Fine cellulose fiber and fiber composite body
By chemically modifying and controlling the sedimentation behavior of fine cellulose fibers, the issue of aggregate formation in resin composites is resolved, resulting in improved physical properties through enhanced dispersion.
Patent Information
- Application Number
- JP2024146319
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2039-10-21
AI Technical Summary
Conventional techniques struggle with achieving uniform dispersion of fine cellulose fibers in resins, leading to aggregate formation that degrades the physical properties of resin composites.
Control the sedimentation behavior of fine cellulose fibers in a specific concentration by chemically modifying them and controlling the sedimentation height ratio, ensuring they remain well-defibrated and moderately entangled to prevent aggregation.
The modified fine cellulose fibers maintain excellent dispersion in resins, enhancing the physical properties of resin composites without forming aggregates, even at low concentrations.
Smart Images

Figure 2024163130000003 
Figure 2024163130000004 
Figure 2024163130000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a fine cellulose fiber and a resin composite. [Background technology]
[0002] Thermoplastic resins are lightweight and have excellent processability, and are therefore widely used in a wide range of applications, including automotive components, electrical and electronic components, office equipment housings, precision parts, etc. However, resins alone often lack sufficient mechanical properties and dimensional stability, and composites of resins and various fibrous materials are generally used.
[0003] In recent years, nanofibers, including fine cellulose fibers (also called cellulose nanofibers (CNF)), have come to be used as fibrous materials. CNF has a tendency to aggregate in a dry state, so it is produced as an aqueous dispersion that allows stable dispersion.
[0004] Various techniques for dispersing cellulose fibers in other materials have been proposed in the past. For example, Patent Document 1 describes a composition containing cellulose nanofibers and a block copolymer for the purpose of improving the dispersibility of cellulose in a resin, and Patent Document 2 describes a resin composition containing polyvinyl alcohol, polyvinylpyrrolidone, and a water-soluble resin consisting of a copolymer of these for the purpose of dispersing cellulose fibers with a high aspect ratio well in a resin composition. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6234037 [Patent Document 2] JP 2012-236906 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even with the above-mentioned conventional techniques, it is still difficult to disperse fine cellulose fibers sufficiently well in a resin. In particular, once agglomerates are formed in fine cellulose fibers, it is difficult to eliminate the agglomerates, and these agglomerates are a cause of a significant decrease or non-uniformity in the physical properties of a resin composite in which fine cellulose fibers are dispersed in a resin.
[0007] The present invention has an object to solve the above problems and to provide fine cellulose fibers which are less likely to form agglomerates and have a good effect of improving the physical properties of a resin composite. [Means for solving the problem]
[0008] As a result of intensive research into solving the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by controlling the sedimentation behavior of fine cellulose fibers in a dilute dispersion of a specific concentration, and thus completed the present invention. That is, the present invention includes the following aspects. [1] Fine cellulose fibers, The fine cellulose fibers have a ratio of the sedimentation height of the fine cellulose fibers to the total liquid height of the test dispersion (100%) of 6% or more when the test dispersion containing the fine cellulose fibers in water at a concentration of 0.05% by mass is allowed to stand at 23°C and normal pressure for 24 hours. [2] The fine cellulose fibers according to the above aspect 1, having an average fiber diameter of 2 to 1,000 nm. [3] The fine cellulose fibers according to the above embodiment 1 or 2, which are chemically modified. [4] The fine cellulose fibers according to the above-mentioned aspect 3, wherein the chemical modification is acylation. [5] Fine cellulose fibers according to any one of the above aspects 1 to 4, having a weight average molecular weight (Mw) of 100,000 or more and a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 6 or less. [6] The fine cellulose fibers according to any one of the above aspects 1 to 5, having an average alkali-soluble polysaccharide content of 12% by mass or less and a crystallinity of 60% or more. [7] A dried material comprising the fine cellulose fibers according to any one of aspects 1 to 6. [8] The dried body according to claim 7, having a moisture content of 50% by mass or less. [9] A resin composite comprising the fine cellulose fiber according to any one of the above aspects 1 to 6 and a resin.
[10] A method for producing fine cellulose fibers according to any one of the above aspects 1 to 6, A cellulose raw material is beaten and then defibrated with a homomixer to obtain a fine cellulose fiber slurry; Optionally, drying the fine cellulose fiber slurry under reduced pressure while stirring; A method comprising:
[11] A method for producing the dried body according to aspect 7 or 8, comprising the steps of: A cellulose raw material is beaten and then defibrated with a homomixer to obtain a fine cellulose fiber slurry; Drying the fine cellulose fiber slurry under reduced pressure while stirring; and Optionally, mixing the microfine cellulose fiber slurry and / or the microfine cellulose fibers with additional ingredients; A method comprising:
[12] A method for producing the resin composite according to aspect 9, comprising the steps of: A cellulose raw material is beaten and then defibrated with a homomixer to obtain a fine cellulose fiber slurry; Optionally, drying the fine cellulose fiber slurry under reduced pressure while stirring; A process for producing fine cellulose fibers by a method comprising the steps of: A mixing step of mixing the fine cellulose fibers and the resin; A method comprising:
[13] The method according to any one of aspects 10 to 12 above, further comprising chemically modifying cellulose before, simultaneously with, and / or after the defibration. Effect of the Invention
[0009] According to one aspect of the present invention, it is possible to provide fine cellulose fibers which are less likely to form agglomerates and have a good effect of improving the physical properties of a resin composite. [Brief description of the drawings]
[0010] [Figure 1] 13 is an explanatory diagram of a method for calculating the IR index 1730 and the IR index 1030. FIG. [Diagram 2] FIG. 2 is an explanatory diagram of a method for calculating the average substitution degree of hydroxyl groups in cellulose. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Exemplary embodiments of the present invention will be described in detail below, but the present invention is not limited to these embodiments.
[0012] <Fine cellulose fiber> One aspect of the present invention provides fine cellulose fibers, in which the ratio of the settling height of the fine cellulose fibers to the total liquid height of the test dispersion (100%) is 6% or more when the test dispersion containing the fine cellulose fibers in water at a concentration of 0.05% by mass is left to stand at 23°C and normal pressure for 24 hours. The fine cellulose fibers refer to cellulose defibrated by a method of mechanically finely pulverizing a cellulose raw material using a refiner, a high-pressure homogenizer, a ball mill, a homomixer, or the like. Fine cellulose fibers are usually very prone to aggregation and have strong interactions between fibers, making it difficult to disperse them well in a resin. The present inventor unexpectedly discovered that fine cellulose fibers that exhibit a high settling height in a specific dilute aqueous dispersion of 0.05% by mass can maintain a suitable space between the fibers, making it difficult to form aggregates and can be dispersed well in a resin, while being able to impart an excellent physical property improving effect to the resin due to the suitable entanglement between the fibers. Even when used in a relatively small amount, such fine cellulose fibers are excellent in improving the physical properties of a composite containing fine cellulose fibers and a resin (also referred to as a resin composite in the present disclosure). The fine cellulose fibers of the present disclosure may be present in a dispersion (i.e., a slurry) or as a dry body. The fine cellulose fibers may be chemically modified as described below. Examples of the dispersion include dispersions containing, for example, 0.001 to 2 mass%, or 0.01 to 1.5 mass%, or 0.1 to 1 mass% of fine cellulose fibers, with the remainder being a dispersion medium. The dispersion medium may be, for example, water and / or an organic solvent. Examples of the organic solvent include water-miscible organic solvents, such as polyols (e.g., polyether polyols such as polypropylene glycol and polyethylene glycol), ethanol, methanol, dimethylformamide, dimethyl sulfoxide, acetonitrile, acetone, acetic acid, and t-butanol.
[0013] The test dispersion is prepared by the following method. When the fine cellulose fibers are present in the form of a dispersion, the dispersion is converted into an aqueous dispersion with a fine cellulose fiber concentration of 0.05% by mass by solvent replacement and / or dilution or concentration to prepare the test dispersion. Concentration is performed by subjecting the dispersion to a filter cloth, membrane filter, centrifugation, etc. When the fine cellulose fibers are in a dry form, water is added and the fibers are redispersed using a homogenizer, etc. to prepare a test dispersion with a fine cellulose fiber concentration of 0.05% by mass.
[0014] The above ratio of the settling height is 6% or more in one aspect, and preferably 10% or more, or 15% or more, or 20% or more, or 25% or more, or 30% or more. A high ratio of the settling height is an indicator that the fine cellulose fibers are well defibrated, and that the fibers maintain a suitable space between each other and are unlikely to form agglomerates, while also having a suitable degree of entanglement. On the other hand, if the ratio is too high (for example, when the fine cellulose fibers are 100%, they are not settled), a network of the fine cellulose fibers is likely to be formed excessively, making it difficult to disperse them in the resin, and as a result, agglomerates are likely to be formed, which may lead to a decrease in the physical properties of the resin composite. From this viewpoint, the upper limit of the ratio may be 80% or less, 70% or less, 60% or less, 50% or less, or 40% or less.
[0015] The sedimentation height ratio is measured by measuring the transmittance of the dispersion at a wavelength of 850 nm (hereinafter also referred to as initial transmittance) using, for example, a liquid dispersion stability evaluation device Turbiscan (manufactured by Sanyo Trading Co., Ltd.). After leaving the test tube at rest for 24 hours at 23° C., the height from the bottom of the dispersion to the separation interface and the height from the bottom of the dispersion to the top of the dispersion are measured using the liquid dispersion stability evaluation device, with the height at which the transmittance becomes 50% at the above wavelength being defined as the separation interface, and the ratio is calculated using the following formula (1): Settlement height ratio (%) = ([A] / [B]) × 100 (1) (In formula (1), [A] is the height from the bottom of the dispersion to the separation interface, and [B] is the height from the bottom of the dispersion to the top of the dispersion.) In addition, when the height at which the above-mentioned permeability becomes 50% is not defined, the region with higher permeability than the above-mentioned initial permeability is defined as the supernatant part, and the region with lower permeability is defined as the sediment part, and the boundary between the supernatant part and the sediment part is defined as the separation interface, and the sedimentation height ratio is calculated according to the above-mentioned (1).
