Laminate, packaging bag and packaged article
A laminate with specific polyethylene layers and a gas barrier adhesive maintains recyclability and gas barrier properties, addressing the recyclability and impact resistance issues of conventional packaging materials.
Patent Information
- Application Number
- JP2023078769
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional packaging materials with laminates of different resin layers are difficult to recycle and suffer from deterioration of gas barrier properties after impact.
A laminate structure comprising a base layer and sealant layer made of polyethylene films with specific tensile moduli, and an adhesive layer formed by a gas barrier adhesive, enhancing recyclability and maintaining gas barrier properties post-impact.
The laminate maintains high recyclability and effectively prevents deterioration of gas barrier properties even after impact, ensuring the contents remain protected over time.
Smart Images

Figure 2024162840000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate, a packaging bag, and a packaging article. [Background technology]
[0002] In recent years, with the growing demand for the creation of a recycling-oriented society, packaging materials with high recyclability are in demand. However, conventional packaging materials are composed of laminates of layers made of different resin materials, and it is difficult to separate the resin materials after use, so it is difficult to recycle each material separately. Therefore, even if packaging bodies such as packaging bags made using conventional packaging materials are recovered, there is no other way than to burn them and recover and reuse them as heat, which is incompatible with the recent standpoint of global environmental protection.
[0003] Therefore, from the viewpoint of recyclability, it is desirable for the packaging material to be composed of a laminate having layers made of the same type of resin material. For example, a laminate having a base material, an adhesive layer, and a heat seal layer, in which the base material and the heat seal layer are made of polyethylene, is known as such a laminate (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-55157 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, although the laminate described in Patent Document 1 has high recyclability, there is room for improvement in terms of gas barrier properties after impact due to being dropped or the like.
[0006] The present disclosure has been made in consideration of the above-mentioned problems, and aims to provide a laminate, a packaging bag, and a packaging article that have high recyclability and can suppress deterioration of gas barrier properties even after impact. [Means for solving the problem]
[0007] One aspect of the present disclosure provides a laminate comprising a base film including a base layer, an adhesive layer, and a sealant layer, wherein the base layer is a first polyethylene film having a tensile modulus of elasticity greater than 500 MPa, the sealant layer is a second polyethylene film having a tensile modulus of elasticity less than 500 MPa, and the adhesive layer is a layer formed by applying a gas barrier adhesive to a surface of the base film. The laminate has high recyclability and is capable of suppressing deterioration of the gas barrier properties even after impact.
[0008] Although the reason why the laminate provides the above-mentioned effects is unclear, the inventors of the present disclosure speculate that it may be as follows. That is, adhesives are generally bonded by mechanical bonding (anchor effect), chemical interaction or physical interaction (intermolecular force), but when a gas barrier adhesive is applied to the surface of a base film to form an adhesive layer, the adhesive layer is considered to act more strongly on the surface of the base film, which is the coated side of the gas barrier adhesive, than on the sealant layer, which is not the coated side of the adhesive, due to the mechanical bonding and physical interaction, which are considered to be the main factors of adhesion. This is because the gas barrier adhesive has high fluidity when applied to the surface of the base film, and follows the unevenness of the surface of the base film. As a result, the surface area of contact between the adhesive layer and the surface of the base film is increased, and the adhesive layer is considered to be strongly fixed to the surface of the base film. Therefore, even if the laminate is impacted and a strain is applied to the base layer of the base film, the strain applied to the base layer is small because the base layer has a tensile modulus higher than 500 MPa, and the strain of the base film having the base layer is also small, and the strain applied to the adhesive layer, which is strongly fixed to the surface of the base film, is also small. In addition, even if an excessive stress is applied to the adhesive layer due to an impact, the stress is mitigated by the sealant layer having a low tensile modulus. Therefore, cracks are less likely to form in the adhesive layer. As a result, deterioration of the gas barrier properties of the adhesive layer is suppressed, and deterioration of the gas barrier properties of the laminate is also suppressed. In addition, since the base layer is a first polyethylene film and the sealant layer is a second polyethylene film, the laminate can have high recyclability. From the above, the inventors of the present disclosure speculate that the above-mentioned effects can be obtained by the laminate of the present disclosure.
[0009] In the above laminate, it is preferable that a ratio R1 of the tensile modulus of the base layer to the tensile modulus of the sealant layer is 2 or more. In this case, the deterioration of the gas barrier property of the laminate can be more sufficiently suppressed even after impact.
