Fluorine-containing yttrium sintered compact and method for producing the same
A fluorine-containing yttrium sintered body with controlled conductivity and strength facilitates yttrium oxyfluoride film formation by DC discharge, addressing the challenges of existing methods and reducing equipment size and cost.
Patent Information
- Application Number
- JP2023078500
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Yttrium oxyfluoride films cannot be effectively formed using DC discharge due to its insulating nature, requiring fluorine gas introduction and large-scale, expensive equipment, making the process difficult.
A fluorine-containing yttrium sintered body with specific composition and properties, enabling film formation by DC discharge without fluorine gas, comprising 10-30% fluorine, 70-90% yttrium, and a relative density of 90% or more, with Y and YF3 crystal phases, allowing for electrical conductivity and high bending strength.
Enables the formation of yttrium oxyfluoride films using DC discharge, reducing equipment size and cost, and preventing cracking during sputtering.
Smart Images

Figure 2024162696000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a fluorine-containing yttrium sintered body, particularly a fluorine-containing yttrium sintered body suitable for a sputtering target for forming an yttrium oxyfluoride film, and a method for producing the same. [Background technology]
[0002] In the manufacturing process of semiconductor devices, etc., microfabrication is performed by dry etching using high density plasma. In dry etching, the processing members themselves, such as jigs, are also affected by the etching as the semiconductor devices are processed. Therefore, materials that are less affected by dry etching are required for the processing members, and yttrium oxyfluoride has attracted attention as such a material.
[0003] In general, a processed member for dry etching is manufactured by forming an yttrium oxyfluoride film on the surface of a substrate made of quartz or the like. For example, a member on which an yttrium oxyfluoride film is formed by using yttrium oxyfluoride (YOF) as a film-forming material and a sputtering method using RF discharge is known. In addition, Patent Document 1 discloses an industrial process in which an yttrium oxyfluoride film is formed by using yttrium (Y) as a film-forming material and a sputtering method while introducing oxygen and fluorine gas. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-84788 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, since yttrium oxyfluoride is an insulator, it is not possible to form an yttrium oxyfluoride film by sputtering using DC discharge. In sputtering using DC discharge with yttrium as a film forming material, the introduction of fluorine gas is essential, and a detoxification facility is required, so the film forming apparatus tends to be large and expensive, making it very difficult to apply industrially.
[0006] The present disclosure aims to provide at least one of a film-forming material for an yttrium oxyfluoride film and a manufacturing method thereof, a sputtering target, and a manufacturing method for a substrate with an yttrium oxyfluoride film, which are capable of forming an yttrium oxyfluoride film by a sputtering method using DC discharge without requiring fluorine gas. [Means for solving the problem]
[0007] The present inventors have investigated a film-forming material that allows film formation by a sputtering method using a DC discharge method. As a result, they have noticed that the conductivity of the film-forming material can be controlled by compounding yttrium (Y) and a fluorine-containing yttrium compound at a specific ratio, and have found that by controlling the composition, a film-forming material having conductivity that allows the formation of an yttrium oxyfluoride film by a sputtering method using a DC discharge can be obtained.