[0016] In one embodiment, the fine cellulose fiber of the present disclosure can be produced by a method including, for example, obtaining a fine cellulose fiber slurry by defibrating a cellulose raw material in dimethyl sulfoxide (also referred to as DMSO) using a homomixer, and optionally drying the fine cellulose fiber slurry under reduced pressure while stirring. When the cellulose raw material is dried under reduced pressure, the fine cellulose fiber of the present disclosure is obtained as a dry body. As a means for controlling the settling height, the above-mentioned cellulose raw material is subjected to a dry or wet pulverization treatment, and in one embodiment, a cellulose raw material having a length-weighted average fiber length of 5 mm or less, preferably 4 mm or less, or 3 mm or less, or 2 mm or less, or 1 mm or less is produced, and the cellulose raw material is refined in a wet manner. When the cellulose raw material is 5 mm or less, uniform fine cellulose fibers are obtained in the subsequent refinement step, and aggregation in water is suppressed. Although the mechanism of this action is not clear, if the cellulose fiber is too long, it becomes difficult to uniformly apply energy such as shear during defibration. The non-uniform fine cellulose fibers thus obtained have a large fiber diameter due to the presence of thick fibers, and are likely to be easily twisted and have poor dispersibility in water. The lower limit of the length-weighted average fiber length of the cellulose raw material is preferably 0.1 mm or more, or 0.2 mm or more, or 0.3 mm or more, or 0.4 mm or more, or 0.5 mm or more in order to prevent a decrease in crystallinity due to excessive pulverization. The length-weighted average fiber length of the cellulose raw material can be measured, for example, by an optical measurement method (see JAPAN TAPPI Paper and Pulp Test Method No. 52 (Pulp and Paper-Fiber Length Test Method-Optical Automatic Measurement Method) or JIS P 8226 (Pulp-Method of Measuring Fiber Length by Optical Automatic Analysis-Part 1: Polarized Light Method), JIS P 8226-2 (Pulp-Method of Measuring Fiber Length by Optical Automatic Analysis-Part 2: Non-Polarized Light Method)).
[0017] As the cellulose raw material, natural cellulose and regenerated cellulose can be used. As the natural cellulose, wood pulp obtained from wood species (broadleaf or coniferous), non-wood pulp obtained from non-wood species (cotton, bamboo, hemp, bagasse, kenaf, cotton linters, sisal, straw, etc.), and cellulose fiber aggregates produced by animals (e.g., ascidians), algae, and microorganisms (e.g., acetic acid bacteria) can be used. As the regenerated cellulose, regenerated cellulose fibers (viscose, cupra, tencel, etc.), cellulose derivative fibers, and ultrafine threads of regenerated cellulose or cellulose derivatives obtained by electrospinning can be used.
[0018] Since the cellulose raw material contains alkali-soluble and sulfuric acid-insoluble components (lignin, etc.), the alkali-soluble and sulfuric acid-insoluble components may be reduced by a purification process such as delignification by cooking and a bleaching process. On the other hand, the purification process such as delignification by cooking and the bleaching process cut the molecular chains of cellulose, changing the weight-average molecular weight and number-average molecular weight, so it is important that the purification process and bleaching process of the cellulose raw material control the weight-average molecular weight of cellulose and the ratio of the weight-average molecular weight to the number-average molecular weight so as not to deviate from appropriate ranges.
[0019] In addition, refining processes such as delignification by cooking and bleaching processes reduce the molecular weight of cellulose molecules, and there is concern that these processes will result in a lower molecular weight of cellulose and an increase in the proportion of alkali-soluble matter present due to the alteration of the cellulose raw material. Since alkali-soluble matter has poor heat resistance, it is important that the refining and bleaching processes of the cellulose raw material are controlled so that the amount of alkali-soluble matter contained in the cellulose raw material is within a certain range or less.
[0020] The cellulose raw material is obtained by a dry grinding process. Any type of grinder can be used in the dry grinding, but a high-speed rotary impact grinder is preferable because it can obtain a cellulose raw material with a good shape. A high-speed rotary impact grinder is a grinder that uses a pin rotating in a grinding chamber or a rotor with a special structure to impact or shear the cellulose raw material and grind it. In order to suppress fiber damage during dry grinding, the cellulose raw material may contain moisture to a certain extent based on its weight.
[0021] Examples of mills of this type include the Jiyuu mill, New Cosmomizer (manufactured by Nara Machinery Works, Ltd.), Victory Mill, Far in Victory Mill (manufactured by Hosokawa Micron, Ltd.), Turbo Mill (manufactured by Turbo Kogyo, Ltd.), Ultra Rotor (manufactured by WIR, Ltd.), Makino type mill, Ultraplex (manufactured by Makino Sangyo, Ltd.), Fine Mill (manufactured by Nippon Pneumatic Industry Co., Ltd.), Impeller Mill (manufactured by Seishin Enterprise Co., Ltd.), and Disc Refiner (manufactured by Aikawa Iron Works, Ltd.).
[0022] There is no particular limitation on the method for reducing the fiber diameter in order to convert the cellulose raw material into fine cellulose fibers, but it is preferable to make the defibration processing conditions (method of applying a shear field, shear field size, etc.) more efficient. In addition, in order to suppress the decrease in crystallinity due to shear, wet defibration using a solvent is preferable. There is no particular limitation on the defibration solvent, but examples include water and aprotic solvents. Water is preferable because it is an inexpensive solvent and does not require explosion-proofing of the production equipment. When the cellulose raw material is immersed in an aprotic solvent, cellulose swells in a short time, and the cellulose is pulverized by only applying slight stirring and shear energy. In addition, by adding a cellulose modifying agent before, during, or after pulverization, chemically modified fine cellulose fibers (also called chemically modified fine cellulose fibers) can be directly obtained without solvent replacement. Therefore, an aprotic solvent is preferable from the viewpoint of production efficiency.
[0023] Examples of the aprotic solvent include alkyl sulfoxides, alkyl amides, pyrrolidones, etc. These solvents may be used alone or in combination of two or more kinds.
[0024] Examples of the alkyl sulfoxides include di-C1-4 alkyl sulfoxides such as dimethyl sulfoxide (DMSO), methyl ethyl sulfoxide, and diethyl sulfoxide.
[0025] Examples of the alkylamides include N,N-diC1-4 alkylformamides such as N,N-dimethylformamide (DMF) and N,N-diethylformamide; and N,N-diC1-4 alkylacetamides such as N,N-dimethylacetamide (DMAc) and N,N-diethylacetamide.
[0026] Examples of pyrrolidones include pyrrolidones such as 2-pyrrolidone and 3-pyrrolidone; and N-C1-4 alkylpyrrolidones such as N-methyl-2-pyrrolidone (NMP).
[0027] These aprotic solvents can be used alone or in combination of two or more. Among these aprotic solvents, DMSO, DMF, DMAc, NMP, etc., especially DMSO, can be used to more efficiently produce chemically modified fine cellulose fibers. Although the mechanism of action is not necessarily clear, it is presumed to be due to uniform micro-swelling of the cellulose raw material in the aprotic solvent. In addition, since the swelling state of the cellulose raw material differs between water and aprotic solvents, which are generally used in the production of fine cellulose fibers, as described above, the fiber diameter and shape of the obtained fine cellulose fibers may differ. The fiber diameter and shape are related to the dispersion state and network formability in water or resin, and are also thought to affect the sedimentation height ratio.
[0028] The cellulose raw material can be pulverized using a device that effectively applies shear to the cellulose raw material, such as a disintegrator, a beater, a refiner, a low-pressure homogenizer, a high-pressure homogenizer, an ultra-high-pressure homogenizer, an emulsifier, a homomixer, a grinder, a mass colloider, a cutter mill, a ball mill, a bead mill, a jet mill, a single-screw extruder, a twin-screw extruder, an ultrasonic agitator, a household juicer mixer, etc. Among these, pulverization using a homomixer using an aprotic solvent is preferred because it can defibrate with low energy and also enables chemical modification of fine cellulose fibers in a non-aqueous system.
[0029] The procedure for pulverization in the homomixer includes, but is not limited to, the following. In one embodiment, the homomixer includes a first means for supplying the contents, a second means having a rotating element capable of generating a shear force and an ejection pressure on the contents from the first means, and optionally a third means capable of returning the contents from the second means to the first means. In one embodiment, the second means is disposed below the first means, and the contents are fed to the second means by the first means, and are returned to the first means via the third means by the discharge pressure of the second means, thereby making it possible to carry out cellulose defibration by shear force extremely efficiently. The first means may be an agitator such as a stirring propeller, and the agitator may have a scraper capable of scraping off the contents along the inner wall surface of the tank. The second means may be an ultra-high speed homogenizer (rotor / stator type) attached to the bottom of the tank, or the like. The second means can pulverize and disperse the contents to a sub-micron level by energy such as shear force and collision between solids. The third means may be a recirculation pipe or the like that delivers the contents from the second means (eg, the discharge from a homogenizer) to the top or middle of the tank and returns it to the first means.
[0030] In one embodiment, in the case of a homomixer with a tank capacity of 35 L or more, extremely low energy of rated power consumption of 0.5 to 80 kWh per kg of dry cellulose solids can be imparted to the cellulose raw material. Such low-energy defibration is preferable in that the settling height of the fine cellulose fibers can be easily controlled. In one embodiment, low-energy defibration using shear force by rotating the rotating element of the second means at a peripheral speed of 20 m / s to 80 m / s and preferably at 20°C to 90°C for 0.5 hours to 8 hours is preferable in that the settling height of the fine cellulose fibers can be easily controlled.
[0031] In one embodiment, the number average fiber diameter of the fine cellulose fibers is preferably 2 to 1000 nm from the viewpoint of obtaining a good effect of improving physical properties by the fine cellulose fibers. The number average fiber diameter of the fine cellulose fibers is more preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, and more preferably 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less.
