The component (C) may be used alone or in combination of two or more types.

[0032] The weight average molecular weight of the oligomer of the component (C) is preferably 500 to 10,000, more preferably 500 to 1,000, from the viewpoint of the handling viscosity of the composition of the present invention. When an oligomer having a weight average molecular weight of less than 500 is used as the component (C), the component (C) is easily volatile, and may volatilize during kneading, resulting in an unstable plasticity of the compound composition. In addition, the amount of volatile components is large, which may be industrially dangerous. On the other hand, when the weight average molecular weight of the component (C) exceeds 10,000, the viscosity of the component (C) becomes very high, making it difficult to mix, or the performance of wetting the component (B) decreases, resulting in an extension of the mixing time or an unstable plasticity of the compound composition obtained, or in the worst case, the silica of the component (B) and the polymer of the component (A) may remain separated, making it impossible to obtain a compound composition. The weight average molecular weight is a value determined by GPC under the same conditions as those described for the component (A).

[0033] The method for producing the component (C) used in the present invention is not particularly limited, but the component (C) can be produced, for example, by using a 3-glycidyloxypropyl group-containing silane compound such as 3-glycidyloxypropyltrimethoxysilane represented by the following formula (i) or 3-glycidyloxypropyltriethoxysilane, or a mixture thereof, as the essential silane monomer raw material, and, if necessary, (co)hydrolyzing under acidic conditions a silane monomer containing one or more of a silane compound represented by the following formula (ii), a silane compound represented by the following formula (iii), and a silane compound represented by the following formula (iv).

[0034] [ka] (In the formula, R 1 ~R 3 is the same as above.)

[0035] Specific examples of the 3-glycidyloxypropyl group-containing silane compound represented by the above formula (i) include 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropyltripropoxysilane, 3-glycidyloxypropyltributoxysilane, and the like. Specific examples of the silane compound represented by the above formula (ii) include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, and decyltriethoxysilane. Specific examples of the silane compound represented by the above formula (iii) include dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, methylethyldimethoxysilane, methylethyldiethoxysilane, methylpropyldimethoxysilane, methylpropyldiethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, cyclopentylmethyldimethoxysilane, cyclohexylmethyldimethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, methyloctyldimethoxysilane, and the like. Specific examples of the silane compound represented by the above formula (iv) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane. In addition, hydrolysis condensation products of these may also be used. These may be used alone or in combination of two or more.

[0036] The amount of water used in the hydrolysis and condensation reaction is determined based on the amount of Si(OR) of the alkoxysilyl groups of the silane monomer used as the raw material. 3 ) group (R 3 is the same as above.) It is preferably 0.8 to 1.1 times the molar amount per 1 mole of the compound.

[0037] The acid component for adjusting the acidic conditions during the hydrolysis reaction is not particularly limited as long as it is a commercially available Brønsted acid, but from the viewpoint of ease of availability, formic acid, acetic acid, citric acid, hydrochloric acid, and nitric acid are preferred. The amount of the acid used is preferably 0.0001 to 0.01 mol per mol of the silane monomer from the viewpoint of suppressing an increase in the molecular weight of the organopolysiloxane obtained by an excessive dehydration condensation reaction between silanols and a decrease in water solubility due to a decrease in the amount of silanol groups.

[0038] In the hydrolysis reaction, an organic solvent may be used as necessary within a range that does not inhibit the reaction. The organic solvent used is preferably one that is compatible with water, which is the reaction raw material, and is preferably an alcohol, an ester, a ketone, an ether, or the like. In addition, taking into consideration the distillation conditions for removing the generated alcohol, the organic solvent preferably has a low boiling point, and is preferably a solvent having a boiling point of 150° C. or less under atmospheric pressure. Specific examples of alcohols include methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentyl alcohol, neopentyl alcohol, hexyl alcohol, and cyclohexyl alcohol. Specific examples of esters include ethyl acetate and butyl acetate. Specific examples of ketones include acetone, methyl ethyl ketone, and cyclohexanone. Specific examples of ethers include tetrahydrofuran, tetrahydropyran, and dioxane.

