Welding wire and method for manufacturing the same
A welding wire with controlled alloying elements and manufacturing process addresses slag formation issues, ensuring a slag-free surface with improved plating and corrosion resistance.
Patent Information
- Application Number
- JP2024061221
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-04-05
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing welding methods using gas-shielded arc welding with mixed argon and carbon dioxide shielding gases result in slag formation due to silicon oxide, affecting weld bead quality, corrosion resistance, and plating properties, which is difficult to control with reduced silicon content.
A welding wire composition with specific alloying elements (manganese, chromium, and titanium) is designed to modify slag formation, ensuring a silicon content of 0.01-0.25 wt.% and a ratio of (manganese content/2 + titanium content + chromium content/1.33)/silicon content > 5, combined with a manufacturing process involving heating, hot rolling, annealing, and cold drawing to produce a slag-free surface.
The solution achieves a slag-free weld bead surface with improved plating properties, enhanced corrosion resistance, and stable mechanical properties, preventing unplated spots and silicon oxide adhesion.
Smart Images

Figure 2024163017000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a welding wire and a manufacturing method thereof, and more particularly to a welding wire component having excellent weld bead plating properties and a manufacturing method thereof. [Background technology]
[0002] Gas-shielded arc welding is a welding method in which the arc is shielded with an inert gas. Compared to other welding methods, gas-shielded arc welding is the most commonly found welding process in industry due to its high welding speed and ease of application to automated processes.
[0003] However, the choice of inert gas affects the arc configuration and changes the shape of the metal droplets during welding.
[0004] When 100% carbon dioxide is used as a shielding gas, the carbon dioxide is in the ultra-high temperature environment of the arc, which causes the gas molecules to decompose. When the carbon dioxide decomposes, it absorbs thermal energy and has the effect of cooling the arc, so the arc is concentrated only on the welding wire in a small area, but the droplets form globular transfer, narrowing the molten area of the weld bead.
[0005] When 100% argon gas is used as a shielding gas, the arc becomes longer and the arc becomes unstable, prone to flowing and shaking, because argon gas is a monoatomic inert gas that does not participate in the reaction. Therefore, it is common in the industry to mix a small amount of carbon dioxide into argon gas to combine the advantages of both and achieve good weld bead quality.
[0006] However, carbon dioxide decomposes under the action of the arc, and the released oxygen also gets mixed into the weld bead. Silicon, a common alloying element in steel, reacts easily with oxygen. Therefore, during welding, silicon reacts preferentially with oxygen before iron and carbon to form slag, which is silicon oxide. If slag is formed during welding, removing the oxygen can prevent large amounts of iron and carbon in the weld bead from being oxidized.
[0007] The slag adheres to the surface of the weld bead, affecting the appearance of the weld bead. In addition, silicon-based slag is resistant to acids and alkalis and is non-conductive, making it difficult to clean the areas where the slag adheres during subsequent processing of the welded workpiece (e.g., pickling). During subsequent electroplating, unplated spots are formed in the silicon oxide-containing areas of the surface.
[0008] In addition, because of the large difference in thermal expansion coefficient and lattice between silicon oxide and steel, residual stress gradually accumulates between the silicon oxide and steel as the workpiece is used, causing the adhesion of the silicon oxide to decrease and even to fall off and become exposed on the steel surface. Corrosion usually occurs at the point where the silicon oxide falls off. Therefore, if slag remains on the surface of the welded workpiece, the corrosion resistance will deteriorate.
[0009] In order to reduce slag generation, the conventional techniques all adopt a similar method of reducing the silicon content. For example, the silicon content is reduced to 0.15% or less. By reducing the silicon content, the generation of silicon-containing slag can be reduced. However, since silicon is a deoxidizer commonly found in the smelting process of molten iron and is a slag-generating element, it is difficult to reduce the silicon content to 0.15% or less. In addition, in the conventional techniques, the alloy components of the welding wire are controlled to satisfy the conditional formulas Si×Mn≦0.3 and (Si+Mn / 5) / (Ti+Al)≦3. However, when the manganese content in the alloy is 2% or more, the silicon content needs to be reduced to 0.15% or less, which is also difficult to control in the steel smelting process.
[0010] The composition of the welding wire needs to be designed to improve the silicon composition range and prevent slag formation, and the hot rolled texture needs to be controlled because the welding wire undergoes multiple passes of stripping.