[0010] In the above laminate, the crystallinity of the base layer is preferably greater than 35%. In this case, the impact resistance of the laminate can be improved more effectively than when the crystallinity of the base material layer is 35% or less.
[0011] The laminate has an oxygen permeability of 200 cc / m at 30°C and 70 RH%. 2 It is preferable that the temperature be less than 100°C / day atm. In this case, the oxygen permeability at 30℃ and 70RH% is 200cc / m 2 When a packaging bag is made using the laminate and contents are placed in the packaging bag to produce a packaged article, deterioration of the contents due to oxygen can be effectively suppressed, compared to when the storage temperature exceeds 100°C / day·atm.
[0012] In the above laminate, the ratio of the thickness of the base layer to the thickness of the sealant layer is preferably 0.1 to 1.0. When the ratio of the thickness of the base layer to the thickness of the sealant layer is 0.1 or more, the ratio of the base layer having a high tensile modulus and high rigidity is relatively high, so that the rigidity of the laminate can be further improved.When the ratio of the thickness of the base layer to the thickness of the sealant layer is 1.0 or less, the ratio of the sealant layer having a low tensile modulus and high flexibility is relatively high, so that the impact absorption of the laminate can be further improved.
[0013] In the laminate, it is preferable that the base film further includes a gas barrier layer between the base layer and the adhesive layer. In this case, the gas barrier property of the laminate is further improved, so that when the laminate is used to prepare a packaging bag and contents are placed in the packaging bag to prepare a packaged article, deterioration of the contents due to gases such as oxygen can be effectively suppressed.
[0014] The content of the polyethylene resin in the entire laminate is preferably 90% by mass or more. In this case, the laminate can have higher recyclability.
[0015] The laminate may be used for a standing pouch, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag or a gusseted bag.
[0016] Another aspect of the present disclosure provides a packaging bag obtained by using the above-mentioned laminate. This packaging bag has high recyclability and can suppress deterioration of the gas barrier properties even after impact.
[0017] Furthermore, still another aspect of the present disclosure provides a packaging article including the above-mentioned packaging bag and contents accommodated in the packaging bag. According to this packaged article, deterioration of the gas barrier property can be suppressed even after impact. Therefore, deterioration of the contents due to gases such as oxygen can be suppressed for a long period of time. In addition, the packaging bag remaining after the contents are discharged can be highly recyclable. Effect of the Invention
[0018] According to the present disclosure, there are provided a laminate, a packaging bag, and a packaging article that have high recyclability and are capable of suppressing deterioration of gas barrier properties even after impact. [Brief description of the drawings]
[0019] [Figure 1] 1 is a cross-sectional view showing one embodiment of a laminate according to the present disclosure. [Diagram 2] FIG. 1 is a cross-sectional view of one embodiment of a packaging article according to the present disclosure. [Diagram 3] FIG. 4 is a cross-sectional view showing another embodiment of a laminate according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, preferred embodiments of the present disclosure will be described in detail. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0021] <Laminate> First, one embodiment of a laminate according to the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing one embodiment of a laminate according to the present disclosure.
[0022] 1, the laminate 100 includes, in this order, a base film 60 including a base layer 10, an adhesive layer 20, and a sealant layer 30. The base layer 10 is a first polyethylene film having a tensile modulus of elasticity greater than 500 MPa, the sealant layer 30 is a second polyethylene film having a tensile modulus of elasticity less than 500 MPa, and the adhesive layer 20 is a layer formed by applying a gas barrier adhesive to the surface of the base film 60.
[0023] The laminate 100 has high recyclability and can suppress deterioration of the gas barrier properties even after impact.
[0024] The base film 60, the adhesive layer 20, the sealant layer 30 and the laminate 100 will be described in detail below.
[0025] (Base film) The base film 60 includes a base layer 10. In FIG.
[0026] The first polyethylene film as the base layer 10 has a tensile modulus of elasticity greater than 500 MPa. The tensile modulus of elasticity of the first polyethylene film is preferably 600 MPa or more, more preferably 700 MPa or more, and particularly preferably 800 MPa or more. When the tensile modulus of elasticity of the first polyethylene film is 600 MPa or more, the gas barrier property of the laminate 100 can be further improved. The tensile modulus of the first polyethylene film is preferably 3000 MPa or less, more preferably 2500 MPa or less, and particularly preferably 1500 MPa or less. When the tensile modulus of the first polyethylene film is 3000 MPa or less, the gas barrier property of the laminate 100 can be further improved.
