Release film

The release film with a silicone resin layer and antistatic properties addresses blocking and releasability issues in silicone release films, ensuring consistent and easy peeling without surface damage or foreign matter interference.

JP2024162758APending Publication Date: 2024-11-21MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023078626
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional silicone release films for pressure-sensitive adhesive sheets face issues with easy releasability leading to blocking, peeling electrification, deformation, and uneven wettability, especially when particles are used to prevent blocking, which can cause foreign matter inspection interference and scratches.

Method used

A release film with a specific configuration featuring a resin layer containing a silicone resin release agent, having a thickness of 0.2 to 2.0 μm, and a surface opposite to the resin layer with an average surface roughness of 30 nm or more and a surface area ratio of 3.5×10^-2% or more, utilizing a non-silicone release agent and an antistatic layer to prevent blocking while ensuring ultra-light releasability.

Benefits of technology

The film achieves ultra-light releasability for various adhesives, maintaining consistent release properties without blocking, reducing surface damage, and preventing peeling and uneven wettability, while minimizing particle interference and foreign matter issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162758000001
    Figure 2024162758000001
  • Figure 2024162758000002
    Figure 2024162758000002
  • Figure 2024162758000003
    Figure 2024162758000003
Patent Text Reader

Abstract

To provide a release film that exhibits ultra-light peeling performance for a variety of adhesives, while suppressing changes in the peeling properties of a release layer due to blocking, and an adhesive sheet (film laminate) including the release film.SOLUTION: A release film has a resin layer (A) on one side of a base film. The resin layer (A) includes a silicone resin-based release agent. The post-dry thickness is 0.2-2.0 μm. The film surface on the opposite side of the resin layer (A) satisfies the following (1) and (2). (1) The average surface roughness Sa (B) is 30 nm or more. (2) The surface area ratio Sdr (B) is 3.5×10-2% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a release film, an adhesive sheet, and a method for using the adhesive sheet. [Background technology]

[0002] Conventionally, release films using polyester film as a base material have been used for various purposes due to their excellent properties such as mechanical strength, dimensional stability, chemical resistance, and optical properties, and excellent cost performance. For example, they are used for various optical purposes such as for manufacturing polarizing plates and retardation plates for liquid crystal displays (hereinafter abbreviated as "LCD"), for manufacturing components for plasma display panels (hereinafter abbreviated as "PDP"), for manufacturing components for organic electroluminescence (hereinafter abbreviated as "organic EL"), for manufacturing components for various displays, etc.

[0003] In recent years, the adhesive design of optically transparent adhesive sheets (OCA) / organic light-emitting diode (OLED) adhesive sheet components has been progressing toward stronger adhesion, lower elasticity, and thinner thickness. Accordingly, silicone release films to protect the adhesive sheets are also required to have easier release properties than before. Methods for making a silicone release film easier to release include formulating the film so that the amount of functional groups remaining in the silicone layer after curing is reduced, or applying a thick silicone layer. On the other hand, when the silicone release film is made to have a light release property by the above-mentioned method, when the film is wound into a roll, the opposite side to the silicone layer sticks to the film, blocking occurs, and the silicone layer is damaged, causing problems such as heavy release, peeling electrification, deformation of the film, and non-uniform wettability of the adhesive. In particular, when a coating layer (in-line coating layer) such as an antistatic layer is formed on the opposite side, blocking tends to become even worse. Therefore, as a countermeasure against blocking, for example, a method of incorporating large particles (lubricant) into the base film or incorporating particles into the resin layer (coating layer) on the film has been used (see Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-255704 A [Patent Document 2] JP 2017-61081 A [Patent Document 3] JP 2016-165825 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when large particles are contained in a base film, this can hinder foreign body inspection, cause scratches due to protrusions caused by the large particles, or cause particles to fall off and generate foreign bodies.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and the problem to be solved is to provide a release film which realizes ultra-easy peelability for various adhesives while being resistant to changes in the peel properties of the release layer due to blocking, and an adhesive sheet (film laminate) using said release film. [Means for solving the problem]

[0007] In view of the above circumstances, the present inventors have conducted intensive research and found that the above problems can be solved by using a release film having a specific composition, and have completed the present invention. That is, the present invention provides the following items [1] to

[23] . [1] A release film comprising a resin layer (A) on one side of a base film, the resin layer (A) containing a silicone resin-based release agent and having a thickness of 0.2 to 2.0 μm after drying, and the film surface opposite to the resin layer (A) satisfies the following (1) and (2): (1) The average surface roughness Sa(B) is 30 nm or more. (2) Surface area ratio Sdr(B) is 3.5×10 -2 % or more [2] The release film according to the above [1], which has a resin layer (B) on the film surface on the side on which the resin layer (A) is not provided. [3] The release film according to the above [2], wherein the resin layer (B) contains a non-silicone release agent. [4] The release film according to any one of the above [1] to [3], wherein the resin layer (A) has an elastic modulus at 25° C. of 500 MPa or less, as measured using a nanoindenter apparatus. [5] The release film according to the above [3] or [4], wherein the non-silicone release agent is at least one selected from the group consisting of wax, a compound containing a long-chain alkyl group, and a fluorine compound. [6] The release film according to any one of the above [3] to [5], wherein the content of the release agent in the non-volatile components of the resin layer (B) is 10 to 70 mass %. [7] The release film according to any one of the above [2] to [6], wherein the resin layer (B) is substantially free of particles. [8] The release film according to any one of the above [1] to [7], wherein the normal peel strength of the resin layer (A) is 5 g / inch or less, as measured by the following evaluation method. <Evaluation method> An acrylic adhesive tape (Tesa's "No. 7475") is attached to the resin layer (A) surface of the release film, then cut to a size of 25 mm x 150 mm and left at room temperature for 1 hour. The peeling is performed at 180° under the conditions of a pulling speed of 0.3 m / min. [9] The release film according to any one of the above [2] to [8], further comprising an undercoat layer between at least one of the resin layer (A) or the resin layer (B) and the base film.

[10] The release film according to the above [9], wherein the undercoat layer is an antistatic layer.

[11] The release film according to the above [9] or

[10] , wherein the undercoat layer contains the following compounds (a) to (c): (a) A polymer in which a compound consisting of thiophene or a thiophene derivative is doped with another anionic compound, or a polymer in which a compound consisting of thiophene or a thiophene derivative has an anionic group and is self-doped. (b) Polyhydroxy compounds (c) one or more compounds selected from the group consisting of polyurethane resins, polyester resins, and acrylic resins

[12] At least one of the surfaces of the resin layer (A) or the resin layer (B) has a surface resistivity of 1×10 12 The release film according to any one of the above [2] to

[11] , which has a resistivity of Ω / □ or less.

[13] The release film according to any one of the above [1] to

[12] , wherein the base film is a polyester film.

[14] The release film according to the above

[13] , wherein the polyester film has a three-layer structure.

[15] The release film according to the above

[14] , wherein the relationship (t / r) between the thickness (t) of the film surface layer on the side opposite to the side where the resin layer (A) is provided and the average particle size (r) of the particles is 2.0 or less.

[16] The release film according to any one of the above [1] to

[15] , wherein the resin layer (A) has a post-press heavy peel rate of 100% or less, as evaluated by the following method. <Evaluation method> An acrylic adhesive tape (Tesa's "No. 7475") was attached to the surface of the resin layer (A), cut to a size of 25 mm x 150 mm, and left at room temperature for 1 hour. The peel strength at 180° under the condition of a tensile speed of 0.3 m / min was defined as (F1). Next, the laminate is laminated so as to contact the resin layer (A) surface, and press-treated for 20 hours at a temperature of 40°C, humidity of 90% RH, and a load of 1 MPa. An acrylic adhesive tape (Tesa's "No. 7475") is attached to the resin layer (A) surface after the treatment, and then cut to a size of 25 mm x 150 mm and left at room temperature for 1 hour. The peel force at 180° peeled under the condition of a tensile speed of 0.3 m / min is defined as (F2). The heavy peeling rate after pressing is calculated using the following formula. Heavy peeling rate after pressing (%) = (F2-F1) / F1 x 100

[17] The release film according to any one of the above [2] to

[16] , wherein the average surface roughness (Sa(B)) of the resin layer (B) surface is 60 nm or less.

[18] The release film according to any one of the above [2] to

[16] , wherein the root mean square roughness (Sq(B)) of the resin layer (B) surface is 100 nm or less.

[19] A pressure-sensitive adhesive sheet comprising the release film according to any one of the above [1] to

[18] and another release film via an adhesive layer.

[20] The pressure-sensitive adhesive sheet according to

[19] above, wherein the pressure-sensitive adhesive layer is formed from an acrylic pressure-sensitive adhesive composition.

[21] The adhesive sheet according to

[19] or

[20] above, which is for use as an optically transparent adhesive sheet.

[22] A method for using the pressure-sensitive adhesive sheet according to any one of the above

[19] to

[21] , comprising peeling off the other release film and then attaching the exposed surface of the pressure-sensitive adhesive layer to an optical member.

[23] A method for using the adhesive sheet described in

[22] above, wherein the optical component is a polarizing plate or a touch sensor. Effect of the Invention

[0008] According to the release film of the present invention, it is possible to provide a release film which realizes ultra-easy peelability against various pressure-sensitive adhesives while the peeling properties of the release layer are not easily changed by blocking, and a pressure-sensitive adhesive sheet (film laminate) using this release film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and can be modified as desired without departing from the gist of the present invention.

[0010] <<<Release film>>> A release film according to an embodiment of the present invention (hereinafter, sometimes referred to as "this release film") is a release film having a resin layer (A) on one side of a base film. The release film is preferably made into a rolled release film (release film roll) and stored in the form of a release film roll. In this case, the resin layer (A) (release layer) may be disposed on either the inside or outside of the roll.

[0011] In the present release film, the resin layer (A) on one side contains a silicone resin-based release agent and has a thickness of 0.2 to 2.0 μm after drying. The elastic modulus of the resin layer (A) at 25° C., measured using a nanoindenter device, is preferably 500 MPa or less. Furthermore, the film surface on the opposite side to the resin layer (A) is characterized in that it satisfies the following (1) and (2). (1) The average surface roughness Sa(B) is 30 nm or more. (2) Surface area ratio Sdr(B) is 3.5×10 -2 % or more When the release film having the above-mentioned configuration is rolled, the surface of the resin layer (A) is superimposed on the film surface on the opposite side of the resin layer (A), and at that time, damage due to adhesion to the surface of the resin layer (A) can be reduced, blocking can be suppressed, and it is possible to prevent the resin layer (A) from peeling hard and the surface appearance from deteriorating at the lower winding part of the roll where more pressure is applied to the film. In addition, while realizing ultra-light peelability, the resin layer (A) preferably does not substantially contain particles, so that the adhesion to the base film is good, and further, since there is no particle shedding, migration to adhesive tape, etc. can be reduced.

[0012] As a specific means for achieving both the above (1) and (2), it is preferable to satisfy, for example, the following requirements (X) to (Z). (X) In the polyester layer forming the surface layer opposite to the surface on which the resin layer (A) is provided, the polyester layer contains particles, and the relationship (t / r) between the polyester layer thickness (t) and the average particle size (r) of the particles is 2.0 or less, preferably 1.5 or less, more preferably 1.0 or less, and particularly preferably 0.8 or less. On the other hand, the lower limit is 0.2 or more, preferably 0.4 or more. (Y) The thickness (t) of the polyester layer of the surface layer is in the range of 0.5 to 5.0 μm, preferably 1.0 to 4.0 μm, and more preferably 1.5 to 3.0 μm. (Z) The content of particles added to the polyester layer forming the surface layer is 2000 ppm or more, preferably 3000 ppm or more, and more preferably 4000 ppm or more. On the other hand, the upper limit is preferably 10,000 ppm or less, more preferably 8,000 ppm or less, taking into consideration damage to the resin layer (A) when it is wound into a roll. It is even more preferable that all of the above requirements (X) to (Z) are satisfied.

[0013] In the present invention, by fixing the particles in the polyester layer containing the particles, it is possible to form moderate unevenness while suppressing the particles from protruding excessively on the film surface.Furthermore, as another effect of fixing the particles in the polyester layer, it was found that by partially burying the particles in the polyester layer, it is possible to suppress an extreme increase in film haze even when the particle addition amount is large. The present invention was completed based on the discovery of the existence of a region exhibiting unique behavior not seen before as described above.

[0014] <<Base film>> The base film in the present release film is not particularly limited in material as long as it has a film shape. For example, it may be made of paper, resin, metal, etc. Among these, it is preferable to use a resin from the viewpoint of mechanical strength and flexibility. Examples of the resin substrate film include films formed from polymers such as polyethylene, polypropylene, polyester, polystyrene, polycarbonate, polyethersulfone, polyamide, polyimide, etc. Furthermore, as long as they can be formed into a film, they may be mixtures of these materials (polymer blends) or composites of their constituent units (copolymers). Among the above-listed films, polyester films containing polyester as a main resin component are particularly preferred because of their excellent physical properties such as heat resistance, flatness, optical properties, and strength. The base film in the present invention preferably has a polyester layer containing particles. Therefore, except when the base film is made of polyester, the polyester layer may be formed by applying a polyester resin composition for forming the polyester layer to the base film. In addition, when the base film is a monolayer polyester film as described later, the base film itself may contain particles, and in that case, it is not necessary to provide a separate polyester layer containing particles. On the other hand, when the base film is a multilayer polyester film as described later in detail, it is preferable that the outermost layer is a polyester layer.

[0015] <Polyester film> The polyester film constituting the laminated film of the present invention may be a single layer or a multilayer, and may be a multilayer of four or more layers other than a two-layer or three-layer structure, as long as it does not exceed the gist of the present invention, and is not particularly limited. In the present invention, a polyester film having at least a three-layer structure is preferable. As the polyester film, a biaxially oriented polyester film is preferable from the viewpoints of thinning and dimensional stability.

