Negative photosensitive resin composition and method for producing cured relief pattern
The negative photosensitive resin composition addresses issues of high curing shrinkage, heat resistance, and adhesion by incorporating specific polymerizable compounds and additives, resulting in improved film properties and device reliability for semiconductor manufacturing.
Patent Information
- Application Number
- JP2024075917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional photosensitive resin compositions used in semiconductor manufacturing face challenges such as high curing shrinkage, insufficient heat resistance and mechanical strength, poor adhesion to copper, and inadequate oxygen barrier properties, particularly during low-temperature curing processes, which are essential for preventing warpage and ensuring device reliability in high-speed semiconductor devices.
A negative photosensitive resin composition comprising a polyimide with a polymerizable functional group at the terminal, a polymerizable compound with a urea bond, and a photoinitiator, optionally including additional components like a monomer without a urea bond, silane coupling agent, organic titanium compound, thermal crosslinking agent, and rust inhibitor, to achieve low curing shrinkage, excellent film properties, and improved adhesion and oxygen barrier properties.
The composition exhibits low curing shrinkage, high heat resistance, mechanical strength, and effective adhesion to copper, along with enhanced oxygen barrier properties, facilitating the production of reliable semiconductor devices with reduced warpage and improved performance.
Smart Images

Figure 2024163067000001 
Figure 2024163067000002 
Figure 2024163067000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative-type photosensitive resin composition and a method for producing a cured relief pattern. [Background technology]
[0002] Conventionally, polyimide resins, polybenzoxazole resins, phenolic resins, etc., which have excellent heat resistance, electrical properties, and mechanical properties, have been used as insulating materials for electronic components, and passivation films, surface protective films, interlayer insulating films, etc. for semiconductor devices. Among these resins, those provided in the form of a photosensitive resin composition can easily form a heat-resistant relief pattern film by coating, exposing, developing, and curing the composition to light, subjecting it to a ring-closing treatment (imidization, benzoxazole formation) or thermal crosslinking, and therefore have the characteristic of enabling a significant shortening of the process compared to conventional non-photosensitive materials, and are used in the production of semiconductor devices.
[0003] Incidentally, semiconductor devices (hereinafter also referred to as "elements") are mounted on printed circuit boards by various methods according to the purpose. Conventional elements were generally fabricated by a wire bonding method in which thin wires connect the external terminals (pads) of the element to the lead frame. However, today, as elements have become faster and the operating frequency has reached GHz, differences in the wiring length of each terminal during mounting have come to affect the operation of the element. As a result, when mounting elements for high-end applications, it has become necessary to precisely control the length of the mounting wiring, and it has become difficult to meet this requirement using wire bonding.
[0004] Therefore, flip-chip mounting has been proposed, in which a rewiring layer is formed on the surface of a semiconductor chip, bumps (electrodes) are formed on the rewiring layer, and then the chip is flipped over and mounted directly on a printed circuit board. This flip-chip mounting allows precise control of the wiring distance, so it is adopted for high-end elements that handle high-speed signals, and for mobile phones and other devices due to its small mounting size, and demand is rapidly expanding. More recently, a semiconductor chip mounting technology called fan-out wafer-level packaging (FOWLP) has been proposed, in which individual chips are manufactured by dicing a wafer that has undergone front-end processing, the individual chips are reassembled on a support, sealed with molding resin, and a redistribution layer is formed after peeling off the support. In FOWLP, the redistribution layer is formed with a thin film thickness, which has the advantages of making it possible to reduce the height of the package, as well as enabling high-speed transmission and low costs.
[0005] Currently, the photosensitive polyimide precursors that are widely used in FOWLP require an imidization step involving heating. On the other hand, because FOWLP requires thinner packages, the heating during the process makes the packages more susceptible to warping. From the standpoint of suppressing warping, it is desirable to have a lower curing temperature for the photosensitive resin composition used in the production of elements, and curing at 200°C or lower is considered preferable. For example, Patent Document 1 discloses low-temperature curing of a polyimide precursor at 200° C. or less. Furthermore, when cured at low temperatures, the photosensitive resin composition has low cure shrinkage and high heat resistance, which are effective in suppressing warping.
[0006] Furthermore, when a film is formed on a substrate using a photosensitive resin composition containing a polyamide and the film is heated to cause ring closure of the polyamide to form a polyimide, the film may shrink due to the ring closure reaction and the associated dehydration. From the viewpoint of eliminating the need for an imidization step by heating and suppressing cure shrinkage, for example, Patent Document 2 discloses a photosensitive resin composition containing a solvent-soluble polyimide having an imide ring structure.
[0007] In addition, from the viewpoint of suppressing warpage and enhancing the reliability of elements, the photosensitive resin composition is required to have high adhesion to copper and high oxygen barrier properties. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent Publication No. 2022-091355 [Patent Document 2] JP 2021-162834 A Summary of the Invention [Problem to be solved by the invention]
[0009] In Patent Document 1, there is a problem that the side chain portion volatilizes as a result of imidization, resulting in large cure shrinkage. Furthermore, there is a problem that under low-temperature curing conditions, imidization does not progress sufficiently, resulting in insufficient heat resistance and mechanical strength (elongation of the cured film).
[0010] Furthermore, Patent Document 2 has a problem in that the adhesion to copper and the oxygen barrier property, which are important properties for device reliability, are insufficient.
[0011] The present invention aims to provide a negative photosensitive resin composition which has low cure shrinkage and which exhibits excellent film properties after low-temperature curing, such as heat resistance, mechanical strength (elongation of the cured film), adhesion to copper, and oxygen barrier properties, and a method for producing a cured relief pattern. [Means for solving the problem]
[0012] That is, the present invention is as follows.
[0013] [1] (A) a polyimide having a polymerizable functional group at its terminal; (B) a polymerizable compound having a urea bond, and (C) Photopolymerization initiator A negative type photosensitive resin composition comprising: [2] The negative photosensitive resin composition according to [1], wherein the (A) polyimide has no polymerizable functional group in a side chain. [3] The negative type photosensitive resin composition according to [1] or [2], wherein the (A) polyimide and the (B) polymerizable compound have a structure derived from the same diamine. [4] The negative photosensitive resin composition according to any one of [1] to [3], wherein the content of the polymerizable compound (B) is 0.1 to 50 parts by mass based on 100 parts by mass of the polyimide (A). [5] The negative photosensitive resin composition according to any one of [1] to [4], wherein the weight average molecular weight Mw of the polyimide (A) is 3,000 or more and 30,000 or less. [6] The negative photosensitive resin composition according to any one of [1] to [5], further comprising (D) a monomer having a polymerizable functional group not having a urea bond. [7] The negative photosensitive resin composition according to any one of [1] to [6], further comprising (E) a silane coupling agent. [8] The negative photosensitive resin composition according to any one of [1] to [7], further comprising (F) an organotitanium compound. [9] The negative photosensitive resin composition according to any one of [1] to [8], further comprising (G) a thermal crosslinking agent.
[10] The negative photosensitive resin composition according to any one of [1] to [9], further comprising (H) a rust inhibitor.
[11] The process is as follows: (1) A step of applying the negative type photosensitive resin composition according to any one of [1] to
[10] onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat treating the relief pattern to form a hardened relief pattern; 2. A method for producing a cured relief pattern comprising:
[12] The negative photosensitive resin composition was post-baked at 170° C. for 120 minutes in a nitrogen atmosphere to obtain a cured film having a thickness of 6 μm. The oxygen permeability (cc / m 2 The negative photosensitive resin composition according to any one of [1] to
[10] , wherein the viscosity at 1000 nm is 1.0 MPa. Effect of the Invention
[0014] According to the present invention, it is possible to provide a negative type photosensitive resin composition having low cure shrinkage and excellent film properties after low-temperature curing, such as heat resistance, mechanical strength (elongation of the cured film), adhesion to copper, and oxygen blocking property, and a method for producing a cured relief pattern. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the present disclosure will be described in detail. Throughout the present disclosure, when a structure represented by the same symbol in a general formula is present in a molecule, each of the structures is independently selected and may be the same or different from each other, unless otherwise specified. In addition, structures represented by common symbols in different general formulas are also independently selected unless otherwise specified, and may be the same or different from each other.
[0016] In the following description, the upper limit or lower limit of a numerical range described in stages may be replaced with the upper limit or lower limit of another numerical range described in stages. In the following description, the upper or lower limit of a certain numerical range may be replaced with a value described in the examples. Furthermore, with regard to the term "step" in the following description, not only an independent step but also a step that cannot be clearly distinguished from other steps can be included in this term as long as the function of that "step" is achieved.
[0017] <Negative-type photosensitive resin composition> The negative type photosensitive resin composition of the present disclosure (hereinafter referred to as the “photosensitive resin composition”) contains (A) a polyimide having a polymerizable functional group at an end, (B) a polymerizable compound having a urea bond, and (C) a photopolymerization initiator. The negative type photosensitive resin composition of the present disclosure may further contain, if desired, in addition to the above-mentioned components, an additive selected from (D) a monomer having a polymerizable functional group not having a urea bond, (E) a silane coupling agent, (F) an organic titanium compound, (G) a thermal crosslinking agent, and (H) an anti-rust agent, and other components.
[0018] (A) Polyimide having polymerizable functional groups at its terminals The polyimide having a polymerizable functional group at its terminal (A) of the present disclosure is represented by the following formula (1): [ka] {In formula (1), X 1 is a tetravalent organic group, and Y 1 is a divalent organic group, and n is an integer of 2 to 150.} It is preferable that the compound contains a structure represented by the following formula:
[0019] From the viewpoints of low cure shrinkage and heat resistance, it is preferable that the polyimide of the present disclosure is substantially free of a polyamic acid or polyamic acid ester structure. In the present disclosure, "substantially free of" a polyamic acid or polyamic acid ester structure means, for example, that the imidization rate of the polyimide is 90% or more, and preferably 95% or more. The imidization rate of polyimide can be measured by a known method, but for example, it can be calculated by the following method. First, the infrared absorption spectrum of the polyimide is measured, and the absorption peak of the imide structure (1780 cm -1 Near, 1377cm -1 Next, the polyimide is heat-treated at 350°C for 1 hour, and the infrared absorption spectrum of the heat-treated polyimide is measured to confirm the presence of a peak at 1377cm -1 By comparing the peak intensity in the vicinity with the intensity of the polyimide before heat treatment, the imidization rate of the polyimide can be calculated.