[0027] The ratio R1 of the tensile modulus of elasticity of the base layer 10 to the tensile modulus of elasticity of the sealant layer 30 is not particularly limited as long as it is greater than 1, but R1 is preferably 2 or more, and more preferably 3 or more. When R1 is 2 or more, the deterioration of the gas barrier property even after impact can be more sufficiently suppressed.
[0028] R1 is preferably 15 or less, and more preferably 10 or less. When R1 is 15 or less, the deterioration of the gas barrier property even after impact can be more sufficiently suppressed.
[0029] The crystallinity of the base layer 10 is not particularly limited, but is preferably greater than 35%, more preferably 40% or more, and particularly preferably 50% or more. When the crystallinity of the base layer 10 is greater than 35%, the base layer 10 has higher rigidity and the strain associated with the plastic deformation of the base layer 10 is smaller than when the crystallinity of the base layer 10 is 35% or less. As a result, the deformation of the base layer 10 due to the strain generated by the momentary impact applied to the laminate 100 is suppressed, and the base layer 10 is less likely to crack. The crystallinity of the base layer 10 may be 100% or less. The crystallinity of the base layer 10 is preferably 90% or less, and more preferably 80% or less. When the crystallinity of the base layer 10 is 90% or less, the base layer 10 has better flexibility and higher shock absorption than when the crystallinity of the base layer 10 is more than 90%. This allows the laminate 100 to have better impact resistance. When the base layer 10 is a laminate of a plurality of layers, the crystallinity of the base layer 10 is the crystallinity of the outermost layer.
[0030] The crystallinity of the base layer 10 is determined by an X-ray diffraction method using a parallel beam method. Specifically, the crystallinity is determined as follows. First, the X-ray diffraction pattern of the base layer 10 is obtained by out-of-plane measurement using a wide-angle X-ray diffractometer manufactured by Rigaku Corporation, scanning the diffraction angle range of 10° to 30° with 2θ / θ. The characteristic X-ray CuKα is used as the X-ray, which is collimated by a multilayer mirror and made incident on the surface of the base layer, and the diffracted X-ray is detected by a scintillation detector equipped with a flat collimator. From the obtained X-ray diffraction pattern, the peak area of the crystalline component and the halo pattern area of the amorphous component are determined, and the ratio of the peak area of the crystalline component to the sum of these areas (100%) is calculated as the crystallinity (%) of the base layer 10.
[0031] The crystallinity of the substrate layer 10 can be adjusted by controlling the degree of elongation of the resin film used for the substrate layer 10, or the thermal history during or after the production of the resin film. For example, if the resin film that will become the substrate layer 10 after film formation is slowly cooled, the crystallinity of the substrate layer 10 increases, and if it is rapidly cooled, the crystallinity of the substrate layer 10 decreases. It is also possible to improve the crystallinity of the substrate layer 10 by adding an additive such as a crystal nucleating agent.
[0032] The first polyethylene film contains a polyethylene-based resin. The polyethylene-based resin is a resin containing ethylene as a constituent unit. Examples of the polyethylene-based resin include ethylene homopolymers and copolymers of ethylene and other monomers. The proportion of ethylene in the polyethylene is, for example, 80 mol % or more.
[0033] Examples of other monomers include α-olefins, vinyl acetate, acrylic esters, and the like. The α-olefin may be an olefin having a carbon number in the range of 3 to 20. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Examples of polyethylene resins include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, etc. These may be used alone or in combination of two or more. Here, high density polyethylene has a density of 0.942 g / cm 3 Medium density polyethylene has a density of 0.930 g / cm or more. 3 More than 0.942g / cm 3 Low density polyethylene is polyethylene with a density of less than 0.910 g / cm 3 More than 0.930g / cm 3 Linear low density polyethylene has a density of less than 0.910 g / cm 3 More than 0.930cm 3 Ultra-low density polyethylene has a density of less than 0.910 g / cm 3 It is polyethylene having a molecular weight of less than 1.001. The density is a value obtained by a method in accordance with JIS K7112:1999.