[0008] That is, the present invention is as described in the claims, and the gist of the present disclosure is as follows. [1] A fluorine-containing yttrium sintered body having a composition in which the fluorine content is 10% by mass or more and 30% by mass or less, the yttrium content is 70% by mass or more and 90% by mass or less, the relative density is 90% or more, and the crystalline phase includes the Y phase and the YF3 phase. [2] The fluorine-containing yttrium sintered body according to [1], having a volume resistivity of 1.0 Ω cm or less. [3] The fluorine-containing yttrium sintered body according to [1] or [2], having a flexural strength of 50 MPa or more. [4] A method for producing a fluorine-containing yttrium sintered body according to any one of [1] to [3], comprising: a mixing step of mixing yttrium (Y) powder at a ratio of 25% by mass or more and 75% by mass or less and yttrium fluoride (YF3) powder at a ratio of 25% by mass or more and 75% by mass or less, so that the total of yttrium (Y) powder and yttrium fluoride (YF3) powder is 100% by mass, to obtain a raw material powder; and a heat treatment step of pressurizing and sintering the raw material powder at 700°C or more in an inert atmosphere. [5] A sputtering target comprising the fluorine-containing yttrium sintered body according to any one of [1] to [3]. [6] A method for producing a substrate with an yttrium oxyfluoride film, comprising forming an yttrium oxyfluoride film on a substrate by a sputtering method using the sputtering target according to [5] to produce a substrate with an yttrium oxyfluoride film. Effect of the Invention
[0009] The present disclosure makes it possible to provide at least one of a film-forming material for an yttrium oxyfluoride film and a manufacturing method thereof, a sputtering target, and a manufacturing method for a substrate with an yttrium oxyfluoride film, which are capable of forming an yttrium oxyfluoride film by a sputtering method using DC discharge without requiring fluorine gas. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present disclosure will be described in detail below. However, the following description of the components is merely an example of an embodiment of the present disclosure, and the present disclosure is not limited to the contents thereof. [Fluorine-containing yttrium sintered body] The present embodiment is a fluorine-containing yttrium sintered body having a composition in which the fluorine content is 10% by mass or more and 30% by mass or less, the yttrium content is 70% by mass or more and 90% by mass or less, the relative density is 90% or more, and the crystalline phase includes the Y phase and the YF3 phase. Such a fluorine-containing yttrium sintered body (hereinafter also referred to as "the sintered body of the present embodiment") can be used as a sputtering target (hereinafter also simply referred to as "target") that enables the production of an yttrium oxyfluoride film by a sputtering method using DC discharge.
[0011] The sintered body of the present embodiment is a fluorine-containing yttrium sintered body, which is a sintered body having a matrix of a component whose constituent elements are fluorine (F) and yttrium (Y), and is preferably an yttrium-yttrium fluoride sintered body.
[0012] The sintered body of this embodiment has a composition in which the fluorine content is 10% by mass or more and 30% by mass or less, and the yttrium content is 70% by mass or more and 90% by mass or less. If the fluorine content is less than 10% by mass, it is difficult to form an yttrium oxyfluoride film by sputtering using DC discharge, and if the fluorine content exceeds 30% by mass, the volume resistivity of the sintered body increases and DC discharge cannot be performed. The fluorine content is preferably 15% by mass or more and 30% by mass or less, and more preferably 15% by mass or more and 25% by mass or less. The yttrium content is preferably 70% by mass or more and 85% by mass or less, and more preferably 75% by mass or more and 85% by mass or less.
[0013] In the sintered body of the present embodiment, the fluorine content and the yttrium content are calculated from the following formulas.
[0014] Fluorine content = b F / (a+b) Yttrium content = (a + b Y ) / (a+b) In the above formula, a is the mass of yttrium contained in the sintered body [g], b is the mass of yttrium fluoride contained in the sintered body [g], b Y is the mass of yttrium contained in yttrium fluoride [g], b F is the mass of fluorine contained in yttrium fluoride [g].
[0015] The sintered body of this embodiment preferably has a composition in which fluorine and yttrium make up 100% by mass, but may contain unavoidable impurities as long as the effect is achieved. Examples of the unavoidable impurities include one or more metal elements selected from the group consisting of silicon (Si), aluminum (Al), calcium (Ca) and iron (Fe), or compounds thereof. The content of the unavoidable impurities can be, for example, 0 ppm by mass or more and 5,000 ppm by mass or less, and in this case, the sintered body of this embodiment may have a composition in which fluorine, yttrium and unavoidable impurities make up 100% by mass.
[0016] The relative density of the sintered body of this embodiment is 90% or more, and preferably 95% or more or 97% or more. By having such a relative density, the flexural strength of the sintered body is likely to be high, and cracking of the sputtering target during DC discharge can be suppressed. The higher the relative density, the more preferable it is, but it can be 100% or less or less than 100%. The relative density is preferably 95% or more and 100% or less, and more preferably 97% or more and 100% or less.
[0017] In this embodiment, "relative density" refers to true density (d) [g / cm 3 ] versus bulk density (d') [g / cm 3 ] is the percentage [%] of the bulk density d' [g / cm 3 ] is the volume [cm ] measured by Archimedes' law 3 The true density is calculated from the mass [g] and the dry mass [g]. d=(a+b) / {(a / d Y )+(b / d YF3 )} (A)
[0018] In the above formula, a is the mass [g] of yttrium (Y) contained in the sintered body, and b is the mass [g] of yttrium fluoride contained in the sintered body. Y is the true density of yttrium (4.470 g / cm 3 ) and d YF3 is the true density of yttrium fluoride (YF3) (5.063 g / cm 3 ).