[0020] X in formula (1) 1The structure is not particularly limited as long as it is a structure derived from a known tetracarboxylic dianhydride, and examples thereof include a structure derived from a tetracarboxylic dianhydride represented by the following formula (2). [ka]
[0021] From the viewpoints of the heat resistance of the cured film obtained from the negative type photosensitive resin composition of the present disclosure and the solvent solubility of the polyimide, 1 In terms of the elongation of the cured film, it is preferable that the structure derived from the tetracarboxylic dianhydride of X has an alicyclic structure. 1 It is preferable that the structure derived from the tetracarboxylic dianhydride has an aromatic structure.
[0022] Y in formula (1) 1 The structure is not particularly limited as long as it is a structure derived from a known diamine, and examples thereof include structures derived from diamines represented by the following formulas (3) to (4). [ka] [ka]
[0023] Furthermore, in terms of the elongation of a cured film obtained from the negative photosensitive resin composition of the present disclosure and the solvent solubility of a polyimide, among the structures derived from the diamines of the formulas (3) to (4), structures derived from diamines represented by the following formulas (5) to (11) are preferred, and in terms of the heat resistance of the cured film, structures derived from diamines represented by the following formulas (12) to (15) are preferred. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0024] The polymerizable functional group of the present disclosure is, in one embodiment, a radical polymerizable functional group, typically a carbon-carbon double bond moiety. The polymerizable functional group is not particularly limited, but is preferably a functional group having an ethylenically unsaturated bond. The polyimide having a polymerizable functional group at its terminal (A) preferably has the polymerizable functional group at the terminal of the main chain or side chain, and more preferably has the polymerizable functional group at the terminal of the main chain. By including the polyimide having a polymerizable functional group at its terminal (A), the negative-type photosensitive resin composition of the present disclosure can have excellent adhesion to copper and can improve oxygen barrier properties. The (A) polyimide having a polymerizable functional group at its terminal may have a polymerizable functional group at the terminal of a side chain. However, from the viewpoint of the elongation and storage stability of the cured film, it is preferable that the polyimide does not have a polymerizable functional group at the terminal of the side chain.
[0025] Specific examples of the polymerizable functional group include those represented by the following formulas (16) to (18). [ka] (R 1 and R 2are each independently selected from a hydrogen atom and a monovalent organic group having 1 to 3 carbon atoms; R 3 R is an organic group having 1 to 20 carbon atoms which may contain a heteroatom, and k is an integer of 1 or 2. 4 is a hydrogen atom or an organic group having 1 to 4 carbon atoms, and * indicates the bonding site with the end of the (A) polyimide. In this disclosure, an organic group refers to a group having one or more carbon atoms. [ka] (In the formula, R 5 and R 6 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms. Also, * indicates a bonding site with an end of the (A) polyimide.) [ka] (In the formula, R 7 , R 8 and R 9 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and j is an integer of 2 to 10. In addition, * indicates a bonding site with an end of the (A) polyimide.
[0026] More specific examples of the structure represented by formula (16) include those represented by the following formulae (19) to (22). [ka] [ka] [ka] [ka] (In the formulas (19) to (22), * indicates a bonding site with the terminal of polyimide (A).)
[0027] More specific examples of the structure represented by formula (17) include those represented by the following formulae (23) and (24). [ka] [ka] (In the formulas (23) to (24), * indicates a bonding site with the terminal of polyimide (A).)
[0028] More specific examples of the compound represented by formula (18) include those represented by the following formulae (25) to (28). [ka] [ka] [ka] [ka] (In the formulas (25) to (28), * indicates a bonding site with the end of polyimide (A).)
[0029] From the viewpoint of oxygen blocking properties, it is preferable that the polymerizable functional group at the end of the polyimide has a urea bond as a linking group with the polymer. Specific examples include those represented by the above formulas (19) to (22).
[0030] The molecular weight distribution (Mw / Mn) of the polyimide (A) is preferably 1.0 or more and 1.9 or less. From the viewpoint of production efficiency, the lower limit of the molecular weight distribution of the polyimide (A) is more preferably 1.15 or more, and even more preferably 1.25 or more. From the viewpoint of resolution, the upper limit of the molecular weight distribution of the polyimide (A) is more preferably 1.6 or less, and even more preferably 1.5 or less.
[0031] The weight average molecular weight (Mw) of the (A) polyimide is not particularly limited as long as the (A) polyimide is soluble in the (I) solvent described below. From the viewpoints of the copper adhesion and heat resistance of a cured film obtained from the negative type photosensitive resin composition of the present disclosure, the weight average molecular weight (Mw) is preferably 3,000 or more and 30,000 or less. From the viewpoint of the elongation of the cured film, the lower limit of the weight average molecular weight of the polyimide (A) is more preferably at least 4,000, and even more preferably at least 5,000. From the viewpoint of the solubility of the polyimide in a solvent, the upper limit of the weight average molecular weight of the polyimide (A) is more preferably at most 25,000, and even more preferably at most 20,000. The weight average molecular weight of the polyimide (A) can be measured, for example, by the method described in the Examples below.
[0032] <Method of manufacturing polyimide having polymerizable functional groups at its terminals> (A) A polyimide having a polymerizable functional group at its terminal can be obtained, for example, by reacting a tetracarboxylic dianhydride with a diamine to obtain a polyamic acid, which is then subjected to a heat treatment to dehydrate and ring-close the polyimide to obtain a polyimide having a reactive group at the terminal of the main chain, and then reacting the polyimide having a reactive group at the terminal of the main chain with a compound having a polymerizable functional group at the terminal. In the present disclosure, reactive groups refer to carboxyl groups or acid anhydride groups derived from tetracarboxylic dianhydrides at the ends of the main chain of polyimide, or amino groups derived from diamines at the ends of the main chain of polyimide. The modification rate of the terminals of the polyimide (A) is measured by the method described in the Examples.
[0033] The temperature at which the polyamic acid is dehydrated and cyclized by heat treatment is not particularly limited, but since the cyclization reaction is not completed at a low temperature, the lower limit is preferably 150° C. or more, and more preferably 160° C. or more. On the other hand, since side reactions proceed at a high temperature, the upper limit is preferably 200° C. or less, and more preferably 180° C.
[0034] The tetracarboxylic dianhydride is not particularly limited, but specific examples include bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (BCD), 4,4'-oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride.
[0035] The diamine is not particularly limited, but specific examples include 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 6-(4-aminophenoxy)[1,1'-biphenyl]-3-amine (PDPE), 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 9,9-bis(4-aminophenyl)fluorene (BAFL), 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine (TFMB), and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP).
[0036] The compound having a polymerizable functional group at its terminal is preferably at least one compound selected from the group consisting of isocyanate-based compounds, chloride-based compounds, and alcohol-based compounds. Specific examples of isocyanate compounds include 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate. Specific examples of chloride compounds include acryloyl chloride and methacryloyl chloride. Specific examples of alcohol-based compounds include 2-hydroxyethyl methacrylate (2-hydroxyethyl methacrylate: HEMA), 2-hydroxyethyl acrylate, 4-hydroxyethyl methacrylate, and 4-hydroxyethyl acrylate.
[0037] The isocyanate compound reacts with the amino group of the dehydrated ring-closed polyimide to form a urea bond. The chloride compound reacts with the amino group of the polyimide that has been dehydrated and ring-closed to form an amide bond. The alcohol compound reacts with the carboxyl group of the dehydrated ring-closed polyimide to form an ester bond.
[0038] The method for reacting the isocyanate compound is not particularly limited, but the compound can be reacted with the amino groups of the dehydrated ring-closed polyimide by stirring at room temperature.
[0039] The method for reacting the chloride compound is not particularly limited, but the chloride compound can be reacted with the amino groups of the dehydrated, ring-closed polyimide by ice-cooling the polyimide solution and adding the chloride compound dropwise.
[0040] The method for reacting the alcohol-based compound is not particularly limited, but it can be reacted with the carboxyl group of the dehydration-ring-closed polyimide using a condensing agent such as N,N'-dicyclohexylcarbodiimide (DCC) or an esterification catalyst such as p-toluenesulfonic acid.
[0041] In the production of (A) polyimide, a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the tetracarboxylic dianhydride, diamine, and compound having a polymerizable functional group at its end. Examples of the reaction solvent include γ-butyrolactone (GBL), dimethylsulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0042] The polyimide (A) may be purified by a known method such as that described in JP 2012-194520 A. For example, a method of dropping a solution of the polyimide (A) dissolved in the solvent (I) into water to reprecipitate and remove unreacted materials, a method of removing a condensing agent insoluble in the reaction solvent by filtration, a method of removing the catalyst using an ion exchange resin, etc. After such purification, the polyimide (A) may be dried by a known method and isolated in a powder state.
[0043] The (A) polyimide is contained in an amount of preferably 20 to 70 mass %, and more preferably 25 to 65 mass %, based on the total solid content mass of the negative photosensitive resin composition of the present disclosure.
[0044] (B) Polymerizable compound having a urea bond The negative type photosensitive resin composition of the present disclosure contains the polymerizable compound having a urea bond (B), and thus the negative type photosensitive resin composition of the present disclosure has excellent adhesion to copper and oxygen blocking properties. Although the reason why the above-mentioned effect is exhibited by using the (B) polymerizable compound having a urea bond is not clear, the present inventors consider it as follows. The urea moiety in the polymerizable compound having a urea bond (B) exhibits strong interaction with the copper surface. Furthermore, when the polymerizable moiety in the polymerizable compound having a urea bond (B) reacts with the polyimide terminal, the polymerizable compound having a urea bond (B) acts as a binder between the photosensitive resin composition and the copper surface, improving adhesion to copper. In addition, since the urea moieties have strong interactions not only with copper but also with each other, the (A) polyimide and (B) polymerizable compound having a urea bond in the photosensitive resin composition are densely packed, thereby improving the oxygen barrier properties.