[0016] The polyester used in the present invention may be either a homopolyester or a copolymer polyester. In the case of a homopolyester, it is preferable that the polyester is obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and examples of the aliphatic glycol include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol. A representative polyester is polyethylene terephthalate. On the other hand, examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, oxycarboxylic acid (e.g., p-oxybenzoic acid, etc.), and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, and the like.

[0017] In the case of copolymer polyester, it may be one obtained by polycondensation of a dicarboxylic acid component and a glycol component. The dicarboxylic acid component may be one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, oxycarboxylic acid (e.g., p-oxybenzoic acid, etc.), and the glycol component may be one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, etc. The copolymer polyester is preferably a copolymer containing 30 mol % or less of a third component based on the total of the dicarboxylic acid component and the glycol component. The term "main component resin" refers to the resin that has the largest mass proportion among the resins constituting the polyester film, and means that it accounts for 50 mass% or more, 75 mass% or more, 90 mass% or more, or 100 mass% of the resins constituting the polyester film.

[0018] The polymerization catalyst for the polyester film is not particularly limited, and can be a conventionally known compound, such as an antimony compound, a titanium compound, a germanium compound, a manganese compound, an aluminum compound, a magnesium compound, a calcium compound, etc. Among them, titanium compounds and germanium compounds are preferred because they have high catalytic activity, can be polymerized in a small amount, and have a small amount of metal remaining in the film, resulting in high brightness of the film. Moreover, titanium compounds are more preferred because germanium compounds are expensive.

[0019] In the case of polyester using a titanium compound, the titanium element content is preferably 50 ppm or less, more preferably 1 to 20 ppm, and further preferably in the range of 2 to 10 ppm. If the titanium compound content is too high, the polyester may deteriorate in the melt extrusion process, resulting in a film with a strong yellowish tinge. On the other hand, if the content is too low, the polymerization efficiency may be poor, leading to increased costs and inability to obtain a film with sufficient strength. In addition, when using a polyester containing a titanium compound, it is preferable to use a phosphorus compound to reduce the activity of the titanium compound in order to suppress deterioration during the melt extrusion process. As the phosphorus compound, orthophosphoric acid is preferable in consideration of the productivity and thermal stability of the polyester. The phosphorus element content is preferably in the range of 1 to 300 mass ppm, more preferably 3 to 200 mass ppm, and even more preferably 5 to 100 mass ppm relative to the amount of polyester to be melt extruded. When the content of the phosphorus compound is equal to or less than the upper limit, gelation or foreign matter is not caused, and when the content is equal to or more than the lower limit, the activity of the titanium compound can be sufficiently reduced, coloration can be suppressed, and a yellowish film is not formed.

[0020] In order to suppress the amount of precipitation of oligomer components, the film may be produced using a polyester having a low content of oligomer components as the raw material. As a method for producing a polyester having a low content of oligomer components, various known methods can be used, such as a method of performing solid phase polymerization after the production of a polyester.

[0021] The amount of oligomer components precipitated may be suppressed by forming the polyester film into a three-layer or more layer structure and forming the outermost layer of the polyester film from a polyester raw material having a low content of oligomer components. The polyester may be obtained by melt polycondensation under reduced pressure at a higher reaction temperature after esterification or transesterification.

[0022] It is also possible to incorporate an ultraviolet absorbing agent into the polyester film in order to improve the weather resistance of the film and prevent deterioration of the adherend (e.g., liquid crystal), etc. The ultraviolet absorbing agent is a compound that absorbs ultraviolet light and is not particularly limited as long as it can withstand the heat applied during the manufacturing process of the polyester film.

[0023] As the ultraviolet absorbing agent, there are organic ultraviolet absorbing agents and inorganic ultraviolet absorbing agents, and from the viewpoint of transparency, organic ultraviolet absorbing agents are preferred.As the organic ultraviolet absorbing agent, there are no particular limitations, but for example, cyclic imino esters, benzotriazoles, benzophenones, etc. are mentioned.From the viewpoint of durability, cyclic imino esters and benzotriazoles are more preferred.In addition, it is also possible to use two or more kinds of ultraviolet absorbing agents in combination.

[0024] In the present release film, the base film (polyester film) has a polyester layer, and particles can be blended in the polyester layer of the polyester film for the main purpose of imparting easy slippage and preventing scratches in each process. When particles are blended, the type of particles to be blended is not particularly limited as long as they are particles that can impart easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, zirconium oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used. Among these, silica particles and calcium carbonate particles are preferred because they are particularly effective in small amounts.

[0025] The particles have an average particle size of preferably 0.01 to 5 μm, more preferably 0.03 to 4 μm, and even more preferably 0.05 to 3.0 μm. When the average particle size is equal to or less than the upper limit, the haze of the film is kept low and the film has slip properties.

[0026] Furthermore, the particle content in the polyester layer of the polyester film is preferably 10% by mass or less, more preferably 1 to 8% by mass, even more preferably 2 to 8% by mass, and particularly preferably 3 to 8% by mass. When there are no particles or when there are only a few particles, the transparency of the film is high and a good film is obtained, but in order to prevent the slipperiness from decreasing, it may be necessary to take measures such as adding particles to the coating layer to improve the slipperiness. Furthermore, when the particle content is equal to or less than the upper limit, the haze does not increase and sufficient film transparency can be ensured.

[0027] The shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. can be used, and there is no particular limit to the hardness, specific gravity, color, etc. Two or more types of these particles may be used in combination as necessary.

[0028] The method of adding particles to the polyester layer is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage in the production of the polyester constituting each layer, but it is preferable to add the particles after the completion of the esterification or transesterification reaction.

[0029] In addition to the above-mentioned particles, conventionally known ultraviolet absorbers, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to the polyester film of the present invention, if necessary.

[0030] The thickness of the polyester film in the present invention is not particularly limited as long as it is within the range that allows production of a film, but is preferably 10 to 300 μm, more preferably 15 to 200 μm, even more preferably 25 to 125 μm, and most preferably 38 to 75 μm.

[0031] <Production method of polyester film> Next, a specific example of the production of a polyester film will be described, but the production method is not limited to the following production example. For example, when producing a biaxially stretched polyester film, the above-mentioned polyester raw material is first melt-extruded from a die using an extruder, and the molten sheet is cooled and solidified by a cooling roll to obtain an unstretched sheet. In this case, it is preferable to increase the adhesion between the sheet and the rotating cooling drum in order to improve the flatness of the sheet, and an electrostatic application adhesion method or a liquid application adhesion method is preferably adopted. Next, the obtained unstretched sheet is stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3.0 to 6 times. Next, in the direction perpendicular to the first-stage stretching direction, the sheet is stretched at usually 70 to 170°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3.0 to 6 times. Subsequently, a method of performing heat treatment under tension or relaxation of 30% or less at a temperature of 180 to 270°C to obtain a biaxially oriented film can be mentioned. In the above stretching, a method of stretching in one direction in two or more stages can be adopted. In that case, it is preferable to perform the stretching so that the final stretch ratios in both directions are each within the above range.

[0032] In addition, a simultaneous biaxial stretching method can also be used for the production of polyester films. The simultaneous biaxial stretching method is a method in which the unstretched sheet is simultaneously stretched and oriented in the machine direction and the width direction under a temperature controlled condition usually at 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 4 to 50 times, preferably 7 to 35 times, more preferably 10 to 25 times in terms of area ratio. Then, the sheet is subsequently heat-treated under tension or relaxation of 30% or less at a temperature of 170 to 270°C to obtain a stretch-oriented film. As for the simultaneous biaxial stretching device employing the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, or a linear drive method can be employed.

[0033] <<Resin layer (A)>> Next, the formation of the resin layer (A) constituting the release film in the present invention will be described.

[0034] The resin layer (A) contains a silicone resin-based release agent and has a thickness of 0.2 to 2.0 μm after drying. If the thickness of the resin layer (A) is less than 0.2 μm, it is difficult to make the resin layer (A) easy to peel, even if the elastic modulus of the resin layer (A) is within a predetermined range, as described below. If the thickness is more than 2.0 μm, the migration of the resin layer (A) components to the adhesive tape or the like may increase, or blocking may not be sufficiently prevented. From the above viewpoints, the thickness is preferably in the range of 0.4 to 1.5 μm, more preferably 0.4 to 1.2 μm, and even more preferably 0.4 to 1.0 μm.

[0035] The silicone resin-based release agent may be a curable silicone resin, and the resin layer (A) is a layer formed by curing a resin layer (A) composition containing a curable silicone resin as a main component resin, and is disposed on at least one side of the above-mentioned base film. The resin layer (A) can also be said to be a release layer containing a cured product formed by curing the resin layer (A) composition.

[0036] The above-mentioned "main component resin" means the resin that has the largest mass proportion among the resins constituting the resin layer (A) composition, and is expected to account for 50 mass % or more, 75 mass % or more, 90 mass % or more, or 100 mass % of the resins constituting the resin layer (A) composition.

[0037] The curable silicone resin may be a resin containing a curable silicone resin as a main component, or a modified silicone obtained by graft polymerization with an organic resin such as an acrylic resin, a urethane resin, an epoxy resin, an alkyd resin, etc. In addition, when the adhesive layer is a silicone adhesive, it is preferable that the adhesive layer contains a fluorosilicone resin, etc.

[0038] The type of curable silicone resin may be any of the existing curing reaction types, such as heat curable types such as addition types and condensation types, and electron beam curable types such as ultraviolet curable types, or a combination of multiple types of curable silicone resins. Furthermore, there is no particular restriction on the form of application of the curable silicone resin when forming the resin layer (A), and it may be in any form, such as a form dissolved in an organic solvent, a solvent-free form, or an aqueous emulsion form.

[0039] Solventless curable silicone is a silicone with a viscosity that allows it to be applied without diluting it with a solvent, and is a silicone resin with a relatively low molecular weight that is made up of short polysiloxane chains. On the other hand, solvent-based curable silicones are silicone resins that are so viscous that they cannot be applied unless they are diluted with a solvent, and have a relatively high molecular weight compared to solventless curable silicones. From the viewpoints of providing good adhesion to the substrate film, providing a uniform coat appearance without coating unevenness, and facilitating adjustment of the thickness of the resin layer (A), solvent-curable silicones are preferred.

[0040] Although there is no limitation on the type of silicone resin used in the present invention, it is preferable to use a curable silicone resin containing an alkenyl group in the present invention from the viewpoint of excellent release properties such as light peelability. As the curable silicone resin containing an alkenyl group, a diorganopolysiloxane represented by the following general formula (1) can be exemplified. R (3-a) X a SiO-(RXSiO) m -(R2SiO) n -SiX a R (3-a) (1)

[0041] In the general formula (1), R is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and X is an organic group containing an alkenyl group. a is an integer of 0 to 3, preferably 1, and m is 0 or more, but when a=0, m is 2 or more, and m and n are numbers that satisfy 100≦m+n≦20000, and the above formula does not mean a block copolymer. R is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl groups, cycloalkyl groups such as cyclohexyl groups, and aryl groups such as phenyl and tolyl groups, with methyl and phenyl groups being particularly preferred. X is preferably an alkenyl-containing organic group having 2 to 10 carbon atoms. Specific examples thereof include a vinyl group, an allyl group, a hexenyl group, an octenyl group, an acryloylpropyl group, an acryloylmethyl group, a methacryloylpropyl group, a cyclohexenylethyl group, and a vinyloxypropyl group. In particular, a vinyl group, a hexenyl group, and the like are preferred. Specific examples include a dimethylsiloxane-methylhexenylsiloxane copolymer capped at both molecular chain terminals with trimethylsiloxy groups (96 mol% dimethylsiloxane units, 4 mol% methylhexenylsiloxane units), a dimethylsiloxane-methylhexenylsiloxane copolymer capped at both molecular chain terminals with dimethylvinylsiloxy groups (97 mol% dimethylsiloxane units, 3 mol% methylhexenylsiloxane units), and a dimethylsiloxane-methylhexenylsiloxane copolymer capped at both molecular chain terminals with dimethylhexenylsiloxy groups (95 mol% dimethylsiloxane units, 5 mol% methylhexenylsiloxane units).

[0042] Next, the polyorganosiloxane containing SiH groups, which is necessary to react with the curable silicone resin containing alkenyl groups to form a stronger silicone release layer, is an organohydrogenpolysiloxane having at least two, and preferably three or more, hydrogen atoms bonded to silicon atoms in one molecule, and linear, branched, cyclic, etc. can be used, and examples of the compound represented by the following general formula (2) include, but are not limited to, these. HbR 1 (3-b) SiO-(HR1 SiO) x -(R 1 2SiO) y -SiR 1 (3-b) H b (2)

[0043] In the general formula (2), R 1 is a monovalent hydrocarbon group having 1 to 6 carbon atoms and not containing an aliphatic unsaturated bond. b is an integer from 0 to 3, and x and y are each an integer. Specific examples include methylhydrogenpolysiloxane capped with trimethylsiloxy groups at both molecular chain terminals, dimethylsiloxane-methylhydrogensiloxane copolymer capped with trimethylsiloxy groups at both molecular chain terminals, methylhydrogenpolysiloxane capped with dimethylhydrogensiloxy groups at both molecular chain terminals, and dimethylsiloxane-methylhydrogensiloxane copolymer capped with dimethylhydrogensiloxy groups at both molecular chain terminals.