[0019] The crystal phase of the sintered body of this embodiment includes a Y phase and a YF3 phase, and is preferably composed of a Y phase (yttrium phase) and a YF3 phase (yttrium fluoride phase). By including the Y phase and the YF3 phase in the crystal phase, fluorine can be contained in the sintered body while retaining the electrical conductivity derived from yttrium.
[0020] The volume resistivity of the sintered body of this embodiment is preferably 1.0 Ω·cm or less. This allows for sputtering film formation by DC discharge when the sintered body of this embodiment is used as a target. The volume resistivity is 1.0×10 -1 Ω cm or less, 1.0×10 -2 Ω cm or less or 1.0×10 -3 The lower the volume resistivity, the more preferable it is. However, the lower limit of the volume resistivity of the sintered body of this embodiment is 1.0×10 -6 Ω cm or more or 1.0×10 -5 An example would be Ω·cm or more.
[0021] The volume resistivity of the sintered body of this embodiment can be measured by processing the sintered body into a plate of length 10 mm × width 20 mm × thickness 1 mm, applying silver paste to the contact points (four points) of the measurement probe, and using a general resistivity meter (for example, device name: Loresta HP MCP-T410, manufactured by Mitsubishi Chemical Corporation) by a four-terminal method in accordance with JIS K 7194.
[0022] The flexural strength of the sintered body of this embodiment is preferably 50 MPa or more, more preferably 70 MPa or more, or 100 MPa or more. This makes it difficult for the target to crack during sputtering by DC discharge when the sintered body of this embodiment is used as a target. The higher the flexural strength, the more preferable it is, but the upper limit of the flexural strength of the sintered body of this embodiment can be, for example, 500 MPa or less, 300 MPa or less, or 200 MPa or less.
[0023] The flexural strength of the sintered body of this embodiment can be measured by a method in accordance with JIS R 1601.
[0024] Test method: Three-point bending test Distance between fulcrums: 30mm Sample size: 3×4×40mm Head speed: 0.5mm / min
[0025] [Sputtering target] The sintered body of the present embodiment can be used for known applications of fluorine-containing yttrium, but is preferably used as a sputtering target, and more preferably used as a sintered body for a sputtering target.
[0026] A sputtering target comprising the sintered body of this embodiment (hereinafter also referred to as "the target of this embodiment") may consist of the sintered body of this embodiment, or may be a target comprising a backing plate and the sintered body of this embodiment.
[0027] Hereinafter, the target of this embodiment will be described by taking as an example a sputtering target including a backing plate and the sintered body of this embodiment.
[0028] The backing plate may be made of any material that can conduct electricity and dissipate heat during sputtering, and examples of such materials include backing plates made of one or more materials selected from the group consisting of copper (Cu), aluminum (Al), titanium (Ti), and SUS.
[0029] In the target of this embodiment, the sintered body of this embodiment is bonded to a backing plate. The sintered body of this embodiment and the backing plate may be bonded directly or through a bonding material. The bonding material may be a known material, such as indium (In).
[0030] The shape of the target of this embodiment may be any shape suitable for sputtering, and examples thereof include one or more shapes selected from the group consisting of a plate shape, a columnar shape, and a cylindrical shape.
[0031] In order to increase the deposition area, the area of the sputtering surface of the target in this embodiment is 200 cm 2 More than 350cm 2 or more than 800cm 2 The area of the sputtering surface is preferably 1500 cm or more. 2 or less than 1200cm 2 The following are some of the reasons:
[0032] [Method of manufacturing sintered body] The method for producing the sintered body of this embodiment is arbitrary, but a preferred method for producing a fluorine-containing yttrium sintered body includes a mixing step of mixing yttrium (Y) powder at a ratio of 25% by mass to 75% by mass and yttrium fluoride (YF3) powder at a ratio of 25% by mass to 75% by mass so that the total of yttrium (Y) powder and yttrium fluoride (YF3) powder is 100% by mass to obtain a raw material powder, and a heat treatment step of pressurizing and firing the raw material powder at 700°C or higher in an inert atmosphere.