[0045] The polymerizable compound having a urea bond (B) is not particularly limited as long as it has a polymerizable functional group that is polymerized by light or heat, but is preferably a radical polymerizable compound. The polymerizable functional group of the polymerizable compound having a urea bond (B) may be one or two or more.
[0046] An example of the polymerizable compound having a urea bond (B) is a compound represented by the following formula (29). [ka] In formula (29), E represents a structure derived from a diamine. 3 and Z 4 may be the same or different and each represent a monovalent organic group containing a urea bond serving as a linking group and a polymerizable functional group, and r and s each represent an integer of 0 to 2 and satisfy r+s≧1.}
[0047] (B) The polymerizable compound having a urea bond can be synthesized, for example, from a diamine and an isocyanate compound. E in the formula (29) is a structure derived from a diamine, Z 3 and Z 4 represents a structure derived from an isocyanate compound.
[0048] The structure of E in formula (29) is not particularly limited as long as it is a structure derived from a known diamine, but for example, structures derived from diamines of the following formulae (30) to (31) are preferred. [ka] [ka]
[0049] Among the structures derived from the diamines of the formulae (30) to (31), structures derived from the diamines of the following formulae (32) to (38) are preferred from the viewpoint of the elongation of the cured film obtained from the negative photosensitive resin composition of the present disclosure. Furthermore, structures derived from the diamines of the following formulae (39) to (42) are preferred from the viewpoint of the heat resistance of the cured film. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0050] From the viewpoint of compatibility with the polyimide (A), the polyimide (A) and the polymerizable compound having a urea bond (B) preferably have a skeleton (structure) derived from the same diamine, and more preferably have a structure derived from the diamine of the formulae (30) to (31). When the polymerizable compound having a urea bond (B) has excellent compatibility with the polyimide (A), the polymerizable functional group at the end of the polyimide (A) and the polymerizable functional group of the polymerizable compound having a urea bond (B) are easily reacted with each other, and the mechanical strength (elongation) of the cured film obtained by curing the photosensitive resin composition containing the polyimide (A) and the polymerizable compound (B) is easily improved, which is preferable.
[0051] Z in formula (29) 3 and Z 4 The structure is not particularly limited as long as it is a structure derived from a known isocyanate compound, and examples thereof include structures derived from isocyanate compounds of the following formulae (43) to (46). [ka] [ka] [ka] [ka] (In the formulas (43) to (46), * indicates a bonding site with the diamine (A).)
[0052] <(B) Method for producing polymerizable compound having urea bond> (B) The polymerizable compound having a urea bond can be produced, for example, by reacting an amino group derived from a diamine compound with an isocyanate group derived from an isocyanate compound. The modification rate of the polymerizable compound having a urea bond (B) is measured by the method described in the Examples.
[0053] The temperature at which the diamine compound and the isocyanate compound are reacted is not particularly limited, but the reaction can be carried out, for example, by stirring at room temperature for about 10 hours.
[0054] The diamine compound is not particularly limited, but specific examples include 4,4'-diaminodiphenyl ether (DADPE), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 6-(4-aminophenoxy)biphenyl-3-amine (PDPE), 4,4'-bis(4-aminophenoxy) ...1, (i) Biphenyl, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 9,9-bis(4-aminophenyl)fluorene (BAFL), 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine (TFMB) and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP). From the viewpoint of the elongation of the cured film obtained from the negative-type photosensitive resin composition of the present disclosure, 4,4'-diaminodiphenyl ether (DADPE), 1,4-bis(4-aminophenoxy)benzene (TPE-Q) and 6-(4-aminophenoxy)biphenyl-3-amine (PDPE) are preferred, and from the viewpoint of heat resistance, 9,9-bis(4-aminophenyl)fluorene (BAFL) is preferred.
[0055] The isocyanate compound is not particularly limited, but examples thereof include 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate.
[0056] In the production of the polymerizable compound having a urea bond (B), a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the diamine, the isocyanate compound, and the polymerizable compound having a urea bond. Examples of reaction solvents include γ-butyrolactone (GBL), dimethylsulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0057] From the viewpoint of copper adhesion and oxygen blocking property, the polymerizable compound having a urea bond (B) is preferably contained in an amount of 0.1 part by mass to 60 parts by mass, or preferably 0.1 part by mass to 50 parts by mass, more preferably 1 part by mass to 60 parts by mass, even more preferably 2 parts by mass to 50 parts by mass, and particularly preferably 3 parts by mass to 40 parts by mass, relative to 100 parts by mass of the polyimide (A). From the viewpoint of copper adhesion, the lower limit of the content of the (B) polymerizable compound having a urea bond is preferably 0.1 part by mass or more, more preferably 1 part by mass or more, even more preferably 2 parts by mass or more, and particularly preferably 3 parts by mass or more, relative to 100 parts by mass of the (A) polyimide. The upper limit of the content of the (B) polymerizable compound having a urea bond is more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, per 100 parts by mass of the (A) polyimide, from the viewpoints of suppression of cure shrinkage (low cure shrinkage) and elongation of the cured film.
[0058] From the viewpoint of oxygen blocking properties, the negative photosensitive resin composition according to this embodiment has an oxygen permeability (cc / m 2 ·24h·atm) is preferably less than 1000, more preferably from 500 to less than 1000, further preferably from 200 to less than 500, and particularly preferably less than 200.
[0059] (Oxygen barrier properties) The oxygen barrier property of the cured film obtained by curing the negative photosensitive resin composition according to this embodiment is measured by the following method. The negative photosensitive resin composition of the present embodiment is prebaked to form a pre-cured film having a thickness of about 7 μm, which is then post-baked for curing at 170° C. for 120 minutes in a nitrogen atmosphere to prepare a cured film (cured film) having a thickness of about 6 μm (5.0 to 7.0 μm in one embodiment). The oxygen permeability (cc / m) was measured using a gas permeability measuring device (GTR Tech Co., Ltd., product name: GTR-10XF (isobaric GC)) according to the isobaric GC method of JIS K 7126-2. 2 ·24h·atm).
[0060] <(C) Photopolymerization initiator> (C) The photopolymerization initiator is a compound that generates radicals when exposed to actinic rays and can polymerize an ethylenically unsaturated group-containing compound or the like. Examples of initiators that generate radicals when exposed to actinic rays include compounds containing structures such as benzophenone, N-alkylaminoacetophenone, oxime ester, acridine, phosphine oxide, and lophine. Specific examples include aromatic ketones such as benzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N,N',N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, acrylated benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide; Benzoin ether compounds such as benzoin methyl ether, benzoin ethyl ether and benzoin phenyl ether; Benzoin compounds such as benzoin, methylbenzoin and ethylbenzoin; 1,2-Octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (BASF Japan Ltd., Irgacure Oxe02), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(o-benzoyloxime) (Changzhou New Power Electronic Materials Co., Ltd., PBG305), 1-(6-O-methylbenzoyl-9-ethylcarbazol-3-yl)-(3-cyclopentylacetone)-1-oxime acetate (Changzhou New Power Electronic Materials Co., Ltd., TR-PBG-304), Oxime ester compounds such as TR-PBG-3057 (manufactured by Changzhou New Strong Electronic Materials Co., Ltd.), 1,2-propanedione, 3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-, 2-(O-acetyloxime) (manufactured by Nikko Chemtech Co., Ltd., product name: TR-PBG-326), and NCI-831 (manufactured by ADEKA Corporation); Benzyl derivatives such as benzyl dimethyl ketal; Acridine derivatives such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; N-phenylglycine derivatives such as N-phenylglycine; Coumarin compounds; Oxazole compounds; Phosphine oxide compounds such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, Examples of the lophine compounds include, but are not limited to, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole. The photopolymerization initiator (C) may be used alone or in combination of two or more. Among the above photopolymerization initiators, oxime ester compounds are more preferred, particularly from the viewpoint of resolution.
[0061] The content of the (C) photopolymerization initiator is preferably 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the (A) polyimide. From the viewpoint of photocurability, the lower limit of the content of the (C) photopolymerization initiator is more preferably 2 parts by mass or more per 100 parts by mass of the (A) polyimide. The upper limit of the content of the (C) photopolymerization initiator is more preferably 20 parts by mass or less per 100 parts by mass of the (A) polyimide, from the viewpoint of curing the bottom of the relief pattern.
[0062] (D) Monomer having a polymerizable functional group that does not have a urea bond In order to improve the resolution of the cured relief pattern and suppress cure shrinkage during thermal curing, the photosensitive resin composition of the present disclosure may optionally contain (D) a monomer having a polymerizable functional group that does not have a urea bond. The monomer (D) having a polymerizable functional group without a urea bond (in one embodiment, a radically polymerizable compound) is preferably a (meth)acrylic compound that undergoes a radical polymerization reaction with a photopolymerization initiator (C). The monomer (D) having a polymerizable functional group without a urea bond more preferably includes a monofunctional monomer (D1) having one polymerizable functional group in the molecule and / or a polyfunctional monomer (D2) having two or more polymerizable functional groups in the molecule.