[0044] Specific examples of commercially available silicone resins that can be used in the present invention include KS-774, KS-775, KS-778, KS-779H, KS-847H, KS-856, X-62-2422, X-62-2461, X-62-1387, X-62-2888L, X-62-5039, X-62-5040, KNS-3051, X-62-1496, KNS320A, KNS316, X-62-1574A / B, X-62-7052, X-62-7028A / B, X-62-7619, X-62-7213, and X-41-3035 manufactured by Shin-Etsu Chemical Co., Ltd.; and YSR-3022 manufactured by Momentive Performance Materials. TPR-6700, TPR-6720, TPR-6721, TPR6500, TPR6501, UV9300, UV9425, XS56-A2775, XS56-A2982, UV9430, TPR6600, TPR6604, TPR6605, SRX357, SRX211, SD7220, S Examples of such silicone rubbers include, but are not limited to, D7292, LTC750A, LTC760A, LTC303E, SP7259, BY24-468C, SP7248S, BY24-452, DKQ3-202, DKQ3-203, DKQ3-204, DKQ3-205, DKQ3-210, and of the DEHESIVE series manufactured by Wacker Asahi Kasei Silicones Co., Ltd., DEHESIVE 636, 919, 920, 921, 924, 929, etc.

[0045] The resin layer (A) preferably uses a platinum-based catalyst that promotes an addition reaction. Examples of this component include platinum-based compounds such as chloroplatinic acid, an alcohol solution of chloroplatinic acid, a complex of chloroplatinic acid and an olefin, and a complex of chloroplatinic acid and an alkenylsiloxane, platinum black, platinum supported on silica, and platinum supported on activated carbon.

[0046] The content of the curing catalyst in the resin layer (A) is preferably 0.5 to 500 mass ppm in terms of metal relative to the curable silicone resin, more preferably 5 mass ppm or more, even more preferably 10 mass ppm or more, more preferably 300 mass ppm or less, and even more preferably 200 mass ppm or less. When the platinum catalyst content in the release layer is equal to or greater than the lower limit, sufficient peeling force is obtained, the curing reaction proceeds sufficiently, and no problems such as deterioration of the coat surface condition occur. On the other hand, when the platinum catalyst content in the resin layer (A) is equal to or less than the upper limit, in addition to being advantageous in terms of cost, reactivity is increased and no problems occur in the process, such as generation of gel foreign matter.

[0047] In addition, because the addition reaction is very reactive, acetylene alcohol may be added as a reaction inhibitor in some cases. The component is an organic compound having a carbon-carbon triple bond and a hydroxyl group, preferably a compound selected from the group consisting of 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, and phenylbutynol.

[0048] The content of the reaction inhibitor is preferably 0.001 to 5.0 parts by mass, more preferably 0.01 to 2.0 parts by mass, even more preferably 0.05 to 1.5 parts by mass, and most preferably 0.1 to 0.5 parts by mass per 100 parts by mass of the total amount of the resin layer (A) composition (based on non-volatile components). By setting the content within the above range, the curable silicone resin is not inhibited from curing without decreasing the reaction activity, and the easy releasability of the release film can be ensured.

[0049] A catalyst can be used in the resin layer (A) constituting the release film in order to promote hydrolysis and condensation reactions. Specific examples of catalysts include organic acids such as acetic acid, butyric acid, maleic acid, and citric acid, inorganic acids such as hydrochloric acid, nitric acid, phosphoric acid, and sulfuric acid, basic compounds such as triethylamine, organic metal salts such as tetrabutyl titanate, dibutyltin dilaurate, dibutyltin diacetate, dibutyltin dioctate, dibutyltin diolate, diphenyltin diacetate, dibutyltin oxide, dibutyltin dimethoxide, dibutylbis(triethoxysiloxy)tin, and dibutyltin benzyl maleate, and fluorine-containing compounds such as KF and NHF. The above catalysts may be used alone or in combination of two or more. Among them, organic metal salts are preferable in that they provide good coating film durability.

[0050] In order to adjust the release property of the resin layer (A), various release control agents may be used in combination. When the release force is to be made stronger, the content of organopolysiloxane resin, silica particles, silicone species with a strong release force, etc. is generally adjusted appropriately in the resin layer (A) to obtain the desired release force.

[0051] Specific examples of commercially available heavy release agents include KS-3800 and X-92-183 manufactured by Shin-Etsu Chemical Co., Ltd., and SD7292, BY24-843, and BY24-4980 manufactured by Dow Corning Toray Co., Ltd.

[0052] In the case of making the release force lighter, various low molecular weight siloxanes are selected and the content in the resin layer (A) is appropriately adjusted so that the siloxane migration component exerts its releasing performance. Examples of low molecular weight siloxane compounds include hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, etc. In addition, other compounds of these low molecular weight cyclic siloxanes include dimethylsiloxane oligomers blocked with trimethylsiloxy groups at both ends of the molecular chain; dimethylsiloxane oligomers blocked with dimethylhydroxysiloxy groups at both ends of the molecular chain; and the like, and these compounds may be used in combination as necessary.

[0053] As described above, the resin layer (A) composition may contain a light release agent as necessary, and a silicone oil having a dimethylsiloxane skeleton (DM) represented by the following formula (3) and a methylphenylsiloxane skeleton (MP) represented by the following formula (4) is preferable. When the light release agent has a dimethylsiloxane skeleton (DM) and a methylphenylsiloxane skeleton (MP), even if it migrates to the adhesive layer to be bonded, it can penetrate into the adhesive layer, and the decrease in adhesive strength can be reduced. The ratio (DM:MP) of the dimethylsiloxane skeleton (DM) represented by the following formula (3) and the methylphenylsiloxane skeleton (MP) represented by the following formula (4) is preferably in the range of 98:2 to 70:30, more preferably in the range of 95:5 to 80:20, and particularly preferably in the range of 92:8 to 85:15, in terms of molar ratio. By setting DM:PM within the above range, the releasability of this release film can be ensured. The light releasing agent preferably has a mass average molecular weight of less than 10,000. When the mass average molecular weight of the light releasing agent is less than 10,000, it is advantageous in terms of migration and light releasing property.

[0054] [ka]

[0055] [ka]

[0056] The desired light release can be achieved by including these low molecular weight siloxane compounds as migratory components in the silicone resin in an amount of usually 0.1 to 15.0% by mass, preferably 0.5 to 10.0% by mass, and more preferably 0.5 to 5.0% by mass. If the amount is 0.1% by mass or more, the migratory components are sufficient to provide sufficient releasability, and if the low molecular weight siloxane content is 15.0% by mass or less, the migratory components do not precipitate excessively, and there is no concern about process contamination.

[0057] The resin layer (A) composition may contain a dilution solvent as necessary. Examples of dilution solvents include aromatic hydrocarbons such as toluene, aliphatic hydrocarbons such as hexane, heptane, and isooctane, esters such as ethyl acetate and butyl acetate, ketones such as methyl ethyl ketone (MEK) and isobutyl methyl ketone, alcohols such as ethanol and 2-propanol, and ethers such as diisopropyl ether and dibutyl ether. These are preferably used alone or in combination, taking into consideration solubility, coatability, boiling point, and the like.

[0058] In order to improve the coating adhesion to the film, it is preferable to use an organosilicon compound represented by the following general formula (5) in the resin layer (A). Si(X) d (Y) e (R 1 ) f (5) [In the above formula, X is an organic group having at least one selected from an epoxy group, a mercapto group, a (meth)acryloyl group, an alkenyl group, a haloalkyl group, and an amino group; R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, Y is a hydrolyzable group, d is an integer of 1 or 2, e is an integer of 2 or 3, f is an integer of 0 or 1, and d+e+f=4.

[0059] The organosilicon compound represented by the general formula (5) can be one having two hydrolyzable groups Y (D unit source) or three hydrolyzable groups Y (T unit source) that can form a siloxane bond by hydrolysis and condensation reaction.

[0060] In the general formula (5), the monovalent hydrocarbon group R 1 has 1 to 10 carbon atoms, and is particularly preferably a methyl group, an ethyl group, or a propyl group.

[0061] In the general formula (5), examples of the hydrolyzable group Y include the following: methoxy group, ethoxy group, butoxy group, isopropenoxy group, acetoxy group, butanoxime group, and amino group. These hydrolyzable groups may be used alone or in combination. The use of a methoxy group or an ethoxy group is particularly preferred because it can provide the coating material with good storage stability and has suitable hydrolyzability.

[0062] Specific examples of organosilicon compounds contained in the resin layer (A) include vinyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 5-hexenyltrimethoxysilane, p-styryltrimethoxysilane, trifluoropropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane.

[0063] It is preferable that the resin layer (A) does not substantially contain particles. By substantially not containing particles in the resin layer (A), it is possible to stabilize the release properties and reduce migration. Incidentally, "substantially not containing" means that the resin layer (A) may contain particles as long as the amount is small enough not to impair the effects of the present invention, and for example, may contain particles that are inevitably mixed in. The specific content of particles in the present resin layer (A) (A layer) is, for example, less than 0.05% by mass, preferably less than 0.01% by mass, more preferably less than 0.0001% by mass, based on the non-volatile components. The range of the content of particles in the present resin layer (A) composition based on the non-volatile components is also the same as the content of the particles described above.

[0064] Furthermore, within the scope of the present invention, the resin layer (A) composition may contain, as necessary, an antifoaming agent, a coatability improving agent, a thickener, an organic lubricant, an antistatic agent, a conductive agent, an ultraviolet absorber, an antioxidant, a foaming agent, a dye, a pigment, and the like.

[0065] The number average molecular weight (Mn) of the curable silicone resin is preferably 1000 or more and 1,000,000 or less. When the number average molecular weight (Mn) of the curable silicone resin is set to the above lower limit value or more, when the adhesive layer is laminated on the release film, the amount of low molecular weight silicone resin that dissolves or migrates to the adhesive layer can be reduced, and the resin layer (A) can be applied thickly to easily obtain a light peeling effect. On the other hand, when the number average molecular weight (Mn) of the curable silicone resin is set to the above upper limit value or less, the viscosity increases and the fluidity of the resin layer (A) composition is prevented from decreasing. Therefore, when the resin layer (A) composition is applied, streaky coating unevenness is prevented from occurring, and the resin layer (A) surface is easily made smooth. From this viewpoint, the number average molecular weight (Mn) of the curable silicone resin is preferably 1000 or more, more preferably 3000 or more, even more preferably 5000 or more, and even more preferably 10000 or more. On the other hand, it is preferably 1000000 or less, more preferably 200000 or less, and even more preferably 100000 or less.

[0066] From the same viewpoint as for the number average molecular weight, the mass average molecular weight (Mw) of the curable silicone resin is preferably 2,000 to 2,000,000, more preferably 5,000 or more, even more preferably 10,000 or more, and particularly preferably 15,000 or more, and more preferably 250,000 or less, and even more preferably 100,000 or less.

[0067] The ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn) of the curable silicone resin is preferably 1.0 to 5.0, more preferably 1.5 to 3.5, and even more preferably 2.0 to 3.0. By satisfying this range, it is expected that the crosslinking reaction will proceed efficiently.

[0068] The curable silicone resin may be a combination of two or more curable silicone resins, and in this case, the average of the number average molecular weight (Mn) and mass average molecular weight (Mw) of the two or more curable silicone resins is preferably within the above range. The average here refers to a weighted average weighted by the mass of each resin. In addition, when a base agent and a silicone crosslinking agent are used as the curable silicone resin, the mass average molecular weight (Mn), number average molecular weight (Mw), and Mw / Mn of the base agent are preferably within the above range.

[0069] The curable silicone resin preferably has a viscosity at 25° C. when adjusted to 15 mass % by dilution with n-heptane solvent of 1 to 400 mcps, more preferably 5 to 300 mcps, and further preferably 10 to 200 mcps. If the viscosity of the curable silicone resin is 1 mcps or more, the appropriate viscosity of the coating liquid suppresses repelling and provides a uniform coat appearance with high visibility, which is preferable. If the viscosity is 400 mcps or less, the fluidity of the resin layer (A) composition can be maintained, the occurrence of streaky coating unevenness when the resin layer (A) composition is applied can be suppressed, and the resin layer (A) surface can be made smooth.

[0070] When the curable silicone resin has an alkenyl group in the silicone resin, the content of the alkenyl group is preferably 0.4 to 2.5 mol%, more preferably 0.5 to 2.0 mol%, and even more preferably 0.5 to 1.5 mol% based on the total amount of siloxane components. By satisfying this range, the release layer is sufficiently cured because the alkenyl group is contained in a certain amount or more, while the amount of the alkenyl group is not excessive, so that the peeling force after exposure to air can be prevented from becoming heavy.

[0071] When the curable silicone resin has a Si-H group in the silicone resin, the content of the Si-H group is preferably 0.8 to 2.5 mol%, more preferably 0.8 to 2.0 mol%, and even more preferably 1.0 to 2.0 mol% based on the total amount of siloxane components. By satisfying this range, the release layer is sufficiently cured because the Si-H group is contained in a certain amount or more, while the amount of Si-H group is not excessive, so that the reaction with the adhesive layer is prevented, and the release film can be suppressed from becoming difficult to release.

[0072] The curable silicone resin may contain alkenyl groups and Si-H groups (also simply referred to as "H groups") in the side chains and / or terminals of the main chain consisting of siloxane bonds in the same structure. In that case, it is preferable that the content of the alkenyl groups and the Si-H groups is within the above range.

[0073] The elastic modulus of the resin layer (A) at 25°C is preferably 500 MPa or less, more preferably 65 to 400 MPa, and even more preferably 80 to 300 MPa. By satisfying these ranges, it is possible to exhibit good peelability from the adhesive layer. The elastic modulus of the resin layer (A) can be adjusted by the type of silicone resin used, the thickness of the resin layer (A), etc., and for example, the thinner the resin layer (A), the higher the elastic modulus tends to be. The elastic modulus referred to here is a value measured by a nanoindenter.