[0034] The polyethylene resin may be a polyethylene resin obtained using a raw material (monomer) obtained from a fossil fuel, or a polyethylene resin obtained using a raw material (monomer) derived from biomass, but from the viewpoint of reducing the environmental load, it is preferable that the polyethylene resin is a polyethylene resin obtained using a raw material derived from biomass. Alternatively, the polyethylene resin may be a recycled resin. The recycled resin may be a mechanically recycled resin or a chemically recycled resin.
[0035] The base layer 10 may contain at least one additive selected from a filler, an antistatic agent, a plasticizer, a lubricant, an antioxidant, and the like, as necessary.
[0036] The substrate layer 10 may be an unstretched film or a stretched film. The stretched film may be a uniaxially stretched film or a biaxially stretched film. The substrate layer 10 may be composed of either a stretched film or an unstretched film. The substrate layer 10 may also be a laminate of at least one stretched film and at least one unstretched film. The substrate layer 10 can improve mechanical strength and dimensional stability by having a biaxially stretched film.
[0037] In order to enhance adhesion to the adhesive layer 20, the surface of the base material layer 10 facing the adhesive layer 20 may be subjected to various pretreatments such as corona treatment, plasma treatment, ozone treatment, and frame treatment, or a coating layer such as an easy-adhesion layer may be provided.
[0038] The ratio R2 of the thickness of the base layer 10 to the thickness of the sealant layer 30 is not particularly limited, but R2 is preferably 0.1 or more, more preferably 0.15 or more, and particularly preferably 0.20 or more. When R2 is 0.1 or more, the proportion of the base material layer 10 having a high tensile elastic modulus and high rigidity is relatively high, so that the rigidity of the laminate 100 can be further improved.
[0039] R2 is preferably 1.0 or less, more preferably 0.7 or less, even more preferably 0.4 or less, and particularly preferably 0.3 or less. When R2 is 1.0 or less, the proportion of the sealant layer 30 having a low tensile modulus and high flexibility is relatively high, so that the impact absorption of the laminate 100 can be further improved.
[0040] The thickness of the substrate layer 10 is not particularly limited, and is, for example, 10 μm or more and 200 μm or less. From the viewpoint of reducing materials to reduce environmental load, and from the viewpoint of obtaining excellent heat resistance, impact resistance, and gas barrier properties, the thickness of the substrate layer 10 may be 20 μm or more, 25 μm or more, 30 μm or more, or 40 μm or more. The thickness of the substrate layer 10 may be 100 μm or less, 60 μm or less, or 50 μm or less. The ratio of the thickness of the substrate layer 10 to the thickness of the laminate 100 is, for example, 5% or more.
[0041] (adhesive layer) The adhesive layer 20 is a layer that bonds the base film 60 and the sealant layer 30, and is a layer formed by applying a gas barrier adhesive to the surface of the base film 60. By having the adhesive layer 20 in the laminate 100, the adhesion between the base layer 10 and the sealant layer 30 can be further improved, and peeling between the base layer 10 and the sealant layer 30 can be suppressed.
[0042] A gas barrier adhesive is one that has an oxygen permeability of 150 cc / m2 or more for the adhesive layer 20 obtained after curing. 2 This adhesive can be used at 100-day atm or less.
[0043] From the viewpoint of more sufficiently improving the gas barrier properties of the laminate 100, the gas barrier adhesive has an oxygen permeability of the adhesive layer 20 of 100 cc / m 2 It is preferable that the adhesive should be less than 80cc / m 2 It is more preferable that the adhesive has a viscosity of 50cc / m or less. 2 Specific examples of such gas barrier adhesives include "Maxive" manufactured by Mitsubishi Gas Chemical Company, Inc. and "Paslim" manufactured by DIC Corporation.
[0044] The adhesive layer 20 may or may not contain a biomass component, but preferably contains a biomass component from the viewpoint of reducing the environmental load. Specific examples of the biomass component include the "DIC Dry BM Series" manufactured by DIC Corporation and the "ECOAD Series" manufactured by Toyo Ink Co., Ltd. The biomass component may be included as a component of the gas barrier adhesive, or may be included as a component other than the gas barrier adhesive.
[0045] The gas barrier adhesive may be an adhesive containing an organic solvent or an adhesive containing no organic solvent, but from the viewpoint of reducing the environmental burden, it is preferably an adhesive containing no organic solvent (solvent-free adhesive).