[0039] The reaction conditions are preferably such that the silane monomer is mixed with water and stirred at 55 to 70°C for 1 to 5 hours to allow the hydrolysis and condensation reaction of the silane monomer to proceed, and then the water / alcohol mixture is distilled off under reduced pressure at a temperature range of 30 to 80°C.

[0040] The 3-glycidyloxypropylsilanol oligomer used in the present invention preferably has a water and free alcohol content of 1% by mass or less. Such a composition can be used as a substance free of volatile organic compounds (VOCs), which is advantageous for reducing the VOC content of the entire silicone composition to which it is added. In the present invention, the absence of VOCs means that the content of free alcohol in the oligomer or the composition of the present invention is preferably 1% by mass or less. Here, alcohol refers to methanol or ethanol in particular. Although water does not fall under VOCs, if present in excess, it may react with epoxy groups, so it is desirable to avoid water as much as possible. If the content is 1% by mass or less, there is little risk of the active ingredient decreasing due to volatilization during storage, or alcohols being generated by hydrolysis due to moisture in the silicone composition or moisture in the air, and there is no concern about foaming or pinholes occurring during heat curing of the silicone composition, and a drying process before use is not required.

[0041] The amount of 3-glycidyloxypropylsilanol oligomer (C) added is 0.1 to 15 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 1 to 8 parts by mass, relative to 100 parts by mass of the (A) component. If the amount of (C) added is less than 0.1 parts by mass, plastic reversion occurs, causing problems in subsequent processability, and in the worst case, the compound composition cannot be obtained. If the amount of (C) added is more than 15 parts by mass, the compound composition obtained becomes sticky, causing subsequent processability to deteriorate, and the mechanical properties of the silicone rubber obtained by curing the compound composition are reduced.

[0042] (2) Manufacturing method of silicone rubber compound The method for producing the silicone rubber compound according to the present invention is not particularly limited, but for example, the silicone rubber compound of the present invention can be obtained by uniformly mixing the above-mentioned components using a rubber kneader such as a two-roll mixer, a Banbury mixer, or a dough mixer (kneader), and then subjecting the mixture to a heat treatment as necessary.

[0043] The base compound of the components (A) to (C) may be mixed under heating at a temperature of preferably 0 to 200° C., more preferably 10 to 180° C., and even more preferably 20 to 170° C. The time for mixing the components (A) to (C) is not particularly limited, but is preferably 1 to 300 minutes, more preferably 10 to 120 minutes, in consideration of production efficiency.

[0044] In the case of hot mixing, it is preferable to uniformly mix the prescribed amounts of components (A) to (C) to form a compound, and then perform low-temperature mixing (cold blending) for 10 to 60 minutes in a temperature range of 20 to 80° C. By providing a low-temperature mixing time, there is no need to worry about the silanol oligomer, component (C), being thermally decomposed or volatilized during blending, and the surface treatment reaction of component (B) can be promoted.

[0045] (3) Silicone rubber composition A millable type silicone rubber composition can be obtained by further compounding the millable type silicone rubber compound obtained as described above with (D) a curing agent (vulcanizing agent).

[0046] -(D) Component- The curing agent for component (D) is not particularly limited as long as it can cure component (A), but generally, any known rubber curing agent can be used, such as the following components (D1) and (D2). Of these, the organic peroxide for component (D2) is preferred. (D1) Addition reaction (hydrosilylation reaction) type curing agent, that is, a hydrosilylation reaction curing agent consisting of a combination of an organohydrogenpolysiloxane (crosslinking agent) and a hydrosilylation catalyst. (D2)Organic peroxide

[0047] (D1) Addition reaction type curing agent (a) Organohydrogenpolysiloxane The organohydrogenpolysiloxane used as the crosslinking agent of the above-mentioned (D1) addition reaction type curing agent is preferably one having two or more hydrosilyl groups in one molecule, and is particularly preferably an organohydrogenpolysiloxane represented by the following formula (2).

[0048] [ka]

[0049] Here, R 4 are each independently a hydrogen atom, and a group selected from an alkyl group having 1 to 8 carbon atoms, preferably 1 to 6 carbon atoms; a cycloalkyl group having 6 to 10 carbon atoms, preferably 6 to 8 carbon atoms; an aryl group having 6 to 10 carbon atoms, preferably 6 to 8 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms, preferably 7 to 9 carbon atoms. However, there may be 2 or more, preferably 2 to 200, more preferably 2 to 130 R 4 is a hydrogen atom. Note that there cannot be more than one hydrogen atom on the same silicon atom.