[0063] Examples of the monofunctional monomer (D1) include, but are not limited to, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexyl (meth)acrylate, butoxydiethylene glycol methacrylate, isobornyl (meth)acrylate, m-phenoxybenzyl acrylate, o-phenylphenoxyethyl acrylate, 4-methacryloyloxybenzophenone, EO (ethylene oxide)-modified paracumylphenol acrylate, nonylphenoxyethyl acrylate, 6-acrylamidohexanoic acid, and tris-(2-acryloxyethyl)isocyanurate. Examples of the polyfunctional monomer (D2) include di(meth)acrylates of ethylene glycol or polyethylene glycol, such as diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, di(meth)acrylates of propylene glycol or polypropylene glycol, di(meth)acrylates or tri(meth)acrylates of glycerol, cyclohexane di(meth)acrylate, di(meth)acrylates of 1,4-butanediol, di(meth)acrylates of 1,6-hexanediol, di(meth)acrylates of neopentyl glycol, di(meth)acrylates of bisphenol A, (Meth)acrylamide and its derivatives, Trimethylolpropane tri(meth)acrylate, di(meth)acrylate or tri(meth)acrylate of glycerol, di(meth)acrylate, tri(meth)acrylate or tetra(meth)acrylate of pentaerythritol, ethylene oxide (e.g., 4-hydroxybutyl acrylate glycidyl ether) or propylene oxide adducts of these compounds, Urethane acrylates such as product name: KRM7735 (manufactured by Daicel-Allnex), product name: EBECRYL230 (manufactured by Daicel-Allnex), product name: EBECRYL4491 (manufactured by Daicel-Allnex), product name: EBECRYL8413 (manufactured by Daicel-Allnex), product name: EBECRYL8411 (manufactured by Daicel-Allnex), product name: EBECRYL8402 (manufactured by Daicel-Allnex), product name: EBECRYL8465 (manufactured by Daicel-Allnex), product name: EBECRYL8667 (manufactured by Daicel-Allnex), product name: EBECRYL4740 (manufactured by Daicel-Allnex), product name: KRM9276 (manufactured by Daicel-Allnex), etc. Mention may be made of the compound tris-(2-hydroxyethyl) isocyanurate acrylate. Among these radically polymerizable compounds, it is preferable to use a compound having three or more radically polymerizable functional groups from the viewpoint of suppressing cure shrinkage. In addition, the weight ratio of the monofunctional monomer (D1) to the polyfunctional monomer (D2) in these monomers is preferably greater than 0.01 from the viewpoint of flatness during coating, and is preferably less than 1.5 from the viewpoint of flatness after curing.
[0064] The content of the (D) monomer having a polymerizable functional group not having a urea bond in the photosensitive resin composition is preferably 0.5 to 100 parts by mass relative to 100 parts by mass of the (A) polyimide. From the viewpoint of photocurability, the lower limit of the content of the (D) monomer having a polymerizable functional group that does not have a urea bond is more preferably 5 parts by mass or more, further preferably 10 parts by mass or more, and particularly preferably 20 parts by mass or more, relative to 100 parts by mass of the (A) polyimide. The upper limit of the content of (D) monomer having a polymerizable functional group that does not have a urea bond is more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of (A) polyimide, from the viewpoints of copper adhesion and bottom curing of the pattern.
[0065] (E) Silane coupling agent To improve the copper adhesion of the cured relief pattern, the negative-type photosensitive resin composition of the present disclosure can optionally include (E) a silane coupling agent. (E) The silane coupling agent is represented by the following general formula (47): [ka] or equation (48): [ka] It is preferable that the compound has a structure represented by the following formula: In formulas (47) and (48), R 10 is at least one selected from the group consisting of substituents containing an epoxy group, a phenylamino group, a ureido group, an isocyanate group, and an isocyanuric group; R 11 is an alkyl group having 1 to 4 carbon atoms, and R 12represents a hydroxyl group or an alkyl group having 1 to 4 carbon atoms, a represents an integer of 1 to 3, and i represents an integer of 1 to 6.
[0066] In general formulas (47) and (48), a is not limited as long as it is an integer of 1 to 3, but from the viewpoint of adhesion to the metal redistribution layer, it is preferably 2 or 3, and more preferably 3. i is not limited as long as it is an integer of 1 to 6, but from the viewpoint of adhesion to the metal redistribution layer, it is preferably 1 or more and 4 or less. From the viewpoint of resolution, it is preferably 2 or more and 5 or less.
[0067] R 10 is not limited as long as it is a substituent containing any one of the structures of the group consisting of an epoxy group, a phenylamino group, a ureido group, an isocyanate group, and an isocyanuric group. Among these, from the viewpoint of resolution and adhesion of the metal redistribution layer, it is preferable that it is at least one selected from the group consisting of a substituent containing a phenylamino group and a substituent containing a ureido group, and a substituent containing a phenylamino group is more preferable. R 11 is not limited as long as it is an alkyl group having 1 to 4 carbon atoms. Examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, and a t-butyl group. R 12 is not limited as long as it is a hydroxyl group or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include R 11 The alkyl groups shown in the above are exemplified.
[0068] Examples of silane coupling agents containing an epoxy group include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane. An example of a silane coupling agent containing a phenylamino group is N-phenyl-3-aminopropyltrimethoxysilane. An example of the silane coupling agent containing a ureido group is 3-ureidopropyltrialkoxysilane. An example of a silane coupling agent containing an isocyanate group is 3-isocyanatepropyltriethoxysilane.
[0069] The content of the silane coupling agent (E) in the negative photosensitive resin composition is 0.2 to 10 parts by mass relative to 100 parts by mass of the polyimide (A). From the viewpoint of copper adhesion, the lower limit of the content of the (E) silane coupling agent is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, per 100 parts by mass of the (A) polyimide. From the viewpoint of preventing the generation of foreign matter due to precipitation, the upper limit of the content of the (E) silane coupling agent is more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, per 100 parts by mass of the (A) polyimide.
[0070] (F) Organotitanium Compounds In order to improve the chemical resistance of the cured film, the negative photosensitive resin composition of the present disclosure may optionally contain (F) an organotitanium compound.
[0071] (F) The organotitanium compound includes those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of the organotitanium compound are shown in I) to VII) below: I) Titanium chelate compounds: Specific examples include titanium(IV) oxide acetylacetonate, titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), and the like.
[0072] II) Tetraalkoxytitanium compounds: For example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], and the like.
[0073] III) Titanocene compounds: For example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like.
[0074] IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc.
[0075] V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, and the like.
[0076] VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate.
[0077] VII) Titanate coupling agents: For example, isopropyl tridodecylbenzenesulfonyl titanate.
[0078] As the (F) organic titanium compound, from the viewpoint of exhibiting better chemical resistance, it is preferable to use at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium and titanium(IV) oxide acetylacetonate are preferred.
[0079] When the negative type photosensitive resin composition of the present disclosure contains an organotitanium compound (F), the content of the organotitanium compound (F) is preferably 0.05 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the polyimide (A). The lower limit of the content of the (F) organotitanium compound is more preferably 0.5 parts by mass or more per 100 parts by mass of the (A) polyimide, from the viewpoint of the heat resistance and chemical resistance of the resulting cured film. The upper limit of the content of the (F) organotitanium compound is more preferably 2 parts by mass or less per 100 parts by mass of the (A) polyimide, from the viewpoint of storage stability of the negative photosensitive resin composition.
[0080] (G) Thermal crosslinking agent From the viewpoint of suppressing cure shrinkage of the cured film, the negative type photosensitive resin composition of the present disclosure may optionally contain a (G) thermal crosslinking agent.
[0081] In the present disclosure, the term "(G) thermal crosslinking agent" refers to a compound that undergoes an addition reaction or a condensation polymerization reaction due to heat. These reactions occur between (A) polyimide and (G) thermal crosslinking agent, between (G) thermal crosslinking agents, and between (G) thermal crosslinking agent and other components described below, and the reaction temperature is preferably 150°C or higher.
[0082] Examples of the (G) thermal crosslinking agent include an alkoxymethyl compound, an epoxy compound, an oxetane compound, a bismaleimide compound, an allyl compound, and a blocked isocyanate compound. From the viewpoint of suppressing cure shrinkage, the (G) thermal crosslinking agent preferably contains a nitrogen atom.
[0083] Examples of the alkoxymethyl compound include, but are not limited to, compounds represented by the following general formulas (49) to (50). [ka] [ka]
[0084] Examples of the epoxy compound include 4-hydroxybutyl acrylate glycidyl ether, epoxy compounds containing a bisphenol A group, and hydrogenated bisphenol A diglycidyl ether (for example, product name: Epolite 4000, manufactured by Kyoeisha Chemical Co., Ltd.). Examples of oxetane compounds include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, bis[1-ethyl(3-oxetanyl)]methyl ether, 4,4'-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl, 4,4'-bis(3-ethyl-3-oxetanylmethoxy)biphenyl, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, diethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, and bis(3-ethyl-3-oxetanylmethyl)diphenoyl. ester, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl)ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, poly[[3-[(3-ethyl-3-oxetanyl)methoxy]propyl]silasesquioxane] derivatives, oxetanyl silicate, phenol novolac type oxetane, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, product name: OXT121 (manufactured by Toagosei Co., Ltd.), and product name: OXT221 (manufactured by Toagosei Co., Ltd.). Examples of bismaleimide compounds include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,3-phenylenebis(maleimide), and 5-methyl-N,N'-1,3-phenylenebis(maleimide). Examples of such maleimide include N,N'-1,4-phenylene bis(maleimide), 3-methyl-N,N'-1,4-phenylene bis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane. Examples of the allyl compound include allyl alcohol, allyl anisole, allyl benzoate, allyl cinnamate, N-allyloxyphthalimide, allylphenol, allyl phenyl sulfone, allyl urea, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl maleate, diallyl isocyanurate, triallyl amine, triallyl isocyanurate, triallyl cyanurate, triallyl amine, triallyl 1,3,5-benzenetricarboxylate, triallyl trimellitate, triallyl phosphate, triallyl phosphite, and triallyl citrate. Examples of the blocked isocyanate compound include hexamethylene diisocyanate-based blocked isocyanates; trade names are Duranate SBN-70D, SBB-70P, SBF-70E, TPA-B80E, 17B-60P, MF-B60B, E402-B80B, MF-K60B, and WM44-L70G (all manufactured by Asahi Kasei Corporation); Product name: Takenate B-882N (manufactured by Mitsui Chemicals, Inc.), product names: 7960, 7961, 7982, 7991, and 7992 (manufactured by Baxenden), etc. Tolylene diisocyanate-based blocked isocyanate (manufactured by Mitsui Chemicals, Inc., product name: Takenate B-830, etc.), 4,4'-diphenylmethane diisocyanate-based blocked isocyanate (manufactured by Mitsui Chemicals, Inc., product name: Takenate B-815N), (manufactured by Daiei Sangyo Co., Ltd., product names: Bronate PMD-OA01 and PMD-MA01), etc. 1,3-bis(isocyanatemethyl)cyclohexane-based blocked isocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate B-846N), (manufactured by Tosoh Corporation, trade names: Coronate BI-301, 2507, and 2554), etc. Examples of the blocked isocyanates include isophorone diisocyanate-based blocked isocyanates (manufactured by Baxenden, trade names: 7950, 7951, and 7990, etc.). Among these compounds, blocked isocyanate compounds and bismaleimide compounds are preferred from the viewpoint of storage stability. (G) The thermal crosslinking agent may be used alone or in combination of two or more kinds.