[0032] From the viewpoint of satisfactorily improving the mechanical properties of a resin composite containing the fine cellulose fibers with a small amount of the fine cellulose fibers, the average L / D of the fine cellulose fibers is preferably 50 or more, or 80 or more, or 100 or more, or 120 or more, or 150 or more. There is no particular upper limit, but from the viewpoint of handleability, it is preferably 5000 or less.
[0033] In the present disclosure, the length, diameter, and L / D ratio of each of the fine cellulose fibers are determined by diluting an aqueous dispersion of the fine cellulose fibers with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.) to 0.01 to 0.1% by mass, dispersing the fibers using a high-shear homogenizer (e.g., manufactured by IKA, trade name "Ultra Turrax T18") under processing conditions: rotation speed 25,000 rpm x 5 minutes, casting the fibers on mica, and air-drying the fibers as measurement samples, and measuring the fibers with a high-resolution scanning electron microscope (SEM) or atomic force microscope (AFM). Specifically, the length (L) and diameter (D) of 100 randomly selected fibrous substances are measured in an observation field where the magnification is adjusted so that at least 100 fibrous substances are observed, and the ratio (L / D) is calculated. The number average value of the length (L), the number average value of the diameter (D), and the number average value of the ratio (L / D) of the fine cellulose fibers are calculated.
[0034] The length, diameter, and L / D ratio of the fine cellulose fibers in the resin composite described below can be confirmed by measuring the solid resin composite as a measurement sample using the above-mentioned measurement method. Alternatively, the length, diameter, and L / D ratio of the fine cellulose fibers in the resin composite can be confirmed by dissolving the resin components in the resin composite in an organic or inorganic solvent that can dissolve the resin components of the resin composite, separating the fine cellulose fibers, thoroughly washing with the solvent, and then replacing with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.), preparing a 0.01 to 0.1 mass% dispersion, and redispersing with a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18"). The redispersion can be confirmed by casting the redispersion on mica, air-drying it, and measuring it as a measurement sample using the above-mentioned measurement method. At this time, the measurement is performed on 100 or more randomly selected fine cellulose fibers.
[0035] The crystallinity of the fine cellulose fibers is preferably 55% or more. When the crystallinity is within this range, the mechanical properties (strength, dimensional stability) of the cellulose fibers themselves are high, and therefore when the cellulose fibers are dispersed in a resin, the strength and dimensional stability of the resin composite tend to be high. A more preferable lower limit of the crystallinity is 60%, even more preferably 70%, and most preferably 80%. There is no particular upper limit for the crystallinity of the fine cellulose fibers, and the higher the better, but from the viewpoint of production, a preferable upper limit is 99%.
[0036] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils of plant-derived cellulose and between the microfibril bundles. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in binding the microfibrils together by hydrogen bonding with cellulose. Lignin is also a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the fine cellulose fibers, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the resin composite during extrusion processing and molding processing, it is desirable to set the crystallinity of the fine cellulose fibers within the above-mentioned range.
[0037] The degree of crystallinity here, when the fine cellulose fibers are cellulose type I crystals (derived from natural cellulose), is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring a sample by wide-angle X-ray diffraction using the Segal method, according to the following formula: Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100
[0038] When the fine cellulose fibers are cellulose type II crystals (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of cellulose type II crystals in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100
[0039] Known crystalline forms of cellulose include type I, type II, type III, and type IV, among which types I and II are particularly widely used, and types III and IV are obtained on a laboratory scale but are not widely used on an industrial scale. As the fine cellulose fiber of the present disclosure, cellulose fibers containing cellulose type I crystals or cellulose type II crystals are preferred, since they have relatively high structural mobility and, by dispersing the fine cellulose fibers in a resin, a resin composite having a lower linear expansion coefficient and superior strength and elongation during tensile and bending deformation can be obtained, and fine cellulose fibers containing cellulose type I crystals and having a crystallinity of 55% or more are more preferred.
[0040] In addition, the degree of polymerization of the fine cellulose fibers is preferably 100 or more, more preferably 150 or more, more preferably 200 or more, more preferably 300 or more, more preferably 400 or more, and preferably 3500 or less, more preferably 3300 or less, more preferably 3200 or less, more preferably 3100 or less, more preferably 3000 or less.
[0041] From the viewpoint of processability and mechanical property expression, it is desirable that the polymerization degree of the fine cellulose fiber is within the above-mentioned range. From the viewpoint of processability, it is preferable that the polymerization degree is not too high, and from the viewpoint of mechanical property expression, it is desirable that the polymerization degree is not too low.
[0042] The degree of polymerization of the fine cellulose fibers means the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "15th Revised Japanese Pharmacopoeia Commentary (published by Hirokawa Shoten)."
[0043] In one embodiment, the weight average molecular weight (Mw) of the fine cellulose fiber is 100,000 or more, more preferably 200,000 or more, and even more preferably 250,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is 10 or less, or 9 or less, or 8 or less, or 7 or less, or 6 or less, and preferably 5.4 or less. The larger the weight average molecular weight, the smaller the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the smaller the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecule are the starting points of thermal decomposition, particularly high heat resistant fine cellulose fibers and resin composites containing fine cellulose fibers and resins can be obtained when the cellulose molecules of the fine cellulose fibers have not only a large weight average molecular weight but also a narrow molecular weight distribution width at the same time. The weight average molecular weight (Mw) of the fine cellulose fiber may be, for example, 1,000,000 or less, or 900,000 or less, or 800,000 or less, or 700,000 or less, or 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more, from the viewpoint of the ease of production of the fine cellulose fiber. Mw can be controlled to the above range by selecting a cellulose raw material having an Mw according to the purpose, appropriately performing physical treatment and / or chemical treatment on the cellulose raw material in an appropriate range, etc. Mw / Mn can also be controlled to the above range by selecting a cellulose raw material having an Mw / Mn according to the purpose, appropriately performing physical treatment and / or chemical treatment on the cellulose raw material in an appropriate range, etc. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, or the like, and physical treatments that apply mechanical forces such as impact, shear, friction, and the like using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, or the like, and examples of the chemical treatment include digestion, bleaching, acid treatment, and conversion to regenerated cellulose.
[0044] The weight average molecular weight and number average molecular weight of cellulose referred to here are values determined by dissolving cellulose in N,N-dimethylacetamide containing added lithium chloride and then subjecting the cellulose to gel permeation chromatography using N,N-dimethylacetamide as a solvent.
[0045] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of fine cellulose fibers include hydrolysis treatment. The hydrolysis treatment advances depolymerization of amorphous cellulose inside the fine cellulose fibers, decreasing the average degree of polymerization. At the same time, the hydrolysis treatment removes impurities such as hemicellulose and lignin in addition to the above-mentioned amorphous cellulose, making the inside of the fibers porous.
[0046] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of protonic acid, carboxylic acid, Lewis acid, heteropolyacid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions such as temperature, pressure, and time at this time vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., but are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which cellulose is treated for 10 minutes or more at 100°C or higher under pressure using an aqueous mineral acid solution of 2% by mass or less can be exemplified. Under these conditions, the catalyst component such as acid penetrates into the inside of the fine cellulose fibers, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.
[0047] Alkali-soluble polysaccharides that may be contained in fine cellulose fibers include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups and have poor heat resistance, and may cause inconveniences such as decomposition when exposed to heat, yellowing during heat aging, and a decrease in strength of cellulose fibers. Therefore, it is preferable that the content of alkali-soluble polysaccharides in fine cellulose fibers is low.
[0048] In one embodiment, the average content of alkali-soluble polysaccharides in the fine cellulose fibers is preferably 20% by mass or less, 18% by mass or less, 15% by mass or less, or 12% by mass or less, based on 100% by mass of the fine cellulose fibers, from the viewpoint of obtaining good dispersibility of the fine cellulose fibers. The content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more, from the viewpoint of ease of production of the fine cellulose fibers.
[0049] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.
[0050] In one embodiment, the average content of acid-insoluble components in the fine cellulose fibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, based on 100% by mass of the fine cellulose fibers, from the viewpoint of avoiding a decrease in heat resistance of the fine cellulose fibers and the associated discoloration. From the viewpoint of ease of production of the fine cellulose fibers, the content may be 0.01% by mass or more, 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.
[0051] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.
[0052] The fine cellulose fibers may be chemically treated (e.g., oxidized or chemically modified using a modifying agent). As an example, fine cellulose fibers obtained by oxidizing cellulose fibers with 2,2,6,6-tetramethylpiperidine-1-oxyl radical as shown in Cellulose (1998) 5, 153-164, followed by washing and mechanical fiberization, may be used.
[0053] The cellulose modification agent can be a compound that reacts with the hydroxyl group of cellulose, and includes an esterification agent, an etherification agent, and a silylating agent. In a preferred embodiment, the chemical modification is acylation using an esterification agent. The esterification agent is preferably an acid halide, an acid anhydride, a vinyl carboxylate, or a carboxylic acid.
[0054] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula (1). R1 -C(=O)-X (1) (In the formula, R 1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I. Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.
[0055] As the acid anhydride, any suitable acid anhydride can be used. For example, Saturated aliphatic monocarboxylic acid anhydrides, such as acetic acid, propionic acid, (iso)butyric acid, and valeric acid; unsaturated aliphatic monocarboxylic acid anhydrides, such as (meth)acrylic acid and oleic acid; Alicyclic monocarboxylic acid anhydrides such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Aromatic monocarboxylic acid anhydrides such as benzoic acid and 4-methylbenzoic acid; Examples of dibasic carboxylic acid anhydrides include saturated aliphatic dicarboxylic acid anhydrides such as succinic anhydride and adipic acid, unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride, alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride and methyltetrahydrophthalic anhydride, and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride. In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0056] The vinyl carboxylate may be represented by the following formula (1): R-COO-CH=CH2…Formula (1) Preferred is a vinyl carboxylate represented by the formula: {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl pivalate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.
[0057] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.
[0058] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.
[0059] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.
[0060] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.
[0061] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.
[0062] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formula (1). R-COOH …(1) (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)
[0063] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, pivalic acid, octylic acid, benzoic acid, and cinnamic acid.
[0064] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0065] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.