[0074] The normal peel strength of the resin layer (A) is preferably 10 g / inch or less, more preferably 0.1 to 5 g / inch, and even more preferably in the range of 0.5 to 3 g / inch. When the normal peel strength is 10 g / inch or less, good peelability can be exhibited even for adhesive layers whose elastic modulus is reduced due to the increase in size and thickness of optical components. On the other hand, when the normal peel strength exceeds 10 g / inch, peeling from the adhesive layer may be difficult, and the adhesive layer may be transferred to the release film side due to deformation or breakage of the adhesive layer.

[0075] The residual adhesion rate of the resin layer (A) is an index of the migration of the migrating component derived from the resin layer (A) to the adhesive tape to be laminated. In the resin layer (A) with high migration, a large amount of the migrating component adheres to the laminated evaluation film, so that the peeling force of the adhesive tape to be laminated to the evaluation film becomes small, and the residual adhesion rate (%) also decreases. Therefore, it is good that the residual adhesion rate (%) is high, preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more.

[0076] The heavy peeling rate of the resin layer (A) after pressing is preferably 100% or less, more preferably 50% or less, and even more preferably 20% or less. If the heavy peeling rate after pressing is 100% or less, when the release film is wound into a roll, the heavy peeling of the resin layer (A) at the lower winding part of the roll where pressure is applied by the film is suppressed to a small extent, and no defects due to heavy peeling occur. The method for calculating the heavy peeling rate after pressing is as described in the examples.

[0077] The resin layer (A) may be formed by in-line coating, which treats the film surface during the film-forming process, or by offline coating, which applies a coating outside the system onto a film that has already been produced. Off-line coating is more preferred.

[0078] The resin layer (A) can be formed on the film by a conventional coating method such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, curtain coating, or the like.

[0079] The film constituting the release film in the present invention may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment.

[0080] The curing conditions for forming the resin layer (A) are not particularly limited. When the resin layer (A) is provided by offline coating, the heat treatment is usually performed at 80°C or higher for 10 seconds or more, preferably at 100 to 200°C for 3 to 40 seconds, more preferably at 120 to 190°C for 3 to 40 seconds, and even more preferably at 150 to 180°C for 3 to 40 seconds.

[0081] If necessary, heat treatment and irradiation with active energy rays such as ultraviolet rays may be used in combination. As an energy source for curing by irradiation with active energy rays, known devices and energy sources can be used. For example, light sources include fusion (H) lamps, metal halide lamps, high-pressure mercury lamps (ozone generating type, ozone-less type), UV-LEDs, etc.

[0082] Although there is no particular limitation on the active energy ray irradiation, in the case of ultraviolet ray irradiation, the cumulative light amount is 10 to 3000 mJ / cm. 2 , preferably 50 to 2000 mJ / cm 2 , and more preferably 100 to 1000 mJ / cm 2 By setting the cumulative light amount of ultraviolet irradiation within the above range, the curing of the resin layer (A) is promoted, while by not irradiating it excessively, the resin layer (A) is not destroyed and the peeling force after irradiation can be prevented from becoming heavy.

[0083] The release film of the present invention has a surface resistivity of 1×10 12 It is preferably Ω / □ or less. The lower the surface resistivity of the resin layer (A) or the resin layer (B), the better the antistatic property, and the more effectively the film can be prevented from being charged during the process and from being contaminated with foreign matter.

[0084] <<Resin layer (B)>> The present release film preferably has a resin layer (B) on the film surface on the side on which the resin layer (A) is not provided. The resin layer (B) in the present invention will be described below.

[0085] The resin layer (B) constituting the release film in the present invention is provided on the surface of the base film opposite to the surface on which the resin layer (A) is provided, and may be a resin layer (B) containing a non-silicone-based release agent, and more preferably is a resin layer (B) containing a non-silicone-based release agent and having antistatic properties.

[0086] The non-silicone release agent used in the resin layer (B) is not particularly limited as long as it is a release agent other than a silicone compound, and any conventionally known release agent can be used. Examples of such release agents include long-chain alkyl group-containing compounds, fluorine compounds, waxes, etc. Among these, long-chain alkyl compounds and waxes are preferred from the viewpoint of less staining and excellent blocking reduction, and long-chain alkyl compounds are particularly preferred from the viewpoint of blocking reduction. These release agents may be used alone or in combination.

[0087] Silicone compounds are compounds having siloxane bonds in the molecule, and also include those having various functional groups at the side chain and / or end of the main chain consisting of siloxane bonds. Examples include ether groups, hydroxyl groups, amino groups, epoxy groups, carboxylic acid groups, halogen groups such as fluorine, perfluoroalkyl groups, and hydrocarbon groups (alkyl groups, alkenyl groups, aryl groups, various aromatic groups, etc.). When the resin layer (B) contains a silicone compound, it is difficult to use it in the present release film because it is strongly blocked with the resin layer (A) and the surface of the resin layer (A) is deformed, etc., and the peeling properties of the resin layer (A) are deteriorated.

[0088] The long-chain alkyl group-containing compound is a compound having a straight-chain or branched alkyl group having a carbon number of usually 6 or more, preferably 8 or more, and more preferably 12 or more. Examples of the alkyl group include a hexyl group, an octyl group, a decyl group, a lauryl group, an octadecyl group, and a behenyl group. Examples of the compound having an alkyl group include various long-chain alkyl group-containing polymer compounds, long-chain alkyl group-containing amine compounds, long-chain alkyl group-containing ether compounds, and long-chain alkyl group-containing quaternary ammonium salts. Considering heat resistance and staining resistance, a polymer compound is preferable. In addition, from the viewpoint of effectively obtaining releasability, a polymer compound having a long-chain alkyl group in the side chain is more preferable.

[0089] The polymer compound having a long-chain alkyl group in the side chain can be obtained by reacting a polymer having a reactive group with a compound having an alkyl group capable of reacting with the reactive group. Examples of the reactive group include hydroxyl group, amino group, carboxyl group, acid anhydride, etc. Examples of the compound having these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, reactive group-containing polyester resin, reactive group-containing poly(meth)acrylic resin, etc. Among these, polyvinyl alcohol is preferable in consideration of releasability and ease of handling.

[0090] Examples of compounds having an alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, behenyl isocyanate, etc., long-chain alkyl group-containing acid chlorides such as hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, behenyl chloride, etc., long-chain alkyl group-containing amines, long-chain alkyl group-containing alcohols, etc. Among these, in consideration of releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred.

[0091] Furthermore, polymeric compounds having a long-chain alkyl group in the side chain can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of long-chain alkyl (meth)acrylate include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.

[0092] The wax is selected from natural wax, synthetic wax, and waxes blended therewith. Natural waxes are vegetable wax, animal wax, mineral wax, and petroleum wax. Examples of vegetable waxes include candelilla wax, carnauba wax, rice wax, wood wax, and jojoba oil. Examples of animal waxes include beeswax, lanolin, and whale wax. Examples of mineral waxes include montan wax, ozokerite, and ceresin. Examples of petroleum waxes include paraffin wax, microcrystalline wax, and petrolatum. Examples of synthetic waxes include synthetic hydrocarbons, modified waxes, hydrogenated waxes, fatty acids, acid amides, amines, imides, esters, and ketones. Examples of synthetic hydrocarbons include Fischer-Tropsch wax (also known as Sazowar wax) and polyethylene wax, as well as the following low molecular weight polymers (specifically, polymers with a viscosity number average molecular weight of 500 to 20,000): polypropylene, ethylene-acrylic acid copolymer, polyethylene glycol, polypropylene glycol, and block or grafted polyethylene glycol and polypropylene glycol. Examples of modified waxes include montan wax derivatives, paraffin wax derivatives, and microcrystalline wax derivatives. The derivatives here are compounds obtained by any of the following processes, or a combination of them: refining, oxidation, esterification, and saponification. Examples of hydrogenated waxes include hydrogenated castor oil and hydrogenated castor oil derivatives.

[0093] Among the above waxes, synthetic waxes are preferred from the viewpoint of stable properties, and among these, polyethylene waxes are more preferred, with oxidized polyethylene wax being even more preferred. The number average molecular weight (Mn) of the synthetic wax is preferably in the range of 500 to 30,000, more preferably 1,000 to 15,000, and even more preferably 2,000 to 8,000, from the viewpoints of stability of properties such as blocking and ease of handling.

[0094] The fluorine compound is a compound containing fluorine atoms in the compound. From the viewpoint of the coating appearance by in-line coating, organic fluorine compounds are preferably used, for example, perfluoroalkyl group-containing compounds, polymers of olefin compounds containing fluorine atoms, aromatic fluorine compounds such as fluorobenzene, etc. From the viewpoint of mold releasability, it is preferable to use a compound having a perfluoroalkyl group. Furthermore, the fluorine compound may also be a compound containing a long chain alkyl compound as described later.

[0095] Examples of the compound having a perfluoroalkyl group include perfluoroalkyl group-containing (meth)acrylates such as perfluoroalkyl (meth)acrylate, perfluoroalkyl methyl (meth)acrylate, 2-perfluoroalkyl ethyl (meth)acrylate, 3-perfluoroalkyl propyl (meth)acrylate, 3-perfluoroalkyl-1-methylpropyl (meth)acrylate, and 3-perfluoroalkyl-2-propenyl (meth)acrylate, and polymers thereof; and perfluoroalkyl group-containing vinyl ethers such as perfluoroalkyl methyl vinyl ether, 2-perfluoroalkyl ethyl vinyl ether, 3-perfluoropropyl vinyl ether, 3-perfluoroalkyl-1-methylpropyl vinyl ether, and 3-perfluoroalkyl-2-propenyl vinyl ether, and polymers thereof. In consideration of heat resistance and contamination, a polymer is preferable. The polymer may be a single compound or a polymer of multiple compounds. In addition, from the viewpoint of releasability, the perfluoroalkyl group preferably has 3 to 11 carbon atoms. Furthermore, it may be a polymer with a compound containing a long-chain alkyl compound as described below. From the viewpoint of adhesion to the substrate, a polymer with vinyl chloride is also preferred.

[0096] In forming the resin layer (B), it is preferable to contain an antistatic agent from the viewpoint of preventing adhesion of foreign matter, etc., and for example, a polymer in which a compound made of thiophene or a thiophene derivative is doped with another anionic compound, a self-doped polymer having an anionic group in a compound made of thiophene or a thiophene derivative, or a polymer containing a monomer having an alkylsulfonate ion as a counter ion as a component can be used. Among them, it is more preferable to contain a compound made of thiophene or a thiophene derivative from the viewpoint of obtaining excellent antistatic performance.

[0097] Examples of the compound made of thiophene or a thiophene derivative include a polymer obtained by doping a compound made of thiophene or a thiophene derivative with another anionic compound, and examples of the self-doped polymer having an anionic group in a compound made of thiophene or a thiophene derivative include a polymer obtained by polymerizing a compound of the following formula (6) or (7) in the presence of a polyanion.

[0098] [ka]

[0099] In the above formula (6), R 1 and R 2 each independently represents a hydrogen atom or an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, or the like having 1 to 20 carbon atoms.

[0100] [ka]

[0101] In the above formula (7), n represents an integer of 1 to 4.

[0102] Examples of polyanions used in polymerization include poly(meth)acrylic acid, polymaleic acid, polystyrene sulfonic acid, polyvinyl sulfonic acid, etc. As a method for producing such a polymer, for example, a method such as that shown in JP-A-7-90060 can be adopted.

[0103] In the present invention, the compound of the above formula (7) in which n is 2 and polystyrene sulfonic acid is used as the polyanion is preferably used.

[0104] When these polyanions are acidic, they may be partially or completely neutralized. The base used for neutralization is preferably ammonia, organic amines, or alkali metal hydroxides.

[0105] A specific example of the polymer containing a monomer having an alkylsulfonate ion as a counter ion as a component is, for example, a polymer having a component represented by the following formula (8) as a repeating unit. These may be homopolymers or copolymers, or may be copolymerized with a plurality of other components. From the viewpoint of improving antistatic properties, homopolymers are preferred.

[0106] [ka]

[0107] The structure of the polymer may be, for example, a substituent R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 is -O- or -NH-, R 3 is an alkylene group having 1 to 6 carbon atoms or other structure capable of forming the structure of formula (8), R 4 , R 5 , R 6 At least one of the substituents is a hydrogen atom, and the other substituents are an alkyl group having 1 to 3 carbon atoms or a hydroxyalkyl group having 2 to 3 carbon atoms in the alkyl group; X - Examples of the cation include alkylsulfonate ions having an alkyl group having 1 to 4 carbon atoms.

[0108] In forming the resin layer (B), it is preferable to include a polyhydroxy compound for the purpose of improving the coating appearance and antistatic performance. As the polyhydroxy compound, it is preferable to use one or more compounds selected from polyglycerin and alkylene oxide adducts to polyglycerin, or derivatives thereof. Polyglycerin is a compound represented by the following general formula (9).

[0109] [ka]

[0110] In the above formula, n is 2 or more, and in the present invention, n in the formula is usually in the range of 2-20, preferably 3-15, and more preferably 3-12.

[0111] The alkylene oxide adduct to polyglycerin has a structure in which alkylene oxide is addition polymerized to the hydroxyl group of polyglycerin represented by the above general formula (9).

[0112] Here, the structure of the alkylene oxide added to each hydroxyl group of the polyglycerin skeleton may be different, and it is sufficient that the alkylene oxide or its derivative is added to at least one hydroxyl group in the molecule, and it is not necessary that the alkylene oxide or its derivative is added to all hydroxyl groups.