[0085] The content of the (G) thermal crosslinking agent in the negative photosensitive resin composition is preferably 0.2 to 40 parts by mass relative to 100 parts by mass of the (A) polyimide. From the viewpoint of chemical resistance, the lower limit of the content of the (G) thermal crosslinking agent is more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, per 100 parts by mass of the (A) polyimide. From the viewpoint of storage stability of the negative photosensitive resin composition, the upper limit of the content of the (G) thermal crosslinking agent is more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of the (A) polyimide.
[0086] (H) Rust inhibitor When the negative type photosensitive resin composition of the present disclosure is used to form a cured film on a substrate made of copper or a copper alloy, the negative type photosensitive resin composition of the present disclosure may optionally contain (H) a rust inhibitor in order to suppress discoloration of the copper. Examples of (H) rust inhibitors include azole compounds and purine compounds.
[0087] Examples of the azole compounds include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, 2-( 3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 3-mercapto-1,2,4-triazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole and 1-methyl-1H-tetrazole.
[0088] Particularly preferred are 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, and 4-methyl-1H-benzotriazole. These azole compounds may be used alone or in combination of two or more.
[0089] Specific examples of purine compounds include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminopurine, 9-methyladenine, 2-hydroxyadenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminopurine, 9 ... Aminoadenine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, 8-azahypoxanthine, and the like, and derivatives thereof.
[0090] Particularly preferred is 8-azaadenine. These purine compounds may be used alone or in combination of two or more.
[0091] When the negative type photosensitive resin composition of the present disclosure contains the rust inhibitor (H), the content of the rust inhibitor (H) is preferably 0.01 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the polyimide (A). The lower limit of the (H) rust inhibitor is more preferably 0.03 parts by mass or more, and even more preferably 0.05 parts by mass or more, because discoloration of the copper or copper alloy surface is suppressed when the negative photosensitive resin composition is formed on copper or a copper alloy. The upper limit of the (H) rust inhibitor is more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, from the viewpoint of photosensitivity.
[0092] The negative type photosensitive resin composition of the present disclosure may further contain other components in addition to the above components (A) to (H). The other components in addition to the components (A) to (H) are not limited, but examples thereof include a thermal polymerization initiator, a plasticizer, a hindered phenol compound, an adhesion aid, a sensitizer, a thermal polymerization inhibitor, a thermal base generator, and a solvent.
[0093] The negative photosensitive resin composition of the present disclosure may contain a thermal polymerization initiator. A thermal polymerization initiator is a compound that generates radicals by heat, and examples thereof include organic peroxides such as dialkyl peroxides, diacyl peroxides, peroxy esters, and peroxy ketals, and azo-based polymerization initiators such as azonitriles, azo esters, and azo amides. Among these, dialkyl peroxides and diacyl peroxides (e.g., dicumyl peroxide) are preferred from the viewpoint of chemical resistance.
[0094] When the negative type photosensitive resin composition of the present disclosure contains a thermal polymerization initiator, the content thereof is preferably 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide. From the viewpoint of chemical resistance, the lower limit of the content of the thermal polymerization initiator is more preferably 0.5 parts by mass or more per 100 parts by mass of the (A) polyimide. From the viewpoint of storage stability of the negative photosensitive resin composition, the upper limit of the content of the thermal polymerization initiator is more preferably 5 parts by mass or less per 100 parts by mass of the (A) polyimide.
[0095] The negative photosensitive resin composition of the present disclosure may contain a plasticizer. Examples of the plasticizer include phthalate ester compounds such as bis(2-ethylhexyl) phthalate, dicyclohexyl phthalate, and diphenyl phthalate, Isophthalic acid ester compounds such as bis(2-ethylhexyl) isophthalate, dicyclohexyl isophthalate, and diphenyl isophthalate, Terephthalate ester compounds such as bis(2-ethylhexyl) terephthalate, dicyclohexyl terephthalate, and diphenyl terephthalate, Trimellitic acid ester compounds such as tris(2-ethylhexyl) trimellitate, tricyclohexyl trimellitate, and triphenyl trimellitate, Pyromellitic acid compounds such as tetrakis(2-ethylhexyl) pyromellitic acid, tetracyclohexyl pyromellitic acid, and tetraphenyl pyromellitic acid, Malonic acid ester compounds such as bis(2-ethylhexyl) malonate, dicyclohexyl malonate, and diphenyl malonate, Succinic acid ester compounds such as bis(2-ethylhexyl) succinate, dicyclohexyl succinate, and diphenyl succinate, Glutarate ester compounds such as bis(2-ethylhexyl) glutarate, dicyclohexyl glutarate, and diphenyl glutarate, Adipic acid ester compounds such as bis(2-ethylhexyl) adipate, dicyclohexyl adipate, and diphenyl adipate, Pimelic acid ester compounds such as bis(2-ethylhexyl) pimelate, dicyclohexyl pimelate, and diphenyl pimelate, Suberic acid ester compounds such as bis(2-ethylhexyl) suberate, dicyclohexyl suberate, and diphenyl suberate, Azelaic acid ester compounds such as bis(2-ethylhexyl) azelaate, dicyclohexyl azelaate, and diphenyl azelaate, Sebacic acid ester compounds such as bis(2-ethylhexyl) sebacate, dicyclohexyl sebacate, and diphenyl sebacate, aliphatic acid tetrahydrofurfuryl compounds, such as tetrahydrofurfuryl propionate, tetrahydrofurfuryl butyrate, and tetrahydrofurfuryl isobutyrate; Acrylic polymers such as Disparlon 230 (manufactured by Kusunoki Chemical Industries, Ltd.) and Disparlon L-1983N (manufactured by Kusunoki Chemical Industries, Ltd.) Silicone compounds such as Disparlon 1711EF (Kusunoki Chemical Industries, Ltd.), Disparlon U-158 (Kusunoki Chemical Industries, Ltd.), Examples include fluorine-based compounds such as Disparlon U-160 (product name: manufactured by Kusunoki Chemical Co., Ltd.). Among these compounds, from the viewpoint of compatibility with the (A) polyimide, phthalate ester compounds, isophthalate ester compounds, terephthalate ester compounds, pyrrolimetic acid ester compounds, trimellitic acid ester compounds, malonate ester compounds, succinate ester compounds, glutaric acid ester compounds, adipic acid ester compounds, pimelic acid ester compounds, suberic acid ester compounds, azelaic acid ester compounds, sebacic acid ester compounds, and aliphatic acid tetrahydrofurfuryl compounds are preferred.
[0096] When the negative type photosensitive resin composition of the present disclosure contains a plasticizer, the content of the plasticizer is preferably 0.5 parts by mass or more and 40 parts by mass or less based on 100 parts by mass of the (A) polyimide. The lower limit of the plasticizer content is more preferably 1 part by mass or more per 100 parts by mass of the polyimide (A) from the viewpoint of flatness during coating. From the viewpoint of flatness during curing, the upper limit of the amount of the plasticizer is more preferably 30 parts by mass or less per 100 parts by mass of the polyimide (A).
[0097] The negative-type photosensitive resin composition of the present disclosure may optionally contain a hindered phenol compound to inhibit discoloration on copper surfaces. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenol), triethylenediamine, 1,6-Hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-Hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-Methylene-bis(4-methyl-6-t-butylphenol), 2,2'-Methylene-bis(4- Ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4- t-Butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-Dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H )-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-( 1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, but are not limited thereto. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione and the like are particularly preferred.
[0098] When the negative type photosensitive resin composition of the present disclosure contains a hindered phenol compound, the content thereof is preferably 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the (A) polyimide. The lower limit of the content of the hindered phenol compound is more preferably 0.5 parts by mass or more per 100 parts by mass of the (A) polyimide, because discoloration and corrosion of the copper or copper alloy are prevented when the negative photosensitive resin composition is formed on the copper or copper alloy. The upper limit of the content of the hindered phenol compound is more preferably 10 parts by mass or less per 100 parts by mass of the (A) polyimide, from the viewpoint of photosensitivity.
[0099] In order to improve the adhesion between the film formed by using the negative photosensitive resin composition and the substrate, the negative photosensitive resin composition of the present disclosure may contain other adhesive aids in addition to the silane coupling agent. As the other adhesive aids, aluminum-based adhesive aids and the like can be used.
[0100] Examples of aluminum-based adhesion promoters include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0101] When the negative type photosensitive resin composition of the present disclosure contains an adhesion aid, the content of the adhesion aid is preferably 0.01 parts by mass or more and 25 parts by mass or less based on 100 parts by mass of the (A) polyimide. From the viewpoint of adhesion, the lower limit of the content of the adhesion aid is more preferably 0.5 parts by mass or more per 100 parts by mass of the (A) polyimide. The upper limit of the content of the adhesion promoter is more preferably 20 parts by mass or less per 100 parts by mass of the (A) polyimide, from the viewpoint of storage stability of the negative photosensitive resin composition.
[0102] The negative type photosensitive resin composition of the present disclosure may optionally contain a sensitizer to improve photosensitivity. Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, and p-dimethylaminocinnamylideneindanone. p-Dimethylaminobenzylideneindanone, 2-(p-Dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-Dimethylaminophenylvinylene)benzothiazole, 2-(p-Dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetate
[0043] Examples of the mercaptobenzoyl compounds include 1-phenyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, Np-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, and 2-(p-dimethylaminobenzoyl)styrene. These may be used alone or in combination of two to five kinds, for example.