[0050] R 4 The alkyl group may be either linear or branched, and specific examples thereof include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, and hexyl groups. Specific examples of the cycloalkyl group include cyclopentyl and cyclohexyl groups. Specific examples of the aryl group include phenyl and tolyl groups. Specific examples of the aralkyl group include benzyl and 2-phenylpropyl groups. In addition, fluoroalkyl groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine atoms may also be used.

[0051] e is an integer satisfying 2≦e≦30, preferably 2≦e≦20. f is an integer satisfying 0≦f≦300, preferably 3≦f≦200. g is an integer satisfying 0≦g≦10, preferably 0≦g≦5. h is an integer satisfying 0≦h≦30, preferably 0≦h≦20. The siloxane units may be bonded in a block or random manner.

[0052] The molecular structure of the organohydrogenpolysiloxane may be any of linear, cyclic, branched, and three-dimensional network structures. In this case, the number of silicon atoms (or degree of polymerization) in one molecule is preferably 2 to 300, more preferably about 4 to 200, and those that are liquid at 25°C are preferably used. The hydrosilyl group may be at the molecular chain terminal, in the side chain (in the middle of the molecular chain), or in both. The method for measuring the degree of polymerization is as explained for component (A). The organohydrogenpolysiloxane may be used alone or in combination of two or more kinds.

[0053] Specific examples of such organohydrogenpolysiloxanes include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, tris(dimethylhydrogensiloxy)methylsilane, tris(dimethylhydrogensiloxy)phenylsilane, methylhydrogenpolysiloxane capped at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer capped at both ends with trimethylsiloxy groups, dimethylpolysiloxane capped at both ends with dimethylhydrogensiloxy groups, Methylhydrogensiloxane-dimethylsiloxane copolymer capped with methylhydrogensiloxane and methylhydrogensiloxane, copolymer of methylhydrogensiloxane and diphenylsiloxane capped with trimethylsiloxy groups at both ends, copolymer of methylhydrogensiloxane, diphenylsiloxane and dimethylsiloxane capped with trimethylsiloxy groups at both ends, cyclic methylhydrogenpolysiloxane, copolymer of cyclic methylhydrogensiloxane and dimethylsiloxane, copolymer of cyclic methylhydrogensiloxane, diphenylsiloxane and dimethylsiloxane, (CH3)2HSiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (C6H5)SiO 3 / 2 and copolymers consisting of these units and the like, and compounds in which some or all of the methyl groups in the above exemplary compounds have been substituted with other alkyl groups such as ethyl groups and propyl groups, or aryl groups such as phenyl groups. Specific examples of such organohydrogenpolysiloxanes include compounds of the following structural formulas:

[0054] [ka] (In the formula, k is an integer of 2 to 10, s and t are each an integer of 0 to 10, and p and q are each an integer of 1 to 30.)

[0055] The organohydrogenpolysiloxane of component (a) preferably has a viscosity of 0.5 to 10,000 mPa·s, and more preferably 1 to 300 mPa·s, at 25° C. The viscosity is a value measured using a rotational viscometer according to the method described in JIS K7117-1:1999.

[0056] The organohydrogenpolysiloxane of component (a) is desirably blended in an amount such that the molar ratio of hydrosilyl groups in the organohydrogenpolysiloxane to alkenyl groups bonded to silicon atoms in component (A) (hydrosilyl groups / alkenyl groups) is preferably 0.5 to 10, more preferably 0.8 to 6, and even more preferably 1 to 5. If the ratio is less than 0.5, crosslinking will be insufficient and sufficient mechanical strength may not be obtained after curing, while if the ratio exceeds 10, the physical properties after curing will decrease, and in particular the heat resistance and compression set resistance may be significantly deteriorated.