[0011] Therefore, in order to solve the problems existing in the prior art, it is necessary to provide a welding wire having excellent weld bead plating properties and a manufacturing method thereof. Summary of the Invention [Problem to be solved by the invention]
[0012] An object of the present invention is to provide a welding wire component having excellent weld bead plating properties and a manufacturing method thereof, which can increase the silicon content in the welding wire components by devising an alloy design, and which makes it easier to smelt steel.
[0013] Another object of the present invention is to provide a welding wire component having excellent weld bead plating properties and a manufacturing method thereof, which is obtained by designing the components of alloy elements such as manganese, chromium, and titanium, and further modifying the slag, thereby preventing the apparent presence of silicon-containing slag on the weld bead surface, and preventing the occurrence of unplated spots in the subsequent plating, which affects the quality of the product. [Means for solving the problem]
[0014] In order to achieve the above object, the present invention provides a method for producing welding wire, the method including the steps of: providing a billet having a total weight of 100 wt.%, the components of the billet including a carbon content of 0.02-0.10 wt.%, a manganese content of 2.00-3.00 wt.%, a silicon content of 0.01-0.25 wt.%, a chromium content of 0.10-0.5 wt.%, a titanium content of 0.10-0.3 wt.%, unavoidable impurities, and the balance being iron, the components of the billet satisfying a judgment formula of (manganese content / 2+titanium content+chromium content / 1.33) / silicon content>5; heating the billet; hot rolling the heated billet to form a wire rod; slowly cooling the wire rod formed by hot rolling; and cold drawing the slowly cooled wire rod to produce a welding wire.
[0015] In some embodiments of the present invention, the billet has a silicon content / manganese content ratio of 0.2-1.
[0016] In some embodiments of the present invention, in the heating step, the billet is heated to a temperature of 1000 to 1050°C.
[0017] In some embodiments of the present invention, in the hot rolling step, the rolling temperature is 820 to 1000°C, and the rolling end temperature is 800 to 850°C.
[0018] In some embodiments of the present invention, the slow cooling step has a cooling rate of 0.1 to 5° C. / sec.
[0019] In some embodiments of the present invention, the proportion of martensite in the welding wire is less than 5%.
[0020] The present invention further provides a welding wire having a total weight of 100 wt.%, a composition of the welding wire consisting of a carbon content of 0.02-0.10 wt.%, a manganese content of 2.00-3.00 wt.%, a silicon content of 0.01-0.25 wt.%, a chromium content of 0.10-0.5 wt.%, a titanium content of 0.10-0.3 wt.%, unavoidable impurities, and the balance being iron, and the composition of the welding wire satisfies a judgment formula of (manganese content / 2+titanium content+chromium content / 1.33) / silicon content>5.
[0021] In some embodiments of the present invention, the welding wire has a silicon content / manganese content ratio of 0.2-1.
[0022] In some embodiments of the present invention, the proportion of martensite in the welding wire is less than 5%.
[0023] In some embodiments of the present invention, the welding wire contains nano-order titanium carbide precipitates. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a flowchart showing a method for manufacturing a welding wire according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an Ellingham diagram of an oxide according to an embodiment of the present invention. [Diagram 3] FIG. 3 is an electron microscope image of the hot-rolled structure of an embodiment of the present invention. [Figure 4] FIG. 4 is an electron microscope photograph of the surface of a weld bead after welding in an embodiment of the present invention. [Diagram 5] FIG. 5 is an electron microscope image of the surface of a weld bead after welding in an embodiment of the present invention. [Figure 6] FIG. 6 is a diagram showing the distribution of the structure and inclusions within the weld bead of an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] In order to make the above contents of the present invention and other objects, features, and advantages of the present invention more clearly understandable, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. Furthermore, directional terms such as upper, lower, top, bottom, front, rear, left, right, inside, outside, side, periphery, center, horizontal, lateral, vertical, longitudinal, axial, radial, top layer, and bottom layer referred to in the present invention are merely directions referring to the accompanying drawings. Therefore, the directional terms used are intended to explain and understand the present invention, and are not intended to limit the present invention.
[0026] As described herein, reference to a numerical range for a variable is intended to indicate that the variable is equal to any value within that range. Thus, for a variable that is itself discrete, the variable is equal to any integer value within the numerical range, including the end points of the range. Similarly, for a variable that is itself continuous, the variable is equal to any real value within the numerical range, including the end points of the range. By way of example, and not of limitation, a variable described as having a value between 0 and 2 can take on values of 0, 1, or 2 if the variable itself is discrete, and can take on values of 0.0, 0.1, 0.01, 0.001, or any other real value between 0 and 2, inclusive, if the variable itself is continuous.