[0033] In the mixing step, the yttrium powder is mixed at a ratio of 25% by mass to 75% by mass, and the yttrium fluoride powder is mixed at a ratio of 25% by mass to 75% by mass, so that the total of the yttrium powder and the yttrium fluoride powder is 100% by mass, to obtain a raw material powder. This results in a raw material powder containing yttrium and yttrium fluoride. If the ratio of the yttrium powder exceeds 75% by mass, it is difficult to form a yttrium oxyfluoride film by a sputtering method using DC discharge, and if the ratio of the yttrium powder is less than 25% by mass, the volume resistivity of the sintered body increases and DC discharge cannot be performed.
[0034] The yttrium powder is preferably 25% by mass or more and 65% by mass or less, and more preferably 35% by mass or more and 65% by mass or less. The yttrium fluoride powder is preferably 35% by mass or more and 75% by mass or less, and more preferably 35% by mass or more and 65% by mass or less.
[0035] The average particle size of the yttrium powder may be 1000 μm or less, or 800 μm or less, and may be 150 μm or more, or 300 μm or more.
[0036] The average particle size of the yttrium fluoride powder may be 100 μm or less, or 50 μm or less, and may be 1 μm or more, or 5 μm or more.
[0037] The purity of the yttrium is preferably 3N or more or 4N or more. A preferred yttrium source is metallic yttrium. The purity of the yttrium fluoride is preferably 3N or more or 4N or more.
[0038] The mixing method may be a dry mixing method, and may be one or more pulverizing methods selected from the group consisting of ball mill, jet mill, roll mill, disk mill, airflow pulverization, and bead mill. The pulverization is preferably carried out in an inert atmosphere, and is preferably carried out in one or more atmospheres selected from the group consisting of a nitrogen atmosphere and an argon atmosphere.
[0039] In the heat treatment step, the mixed powder is pressure-sintered in an inert atmosphere at 700° C. or higher. This results in the sintered body of the present embodiment. The sintering method may be pressure-sintering, and specific examples of pressure-sintering include one or more selected from the group consisting of hot pressing, hot isostatic pressing (HIP), and discharge plasma sintering, with hot pressing being preferred.
[0040] The treatment temperature in the heat treatment step is 700°C or higher. If the temperature is lower than the above, the density of the sintered body decreases. Since the density of the obtained sintered body is likely to be improved, the treatment temperature is preferably 800°C or higher, and more preferably 900°C or higher. The upper limit of the treatment temperature is, for example, 1200°C or lower, or 1100°C or lower. In addition, the pressure during pressurized sintering is, for example, 50 MPa or 30 MPa or lower. The lower limit of the pressure is, for example, 10 MPa or higher, or 20 MPa or higher.
[0041] The heat treatment time may be appropriately adjusted depending on the performance of the heat treatment furnace, and may be, for example, from 1 hour to 15 hours.
[0042] The atmosphere in the heat treatment step may be an inert atmosphere, and is preferably one or more atmospheres selected from the group consisting of a nitrogen atmosphere, a helium atmosphere, and an argon atmosphere.
[0043] The sintered body obtained by the above-mentioned heat treatment process may be used as the target of the present embodiment as it is, or may be processed to a desired size to be used as the target of the present embodiment. Also, the above-mentioned sintered body may be bonded to a backing plate to be used as the target of the present embodiment. EXAMPLES
[0044] The present disclosure will be described below with reference to examples. However, the present disclosure is not limited to these examples.
[0045] (Relative Density) The relative density (%) of the sintered body was calculated according to JIS R 1634, as the bulk density (d') of the sintered body relative to the true density (d) of the sintered body, from the following formula: Relative density [%] = (d' / d) x 100
[0046] Bulk density of sintered body d' [g / cm 3 ] is the volume [cm ] measured by Archimedes' law 3 ] and the dry mass [g] of the sintered body.
[0047] True density of sintered body d [g / cm 3 ] was calculated using the following formula (A). d=(a+b) / {(a / d Y )+(b / d YF3 )} (A)
[0048] In the above formula, a is the mass of yttrium contained in the sintered body [g], b is the mass of yttrium fluoride contained in the sintered body [g]d Y is the true density of yttrium (4.470 g / cm 3 ) and d YF3 is the true density of yttrium fluoride (5.063 g / cm 3 ).