[0066] The degree of modification of the chemically modified fine cellulose fiber of this embodiment is expressed as the average degree of substitution of hydroxyl groups (also referred to as DS, the average number of hydroxyl groups substituted per glucose, which is the basic structural unit of cellulose). In one aspect, the DS of the chemically modified fine cellulose fiber is preferably 0.01 or more and 2.0 or less. If the DS is 0.01 or more, a resin composite containing chemically modified fine cellulose with a high thermal decomposition onset temperature can be obtained. On the other hand, if the DS is 2.0 or less, an unmodified cellulose skeleton remains in the chemically modified fine cellulose, so that a resin composite containing chemically modified fine cellulose having both high tensile strength and dimensional stability derived from cellulose and a high thermal decomposition onset temperature derived from chemical modification can be obtained. The DS is more preferably 0.05 or more, even more preferably 0.1 or more, particularly preferably 0.2 or more, and most preferably 0.3 or more, and more preferably 1.8 or less, even more preferably 1.5 or less, particularly preferably 1.2 or less, and most preferably 1.0 or less.
[0067] When the modifying group of the chemically modified fine cellulose fiber is an acyl group, the degree of acyl substitution (DS) can be calculated from the reflection infrared absorption spectrum of the esterified fine cellulose fiber based on the peak intensity ratio between the peak derived from the acyl group and the peak derived from the cellulose skeleton. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of the esterified fine cellulose fiber is calculated by plotting a correlation graph between the DS obtained from the solid-state NMR measurement of the esterified fine cellulose fiber described below and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on the acyl group to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating the calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using
[0068] The method for calculating the DS of esterified fine cellulose fiber by solid-state NMR is as follows: 13 C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 may be used. Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)
[0069] ≪Dry body≫ One aspect of the present invention provides a dried body (also referred to as a fine cellulose fiber dried body or a dried body) containing the fine cellulose fibers of the present disclosure. The dried body may be composed of only fine cellulose fibers, or may contain fine cellulose fibers and additional components. Examples of the additional components include dispersants, fine fiber filler components made of highly heat-resistant organic or inorganic polymers such as aromatic aramids, compatibilizers, plasticizers, polysaccharides, natural proteins, inorganic compounds, colorants, fragrances, pigments, flow control agents, leveling agents, conductive agents, antistatic agents, ultraviolet absorbers, ultraviolet dispersants, deodorants, and preservatives. The dried body can be produced, for example, by obtaining a fine cellulose fiber slurry by the above-mentioned method for producing fine cellulose fibers, and then heating and drying the slurry under stirring or drying under reduced pressure. The dried body containing fine cellulose fibers and additional components can be produced by a method of adding additional components to a fine cellulose fiber slurry, and then heating and drying the slurry under stirring or drying under reduced pressure, or a method of mixing a dried body of fine cellulose fibers with additional components, or the like.
[0070] <Dispersant> The dispersant means a compound that has the function of stably dispersing fine cellulose fibers and improves or controls the dispersion state of the fine cellulose fibers in the resin, thereby improving the mechanical properties of the resin composite produced using the fine cellulose fibers. In a preferred embodiment, the fine cellulose fibers are dispersed in the resin composite in the form of a dispersion containing a dispersant and the fine cellulose fibers dispersed in the dispersant. That is, the resin composite is preferably a dispersion in which the fine cellulose fibers are dispersed in the dispersant, and the dispersion is dispersed in the resin. The mass ratio of the fine cellulose fibers to the total of the fine cellulose fibers and the dispersant (100 mass%) is preferably 10 mass% or more, or 20 mass% or more, or 30 mass% or more, and preferably 99 mass% or less, or 95 mass% or less, or 90 mass% or less. The dispersant can be at least one selected from the group consisting of surfactants, organic compounds with a boiling point of 160°C or more, and resins having a chemical structure capable of highly dispersing the fine cellulose fibers, and is preferably at least one selected from the group consisting of surfactants and organic compounds with a boiling point of 160°C or more.
[0071] As the surfactant, any of anionic surfactants, nonionic surfactants, amphoteric surfactants, and cationic surfactants can be used. From the viewpoint of affinity with fine cellulose fibers, however, anionic surfactants and nonionic surfactants are preferred, and nonionic surfactants are more preferred.
[0072] As the hydrophilic group of the surfactant, from the viewpoint of affinity with fine cellulose fibers, polyoxyethylene chain, carboxyl group, and hydroxyl group are preferred, and polyoxyethylene chain is particularly preferred. Nonionic polyoxyethylene derivatives are particularly preferred. The polyoxyethylene chain length of the polyoxyethylene derivative may be 3 or more, or 5 or more, or 10 or more, or 15 or more. The longer the chain length, the higher the affinity with fine cellulose fibers, but from the viewpoint of the balance with the desired properties (e.g., mechanical properties) of the resin composite, the polyoxyethylene chain length may be 60 or less, or 50 or less, or 40 or less, or 30 or less, or 20 or less.
[0073] As the structure of the hydrophobic group of the surfactant, alkyl ether type, alkyl phenyl ether type, rosin ester type, bisphenol A type, β-naphthyl type, styrenated phenyl type, and hardened castor oil type are preferred in terms of high affinity with resin. The number of carbon atoms of the alkyl chain of the hydrophobic group (in the case of alkyl phenyl, the number of carbon atoms excluding the phenyl group) is preferably 5 or more, or 10 or more, or 12 or more, or 16 or more. For example, when the resin is a polyolefin resin, the more carbon atoms of the surfactant, the higher the affinity with the resin. The number of carbon atoms may be, for example, 30 or less, or 25 or less.
[0074] As the hydrophobic group, those having a cyclic structure or those having a bulky and multifunctional structure are more preferred. As the hydrophobic group having a cyclic structure, alkylphenyl ether type, rosin ester type, bisphenol A type, β-naphthyl type, and styrenated phenyl type groups are preferred, and as the one having a multifunctional structure, hydrogenated castor oil type (e.g. hydrogenated castor oil ether) groups are preferred. Rosin ester type and hydrogenated castor oil type are particularly preferred.
[0075] In a preferred embodiment, the surfactant is a polyethylene glycol (PEG)-polypropylene glycol (PPG) copolymer.
[0076] In one embodiment, the moisture content of the dry material containing fine cellulose fibers can be controlled to preferably 50 mass% or less, more preferably 0.01 to 40 mass%, even more preferably 0.1 to 30 mass%, particularly preferably 0.1 to 20 mass%, and most preferably 0.1 to 10 mass%, based on the total amount of the dry material.
[0077] In one embodiment, the bulk density of the dry material containing the fine cellulose fibers is preferably 0.05 g / ml to 1 g / ml, or 0.1 g / ml to 0.8 g / ml, or 0.2 g / ml to 0.7 g / ml, or 0.3 g / ml to 0.6 g / ml, in terms of keeping the storage and transportation costs low while maintaining good dispersion of the fine cellulose fibers in the resin composite. The bulk density is measured using a powder tester (PT-N type, manufactured by Hosokawa Micron Corporation), and the value of Pack Density is measured as the bulk density.
[0078] In one embodiment, the settling height ratio of the slurry when the dried fine cellulose fiber having a fine cellulose fiber concentration of 0.05% by mass is redispersed in water is preferably 5% to 50%, or 5% to 40%, or 5% to 30%, or 5% to 20%, or 10% to 20% in order to achieve good dispersion of the fine cellulose fiber in the resin composite. The settling height ratio is a value measured after preparing a dispersion as described below. Distilled water is added to the dried fine cellulose fiber so that the fine cellulose fiber is 0.05% by mass to prepare 20 g of a test dispersion. 20 g of the test dispersion is dispensed into a 30 ml glass vial, dispersed with a homogenizer (rotation speed 10,000 rpm, 5 minutes), placed in a screw-cap test tube (inner diameter 12 mm), sealed, and manually shaken to obtain a uniform dispersion.
[0079] <Resin composite> One aspect of the present invention provides a resin composite comprising the fine cellulose fibers of the present disclosure and a resin. In one aspect, the fine cellulose fibers are well dispersed in the resin with an appropriate space between them, so that they are unlikely to form aggregates, while the moderate entanglement between the fibers provides an excellent property-improving effect on the resin, so that even if a small amount of fine cellulose fibers is used, the resin composite can have excellent properties.
[0080] <Resin> The resin may be a thermoplastic resin, a thermosetting resin, or a photocurable resin. The resin may be an elastomer. From the viewpoints of moldability and productivity, a thermoplastic resin is more preferable.
[0081] (thermoplastic resin) When the resin is a thermoplastic resin, the melting point of the thermoplastic resin may be appropriately selected depending on the application of the resin composite, etc. The melting point of the thermoplastic resin can be, for example, 150°C to 190°C or 160°C to 180°C for a resin with a relatively low melting point (e.g., polyolefin resin), and 220°C to 350°C or 230°C to 320°C for a resin with a relatively high melting point (e.g., polyamide resin).
[0082] The thermoplastic resin may preferably be at least one selected from the group consisting of polyolefin-based resins, polyacetate-based resins, polycarbonate-based resins, polyamide-based resins, polyester-based resins, polyphenylene ether-based resins, and acrylic-based resins.
[0083] The polyolefin resin preferred as the thermoplastic resin is a polymer obtained by polymerizing olefins (e.g., α-olefins) and / or alkenes as monomer units.Specific examples of the polyolefin resin include ethylene (co)polymers such as low-density polyethylene (e.g., linear low-density polyethylene), high-density polyethylene, ultra-low-density polyethylene, and ultra-high-molecular-weight polyethylene, polypropylene (co)polymers such as polypropylene, ethylene-propylene copolymer, and ethylene-propylene-diene copolymer, and copolymers of ethylene and α-olefins such as ethylene-acrylic acid copolymer, ethylene-methyl methacrylate copolymer, and ethylene-glycidyl methacrylate copolymer.