[0057] (b) Hydrosilylation catalyst The hydrosilylation catalyst used in the above (D1) addition reaction type curing agent is a catalyst that promotes the addition reaction between the alkenyl groups in the above component (A) and the hydrosilyl groups in the above organohydrogenpolysiloxane serving as a crosslinking agent. Examples of hydrosilylation catalysts include platinum group metal catalysts such as ruthenium and platinum. Platinum group metal catalysts include platinum group metals and their compounds. For these, catalysts that have been known as catalysts for addition reaction curing silicone rubber compositions can be used. Specific examples thereof include platinum-based catalysts such as particulate platinum metal adsorbed on a carrier such as platinum black, silica, alumina, or silica gel, platinic chloride, chloroplatinic acid, a reaction product of chloroplatinic acid with a monohydric alcohol, a complex of chloroplatinic acid with an olefin, a complex of chloroplatinic acid with a vinyl group-containing (poly)siloxane, a complex of chloroplatinic acid with a phosphorous ester, and a complex of these with a vinyl group-containing (poly)siloxane; a palladium catalyst; a rhodium catalyst; a ruthenium catalyst, etc. Among these, platinum or a platinum compound is particularly preferred.

[0058] The amount of hydrosilylation catalyst added may be a so-called catalytic amount capable of promoting the addition reaction, and is usually preferably 1 ppm to 1 mass %, more preferably 10 to 500 ppm, calculated as the mass of platinum group metal relative to the mass of component (A). If the amount added is less than 1 ppm, the addition reaction may not be promoted sufficiently, leading to insufficient curing, whereas if the amount added exceeds 1 mass %, the effect on reactivity is small even if more is added, and this may be uneconomical.

[0059] In addition to the above catalysts, an addition crosslinking regulator may be used to adjust the curing rate, specific examples of which include ethynylcyclohexanol, tetramethyltetravinylcyclotetrasiloxane, etc.

[0060] (D2)Organic peroxide On the other hand, examples of the (D2) organic peroxide include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, 2,4-dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-butyl peroxide, t-butyl perbenzoate, 1,6-hexanediol-bis-t-butylperoxycarbonate, etc. Among these, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane is preferred.

[0061] The amount of organic peroxide added is an effective curing amount, and is preferably 0.1 to 8 parts by mass, more preferably 0.2 to 3 parts by mass, relative to 100 parts by mass of component (A). If the amount added is sufficient, the crosslinking reaction proceeds sufficiently, and deterioration of physical properties such as a decrease in hardness, insufficient rubber strength, and an increase in compression set does not occur. In addition, if the amount added does not exceed the above amount, it is economically preferable, and the amount of decomposition product of the curing agent is sufficiently small, and deterioration of physical properties such as an increase in compression set and discoloration of the obtained sheet do not increase.

[0062] -Other ingredients- In addition to the above-mentioned components, the millable type silicone rubber composition of the present invention may optionally contain electrical conductivity imparting agents such as carbon black, flame retardant imparting agents such as iron oxides and halogen compounds, antistatic agents, softeners, antioxidants, ultraviolet absorbers, colorants, etc., within the scope of the invention not impairing its effects.

[0063] (4) Method for producing and curing the composition The method for producing the silicone rubber composition according to the present invention is not particularly limited, but it can be obtained, for example, by the same method as the method for producing the silicone rubber compound described above. In this case, for example, it is preferable to previously mix (A) organopolysiloxane, (B) fine powder silica-based filler as reinforcing silica, (C) silanol oligomer, etc. to prepare a base compound, and then add and mix (D) curing agent to this.

[0064] The millable type silicone rubber composition of the present invention thus obtained can be cured at preferably 80 to 300°C, more preferably 100 to 200°C, for preferably 1 minute to 10 hours, more preferably 5 minutes to 5 hours, to obtain a silicone rubber cured product. EXAMPLES

[0065] The present invention will be specifically described below using synthesis examples, comparative synthesis examples, examples, and comparative examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass", respectively. The devices and measurement conditions used in the examples are as follows.

[0066] (1) GPC Measurement Conditions (Measurement of Weight Average Molecular Weight) Equipment: Tosoh Corporation HLC-8320GPC Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-H TSKgel SuperHM-N(6.0mmI.D.×15cm×1) TSKgel SuperH2500(6.0mmI.D.×15cm×1) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 50 μL (2.0% by mass in THF solution) Standard: Monodisperse polystyrene (2) Proton nuclear magnetic resonance spectrum ( 1 H-NMR spectrum) measurement conditions Equipment: BURKER AVANCE III400 Solvent: CDCl3 (deuterated chloroform) Internal standard: tetramethylsilane (TMS) (3) Kinematic viscosity: Cannon-Fenske viscosity measured according to the method described in JIS Z8803:2011 The measurements were performed at 25°C using a thermometer.