[0103] When the negative type photosensitive resin composition of the present disclosure contains a sensitizer for improving photosensitivity, the content of the sensitizer is preferably 0.1 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0104] The negative-type photosensitive resin composition of the present disclosure may optionally contain a thermal polymerization inhibitor in order to improve the stability of viscosity and photosensitivity, particularly when stored in the form of a solution containing a solvent. Examples of the thermal polymerization inhibitor that can be used include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0105] The negative type photosensitive resin composition of the present disclosure may optionally contain a thermal base generator.
[0106] The negative type photosensitive resin composition of the present disclosure may optionally contain a solvent (I). The solvent (I) is not limited as long as it can uniformly dissolve or suspend the polyimide (A) and the photopolymerization initiator (C). Examples of the solvent (I) include γ-butyrolactone (GBL), dimethyl sulfoxide, tetrahydrofurfuryl alcohol, ethyl acetoacetate, N,N-dimethylacetoacetamide, ε-caprolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide. These solvents (I) may be used alone or in combination of two or more.
[0107] The solvent (I) can be used in an appropriate amount depending on the desired coating thickness and viscosity of the negative photosensitive resin composition. The content of the solvent (I) is, for example, in the range of 30 to 1,000 parts by mass, preferably 140 to 1,000 parts by mass, based on 100 parts by mass of the polyimide (A).
[0108] When the solvent (I) contains an alcohol having no olefinic double bond, the content of the alcohol having no olefinic double bond in the total solvent including the reaction solvent is preferably 5 to 50 mass%. From the viewpoint of storage stability of the negative photosensitive resin composition, the upper limit of the content of the solvent (I) is more preferably 10 mass% or more in the total solvent. From the viewpoint of solubility of the (A) polyimide, the lower limit of the content of the solvent (I) is more preferably 30 mass% or less in the total solvent.
[0109] <Method for Producing Cured Relief Pattern> The method of producing a cured relief pattern of the present disclosure includes: (1) a step of applying the above-described negative photosensitive resin composition of the present disclosure onto a substrate to form a photosensitive resin layer on the substrate (a resin layer forming step); (2) a step of exposing the photosensitive resin layer to light (exposure step); (3) developing the exposed photosensitive resin layer to form a relief pattern (relief pattern formation step); (4) a step of heat-treating the relief pattern to form a hardened relief pattern (hardened relief pattern forming step); Includes.
[0110] (1) Resin layer formation process In this step, the negative photosensitive resin composition of the present disclosure is applied onto a substrate, and then dried, if necessary, to form a photosensitive resin layer. As the coating method, a method that has conventionally been used for coating a negative photosensitive resin composition, such as a coating method using a spin coater, a bar coater, a blade coater, a curtain coater, a screen printing machine, or the like, or a spray coating method using a spray coater, can be used.
[0111] If necessary, the coating film containing the negative photosensitive resin composition can be dried. Drying methods that can be used include air drying, heat drying using an oven or a hot plate, vacuum drying, etc. Specifically, in the case of air drying or heat drying, drying can be performed under conditions of 20°C to 150°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on a substrate. The thickness of the coating film (hereinafter referred to as the film thickness) may be appropriately adjusted depending on the desired thickness of the polyimide film and the content of the polyimide (A) in the photosensitive resin composition, and is preferably about 1 to 500 μm, and particularly preferably about 3 to 100 μm.
[0112] (2) Exposure process In this process, the photosensitive resin layer is exposed to an ultraviolet light source or the like through a patterned photomask or reticle or directly using an exposure device such as a contact aligner, mirror projection, or stepper. This exposure causes the polymerizable functional groups of the polyimide (A) contained in the negative photosensitive resin composition to crosslink due to the action of the photopolymerization initiator (C). This crosslinking makes the exposed portion insoluble in the developer described below, making it possible to form a relief pattern.
[0113] After the exposure, for the purpose of improving the photosensitivity, etc., a post-exposure bake (PEB) or a pre-development bake, or both, may be performed at any combination of temperature and time, as necessary. The baking conditions are preferably a temperature of 40° C. to 120° C. and a time of 10 seconds to 240 seconds, but are not limited to these ranges as long as they do not impair the various properties of the negative-type photosensitive resin composition of the present disclosure.
[0114] (3) Relief pattern formation process In this step, the unexposed areas of the photosensitive resin layer after exposure are developed and removed to form a relief pattern. As a developing method for developing the photosensitive resin layer after exposure (irradiation), any method can be selected from conventionally known photoresist developing methods, such as a rotary spray method, a paddle method, an immersion method accompanied by ultrasonic treatment, etc. After development, for the purpose of adjusting the shape of the relief pattern, etc., post-development baking may be performed at any combination of temperature and time, as necessary.
[0115] The developer used for development is preferably, for example, a good solvent for the negative photosensitive resin composition, or a combination of a good solvent and a poor solvent. Preferred good solvents include, for example, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, and α-acetyl-γ-butyrolactone. As the poor solvent, for example, toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, water, etc. are preferable. When a good solvent and a poor solvent are used in combination, it is preferable to adjust the ratio of the good solvent to the poor solvent depending on the solubility of the polymer in the negative photosensitive resin composition. The developer can be used in combination of two or more kinds, for example, several kinds of good solvents and poor solvents.
[0116] (4) Hardened relief pattern formation process In this step, the relief pattern obtained by development is subjected to a heat treatment to disperse the photosensitive component, thereby forming a cured relief pattern made of polyimide. The heat treatment method can be selected from various methods, such as using a hot plate, an oven, or a temperature-programmable heating oven. The heat treatment can be carried out, for example, at 160° C. to 350° C. for 30 minutes to 5 hours. The temperature of the heat treatment is preferably 300° C. or lower, more preferably 250° C. or lower, and particularly preferably 200° C. or lower. The atmospheric gas during heat curing may be air, or an inert gas such as nitrogen or argon may also be used.
[0117] The photosensitive resin layer after exposure has a crosslinked structure formed by crosslinking (A) the polymerizable functional group of the polyimide and (B) the polymerizable compound having a urea bond.
[0118] <Polyimide cured film> The present disclosure also provides a cured film formed from the negative photosensitive resin composition of the present disclosure. The cured film of the present disclosure includes a cured product of the negative photosensitive resin composition of the present disclosure.
[0119] <Semiconductor device> The present disclosure also provides a semiconductor device having a cured relief pattern obtained from the above-mentioned negative photosensitive resin composition. More specifically, a semiconductor device having a substrate that is a semiconductor element and a cured relief pattern is provided. The cured relief pattern may be produced by the above-mentioned method for producing a cured relief pattern using the above-mentioned negative photosensitive resin composition.
[0120] The present disclosure also provides a method for manufacturing a semiconductor device, using a semiconductor element as a substrate and including the method for manufacturing a cured relief pattern of the present embodiment as part of the steps. In this case, the cured relief pattern formed by the method for manufacturing a cured relief pattern of the present disclosure can be formed as a surface protective film, an interlayer insulating film, an insulating film for rewiring, a protective film for a flip chip device, or a protective film for a semiconductor device having a bump structure, or the like, and can be manufactured by combining it with a known method for manufacturing a semiconductor device.
[0121] <Display device> The present disclosure also provides a display device comprising a display element and a cured film provided on the upper portion of the display element, the cured film being the above-mentioned cured relief pattern. Here, the cured relief pattern may be laminated in direct contact with the display element, or may be laminated with another layer sandwiched therebetween. The cured film can be applied to, for example, surface protection films, insulating films, planarizing films, etc. of TFT liquid crystal display elements and color filter elements; protrusions for MVA type liquid crystal display devices; partition walls for cathodes of organic EL elements; and the like.
[0122] The negative photosensitive resin composition of the present disclosure is useful not only for application to the semiconductor device described above, but also for applications such as interlayer insulation in multilayer circuits, cover coats for flexible copper-clad boards, solder resist films, and liquid crystal alignment films.
[0123] <Method for producing negative type photosensitive resin composition> In one embodiment, the method for producing a negative type photosensitive resin composition of the present disclosure includes a step of producing (A) a polyimide having a polymerizable functional group at its terminal by the method of the present disclosure as described above in the "Method for producing a polyimide having a polymerizable functional group at its terminal". In one embodiment, the method for producing a negative type photosensitive resin composition of the present disclosure includes a step of mixing (A) a polyimide having a polymerizable functional group at an end, (B) a polymerizable compound having a urea bond, and (C) a photopolymerization initiator to obtain a negative type photosensitive resin composition (hereinafter, a mixing step). The mixing step is a step of mixing the above-mentioned (A) polyimide having a polymerizable functional group at its end, (B) polymerizable compound having a urea bond, (C) photopolymerization initiator, and (I) solvent to obtain a photosensitive resin composition solution. In the mixing step, the descriptions regarding (A) polyimide having a polymerizable functional group at its terminal, (B) polymerizable compound having a urea bond, (C) photopolymerization initiator, and (I) solvent are the same as those described above.
[0124] Optionally, it may further contain a monomer having a polymerizable functional group without the (D) urea bond described above (in one embodiment, a radically polymerizable compound), (E) a silane coupling agent, (F) an organotitanium compound, (G) a thermal crosslinking agent, an additive selected from (H) a rust inhibitor, and other components.
Examples
[0125] Hereinafter, the present embodiment will be specifically described by way of examples, but the present embodiment is not limited thereto. In the examples, comparative examples, production examples, and synthesis examples, the physical properties of the polyimide, polyimide precursor, or negative photosensitive resin composition were measured and evaluated according to the following methods.
[0126] <Measurement and Evaluation Methods> (1) Measurement of weight average molecular weight (Mw) and number average molecular weight (Mn) The weight average molecular weight (Mw) and number average molecular weight (Mn) of each resin were measured by gel permeation chromatography (GPC) under the following conditions. The molecular weight distribution was calculated as Mw / Mn. A calibration curve for calculating the weight average molecular weight was prepared using standard polystyrene (Easical Type PS-1, manufactured by Agilent Technologies).