[0084] Here, the most preferred polyolefin resin is polypropylene. In particular, polypropylene having a melt mass flow rate (MFR) of 3 g / 10 min or more and 30 g / 10 min or less, measured at 230° C. and a load of 21.2 N according to ISO1133, is preferred. The lower limit of MFR is more preferably 5 g / 10 min, even more preferably 6 g / 10 min, and most preferably 8 g / 10 min. The upper limit is more preferably 25 g / 10 min, even more preferably 20 g / 10 min, and most preferably 18 g / 10 min. From the viewpoint of improving the toughness of the resin composite, it is desirable that the MFR does not exceed the above upper limit, and from the viewpoint of the fluidity of the resin composite, it is desirable that the MFR does not exceed the above lower limit.
[0085] In addition, in order to increase the affinity with fine cellulose fibers, an acid-modified polyolefin resin can also be suitably used. As the acid used for the acid modification, a mono- or polycarboxylic acid can be used, and examples thereof include maleic acid, fumaric acid, succinic acid, phthalic acid and their anhydrides, and citric acid. Maleic acid or its anhydride is particularly preferred because it is easy to increase the modification rate. There is no particular restriction on the modification method, but a method in which a polyolefin resin is heated to a melting point or higher in the presence or absence of a peroxide and melt-kneaded is common. As the polyolefin resin to be acid-modified, all of the above-mentioned polyolefin resins can be used, but polypropylene is particularly suitable. The acid-modified polypropylene resin may be used alone, but it is more preferable to use it in combination with an unmodified polypropylene resin in order to adjust the modification rate of the resin as a whole. In this case, the ratio of the acid-modified polypropylene resin to all polypropylene resins is preferably 0.5% by mass to 50% by mass. A more preferred lower limit is 1 mass%, or 2 mass%, or 3 mass%, or 4 mass%, or 5 mass%. A more preferred upper limit is 45 mass%, or 40 mass%, or 35 mass%, or 30 mass%, or 20 mass%. In order to maintain the interfacial strength between the resin and the fine cellulose fibers, a content equal to or greater than the lower limit is preferred, and in order to maintain the ductility of the resin, a content equal to or less than the upper limit is preferred.
[0086] The melt mass flow rate (MFR) of the acid-modified polypropylene resin measured in accordance with ISO 1133 at 230°C and a load of 21.2 N is preferably 50 g / 10 min or more, 100 g / 10 min or more, 150 g / 10 min or more, or 200 g / 10 min or more from the viewpoint of increasing the affinity at the interface between the resin and the fine cellulose fibers. The upper limit is not particularly limited, but is preferably 500 g / 10 min from the viewpoint of maintaining mechanical strength.
[0087] Examples of polyamide-based resins that are preferable as the thermoplastic resin include polyamides obtained by polycondensation reaction of lactams (e.g., polyamide 6, polyamide 11, polyamide 12, etc.); diamines (e.g., 1,6-hexanediamine, 2-methyl-1,5-pentanediamine, 1,7-heptanediamine, 2-methyl-1-6-hexanediamine, 1,8-octanediamine, 2-methyl-1,7-heptanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, m-xylylenediamine, etc.) and dicarboxylic acids (e.g., butanedioic acid, pentanedioic acid, hexanedioic acid, , heptanedioic acid, octanedioic acid, nonanedioic acid, decanedioic acid, benzene-1,2-dicarboxylic acid, benzene-1,3-dicarboxylic acid, benzene-1,4-dicarboxylic acid, cyclohexane-1,3-dicarboxylic acid, cyclohexane-1,4-dicarboxylic acid, etc.) (for example, polyamide 6,6, polyamide 6,10, polyamide 6,11, polyamide 6,12, polyamide 6,T, polyamide 6,I, polyamide 9,T, polyamide 10,T, polyamide 2M5,T, polyamide MXD,6, polyamide 6,C, polyamide 2M5,C, etc.); and copolymers in which these are copolymerized (for example, polyamide 6,T / 6,I, etc.).
[0088] Among these polyamide resins, aliphatic polyamides such as polyamide 6, polyamide 11, polyamide 12, polyamide 6,6, polyamide 6,10, polyamide 6,11, and polyamide 6,12, and alicyclic polyamides such as polyamide 6,C and polyamide 2M5,C are more preferred.
[0089] From the viewpoint of improving the heat resistance of the resin composite, the melting point of the polyamide resin is preferably 220°C or more, or 230°C or more, or 240°C or more, or 245°C or more, or 250°C or more, and from the viewpoint of ease of production of the resin composite, the melting point is preferably 350°C or less, or 320°C or less, or 300°C or less.
[0090] The terminal carboxyl group concentration of the polyamide resin is not particularly limited, but is preferably 20 μmol / g or more, or 30 μmol / g or more, and preferably 150 μmol / g or less, or 100 μmol / g or less, or 80 μmol / g or less.
[0091] In the polyamide resin, the ratio of carboxyl end groups to all end groups ([COOH] / [total end groups]) is preferably 0.30 or more, or 0.35 or more, or 0.40 or more, or 0.45 or more from the viewpoint of dispersibility of the fine cellulose fibers in the resin composite, and is preferably 0.95 or less, or 0.90 or less, or 0.85 or less, or 0.80 or less from the viewpoint of the color tone of the resin composite.
[0092] The terminal group concentration of the polyamide resin can be adjusted by a known method, such as adding a terminal regulator (e.g., a diamine compound, a monoamine compound, a dicarboxylic acid compound, a monocarboxylic acid compound, an acid anhydride, a monoisocyanate, a monoacid halide, a monoester, a monoalcohol, etc.) that reacts with the terminal group during polymerization of the polyamide to the polymerization liquid so as to obtain a predetermined terminal group concentration.
[0093] Examples of the terminal regulator that reacts with the terminal amino group include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; and mixtures of a plurality of terminal regulators selected from the above. Among these, from the viewpoints of reactivity, stability of the blocked terminal, and cost, one or more terminal regulators selected from the group consisting of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid are preferred, and acetic acid is most preferred.
[0094] Examples of the terminal regulator that reacts with the terminal carboxyl group include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, etc., alicyclic monoamines such as cyclohexylamine, dicyclohexylamine, etc., aromatic monoamines such as aniline, toluidine, diphenylamine, naphthylamine, etc., and any mixtures thereof. Among these, one or more terminal regulators selected from the group consisting of butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline are preferred in terms of reactivity, boiling point, stability of the blocked terminal, price, etc.
[0095] The concentration of amino end groups and carboxyl end groups of the polyamide resin is 1 It can be determined from the integral value of the characteristic signal corresponding to each terminal group by H-NMR. This method is preferable in terms of accuracy and simplicity. More specifically, it is recommended to use the method described in JP-A-7-228775, use deuterated trifluoroacetic acid as the measurement solvent, and set the number of integration scans to 300 or more.
[0096] The intrinsic viscosity [η] of the polyamide resin measured under the condition of 30°C in concentrated sulfuric acid is preferably 0.6 to 2.0 dL / g, or 0.7 to 1.4 dL / g, or 0.7 to 1.2 dL / g, or 0.7 to 1.0 dL / g, from the viewpoint that the fluidity in the mold is good and the appearance of the molded piece is good when the resin composite is, for example, injection molded. In the present disclosure, the "intrinsic viscosity" is synonymous with the viscosity generally called the limiting viscosity. The intrinsic viscosity is obtained by measuring the ηsp / c of several measurement solvents having different concentrations under the temperature condition of 30°C in 96% concentrated sulfuric acid, deriving the relational equation between each of the ηsp / c and the concentration (c), and extrapolating the concentration to zero. The value extrapolated to zero is the intrinsic viscosity. Details of the above method are described, for example, in Polymer Process Engineering (Prentice-Hall, Inc. 1994), pages 291 to 294, etc. From the viewpoint of accuracy, it is desirable to set the concentrations in the measurement solvents having different concentrations to at least four points (for example, 0.05 g / dL, 0.1 g / dL, 0.2 g / dL, and 0.4 g / dL).
[0097] As the polyester resin preferred as the thermoplastic resin, one or more selected from polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polyhydroxyalkanoic acid (PHA), polylactic acid (PLA), polyarylate (PAR), etc. can be used. Among them, PET, PBS, PBSA, PBT and PEN are more preferred, and PBS, PBSA and PBT are particularly preferred.
[0098] The terminal groups of the polyester resin can be arbitrarily changed by the monomer ratio during polymerization, the presence or absence and amount of addition of a terminal stabilizer, etc. The ratio of carboxyl terminal groups to all terminal groups of the polyester resin ([COOH] / [total terminal groups]) is preferably 0.30 or more, or 0.35 or more, or 0.40, or 0.45 from the viewpoint of dispersibility of the fine cellulose fibers in the resin composite, and is preferably 0.95 or less, or 0.90 or less, or 0.85 or less, or 0.80 or less from the viewpoint of the color tone of the resin composite.
[0099] As the polyacetal resin preferred as the thermoplastic resin, homopolyacetal made from formaldehyde and copolyacetal containing trioxane as the main monomer and 1,3-dioxolane as the comonomer component are generally used, and although both can be used, copolyacetal is preferred from the viewpoint of thermal stability during processing. The amount of the structure derived from the comonomer component (e.g., 1,3-dioxolane) is preferably 0.01 mol% or more, or 0.05 mol% or more, or 0.1 mol% or more, or 0.2 mol% or more from the viewpoint of thermal stability during extrusion processing and molding processing, and is preferably 4 mol% or less, or 3.5 mol% or less, or 3.0 mol% or less, or 2.5 mol% or less, or 2.3 mol% or less from the viewpoint of mechanical strength.
[0100] (thermosetting resin) Examples of thermosetting resins include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol E type epoxy resin, bisphenol M type epoxy resin, bisphenol P type epoxy resin, and bisphenol Z type epoxy resin; novolac type epoxy resins such as bisphenol A novolac type epoxy resin, phenol novolac type epoxy resin, and cresol novolac epoxy resin; biphenyl type epoxy resin, biphenyl aralkyl type epoxy resin, aryl alkylene type epoxy resin, tetraphenylol ethane type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, phenoxy type epoxy resin, dicyclopentadiene type epoxy resin, norbornene type epoxy resin, adamantane type epoxy resin, fluorene type epoxy resin, glycidyl methacrylate copolymer epoxy resin, cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resin, epoxy modified polybutadiene rubber derivative, CTBN modified epoxy resin, trimethylolpropane polyglycidyl ether, Phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ether of ethylene glycol or propylene glycol, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl)isocyanurate, triglycidyl tris(2-hydroxyethyl)isocyanurate, novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin, unmodified resol phenolic resin, paulownia wood Examples of the resin include phenolic resins such as resol-type phenolic resins, such as oil-modified resol phenolic resins modified with oil, linseed oil, walnut oil, etc.; triazine ring-containing resins, such as phenoxy resins, urea (urea) resins, and melamine resins; unsaturated polyester resins, bismaleimide resins, diallyl phthalate resins, silicone resins, resins having a benzoxazine ring, norbornene resins, cyanate resins, isocyanate resins, urethane resins, benzocyclobutene resins, maleimide resins, bismaleimide triazine resins, polyazomethine resins, and thermosetting polyimides.