[0067] (4) Measurement of plasticity: The silicone rubber compound was kneaded 15 times with a three-roll mill. After 10 minutes (initial stage), measure the plasticity according to the method described in JIS K6249:2003. The plasticity after aging at 40°C for 24 hours (accelerated at 40°C) was also measured in the same manner. The storage stability of silicone rubber compounds was investigated. If the difference in plasticity between the two is 50 or more, it is determined that the long-term storage stability is deteriorated. A difference of less than 50 was considered to be acceptable.

[0068] (5) Measurement of physical properties of cured silicone rubber: 100 parts of silicone rubber compound described below Add a specified amount of hardener (D) to the mixture, mix uniformly with two rolls, and then The composition was heated at 120°C for 10 minutes (Example 5, Comparative Example 6) or at 165°C for 10 minutes ( In Examples 1 to 4 and Comparative Examples 1 to 5, press curing was performed. Then, the mixture was heated at 200° C. for 4 hours. After post-curing between test sheets, 2 mm thick, 6 mm thick, and 29.5 mm thick A cylindrical rubber molding of Φ was prepared. The density and hardness (Du) of the molded object were measured based on the description in JIS K6249:2003. The compression set (180°C / 22 hours, 25% compression) and permanent compression set (180°C / 22 hours) were measured. In addition, the resilience was measured according to the method described in JIS K6255:2013. A rubber with high elastic modulus and low compression set is considered to have good rubber properties. did.

[0069] [1] Synthesis of 3-glycidyloxypropylsilanol oligomer [Synthesis Example 1] Synthesis of component (C-1) 472 g (2.0 mol) of 3-glycidyloxypropyltrimethoxysilane was placed in a 1 L three-neck flask equipped with a stirrer, a cooling tube, a dropping funnel, and a thermometer. 108 g (6.0 mol as the amount of water) of 0.2% hydrochloric acid was dropped into this. During the dropping, the temperature was appropriately cooled and controlled so that the internal temperature was in the range of 20 to 40°C. After the dropping was completed, the mixture was heated and stirred at 70°C for 1 hour to proceed with the hydrolysis and condensation reaction of the methoxysilyl group, and then the by-product methanol and excess water were distilled off under reduced pressure at 70°C to obtain a colorless and transparent liquid. This liquid is compatible and soluble in any water, and the kinematic viscosity of the resulting oligomer is 726 mm 2 The epoxy functional group content was 189 g / mol, and the weight average molecular weight was 830. 1 As a result of analysis by 1 H-NMR, GPC, etc., this was found to have the average composition structure shown in the following formula (3). 1 The H-NMR spectrum chart is shown in Figure 1.

[0070] [ka]

[0071] [Synthesis Example 2] Synthesis of component (C-2) The target 3-glycidyloxypropyl group-containing silanol oligomer was obtained in the same manner as in Synthesis Example 1, except that the amounts of 3-glycidyloxypropyltrimethoxysilane and dimethyldimethoxysilane were 236 g (1.0 mol), 120 g (1.0 mol), and 90 g (5.0 mol as water) of 0.2% hydrochloric acid were used. The kinematic viscosity of the obtained oligomer was 218 mm 2 The epoxy functional group content was 258 g / mol, and the weight average molecular weight was 700. 1 As a result of analysis by 1 H-NMR and GPC measurement, this product had the structure shown in formula (4) below.

[0072] [ka]

[0073] [Synthesis Example 3] Synthesis of component (C-3) The target 3-glycidyloxypropyl group-containing silanol oligomer was obtained in the same manner as in Synthesis Example 1, except that the amounts of 3-glycidyloxypropyltrimethoxysilane and 3-glycidyloxypropylmethyldimethoxysilane were 425 g (1.8 mol), 44 g (0.2 mol), and 104.4 g (5.8 mol as water) of 0.2% hydrochloric acid were used. The kinematic viscosity of the obtained oligomer was 361 mm 2 The epoxy functional group content was 200 g / mol, and the weight average molecular weight was 510. 1 As a result of analysis by 1 H-NMR and GPC measurement, this product had the structure shown in formula (5) below.