[0027] In order to facilitate understanding of the design principle of the present invention, the effect of each component of the welding wire of the present invention on welding will be described below.
[0028] Carbon (C): Carbon may affect the strength after welding. Generally, the higher the carbon content, the higher the hardness after welding. If the carbon content is less than 0.02%, the hardness after welding may be insufficient, and if the carbon content is too high, the ratio of hard and brittle structures after welding increases, so the hardness increases, but the toughness may be poor. The toughness after welding can be improved by heat treatment after welding, but the heat treatment increases costs, lengthens the processing time of the workpiece, and increases production costs. Therefore, in the present invention, the upper limit of the carbon content of the welding wire is set to about 0.15%.
[0029] Silicon (Si): Silicon is a common deoxidizer, and during welding, silicon reacts preferentially with oxygen before iron to form silicon oxide. Therefore, the conventional technology reduces the silicon content to prevent the generation of silicon-containing slag and improve corrosion resistance. On the other hand, adding silicon can increase the hardness of the weld bead through solid solution strengthening. As will be described later, the composition design of manganese, chromium, and titanium can improve the margin of alloy smelting after slag modification, so the present invention designs silicon to be 0.01-0.25 wt.%.
[0030] Manganese (Mn): During welding, manganese captures sulfur and forms manganese sulfide (MnS), preventing the formation of iron sulfide (FeS). Because the melting point of iron sulfide is low, the cold-heat change during welding is large, which generates thermal stress due to contraction and expansion. If a low-melting point liquid phase such as iron sulfide exists in the structure, high-temperature cracks will occur during welding. Manganese can delay the ferrite phase transformation, so it can adjust the weld bead structure and increase the strength after welding. Manganese also has the effect of deoxidization. Furthermore, referring to the Ellingham diagram in Figure 2, it can be seen that the deoxidization ability of manganese is only slightly inferior to that of silicon. When manganese oxide is generated, the conductivity of manganese oxide falls into the category of conductor, so manganese oxide does not affect the subsequent electroplating process and no unplated spots will be formed. However, if the manganese content is too high, martensite will be generated in the structure after welding, and the hardness of the weld bead will be too high, the toughness will decrease, and low-temperature cracks will be easily generated. Therefore, the manganese content in the present invention is designed to be 2.00 to 3.00 wt.%.
[0031] Chromium (Cr): Chromium can delay the ferrite phase transformation, so it can adjust the weld bead structure and increase the strength after welding. Chromium also has a deoxidizing effect. However, chromium oxide has a somewhat low electrical conductivity, so it is only used as an auxiliary. Therefore, the chromium of the present invention is designed to be 0.10 to 0.5 wt.%.
[0032] Titanium (Ti): Titanium has a strong deoxidizing effect. In addition, the oxides generated by titanium in the weld bead promote the generation of acicular ferrite groups, which helps to improve the mechanical strength and toughness of the weld bead. However, if the titanium content is too high, titanium will combine with carbon after hot rolling to generate nano-order titanium carbide (TiC) precipitates, which significantly improves the strength of the steel material. When manufacturing welding wire, it is necessary to go through a wire drawing process that involves large deformation, so high-strength welding wire makes cold wire drawing difficult, causing wear of the mold and further causing wire drawing cracks. Therefore, the amount of titanium added in the present invention is designed to be 0.10 to 0.3 wt.%.
[0033] Based on the above design principle, the present invention proposes a method for manufacturing a welding wire, including the steps of: providing a billet having a total weight of 100 wt.%, the components of the billet including a carbon content of 0.02-0.10 wt.%, a manganese content of 2.00-3.00 wt.%, a silicon content of 0.01-0.25 wt.%, a chromium content of 0.10-0.5 wt.%, a titanium content of 0.10-0.3 wt.%, unavoidable impurities, and the balance being iron, and the components of the billet satisfy a judgment formula of (manganese content / 2+titanium content+chromium content / 1.33) / silicon content>5; heating the billet; hot rolling the heated billet to form a wire rod; slowly cooling the wire rod formed by hot rolling; and cold drawing the slowly cooled wire rod to manufacture a welding wire.
[0034] By designing the composition of manganese, chromium, and titanium, the slag can be modified. This allows a uniform iron oxide thin film to be formed on the weld bead surface after welding, and prevents the formation of silicon-based slag on the surface, improving plating properties. The modified composition increases the silicon margin in the welding wire composition, making it easier to smelt steel.