[0101] (light curing resin) Examples of photocurable resins include (meth)acrylate resins, vinyl resins, and epoxy resins. These are generally classified into radical reaction types in which a monomer reacts with radicals generated by light, and cationic reaction types in which a monomer undergoes cationic polymerization, according to the reaction mechanism. Examples of radical reaction type monomers include (meth)acrylate compounds and vinyl compounds (e.g., certain vinyl ethers). Examples of cationic reaction types include epoxy compounds and certain vinyl ethers. For example, an epoxy compound that can be used as a cationic reaction type can be a monomer for both thermosetting resins and photocurable resins.
[0102] The (meth)acrylate compound is a compound having one or more (meth)acrylate groups in the molecule. Examples of the (meth)acrylate compound include monofunctional (meth)acrylates, polyfunctional (meth)acrylates, epoxy acrylates, polyester acrylates, and urethane acrylates.
[0103] Examples of vinyl compounds include vinyl ether, styrene, and styrene derivatives. Examples of vinyl ether include ethyl vinyl ether, propyl vinyl ether, hydroxyethyl vinyl ether, and ethylene glycol divinyl ether. Examples of styrene derivatives include methyl styrene and ethyl styrene. Other examples of vinyl compounds include triallyl isocyanurate and trimethallyl isocyanurate.
[0104] As a raw material for the photocurable resin, a so-called reactive oligomer may be used. Examples of the reactive oligomer include an oligomer having any combination selected from a (meth)acrylate group, an epoxy group, a urethane bond, and an ester bond in the same molecule, such as a urethane acrylate having a (meth)acrylate group and a urethane bond in the same molecule, a polyester acrylate having a (meth)acrylate group and an ester bond in the same molecule, and an epoxy acrylate derived from an epoxy resin having an epoxy group and a (meth)acrylate group in the same molecule.
[0105] (Elastomer) Examples of elastomers (i.e. rubber) include natural rubber (NR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), isoprene rubber (IR), butyl rubber (IIR), acrylonitrile-butadiene rubber (NBR), acrylonitrile-styrene-butadiene copolymer rubber, chloroprene rubber, styrene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, isoprene-butadiene copolymer rubber, chlorosulfonated polyethylene rubber, modified natural rubber (epoxidized natural rubber (ENR), hydrogenated natural rubber, deproteinized natural rubber, etc.), ethylene-propylene copolymer rubber, acrylic rubber, epichlorohydrin rubber, polysulfide rubber, silicone rubber, fluororubber, urethane rubber, and the like.
[0106] The amount of the fine cellulose fibers relative to 100 parts by mass of the resin (thermoplastic resin in one embodiment) is preferably within the range of 0.001 to 100 parts by mass. The lower limit of the amount of the fine cellulose fibers is more preferably 0.01 parts by mass, even more preferably 0.1 parts by mass, and most preferably 1 part by mass. The upper limit of the amount of the fine cellulose fibers is more preferably 80 parts by mass, even more preferably 70 parts by mass, and most preferably 50 parts by mass. From the viewpoint of the balance between processability and mechanical properties, it is desirable to set the amount of the fine cellulose fibers within the above-mentioned range.
[0107] <Method for producing resin composite> In one embodiment, the resin composite can be produced by a method including a fine cellulose fiber production step of obtaining fine cellulose fibers by a method including beating a cellulose raw material and then defibrating it with a homomixer to obtain a fine cellulose fiber slurry, and optionally drying the fine cellulose fiber slurry under reduced pressure while stirring, and a mixing step of mixing the fine cellulose fibers (i.e., the fine cellulose fiber slurry or dried body) with a resin. More specifically, the resin composite can be produced by, for example, the following methods depending on the type of resin. When producing a resin composite containing chemically modified fine cellulose fibers, the order of chemical modification and defibration does not matter, and cellulose may be chemically modified before defibration, simultaneously with defibration, and / or after defibration.
[0108] When the resin is a thermoplastic resin, the fine cellulose fibers of the present disclosure can be kneaded with the thermoplastic resin in the form of a dispersion or a dried body (which may further contain additional components) to produce a resin composite. - A method of mixing a resin monomer and fine cellulose fibers, carrying out a polymerization reaction, extruding the resulting resin composition into a strand shape, and cooling and solidifying it in a water bath to obtain a pellet-shaped molded product; - A method in which a mixture of a resin and fine cellulose fibers is melt-kneaded using a single-screw or twin-screw extruder, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product; - A method in which a mixture of a resin and fine cellulose fibers is melt-kneaded using a single-screw or twin-screw extruder, extruded into a rod-like or tubular shape, and cooled to obtain an extrusion molded product; - A method of melt-kneading a mixture of resin and fine cellulose fibers using a single-screw or twin-screw extruder, and extruding the mixture through a T-die to obtain a sheet or film-like molded product; In a preferred embodiment, a mixture of resin and fine cellulose fibers is melt-kneaded using a single-screw or twin-screw extruder, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product. A specific example of a method for melt-kneading a resin and fine cellulose fibers is a method in which a resin and fine cellulose fibers transported in a desired ratio are mixed and then melt-kneaded.
[0109] When the resin is a thermoplastic resin, the minimum processing temperature recommended by thermoplastic resin suppliers is 255 to 270°C for nylon 66, 225 to 240°C for nylon 6, 170 to 190°C for polyacetal resin, and 160 to 180°C for polypropylene. The heating temperature setting is preferably in the range of 20°C higher than these recommended minimum processing temperatures. By setting the mixing temperature within this temperature range, the fine cellulose fibers and the resin can be mixed uniformly.
[0110] Resin composites containing a thermoplastic resin as a resin can be provided in various shapes. Specifically, resin pellets, sheets, fibers, plates, rods, etc. can be mentioned, but the resin pellet shape is more preferable from the viewpoint of ease of post-processing and ease of transportation. In this case, preferred pellet shapes include round, elliptical, and cylindrical shapes, which differ depending on the cutting method used during extrusion processing. Pellets cut by a cutting method called underwater cutting are often round, pellets cut by a cutting method called hot cutting are often round or elliptical, and pellets cut by a cutting method called strand cutting are often cylindrical. In the case of round pellets, the preferred size is a pellet diameter of 1 mm or more and 3 mm or less. In the case of cylindrical pellets, the preferred diameter is 1 mm or more and 3 mm or less, and the preferred length is 2 mm or more and 10 mm or less. It is desirable to set the above diameter and length to the lower limit or more from the viewpoint of operational stability during extrusion, and it is desirable to set them to the upper limit or less from the viewpoint of bite into the molding machine in post-processing.
[0111] A resin composite containing a thermoplastic resin as a resin can be used as various resin molded products. There is no particular limitation on the manufacturing method of the resin molded product, and any manufacturing method may be used, but injection molding, extrusion molding, blow molding, inflation molding, foam molding, etc. can be used. Among these, injection molding is most preferable from the viewpoint of design and cost.
[0112] When the resin is a thermosetting resin or a photocurable resin, the resin composite can be produced by, for example, a method of thoroughly dispersing fine cellulose fibers in a resin solution or resin powder dispersion and drying the resulting mixture, a method of thoroughly dispersing fine cellulose fibers in a resin monomer liquid and polymerizing the resulting mixture by heat, UV irradiation, a polymerization initiator, etc., a method of thoroughly impregnating a molded body (e.g., a sheet, a powder particle molded body, etc.) made of fine cellulose fibers with a resin solution or resin powder dispersion and drying the resulting mixture, a method of thoroughly impregnating a molded body made of fine cellulose fibers with a resin monomer liquid and polymerizing the resulting mixture by heat, UV irradiation, a polymerization initiator, etc. When curing, various polymerization initiators, curing agents, curing accelerators, polymerization inhibitors, etc. can be blended.
[0113] When the resin is a thermosetting resin or a photocurable resin, a method may be used in which an uncured or semi-cured sheet called a prepreg is prepared, the prepreg is made into a single layer or a laminate, and the resin is cured and molded by applying pressure and heat. Examples of the method of applying pressure and heat include a press molding method, an autoclave molding method, a bagging molding method, a wrapping tape method, and an internal pressure molding method.
[0114] When the resin is a photocurable resin, various curing methods using active energy rays can be used to produce a resin molded product.
[0115] When the resin is an elastomer, the resin composite can be produced by a method of kneading fine cellulose fibers and raw rubber in a dry state, or a method of dispersing or dissolving fine cellulose fibers and raw rubber in a dispersion medium, then drying and mixing. As a mixing method, a mixing method using a homogenizer is preferable because it can apply high shear force and pressure to promote dispersion, but other methods such as a propeller type stirring device, a rotary stirring device, an electromagnetic stirring device, and manual stirring can also be used. The resin composite containing the elastomer can be molded using a desired molding method such as mold molding, injection molding, extrusion molding, hollow molding, and foam molding to obtain an unvulcanized molded body of a desired shape such as a sheet, pellet, or powder. The unvulcanized molded body can be vulcanized by heat treatment or the like as necessary to obtain a resin molded body.
[0116] The resin molded product containing a thermoplastic resin or an elastomer may be partially (e.g., several portions) melted by heat treatment and then bonded to, for example, a resin or metal substrate. The resin molded product may be a coating applied to a resin or metal substrate, or may form a laminate with the substrate. The sheet-, film-, or fiber-shaped resin molded product may be subjected to secondary processing such as annealing, etching, corona treatment, plasma treatment, grain transfer, cutting, and surface polishing.