[0074] [ka]

[0075] [Comparative Synthesis Example 4] Synthesis of component (compared to C-4) A silanol group-containing oligomer not containing 3-glycidyloxypropyl groups was obtained in the same manner as in Synthesis Example 1, except that 31.2 g (0.3 mol) of trimethylmethoxysilane, 48.0 g (0.4 mol) of dimethyldimethoxysilane, and 40.8 g (0.3 mol) of methyltrimethoxysilane were used instead of 3-glycidyloxypropyltrimethoxysilane. The kinematic viscosity of the obtained oligomer was 15 mm 2 / s and the weight average molecular weight was 1,150. 1 As a result of analysis by 1 H-NMR and GPC measurement, this product had the structure shown in formula (6) below.

[0076] [ka]

[0077] [Comparative Synthesis Example 5] Synthesis of component (C-5 ratio) A linear polymer having silanol ends at both ends and not containing 3-glycidyloxypropyl groups was obtained by the same procedure as in Synthesis Example 1, except that 120 g (1.0 mol) of dimethyldimethoxysilane was used instead of 3-glycidyloxypropyltrimethoxysilane, and 90 g (5.0 mol as water) of 0.2% hydrochloric acid was used. The kinematic viscosity of the resulting polymer was 13 mm 2 / s and the weight average molecular weight was 270. 1 As a result of analysis by 1 H-NMR and GPC measurement, this product had the structure shown in formula (7) below.

[0078] [ka]

[0079] [2] Ingredients The components used in the examples and comparative examples of the present invention are shown below. (A) Organopolysiloxane rubber An organopolysiloxane gum consisting of 99.825 mol % dimethylsiloxane units, 0.15 mol % methylvinylsiloxane units, and 0.025 mol % dimethylvinylsiloxy units, with one vinyl group bonded to a silicon atom at each end of the molecular chain and ten vinyl groups at each side chain of the molecular chain, and with an average degree of polymerization of 8,000. (B) Reinforcing Silica (B-1) Reinforcing silica with an untreated BET specific surface area of ​​200 m 2 / g of fumed silica (product name: Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) (B-2) Reinforcing silica with a BET specific surface area of ​​110 m2 and surface-treated with dimethyldichlorosilane 2 The fumed silica (product name: R-972, manufactured by Nippon Aerosil Co., Ltd.) having a carbon content of 0.9% was used. (C) 3-Glycidyloxypropylsilanol oligomer (C-1): Oligomer synthesized in Synthesis Example 1 (C-2): Oligomer synthesized in Synthesis Example 2 (C-3): Oligomer synthesized in Synthesis Example 3 (Comparative ingredients) (Comparative to C-4): Oligomer synthesized in Comparative Synthesis Example 4 (Comparative to C-5): Polymer synthesized in Comparative Synthesis Example 5 (Compared to C-6): 3-glycidyloxypropyltrimethoxysilane (product name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity 3.0 mm 2 / s, molecular weight 236) (D) Hardener (D-1) Addition reaction type curing agent: (a) Organohydrogenpolysiloxane represented by the following formula (8) (manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity 17 mm 2 / s)0.85 copies, (b) 0.01 parts of a platinum catalyst (manufactured by Shin-Etsu Chemical Co., Ltd.) containing 1% by mass of platinum atom of chloroplatinic acid-divinyldisiloxane complex as a hydrosilylation catalyst; Also, 0.05 parts of ethynylcyclohexanol was added to 100 parts of the silicone rubber compound as an addition reaction inhibitor.

[0080] [ka] (D-2) Organic peroxide curing agent: 0.5 parts of 2,5-dimethyl-2,5-di-(t-butylperoxy)hexane was added to 100 parts of the silicone rubber compound.