[0127] <GPC Conditions> Apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Eluent: N-methyl-2-pyrrolidone Lithium bromide monohydrate 30 mmol / L Phosphoric acid 50 mmol / L Flow rate: 0.5 mL / min Columns: 2 TSK-GEL SUPER HM-H / 1 TSK-GEL SUPER H-RC (manufactured by Tosoh Corporation) Column temperature: 40 °C Detector: UV-8320
[0128] (2) Evaluation of low curing shrinkage: Method for measuring curing shrinkage rate A negative photosensitive resin composition described below was spin-coated onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.), and pre-baked on a hot plate at 110° C. for 240 seconds to form a pre-cured film having a thickness of approximately 7 μm. This film was irradiated with 800mJ / cm using Prisma GHI (Ultratech). 2 The applied energy was then irradiated to the coating. The coating was then cured by post-baking for 120 minutes at 170° C. in a nitrogen atmosphere using a temperature-ramp programmable curing oven (VF-2000 model, manufactured by Koyo Lindberg Co., Ltd.) to prepare a cured film (in one embodiment, a cured membrane) having a thickness of 6 μm. The thickness of the obtained film after pre-baking was defined as thickness A, and the thickness of the film after post-baking was defined as thickness B. The thicknesses A and B were substituted into the following formula to calculate the cure shrinkage rate. Curing shrinkage rate [%] = {(film thickness A - film thickness B) / film thickness A} x 100
[0129] (3) Evaluation of heat resistance: Method for measuring Tg of cured film The heat resistance of the post-baked film obtained by the method (2) above was measured by the following method. Using a thermomechanical analyzer (Seiko Instruments, product name: TMA / EXSTAR 6000), the obtained test piece (width 3 mm) was heated to 350°C at a heating rate of 10°C / min, and the thermal expansion coefficient of the obtained test piece was measured. Next, based on the obtained measurement results, the glass transition temperature (Tg) of the cured film was calculated from the inflection point of the thermal expansion coefficient. The unit of Tg is °C.
[0130] (4) Method for measuring the elongation of the cured film Using the post-baked film obtained by the method (2) above, the elongation of the cured film was measured by the following method. A tensile test was carried out on the obtained test piece using a tensile tester (manufactured by Orientec Co., Ltd., product name: Tensilon UTM-II-20) in an atmosphere of 23°C according to a method conforming to JIS K 7161, and the tensile elongation (elongation) of the test piece was measured. The stretching speed in the tensile test was 40 mm / min. The elongation of the cured film is expressed in %.
[0131] (5) Measurement and evaluation methods for copper adhesion A 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) was sputtered with a 200 nm thick Ti layer and a 400 nm thick Cu layer in that order using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Next, a photosensitive resin composition prepared by the method described below was spin-coated on the wafer using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.), and prebaked on a hot plate at 110° C. for 240 seconds to form a film on the Cu layer. This film was irradiated with 800mJ / cm using Prisma GHI (Ultratech). 2 Next, using a temperature-rise programmable curing furnace (VF-2000 model, manufactured by Koyo Lindberg), heat treatment was performed at 170°C for 2 hours under a nitrogen atmosphere to obtain a cured film of the photosensitive resin composition having a thickness of about 6 µm on the Cu. The heat-treated film was evaluated for adhesion between the copper substrate and the cured film according to the cross-cut method of JIS K 5600-5-6 standard, based on the following criteria. "Excellent": The lattice number of the cured film adhered to the substrate is more than 100. "Good": The lattice number of the cured film adhered to the substrate is between 80 and 100. "Acceptable": The number of lattices of the cured film adhered to the substrate is 50 or more and less than 80. "Not acceptable": The number of lattices of the cured film adhered to the substrate is less than 50.
[0132] (6) Measurement and evaluation methods for oxygen barrier properties The post-baked cured film obtained by the method (2) above was used to measure the oxygen barrier property by the following method. The oxygen permeability (cc / m) was measured using a gas permeability measuring device (GTR Tech Co., Ltd., product name: GTR-10XF (isobaric GC)) according to the isobaric GC method of JIS K 7126-2. 2 The oxygen barrier properties were evaluated based on the following criteria: "Excellent": Oxygen permeability (cc / m 2 ·24h·atm) is less than 200 "Good": Oxygen permeability (cc / m 2 ·24h·atm) is between 200 and 500 "Acceptable": Oxygen permeability (cc / m 2 ·24h·atm) is between 500 and 1000 "Not possible": Oxygen permeability (cc / m 2 ·24h·atm) is more than 1000
[0133] <Synthesis Example 1: Polyimide A-1> [ka] A Dean-Stark extraction apparatus was attached, and 148 g of N-methylpyrrolidone (hereinafter NMP) and 22.1 g (0.08 mol) of 6-(4-aminophenoxy)biphenyl-3-amine (hereinafter PDPE) were added and dissolved in a three-neck flask substituted with nitrogen, to which 14.9 g (0.06 mol) of bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (hereinafter BCD) and 43.8 g of toluene were added and heated to 180° C. After confirming that the theoretical amount of water (2.16 g) and the added toluene (43.8 g) were extracted in the Dean-Stark extraction apparatus, heating was stopped and the mixture was cooled to room temperature. The resulting reaction liquid was dropped into 2.0 kg of ethyl alcohol to precipitate the polymer, which was then filtered and dried in vacuum to obtain a polyimide powder. The obtained polyimide was dissolved by adding 148 g of NMP, and then 6.2 g (0.04 mol) of 2-methacryloyloxyethyl isocyanate (trade name: Karenz MOI, manufactured by Resonac Co., Ltd.) was added and stirred at room temperature for 10 hours to obtain a polymer solution. The obtained polymer solution was dropped into 2.0 kg of water to precipitate the polymer, which was then filtered and vacuum dried to obtain a powder of solvent-soluble polyimide A-1 having polymerizable functional groups at its ends. The molecular weight of A-1 was measured by gel permeation chromatography (standard polystyrene equivalent), and was found to be Mw 10300, Mn 7400, and Mw / Mn 1.39. The terminal modification rate was confirmed to be 99% from the integral ratio of proton NMR.
[0134] <Synthesis example: Polyimide A-2> The reaction was carried out in the same manner as in Synthesis Example 1, except that the amount of PDPE in Synthesis Example 1 was changed to 33.2 g (0.12 mol) and the amount of Karenz MOI was changed to 18.6 g (0.12 mol), to obtain a solvent-soluble polyimide A-2 having a polymerizable functional group at the end. The molecular weight of A-2 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 5300, Mn was 4800, and Mw / Mn was 1.10. The terminal modification rate was confirmed to be 98% from the integral ratio of proton NMR.
[0135] <Synthesis Example 3: Polyimide A-3> [ka] The reaction was carried out in the same manner as in Synthesis Example 1, except that the BCD in Synthesis Example 1 was changed to 18.6 g (0.06 mol) of 4,4'-oxydiphthalic dianhydride (hereinafter referred to as ODPA), to obtain a solvent-soluble polyimide A-3 having a polymerizable functional group at its end. The molecular weight of A-3 was measured by gel permeation chromatography (standard polystyrene equivalent), and was found to be Mw 12100, Mn 8600, and Mw / Mn 1.41. The terminal modification rate was confirmed to be 99% from the integral ratio of proton NMR.
[0136] <Synthesis Example 4: Polyimide A-4> The reaction was carried out in the same manner as in Synthesis Example 1, except that Karenz MOI in Synthesis Example 1 was changed to Karenz MOI-EG (manufactured by Resonac Co., Ltd.) 2-(2-methacryloyloxyethyloxy)ethyl isocyanate (8.0 g (0.04 mol)), to obtain a solvent-soluble polyimide A-4 having a polymerizable functional group at its end. The molecular weight of A-4 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 11,400, Mn was 8,500, and Mw / Mn was 1.34. The terminal modification rate was confirmed to be 100% from the integral ratio of proton NMR.
[0137] <Synthesis Example 5: Polyimide A-5> The reaction was carried out in the same manner as in Synthesis Example 1, except that Karenz MOI in Synthesis Example 1 was changed to Karenz AOI (manufactured by Resonac Co., Ltd.) 5.6 g (0.04 mol) of 2-acryloyloxyethyl isocyanate, to obtain a solvent-soluble polyimide A-5 having a polymerizable functional group at its end. The molecular weight of A-5 was measured by gel permeation chromatography (standard polystyrene equivalent), and was found to be Mw 10600, Mn 7700, and Mw / Mn 1.38. The terminal modification rate was confirmed to be 100% from the integral ratio of proton NMR.
[0138] <Synthesis Example 6: Polyimide A-6> The reaction was carried out in the same manner as in Synthesis Example 1, except that Karenz MOI in Synthesis Example 1 was changed to Karenz BEI (manufactured by Resonac Corporation) (trade name) 9.6 g (0.04 mol) of 1,1-(bisacryloyloxymethyl)ethyl isocyanate, to obtain a solvent-soluble polyimide A-6 having a polymerizable functional group at its end. The molecular weight of A-6 was measured by gel permeation chromatography (standard polystyrene equivalent), and was found to be Mw 11900, Mn 8800, and Mw / Mn 1.35. The terminal modification rate was confirmed to be 98% from the integral ratio of proton NMR.
[0139] <Synthesis Example 7: Polyimide A-7> The reaction was carried out in the same manner as in Synthesis Example 1, except that the amount of PDPE in Synthesis Example 1 was changed to 17.5 g (0.06 mol) and the amount of Karenz MOI was changed to 1.0 g (0.006 mol), to obtain a solvent-soluble polyimide A-7 having a polymerizable functional group at the end. The molecular weight of A-7 was measured by gel permeation chromatography (standard polystyrene equivalent), and the Mw was 38700, the Mn was 27100, and the Mw / Mn was 1.43. The terminal modification rate was confirmed to be 99% from the integral ratio of proton NMR.