[0117] In the resin composite, the amount of fine cellulose fibers per 100 parts by mass of resin may be, from the viewpoint of the balance between processability and mechanical properties, preferably 0.001 parts by mass or more, or 0.01 parts by mass or more, or 0.1 parts by mass or more, or 1 part by mass or more, and may be preferably 100 parts by mass or less, or 80 parts by mass or less, or 70 parts by mass or less, or 50 parts by mass or less.
[0118] The resin composite of the present embodiment is highly heat resistant and lightweight, and can therefore be used as a substitute for steel plates, fiber reinforced plastics such as carbon fiber reinforced plastics and glass fiber reinforced plastics, and resin composites containing inorganic fillers. For example, they can be used as industrial machine parts (e.g., electromagnetic device casings, roll materials, transport arms, medical device parts, etc.), general machine parts, automobile, railway, and vehicle parts (e.g., outer panels, chassis, aerodynamic parts, seats, friction materials inside transmissions, etc.), ship parts (e.g., hulls, seats, etc.), aviation-related parts (e.g., fuselages, main wings, tails, movable surfaces, fairings, cowls, doors, seats, interior materials, etc.), spacecraft and artificial satellite parts (motor cases, main wings, structures, antennas, etc.), electronic and electrical parts (e.g., personal computer casings, mobile phone casings, office automation equipment, audio-visual equipment, telephones, facsimiles, home appliances, toys, etc.), construction and civil engineering materials (e.g., rebar substitute materials, truss structures, cables for suspension bridges, etc.), daily necessities, sports and leisure goods (e.g., golf club shafts, fishing rods, tennis or badminton rackets, etc.), wind power generation casing parts, and container and packaging parts. EXAMPLES
[0119] The present invention will be further described with reference to examples, but the present invention is not limited to these examples.
[0120] <Production of fine cellulose fibers> [Production Example 1] The cotton linter pulp was treated with a hammer mill (HM-500, manufactured by LabNect, screen mesh φ0.7 mm) to obtain pulverized pulp P1.
[0121] [Production Example 2] A pulverized pulp P2 was obtained in the same manner as in Production Example 1, except that the screen mesh was changed to φ0.3 mm.
[0122] [Production Example 3] Ground pulp P3 was obtained by the method of Production Example 2, except that the cotton linter pulp was replaced with abaca pulp.
[0123] [Production Example 4] Ground pulp P4 was obtained by the method of Production Example 1, except that cotton linter pulp was replaced with NBKP.
[0124] [Example 1: Defibration only, pulverized pulp P1] A KAPPA VITA (registered trademark) homomixer (tank size 35 L) was charged with 1 part by mass of ground pulp P1 and 19 parts by mass of DMSO, and treated for 8 hours at a homomixer rotation speed of 6000 rpm (circumferential speed 29 m / s) to obtain a fine cellulose fiber slurry (slurry S1, DMSO solvent). The slurry S1 was concentrated in a dehydrator, and then 30 parts by mass of pure water was added and thoroughly stirred, and the slurry was again placed in the dehydrator for concentration. After this, a series of washing operations, including the addition of 30 parts by mass of pure water, stirring, and concentration, was repeated a total of five times to remove DMSO, and 10 parts by mass of a fine cellulose fiber cake (cake K1, water solvent) with a solid content of 10% by mass was obtained.
[0125] [Example 2: Sequential method (acetylation after defibration), ground pulp P1] 2.1 parts by mass of vinyl acetate and 0.32 parts by mass of sodium bicarbonate were added to the fine cellulose fiber slurry (slurry S2, DMSO solvent) obtained by the same method as in Example 1, and acetylation was carried out at 60 ° C for 4 hours to obtain a fine cellulose fiber slurry (slurry S3, DMSO solvent). In order to prevent retention in the circulation line, the treatment was carried out at a homomixer rotation speed of 2000 rpm (circumferential speed 12 m / s). The acetylation reaction was stopped by adding 30 parts by mass of pure water to the slurry S3 and thoroughly stirring it, and the slurry was concentrated in a dehydrator. After this, the same washing operation as in Example 1 was repeated five times to remove DMSO, vinyl acetate, sodium bicarbonate, and by-products, and 10 parts by mass of an acetylated fine cellulose fiber cake (cake K2, water solvent) with a solid content of 10% by mass was obtained.
[0126] [Example 3: Simultaneous method (simultaneous defibration and acetylation), ground pulp P2] In a KAPPA VITA (registered trademark) homomixer (tank size 35 L), 1 part by mass of ground pulp P2, 19 parts by mass of DMSO, 2.1 parts by mass of vinyl acetate, and 0.32 parts by mass of sodium bicarbonate were added, and defibration and acetylation were simultaneously performed for 4 hours at a homomixer rotation speed of 6000 rpm (circumferential speed 29 m / s) and a treatment temperature of 60°C to obtain a fine cellulose fiber slurry (slurry S4, DMSO solvent). The subsequent reaction termination by addition of water and washing operations were performed in the same manner as in Example 2, and 10 parts by mass of an acetylated fine cellulose fiber cake (cake K3, water solvent) with a solid content of 10% by mass was obtained.
[0127] [Example 4: Sequential process, ground pulp P3] 10 parts by mass of a fine cellulose fiber cake (cake K4, water solvent) having a solid content of 10% by mass was obtained in the same manner as in Example 2, except that the ground pulp P3 was used instead of the ground pulp P1.
[0128] [Example 5: Defibration only, pulverized pulp P1] In the same manner as in Example 1 except that the homomixer treatment time was changed to 24 hours, 10 parts by mass of a fine cellulose fiber cake (cake K5, water solvent) having a solid content of 10% by mass was obtained.
[0129] [Comparative Example 1: Simultaneous method, cotton linter pulp] 10 parts by mass of an acetylated fine cellulose fiber cake (cake K6, water solvent) having a solid content of 10% by mass was obtained in the same manner as in Example 3, except that cotton linter pulp was used instead of the ground pulp P1.
[0130] [Comparative Example 2: Sequential process, abaca pulp] 10 parts by mass of a fine cellulose fiber cake (cake K7, water solvent) having a solid content of 10% by mass was obtained in the same manner as in Example 2, except that abaca pulp was used instead of the ground pulp P1.
[0131] [Comparative Example 3: Defibration only (water solvent), ground pulp P4] One part by mass of the ground pulp P4 was stirred in 50 parts by mass of water at room temperature for 1 hour at 500 rpm using a single-shaft stirrer (DKV-1 φ125 mm dissolver manufactured by Aimex). The mixture was then fed to a bead mill (NVM-1.5 manufactured by Aimex) using a hose pump, and circulated for 180 minutes using only water to obtain 51 parts by mass of fine cellulose fiber slurry (slurry S5, water solvent) with a solid content of 2.0% by mass. Finally, the slurry S5 was concentrated in a dehydrator to obtain 10 parts by mass of fine cellulose fiber cake (K8, water solvent) with a solid content of 10% by mass. During circulation operation, the rotation speed of the bead mill was 2500 rpm, the peripheral speed was 12 m / s, the beads used were made of zirconia, had a diameter of 2.0 mm, and a filling rate of 70% (the slit gap of the bead mill was 0.6 mm). During circulation operation, the slurry temperature was controlled at 40°C using a chiller to absorb heat generated by friction.
[0132] [Comparative Example 4: Defibration only (DMSO solvent), ground pulp P4] A method similar to that of Comparative Example 3 was used to obtain 31 parts by mass of a fine cellulose fiber slurry (Slurry S6, DMSO solvent) having a solid content of 3.2% by mass, except that 30 parts by mass of DMSO was used instead of 50 parts by mass of water. 30 parts by mass of pure water was added to the slurry S6, which was thoroughly stirred, and then placed in a dehydrator for concentration. The obtained wet cake was dispersed again in 30 parts by mass of pure water, stirred, and concentrated, and this washing operation was repeated a total of five times to remove DMSO, and 10 parts by mass of a fine cellulose fiber cake (K9, water solvent) having a solid content of 10% by mass was obtained. The physical properties of the cellulose raw material, pulverized pulp, and fine cellulose fibers are shown in Table 1.
[0133] The settling height ratio of fine cellulose fibers made from ground pulp was higher than that of fibers made from unground cellulose raw materials. When the solvent used for defibration was water, the number average fiber diameter was smaller and the settling height ratio was higher than when DMSO was used. For wood pulp-based NBKP, the length-weighted average fiber diameter of the ground pulp was smaller, but the settling height ratio was smaller.
[0134] <Method for producing dried fine cellulose fiber body> To the fine cellulose fiber cakes K1 to K9 obtained in Examples 1 to 5 and Comparative Examples 1 to 4, 3% by mass of hydrogenated castor oil ether (RCW-20, manufactured by Aoki Oil & Fat) was added, and the mixture was stirred in a planetary mixer (Primix Corporation, product name "Hibismix 2P-1") at 50 rpm for 10 minutes at 25°C and atmospheric pressure, and then dried under reduced pressure at 50 rpm for 8 hours under reduced pressure conditions of a jacket temperature of 80°C and -0.1 MPa to obtain dried fine cellulose fibers (CNF1 to 9). In the dried fine cellulose fiber, the mass ratio of fine cellulose fiber / hydrogenated castor oil ether was 10 / 3. The physical properties of the dried fine cellulose fiber and the resin composite are shown in Table 2. When the settling height ratio of the fine cellulose fiber itself was high, the settling height ratio of the dried fine cellulose fiber also showed a high value. This is thought to be because the fine cellulose fiber was well defibrated and an advanced network was formed in water. In addition, various physical properties of the resin composite were also excellent.
[0135] <Evaluation of cellulose raw materials and crushed pulp> [Length-weighted average fiber length] Measurements were performed using a fiber length measuring device (Kajaani FiberLab V4 (Metso Automation)) in accordance with JIS P 8226-2 "Pulp - Fiber length measurement method by optical automatic analysis method, Part 2: Non-polarized method."