[0049] The contents of yttrium and fluoride contained in the sintered body were calculated by the following formulas. Fluorine content = b F / (a+b) Yttrium content = (a + b Y ) / (a+b)
[0050] In the above formula, a is the mass of yttrium contained in the sintered body [g], b is the mass of yttrium fluoride contained in the sintered body [g], b Y is the mass of yttrium contained in yttrium fluoride [g], b F is the mass of fluorine contained in yttrium fluoride [g].
[0051] (flexural strength) The flexural strength of the sintered body was measured by a method conforming to JIS R 1601 under the following conditions.
[0052] Test method: Three-point bending test Distance between fulcrums: 30mm Sample size: 3×4×40mm Head speed: 0.5mm / min
[0053] (crystalline phase) The crystal phase contained in the sintered body was identified from the powder X-ray diffraction (hereinafter also referred to as "XRD") pattern. An XRD device (device name: RINT Ultima III, manufactured by Rigaku Corporation) was used to obtain the XRD pattern of the sintered body by the following measurements.
[0054] Acceleration current / voltage: 40mA / 40kV Radiation source: CuKα radiation (λ=1.5405Å) Measurement mode: Continuous scan Scan condition: 2° / min Measurement range: 2θ=20° to 80° Divergence vertical limit slit: 10mm Divergence / entrance slit: 1 / 2° Receiving slit: 0.3mm The crystal phase of the sintered body was identified by comparing the obtained XRD pattern with the ICDD database.
[0055] (Volume resistivity) The sintered body was processed into a plate of 10 mm length × 20 mm width × 1 mm thickness, and silver paste was applied to the contact points (4 points) of the measurement probe. Measurements were then performed using a resistivity meter (device name: Loresta HP MCP-T410, manufactured by Mitsubishi Chemical Corporation) using the four-terminal method in accordance with JIS K 7194. Correction factor: 3.923 Probe: TFP
[0056] Example 1 Commercially available yttrium powder (purity: 99.9%, average particle size: 700±100 μm, product name: Y metal powder, manufactured by Nippon Yttrium Co., Ltd.) and commercially available yttrium fluoride powder (purity: 99.9%, average particle size: 9.4 μm, product name: yttrium fluoride powder, manufactured by Nippon Yttrium Co., Ltd.) were weighed out so that the mixture was 54.9% by mass of yttrium (Y) powder and 45.1% by mass of yttrium fluoride (YF3) powder. The mixture was then dry-mixed for 1 hour in an argon atmosphere using a ball mill with nylon balls (15 mmφ) to obtain a mixed powder of yttrium and yttrium fluoride.
[0057] The mixed powder was placed in a carbon mold (press die: diameter 15.2 cm) and sintered by hot pressing under the following conditions to obtain a disk-shaped sintered body of this example having a diameter of 15.2 cm and a thickness of 7 mm.
[0058] Firing method: Hot press Heating rate: 200℃ / hour Firing atmosphere: Argon Firing temperature: 1050℃ Firing pressure: 40MPa Baking time: 3 hours The sintered body of this example contained yttrium (Y) and yttrium fluoride (YF3) in the crystal phase, with the yttrium content being 82.4 mass % and the fluorine content being 17.6 mass %.
[0059] Example 2 The sintered body of this example was produced in the same manner as in Example 1, except that the sintering was carried out under the following conditions. Firing method: Hot press Heating rate: 200℃ / hour Firing atmosphere: Argon Firing temperature: 900℃ Firing pressure: 20MPa Baking time: 3 hours
[0060] Example 3 The sintered body of this example was produced in the same manner as in Example 1, except that the sintering was carried out under the following conditions. Firing method: Hot press Heating rate: 200℃ / hour Atmosphere: Argon Firing temperature: 800℃ Pressure: 20MPa Baking time: 3 hours
[0061] Example 4 The sintered body of this example was produced in the same manner as in Example 1, except that yttrium (Y) powder and yttrium fluoride (YF3) powder were weighed out and mixed so that the yttrium (Y) powder was 71.8 mass% and the yttrium fluoride (YF3) powder was 28.2 mass%.