[0035] The welding wire according to one embodiment of the present invention is manufactured using two steps: (1) hot rolling a billet into a wire disk-shaped member; and (2) cold drawing the wire into a welding wire. When hot rolling, the billet (e.g., a small billet) needs to be reheated at a temperature of 1000 to 1050°C (e.g., about 1030°C) through a heating process. If the reheating temperature is too high, titanium carbide will be dissolved. Titanium combines with carbon after hot rolling to generate nano-order titanium carbide precipitates, which greatly improves the strength of the steel material, makes cold drawing difficult, and increases the wear of the mold. If the reheating temperature is too low, the wear of the hot rolling rollers will be too large, the load on the rolling machine will easily increase, and rolling unevenness will occur.
[0036] In the hot rolling process, a rolling temperature of about 820 to 1000°C is used, and the rolling end temperature is set to 800 to 850°C (for example, about 820°C). If the rolling end temperature is too high, the crystal grains of the structure become coarse after hot rolling, which is disadvantageous for the subsequent wire drawing. In addition, since the composition contains 2 to 3% manganese, island martensite is generated due to the coarse hot rolling structure, which makes it easier for wire breakage to occur after wire drawing. If the rolling end temperature is too low, the load on the rolling machine is likely to increase, which causes rolling unevenness. In the slow cooling process after hot rolling, the hot rolled wire is dispersed on a Stelmor cooling conveyor and slowly cooled, and the cooling rate is designed to be about 0.1 to 5°C / sec. If the cooling rate is too high, the wire will form bainite and martensite, which is disadvantageous for the subsequent wire drawing. If the cooling rate is too low, the production yield is too low, which increases the production cost. The wire produced by hot rolling can be produced as a welding wire by undergoing multiple passes of cold drawing. EXAMPLES
[0037] When an oxidation reaction occurs during welding, the following reaction occurs: Si+O 2 →SiO 2 4 / 3Cr+O 2 →2 / 3Cr 2 O 3 Ti+O2 →TiO 2 2Mn+O 2 →2MnO
[0038] Therefore, the present invention designs an index α that represents the ratio of oxygen captured by manganese, chromium, and titanium to the ratio captured by silicon, where α=(Mn / 2+Ti+Cr / 1.33) / Si. It is expected that the larger the α value, the higher the ratio of oxygen captured by manganese, chromium, and titanium. The components of the examples of the present invention are shown in Table 1. The present invention has an α value of more than 5, which provides excellent performance of the weld bead after welding, and the specific results are as follows:
[0039] [Table 1]
[0040] As shown in FIG. 3, the hot-rolled structure of the embodiment of the present invention after hot rolling is shown, and contains a ferrite structure of more than 95% by volume and a martensite structure of less than 5% by volume.
[0041] Therefore, if desired, the proportion of martensite in the welding wire is designed to be less than 5%.
[0042] Fig. 4 is an electron microscope image of the weld bead surface after welding in the examples of the present invention. As shown in Fig. 4, it was visually confirmed that there was no slag on the surface in any of the examples.
[0043] FIG. 5 is an electron microscope image of the weld bead surface after welding of an example of the present invention. Example 1, which has the lowest α value, was selected to analyze the weld bead surface. As shown in FIG. 5, no silicon-rich oxide was present. FIG. 6 is a diagram showing the distribution of the structure and inclusions inside the weld bead of an example of the present invention. As shown in FIG. 6, many inclusions (i.e., oxides) were observed. The composition of the oxides was evaluated by measuring the composition of the inclusions, and the silicon / manganese (Si / Mn) ratio of the example of the present invention is about 0.2 to 1. The composition of the comparative example has a silicon / manganese (Si / Mn) ratio of about 1.5 or more.
[0044] Therefore, the ratio of silicon content / manganese content of the welding wire is designed to be 0.2-1, if desired.
[0045] By adjusting the components of the welding wire according to the embodiment of the present invention in an exemplary manner, the slag properties are improved and silicon oxide is less likely to be generated, thereby improving the surface quality and plating properties.
[0046] The present invention can modify the slag by designing the composition of alloy elements such as manganese, chromium, and titanium. The composition of the welding wire is designed to use 2-3% manganese, 0.1-0.3% titanium, and auxiliary 0.1-0.5% chromium, so that the silicon content can reach about 0.25wt.% for example. Furthermore, the alloy composition satisfies α>5 (where α=(manganese content / 2+titanium content+chromium content / 1.33) / silicon content), and the surface after testing can achieve a surface that is apparently free of slag containing silicon. In this way, no unplated spots will occur during subsequent plating.