[0113] The alkylene oxide added to polyglycerin is preferably ethylene oxide or propylene oxide. If the alkylene chain of the alkylene oxide is too long, the hydrophobicity becomes strong, dispersibility in the coating liquid deteriorates, and the antistatic property and transparency of the resin layer (B) tend to deteriorate. Ethylene oxide is particularly preferable. The number of additions is preferably in the range of 200 to 2000, more preferably in the range of 300 to 1000, and even more preferably in the range of 400 to 900, in terms of the number average molecular weight (Mn) of the final compound.

[0114] The above polyglycerols or alkylene oxide adducts of polyglycerols may be used alone or in combination of two or more kinds.

[0115] In forming the resin layer (B), various conventionally known polymers can be used as binder components from the viewpoint of improving the coating appearance and transparency, and specific examples of the polymers include polyester resins, urethane resins, acrylic resins, polyvinyl alcohol, vinyl chloride-vinyl acetate copolymers, etc. From the viewpoint of making the resin layer (B) stronger and reducing blocking, it is preferable to use polyester resins and urethane resins.

[0116] The polyester resin may be composed of, for example, the following polyvalent carboxylic acid and polyvalent hydroxy compound as main components. That is, as the polyvalent carboxylic acid, terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, p-hydroxybenzoic acid, trimellitic acid monopotassium salt, and ester-forming derivatives thereof may be used. Examples of polyhydric hydroxy compounds that can be used include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. The polyester resin is a polycondensation product of a polyvalent carboxylic acid and a polyvalent hydroxy compound. One or more polyvalent carboxylic acids and one or more polyvalent hydroxy compounds are appropriately selected from the above-mentioned compounds, and the polyester resin may be synthesized by a conventional polycondensation reaction. The polyester resin may be made into a water dispersion, and in this case, a hydrophilic functional group or the like may be appropriately introduced into the polyester resin.

[0117] A urethane resin is a polymeric compound that has a urethane bond in the molecule. Usually, a urethane resin is produced by the reaction of a polyol with an isocyanate. Examples of polyols include polycarbonate polyols, polyester polyols, polyether polyols, polyolefin polyols, and acrylic polyols. These compounds may be used alone or in combination.

[0118] Polycarbonate polyols are obtained by dealcoholization reaction between polyhydric alcohols and carbonate compounds. Examples of polyhydric alcohols include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and 3,3-dimethylolheptane. Examples of carbonate compounds include dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, etc., and examples of polycarbonate-based polyols obtained by the reaction of these compounds include poly(1,6-hexylene) carbonate, poly(3-methyl-1,5-pentylene) carbonate, etc.

[0119] Examples of polyester polyols include polycarboxylic acids (malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, fumaric acid, maleic acid, terephthalic acid, isophthalic acid, etc.) or their acid anhydrides and polyhydric alcohols (ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, 1,6 ... 2-ethyl-2,4-pentanediol, 2-methyl-2-propyl-1,3-propanediol, 1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-2-hexyl-1,3-propanediol, cyclohexanediol, bishydroxymethylcyclohexane, dimethanolbenzene, bishydroxyethoxybenzene, alkyldialkanolamines, lactonediols, etc.

[0120] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene ether glycol, and polyhexamethylene ether glycol.

[0121] Of the above polyols, polycarbonate polyols and polyester polyols are more preferably used in order to improve adhesion to various functional layers.

[0122] Examples of polyisocyanate compounds used to obtain urethane resins include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate, aliphatic diisocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate, aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate, and alicyclic diisocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and isopropylidenedicyclohexyl diisocyanate. These may be used alone or in combination.

[0123] A chain extender may be used when synthesizing the urethane resin. The chain extender is not particularly limited as long as it has two or more active groups that react with an isocyanate group, and generally, a chain extender having two hydroxyl groups or two amino groups can be mainly used.

[0124] Examples of chain extenders having two hydroxyl groups include glycols such as aliphatic glycols, such as ethylene glycol, propylene glycol, and butanediol; aromatic glycols, such as xylylene glycol and bishydroxyethoxybenzene; and ester glycols, such as neopentyl glycol hydroxypivalate. Examples of chain extenders having two amino groups include aromatic diamines such as tolylenediamine, xylylenediamine, and diphenylmethanediamine; aliphatic diamines such as ethylenediamine, propylenediamine, hexanediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-1,5-pentanediamine, trimethylhexanediamine, 2-butyl-2-ethyl-1,5-pentanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine; and alicyclic diamines such as 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, dicyclohexylmethanediamine, isopropylidenecyclohexyl-4,4'-diamine, 1,4-diaminocyclohexane, and 1,3-bisaminomethylcyclohexane.

[0125] The urethane resin in the present invention may be a solvent-based resin, and is preferably a water-based resin. To disperse or dissolve the urethane resin in water, there are forced emulsification types using an emulsifier, self-emulsification types in which a hydrophilic group is introduced into the urethane resin, and water-soluble types. In particular, the self-emulsification type in which an ionic group is introduced into the structure of the urethane resin to form an ionomer is preferred, since it has excellent storage stability of the liquid and excellent water resistance, transparency, and adhesion of the resulting coating layer.

[0126] The ionic group to be introduced may be a carboxyl group, sulfonic acid, phosphoric acid, phosphonic acid, quaternary ammonium salt, or the like, but the carboxyl group is preferred. Various methods can be used to introduce the carboxyl group into the urethane resin at each stage of the polymerization reaction. For example, a method of using a resin having a carboxyl group as a copolymerization component during prepolymer synthesis, or a method of using a component having a carboxyl group as one component of a polyol, polyisocyanate, chain extender, or the like, is used. In particular, a method of using a carboxyl group-containing diol and introducing a desired amount of carboxyl groups depending on the amount of this component is preferred. For example, dimethylolpropionic acid, dimethylolbutanoic acid, bis-(2-hydroxyethyl)propionic acid, bis-(2-hydroxyethyl)butanoic acid, or the like can be copolymerized with the diol used in the polymerization of the urethane resin. In addition, the carboxyl group is preferably in the form of a salt neutralized with ammonia, amine, alkali metals, inorganic alkalis, or the like. Particularly preferred are ammonia, trimethylamine, and triethylamine. In such polyurethane resins, the carboxyl groups from which the neutralizing agent is removed during the drying process after coating can be used as crosslinking reaction points with other crosslinking agents, which not only provides excellent stability in the liquid state before coating, but also makes it possible to further improve the durability, solvent resistance, water resistance, blocking resistance, etc. of the resulting coating layer.

[0127] The acrylic resin is a polymer made of polymerizable monomers including acrylic and methacrylic monomers. These may be homopolymers or copolymers, or copolymers with polymerizable monomers other than acrylic and methacrylic monomers. The acrylic resin also includes copolymers of these polymers with other polymers (e.g., polyester, polyurethane, etc.). For example, block copolymers and graft copolymers. That is, the acrylic resin may be an acrylic-modified polyester resin or an acrylic-modified polyurethane resin. The acrylic resin also includes a polymer (or a mixture of polymers in some cases) obtained by polymerizing a polymerizable monomer in a polyester solution or polyester dispersion. Similarly, the acrylic resin also includes a polymer (or a mixture of polymers in some cases) obtained by polymerizing a polymerizable monomer in a polyurethane solution or polyurethane dispersion. Similarly, the acrylic resin also includes a polymer (or a mixture of polymers in some cases) obtained by polymerizing a polymerizable monomer in another polymer solution or dispersion, and these are also referred to as acrylic-modified polyester resins and acrylic-modified polyurethane resins in this specification. The polyesters and polyurethanes used in the acrylic resins can be appropriately selected from those exemplified as the polyesters and polyurethanes as the binder components described above. The acrylic resin may contain a hydroxyl group or an amino group in order to further improve adhesion to the substrate film.

[0128] The polymerizable monomer is not particularly limited, but representative compounds include, for example, various carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, and citraconic acid, and salts thereof; various hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, monobutyl hydroxyl fumarate, and monobutyl hydroxy itaconate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, and the like. various nitrogen-containing compounds such as (meth)acrylamide, diacetone acrylamide, N-methylol acrylamide, or (meth)acrylonitrile; various styrene derivatives such as styrene, α-methylstyrene, divinylbenzene, or vinyl toluene; various vinyl esters such as vinyl propionate; various silicon-containing polymerizable monomers such as γ-methacryloxypropyltrimethoxysilane or vinyltrimethoxysilane; phosphorus-containing vinyl monomers; various vinyl halides such as vinyl chloride or vinylidene chloride; and various conjugated dienes such as butadiene.

[0129] In order to improve the strength of the resin layer (B), a crosslinking agent can be used in combination. The crosslinking agent can be a conventionally known material, for example, an oxazoline compound, an epoxy compound, a melamine compound, an isocyanate compound, a carbodiimide compound, an organic silicon compound, etc. From the viewpoint of increasing the strength of the resin layer (B), a melamine compound is more preferable. In addition, two or more types of crosslinking agents can be used in combination.

[0130] The resin layer (B) in the present release film may contain particles for the purpose of improving the slipperiness of the film, but a more preferred embodiment is one in which the resin layer (B) does not substantially contain particles. By substantially not containing particles in the resin layer (B), the release properties can be stabilized while the migration of the release component can be reduced.

[0131] In addition, "substantially not containing" means that the resin layer (B) may contain particles as long as the amount is small enough not to impair the effects of the present invention, and may contain particles that are inevitably mixed in. The specific content of particles in the resin layer (B) is, for example, less than 0.05% by mass, preferably less than 0.01% by mass, and more preferably less than 0.0001% by mass, based on the non-volatile components. The range of the content of particles in the resin layer (B) based on the non-volatile components is also the same as the content of the particles.

[0132] Furthermore, within the scope of the present invention, the resin layer (B) may contain, as necessary, an antifoaming agent, a coatability improving agent, a thickener, an organic lubricant, an antistatic agent, an ultraviolet absorber, an antioxidant, a foaming agent, a dye, a pigment, etc.

[0133] In the resin layer (B), the content of the release agent in the non-volatile components is preferably 10 to 70% by mass. When the content of the release agent is 10% by mass or more, good anti-blocking performance is obtained. In the resin layer (B), when a long-chain alkyl group-containing compound is used as a non-silicone-based release agent, the long-chain alkyl group-containing compound is preferably 5 to 90% by mass, more preferably 10 to 70% by mass, even more preferably 20 to 60% by mass, and most preferably 20 to 40% by mass, as a proportion of the total non-volatile components in the resin layer (B) composition. When the proportion of the long-chain alkyl group-containing compound is in the above range, good blocking prevention performance is obtained, and by reducing the change in the release properties of the release layer due to blocking, it is possible to greatly suppress the heavy peeling of the release layer at the lower winding part of the roll where more pressure is applied to the film.

[0134] When wax is used as a non-silicone release agent in the resin layer (B), the wax is preferably 5 to 90% by mass, more preferably 10 to 80% by mass, and even more preferably 25 to 70% by mass, of the total non-volatile components in the resin layer (B). When the wax ratio is within the above range, good blocking prevention performance is obtained, and the change in the release properties of the release layer due to blocking is reduced, so that the heavy peeling of the release layer at the lower winding part of the roll where the film is subjected to more pressure can be greatly suppressed. In addition, when used in combination with a melamine compound, heavy peeling may progress. Therefore, when using wax, it is necessary to pay attention to the combination with a crosslinking agent, etc. On the other hand, a compound containing a long chain alkyl group is more preferable because it does not have the following problems.

[0135] The reason (estimate) why wax, as a non-silicone release agent, has a higher heavy release rate than a compound containing a long-chain alkyl group depending on the combination with a crosslinking agent is thought to be as follows. In addition to being water-repellent, wax also has oil-repellent properties, which makes it less compatible with the melamine compounds it is combined with, making the melamine compounds more likely to be repelled. On the other hand, in the evaluation of the heavy peeling rate of the present invention, since the pressing process is performed under high temperature (40°C) and high humidity (90% RH) in the presence of moisture, it is presumed that agglomerates are easily formed on the surface of the resin layer (B) which combines wax and a melamine compound, and this improves the adhesion with the silicone release layer on the opposite side, resulting in a higher heavy peeling rate. As described above, the present invention is characterized in that a release agent is selected with an eye on the oil repellency effect, which has not been given much attention in conventional non-silicone release agents, and a release film is constructed having a resin layer (B).

[0136] In the case where a compound made of thiophene or a thiophene derivative is used as an antistatic agent in the resin layer (B), the proportion of the compound made of thiophene or a thiophene derivative in the total non-volatile components of the resin layer (B) is preferably in the range of 5 to 50 mass%, more preferably 5 to 40 mass%, and further preferably 5 to 30 mass%. When it is in the above range, good antistatic properties can be obtained.

[0137] In the resin layer (B), the polyhydroxy compound is preferably in the range of 10 to 80 mass %, more preferably 20 to 70 mass %, and further preferably 30 to 65 mass %, as a ratio of the total non-volatile components of the resin layer (B). When it is in the above range, good antistatic properties can be obtained.

[0138] The proportion of the binder component in the total non-volatile components of the resin layer (B) is preferably in the range of 5 to 50 mass%, more preferably 5 to 40 mass%, and further preferably 5 to 30 mass%. When the proportion of the binder component is in the above range, the strength of the resin layer (B) is good, and blocking can be reduced.

[0139] The crosslinking agent preferably accounts for 5 to 70% by mass, more preferably 10 to 60% by mass, and further preferably 15 to 50% by mass of the total non-volatile components of the resin layer (B). When the crosslinking agent ratio is within the above range, the strength of the resin layer (B) is good, and blocking can be reduced.

[0140] <Characteristics of resin layer (B)> The resin layer (B) in the present invention may have the following properties.