[0136] <Evaluation of fine cellulose fibers> The physical properties of the fine cellulose fibers were evaluated using a porous sheet prepared by the following method. [Porous sheet] First, the wet cake was added to tert-butanol, and further dispersed in a mixer or the like until no aggregates were formed. The concentration was adjusted to 0.5% by mass per 0.5 g of the fine cellulose fiber solid content. 100 g of the obtained tert-butanol dispersion was filtered on filter paper, dried at 150°C, and then the filter paper was peeled off to obtain a sheet. The air resistance of this sheet was 10 g / m2. 2 The porous sheets with a permeability of 100 sec / 100 ml or less were used as measurement samples. The basis weight W (g / m2) of the sample left standing for one day in an environment of 23°C and 50% RH 2 After measuring the air permeability, the air permeability resistance R (sec / 100ml) was measured using an Oken air permeability tester (manufactured by Asahi Seiko Co., Ltd., model EG01). 2 The value per unit area was calculated. Weight 10g / m 2 Air resistance per unit (sec / 100ml) = R / W x 10
[0137] [Average fiber diameter] The wet cake was diluted to 0.01% by mass with tert-butanol, dispersed using a high-shear homogenizer (IKA, product name "Ultra Turrax T18") at 25,000 rpm for 5 minutes, cast onto mica, air-dried, and measured with a high-resolution scanning microscope. The magnification was adjusted so that at least 100 cellulose fibers were observed, and the minor diameter (D) of 100 randomly selected cellulose fibers was measured, and the arithmetic average of the 100 cellulose fibers was calculated.
[0138] [DS] The infrared spectrum of the porous sheet at five points was measured by the ATR-IR method using a Fourier transform infrared spectrophotometer (FT / IR-6200 manufactured by JASCO Co., Ltd.) The infrared spectrum measurement was performed under the following conditions. Number of times accumulated: 64 times, Wavenumber resolution: 4cm -1 , Measurement wave number range: 4000~600cm -1 , ATR crystal: Diamond, Incident angle: 45° From the obtained IR spectrum, the IR index was calculated according to the following formula (1): IR index = H1730 / H1030 (1) In the formula, H1730 and H1030 are at 1730 cm -1 , 1030cm -1 (absorption band of CO stretching vibration of cellulose backbone chain) -1 and 1500cm -1 The line connecting the -1 and 1500cm -1 The line connecting these points is taken as the baseline, and the absorbance is calculated when this baseline is taken as 0. Then, the average degree of substitution at each measurement site was calculated from the IR index according to the following formula (2), and the average value was taken as DS. DS = 4.13 × IR index (2)
[0139] [Crystallization degree] The porous sheet was subjected to X-ray diffraction measurement, and the crystallinity was calculated according to the following formula. Crystallinity (%)=[I (200) -I (amorphous) ] / I (200) ×100 I (200) : Diffraction peak intensity due to 200 plane (2θ=22.5°) in cellulose I crystal I (amorphous) : The halo peak intensity due to the amorphous phase in cellulose I crystals, which is the peak intensity at an angle 4.5° lower than the diffraction angle of the 200 plane (2θ=18.0°)
[0140] (X-ray diffraction measurement conditions) Equipment: MiniFlex (manufactured by Rigaku Corporation) Operation axis 2θ / θ Source CuKα Measurement method: Continuous Voltage 40kV Current 15mA Starting angle 2θ=5° End angle 2θ=30° Sampling width 0.020° Scan speed: 2.0° / min Sample: A porous sheet is attached onto the sample holder.
[0141] [Weight average molecular weight (Mw), number average molecular weight (Mn) and Mw / Mn ratio] 0.88 g of the porous sheet was weighed, cut into small pieces with scissors, lightly stirred, 20 mL of pure water was added, and left for one day. Next, the water and solids were separated by centrifugation. Next, 20 mL of acetone was added, lightly stirred, and left for one day. Next, the acetone and solids were separated by centrifugation. Next, 20 mL of N,N-dimethylacetamide was added, lightly stirred, and left for one day. N,N-dimethylacetamide and solids were separated again by centrifugation, and then 20 mL of N,N-dimethylacetamide was added, lightly stirred, and left for one day. N,N-dimethylacetamide and solids were separated by centrifugation, and 19.2 g of N,N-dimethylacetamide solution prepared so that lithium chloride was 8 mass percent was added to the solids, and the mixture was stirred with a stirrer and visually confirmed to be dissolved. The solution in which cellulose was dissolved was filtered through a 0.45 μm filter, and the filtrate was used as a sample for gel permeation chromatography. The apparatus and measurement conditions used are as follows. Equipment: Tosoh HLC-8120 Column: TSKgel SuperAWM-H (6.0mm I.D. x 15cm) x 2 Detector: RI detector Eluent: N,N-dimethylacetamide (lithium chloride 0.2%) Flow rate: 0.6mL / min Calibration curve: Pullulan conversion
[0142] [Average content of alkali-soluble polysaccharides] The alkali-soluble polysaccharide content was determined by subtracting the α-cellulose content from the holocellulose content (Wise method) according to the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pp. 92-97, 2000) for fine cellulose fibers. The alkali-soluble polysaccharide content was calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents was taken as the average alkali-soluble polysaccharide content of the fine cellulose fibers.
[0143] [Subsidence height ratio] A test dispersion was prepared by adding distilled water to the fine cellulose fiber cake so that the fine cellulose fibers were 0.05% by mass. 20 ml of the test dispersion was dispensed into a 30 ml glass vial, and then dispersed using a homogenizer (10,000 rpm for 1 minute). Then, 8 ml of the test dispersion was quickly placed in a screw-top test tube (12 mm inner diameter), sealed, and manually shaken to homogenize the dispersion. The transmittance (hereinafter also referred to as initial transmittance) of the dispersion at a wavelength of 850 nm was measured using a liquid dispersion stability evaluation device Turbiscan (manufactured by Sanyo Trading Co., Ltd.). In addition, after leaving this test tube at rest for 24 hours at 23°C, the height from the bottom of the dispersion to the separation interface and the height from the bottom of the dispersion to the top of the dispersion were measured using the liquid dispersion stability evaluation device, with the height at which the transmittance becomes 50% at the above wavelength being defined as the separation interface, and the following formula (1): Settlement height ratio (%) = ([A] / [B]) × 100 (1) (In formula (1), [A] is the height from the bottom of the dispersion to the separation interface, and [B] is the height from the bottom of the dispersion to the top of the dispersion.) In addition, when the height at which the above-mentioned permeability becomes 50% was not defined, the region with higher permeability than the above-mentioned initial permeability was defined as the supernatant part, and the region with lower permeability than the above-mentioned initial permeability was defined as the sediment part, and the boundary between the supernatant part and the sediment part was defined as the separation interface, and the sedimentation height ratio was calculated according to the above-mentioned (1). The larger the sedimentation height ratio, the better the dispersibility in the resin composite, the easier it is to form a network of fine cellulose fibers, and the better the mechanical properties (particularly tensile elongation and tensile strength).
[0144] <Evaluation of dried fine cellulose fiber> [Subsidence height ratio] Distilled water was added to the dried fine cellulose fibers so that the fine cellulose fibers were 0.5% by mass to prepare 20 g of a test dispersion. 20 g of the test dispersion was dispensed into a 30 ml glass vial, and then dispersed using a homogenizer (IKA, product name "Ultra Turrax T18", rotation speed 10,000 rpm, 5 minutes). Next, 7.2 ml of distilled water and 0.8 ml of the test dispersion were placed in a screw-cap test tube (inner diameter 12 mm), sealed, and manually shaken to make the dispersion uniform. The obtained dispersion was calculated according to the above-mentioned method for measuring the sedimentation height ratio.
[0145] <Production and evaluation of resin composite> The obtained dried fine cellulose fiber body and the following thermoplastic resin were melt-kneaded under the following conditions using a twin-screw extruder with 13 cylinder blocks (OMEGA30H manufactured by STEER, L / D=60) so that the weight of the fine cellulose fiber was 1 part by weight per 9 parts by weight of the thermoplastic resin, thereby obtaining pellets of fine cellulose fiber reinforced thermoplastic resin.
[0146] (thermoplastic resin) -UBE Nylon 1013B manufactured by Ube Industries, Ltd. Polyamide 6 (hereinafter referred to as PA) Carboxyl end group ratio: ([COOH] / [total end groups]) = 0.59 Prime Polypro J105G Made by Prime Polymer Polypropylene (hereinafter referred to as PP)
[0147] (Melt mixing conditions) Rotation speed: 300 rpm Cylinder temperature: 250°C (for PA) or 200°C (for PP)
[0148] [Tensile yield strength, tensile elongation at yield (TEy), tensile elongation at break (TEb)] Multipurpose test pieces conforming to ISO294-3 were molded using an injection molding machine with a maximum clamping pressure of 75 tons, and tests were conducted under conditions conforming to JIS K6920-2 with n=10. Note that since polyamide resin changes due to moisture absorption, it was stored in an aluminum moisture-proof bag immediately after molding to suppress moisture absorption. The ratio of the tensile elongation at yield (TEy) to the tensile elongation at break (TEb) [TEb / TEy] was calculated.
[0149] [Table 1]
[0150] [Table 2] [Industrial Applicability]
[0151] The fine cellulose fibers of the present disclosure can impart a favorable effect of improving the physical properties of a resin composite, and therefore can be suitably used in fields such as automobile interior and exterior materials.
Claims
[Claim 1] A fine cellulose fiber, The fine cellulose fibers have a ratio of the sedimentation height of the fine cellulose fibers to the total liquid height of the test dispersion (100%) of 6% or more when the test dispersion containing the fine cellulose fibers in water at a concentration of 0.05% by mass is allowed to stand at 23°C and normal pressure for 24 hours.
Citation Information
Patent Citations
Fibers containing microfibrillated cellulose and methods for producing fibers and nonwoven materials therefrom
JP2019515144A
Method for producing cellulosic resin composite
JP2020152879A
Method for producing cellulose nanofiber dispersion
WO2019176465A1
Apparatus for detecting density of manuscript
JP1987034037A
Resin composition
JP2012236906A