[0047] In addition, when manufacturing the welding wire of the present invention, it is necessary to reduce the amount of titanium carbide dissolved by dissolving at a low discharging temperature between 1000 and 1050°C (for example, about 1030°C). If a large amount of titanium carbide is dissolved, titanium will combine with carbon after hot rolling to form nano-order titanium carbide precipitates, and the strength of the welding wire tends to be too high. The hot rolling temperature is set to about 820 to 1000°C, and the rolling end temperature is set to about 800 to 850°C (for example, about 820°C), thereby promoting the formation of ferrite. If the rolling end temperature is too high, an island martensite structure will appear, and the martensite structure will cause wire drawing cracks. If the discharging temperature or the rolling end temperature is too low, it will be difficult to apply a load to the rolling machine.
[0048] After the rolling process, the wire rod is dispersed and cooled on a Stelmor cooling conveyor at a cooling rate of 0.1 to 5°C / sec. If the cooling rate is too high, high-strength bainite and martensite are formed, making the subsequent wire drawing difficult. If the cooling rate is too low, the yield is too low.
[0049] The present invention further provides a welding wire having a total weight of 100 wt.%, a composition of the welding wire consisting of a carbon content of 0.02-0.10 wt.%, a manganese content of 2.00-3.00 wt.%, a silicon content of 0.01-0.25 wt.%, a chromium content of 0.10-0.5 wt.%, a titanium content of 0.10-0.3 wt.%, unavoidable impurities, and the balance being iron, and wherein the composition of the welding wire satisfies a determination formula of (manganese content / 2+titanium content+chromium content / 1.33) / silicon content>5.
[0050] In some embodiments of the present invention, the welding wire has a silicon content / manganese content ratio of 0.2-1.
[0051] In some embodiments of the present invention, the proportion of martensite in the welding wire is less than 5%.
[0052] In some embodiments of the present invention, the welding wire contains nano-order titanium carbide precipitates. [Explanation of symbols]
[0053] S100: Manufacturing method of welding wire S101~S105: Step
Claims
1. providing a billet having a total weight of 100 wt. %, the billet having a carbon content of 0.02-0.10 wt. %, a manganese content of 2.00-3.00 wt. %, a silicon content of 0.01-0.25 wt. %, a chromium content of 0.10-0.5 wt. %, a titanium content of 0.10-0.3 wt. %, unavoidable impurities, and the balance being iron, the billet satisfying a determination formula of (manganese content / 2+titanium content+chromium content / 1.33) / silicon content>5; heating the billet; hot rolling the heated billet to form a wire; a step of slowly cooling the wire rod formed by hot rolling; and cold drawing the slowly cooled wire rod to form a welding wire.
2. 2. The method of claim 1, wherein the billet has a silicon content / manganese content ratio of 0.2-1.
3. 2. The method according to claim 1, wherein in the heating step, the billet is heated to a temperature of 1000 to 1050°C.
4. 2. The method according to claim 1, wherein in the hot rolling step, the rolling temperature is 820 to 1000°C, and the rolling end temperature is 800 to 850°C.
5. 2. The method according to claim 1, wherein the cooling rate in the slow cooling step is 0.1 to 5° C. / sec.
6. The manufacturing method according to claim 1 , wherein the ratio of martensite in the welding wire is less than 5%.
7. A welding wire having a total weight of 100 wt. %, a composition of the welding wire consisting of a carbon content of 0.02 to 0.10 wt. %, a manganese content of 2.00 to 3.00 wt. %, a silicon content of 0.01 to 0.25 wt. %, a chromium content of 0.10 to 0.5 wt. %, a titanium content of 0.10 to 0.3 wt. %, unavoidable impurities, and the balance being iron, and the composition of the welding wire satisfies a judgment formula of (manganese content / 2+titanium content+chromium content / 1.33) / silicon content>5.
8. 8. The welding wire according to claim 7, wherein the ratio of silicon content to manganese content of the welding wire is 0.2 to 1.
9. The welding wire according to claim 7 , wherein the ratio of martensite in the welding wire is less than 5%.
10. The welding wire according to claim 7 , wherein the welding wire contains nano-order titanium carbide precipitates.
Citation Information
Patent Citations
70kg-grade high-strength and high-toughness gas shielded solid welding wire special for coal machine industry
CN111571060A
Submerged arc welding method
JP1988188491A
High strength steel wire rod having excellent wire drawability and production method therefor
JP2003321742A
Electro-slag welding method
JP2009050867A
Wire for gas shield arc welding
JP2021074777A