[0141] In this release film, the average surface roughness (Sa(B)) of the film surface on the side opposite to the resin layer (A), i.e., the side of the film having the resin layer (B), is 30 nm or more. If Sa(B) is 30 nm or more, blocking is unlikely to occur in the rolled state after the release layer is provided. On the other hand, Sa(B) is preferably 60 nm or less. If Sa(B) is 60 nm or less, when this release film is wound into a roll, the unevenness of the film is not transferred to the release layer, and the release properties of the release layer are maintained. From the above viewpoints, Sa(B) is preferably in the range of 30 nm or more and 55 nm or less, and more preferably in the range of 35 nm or more and 50 nm or less. When the resin layer (B) is provided, it is preferable that Sa(B) of the resin layer (B) is within the above range.

[0142] The average surface roughness (Sa) is one of the surface roughness parameters (ISO 25178), and is a three-dimensional extension of the two-dimensional Ra. It is calculated by dividing the volume enclosed by the surface profile and the average surface by the measured area, and is calculated by the following formula (i). If the surface is the XY plane and the height direction is the Z axis, A is the defined area (the entire image), and Z(x,y) is the height of the image point (x,y) from the surface with height 0, then it can be expressed as in the following equation (i).

[0143]

number

[0144] The root mean square roughness (Sq(B)) of the film surface on the side having the resin layer (B) is preferably 100 nm or less. If Sq(B) is 100 nm or less, when the present release film is wound into a roll, the unevenness of the film is not transferred to the release layer, and the release properties of the release layer are maintained. On the other hand, Sq(B) is preferably 40 nm or more. If it is 40 nm or more, blocking is less likely to occur in the rolled state after the release layer is provided. From the above viewpoints, Sq(B) is more preferably in the range of 40 nm or more and 90 nm or less, and further preferably in the range of 40 nm or more and 80 nm or less. It is preferable that the root mean square roughness (Sq(B2)) of the surface of the resin layer (B) also satisfies the above range.

[0145] In the above formula, Sq is the three-dimensional extension of the two-dimensional Rq (RMS), which represents the standard deviation σ in statistics. It is the root-mean-square deviation obtained by dividing the volume of the area between the curved surface obtained by squaring the distance between the surface shape curved surface and the average surface and the average surface by the measured area, and then calculating the square root, and can be calculated from the following formula (ii).

[0146]

number

[0147] The surface area ratio Sdr(B) of the film surface on the side having the resin layer (B) is 3.5×10 -2 % or more. Sdr(B) must be 3.5×10 -2 % or more, a suitably fine uneven shape can be imparted to the film surface on the side having the resin layer (B). From the above viewpoints, Sdr(B) is preferably 4.0×10 -2 % or more, and more preferably 4.5 × 10 -2 % or more, especially 5.0×10 -2 % or more is preferable. The upper limit is 6.0×10 -2 % is a good guideline. The upper limit is 5.0×10 -1 % or less, and preferably 2.0×10 -1 % or less, and preferably 1.0×10 -1 % or less is particularly preferable. Furthermore, it is preferable that the surface area ratio Sdr(B2) of the resin layer (B) surface also satisfies the above range. The surface area ratio Sdr(B2) is defined by ISO 25178 and is a value measured in accordance with this definition.

[0148] The maximum peak height (Sp) of the film surface on the side having the resin layer (B) is 880 nm or more, preferably 900 nm or more, and more preferably 950 nm or more. More preferably, it is 80 nm or less. There is no particular upper limit to the maximum peak height (Sp), but from the viewpoint of reducing damage to the release surface, it is preferably 1500 nm or less, more preferably 1300 nm or less, and of these, particularly 1100 nm or less. The maximum peak height (Sp) is one of the surface roughness parameters (ISO 25178), and indicates the maximum value of the height from the average plane of the surface, and is expressed by the following formula (iii).

[0149]

number

[0150] The thickness of the resin layer (B) is preferably 0.005 to 0.25 μm, more preferably 0.008 to 0.15 μm, and even more preferably 0.01 to 0.10 μm. By making the thickness of the resin layer (B) 0.25 μm or less, the non-silicone release agent component in the resin layer (B) is prevented from migrating to the release layer when the present release film is wound into a roll, and if the thickness of the resin layer (B) is 0.005 μm or more, good blocking prevention properties can be imparted. It can be assumed that unreacted compounds of various compounds, reacted compounds, or a mixture thereof are present in the resin layer (B).

[0151] The surface resistivity of the resin layer (B) surface is preferably 1×10 12 Ω / □ or less, more preferably 1×10 10 Ω / □ or less, more preferably 1×10 8 Ω / □ or less, most preferably 1×10 6 Ω / □ or less. There is no particular lower limit for the surface resistivity, but taking into account the cost of antistatic agents, it is 1×10 4 It is preferably Ω / □ or more. The lower the surface resistivity of the resin layer (B), the better the antistatic property, and the more effectively the film can be prevented from being charged up during the process, thereby preventing adhesion of foreign matter and the like.

[0152] The normal peel strength of the resin layer (B) is preferably 400 to 2000 g / inch, more preferably 400 to 1500 g / inch, and even more preferably 400 to 1000 g / inch. By making the normal peel strength of the resin layer (B) 2000 g / inch or less, good blocking prevention properties can be imparted, and when the present release film is wound into a roll, heavy peeling of the resin layer (A) can be suppressed at the lower winding part of the roll where pressure is applied by the film.

[0153] The surface free energy of the resin layer is preferably 50 mN / m or less, more preferably 40 mN / m or less, and even more preferably 30 mN / m or less. By making the surface free energy of the resin layer 50 mN / m or less, good blocking prevention properties can be imparted, and when the present release film is wound into a roll, heavy peeling of the release layer (A) at the bottom winding part of the roll where pressure is applied by the film can be suppressed. Details of the surface free energy are as described in the examples.

[0154] The elastic modulus of the resin layer (B) at 25° C. is preferably 500 MPa or more. The elastic modulus here is a value measured by a nanoindenter. If the elastic modulus is 500 MPa or more, when the present release film is wound into a roll, heavy peeling of the resin layer (A) does not occur even in the lower winding part of the roll where pressure is applied by the film.

[0155] <Undercoat layer> The present release film preferably has an undercoat layer between the substrate film and the resin layer (A) or (B).

[0156] The undercoat layer is used not only for the purpose of improving the adhesion between the base film and the resin layer (A) or the resin layer (B), but also for the purpose of imparting various functions to the release film. Examples of the undercoat layer include antistatic performance for suppressing peeling electrification in the process of peeling off a functional layer such as a pressure-sensitive adhesive layer provided on the resin layer (A) and preventing adhesion of foreign matter, and oligomer sealing performance for sealing the precipitation of oligomers from the polyester film when performing heat treatment at high temperature for a long time. In the present release film, it is preferable that the undercoat layer has antistatic performance. The undercoat layer may be a single layer or may be a structure of two or more layers. The undercoat layer preferably contains the following compounds (a) to (c). (a) A polymer in which a compound consisting of thiophene or a thiophene derivative is doped with another anionic compound, or a polymer in which a compound consisting of thiophene or a thiophene derivative has an anionic group and is self-doped. (b) Polyhydroxy compounds (c) one or more compounds selected from the group consisting of polyurethane resins, polyester resins, and acrylic resins

[0157] The undercoat layer having antistatic properties can use, as an antistatic agent, for example, a polymer in which a compound made of thiophene or a thiophene derivative described above as component (a) is doped with another anionic compound, or a self-doped polymer having an anionic group in a compound made of thiophene or a thiophene derivative, or a polymer containing as a component a monomer with an alkylsulfonate ion as a counter ion. Furthermore, for the purpose of improving the coating appearance and antistatic performance, the above-mentioned component (b) can be used. In the present release film, from the viewpoint of having good antistatic performance, it is more preferable that the undercoat layer contains a compound made of thiophene or a thiophene derivative.

[0158] In forming an undercoat layer having antistatic properties, it is preferable to use one or more compounds selected from the group consisting of polyglycerin represented by the general formula (9) and alkylene oxide adducts of polyglycerin, or derivatives thereof, in order to improve the antistatic properties.

[0159] The undercoat layer having antistatic properties may contain a binder component. As the binder, various conventionally known polymers such as polyester resin, acrylic resin, polyurethane resin, polyvinyl alcohol resin, etc. can be used. Among these, polyurethane resin, polyester resin, and acrylic resin described as the above component (c) are preferred, and polyurethane resin is particularly preferred from the viewpoint of improving the transparency and antistatic properties of the undercoat layer. These binder components may be used alone or in combination of two or more.

[0160] In order to improve the strength of the undercoat layer, a crosslinking agent can be used in combination. The crosslinking agent can be a conventionally known material, for example, an oxazoline compound, an epoxy compound, a melamine compound, an isocyanate compound, a carbodiimide compound, an organic silicon compound, etc. From the viewpoint of increasing the strength of the undercoat layer, a melamine compound is more preferable. Two or more crosslinking agents can be used in combination.

[0161] In the case where a compound made of thiophene or a thiophene derivative is used as an antistatic agent in the undercoat layer, the compound made of thiophene or a thiophene derivative is preferably in the range of 5 to 50% by mass, more preferably 5 to 40% by mass, and further preferably 5 to 30% by mass, in terms of the ratio of the total non-volatile components of the undercoat layer. When in the above range, good antistatic properties can be obtained.

[0162] In the undercoat layer, the proportion of one or more compounds selected from polyglycerin and alkylene oxide adducts of polyglycerin or derivatives thereof in the total non-volatile components of the undercoat layer is preferably in the range of 10 to 80% by mass, more preferably 20 to 70% by mass, and even more preferably 30 to 65% by mass. When in the above range, good antistatic properties can be obtained.

[0163] The proportion of the binder component in the total non-volatile components of the undercoat layer is preferably in the range of 5 to 50 mass%, more preferably 5 to 40 mass%, and even more preferably 5 to 30 mass%. When the proportion of the binder component is in the above range, the strength of the undercoat layer is good, and the antistatic properties can be improved.

[0164] The crosslinking agent preferably accounts for 5 to 70% by mass, more preferably 10 to 60% by mass, and even more preferably 15 to 50% by mass of the total non-volatile components of the undercoat layer. When the crosslinking agent ratio is within the above range, the strength of the undercoat layer is good, and blocking can be reduced.

[0165] The undercoat layer having oligomer sealing properties may be provided with an undercoat layer having oligomer sealing properties that contains an organic compound containing one or more metal elements selected from aluminum, titanium and zirconium.

[0166] The undercoat layer having oligomer sealing properties may be provided directly on the substrate film, or may be provided on the undercoat layer having antistatic properties.

[0167] It is assumed that the undercoat layer contains unreacted compounds of the various compounds in the resin composition, reacted compounds, or a mixture thereof.

[0168] <Characteristics of the undercoat layer> The thickness of the undercoat layer having antistatic properties is preferably 0.005 μm or more and 0.25 μm or less, more preferably 0.008 μm or more and 0.15 μm or less, and even more preferably 0.01 μm or more and 0.10 μm or less. If the thickness of the undercoat layer is within the above range, good antistatic properties can be imparted.

[0169] The surface resistivity of the undercoat layer surface having antistatic properties is preferably 1×10 12 Ω / □ or less, more preferably 1×10 10 Ω / □ or less, more preferably 1×10 8 Ω / □ or less, most preferably 1×10 6 Ω / □ or less. There is no particular lower limit for the surface resistivity, but taking into account the cost of antistatic agents, it is 1×10 4 It is preferably Ω / □ or more. The lower the surface resistivity of the resin layer (B), the better the antistatic property, and the more effectively the film can be prevented from being charged up during the process, thereby preventing adhesion of foreign matter and the like.

[0170] <Method of forming resin layer (B) and undercoat layer> Next, the method for forming the resin layer (B) and the undercoat layer will be described.

[0171] The resin layer (B) and the undercoat layer are formed by coating a coating liquid onto a film, and may be formed by in-line coating carried out during the film production process, or may be formed by applying the coating outside the system onto a film that has already been produced, so-called off-line coating, more preferably in-line coating.

[0172] In-line coating is a method of coating within the polyester film production process, specifically, a method of coating at any stage from melt extrusion of polyester to stretching, heat setting and winding up. Usually, coating is performed on any of the following: an unstretched sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, or a film after heat setting and before winding up. Although not limited to the following, for example, in the case of sequential biaxial stretching, a method in which a uniaxially stretched film stretched in the longitudinal direction (machine direction) is coated and then stretched in the transverse direction is particularly excellent. According to such a method, film formation and formation of the resin layer (B) can be performed simultaneously, which is advantageous in terms of production costs, and since stretching is performed after coating, the thickness of the resin layer (B) can be changed by the stretching ratio, making it easier to perform thin film coating than with offline coating films. In addition, by providing the resin layer (B) on the film before stretching, the resin layer (B) can be stretched together with the polyester film, which allows the resin layer (B) to be firmly attached to the polyester film. Furthermore, in the production of biaxially oriented polyester film, by stretching while holding the film ends with clips or the like, the film can be restrained in the longitudinal and transverse directions, and in the heat setting step, high temperatures can be applied while maintaining flatness and without wrinkles, etc. Therefore, since the heat treatment performed after coating can be performed at a high temperature that cannot be achieved by other methods, the resin layer (B) and the undercoat layer are cured more rapidly than in offline coating, and a stronger coating film can be formed.

[0173] When the resin layer (B) is provided by in-line coating, it is preferable to produce the base film by coating a resin layer (B) composition, which is prepared by preparing an aqueous solution or aqueous dispersion of the above-mentioned series of compounds so that the solid content (total non-volatile components) is adjusted to approximately 0.1 to 50 mass %, onto a polyester film.