[0046] The thickness of the adhesive layer 20 is not particularly limited and may be, for example, 1 μm or more. By setting the thickness of the adhesive layer 20 to 2 μm or more, sufficient adhesive strength can be obtained. The thickness of the adhesive layer 20 may be 2 μm or more. The thickness of the adhesive layer 20 may be 50 μm or less, 5 μm or less, or 3 μm or less.
[0047] (Sealant layer) The sealant layer 30 is a second polyethylene film having a tensile modulus of elasticity of less than 500 MPa. The second polyethylene film contains a polyethylene-based resin. As the polyethylene-based resin, the same polyethylene-based resin as that used in the base layer 10 can be used. As the polyethylene-based resin, linear low-density polyethylene is preferable.
[0048] The tensile modulus of the sealant layer 30 may be less than 500 MPa, but from the viewpoint of further improving the impact resistance of the laminate 100, it is preferably 400 MPa or less, and more preferably 300 MPa or less.
[0049] The tensile modulus of the sealant layer 30 may be 50 MPa or more, or may be 100 MPa or more. If the tensile modulus of the sealant layer 30 is 150 MPa or more, and if the tensile modulus of the sealant layer 30 is less than 150 MPa, the film forming suitability and handling in film processing are poor, resulting in low productivity.
[0050] The crystallinity of the sealant layer 30 is not particularly limited, but may be 20% or less, 15% or less, or 13% or less. When the crystallinity of the sealant layer 30 is 20% or less, the sealant layer 30 has better flexibility and higher impact absorption than when the crystallinity of the sealant layer 30 is greater than 20%. This allows the laminate 100 to have better impact resistance. When the sealant layer 30 is a laminate of a plurality of layers, the crystallinity of the sealant layer 30 is the crystallinity of the outermost layer. The crystallinity of the sealant layer 30 is determined in the same manner as the crystallinity of the base layer 10 . The crystallinity of the sealant layer 30 can be adjusted in the same manner as the crystallinity of the base layer 10 .
[0051] The sealant layer 30 preferably has a melting point lower than that of the base layer 10. In this case, when the laminate 100 is heat-sealed, it is possible to heat-seal the sealant layer 30 while suppressing melting of the base layer 10. In addition, by heating the laminate 100, the base layer 10 and the sealant layer 30 can be easily separated, and material recycling can be easily performed for each of the base layer 10 and the sealant layer 30.
[0052] The sealant layer 30 may contain various additives, such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, and an antistatic agent, as necessary.
[0053] The thickness of the sealant layer 30 is not particularly limited and is appropriately adjusted depending on the application of the laminate 100. The thickness of the sealant layer 30 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the sealant layer 30 may be 200 μm or less, 180 μm or less, 160 μm or less, 150 μm or less, 120 μm or less, or 100 μm or less.
[0054] (Laminate) The oxygen permeability of the laminate 100 at 30° C. and 70% RH is not particularly limited, but is preferably 200 cc / m 2 It is preferable that the temperature be less than 100°C / day atm. In this case, the oxygen permeability at 30℃ and 70RH% is 200cc / m 2 Compared to the case where the storage temperature exceeds 100°C / day·atm, when a packaging bag is made using the laminate 100 and contents are placed in the packaging bag to produce a packaged article, deterioration of the contents due to oxygen can be effectively suppressed.
[0055] The oxygen permeability of the laminate 100 at 30° C. and 70% RH is more preferably 100 cc / m 2 ·day·atm or less, and particularly preferably 50cc / m 2 ·day·atm or less.
[0056] In the laminate 100, both the base layer 10 and the sealant layer 30 contain a polyethylene-based resin. In this case, the proportion of the polyethylene-based resin in the entire laminate 100 is not particularly limited, but is preferably 90% by mass or more. By making the proportion of the polyethylene-based resin in the entire laminate 100 90% by mass or more, it becomes possible for the laminate 100 to have higher recyclability. The proportion of the polyethylene resin in the entire laminate 100 is more preferably 75% by mass or more, and particularly preferably 90% by mass.
[0057] <Packaged goods> Next, an embodiment of the packaging article of the present disclosure will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing one embodiment of the packaging article of the present disclosure.