[0062] Example 5 The sintered body of this example was produced in the same manner as in Example 1, except that yttrium (Y) powder and yttrium fluoride (YF3) powder were weighed out and mixed so that the yttrium (Y) powder was 51.4 mass% and the yttrium fluoride (YF3) powder was 48.6 mass%.
[0063] Example 6 The sintered body of this example was produced in the same manner as in Example 1, except that yttrium (Y) powder and yttrium fluoride (YF3) powder were weighed out and mixed so that the yttrium (Y) powder was 28.0 mass% and the yttrium fluoride (YF3) powder was 72.0 mass%. The mixture was fired under the following firing conditions. Firing method: Hot press Heating rate: 200℃ / hour Firing atmosphere: Argon Firing temperature: 1050℃ Firing pressure: 20MPa Baking time: 3 hours
[0064] Comparative Example 1 Commercially available yttrium fluoride powder (purity: 99.9%, average particle size: 9.4 μm, product name: yttrium fluoride powder, manufactured by Nippon Yttrium Co., Ltd.) was placed in a carbon mold (press die: diameter 15.2 cm) and sintered by hot pressing under the following sintering conditions to produce a sintered body for this comparative example.
[0065] Firing method: Hot press Heating rate: 200℃ / hour Firing atmosphere: Argon Firing temperature: 1050℃ Firing pressure: 40MPa Baking time: 3 hours As a result, a disk-shaped sintered body having a diameter of 15.2 cm and a thickness of 7 mm was obtained, which was used as the sintered body of this comparative example.
[0066] Comparative Example 2 The sintered body of this comparative example was produced in the same manner as in Example 1, except that the sintering was carried out under the following conditions. Firing method: Hot press Heating rate: 200℃ / hour Atmosphere: Argon Firing temperature: 650℃ Pressure: 20MPa Baking time: 3 hours
[0067] Comparative Example 3 The sintered body of this comparative example was produced in the same manner as in Example 1, except that yttrium and yttrium fluoride were mixed so that the yttrium (Y) powder was 16.0 mass% and the yttrium fluoride (YF3) powder was 84.0 mass%, and that the sintered body was fired under the following conditions. Firing method: Hot press Heating rate: 200℃ / hour Atmosphere: Argon Firing temperature: 1050℃ Pressure: 20MPa Baking time: 3 hours Table 1 shows the evaluation results of the sintered bodies obtained in the examples and comparative examples.
[0068] [Table 1]
[0069] It was confirmed that the sintered bodies of this embodiment all have a volume resistivity of 1.0 Ω·cm or less and have electrical conductivity that allows the application of sputtering by DC discharge. It was also confirmed that the sintered bodies of this embodiment have a flexural hardness of 50 MPa or more, and even 100 MPa or more, and have a strength that makes them less likely to crack during sputtering.
Claims
1. The composition has a fluorine content of 10% by mass or more and 30% by mass or less, a yttrium content of 70% by mass or more and 90% by mass or less, a relative density of 90% or more, and is a Y phase and a YF 3 A fluorine-containing yttrium sintered body comprising a crystalline phase including a yttrium fluoride phase.
2. 2. The fluorine-containing yttrium sintered body according to claim 1, having a volume resistivity of 1.0 Ω·cm or less.
3. 3. The fluorine-containing yttrium sintered body according to claim 1 or 2, having a bending strength of 50 MPa or more.
4. Yttrium (Y) powder is 25% by mass or more and 75% by mass or less, and yttrium fluoride (YF 3 ) powder in a ratio of 25 mass% to 75 mass% or less, and yttrium (Y) powder and yttrium fluoride (YF 3 ) powders so that the total amount of the powders is 100 mass% to obtain a raw material powder, and a heat treatment process of pressurizing and sintering the raw material powder in an inert atmosphere at 700 ° C. or higher. A method for producing a fluorine-containing yttrium sintered body according to claim 1 or 2.
5. A sputtering target comprising the fluorine-containing yttrium sintered body according to claim 1 or 2.
6. A method for producing a substrate with an yttrium oxyfluoride film, comprising forming an yttrium oxyfluoride film on a substrate by a sputtering method using the sputtering target according to claim 5 to produce a substrate with an yttrium oxyfluoride film.