[0174] Examples of a method for applying the resin layer (B) composition or the undercoat layer composition to the film include conventional coating methods such as air doctor coating, blade coating, rod coating, bar coating, knife coating, squeeze coating, impregnation coating, reverse roll coating, transfer roll coating, gravure coating, kiss roll coating, cast coating, spray coating, curtain coating, calendar coating, and extrusion coating.

[0175] The drying and curing conditions when forming the resin layer (B) and the undercoat layer on the film are not particularly limited. When the resin layer (B) is provided by in-line coating, the heat treatment is preferably performed at 70 to 270°C for 3 to 200 seconds, more preferably at 100 to 260°C, and even more preferably at 110 to 250°C for 10 to 100 seconds.

[0176] On the other hand, when the resin layer (B) is provided by off-line coating, the heat treatment is preferably carried out at 80 to 200° C. for 3 to 40 seconds, more preferably at 100 to 180° C. for 3 to 40 seconds.

[0177] Regardless of whether off-line coating or in-line coating is used, heat treatment and irradiation with active energy rays such as ultraviolet rays may be used in combination as necessary. The film constituting the release film in the present invention may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment.

[0178] <<Adhesive sheet>> The release film in the present invention may have a laminated structure, and a suitable example is an adhesive sheet comprising the present release film and another release film via an adhesive layer (hereinafter sometimes referred to as "the present adhesive sheet"). A preferred embodiment is one in which an adhesive layer is laminated on the surface of the resin layer (A) side of the present release film. A more preferred embodiment is one in which the present release film is used as the first release film, an adhesive layer is used on the resin layer (A) side of the present release film, and a release film having a different peeling strength from the present release film is used as the second release film on the other surface of the adhesive layer to which the resin layer (A) of the present release film is attached, and they are attached to each other. A further preferred embodiment is one in which the adhesive layer is an optical transparent adhesive sheet (OCA), and the present release film is used as the release film with a lighter peeling strength, and they are attached to each other. The adhesive layer may be a single layer or a structure of two or more layers. In addition, the above-mentioned "release film having a different peeling force from that of the present release film" means that the peeling force of the release film evaluated by the measurement method as described in the examples is different from the peeling force of the resin layer (A) side of the present release film. In addition, the release film having a different peeling force from that of the present release film is preferably larger than the peeling force of the resin layer (A) of the present release film, and specifically, the peeling force is preferably 1.5 to 10 times, more preferably 1.5 to 8 times, and even more preferably about 1.5 to 6 times. By satisfying the above-mentioned peeling force, it is possible to reduce the problem of peeling of the resin layer (A) of the present release film in a situation where peeling is not originally required.

[0179] <Adhesive layer> The adhesive layer will be described below. The adhesive layer is a layer made of an adhesive composition, and may be an acrylic adhesive composition mainly made of an acrylic resin, a rubber-based adhesive composition mainly made of rubber, a urethane-based adhesive composition mainly made of a urethane resin, or a silicone-based adhesive composition mainly made of a silicone resin. Among them, an acrylic adhesive composition mainly made of an acrylic resin is preferred because the adhesive composition can adjust the adhesive strength and peel strength in a well-balanced manner and is inexpensive. The above-mentioned "main component resin" means a resin having the highest mass ratio among the resins constituting the adhesive composition. For example, it means a component that occupies 50 mass% or more, preferably 60 mass% or more, more preferably 70 mass% or more of the total amount of resins constituting the adhesive composition. The upper limit is 100 mass%, but is usually 99.99 mass%.

[0180] (Acrylic resin) The acrylic resin that is the main component resin of the pressure-sensitive adhesive composition may be a (meth)acrylic polymer. The (meth)acrylic polymer is a polymer having a (meth)acrylic acid alkyl ester as a main constituent unit. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, isobornyl (meth)acrylate, 4-t-butylcyclohexyl (meth)acrylate, tricyclodecanyl (meth)acrylate, dicyclopentaenyl (meth)acrylate, and adamantyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, methyl (meth)acrylate is preferred from the viewpoints of compatibility with other (meth)acrylates constituting the (meth)acrylic polymer and heat resistance of the cured resin layer (B)(B). The content of the (meth)acrylic acid alkyl ester in the monomers forming the (meth)acrylic polymer is, for example, 50% by mass or more, preferably 60 to 99.99% by mass, more preferably 75 to 98.9% by mass, and further preferably 87 to 97.8% by mass. The (meth)acrylic polymer may have a radically polymerizable double bond.

[0181] For the purpose of improving the glass transition temperature, mechanical properties, compatibility, etc., the (meth)acrylic polymer can be copolymerized with (meth)acrylic acid esters other than (meth)acrylic acid alkyl esters, (meth)acrylic acid, and other compounds having a vinyl group. Examples of (meth)acrylic acid esters other than the above-mentioned (meth)acrylic acid alkyl esters that can be used as copolymerization components include hydroxyalkyl (meth)acrylates, alkoxyalkyl (meth)acrylates such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate, as described below, phenyl (meth)acrylate, benzyl (meth)acrylate, glycidyl (meth)acrylate, and γ-butyrolactone (meth)acrylate. Examples of the compound having a vinyl group include acrylamide compounds such as dimethylacrylamide, hydroxyethylacrylamide, and dimethylaminopropylacrylamide; styrene compounds such as styrene, α-methylstyrene, and p-methoxystyrene; and maleic anhydride. In addition, components (a1) and (a2) described below can also be used appropriately.

[0182] In the present invention, the monomer constituting the (meth)acrylic polymer may contain, in addition to the (meth)acrylic acid alkyl ester, an acrylic monomer (a1) as a copolymerization component, which serves as a reaction site with the crosslinking agent described below.

[0183] The acrylic monomer (a1) is a reactive site of a crosslinking structure when it is copolymerized with other copolymerization components to form an acrylic resin, and a monomer containing a functional group capable of reacting with a functional group contained in a crosslinking agent described later may be used. Examples of such an acrylic monomer (a1) include a hydroxyl group-containing monomer, an amino group-containing monomer, an acetoacetyl group-containing monomer, an isocyanate group-containing monomer, and a glycidyl group-containing monomer. Among these, a hydroxyl group-containing monomer is preferably used because it can efficiently crosslink with a crosslinking agent. The acrylic monomer (a1) may be used alone or in combination of two or more kinds.

[0184] Examples of hydroxyl group-containing monomers include acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl 2-hydroxyethyl phthalate and N-methylol (meth)acrylamide; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro 2-hydroxypropyl (meth)acrylate; and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate.

[0185] Among the above hydroxyl group-containing monomers, primary hydroxyl group-containing monomers are preferred because of their excellent reactivity with crosslinking agents. Furthermore, the use of 2-hydroxyethyl acrylate is particularly preferred because it contains less impurities such as di(meth)acrylates and is easy to produce.

[0186] In addition, as the hydroxyl group-containing monomer used in the present invention, it is also preferable to use one having a content of di(meth)acrylate as an impurity of 0.5% by mass or less, more preferably 0.2% by mass or less, and particularly preferably 0.1% by mass or less. Specifically, as the hydroxyl group-containing monomer, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, etc. are particularly preferable, and these are preferable in that they have a low molecular weight and are easy to purify.

[0187] Examples of the amino group-containing monomer include t-butylaminoethyl (meth)acrylate, ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate.

[0188] Examples of acetoacetyl group-containing monomers include 2-(acetoacetoxy)ethyl (meth)acrylate and allyl acetoacetate.

[0189] Examples of the isocyanate group-containing monomer include 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, and alkylene oxide adducts thereof.

[0190] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and allyl glycidyl (meth)acrylate.

[0191] The content of the acrylic monomer (a1) in the monomers constituting the (meth)acrylic polymer is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and particularly 0.2 to 3 mass%. When the acrylic monomer (a1) is equal to or more than the lower limit, the crosslinking points during crosslinking are appropriate, so that the cohesive strength after crosslinking is good. When the content is equal to or less than the upper limit, the adhesive strength can be prevented from decreasing due to the (a1) component.

[0192] Furthermore, the monomer constituting the (meth)acrylic polymer may contain, in addition to the (meth)acrylic acid alkyl ester, or the (meth)acrylic acid alkyl ester and the component (a1), a copolymerizable monomer (a2) other than (a1) as a copolymerization component, as necessary. Examples of the copolymerizable monomer (a2) include aromatic ring-containing monomers such as phenyl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, ethoxylated o-phenylphenyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, and styrene; amide monomers such as (meth)acryloylmorpholine, dimethyl(meth)acrylamide, diethyl(meth)acrylamide, and (meth)acrylamide; acrylonitrile, methacrylonitrile, vinyl acetate, vinyl propionate, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ethers, vinyl toluene, vinyl pyridine, vinyl pyrrolidone, dialkyl itaconic acid esters, dialkyl fumaric acid esters, allyl alcohol, acrylic chloride, methyl vinyl ketone, N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, and dimethylallyl vinyl ketone.

[0193] The content of the copolymerizable monomer (a2) in the monomers forming the (meth)acrylic polymer is preferably 0 to 20 mass%, more preferably 1 to 15 mass%, and particularly preferably 2 to 10 mass%. When the content of the copolymerizable monomer (a2) is within the above range, a decrease in adhesive properties due to the (a2) component can be prevented.

[0194] The adhesive composition may contain, other than the main component resin, as necessary, a crosslinking agent and other resins (other than the main component resin and the crosslinking agent) that constitute the adhesive components (e.g., acrylic resins, rubber, silicone resins, urethane resins).

[0195] (Crosslinking agent) The pressure-sensitive adhesive composition may contain a crosslinking agent depending on the curing method. Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, aldehyde-based crosslinking agents, and amine-based crosslinking agents. Among them, isocyanate-based crosslinking agents are preferably used in terms of improving adhesion to the substrate or reactivity with acrylic resins. The crosslinking agents may be used alone or in combination of two or more. The content of the crosslinking agent is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the main component resin. If the content of the crosslinking agent is within the above range, the cohesive strength is not insufficient, and the desired durability can be obtained, while a decrease in flexibility and adhesive strength can be prevented.

[0196] In addition, when the curing reaction is photocuring by irradiation with active energy rays, it is preferable to mix a polyfunctional (meth)acrylate into the adhesive composition as a crosslinking agent. Examples of such polyfunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and glycerin polyglycidyl ether poly(meth)acrylate.

[0197] (Other resins constituting adhesive components) The pressure-sensitive adhesive composition may contain, if necessary, other resins (e.g., acrylic resins, rubber, silicone resins, urethane resins) that constitute pressure-sensitive adhesive components other than the main component resin and crosslinking agent. For example, additives that may be blended include tackifiers such as rosin, rosin esters, hydrogenated rosin esters, phenolic resins, aromatic modified terpene resins, aliphatic petroleum resins, alicyclic petroleum resins, styrene-based resins, and xylene-based resins; conventional additives such as silane coupling agents, antistatic agents, colorants, fillers, antioxidants, ultraviolet absorbers, and functional dyes; and additives such as compounds that change color or undergo color change when exposed to ultraviolet rays or radiation. The amount of these additives is preferably 10 mass % or less of the entire pressure-sensitive adhesive composition (based on non-volatile components), and more preferably 5 mass % or less. In terms of excellent durability, it is preferable that the additives contain as few low molecular weight components with a molecular weight of less than 10,000 as possible.

[0198] <Method of forming adhesive layer> The method for forming the adhesive layer is not particularly limited, and the adhesive layer may be formed by coating the above-mentioned adhesive composition on the resin layer (A) of the present release film, followed by suitable drying, curing, etc. Alternatively, the adhesive composition may be coated on a base film or a release film having a release strength different from that of the present release film, followed by suitable drying, curing, etc., and then laminating the release layer (A layer) of the present release film to the surface opposite to the surface provided with the release film having a release strength different from that of the present release film. The pressure-sensitive adhesive composition may be cured depending on the crosslinking agent and main component resin, and may be cured by heating or by irradiation with light such as ultraviolet light. The pressure-sensitive adhesive composition may be appropriately diluted with an organic solvent or the like and then applied onto a release layer or the like.

[0199] <Characteristics of the adhesive layer> (Adhesive layer thickness) The thickness of the adhesive layer is not particularly limited. For example, from the viewpoint of imparting sufficient adhesive strength and filling unevenness or steps of the substrate to which the adhesive is attached, the thickness is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. On the other hand, from the viewpoint of material usage efficiency, transmittance, and outgassing, the thickness is preferably 10,000 μm or less, more preferably 3,000 μm or less, and even more preferably 1,000 μm or less.

[0200] (Elastic modulus of adhesive layer) In the present invention, the adhesive layer has an elastic modulus of 1×10 9 The elastic modulus here is a value measured by a nanoindenter. 9 When the elastic modulus is 1×10 Pa or less, the adhesive layer has good step absorbency. 8 Pa or less, more preferably 1×10 7 From the viewpoint of adhesive layer formability, the elastic modulus of the adhesive layer at 25°C is 1 × 10 4 Pa or more is preferable, 1×10 5 Pa or more is preferable, and 1×10 6 Pa or more is more preferable.

[0201] <<How to use the adhesive sheet>> The pressure-sensitive adhesive sheet of the present invention can be used in various laminated configurations. For example, the release film with the pressure-sensitive adhesive layer may be a film laminate in which an optical member is attached to the surface of the pressure-sensitive adhesive layer. Such a film laminate can be produced by peeling off the release film and attaching the optical member to an adherend by the exposed pressure-sensitive adhesive layer. Examples of the optical member include a polarizing plate and a touch sensor. The optical member may also be an in-vehicle optical member such as a touch panel mounted on an automobile.

[0202] (Polarizing plate) The material and structure of the polarizing plate are arbitrary, and for example, a polarizing plate of this type is widely used in which a TAC (triacetyl cellulose) film is laminated as a protective film on a stretched polyvinyl alcohol film using iodine as an orientation dye. The polarizing plate may have a layer structure on the surface that has a hard coat having substantially no phase difference, anti-glare, low reflection, anti-static, etc.