[0140] <Synthesis example: Polyimide A-8> The reaction was carried out in the same manner as in Synthesis Example 1, except that the amount of PDPE in Synthesis Example 1 was changed to 49.7 g (0.18 mol) and the amount of Karenz MOI was changed to 37.2 g (0.24 mol), to obtain a solvent-soluble polyimide A-8 having a polymerizable functional group at the end. The molecular weight of A-8 was measured by gel permeation chromatography (standard polystyrene equivalent), and the Mw was 2900, the Mn was 2700, and the Mw / Mn was 1.07. The terminal modification rate was confirmed to be 99% from the integral ratio of proton NMR.
[0141] <Synthesis Example 9: Polyimide A-9> [ka] The reaction was carried out in the same manner as in Synthesis Example 1, except that Karenz MOI was not added, to obtain a solvent-soluble polyimide A-9 having no polymerizable functional group at the end. The molecular weight of A-9 was measured by gel permeation chromatography (standard polystyrene equivalent), and was found to be Mw 10200, Mn 7200, and Mw / Mn 1.42. The terminal modification rate was confirmed to be 0% from the integral ratio of proton NMR.
[0142] <Synthesis Example 10: Polyimide Precursor A-10> 18.6g (0.06mol) of ODPA was placed in a 1L separable flask and 60g of γ-butyrolactone was added. Next, 15.6g (0.12mol) of 2-hydroxyethyl methacrylate was added, and 9.5g (0.12mol) of pyridine was added while stirring. The mixture was stirred at 40°C for 5 hours using an oil bath to obtain a reaction mixture. After the reaction was completed, the mixture was allowed to cool to room temperature and left to stand for 16 hours. Next, while stirring the resulting reaction mixture, a solution of 24.2 g (0.12 mol) of N,N'-dicyclohexylcarbodiimide dissolved in 30 g of γ-butyrolactone was added over 40 minutes under ice cooling, followed by a solution of 22.1 g (0.08 mol) of PDPE dissolved in 90 g of γ-butyrolactone added over 60 minutes. After stirring at room temperature for 2 hours, 180 g of ethyl alcohol was added and stirred for another hour, and then 140 g of γ-butyrolactone was added. The reaction mixture was filtered to remove the precipitate generated in the reaction system, and a reaction solution was obtained. The resulting reaction solution was added to 1.4 kg of ethyl alcohol to precipitate a crude polymer. The precipitated crude polymer was filtered and dissolved in 180 g of γ-butyrolactone to obtain a crude polymer solution. The resulting crude polymer solution was dropped into 2.0 kg of water to reprecipitate the polymer. The resulting reprecipitate was filtered and then vacuum dried to obtain a powdered polyimide precursor A-10. The molecular weight of A-10 was measured by gel permeation chromatography (standard polystyrene equivalent), and was found to be Mw 12,700, Mn 6,900, and Mw / Mn 1.84.
[0143] <Synthesis example 11:B-1> [ka] 27.6 g (0.10 mol) of PDPE was placed in a 300 mL separable flask, and 58.6 g of NMP was added thereto. While stirring and cooling with ice, 31.0 g (0.20 mol) of Karenz MOI 2-methacryloyloxyethyl isocyanate was added, and the mixture was stirred at room temperature for 10 hours to obtain an NMP solution of polymerizable compound B-1 having a urea bond. The denaturation rate of B-1 was confirmed to be 100% based on the integral ratio of proton NMR.
[0144] <Synthesis example 12:B-2> The reaction was carried out in the same manner as described in Synthesis Example 11, except that Karenz MOI in Synthesis Example 11 was replaced with Karenz MOI-EG: 2-(2-methacryloyloxyethyloxy)ethyl isocyanate 39.8 g (0.20 mol), to obtain a NMP solution of polymerizable compound B-2 having a urea bond. The degree of modification of B-2 was confirmed to be 100% based on the integral ratio of proton NMR.
[0145] <Synthesis example 13:B-3> The reaction was carried out in the same manner as described in Synthesis Example 11, except that Karenz MOI in Synthesis Example 11 was replaced with Karenz AOI: 2-acryloyloxyethyl isocyanate 28.2 g (0.20 mol), to obtain an NMP solution of polymerizable compound B-3 having a urea bond. The degree of modification of B-3 was confirmed to be 100% based on the integral ratio of proton NMR.
[0146] <Synthesis example 14:B-4> The reaction was carried out in the same manner as described in Synthesis Example 11, except that Karenz MOI in Synthesis Example 11 was replaced with Karenz BEI: 1,1-(bisacryloyloxymethyl)ethyl isocyanate 47.8 g (0.20 mol), to obtain a NMP solution of polymerizable compound B-4 having a urea bond. The degree of modification of B-4 was confirmed to be 100% based on the integral ratio of proton NMR.
[0147] <Synthesis example 15:B-5> A reaction was carried out in the same manner as in Synthesis Example 11, except that the PDPE in Synthesis Example 11 was changed to 20.0 g (0.10 mol) of 4,4'-diaminodiphenyl ether, to obtain an NMP solution of a polymerizable compound B-5 having a urea bond. The modification rate of B-5 was confirmed to be 100% based on the integral ratio of proton NMR.
[0148] Example 1 (Preparation of negative photosensitive resin composition) Negative photosensitive resin compositions were prepared by the following method, and the prepared compositions were evaluated. (A) 100g of A-1 as a polyimide having a polymerizable functional group at the end, (B) 10g of B-1 as a polymerizable compound having a urea bond, (C) 2g of TR-PBG-3057 (trade name, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) as a photopolymerization initiator (C-1) were dissolved in 208g of N-methyl-2-pyrrolidone (NMP) as a solvent (I-1) to obtain a negative photosensitive resin composition having a total solid content of 35% by mass. The composition was evaluated according to the above-mentioned method. The results are shown in Table 1. Unless otherwise specified, the units of the values shown in the tables are parts by mass.
[0149] <Examples 1 to 28 and Comparative Examples 1 to 3> A negative type photosensitive resin composition similar to that in Example 1 was prepared, except that the polymer and other additives (B) to (I) shown in Table 1 were used, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0150] [Table 1-1]
[0151] [Table 1-2]
[0152] [Table 1-3]
[0153] [Table 1-4]
[0154] <Other additives> C-1:TR-PBG-3057 (Product name; Changzhou Strong Electronic New Materials Co., Ltd.) C-2:TR-PBG-304 (Product name; Changzhou Strong Electronic New Materials Co., Ltd.) D-1: Tetraethylene glycol dimethacrylate D-2: Tris-(2-acryloxyethyl) isocyanurate D-3: Pentaerythritol tetraacrylate E-1: N-phenyl-3-aminopropyltrimethoxysilane E-2: 3-glycidoxypropyltrimethoxysilane F-1: Titanium(IV) oxide acetylacetonate G-1: 1,3-bis(methoxymethyl)urea G-2: 1,3,4,6-tetrakis(methoxymethyl)glycoluril H-1:8-azaadenine H-2: 5-amino-1H-tetrazole I-1: N-methyl-2-pyrrolidone
[0155] Looking at the evaluation results in Table 1, Comparative Examples 1 to 3, which do not satisfy the requirements of the present disclosure, are unable to achieve good performance in all of the following areas in a balanced manner: low cure shrinkage, heat resistance, elongation of the cured film, copper adhesion, and oxygen barrier properties. On the other hand, Examples 1 to 28 show excellent performance in all of low cure shrinkage, heat resistance, elongation of the cured film, copper adhesion, and oxygen barrier properties.
[0156] In the present disclosure, excellent performance means that the cure shrinkage is 6% or less, the heat resistance is 235°C or more, the elongation of the cured film is 20% or more, and the copper adhesion and oxygen barrier properties are "fair" or better. [Industrial Applicability]
[0157] By using the photosensitive resin composition according to the present invention, it is possible to obtain a photosensitive resin composition having low cure shrinkage and excellent film properties after low-temperature curing, such as heat resistance, mechanical strength (elongation of the cured film), adhesion to copper, and oxygen blocking property, as well as a method for producing a cured relief pattern and a polyimide cured film using the same. The present invention can be suitably used in the field of photosensitive materials useful for producing electric and electronic materials such as semiconductor devices and multilayer wiring boards.
Claims
1. (A) a polyimide having a polymerizable functional group at its terminal; (B) a polymerizable compound having a urea bond, and (C) Photopolymerization initiator A negative type photosensitive resin composition comprising:
2. The negative type photosensitive resin composition according to claim 1 , wherein the polyimide (A) has no polymerizable functional group in a side chain.
3. The (A) polyimide and the (B) polymerizable compound have a structure derived from the same diamine, The negative photosensitive resin composition according to claim 1 or 2.
4. 3. The negative type photosensitive resin composition according to claim 1, wherein the content of the polymerizable compound (B) is 0.1 to 50 parts by mass relative to 100 parts by mass of the polyimide (A).
5. 3. The negative type photosensitive resin composition according to claim 1, wherein the weight average molecular weight Mw of the polyimide (A) is 3,000 or more and 30,000 or less.
6. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (D) a monomer having a polymerizable functional group having no urea bond.
7. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (E) a silane coupling agent.
8. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (F) an organotitanium compound.
9. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (G) a thermal crosslinking agent.
10. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (H) a rust inhibitor.
11. The following steps: (1) applying the negative type photosensitive resin composition according to claim 1 or 2 onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat treating the relief pattern to form a hardened relief pattern; 2. A method for producing a cured relief pattern comprising:
12. The negative photosensitive resin composition was post-baked at 170° C. for 120 minutes in a nitrogen atmosphere to obtain a cured film having a thickness of 6 μm, and the oxygen permeability (cc / m 2 3. The negative type photosensitive resin composition according to claim 1 or 2, wherein the viscosity (T / 24h atm) is less than 1,000.
Citation Information
Patent Citations
Photosensitive resin composition, method for producing electronic device, and electronic device
JP2021162834A
Negative photosensitive resin composition and method for manufacturing cured relief pattern using the same
JP2022091355A
Cited By
Photosensitive resin composition, cured product, and semiconductor device
WO2025142647A1