[0058] As shown in FIG. 2, the packaged article 500 includes a packaging bag 400 and a content C contained in the packaging bag 400. The packaging bag 400 is obtained by using a pair of laminates 100. The packaging bag 400 is obtained, for example, by placing the sealant layers 30 of a pair of laminates 100 facing each other and bonding the peripheral portions. The packaging bag 400 is composed of a storage section that stores the content C and an adhesive section provided around the storage section. The adhesive section is a portion formed by bonding the sealant layers 30 of opposing laminates 100 to each other, and the storage section is a portion where the sealant layers 30 of opposing laminates 100 are not bonded to each other.
[0059] According to the packaged article 500, deterioration of the gas barrier property can be suppressed even after impact. Therefore, deterioration of the contents C due to gas such as oxygen is suppressed for a long period of time. In addition, the packaging bag 400 remaining after the contents C are discharged can have high recyclability.
[0060] (Contents) The contents C are not particularly limited and may be appropriately selected depending on the application of the packaging bag 400. The contents C are not particularly limited, and examples of the contents C include food, shampoo, rinse, body soap, detergent, and the like.
[0061] (packaging bag) The pair of laminates 100 constituting the packaging bag 400 may have the same configuration as each other, or may have different configurations from each other.
[0062] The packaging bag 400 may have a half-cut line, and may further have an easy-open processed part at both ends or one end of the half-cut line. Examples of the easy-open processed part include a group of scars, and a V-shaped, U-shaped, or I-shaped notch.
[0063] In the adhesive portion of the packaging bag 400, the sealant layers 30 of the pair of laminates 100 may be directly bonded to each other by heat sealing (see FIG. 2), or may be bonded to each other by an adhesive.
[0064] (Method of manufacturing packaging articles) Next, a method for producing a packaged article 500 using the laminate 100 will be described.
[0065] First, a pair of laminates 100 is prepared. Then, the sealant layers 30 of the pair of laminates 100 are placed opposite each other, and the sealant layers 30 are bonded together. At this time, a part of the peripheral portion of the laminate is bonded to form a U-shape to form a bonded portion, and a non-bonded portion (unbonded portion) is also formed. In this manner, a packaging bag having an opening formed by the unbonded portion is obtained.
[0066] Next, the contents C are filled in through the opening of the packaging bag. Thereafter, the sealant layers 30 of the laminate 100 are bonded together at the unbonded portions, so that the unbonded portions also become bonded portions. In this manner, a packaged article 500 including the packaging bag 400 and the contents C contained therein can be manufactured.
[0067] Although the preferred embodiment of the present disclosure has been described above, the present disclosure is not limited to the above embodiment. For example, in the laminate of the present disclosure, as in the laminate 200 shown in FIG. 3, the base film 60 may further include a gas barrier layer 50 between the base layer 10 and the adhesive layer 20. When the base film 60 further includes the gas barrier layer 50, the gas barrier property of the laminate 200 is further improved. The gas barrier layer 50 has a barrier property against gases such as water vapor or oxygen.
[0068] The gas barrier layer 50 contains an inorganic compound. The inorganic compound contains at least one of a metal and an inorganic oxide. Metals include aluminum, silicon, etc. Inorganic oxides include aluminum oxide and silica, etc. The gas barrier layer 50 can be produced by a vacuum deposition method or the like.
[0069] 3, the base film 60 may further include a printed layer between the base layer 10 and the gas barrier layer 50. The printed layer may be free of chlorine in order to prevent discoloration and odor generation when the printed layer is remelted. The printed layer may be made of a biomass material in consideration of the environment.
[0070] The printing layer is a layer formed by using ink made of, for example, a urethane-based, acrylic-based, nitrocellulose-based, or rubber-based binder resin to which various pigments, plasticizers, drying agents, stabilizers, etc. are added. This printing layer can display characters, pictures, etc.
[0071] The ink may be either water-based or oil-based, but is preferably water-based. Water-based inks use water or alcohol as a solvent, and therefore can further reduce the environmental impact. In particular, when the adhesive is a solventless adhesive, the use of water-based ink as the ink can significantly reduce the environmental impact. In addition, the ink may be biomass ink or not, but from the viewpoint of reducing the environmental impact, it is preferable that the ink is biomass ink. Here, biomass ink refers to ink containing components obtained from biological resources (biomass) such as cotton, pulp, rice bran, vegetable oil, and angiosperm seeds.
[0072] The base material layer 10 and the gas barrier layer 50 may be bonded to each other via an adhesive layer 40 as shown in FIG. 3, but the base material layer 10 and the gas barrier layer 50 may also be bonded directly to each other.