[0203] (Touch Sensor) A touch sensor is a component that detects the touched point when a user touches an image displayed on a screen with a finger or a touch pen. Depending on the sensor technology, examples include a capacitive type, a resistive film type, and a surface wave type using infrared rays or ultrasound. Touch sensors are generally installed in display devices such as liquid crystal display panels and organic electroluminescence (EL) displays. In recent years, there has been a trend to use a base film as an alternative to a glass substrate, focusing on flexibility, and it is preferable to use a touch sensor film. The touch sensor film generally has a patterned transparent conductive layer for performing the function of a sensing electrode.

[0204] <<<Explanation of terms, etc.>>> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". Furthermore, when the term "panel" is used, such as an image display panel, a protective panel, a touch panel, etc., it encompasses a plate, a sheet, and a film.

[0205] In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0206] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. The evaluation methods in the examples and comparative examples are as follows.

[0207] (1) Method for measuring intrinsic viscosity of polyester 1 g of polyester from which other polymer components incompatible with polyester and pigments had been removed was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and measured at 30°C.

[0208] (2) Measurement method for average particle size (d50: μm) The cumulative 50% (mass basis) value in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device (SA-CP3 type manufactured by Shimadzu Corporation) was taken as the average particle size.

[0209] (3) Method for measuring the thickness of the resin layer (A) To suppress reflection from the back side, black tape (Vinyl Tape VT-50, manufactured by Nichiban Co., Ltd.) was applied to the back side of the sample film beforehand. For the measurement, a spectrophotometer (UV-Visible Spectrophotometer V-670, manufactured by JASCO Corporation) was used to measure the absolute reflectance in the wavelength range of 300 to 800 nm under the following conditions: synchronous mode, incident angle 5°, N polarization, response Fast, data acquisition interval 1.0 nm, bandwidth 10 nm, and scanning speed 1000 m / min. The film thickness was calculated by comparing the data obtained from this measurement with the data calculated assuming the refractive index of silicone to be 1.43.

[0210] (4) Measurement of average surface roughness Using a ContourGT-I (manufactured by Bruker), the average surface roughness (Sa), maximum peak height (Sp), root mean square roughness (Sq), surface area ratio (Sdr), and number of protrusions per protrusion height were measured for the film surface opposite the resin layer (A). Observation mode: VXI SNR threshold: 2 Lens magnification: External: x20 Internal: x1 Measurement field of view: 316 μm (MD direction) × 237 μm (TD direction) × 10 fields of view (MD direction × 5, TD direction × 2) × 3 points on the same surface = 2.25 mm 2

[0211] (5) Molecular weight measurement of curable silicone resin The chromatogram was measured using a GPC measuring device, and the number average molecular weight (Mn) was calculated based on a calibration curve using standard polystyrene. Specifically, 4 mg of the sample for measurement was dissolved in 4 mL of THF to prepare a measurement solution, and 100 μL of the measurement solution was injected into the GPC measuring device for measurement. Tetrahydrofuran (THF) was used as the eluent. For the analysis, Tosoh Corporation's "Ecosec8320" was used, Tosoh Corporation's "TSKgel guardcolumn HXL-L" was used as the guard column, and four Tosoh Corporation's "TSKgel GMHXL" were used in connection as the column. The analysis was performed under the conditions of an oven temperature of 40°C and a THF flow rate of 1.0 mL / min, and RI was used for detection.

[0212] (6) Composition analysis of curable silicone resin The composition of the curable silicone resin used in the examples and comparative examples was analyzed using a 400 MHz-NMR (Bruker Avance400M). 1 The H-NMR measurement was performed at 30° C. using CDCl as a solvent and using the peak derived from the methyl group of dimethylsiloxane as the chemical shift standard.

[0213] (7) Measurement of normal peel strength of resin layer (A) The resin layer (A) surface of the sample film was pressed (twice back and forth) with a rubber roller (2 kg), and adhesive tape (Tesa's "No. 7475") was attached, then cut to a size of 25 mm x 150 mm and left at room temperature (23°C) for 1 hour, after which the peel strength was measured. The peel strength was measured using Intesco Model 2001 manufactured by Intesco Co., Ltd., and the sample film was peeled at 180° under the condition of a tensile speed of 0.3 m / min.

[0214] (8) Heavy peeling rate after pressing of resin layer (A) (alternative evaluation of blocking property) An acrylic adhesive tape ("No. 7475" manufactured by Tesa) was attached to the resin layer (A) surface of the release film of the examples and comparative examples, then cut to a size of 25 mm x 150 mm and left at room temperature for 1 hour. The peel force at 180° under the condition of a pulling speed of 0.3 m / min was defined as (F1). Next, the other side is placed facing the resin layer (A) side of the release film of the examples and comparative examples, and press treatment is performed for 20 hours at a temperature of 40°C, a humidity of 90% RH, and a load of 1 MPa. An acrylic adhesive tape (Tesa's "No. 7475") is attached to the resin layer (A) side after the treatment, and then cut to a size of 25 mm x 150 mm and left at room temperature for 1 hour. The peel force at 180° peeled under the condition of a tensile speed of 0.3 m / min is defined as (F2). The heavy peeling rate after pressing was calculated using the following formula, and this heavy peeling rate was used as an index of blocking resistance. Note that the blocking resistance is judged to be better as the heavy peeling rate is smaller. Heavy peeling rate after pressing (%) = (F2-F1) / F1 x 100

[0215] The polyesters used in the examples and comparative examples were prepared as follows.

[0216] <Polyester (A)> Homopolyethylene terephthalate (intrinsic viscosity = 0.65 dL / g)

[0217] <Polyester (B)> Masterbatch made by blending homopolyethylene terephthalate with 0.7% by mass of silica particles with an average particle size of 2.7 μm (intrinsic viscosity = 0.59 dL / g)

[0218] Example 1 The mixed raw material of polyester (A) and (B) mixed at a ratio of 40% by mass and 60% by mass, respectively, was used as the raw material for the outermost layer (surface layer), and 100% by mass of polyester (A) was used as the raw material for the intermediate layer. Each was fed to two extruders, melted at 290°C, and then co-extruded on a cooling roll set at 25°C in a layer structure of two types and three layers (surface layer / intermediate layer / surface layer = 1:18:1 discharge amount), cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.4 times in the longitudinal direction at a film temperature of 85°C using the roll peripheral speed difference, then introduced into a tenter, stretched 4.5 times in the transverse direction at 120°C, heat-treated at 225°C, and then relaxed 2% in the transverse direction to obtain a biaxially stretched polyester film with a thickness of 50 μm.

[0219] Next, resin layer (A) was formed on one side of the obtained polyester film by applying coating solution 1 for resin layer (A) shown in Table 2 using a No. 4 bar by bar coating method so that the coating thickness (after drying) was 0.5 μm, and then dried at 150° C. for 30 seconds to obtain a release film. The thicknesses of the surface layer / intermediate layer are as shown in Table 3. The physical properties measured by the above-mentioned methods are also shown in Table 3.

[0220] Comparative Example 1 A release film was obtained by producing in the same manner as in Example 1, except that the raw material composition of the polyester film and the thickness of the surface layer / intermediate layer were different. The physical property values ​​measured by the above-mentioned methods are shown in Table 3.

[0221] Examples of the compound constituting the resin layer (A) are as follows. a1: Curable silicone resin (a silicone resin in which vinyl groups have been introduced to the side chains and / or ends of the main chain consisting of siloxane bonds, number average molecular weight: 10600, viscosity at 25°C when adjusted to 15% by mass with n-heptane solvent: 1.7mcps)

[0222] The content (mol %) of the functional group in the curable silicone resin is as shown in Table 1 below.

[0223] [Table 1]

[0224] b1: Silicone crosslinker (CL750: manufactured by Momentive Performance Materials) c1: Addition type platinum catalyst (CM678: Momentive Performance Materials)

[0225] The coating liquid 1 constituting the resin layer (A) is as shown in Table 2 below.

[0226] [Table 2]

[0227] [Table 3] [Industrial Applicability]

[0228] According to the release film of the present invention, a release film can be provided that realizes super-easy peelability while being unlikely to change the peeling properties of the release layer due to blocking, and has high industrial value.In addition, the release film of the present invention and the film laminate including the release film have the characteristics of both super-easy peelability and blocking resistance, and are therefore suitable for applications in which changes in the peeling properties of the release layer and deterioration of the appearance of the resin layer (A) surface are undesirable, and are suitable for use in various applications in which the release layer is bonded via an adhesive layer, such as for the manufacture of capacitive touch panels, optical members (polarizing plates, retardation plates, prism sheets, conductive films, resin films, glass substrates, etc.) used in LCDs, for the manufacture of organic EL components, and for the manufacture of various display components such as LCDs and PDPs, as well as for the protection of various adhesive layers.

Claims

1. A release film comprising a resin layer (A) on one side of a base film, the resin layer (A) containing a silicone resin-based release agent and having a thickness of 0.2 to 2.0 μm after drying, and a film surface on the side opposite to the resin layer (A) that satisfies the following (1) and (2): (1) The average surface roughness Sa(B) is 30 nm or more. (2) Surface area ratio Sdr(B) is 3.5×10 -2 % or more

2. 2. The release film according to claim 1, further comprising a resin layer (B) on the surface of the film on which the resin layer (A) is not provided.

3. The release film according to claim 2 , wherein the resin layer (B) contains a non-silicone release agent.

4. 2. The release film according to claim 1, wherein the resin layer (A) has an elastic modulus at 25°C of 500 MPa or less, as measured using a nanoindenter apparatus.

5. The release film according to claim 3 , wherein the non-silicone release agent is at least one selected from the group consisting of waxes, compounds containing a long-chain alkyl group, and fluorine compounds.

6. The release film according to claim 3, wherein the content of the release agent in the non-volatile components of the resin layer (B) is 10 to 70 mass %.

7. The release film according to claim 2 , wherein the resin layer (B) is substantially free of particles.

8. 2. The release film according to claim 1, wherein the normal peel strength of the resin layer (A) is 5 g / inch or less, as measured by the following evaluation method. <Evaluation method> An acrylic adhesive tape ("No. 7475" manufactured by Tesa) is attached to the resin layer (A) surface of the release film, cut to a size of 25 mm x 150 mm, and left at room temperature for 1 hour. The peeling force is 180° at a pulling speed of 0.3 m / min.

9. The release film according to claim 2 , further comprising an undercoat layer between at least one of the resin layer (A) or the resin layer (B) and the base film.

10. The release film according to claim 9 , wherein the undercoat layer is an antistatic layer.

11. The release film according to claim 9, wherein the undercoat layer contains the following compounds (a) to (c): (a) A polymer in which a compound consisting of thiophene or a thiophene derivative is doped with another anionic compound, or a polymer in which a compound consisting of thiophene or a thiophene derivative has an anionic group and is self-doped. (b) Polyhydroxy Compound (c) one or more compounds selected from the group consisting of polyurethane resins, polyester resins, and acrylic resins

12. At least one of the surfaces of the resin layer (A) and the resin layer (B) has a surface resistivity of 1×10 12 The release film according to claim 2 , having a resistance to deformation of Ω / □ or less.

13. The release film according to claim 1 , wherein the base film is a polyester film.

14. The release film according to claim 13 , wherein the polyester film has a three-layer structure.

15. 15. The release film according to claim 14, wherein the relationship (t / r) between the thickness (t) of the film surface layer on the side opposite to the side where the resin layer (A) is provided and the average particle size (r) of the particles is 2.0 or less.

16. 2. The release film according to claim 1, wherein the resin layer (A) has a heavy peeling rate after pressing of 100% or less, as evaluated by the following method. <Evaluation method> An acrylic adhesive tape ("No. 7475" manufactured by Tesa) was attached to the surface of the resin layer (A), cut to a size of 25 mm x 150 mm, and left at room temperature for 1 hour. The peel strength at 180° under the condition of a tensile speed of 0.3 m / min was defined as (F1). Next, the resin layer (A) is laminated so as to contact the surface, and pressed for 20 hours at a temperature of 40° C., a humidity of 90% RH, and a load of 1 MPa. An acrylic adhesive tape (Tesa's "No. 7475") is attached to the resin layer (A) surface after the treatment, and then cut to a size of 25 mm x 150 mm and left at room temperature for 1 hour. The peel force at 180° peeled under the condition of a pulling speed of 0.3 m / min is defined as (F2). The heavy peeling rate after pressing is calculated using the following formula. Heavy peeling rate after pressing (%) = (F2 - F1) / F1 x 100

17. The release film according to claim 2 , wherein the average surface roughness (Sa(B)) of the resin layer (B) surface is 60 nm or less.

18. The release film according to claim 2, wherein the root mean square roughness (Sq(B)) of the resin layer (B) surface is 100 nm or less.

19. A pressure-sensitive adhesive sheet comprising the release film according to any one of claims 1 to 18 and another release film via an adhesive layer.

20. The adhesive sheet according to claim 19 , wherein the adhesive layer is formed from an acrylic adhesive layer composition.

21. The adhesive sheet according to claim 19, which is for use as an optically transparent adhesive sheet.

22. 20. A method for using the pressure-sensitive adhesive sheet according to claim 19, comprising peeling off the other release film and then attaching the exposed surface of the pressure-sensitive adhesive layer to an optical member.

23. The method for using the pressure-sensitive adhesive sheet according to claim 22, wherein the optical component is a polarizing plate or a touch sensor.

Citation Information

Patent Citations

  • Release film

    JP2004255704A

  • Mold release film excellent in releaseability

    JP2016165825A

  • Release film with excellent releasability

    JP2017061081A