[0081] [3] Manufacturing and evaluation of silicone rubber compounds [Example 1-1] 100 parts of (A) organopolysiloxane raw rubber were charged with 25 parts of (B-1) reinforcing silica and 3 parts of (C-1) as 3-glycidyloxypropylsilanol oligomer in a kneader with a heating function, and the above components were mixed at room temperature until they were uniformly mixed, and then cold blended for 30 minutes. After that, the mixture was heated to 170°C using the heating temperature control function of the kneader and heated and kneaded for 2 hours to obtain silicone rubber compound 1. The plasticity of the obtained compound 1 was measured. The results are shown in Table 1.

[0082] [Examples 1-2 to 1-4, Comparative Examples 1-1 to 1-5] Silicone rubber compounds 2 to 4 and comparative silicone rubber compounds 1 to 5 were obtained in the same manner as in Example 1-1, except that instead of 3 parts of component (C-1), components (C-2), (C-3), and (C-4 ratio) to (C-6 ratio) were used in the proportions shown in Table 1. The plasticity of the obtained silicone rubber compounds was measured. The results are shown in Table 1.

[0083] [Examples 1-5, Comparative Examples 1-6] 100 parts of (A) organopolysiloxane raw rubber was charged with 40 parts of (B-2) reinforcing silica, and 5 parts of (C-2) (Example 1-5) or 5 parts (Comparative Example 1-6) (compared to C-4) as 3-glycidyloxypropylsilanol oligomer in a kneader, and the above components were simply mixed for 2 hours until they were uniformly mixed, to obtain silicone rubber compound 5 (Example 1-5) or comparative silicone rubber compound 6 (Comparative Example 1-6). The maximum temperature reached was 76°C. The plasticity of the obtained compound was measured. The results are shown in Table 1.

[0084] [4] Manufacture of silicone rubber composition, manufacture and evaluation of cured products [Example 2-1] 100 parts of the above silicone rubber compound 1 and 0.5 parts of the curing agent (D-2) were mixed uniformly using a two-roll mill. Then, the mixture was molded by heating at 165°C for 10 minutes, and then post-cured at 200°C for 4 hours to prepare a 2 mm thick test sheet and a 6 mm thick, 29.5 mm diameter cylindrical rubber molded product. The obtained sheets or cylindrical rubber moldings were used to evaluate the rubber properties shown in Table 1. The results are also shown in Table 1.

[0085] [Examples 2-2 to 2-4, Comparative Examples 2-1 to 2-5] Except for using silicone rubber compounds 2 to 4 and comparative silicone rubber compounds 1 to 5 instead of silicone rubber compound 1, silicone rubber compositions were prepared in the same manner as in Example 2-1, rubber sheets and cylindrical rubber moldings were produced in the same manner as in Example 1, and various rubber properties were evaluated. The results are shown in Table 1.

[0086] [Examples 2-5, Comparative Examples 2-6] A predetermined amount of curing agent (D-1) was added to 100 parts of the above silicone compound 5 (Example 2-5) or comparative silicone rubber compound 6 (Comparative Example 2-6), and the mixture was mixed uniformly using a two-roll mill. The mixture was then molded in a mold at 120°C for 10 minutes, and post-cured at 200°C for 4 hours to produce a 2 mm thick test sheet and a 6 mm thick, 29.5 mm diameter cylindrical rubber molded product. The rubber properties shown in Table 1 were evaluated using the obtained rubber sheets or cylindrical rubber moldings. The results are also shown in Table 1.

[0087] [Table 1]

[0088] [Evaluation Results] Each of the silicone rubber compounds obtained in Examples 1-1 to 1-5 satisfied the requirements of the present invention. As shown in Table 1, the initial plasticity of each of the millable type silicone rubber compounds of the Examples to which the 3-glycidyloxypropylsilanol oligomer of component (C) was added was high, and the increase in plasticity after 40°C / 24h was kept low, indicating that they had excellent long-term storage properties.

[0089] In contrast, in Comparative Example 1-1, the component (C) was a silanol oligomer that did not contain a 3-glycidyloxypropyl group, and the initial plasticity was low and the long-term storage stability was also unacceptable.

[0090] In Comparative Example 1-2, a linear silanol polymer not containing 3-glycidyloxypropyl groups is used in component (C), and although the silica surface is well treated and the long-term storage stability is good, the plasticity is significantly lowered. Comparative Example 1-4 is the same as Comparative Example 1-2 except that the amount of wetter is reduced by half. The initial plasticity is high and good, but the silica surface is not treated, and the plasticity increases significantly after 40°C / 24h, showing that high plasticity and long-term storage stability are not compatible.