[0073] 2, the packaging bag 400 is formed using a pair of laminates 100, but the laminate 200 may be used instead of the laminate 100. The packaging bag may be produced by folding one of the laminates 100, 200 with the sealant layer 30 on the inside and bonding the overlapping peripheral portions together.
[0074] 2, the shape of the packaging bag 400 may be a standing pouch-shaped packaging bag, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag, or a gusset bag. The packaging bag 400 may be provided with a spout or a synthetic resin fastener that can be repeatedly sealed by fitting a strip-shaped protrusion and a strip-shaped groove.
[0075] The embodiments of the present disclosure have been described above, and the outline of the present disclosure is as follows. [1] A laminate comprising a base film including a base layer, an adhesive layer, and a sealant layer, wherein the base layer is a first polyethylene film having a tensile modulus of elasticity greater than 500 MPa, the sealant layer is a second polyethylene film having a tensile modulus of elasticity less than 500 MPa, and the adhesive layer is a layer formed by applying a gas barrier adhesive to the surface of the base film. [2] The laminate according to [1], wherein a ratio R1 of the tensile modulus of the base layer to the tensile modulus of the sealant layer is 2 or more. [3] The laminate according to [1] or [2], wherein the crystallinity of the base layer is greater than 35%. [4] Oxygen permeability at 30℃ and 70% RH is 200cc / m 2 The laminate according to any one of [1] to [3], wherein the maximum permeability is 1.0·day·atm or less. [5] The laminate according to any one of [1] to [4], wherein the ratio of the thickness of the base layer to the thickness of the sealant layer is 0.1 to 1.0. [6] The laminate according to any one of [1] to [5], wherein the base film further comprises a gas barrier layer between the base layer and the adhesive layer. [7] The laminate according to any one of [1] to [6], wherein the content of the polyethylene resin in the entire laminate is 90 mass % or more. [8] The laminate according to any one of [1] to [7], which is used for a standing pouch, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag, or a gusseted bag. [9] A packaging bag obtained by using the laminate according to any one of [1] to [8].
[10] A packaging article comprising the packaging bag described in [9] and contents contained in the packaging bag. EXAMPLES
[0076] The present disclosure will be described more specifically with reference to the following examples, but the present disclosure is not limited to these examples.
[0077] Example 1 First, the base layer had a thickness of 30 μm, a tensile modulus of 900 MPa, a crystallinity of 23.2%, and a density of 0.947 g / cm 3 A first polyethylene film made of high density polyethylene was prepared. Next, a silicon oxide (SiOx) vapor deposition film having a thickness of 30 nm was formed as an inorganic compound layer on one surface of the base layer by using a vacuum deposition apparatus using an electron beam heating method, thus obtaining a base film. Next, a gas barrier adhesive was applied onto the surface of the inorganic compound layer of the base film and dried to form an adhesive layer having a thickness of 2 μm. At this time, the gas barrier adhesive was prepared by mixing 23 parts by mass of a solvent in which ethyl acetate and methanol were mixed at a mass ratio of 1:1 with 16 parts by mass of "Maxive C93T" manufactured by Mitsubishi Gas Chemical Co., Ltd. and 5 parts by mass of "Maxive M-100" manufactured by Mitsubishi Gas Chemical Co., Ltd. Then, a second polyethylene film having a thickness of 100 μm and made of linear low-density polyethylene having a tensile modulus of 250 MPa was bonded to the base layer as a sealant layer via this adhesive layer. In this way, a laminate was produced.
[0078] Example 2 The base layer has a thickness of 25 μm, a tensile modulus of 2000 MPa, a crystallinity of 71.8%, and a density of 0.96 g / cm 3 A laminate was produced in the same manner as in Example 1, except that the first polyethylene film made of high density polyethylene was used.
[0079] Comparative Example 1 The sealant layer has a thickness of 30 μm, a tensile modulus of 900 MPa, a crystallinity of 23.2%, and a density of 0.947 g / cm 3 A laminate was produced in the same manner as in Example 1, except that the second polyethylene film made of high density polyethylene was used.
[0080] Comparative Example 2 A laminate was produced in the same manner as in Example 1, except that a first polyethylene film made of linear low-density polyethylene having a thickness of 100 μm and a tensile modulus of elasticity of 250 MPa was used as the base layer.