[0091] Comparative Example 1-3 is a compound to which 3-glycidyloxypropyltrimethoxysilane (KBM-403), which is the starting material for the 3-glycidyloxypropylsilanol oligomer of component (C-1), was added. However, the initial plasticity was low and the change in plasticity after 24 hours at 40°C was large, making it unacceptable. Furthermore, the compression set of the cured product of the composition of Comparative Example 2-3 was significantly worse than that of the cured product of the composition of Comparative Example 2-1, indicating that it does not function as a surface treatment agent for silica.

[0092] Examples 1-4 and Comparative Examples 1-5 are comparative studies of a combination of a linear silanol polymer and a silanol oligomer having a 3-glycidyloxypropyl group, and a combination of a linear silanol polymer and a silanol oligomer not containing a 3-glycidyloxypropyl group. It can be seen that even when a linear silanol polymer is used in combination, high plasticity and long-term storage stability are maintained by the addition of 3-glycidyloxypropyl silanol oligomer.

[0093] Examples 1-5 and Comparative Examples 1-6 were used to verify the effect of 3-glycidyloxypropylsilanol oligomer in a simple blend system in which treated silica was used and no heat treatment was performed. It was confirmed that even in a simple blend system, the addition of 3-glycidyloxypropylsilanol oligomer resulted in high plasticity and good long-term storage stability.

[0094] From the above results, it was found that the silicone rubber compounds of Examples 1-1 to 1-5 to which 3-glycidyloxypropylsilanol oligomer was added had high plasticity and excellent long-term storage stability.

Claims

1. (A) organopolysiloxane gum having two or more alkenyl groups bonded to silicon atoms in each molecule and an average degree of polymerization of 3,000 to 100,000: 100 parts by mass, (B) A specific surface area measured by the BET adsorption method is 50 to 450 m 2 / g reinforcing silica: 5 to 50 parts by mass, (C) 3-glycidyloxypropylsilanol oligomer represented by the following formula (1): 0.1 to 15 parts by mass 【Chemistry 1】 (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a glycidyloxy group, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, a, b, c, and d are numbers that satisfy a ≧ 0.5, b ≧ 0, c ≧ 0, d ≧ 0, and a + b + c + d = 1, and x and y are numbers that satisfy x ≧ 1.0, y ≦ 0.

5. A millable type silicone rubber compound comprising:

2. 2. The millable type silicone rubber compound according to claim 1, wherein the weight average molecular weight of component (C) is 500 to 10,000.

3. 2. The millable type silicone rubber compound according to claim 1, wherein in the above formula (1), b, c, and d are numbers that satisfy b=0, 0≦c≦0.5, and 0≦d≦0.

2.

4. 100 parts by mass of the millable type silicone rubber compound according to any one of claims 1 to 3, (D) Curing agent: effective curing amount A millable type silicone rubber composition comprising:

5. The component (D) is an addition reaction type curing agent (D1), and the component (D1) is (a) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in the organohydrogenpolysiloxane (a) to alkenyl groups bonded to silicon atoms in component (A) (hydrosilyl groups / alkenyl groups) is 0.5 to 10; and (b) Hydrosilylation catalyst: 1 ppm to 1% by mass calculated as the mass of platinum group metal based on the mass of component (A). The millable silicone rubber composition according to claim 4, which comprises

6. 5. The millable silicone rubber composition according to claim 4, wherein the component (D) is an organic peroxide curing agent (D2), and the millable silicone rubber composition contains 0.1 to 8 parts by mass of the component (D2) per 100 parts by mass of the millable silicone compound.

Citation Information

Patent Citations

  • Silicone rubber composition for extrusion molding and method for producing the same

    JP2008127415A

  • Curable silicone composition and cured product thereof

    JP2014065900A

  • Hot-meltable curable silicone composition, sealant, film, opto-semiconductor element

    JP2021021058A

  • Silicone composition for die bonding, cured product of the same, and optical semiconductor device

    JP2021167364A

  • Curable organopolysiloxane composition having excellent cold resistance, pattern forming method, electronic components, etc.

    WO2020080326A1