[0081] <Tensile modulus> The tensile modulus of elasticity of the first polyethylene film and the second polyethylene film (hereinafter also referred to as "polyethylene film") was determined as follows. That is, first, a rectangular piece having a total length of 200 mm and a width of 15 mm was cut out from a polyethylene film to prepare a test piece. Three test pieces were prepared as described above, and the tensile modulus of each test piece was determined as follows. That is, both ends of the test piece were attached to the fixed and movable grips of a tensile testing machine (a test device conforming to JIS K7127) so that the distance between the grips was 150 mm, and the movable grip was moved at a tensile speed of 50 mm / min. The ratio of the tensile stress within the tensile proportional limit to the corresponding strain was calculated as the tensile modulus. The arithmetic mean value of the tensile modulus calculated for the three test pieces was determined as the tensile modulus of the polyethylene film. The results are shown in Table 1. The ratio R1 (=A / B) of the tensile modulus A of the first polyethylene film to the tensile modulus B of the second polyethylene film was also determined. The results are shown in Table 1.
[0082] <Gas barrier properties of laminate after impact> (1) Preparation of packaging items From the laminates of the examples and comparative examples, rectangular sheets measuring 400 mm x 300 mm were cut out, folded in half, and the overlapping edges were heat-sealed to prepare packaging bags. At this time, the packaging bags were formed with openings for inserting contents. The dimensions of the packaging bags were 200 mm x 300 mm. Next, 1200 mL of tap water was filled into each packaging bag through the opening, and the opening was then sealed. In this manner, packaging articles were prepared. (2) Drop bag test The drop bag test was carried out by storing the packaged article obtained as described above in an environment at 5° C. for one day, and then dropping it from a height of 1 m ten times. (3) Oxygen permeability After the bag drop test, test pieces measuring 100 mm x 100 mm were taken from each package. The oxygen permeability (unit: cc / m) of these test pieces was measured using an oxygen permeability measuring device (product name "OX-TRAN2 / 20", manufactured by MOCON) at a temperature of 30°C and a relative humidity (RH) of 70%. 2 ·day·atm) was measured. The oxygen permeability was measured in accordance with JIS K-7126-2. The arithmetic mean value of the oxygen permeability of these test pieces was calculated as the oxygen permeability of the laminate after the impact. The results are shown in Table 1.
[0083] [Table 1]
[0084] From the results shown in Table 1, the laminates of Examples 1 and 2 had sufficiently low oxygen transmission rates after the drop bag test, compared to the laminates of Comparative Examples 1 and 2. From the above, it was confirmed that the laminate of the present disclosure can suppress deterioration of the gas barrier property even after impact. [Explanation of symbols]
[0085] Reference Signs List 10...base material layer, 20...adhesive layer, 30...sealant layer, 50...gas barrier layer, 60...base material film, 100, 200...laminate, 400...packaging bag, 500...packaged article, C...contents.
Claims
1. The film has a base material layer, an adhesive layer, and a sealant layer, the substrate layer is a first polyethylene film having a tensile modulus greater than 500 MPa; the sealant layer is a second polyethylene film having a tensile modulus of less than 500 MPa; The adhesive layer is a layer formed by applying a gas barrier adhesive to the surface of the base film.
2. The laminate according to claim 1 , wherein a ratio R1 of the tensile modulus of the base layer to the tensile modulus of the sealant layer is 2 or more.
3. The laminate of claim 1 , wherein the substrate layer has a crystallinity of greater than 35%.
4. Oxygen permeability at 30°C and 70% RH is 200cc / m 2 2. The laminate according to claim 1, wherein the thermal expansion coefficient is 0.05-0.55×day·atm or less.
5. 2. The laminate according to claim 1, wherein the ratio of the thickness of the base layer to the thickness of the sealant layer is 0.1 to 1.
0.
6. The laminate according to claim 1 , wherein the base film further comprises a gas barrier layer between the base layer and the adhesive layer.
7. The laminate according to claim 1 , wherein the content of the polyethylene resin in the entire laminate is 90 mass % or more.
8. The laminate according to claim 1, which is used for a standing pouch, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag or a gusseted bag.
9. A packaging bag obtained by using the laminate according to any one of claims 1 to 8.
10. The packaging bag according to claim 9 , and contents contained within the packaging bag.
Citation Information
Patent Citations
Laminate, packaging material, packaging bag and stand pouch
JP2020055157A